Surface-enhancing Raman scattering agent
A viscous dispersion of thin pieces with noble metal layers in a viscous liquid addresses the rigidity and flexibility issues of existing substrates, enabling sensitive quantitative analysis on various surfaces by enhancing Raman scattering.
Patent Information
- Application Number
- JP2022548353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-14
- Filing Date
- 2021-09-10
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-09-10
AI Technical Summary
Existing surface-enhanced Raman scattering substrates are rigid and inflexible, limiting their application to non-flat surfaces and making it difficult to perform measurements on curved surfaces, while flexible agents have limited use methods and sensitivity.
A viscous dispersion of thin pieces with noble metal layers or particles in a viscous liquid, providing flexibility and enhancing the local electric field for improved sensitivity and applicability to various surfaces.
The surface-enhanced Raman scattering agent allows for highly sensitive quantitative analysis on diverse surfaces, including direct measurements on skin and non-flat surfaces, with enhanced Raman scattered light amplification.
Smart Images

Figure 0007948837000001 
Figure 0007948837000002 
Figure 0007948837000003
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a surface-enhanced Raman scattering agent, a method for performing quantitative analysis by Raman spectroscopy using the surface-enhanced Raman scattering agent, and a kit for performing the quantitative analysis. This disclosure claims priority to Japanese Patent Application No. 2020-153721, filed in Japan on September 14, 2020, which is incorporated herein by reference. [Background technology]
[0002] Raman spectroscopy is an analytical method that identifies substances by analyzing the spectrum of scattered light generated when light is shone on the substance. However, a problem with Raman spectroscopy has been its low sensitivity.
[0003] Therefore, in recent years, there has been a great deal of research on surface-enhanced Raman scattering, which improves sensitivity by amplifying Raman scattering through the enhancement effect of the local electric field that occurs when local plasmons of noble metal components such as Au and Ag are excited.
[0004] Furthermore, Patent Document 1 describes a surface-enhanced Raman scattering substrate in which metal-coated silica is laminated on the surface of a glass substrate. It states that by placing a sample on the substrate and performing analysis by Raman spectroscopy, an effect of enhancing Raman scattering can be obtained, and measurements can be performed with high sensitivity.
[0005] Furthermore, Non-Patent Document 1 describes a surface-enhanced Raman scattering agent having minute columnar structures constructed on a flexible sheet by dynamic oblique deposition. In addition, Non-Patent Document 2 describes a surface-enhanced Raman scattering agent comprising noble metal nanostructures supported on nanocellulose. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2004-170334 [Non-patent literature]
[0007] [Non-Patent Document 1] K. Xu, R. Zhou, K. Takei, and M. Hong, Adv. Sci., 2019,1900925. [Non-Patent Document 2] J. Chen, M. Huang, L. Kong, and M. Lin, Carbonhydr. Polymn., 205, 516(2019). [Overview of the project] [Problems that the invention aims to solve]
[0008] However, the surface-enhanced Raman scattering substrate described in Patent Document 1 had the problem of having limited usage methods. For example, even when attempting to directly measure biomarkers from the skin surface of a subject, the surface-enhanced Raman scattering substrate is hard and rigid and lacks flexibility, making it impossible to make the substrate conform to the examination site, and thus the surface-enhanced Raman scattering effect could not be obtained. In addition, it was difficult to fix the surface-enhanced Raman scattering substrate along the non-flat surface of a Raman measuring instrument with a sample collection function (for example, a curved surface such as a toilet or chamber pot) and perform surface-enhanced Raman scattering measurements.
[0009] Furthermore, while the surface-enhanced Raman scattering agents described in Non-Patent Documents 1 and 2 have greater flexibility compared to the surface-enhanced Raman scattering substrate described in Patent Document 1, their methods of use were still limited.
[0010] Therefore, the object of this disclosure is to provide a surface-enhanced Raman scattering agent that enables highly sensitive quantitative analysis by Raman spectroscopy and is applicable to various usage methods. Another object of this disclosure is to provide a surface-enhanced Raman scattering agent that enables direct surface-enhanced Raman scattering measurement by being attached in close contact with the skin surface of a subject or fixed to a Raman measuring instrument with a sample collection function. Another object of this disclosure is to provide a surface-enhanced Raman scattering measurement kit applicable to various measurement methods. Another object of this disclosure is to provide a surface-enhanced Raman scattering measurement method using the surface-enhanced Raman scattering agent. Another object of this disclosure is to provide a method for producing the surface-enhancing Raman scattering agent. [Means for solving the problem]
[0011] The present inventors, after diligent research to solve the above problems, have found that a surface-enhanced Raman scattering substrate, in which a surface-enhanced Raman scattering agent is fixed to a glass substrate, exhibits rigidity and lacks flexibility, whereas a viscous dispersion, in which thin pieces having a noble metal layer and / or noble metal particles on the surface are dispersed in a viscous liquid, is flexible or fluid, and therefore applicable to various uses. Furthermore, they have found that using the viscous dispersion significantly enhances the local electric field generated when local plasmons are excited, dramatically increasing the enhancement effect of Raman scattered light, thereby improving the sensitivity of Raman spectroscopy and enabling minute quantitative analysis. This disclosure is completed based on these findings.
