Method and apparatus for manufacturing press-formed products
By controlling mold surface roughness and applying P3HA resin press-molding techniques, the method addresses air bubble formation and release issues, enhancing the production of biodegradable plastics with improved demolding and environmental sustainability.
Patent Information
- Application Number
- JP2023021832
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-02-15
AI Technical Summary
Press-molding poly(3-hydroxyalkanoate) resin (P3HA-based) resins using metal or metal alloy molds results in air bubble formation causing cloudiness and poor release properties, leading to deformation during demolding.
The method involves heating a P3HA resin composition to form a molten resin, supplying it between molds with specific surface roughness (Ra 0.1 μm to 1.0 μm and Rz 0.5 μm to 10.0 μm) and cooling it to prevent bubble formation and enhance release properties.
Suppresses air bubble generation and improves mold releaseability, contributing to sustainable production by reducing marine pollution through biodegradable materials.
Smart Images

Figure 0007948860000002 
Figure 0007948860000003 
Figure 0007948860000001
Abstract
Description
Technical Field
[0001] The present invention relates to a method and an apparatus for producing a press-molded body of a poly(3-hydroxyalkanoate) resin (hereinafter sometimes referred to as "P3HA-based resin").
Background Art
[0002] In recent years, the use of biodegradable plastics is expected to address marine pollution caused by plastics. However, in a report compiled by the United Nations Environment Programme in 2015, it was pointed out that compost-biodegradable plastics such as polylactic acid cannot be expected to degrade in a short period of time in actual low-temperature marine environments, and thus cannot serve as a countermeasure against marine pollution.
[0003] Under such circumstances, P3HA-based resins are materials that can undergo biodegradation even in seawater, and thus have attracted attention as materials that can solve the above-mentioned problems.
[0004] There is also known a technique in which a thermoplastic biodegradable resin is heated to form a molten resin, the molten resin is supplied between molds, the molds are closed to perform press molding, and the resulting product is cooled to obtain a molded article.
[0005] Patent Document 1 discloses, for example, thermoplastic resin molded members such as molds and injection members. The thermoplastic resin molded member of Patent Document 1 has a thermoplastic resin flow path portion through which a melt of the thermoplastic resin flows, and at least the surface of the thermoplastic resin flow path portion exhibits an arithmetic average roughness Ra in the range of 0.1 μm to 0.5 μm, and a maximum height Rz in the range of 0.5 μm to 5.5 μm. The technical subject of Patent Document 1 is not press molding but injection molding. Further, the thermoplastic resin used is not a P3HA-based resin. Furthermore, of the portions through which the melt of the thermoplastic resin flows in the molding apparatus, the thermoplastic resin flow path portion is a portion excluding the cavity.
Prior Art Documents
Patent Documents
[0006] [Patent Document 1] Japanese Patent Publication No. 2022-053734 [Overview of the project] [Problems that the invention aims to solve]
[0007] It was found that when a resin composition containing poly(3-hydroxyalkanoate) resin is heated to form a molten resin composition and then subjected to the above-mentioned press molding, the following problems occur.
[0008] In other words, it was found that when press-formed using a mold made of metal or a metal alloy, air bubbles form on the side surface of the resulting press-formed body, causing it to become cloudy.
[0009] Furthermore, press-formed articles obtained using metal or metal alloy molds adhere tightly to the mold due to very strong force, making them difficult to remove from the mold (poor release properties). Therefore, there was a problem in that the press-formed articles deformed during demolding.
[0010] One aspect of the present invention aims to provide a method and apparatus for manufacturing press-molded articles made of P3HA resin that can suppress the generation of air bubbles and have excellent release properties. [Means for solving the problem]
[0011] To solve the above problems, a method for manufacturing a press-molded article according to one aspect of the present invention comprises a heating step of heating a resin composition containing a poly(3-hydroxyalkanoate) resin to form a molten resin composition, a resin supply step of supplying the molten resin composition between a pair of molds by discharging it from a discharge unit, and a molding step of closing the pair of molds to press-mold the flowable molten resin composition and cool it, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm.
