Adhesive film, optical component containing the same, and optical display device containing the same

The adhesive film with a refractive index of 1.55 or higher, made from a polymer mixture of aromatic group-containing (meth)acrylates, addresses low light efficiency and adhesion issues in OLEDs by enhancing light extraction and ensuring reliable adhesion, thus reducing power consumption and extending device lifespan.

JP7948788B2Active Publication Date: 2026-11-11SAMSUNG SDI CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022118582
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-26
Filing Date
2022-07-26
Publication Date
2026-11-11
Estimated Expiration
2042-07-26

AI Technical Summary

Technical Problem

Existing adhesive films for organic light-emitting devices (OLEDs) suffer from low light efficiency due to reflection and absorption of light within the device, leading to increased power consumption and reduced lifespan, and the inclusion of inorganic particles complicates adhesion and increases costs.

Method used

An adhesive film with a refractive index of 1.55 or higher, composed of a polymer mixture containing aromatic group-containing (meth)acrylates, achieving a gel fraction of 50% to 70% and an initial decomposition rate of 10% to 20%, which enhances adhesion and eliminates the need for inorganic particles, thereby improving light extraction efficiency and adhesion to patterned optical elements.

Benefits of technology

The adhesive film enhances light extraction efficiency, reduces power consumption, extends the service life of OLEDs, and ensures reliable adhesion without the drawbacks of inorganic particles, such as increased storage modulus and manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948788000008
    Figure 0007948788000008
  • Figure 0007948788000009
    Figure 0007948788000009
  • Figure 0007948788000010
    Figure 0007948788000010
Patent Text Reader

Abstract

To provide an adhesive film that improves the utilization efficiency of light entering it.SOLUTION: An adhesive film comprises a cured adhesive composition containing a polymerized monomer mixture containing at least one aromatic group-containing methacrylate. The adhesive film has a refractive index of 1.55 or more, an initial degradation rate of 10%-20%, and a gel fraction of 50%-70%. There are also provided an optical member comprising the same, and an optical display device comprising the same.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an adhesive film, an optical component containing the same, and an optical display device containing the same. [Background technology]

[0002] Organic light-emitting devices (OLEDs) contain a stacked structure of several thin films, but more than 80% of the light generated by the emitting layer is reflected or absorbed within or at the interface of the OLED, and does not exit to the front, thus reducing its light efficiency. Low light efficiency necessitates increased power consumption to achieve the desired brightness, and also reduces the lifespan of the OLED. Therefore, research to improve light efficiency is a crucial issue.

[0003] In connection with this, research is being conducted to improve the optical efficiency by stacking patterned optical elements on top of organic light-emitting elements. As one form of such research, as shown in Figure 3, a structure has been proposed in which an inorganic layer 200, a low refractive index organic layer 300, and a high refractive index organic layer 400 are sequentially formed on the upper surface of the organic light-emitting element 100. The inorganic layer 200 is formed of inorganic particles such as silicon nitride, silicon oxynitride, silicon oxide, titanium oxide, and aluminum oxide and exhibits a high refractive index. Since the high refractive index organic layer 400 is in contact with the inorganic layer 200, if it does not adhere well to the inorganic layer 200 and does not have a high refractive index, for example, a refractive index of 1.55 or higher, visibility and optical efficiency will not be improved.

[0004] Generally, to increase the refractive index, methods involving the inclusion of inorganic particles can be considered. However, the inclusion of inorganic particles makes it difficult to control the compatibility with the organic (meth)acrylate binder, increases the storage modulus (G') and reduces the adhesive strength, and the use of expensive inorganic particles leads to increased material costs. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Korean Published Patent No. 10-2007-0055363 Specification [Overview of the project] [Problems that the invention aims to solve]

[0006] The object of the present invention is to provide an adhesive film that enhances the light efficiency of incident light.

[0007] Another object of the present invention is to provide an adhesive film in which the degree of adhesion to patterned optical elements is significantly improved.

[0008] Another object of the present invention is to provide an adhesive film with high peel strength and excellent heat resistance and moisture-heat resistance.

[0009] Another object of the present invention is to provide an adhesive film that eliminates the problem of having to match compatibility with inorganic particles and the problem of increased manufacturing costs for the adhesive film. [Means for solving the problem]

[0010] The adhesive film of the present invention is obtained by curing an adhesive composition containing a polymer of monomer mixture containing one or more aromatic group-containing (meth)acrylates, wherein the adhesive film has a refractive index of 1.55 or higher, an initial decomposition rate of 10% to 20%, and a gel fraction of 50% to 70%.

[0011] Another aspect of the present invention is an optical component.

[0012] The optical component includes the adhesive film of the present invention.

[0013] Another aspect of the present invention is an optical display device.

[0014] The optical display device includes the optical film of the present invention. [Brief explanation of the drawing]

[0015] [Figure 1] This is a graph for explaining the calculation of the initial decomposition rate. [Figure 2] It is a schematic cross-sectional view showing an optical display device according to an embodiment of the present invention. [Figure 3] It is an exemplary schematic cross-sectional view of a structure for enhancing the light efficiency of an organic light-emitting element. MODES FOR CARRYING OUT THE INVENTION

[0016] The present invention will be described in detail with reference to the accompanying drawings and examples so that those of ordinary skill in the art to which the present invention pertains can easily carry out the invention. The present invention can be embodied in various different forms and is not limited to the embodiments described herein. In the drawings, portions irrelevant to the description are omitted to clearly describe the present invention, and the same or similar constituent elements are denoted by the same reference numerals throughout the entire specification.

[0017] In the present specification, "upper" and "lower" are defined based on the drawings, and depending on the viewing angle, "upper" may be changed to "lower" and "lower" to "upper". References to "on" may include not only the case of being directly on top but also the case where another structure is interposed in the middle. Meanwhile, references to "directly on", "right above", "directly formed" or "formed in direct contact" mean that no other structure is interposed in the middle.