[0012] In other words, this disclosure relates to a viscous liquid having a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10(1 / s), A small piece containing a noble metal is dispersed in the aforementioned viscous liquid, The present invention provides a surface-enhancing Raman scattering agent containing the following:
[0013] This disclosure also provides the surface-enhancing Raman scattering agent wherein the precious metal is gold, silver, or copper.
[0014] This disclosure also provides a surface-enhancing Raman scattering agent wherein the precious metal-containing thin piece has a structure on its surface in which minute columnar bodies are arranged, and at least a portion of the minute columnar bodies is formed of a precious metal layer or precious metal particles.
[0015] The present disclosure also provides the surface-enhanced Raman scattering agent, wherein the thin pieces are thin pieces composed of an inorganic oxide having a hydroxyl group.
[0016] The present disclosure also provides the surface-enhanced Raman scattering agent, wherein the thin pieces are thin pieces of glass, silica, talc, mica, or titanium oxide.
[0017] The present disclosure also provides a surface-enhanced Raman scattering measurement kit comprising the surface-enhanced Raman scattering agent.
[0018] The present disclosure also provides a surface-enhanced Raman scattering measurement method, which comprises performing surface-enhanced Raman scattering measurement using the surface-enhanced Raman scattering agent.
[0019] The present disclosure also provides a method for producing the surface-enhanced Raman scattering agent, comprising a step of pulverizing a noble metal-containing thin plate in a viscous liquid having a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10 (1 / s).
Effects of the Invention
[0020] The surface-enhanced Raman scattering agent of the present disclosure has flexibility or fluidity, and also has adhesiveness. Therefore, it can be applied to various usage methods. For example, a test specimen can be obtained by adhering the agent to a potty for infants, a toilet bowl, or the like, and discharging urine so as to come into contact with the surface-enhanced Raman scattering agent. If a surface-enhanced Raman scattering spectrum is acquired from the test specimen thus obtained, components in urine can be measured. Further, by using the surface-enhanced Raman scattering agent, the Raman scattered light emitted by the test substance can be remarkably amplified. Thereby, the test substance can be identified and / or quantified with high sensitivity.
[0021] By using the aforementioned surface-enhancing Raman scattering agent, the Raman peak characteristic of equol can be recognized with high sensitivity. Therefore, even in samples containing both equol and equol-like substances, it is possible to distinguish between equol and equol-like substances, and to selectively and sensitively quantify equol in the sample.
[0022] Therefore, by using the surface-enhanced Raman scattering agent, the presence or absence of equol production ability can be easily and accurately determined by measuring the equol concentration in the urine, blood, etc., of the subject. Thus, the surface-enhanced Raman scattering agent is also useful for testing the presence or absence of equol production ability. [Brief explanation of the drawing]
[0023] [Figure 1] This is a typical surface-enhanced Raman scattering spectrum of 4,4'-bipyridine obtained using the surface-enhanced Raman scattering agent of the present disclosure. [Figure 2] This figure shows the relationship between the stirring time during the preparation stage and the peak height around 1600 cm⁻¹ obtained using the surface-enhanced Raman scattering agent. [Figure 3] This figure shows the Raman spectrum obtained by surface-enhanced Raman scattering measurement of 4,4'-bipyridine using a gel-like dispersion containing gold colloid. [Modes for carrying out the invention]
[0024] [Surface-enhancing Raman scattering agent] The surface-enhancing Raman scattering agent of this disclosure comprises a viscous liquid and thin pieces containing a noble metal dispersed in the viscous liquid. The viscous liquid is a viscous liquid having a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10¹ / s.
[0025] The surface-enhancing Raman scattering agent has a configuration in which thin pieces containing noble metals are dispersed in the viscous liquid.
[0026] The surface-enhancing Raman scattering agent comprises at least a small piece containing a precious metal and the viscous liquid, and may further contain one or more other components. Examples of other components include thickeners, surfactants, dispersion stabilizers (e.g., citric acid), pH adjusters (e.g., toluene, xylene, hydrochloric acid), preservatives (e.g., neutral formalin, sodium azide, thymol, isothiazolone compounds), deodorants, fragrances, and the like.
[0027] As the surface-enhancing Raman scattering agent, a gel-like dispersion is particularly preferred because it allows for high-concentration contact of thin, precious metal-containing fragments with the substance under test, and improves the surface-enhancing Raman scattering effect by maintaining the contact.
[0028] The viscosity of the surface-enhancing Raman scattering agent at 25°C and a shear rate of 10¹ / s is, for example, 50 to 100,000 mPa·s, preferably 100 to 50,000 mPa·s, and particularly preferably 200 to 30,000 mPa·s.
[0029] Furthermore, the viscosity can be measured using a viscosity / viscoelasticity measuring device (rheometer, product name "RheoStress600", manufactured by HAAKE).
[0030] With the aforementioned surface-enhancing Raman scattering agent, the intensity of the Raman scattered light is amplified by the interaction between the Raman scattered light and the electromagnetic waves on the surface of the noble metal structure. Therefore, even if the concentration of the test substance in the sample is very small, it can be quantified with high accuracy.
[0031] Generally, the limit of 4,4'-bipyridine concentration that can be measured by Raman spectroscopy is at most about 10 mmol / L. However, by using the surface-enhanced Raman scattering agent disclosed herein, even if the 4,4'-bipyridine content in the sample is very small, it can be accurately quantified. Using the surface-enhanced Raman scattering agent disclosed herein, for example, 4,4'-bipyridine at a concentration of 1 mmol / L can be measured.
[0032] The aforementioned surface-enhanced Raman scattering agent allows for highly sensitive measurement of equol. It is known that in adult subjects with equol-producing ability, the equol concentration in their urine is typically 1 to 75 μmol / L. Therefore, by quantifying the equol contained in a subject's urine using the aforementioned surface-enhanced Raman scattering agent, it is easy to determine whether or not the subject has equol-producing ability.
[0033] (Thin pieces containing precious metals) The aforementioned precious metal-containing thin piece is a structure having a configuration in which a precious metal component is attached to the surface of the thin piece.
[0034] The average thickness of the thin pieces is, for example, 10 to 50 μm. The average thickness of the thin pieces can be determined by dividing the weight of the piece by its density to obtain its volume, and then dividing this volume by the area of the piece.
[0035] The average value of the equivalent circular diameter (measured by image analysis) of the aforementioned thin pieces is, for example, 10 to 500 μm, preferably 20 to 50 μm.
[0036] The surface of the thin piece may be flat, but it may also be mechanically or chemically surface-treated.
[0037] The thin flakes are preferably made of an inorganic oxide having hydroxyl groups, such as silica, talc, mica, titanium oxide, glass, etc. Among these, mica flakes are preferred. This is because mica is easy to crush into thin flakes and also functions as an internal standard for surface-enhanced Raman scattering.
[0038] The aforementioned precious metal is preferably at least one selected from gold, silver, and copper.
[0039] The aforementioned precious metal-containing thin piece is preferably a structure having a precious metal layer on the surface of the thin piece, or having precious metal particles on the surface of the thin piece, or having a precious metal layer and precious metal particles on the surface of the thin piece.
[0040] The aforementioned precious metal-containing thin piece is preferably a structure in which minute columnar bodies are arranged in a forest on the surface of the thin piece, in that it is particularly excellent in enhancing Raman scattering light, and at least a part of the minute columnar bodies is formed of a precious metal layer or precious metal particles, more preferably a structure having a configuration in which minute columnar bodies having a precious metal layer are arranged in a forest on the surface of the thin piece, and particularly preferably a structure having a precious metal layer on the surface of the thin piece, and having a configuration in which minute columnar bodies having a precious metal layer are arranged in a forest on the surface of the precious metal layer.
[0041] The aforementioned minute columnar bodies may be minute columnar bodies composed of precious metal particles, i.e., rod-shaped precious metal particles, or they may be minute columnar layers composed of materials other than precious metals on which precious metal layers are laminated.
[0042] Preferably, the aforementioned precious metal-containing thin piece is a structure in which minute columnar bodies are arranged in a forest on the surface of the thin piece, with layers of materials other than precious metals and layers of precious metals laminated together.
[0043] Other materials besides the aforementioned precious metals are preferably transparent materials in that they generate plasma resonance when irradiated with light from a light source. Examples of such transparent materials include SiO2, Ta2O5, TiO2, and LiF.
[0044] The area where the precious metal layer is provided may be at least a part of the minute columnar body, and may be the tip, end, or central part of the minute columnar body. Furthermore, the layer may be provided in only one of the aforementioned areas, or in two or more areas.
[0045] The minute columnar bodies are preferably standing perpendicular to the surface of the thin piece, but they may be slightly inclined. Furthermore, the spacing between adjacent minute columnar bodies is preferably small enough that scattering of light from the light source does not become a problem. Adjacent minute columnar bodies may be in contact with each other.
[0046] Furthermore, it is preferable that the minute columnar bodies exhibit an anisotropic shape, as this is particularly excellent in enhancing the Raman scattered light. Regarding the anisotropic shape, it is preferable that the ratio (aspect ratio) of the longitudinal length to the transverse length of the cut surface when the minute columnar body is cut by a plane substantially parallel to the thin piece is 2 or more, as this creates a difference in the transmission characteristics with respect to the optical axis of the incident light, resulting in a remarkable enhancement effect of the Raman scattered light.
[0047] Furthermore, it is preferable that the minute columnar bodies exhibiting an anisotropic shape on the surface of the thin piece are formed while being oriented in one direction.