[0018] In the present specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0019] In the present specification, the "refractive index" is a value measured in the visible light region, specifically with light having a wavelength of 633 nm.

[0020] In the present specification, the "adhesive force" is a value measured in accordance with the standard of JIS C2107:2011 for a glass plate (alkali-free glass plate) as an adherend.

[0021] In the present specification, the numerical range "X to Y" means "X or more and Y or less" (X ≤ ≤ Y).

[0022] The present invention relates to an adhesive film to be laminated on the upper surface of a patterned optical element. An inorganic layer is laminated on the upper surface of the optical element, and a pattern having a predetermined shape is formed on at least a part of the inorganic layer. The patterned optical element will be described in detail below.

[0023] The adhesive film of the present invention has the effect of increasing the light extraction efficiency of light emitted from the patterned optical element, thereby enabling high luminance to be achieved with relatively low power consumption, and thus extending the service life of the light-emitting element.

[0024] As will be described below, the above effect can be provided by setting the refractive index of the adhesive film to 1.55 or more. The adhesive film of the present invention does not contain inorganic particles with a high refractive index (e.g., a refractive index of 1.55 or more, specifically 1.55 to 2.0), such as zirconia (ZrO₂), titania (TiO₂), and the like. As a result, the adhesive film of the present invention can eliminate the problem that the compatibility between the inorganic particles and the organic polymer must be matched, the problem that the introduction of inorganic particles increases the storage elastic modulus (G') of the adhesive film and reduces the adhesive force, and the problem of increased manufacturing cost of the adhesive film due to the use of inorganic particles.

[0025] The adhesive film of the present invention exhibits remarkably superior adhesion to patterned optical elements. Here, "remarkably superior adhesion" means that the space between the patterned surface of the optical element and the adhesive film is minimized, there are no air bubbles, and the patterned surface is completely filled, resulting in perfect adhesion between the adhesive film and the patterned surface. As a result, the adhesive film of the present invention can prevent detachment and / or separation between the patterned optical element and another optical element laminated on the upper surface of the optical element, such as a polarizing plate, thereby improving the reliability of the display device. Furthermore, by minimizing the area between the patterned optical element and the adhesive film that does not adhere to each other, the adhesive film of the present invention can eliminate problems such as low light efficiency.

[0026] The adhesive film of the present invention exhibits excellent heat resistance and moisture-heat resistance. Therefore, the adhesive film of the present invention can prevent detachment and / or separation between a patterned optical element and another optical element laminated on the upper surface of the optical element, such as a polarizing plate, thereby improving the reliability of the display device.

[0027] As will be explained below, all of the effects of the present invention described above cannot be achieved simply by unconditionally increasing the peeling force of the adhesive film. Rather, they can be achieved by adjusting the gel fraction of the adhesive film to 50% to 70% and the initial decomposition rate to 10% to 20%. The gel fraction and initial decomposition rate will be explained in detail below.

[0028] The following describes an adhesive film according to one embodiment of the present invention.

[0029] The adhesive film of the present invention has a refractive index of 1.55 or higher. When the refractive index is within this range, it can provide the effect of improving the light extraction efficiency of light emitted from a light-emitting element when laminated on the light-emitting surface of a patterned optical element. For example, the adhesive film may have a refractive index of 1.55 to 1.65, specifically 1.55, 1.56, 1.57, 1.58, 1.59, 1.60, 1.61, 1.62, 1.63, 1.64, or 1.65.

[0030] The adhesive film of the present invention has an initial decomposition rate of 10% to 20% and a gel fraction of 50% to 70%. Within this range, the degree of adhesion to patterned optical elements is excellent, providing superior reliability, preventing a reduction in optical efficiency due to poor adhesion, and also providing excellent heat resistance and humidity resistance reliability. For example, the initial decomposition rate is preferably 13% to 18%, specifically 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%, and the gel fraction is preferably 50% to 65%, specifically 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, and 70%.

[0031] The initial decomposition rate is calculated from thermogravimetric analysis (TGA). Specifically, the method for determining the initial decomposition rate will be explained with reference to Figure 1.

[0032] Referring to Figure 1, when DSC is measured on an adhesive film test piece with a predetermined content, a graph (solid line graph in Figure 1) can be obtained in which the X axis is temperature (unit: °C) and the Y axis is the percentage of the weight at a specific temperature relative to the initial weight of the test piece (unit: %). The measurement conditions for DSC are as follows: 1) Temperature range: Temperature can be increased from 25°C to 700°C. 2) Heating rate: 10°C / min 3) Under a nitrogen atmosphere.

[0033] The obtained TGA graph is differentiated using a program within the DSC measuring instrument to obtain differential curves (dotted-dotted line graph in Figure 1) for temperature (T) (X-axis, unit: °C) and d(W) / d(T) (Y-axis, unit: %). After obtaining the first inflection point (A in Figure 1), the start temperature (B in Figure 1) containing the first inflection point, and the end temperature (C in Figure 1) from the obtained differential curve, the initial resolution rate is calculated by the ratio of the area between the interval from the start temperature to the end temperature and the reference line to the total area between the differential curve and the reference line. Here, the "reference line" is the line where d(W) / d(T) is 0. The initial resolution rate can be obtained using, but is not limited to, the analysis program (TRIOS, Discovery TA).

[0034] The inventors have confirmed that the initial decomposition rate is another factor that enhances the degree of adhesion to the patterned optical element. Although the specific reason for this is unknown, the initial decomposition rate is determined by the low molecular weight components among the multiple components in the adhesive film, such as the low molecular weight copolymer or oligomer in the copolymer. In the adhesive film, the low molecular weight copolymer or oligomer, or their cured products, can be expected to adhere better to the patterned surface of the optical element because they are relatively more flexible than the high molecular weight copolymer or oligomer.