[0048] A structure (1) having a configuration in which anisotropic micro-columnar bodies, each having a laminated structure of a transparent layer and a precious metal layer, stand in a forest on the surface of a thin piece can be manufactured, for example, by a process of manufacturing a micro-columnar transparent layer, a process of manufacturing a precious metal layer, and a process of crushing the thin plate (preferably a thin plate made of an inorganic oxide having hydroxyl groups) on top of a thin plate. The order in which the manufacturing process of the micro-columnar transparent layer and the manufacturing process of the precious metal layer can be appropriately selected according to the desired structure of the micro-columnar bodies.
[0049] Furthermore, when alternating between a transparent layer and a precious metal layer, the manufacturing process for the micro-columnar transparent layer and the manufacturing process for the precious metal layer can be repeated alternately.
[0050] <Manufacturing process for micro-columnar transparent layers> This process involves forming a micro-columnar transparent layer. For example, when forming a micro-columnar transparent layer directly on a thin plate, the thin plate is tilted at an angle of approximately 45° to 88° with respect to the incident direction of the deposition flow of the transparent micro-columnar material. Once a film with a thickness of 5 to 100 nm is formed, the in-plane orientation of the thin plate is reversed by 180°. This results in a thin plate with an anisotropic transparent layer that extends long in the direction perpendicular to the surface.
[0051] Furthermore, the aforementioned thin plate will be crushed into thin fragments, and is a thin plate-like material formed from the same material as the thin fragments.
[0052] <Manufacturing process for precious metal layers> This process involves laminating a precious metal layer. For example, when laminating a precious metal layer on a micro-columnar transparent layer, the precious metal can be deposited on the surface of the transparent layer formed on the thin plate obtained through the above process, from a direction perpendicular to the upright transparent layer, at a deposition angle of 45° to 88°. This allows the precious metal to be deposited on the tip of the micro-columnar layer. This makes it possible to form a micro-columnar body consisting of a laminated transparent layer and a precious metal layer.
[0053] The deposition of the precious metal may be carried out while inverting the thin plate in the plane, similar to the process used to manufacture transparent micro-columnar layers, or it may be carried out obliquely from only one direction without inverting the plate in the plane.
[0054] The thickness of the precious metal layer can be appropriately selected depending on the light source used, but for example, it is 50 nm or less.
[0055] Through the above process, a structure (2) is obtained having a configuration in which anisotropic minute columnar bodies having a transparent layer / precious metal layer laminated structure stand in a forest on the surface of a thin plate.
[0056] <Grinding process> The next step is to pulverize the thin plate portion of the structure (2) obtained through the above process. In this step, it is preferable to pulverize the structure in a viscous liquid because it is possible to pulverize the thin plate while maintaining the structure of the minute columnar bodies formed on the surface of the thin plate.
[0057] It is preferable to use a viscous liquid that may contain a surface-enhancing Raman scattering agent as the viscous liquid used in the grinding process, and in particular, it is preferable to use a viscous liquid (especially preferably a gel-like dispersion) with a viscosity of 50 to 100,000 mPa·s at 25°C and a shear rate of 10¹ / s. This can reduce the impact of grinding and improve the structural integrity of the micro-columnar bodies.
[0058] The grinding time varies depending on the grinding method, but for example, when grinding stainless steel balls (SUS balls) with a diameter of 1.0 mm by rotating them at a rotation speed of 2000 rpm on the orbit and 800 rpm on the axis, the grinding time is about 1 to 10 minutes, and preferably 4 to 9 minutes, and especially preferably more than 4 minutes but less than 6 minutes, in order to improve the surface-enhanced Raman scattering effect.
[0059] (viscous liquid) The viscous liquid is a liquid with a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10¹ / s. Using a liquid with low Raman activity as the viscous liquid is preferable in terms of improving the quantitative accuracy of the substance being tested.
[0060] The viscous liquid is preferably a gel-like dispersion, as it allows for high-concentration contact of the noble metal-containing thin fragments with the substance to be tested and improves the surface-enhanced Raman scattering effect by maintaining the contact state.
[0061] The viscous liquid contains a water-soluble solvent and an oil-based solvent. Specifically, the viscous liquid contains solvents such as water, alcohol, and oils. These can be used individually or in combination of two or more.
[0062] Examples of the aforementioned alcohols include methanol, ethanol, propanol, butanol, and other alcohols; and polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, and glycerin.
[0063] Examples of the aforementioned oils include hydrocarbon oils such as mineral oil and liquid paraffin; sunflower oil, macadamia nut oil, avocado oil, almond oil, wheat germ oil, rice germ oil, olive oil, soybean oil, corn oil, castor oil, beef tallow, jojoba oil, evening primrose oil, coconut oil, camellia oil, rosehip oil, squalane, turtle oil, mink oil, egg yolk oil, lanolin, whale wax, candelilla wax, montan wax, rice wax, lanolin wax, shellac, and other animal and vegetable oils; and carbonated water such as hexane, cyclohexane, isododecane, benzene, toluene, poly-alpha-olefin, and liquid paraffin. Examples include raw oils; ethers such as tetrahydrofuran; halogenated hydrocarbons such as carbon tetrachloride and chlorobenzene; petroleum components such as kerosene, gasoline, diesel fuel, and heavy oil; silicone oils such as dimethylpolysiloxane and methylphenylpolysiloxane; ester oils such as octyldodecyl oleate, cetyl ethylhexanoate, glyceryl triisooctanate, and neopentyl glycol diisooctanate; higher alcohols such as hexadecyl alcohol and oleyl alcohol; higher fatty acids such as lauric acid, isostearic acid, and oleic acid; aromatic carboxylic acids, pyridine, etc.
[0064] Examples of solvents with high Raman activity include N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dimethylacetamide (DMAA), N-methylpyrrolidone (NMP), tetrahydrofuran (THF), cyclohexanone, lactam, lactone, and N,N,N,N-tetramethylurea. When using these solvents, the amount used (or the total amount if two or more are used in combination) is preferably, for example, 30% by weight or less, more preferably 20% by weight or less, particularly preferably 10% by weight or less, most preferably 5% by weight or less, and especially preferably 1% by weight or less of the total amount of viscous liquid contained in the surface-enhancing Raman scattering agent.
[0065] (Thickening agent) If the viscosity of the solvent is low, a thickening agent can be added to increase its viscosity. The thickening agent can be appropriately selected depending on the type of solvent.
[0066] When the solvent is a water-soluble solvent, examples of thickeners include cellulosic polymer compounds such as hydroxyethylcellulose, methylcellulose, ethylcellulose, and carboxymethylcellulose; plant-derived natural polymer compounds such as carrageenan and guar gum; microbial-derived natural polymer compounds such as xanthan gum; animal-derived natural polymer compounds such as casein and gelatin; starch-based polymer compounds such as carboxymethyl starch; vinyl-based polymer compounds such as polyvinyl alcohol, polyvinylpyrrolidone, sodium polyacrylate, and carboxyvinyl polymer; polyether-based polymer compounds such as polyethylene glycol, polypropylene glycol, and polyglycerin; and polyoxyalkylene-modified sugars such as polyoxyethylene methyl glucoside and polyoxypropylene methyl glucoside.
[0067] When the solvent is an oily solvent, examples of thickeners include sugar fatty acid esters, 12-hydroxystearic acid, 1,3,2,4-dibenzylidene-D-sorbitol, N-lauroyl-L-glutamic acid-α,γ-bis-n-butylamide, benzene fatty acid amide, cyclohexane fatty acid amide, and the like. The sugar fatty acid esters also include, for example, dextrin fatty acid esters such as dextrin palmitate and dextrin myristate; and inulin fatty acid esters such as inulin stearate.
[0068] [Surface-enhanced Raman scattering measurement method] The surface-enhanced Raman scattering measurement method disclosed herein is a measurement method using the surface-enhanced Raman scattering agent and surface-enhanced Raman scattering spectroscopy. More specifically, the method involves contacting a sample with the surface-enhanced Raman scattering agent to create a test specimen, and then identifying and quantifying the substances contained in the test specimen by analyzing the scattered light produced when the test specimen is irradiated with excitation light.
[0069] There are no particular limitations on the method for bringing the surface-enhancing Raman scattering agent into contact with the sample, as long as the sample can be brought into contact with the surface of the precious metal-containing thin fragments in the surface-enhancing Raman scattering agent. Examples include fixing the surface-enhancing Raman scattering agent on the surface of a substrate and dropping a liquid sample (or a liquid preparation if the sample is not liquid) onto it, or mixing the surface-enhancing Raman scattering agent and the liquid sample on a sample stage or the like.
[0070] [Method for measuring equol] The above-mentioned method for measuring equol is a method for measuring (identifying and / or quantifying) equol contained in a sample using the above-described surface-enhanced Raman scattering measurement method. More specifically, the method involves contacting the sample with the surface-enhanced Raman scattering agent to create a test specimen, and then analyzing the scattered light produced when the test specimen is irradiated with excitation light to quantify the equol contained in the test specimen.
[0071] In the aforementioned method for measuring equol, by analyzing the peak that is characteristic of equol, that is, the peak that appears in equol but not in equol-like substances, it is possible to selectively quantify equol in a sample in which equol and equol-like substances are present.
[0072] The peak characteristic of the aforementioned equol may vary slightly depending on experimental conditions such as the measuring equipment used, but for example, it is 1530-1630 cm⁻¹. -1 , 1230~1330cm -1 , 1140~1240cm -1 , and 535~635cm -1 At least one wavenumber region selected from the group, preferably 1570-1590 cm⁻¹ -1 , 1270~1290cm -1 , 1180~1200cm -1 , and 570~590cm -1 Examples include a peak appearing in at least one wavenumber region selected from the group (= a peak having its peak position in the wavenumber region).
[0073] According to the above-described method for measuring equol, the surface-enhancing Raman scattering agent is used to amplify the Raman scattering of equol contained in the sample, thereby enabling selective and highly sensitive measurement of equol.
[0074] [Method for testing equol production ability] The method for testing equol production ability is a method for testing whether or not a subject has the ability to produce equol, and the method for testing equol production ability includes measuring equol in a sample taken from the subject using the method for measuring equol described above.