[0035] The gel fraction is calculated using the following formula 1. Generally, the gel fraction is used to evaluate the degree of maturation of an adhesive film when manufacturing an adhesive film from an adhesive composition. However, the inventors have confirmed that the gel fraction is one factor that enhances the degree of adhesion to patterned optical elements.

[0036]

number

[0037] In formula 1 above, W A This is the weight of the wire mesh (in grams), W B This is the total weight (in grams) of the wire mesh and adhesive film measured after preparing a test specimen by placing 0.5 g of adhesive film inside the wire mesh. W C The weight (in grams) is measured after placing the above test specimen in a 100cc sample bottle, adding 50cc of toluene to completely immerse the test specimen in the toluene, leaving it at 25°C for 1 day, removing the test specimen from the sample bottle, and drying it at 120°C for 12 hours.

[0038] In one specific example, the mesh size of the wire mesh described above may be 100 mesh.

[0039] The adhesive film may have an adhesive strength of 800 gf / inch or more to a glass plate. Within this range of adhesive strength, it can be reliably adhered to patterned optical elements. For example, the adhesive film may have an adhesive strength of 800 gf / inch to 2000 gf / inch, specifically 800 gf / inch, 850 gf / inch, 900 gf / inch, 950 gf / inch, 1000 gf / inch, 1050 gf / inch, 1100 gf / inch, 1150 gf / inch, 1200 gf / inch, 1250 gf / inch, and 1300 gf / inch. Possible values ​​for inch are 1350gf / inch, 1400gf / inch, 1450gf / inch, 1500gf / inch, 1550gf / inch, 1600gf / inch, 1650gf / inch, 1700gf / inch, 1750gf / inch, 1800gf / inch, 1850gf / inch, 1900gf / inch, 1950gf / inch, and 2000gf / inch. Note that 1gf / inch = 0.386kg / s 2 That is the case.

[0040] The adhesive film of the present invention is optically transparent and can be used in optical display devices. In one specific example, the adhesive film may have a light transmittance of 90% or more, for example, 90% to 100%.

[0041] The adhesive film of the present invention may have a haze of 1% or less, for example, 0.001% to 0.5%. If the haze is within this range, it can be applied to optical display devices. The haze can be easily achieved because the adhesive film does not contain the aforementioned inorganic particles, thus eliminating the problem of adjusting the compatibility between the organic copolymer and the inorganic particles. The haze can be measured according to JIS K7136:2000.

[0042] The adhesive film typically has a thickness of 50 μm or less, for example, 5 μm to 30 μm. If the thickness is within this range, it can be used in optical display devices.

[0043] The adhesive film is a pressure-sensitive adhesive (PSA) film obtained by curing the adhesive composition described below. For example, the adhesive film can be manufactured by applying the adhesive composition to one surface of a release film to a predetermined thickness, drying it, and then aging it. Drying can be carried out at 100°C to 150°C for 30 seconds to 5 minutes, but is not limited to this. Aging can be carried out by leaving it at 25°C to 40°C for 1 to 5 days. After aging, a further step of leaving it at a lower aging temperature, for example, 20°C to 30°C for about 5 to 15 hours, may be performed.

[0044] The adhesive composition will be described below.

[0045] The adhesive composition of the present invention comprises a polymer of a monomer mixture containing one or more aromatic group-containing (meth)acrylic monomers and a curing agent. Here, "aromatic group" may mean an aryl group having 6 to 20 carbon atoms. The aryl group may include monocyclic, bicyclic (condensed) or ring aggregates of linked monocyclics (e.g., biphenyl group). Here, "polymer" may include one or more copolymers, oligomers, and prepolymers.

[0046] Polymers of monomer mixtures containing one or more aromatic group-containing (meth)acrylic monomers may be useful in achieving the refractive index and initial decomposition rate according to the present invention.

[0047] The above monomer mixture may contain one or more aromatic group-containing (meth)acrylic monomers and a hydroxyl group-containing (meth)acrylic monomer.

[0048] Aromatic group-containing (meth)acrylic monomers can increase the refractive index of adhesive films. In one specific example, the aromatic group-containing (meth)acrylic monomer may have a homopolymer refractive index of 1.5 or higher, specifically 1.5, 1.55, 1.6, 1.65, 1.7, for example, 1.55 to 1.7. Within this range of refractive indices, the refractive index of the present invention can be easily achieved.

[0049] Aromatic group-containing (meth)acrylic monomers may have a homopolymer glass transition temperature of 0°C to 40°C. Within this range, the adhesive film does not become too rigid, allowing it to adhere well to patterned optical elements. For example, the glass transition temperature may be 0°C to 35°C, specifically 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, and 40°C. In this specification, the “homopolymer glass transition temperature” can be determined by referring to the product catalog or by measuring it using a method commonly known to those skilled in the art.

[0050] The adhesive film of the present invention contains a large amount of aromatic group-containing (meth)acrylic monomers having the glass transition temperature of the homopolymer described above, as explained below, in order to increase the refractive index and achieve an initial decomposition rate. The adhesive film may have a glass transition temperature of -5°C to 20°C, specifically -5°C, -4°C, -3°C, -2°C, -1°C, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, and 20°C.

[0051] Aromatic group-containing (meth)acrylic monomers can be those containing one aromatic group, but it is preferable to use monomers containing two or more aromatic groups. Monomers containing two or more aromatic groups can easily increase the refractive index of the adhesive film even when used in the same amount compared to monomers containing one aromatic group. In one specific example, the aromatic group-containing (meth)acrylic monomer can contain two to five aromatic groups.