[0075] If a subject has the ability to produce equol, they will have equol-producing bacteria in their intestines. When a subject ingests daidzein, a type of isoflavone, these bacteria metabolize daidzein to produce equol. The produced equol is then absorbed from the intestinal tract into the bloodstream, and a portion of it is excreted in the urine. Therefore, by using urine, blood, or intestinal contents, or the supernatant obtained by centrifugation of these, as a sample and quantifying the amount of equol contained in the sample, it is easy to determine whether or not a subject has the ability to produce equol (or whether or not a subject has equol-producing bacteria).
[0076] Examples of equol-producing bacteria include microorganisms belonging to the genera Lactococcus, Slackia, Adlercreutzia, Asaccharobacter, and Eggerthella. More specifically, examples include Lactococcus garvieae, Adlercreutzia equolifaciens, Asaccharobacter celatus, and Eggerthella sp.YY7918.
[0077] In the aforementioned method for testing equol production ability, equol is measured selectively and with high sensitivity using the equol measurement method described above, making it possible to accurately determine whether or not equol production ability is present, or whether or not equol-producing bacteria are present.
[0078] [Surface-enhanced Raman scattering measurement kit] The surface-enhanced Raman scattering measurement kit disclosed herein is a kit for performing measurements by surface-enhanced Raman scattering spectroscopy and includes at least the surface-enhanced Raman scattering agent described above.
[0079] The kit may also include other components besides the surface-enhancing Raman scattering agent, and preferably includes a device capable of identifying Raman peaks. The device is preferably a Raman spectrometer (for example, including a light source, a filter to remove Rayleigh scattered light, a spectrometer to decompose Raman scattered light into a spectrum, a detector, etc.).
[0080] As the light source, for example, a light source that emits laser light (preferably near-infrared laser light) is preferred.
[0081] Examples of how to use the aforementioned measurement kit include the following methods. 1. A test specimen is formed by bringing the surface-enhancing Raman scattering agent into contact with the sample. 2. The test specimen is irradiated with light from a light source to produce Raman scattered light and Rayleigh scattered light. 3. The scattered light is passed through a filter to remove Rayleigh scattered light. 4. The scattered light after Rayleigh scattering has been removed is introduced into a spectrometer, and the introduced scattered light is decomposed into a spectrum in the spectrometer. 5. Detect the spectrum with a detector.
[0082] As the light source, for example, a light source that emits laser light (preferably near-infrared laser light) is preferred.
[0083] By using the aforementioned measurement kit, Raman scattering of the test substance can be amplified by the surface-enhanced Raman scattering agent. Therefore, microquantitation of the test substance is possible.
[0084] Furthermore, by using the aforementioned measurement kit, equol can be selectively identified and / or quantified with high sensitivity, so the aforementioned measurement kit may be, for example, an equol measurement kit.
[0085] Furthermore, by using the aforementioned measurement kit and using a subject's urine, blood, or intestinal contents, or a supernatant thereof as a specimen to perform identification and / or quantitation of equol, it is possible to easily determine whether the subject has equol-producing ability. Therefore, the aforementioned measurement kit may be a test kit for equol-producing ability.
[0086] As described above, the respective configurations of the present disclosure and combinations thereof are examples, and additions, omissions, substitutions, and modifications of the configurations can be appropriately made without departing from the gist of the present disclosure. In addition, the present disclosure is not limited by the embodiments, and is limited only by the description of the claims. [Examples]
[0087] Hereinafter, the present disclosure will be described more specifically with reference to Examples, but the present disclosure is not limited by these Examples.
[0088] Preparation Example 1 (Production of a structure having a configuration in which micro-pillars having a transparent layer / noble metal layer laminated structure are erected in a forest arrangement) The surface-enhanced Raman scattering substrate of the structure having a configuration in which anisotropic micro-pillars having a transparent layer / noble metal layer laminated structure are erected in a forest arrangement was produced by the dynamic oblique deposition method described in Japanese Patent No. 4783907. Specifically, it was produced by the following method.
[0089] 50×50mm 2 A mica substrate cut to the size of was cleaved to a thickness of 15 to 30 μm that can maintain its shape, and subjected to ultraviolet cleaning to obtain a thin mica plate. After that, the mica thin sheet was attached to the dynamic oblique deposition apparatus, 3 × 10 -4 The system was evacuated until the pressure dropped below Pa, and then the film was deposited in the following order: Ag mirror layer, SiO2 micro-columnar layer, and Ag layer. First, silver was deposited to a thickness of 200 nm at a deposition angle of 0° and an average deposition rate of approximately 0.20 nm / s to create an Ag mirror-finish layer. Next, 99.99% pure silica (SiO2) particles were deposited onto the Ag mirror layer at a deposition angle of 0° and an average deposition rate of 0.2-0.3 nm / s to a film thickness of 105 nm. Then, a continuous bidirectional oblique deposition method, a type of dynamic oblique deposition method, was used to construct a micro-columnar layer of SiO2. In the continuous bidirectional oblique deposition method, the mica sheet was quickly rotated 180° every 20 nm of film thickness deposited at a deposition angle of approximately 82°, and then deposited again until a film thickness of 20 nm was reached. This inversion of the mica sheet was repeated 30 times. Finally, silver was deposited onto the SiO2 micro-columnar layer using an electron beam at a deposition angle of 70° and an average deposition rate of 0.20 nm / s, creating an Ag layer with an average thickness of approximately 8 nm. In this way, a structure was obtained in which minute columnar bodies were arranged in a manner in which an SiO2 layer and a noble metal layer were laminated on the surface of a mica thin sheet on which an Ag mirror layer was provided.
[0090] Example 1 (Preparation of thin pieces containing precious metals dispersed in a viscous liquid) Ultrapure water and hydroxyethylcellulose (HEC) powder (SE400, Daicel FineChem Ltd.) were placed in a 30mm lidded container and stirred with a stirrer for 2 minutes. The stirring speed was 2000 rpm orbital and 800 rpm rotational. The HEC concentration was 10% by weight. A viscous liquid was obtained. The viscosity of the viscous liquid was measured using a rheometer (product name "Physica MCR301", manufactured by Anton Paar) under conditions of 25°C and a shear rate of 10¹ / s, and was found to be approximately 10⁴ Pa·s.
[0091] 1.0 g of the obtained viscous liquid was placed in a lidded container with a base diameter of 30 mm and a capacity of 12 mL. Next, the structure obtained in Preparation Example 1 was placed in a 9.0 cm container. 2The material was cut into approximately 5mm squares and placed in the viscous liquid so that the mica sheet side was in contact with it. Furthermore, stainless steel balls (SUS balls) with a diameter of 1.0mm were added and stirred to create a dispersion. The stirring was performed with the rotation speed fixed at 2000 rpm orbit and 800 rpm rotation, and the stirring time was varied in 1-minute increments up to 10 minutes.
[0092] Under these conditions, it was found that when the stirring time was 4 to 6 minutes, a gel-like dispersion was obtained in which thin pieces of the aforementioned structure were dispersed in a viscous liquid.
[0093] Example 2 (Measurement of surface-enhanced Raman scattering) In Example 1, the gel-like dispersion 1 obtained after stirring for 5 minutes was subjected to the following surface-enhanced Raman scattering measurement.
[0094] 5x5mm on a 1.5mm thick silicone rubber 2 A cell was prepared by creating a pore and placing the gel-like dispersion 1 inside. 30 μL of a 1 mM 4,4'-bipyridine aqueous solution was dropped onto the top surface of the gel-like dispersion 1, and then a coverslip was placed over it. After 60 minutes, the cell was placed in the measurement area of a LambdaVision RAM200 Raman spectrometer, and a 785 nm (100 mW) laser was irradiated for 1 second. The Raman scattering spectrum was obtained by averaging two measurements (Figure 1). A typical surface-enhanced Raman scattering spectrum of 4,4'-bipyridine is shown in Figure 1.
[0095] From the above, it was confirmed that the gel-like dispersion 1 obtained in Example 1 exhibits excellent surface-enhanced Raman scattering effect.
[0096] Example 3 Surface-enhanced Raman scattering measurements were performed in the same manner as in Example 2, except that the dispersions obtained by varying the stirring time from 1 to 10 minutes were used, and Raman scattering spectra were obtained. Then, at 1600 cm², -1 The peak heights in the surrounding area were plotted for each stirring time of the dispersion (Figure 2).
[0097] As shown in Figure 2, the strongest surface-enhanced Raman scattering effect was obtained when using a dispersion with a stirring time of 5 minutes.
[0098] Comparative Example 1 Gold colloid was agglomerated with salt and immediately dispersed in a 10% by weight viscous HEC liquid. The dispersion method was carried out by stirring, following the same procedure as in Example 1. This yielded gel-like dispersion 3.
[0099] The Raman scattering spectrum of 4,4'-bipyridine was obtained in the same manner as in Example 2, except that gel dispersion 3 was used instead of gel dispersion 1 (Figure 3).
[0100] As shown in Figure 3, the characteristic peak of 4,4'-bipyridine was not observed even when a gel-like dispersion containing gold colloid was used.