[0052] In one specific example, an aromatic group-containing (meth)acrylic monomer may have a structure represented by the following chemical formula 1:

[0053] [ka]

[0054] In the above chemical formula 1, * represents a linking site. X is a single bond, an alkylene group with 1 to 5 carbon atoms, or an oxygen atom (O).

[0055] The aromatic group-containing (meth)acrylic monomer may be a monofunctional (meth)acrylate having one (meth)acryloyloxy group. This minimizes the problem of the adhesive film becoming hard and causing poor adhesion to patterned optical elements due to excessive polymerization of the monomer during polymer production, and makes it easy to reach the initial decomposition rate and adhesive strength specified in the present invention.

[0056] In one specific example, the aromatic group-containing (meth)acrylic monomer may include the compound represented by the following chemical formula 2:

[0057] [ka]

[0058] In the above chemical formula 2, X is a single bond, an alkylene group with 1 to 5 carbon atoms, or an oxygen atom (O). Y is either a hydrogen or a methyl group. R1 is an alkyl group having 1 to 10 carbon atoms, a halogen atom, or an aryl group having 6 to 20 carbon atoms. n is an integer between 0 and 5. R2 is an alkylene group having 1 to 10 carbon atoms or a mono or polyalkylene oxy group with a total of 1 to 30 carbon atoms.

[0059] In one specific example, in the above chemical formula 2, the mono or polyalkylene oxy group with a total number of carbon atoms from 1 to 30 is -*(-O-R3-) n -*(* represents a linking site, R3 is an alkylene group with 1 to 3 carbon atoms, and n is an integer from 1 to 10).

[0060] For example, an aromatic group-containing (meth)acrylic monomer may include one or more of the following: phenylbenzyl (meth)acrylate, including o-phenylbenzyl acrylate, m-phenylbenzyl acrylate, or p-phenylbenzyl acrylate; phenoxybenzyl (meth)acrylate; monoethoxylated phenylphenoxy (meth)acrylate; polyethoxylated phenylphenoxy (meth)acrylate, including diethoxylated phenylphenoxy (meth)acrylate; etc.

[0061] In one specific example, the monomer mixture may include at least one (meth)acrylic monomer having an aromatic group.

[0062] In another specific example, since the refractive index, glass transition temperature, etc. of the homopolymer differ for each (meth)acrylic monomer having an aromatic group, the effects of the present invention can be more easily realized by mixing and including two or more (meth)acrylic monomers having an aromatic group.

[0063] For example, an aromatic group-containing (meth)acrylic monomer may be a mixture of a (meth)acrylic monomer having a first aromatic group in which X in the above chemical formula 2 is a single bond or an alkylene group having 1 to 5 carbon atoms, and a second aromatic group having a second aromatic group in which X in the above chemical formula 2 is oxygen (O). By using such a mixture, an increase in adhesiveness and an improvement in flexibility can be obtained.

[0064] The (meth)acrylic monomer having the first aromatic group may, but is not limited to, phenylbenzyl acrylate. The (meth)acrylic monomer having the second aromatic group may, but is not limited to, phenoxybenzyl (meth)acrylate.

[0065] The (meth)acrylic monomer having the first aromatic group may be included in a content of 70% to 90% by mass, specifically 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, for example, 70% to 80% by mass, based on the total mass of the monomer mixture. The (meth)acrylic monomer having a second aromatic group may be included in the total mass of the monomer mixture in an amount of 1% to 15% by mass, specifically 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, for example, 5% to 15% by mass.

[0066] To give another example, the (meth)acrylic monomer having an aromatic group may include a mixture of a (meth)acrylic monomer having a third aromatic group in which R2 in the above chemical formula 2 is an alkylene group having 1 to 10 carbon atoms or an oxygen atom, and a (meth)acrylic monomer having a fourth aromatic group in which R2 in the above chemical formula 2 is a (poly)alkylene oxy group having 1 to 30 carbon atoms. The (meth)acrylic monomer having the fourth aromatic group provides flexibility, which can further enhance the degree to which the adhesive film adheres to the patterned optical element.

[0067] The (meth)acrylic monomer having a third aromatic group may include, but is not limited to, one or more phenylbenzyl acrylate and phenoxybenzyl (meth)acrylate. The (meth)acrylic monomer having a fourth aromatic group may include, but is not limited to, one or more monoethoxylated phenylphenoxy(meth)acrylate and poly(ethoxylated)phenylphenoxy(meth)acrylate.

[0068] The (meth)acrylic monomer having a third aromatic group may be included in a content of 70% to 90% by mass, specifically 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, for example, 70% to 80% by mass, based on the total mass of the monomer mixture. The (meth)acrylic monomer having a fourth aromatic group may be included in the monomer mixture in an amount of 1% to 15% by mass, specifically 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, for example, 5% to 15% by mass, relative to the total mass.

[0069] One or more aromatic group-containing (meth)acrylic monomers may be included in a content of 75% to 95% by mass, specifically 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, for example, 75% to 90% by mass and 75% to 85% by mass, based on the total mass of the monomer mixture. Within the above content range, the refractive index of the adhesive film can be ensured, and the problem of low adhesive strength of the adhesive film can be eliminated.

[0070] The (meth)acrylic monomer having a hydroxyl group may include one or more (meth)acrylic monomers having an alkyl group with 1 to 20 carbon atoms and containing one or more hydroxyl groups in the ester moiety, and one or more (meth)acrylic monomers having a cycloalkyl group with 3 to 20 carbon atoms and containing one or more hydroxyl groups in the ester moiety.

[0071] (Meth)acrylic monomers containing hydroxyl groups may have a lower glass transition temperature for their homopolymers compared to (meth)acrylic monomers containing aromatic groups. This can increase the adhesive strength of adhesive films, allowing them to adhere well to patterned optical elements and improve overall adhesion. For example, (meth)acrylic monomers containing hydroxyl groups may have a glass transition temperature of -10°C or lower for their homopolymers, specifically -50°C, -45°C, -40°C, -35°C, -30°C, -25°C, -20°C, -15°C, -10°C, for example, -50°C to -10°C.

[0072] In one specific example, as the (meth)acrylic monomer having a hydroxyl group, a (meth)acrylate having an alkyl group with 1 to 20 carbon atoms and one or more hydroxyl groups in the ester moiety can be used. Specifically, the (meth)acrylic monomer having a hydroxyl group may include one or more of the following: 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 1-chloro-2-hydroxypropyl (meth)acrylate. The (meth)acrylic monomer having a hydroxyl group can be used alone or as a mixture of two or more.

[0073] The (meth)acrylic monomer having hydroxyl groups can be included in the monomer mixture in an amount of 5% to 25% by mass, specifically 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, for example, 10% to 25% by mass and 15% to 25% by mass, based on the total mass of the monomer mixture. Within the above content range, the effects of the present invention can be easily achieved. In the present invention, in order to provide an adhesive film that adheres well to patterned optical elements, a (meth)acrylic monomer having a relatively high content of hydroxyl groups compared to conventional methods is used.

[0074] The total content of (meth)acrylic monomers having aromatic groups and (meth)acrylic monomers having hydroxyl groups may be 95% by mass or more, for example, 98% to 100% by mass, preferably 100% by mass, in the monomer mixture.

[0075] The monomer mixture may contain (meth)acrylic acid esters having a linear or branched alkyl group with 1 to 10 carbon atoms in the ester moiety. The (meth)acrylic acid esters having a linear or branched alkyl group with 1 to 10 carbon atoms may include one or more of the following: methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, iso-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate.

[0076] Because the above polymer has a high polydispersity index (PDI), the molecular weight distribution of the oligomers, copolymers, etc. contained in the polymer is broad. The inventors have confirmed that such a high polydispersity index can be useful in achieving the initial decomposition rate and gel fraction in the present invention. In one specific example, the above polymer may have a polydispersity index (PDI) of 5 or higher, specifically about 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, for example, 5 to 10.

[0077] The above polymers have a weight-average molecular weight of 100,000 g / mol to 5,000,000 g / mol, specifically 100,000, 500,000, 1,000,000, 1,500,000, 2,000,000, 2,500,000, 3,000,000, 3,500,000, 4,000,000, 4,500,000, and 5,000,000 g / mol, for example, 100,000 g / mol to 3,000,000 g / mol and 100,000 g / mol to 2,000,000 g / mol. If the weight-average molecular weight is within the above range, the adhesive strength and durability reliability of the adhesive film can be ensured.

[0078] The polydispersion index mentioned above can be calculated (Mw / Mn) by measuring the weight-average molecular weight (Mw) and number-average molecular weight (Mn) using gel permeation chromatography (GPC).

[0079] The above polymer can be produced by adding an initiator to the monomer mixture and then polymerizing it. The initiator may include one or more photopolymerization initiators and thermal polymerization initiators. The photopolymerization initiator and thermal polymerization initiator may be conventional ones known to those skilled in the art. For example, the initiator may be azo polymerization initiator; and / or a conventional one containing a peroxide such as benzoyl peroxide or acetyl peroxide.

[0080] The initiator may be included in an amount of 0.01 to 0.5 parts by mass, preferably 0.01 to 0.1 parts by mass, and more preferably 0.03 to 0.08 parts by mass, per 100 parts by mass of the monomer mixture. Within the above content range, polymers can be easily obtained.

[0081] Polymerization can include conventional polymerization methods known to those skilled in the art, such as suspension polymerization, emulsion polymerization, and solution polymerization. The polymerization temperature may be 60°C to 80°C, and the polymerization time may be 4 to 8 hours. Within this range, polymers can be easily obtained.

[0082] The curing agent can cure the polymer to form the matrix of the adhesive film and enhance its adhesive strength. The curing agent may include one or more isocyanate-based curing agents, epoxy-based curing agents, metal chelate-based curing agents, and aziridine-based curing agents. Preferably, an isocyanate-based curing agent can be used as the curing agent.

[0083] Isocyanate-based curing agents include toluene diisocyanates (TDI) containing hexamethylene diisocyanate (HDI), 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, etc., 4,4'-methylenediphenyl diisocyanate (MDI), xylylene diisocyanates (XDI) containing 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, etc., hydrogenated toluene diisocyanate, isophorone diisocyanate, 1,3-bisisocyanate methylcyclohexane, and tetramethylxylene. This may include diisocyanates, 1,5-naphthalene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, trimethylolpropane / toluene diisocyanate trimer adducts, trimethylolpropane xylylene diisocyanate adducts, triphenylmethane triisocyanate, methylenebistriisocyanate, and other isocyanate-based curing agent adducts as described above.

[0084] A curing agent, such as an isocyanate-based curing agent, may be included in an amount of 0.01 to 1 part by mass per 100 parts by mass of the polymer, specifically 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, or 1 part by mass, for example, from 0.01 to 0.5 parts by mass. Within this range of content, it is possible to achieve the effect of simultaneously satisfying durability and adhesive strength.

[0085] The adhesive composition may further contain a silane coupling agent.

[0086] Silane coupling agents can enhance the adhesive strength and reliability of adhesive films.

[0087] Silane coupling agents may include one or more acetylacetonate-based silane coupling agents having an acetylacetonate group, acetacetate-based silane coupling agents having an acetacetate group, and epoxy-based silane coupling agents having an epoxy group. For example, epoxy-based silane coupling agents may include, but are not limited to, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc. Acetylacetonate-based silane coupling agents or acetacetate-based silane coupling agents may include, but are not limited to, 3-(trimethoxysilyl)propylacetate, acetylacetonatetrimethoxysilane, acetylacetonatetriethoxysilane, etc.