[0101] In summary, the structure of this disclosure and its variations are described below. [1] Having a configuration in which thin pieces containing precious metals are dispersed in a viscous liquid, The viscous liquid is a surface-enhancing Raman scattering agent, wherein the viscous liquid has a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10¹ / s. [2] A surface-enhancing Raman scattering agent having a configuration in which thin pieces containing precious metals are dispersed in a gel-like dispersion. [3] The surface-enhancing Raman scattering agent according to [1] or [2], wherein the precious metal is gold, silver, or copper. [4] The surface-enhancing Raman scattering agent according to any one of [1] to [3], wherein the precious metal-containing thin piece has a forest of minute columnar bodies on its surface, and at least a portion of the minute columnar bodies is a structure formed of a precious metal layer or precious metal particles. [5] The surface-enhancing Raman scattering agent according to any one of [1] to [4], wherein the precious metal-containing thin piece is a structure having a configuration in which minute columnar bodies having a precious metal layer on the surface of the thin piece are arranged in a forest. [6] The surface-enhancing Raman scattering agent according to any one of [1] to [5], wherein the precious metal-containing thin piece has a precious metal layer on the surface of the thin piece, and the structure has a configuration in which minute columnar bodies having the precious metal layer are arranged in a forest on the surface of the precious metal layer. [7] The surface-enhancing Raman scattering agent according to any one of [1] to [6], wherein the precious metal-containing thin piece has a structure in which minute columnar bodies exhibiting an anisotropic shape are oriented in one direction and stand in a forest on the surface of the thin piece. [8] The surface-enhancing Raman scattering agent according to any one of [1] to [7], wherein the precious metal-containing thin piece is a structure having a configuration in which minute columnar bodies, each having a transparent layer and a precious metal layer composed of a substance other than the precious metal, stand in a forest on the surface of the thin piece. [9] The surface-enhancing Raman scattering agent according to any one of [1] to [8], wherein the noble metal-containing thin piece is a structure having a forest of minute columnar bodies on the surface of the thin piece, each having a layer composed of at least one selected from SiO2, Ta2O5, TiO2, and LiF and a noble metal layer.
[10] The surface-enhanced Raman scattering agent according to any one of claims 1 to 3, wherein the thin piece is a thin piece made of an inorganic oxide having a hydroxyl group. The surface-enhanced Raman scattering agent according to any one of claims [1] to [9].
[11] The surface-enhancing Raman scattering agent according to any one of [1] to
[10] , wherein the thin piece is a thin piece of glass, silica, talc, mica, or titanium oxide.
[12] The surface-enhancing Raman scattering agent according to any one of [1] to
[11] , wherein the thin piece is a thin piece with an average thickness of 10 to 50 μm.
[13] The surface-enhancing Raman scattering agent according to any one of [1] to
[12] , wherein the thin piece is a thin piece with an average equivalent circle diameter of 10 to 500 μm as determined by image analysis. A surface-enhanced Raman scattering measurement kit containing a surface-enhanced Raman scattering agent described in any one of [1] to
[13] . A surface-enhanced Raman scattering measurement method that uses a surface-enhanced Raman scattering agent described in any one of [1] to
[13] .
[16] A method for producing a surface-enhancing Raman scattering agent as described in any one of [1] to
[13] , comprising the step of grinding a noble metal-containing thin plate in a viscous liquid having a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10(1 / s). [Industrial applicability]
[0102] Using the surface-enhanced Raman scattering agent disclosed herein, the Raman peak characteristic of equol can be recognized with high sensitivity. Therefore, the surface-enhanced Raman scattering agent is suitable as a surface-enhanced Raman scattering agent for equol quantification.
Claims
1. A viscous liquid with a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10 (1 / s), A small piece containing a noble metal is dispersed in the aforementioned viscous liquid, A surface-enhancing Raman scattering agent comprising a viscous liquid containing a cellulose-based polymer compound.
2. The surface-enhancing Raman scattering agent according to claim 1, wherein the precious metal is gold, silver, or copper.
3. The surface-enhancing Raman scattering agent according to claim 1 or 2, wherein the precious metal-containing thin piece has a forest of minute columnar bodies on its surface, and at least a portion of the minute columnar bodies is a structure formed of a precious metal layer or precious metal particles.
4. The surface-enhancing Raman scattering agent according to any one of claims 1 to 3, wherein the thin piece is a thin piece made of an inorganic oxide having a hydroxyl group.
5. The surface-enhancing Raman scattering agent according to any one of claims 1 to 3, wherein the thin piece is a thin piece of glass, silica, talc, mica, or titanium oxide.
6. The surface-enhancing Raman scattering agent according to any one of claims 1 to 3, wherein the thin piece is a thin piece of silica, talc, mica, or titanium oxide.
7. A surface-enhanced Raman scattering measurement kit comprising a surface-enhanced Raman scattering agent according to any one of claims 1 to 6.
8. A method for measuring surface-enhanced Raman scattering, comprising: performing surface-enhanced Raman scattering using a surface-enhanced Raman scattering agent described in any one of claims 1 to 6; using a specimen in contact with the surface-enhanced Raman scattering agent as a test specimen; identifying and quantifying a substance contained in the test specimen by analyzing the scattered light produced when the test specimen is irradiated with excitation light.
9. A method for producing a surface-enhancing Raman scattering agent according to any one of claims 1 to 6, A method for producing a surface-enhancing Raman scattering agent, comprising the step of grinding a thin sheet containing a precious metal in a viscous liquid having a viscosity of 50 mPa·s or more at 25°C and a shear rate of 10 (1 / s).
Citation Information
Patent Citations
Preparation and detection method of microchip-based surface Raman-enhanced substrate
CN109030455A
Nano-silver loaded POSS polymer composite material as well as preparation method and application thereof
CN111269577A
Raman scattering measuring sensor, and its manufacturing method
JP2004170334A
Ink composition and oxygen indicator
JP2009504806A