[0088] The silane coupling agent may be included in an amount of 0.1 to 1 part by mass per 100 parts by mass of the polymer, specifically 0.1 parts by mass, 0.15 parts by mass, 0.2 parts by mass, 0.25 parts by mass, 0.3 parts by mass, 0.35 parts by mass, 0.4 parts by mass, 0.45 parts by mass, 0.5 parts by mass, 0.55 parts by mass, 0.6 parts by mass, 0.65 parts by mass, 0.7 parts by mass, 0.75 parts by mass, 0.8 parts by mass, 0.85 parts by mass, 0.9 parts by mass, 0.95 parts by mass, or 1 part by mass, for example, 0.1 to 0.5 parts by mass. Within the above content range, the adhesive strength of the adhesive film can be further improved.

[0089] The adhesive composition may further include a curing catalyst, additives, etc.

[0090] The curing catalyst may include, for example, tin-based catalysts such as dibutyltin dilaurate and dioctyltin dilaurate, and iron-based catalysts such as tris(acetylacetonate)iron, tris(hexane-2,4-dionate)iron, and tris(heptane-2,4-dionate)iron, as metal catalysts. The curing catalyst may be included in an amount of 0.001 to 0.01 parts by mass, specifically 0.005 to 0.01 parts by mass, per 100 parts by mass of the polymer. Within this content range, the effects of the present invention may be more easily realized.

[0091] The additives may include, for example, common additives known to those skilled in the art, such as antistatic agents, particles, fillers, antioxidants, heat stabilizers, ultraviolet absorbers, and surfactants. The additive may be included in an amount of 0.001 to 5 parts by mass, specifically 0.01 to 1 part by mass, per 100 parts by mass of the polymer. Within this content range, the effect of the additive can be obtained without affecting the physical properties of the adhesive layer.

[0092] The adhesive composition may be solvent-free or may further contain a solvent. When the adhesive composition contains a solvent, the adhesive film can be made thinner, improving its applicability. The solvent can be any ordinary solvent known to those skilled in the art. For example, the solvent may include one or more of methyl ethyl ketone, ethyl acetate, and toluene.

[0093] The optical component of the present invention includes the adhesive film of the present invention.

[0094] The following describes an optical component according to one embodiment of the present invention.

[0095] The optical component includes a first adhesive film and a polarizing plate laminated on the upper surface of the first adhesive film, and the first adhesive film may include the adhesive film of the present invention.

[0096] A polarizing plate may include a polarizer and a protective layer or protective film laminated on at least one surface of the polarizer. The polarizer, protective layer, and protective film may be of ordinary types known to those skilled in the art.

[0097] The optical component may further include a second adhesive film between the first adhesive film and the polarizing plate. The second adhesive film has a lower refractive index than the first adhesive film. The second adhesive film can increase the adhesive force between the first adhesive film and the polarizing plate, thereby improving the reliability of the optical component.

[0098] The optical display device includes the adhesive film or optical component of the present invention. The optical display device may include an light-emitting element display device that includes an organic light-emitting element, an inorganic light-emitting element, an organic-inorganic hybrid light-emitting element, and the like.

[0099] An optical display device, which is one embodiment of the present invention, will be described below with reference to Figure 2.

[0100] Referring to Figure 2, the optical display device includes an organic light-emitting element 100, a patterned optical element laminated on the upper surface of the organic light-emitting element 100, and a high refractive index organic layer 500. The patterned optical element includes an inorganic layer 200 and a low refractive index organic layer 300 laminated sequentially from the organic light-emitting element 100, and the high refractive index organic layer 500 may include the adhesive film of the present invention. The low refractive index organic layer 300 is placed on the inorganic layer 200 and can be a protruding pattern having a predetermined cross-sectional shape. Such a patterned optical element can ensure process stability. As shown in Figure 2, the low refractive index organic layer 300 may have a pattern surface in which a plurality of patterns having a predetermined cross-section are spaced apart from each other, with spacing between patterns of 10 μm to 1000 μm, and pattern height, i.e., step difference, of 1 μm to 100 μm. The low refractive index organic layer 300 is not particularly limited, but can be formed from an acrylic material. [Examples]

[0101] The configuration and operation of the present invention will be described in more detail below with reference to preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be construed as limiting the present invention in any way.

[0102] Manufacturing Example 1: Production of (meth)acrylic polymers 80 parts by mass of ethyl acetate was added to a 1 L reactor equipped with a cooling device to facilitate temperature control and reflux of nitrogen gas. 100 parts by mass of a monomer mixture containing 70 parts by mass of p-phenylbenzyl acrylate (PBA), 15 parts by mass of phenoxybenzyl acrylate (PoBA), and 15 parts by mass of 4-hydroxybutyl acrylate (4-HBA, homopolymer glass transition temperature: -40°C) was added to the reactor. A mixture of ethyl acetate and methyl ethyl ketone was further added to the reactor. To remove oxygen from the monomer mixture, nitrogen gas was introduced into the reactor for 1 hour to purge it, and then the internal temperature of the reactor was maintained at 70°C. After uniformly stirring the monomer mixture, 0.05 parts by mass of azobisisobutyronitrile (AIBN), an initiator, was added, and the polymerization reaction was carried out for 4 hours to produce a solution containing a (meth)acrylic polymer. Ethyl acetate was then added to produce a (meth)acrylic polymer solution with a solid content of 35% by mass.

[0103] Manufacturing Examples 2-7: Production of (meth)acrylic polymers A (meth)acrylic polymer solution was prepared in the same manner as in Production Example 1, except that the content of each monomer, polymerization time, and / or initiator were changed as shown in Table 1 below (unit: parts by mass). In Table 1 below, "-" indicates that the corresponding component is not included.

[0104] [Table 1]

[0105] The components used in the following examples and comparative examples are as follows: (1) Hardener: Hexamethylene diisocyanate hardener (CK-164, manufactured by NCI) (2) Silane coupling agent: Acetylacetone trimethoxysilane (A-50, manufactured by Soken Chemical Co., Ltd.).

[0106] Example 1 Based on the solid content, 100 parts by mass of the (meth)acrylic polymer from Production Example 1, 0.4 parts by mass of the curing agent, and 0.25 parts by mass of the silane coupling agent were mixed, and 10 parts by mass of toluene was added and the mixture was stirred for 30 minutes to produce an adhesive composition.

[0107] The manufactured adhesive composition was applied to a first release film (peel strength of the adhesive film relative to the first release film: 12 gf / inch, PET film, RPK501, manufactured by Toray Industries, Inc.) to a predetermined thickness and dried at 120°C for 2 minutes to form an adhesive film coating (thickness: 20 μm). A second release film (peel strength of the adhesive film relative to the second release film: 3 gf / inch, PET film, RPK201, manufactured by Toray Industries, Inc.) was laminated onto the adhesive film coating, and the mixture was subjected to primary aging for 2 days under constant temperature and humidity conditions (35°C and 45% RH relative humidity), followed by an additional aging for 12 hours under constant temperature and humidity conditions (23°C and 55% RH relative humidity) to produce an adhesive sheet in which the first release film, adhesive film (thickness: 20 μm), and second release film were laminated in that order.

[0108] Examples 2 to 5 An adhesive sheet was manufactured in the same manner as in Example 1, except that the type of (meth)acrylic polymer and / or the content of the curing agent were changed as shown in Table 2 below, by laminating a first release film, an adhesive film (thickness: 20 μm), and a second release film in that order.

[0109] Comparative Example 1 and Comparative Example 2 An adhesive sheet was manufactured in the same manner as in Example 1, except that the type of (meth)acrylic polymer and / or the content of the curing agent were changed as shown in Table 2 below, by laminating a first release film, an adhesive film (thickness: 20 μm), and a second release film in that order.

[0110] The adhesive sheets produced in the examples and comparative examples were evaluated for the following physical properties, and the results are shown in Table 2 below.

[0111] (1) Initial decomposition rate (unit: %): The initial decomposition rate was measured using a thermogravimetric analyzer (TGA) instrument, Discovery (first generation) manufactured by TA Instruments. The release film was completely peeled off the adhesive sheet to obtain the adhesive film, and 0.1 g of the adhesive film was placed in a Discovery (first generation) instrument manufactured by TA Instruments. The temperature was increased from 25°C to 700°C at a heating rate of 10°C / min under a nitrogen atmosphere, and the result of temperature (T) (X axis, unit: °C) - weight (W) (Y axis, unit: %) was obtained as shown in Figure 1. By differentiating the obtained result, temperature (T) (X axis, unit: °C) - d(W) / d(T) (Y axis, unit: %) was obtained. The first inflection point was found in the obtained differential curve, and after setting a temperature range that includes the inflection point and the start and end temperatures, the initial decomposition rate was obtained using the analysis program (TRIOS, Discovery TA).

[0112] (2) Gel fraction (unit: %): The release film was completely peeled off from the adhesive sheet to obtain the adhesive film, and 0.5g of the adhesive film was taken from it. The weight (W) was measured in advance against a wire mesh (100 mesh). A The weight (W) was measured. 0.5g of adhesive film was completely wrapped in this wire mesh to prevent any leakage of the adhesive film, and the weight (W) of the adhesive film and the entire wire mesh was measured. B The weight (W) was measured again. Next, the adhesive film and the entire wire mesh were placed in a 100cc sample bottle for gel fraction measurement. Subsequently, 50cc of toluene was added to the sample bottle so that the adhesive film and the entire wire mesh were completely submerged in toluene. This was left at 25°C for 1 day. Then, the adhesive film and the entire wire mesh were removed from the sample bottle and dried in a 120°C oven for 12 hours, and the weight (W) was measured again. C The following values ​​were measured. The gel fraction was calculated according to formula 1 below.

[0113]

number

[0114] (3) Refractive index: All release films were peeled off from the pressure-sensitive adhesive sheet to obtain a pressure-sensitive adhesive film. The pressure-sensitive adhesive film was measured using a prism coupler (Metricon, model 2010 / M) with light at a wavelength of 633 nm.

[0115] (4) Adhesive strength (unit: gf / inch): The adhesive strength is the 180° adhesive strength between the pressure-sensitive adhesive film and a glass plate (alkali-free glass plate), which was measured in accordance with the JIS C2107:2011 standard. The pressure-sensitive adhesive sheet was cut into a size of 25 mm in length × 100 mm in width, the second release film was peeled off, the resulting sheet was attached to a glass plate [35 mm in length × 110 mm in width], and the first release film was peeled off from the pressure-sensitive adhesive film. Using a 30 kgf load cell, the glass plate and the pressure-sensitive adhesive film were connected to the upper jig and the lower jig of a tensile tester, respectively, and the load (adhesive strength) when the pressure-sensitive adhesive film was peeled off from the glass plate at a tensile speed of 300 mm / min, a tensile angle of 180°, and a tensile temperature of 25°C was measured.

[0116] (5) Durability: The pressure-sensitive adhesive sheet was cut into 150 mm in width × 90 mm in length, the second release film was removed, and the resulting sheet was attached to one surface of a glass plate (alkali-free glass plate) [170 mm in length × 110 mm in width], at 4 to 5 kg / cm 2 of pressure, the first release film was removed to prepare a test specimen. This test specimen was left to stand at 85°C for 500 hours (heat resistance reliability), then further left to stand at normal temperature for 1 hour, and the appearance was evaluated according to the following criteria. This test specimen was left to stand in a constant temperature chamber at 85°C and a relative humidity of 95% RH for 500 hours (moisture resistance reliability), then further left to stand at normal temperature for 1 hour, and the appearance was evaluated according to the following criteria: ◎: No bubbles or lifting at all ○: Slight presence of bubbles or lifting △: Moderate presence of bubbles or lifting ×: Both bubbles and lifting occur, making the product unusable.

[0117] (6) Degree of adhesion to the patterned structure: An acrylic organic patterned structure was prepared with a patterned surface having a pattern spacing of 500 μm and a step height of 10 μm, and the adhesive side of an adhesive film was laminated to the patterned surface. After that, it was autoclaved (50°C, 5 bar, 1000 seconds), and the degree of filling of the step height was observed using a microscope and evaluated according to the following criteria: ◎: No air bubbles, completely filled. ○: No air bubbles, filled to 90% or more. △: Some air bubbles are present and more than 50% is filled. ×: There are many air bubbles and it is less than 50% filled.

[0118] [Table 2]

[0119] As shown in Table 2 above, the adhesive film of the present invention has a high refractive index. Therefore, although not shown in Table 2 above, when applied to an optical display device, the light efficiency of the incident light can be increased. As shown in Table 2 above, the adhesive film of the present invention has excellent adhesion to the patterned surface. Therefore, although not shown in Table 2 above, by minimizing the area between the patterned surface and the adhesive film that is not adhered to each other, the problem of low light efficiency is almost eliminated. As shown in Table 2 above, the adhesive film of the present invention has excellent moisture and heat resistance and heat resistance. Therefore, although not shown in Table 2 above, by preventing separation and / or detachment between the patterned optical element and other optical elements laminated on the upper surface of the optical element, such as a polarizing plate, the reliability of the display device can be increased.

[0120] Therefore, the present invention can provide an adhesive film that enhances the optical efficiency of incident light. Furthermore, the present invention can provide an adhesive film that exhibits remarkably superior adhesion to patterned optical elements. Furthermore, the present invention can provide an adhesive film with high peel strength and excellent heat resistance and moisture-heat resistance. Moreover, the present invention can provide an adhesive film that virtually eliminates the problem of having to match compatibility with inorganic particles and the problem of increased manufacturing costs for the adhesive film.

[0121] On the other hand, the comparative adhesive films that did not satisfy one or more of the gel fraction range and initial decomposition rate ranges of the present invention could not obtain the effects of the present invention.

[0122] Simple modifications or alterations of the present invention can be easily carried out by a person with ordinary skill in the art, and all such modifications or alterations can be considered to fall within the scope of the present invention. [Explanation of Symbols]

[0123] 100 Organic light-emitting elements, 200 inorganic layer, 300 Low refractive index organic layer, 400, 500 high refractive index organic layer.

Claims

1. An adhesive film obtained by curing an adhesive composition containing a polymer of monomer mixtures containing one or more aromatic group-containing (meth)acrylates, The aromatic group-containing (meth)acrylate is a mixture of a (meth)acrylic monomer having a first aromatic group in which X in the following chemical formula 2 is a single bond or an alkylene group having 1 to 5 carbon atoms, and a (meth)acrylic monomer having a second aromatic group in which X in the following chemical formula 2 is an oxygen atom (O). The monomer mixture comprises a (meth)acrylic monomer having a hydroxyl group, The monomer mixture contains, with respect to the total mass of the monomer mixture, two or more aromatic group-containing (meth)acrylates in an amount of 75% to 95% by mass, and the hydroxyl group-containing (meth)acrylic monomer in an amount of 5% to 25% by mass. The adhesive film has a refractive index of 1.55 or higher, an initial decomposition rate of 10% to 20%, and a gel fraction of 50% to 70%. 【Chemistry 1】 In the aforementioned chemical formula 2, X is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxygen atom (O). Y is a hydrogen atom or a methyl group. R 1 This is an alkyl group having 1 to 10 carbon atoms, a halogen atom, or an aryl group having 6 to 20 carbon atoms. n is an integer between 0 and 5. R 2 This is an alkylene group having 1 to 10 carbon atoms, or a (poly)alkylene oxy group having 1 to 30 carbon atoms.

2. The adhesive film according to claim 1, wherein the adhesive film has a peeling force of 800 gf / inch or more on a glass plate.

3. The adhesive film according to claim 1, wherein the glass transition temperature is -5°C to 20°C.

4. The adhesive film according to claim 1, wherein the adhesive film does not contain inorganic particles with a high refractive index.

5. The adhesive film according to claim 1, wherein the aromatic group-containing (meth)acrylate has a homopolymer glass transition temperature of 0°C to 40°C.

6. The adhesive film according to claim 1, wherein the (meth)acrylic monomer having the first aromatic group is phenylbenzyl (meth)acrylate, and the (meth)acrylic monomer having the second aromatic group is phenoxybenzyl (meth)acrylate.

7. The adhesive film according to claim 1, wherein the (meth)acrylic monomer having a hydroxyl group has a homopolymer glass transition temperature lower than that of the aromatic group-containing (meth)acrylic monomer.

8. The adhesive film according to claim 1, wherein the adhesive composition further comprises one or more isocyanate-based curing agents and silane coupling agents.

9. An optical component comprising an adhesive film according to any one of claims 1 to 8.

10. An optical display device comprising an adhesive film according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Optics adhesive composition, optics adhesive sheet and optical product

    JP2015081288A

  • Composition for transparent adhesive sheet, and transparent adhesive sheet

    JP2016020442A

  • Photocurable resin composition having high refractive index

    JP2018127528A

  • Acrylic resin and adhesive composition

    JP2020158564A

  • Acrylic pressure sensitive adhesive compositions

    KR1020070055363A