[0012] Furthermore, in order to solve the above problems, a press molded article manufacturing apparatus according to one aspect of the present invention is a press molded article manufacturing apparatus equipped with a pair of molds for filling with a molten resin composition containing a poly(3-hydroxyalkanoate) resin, comprising: a molten resin generation unit that heats the poly(3-hydroxyalkanoate) resin composition to generate a molten resin composition; a supply unit having a discharge unit that discharges the molten resin composition and supplies the molten resin composition between the pair of molds by the discharge unit; and a molding unit that closes the pair of molds to press mold the flowable molten resin composition and cool it, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm. [Effects of the Invention]
[0013] According to one aspect of the present invention, the generation of air bubbles in press-molded articles of P3HA-based resin can be suppressed, and the article exhibits excellent release properties. [Brief explanation of the drawing]
[0014] [Figure 1] This figure schematically shows the general configuration of a press-formed article manufacturing apparatus according to an embodiment of the present invention. [Figure 2] This figure schematically shows the general configuration of the molding section of a press-formed article manufacturing apparatus according to an embodiment of the present invention. [Modes for carrying out the invention]
[0015] One embodiment of the present invention will be described in detail below. Unless otherwise specified in this specification, "A to B" representing a numerical range means "greater than or equal to A and less than or equal to B". Furthermore, all references cited in this specification are incorporated herein by reference.
[0016] [Technical philosophy] The present inventors, when performing press molding using a P3HA-based resin as a biodegradable resin, adopted Method B, in which a molten resin obtained by heating the P3HA-based resin is press-molded in a flowable molten state within a mold, instead of Method A, in which a flat plate made of the P3HA-based resin is press-molded with a mold.
[0017] In the course of advancing research on the production of press-molded articles by the above Method B, the present inventors found that there is a new problem that when press molding is performed using a mold made of metal or metal alloy, a phenomenon of clouding occurs mainly at the side surface portion of the press-molded article. It was also found that this clouding phenomenon is particularly likely to occur in the relatively thin thin-walled portion (film thickness 0.2 mm to 0.3 mm) of the side surface portion of the press-molded article. Furthermore, it was found that the clouded portion appears cloudy due to the accumulation of fine air bubbles.
[0018] Note that such a problem does not occur in the method of press molding by heating and softening a flat plate (the above Method A). Further, when a polyethylene resin commonly used in press molding was press-molded using a mold made of metal or metal alloy, the above clouding phenomenon did not occur. Therefore, it can be said that the above problem is a unique problem that occurs when a molten resin composition of a P3HA-based resin is press-molded in a flowable molten state within a mold.
[0019] Furthermore, when press molding is performed using a P3HA-based resin, as described above, there is also a problem that the press-molded article is difficult to release from the mold (poor mold releasability).
[0020] Accordingly, as a result of intensive studies to solve the above problems, the present inventors have found that by subjecting the molding surface of a mold to surface unevenness treatment to set the arithmetic mean surface roughness Ra and the maximum height Rz within respective specific ranges, the generation of air bubbles in the press-molded article of P3HA-based resin can be suppressed, and a press-molded article having excellent mold releasability can be obtained.
[0021] A method for producing a press-molded article according to one embodiment of the present invention (hereinafter sometimes referred to as the present production method) is obtained based on the above findings, and comprises: a heating step of heating a resin composition containing a poly(3-hydroxyalkanoate)-based resin to form a molten resin composition; a resin supplying step of supplying the molten resin composition between a pair of molds by discharging the molten resin composition from a discharge unit; and a molding step of closing the pair of molds to press-mold the flowable molten resin composition and cooling the same, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm, and a maximum height Rz in the range of 0.5 μm to 10.0 μm.
[0022] According to the present production method, generation of bubbles can be suppressed, and a press-molded article having excellent mold releasability can be obtained.
[0023] Furthermore, according to the present production method, marine pollution due to disposal can be suppressed, thereby contributing to the achievement of Sustainable Development Goals (SDGs) such as Goal 12 "Ensure sustainable consumption and production patterns" and Goal 14 "Conserve and sustainably use the oceans and marine resources for sustainable development". Hereinafter, the present production method will be described in detail.
[0024] [Method for Producing Press-Molded Article] As described above, the present production method includes a heating step, a resin supplying step, and a press molding step. In the present production method, a press-molded article of a P3HA-based resin is produced through the heating step, the resin supplying step, and the press molding step.
[0025] In the heating step, the resin composition containing the P3HA-based resin is heated to form a molten resin composition. As a method for heating the resin composition, a conventionally known method can be adopted as long as the method can form a molten resin composition containing the P3HA-based resin. Preferably, the heating step includes a melt-kneading step of melt-kneading the resin composition containing the P3HA-based resin.
[0026] The form of the melt-kneading process is not particularly limited, as long as a melt-kneaded resin composition can be obtained. Specific examples of the melt-kneading process include, for example, the following methods (a1) and (a2): (a1) A resin composition containing a P3HA-based resin is prepared by mixing or blending using a mixing device or the like. Then, the resin composition is supplied to a melt-kneading device and melt-kneaded; (a2) A method of supplying raw materials for a resin composition containing P3HA resin to a melt-kneading apparatus, preparing (completing) the resin composition in the melt-kneading apparatus, and melt-kneading the resin composition.
[0027] In method (a1) above, the order in which the raw materials for the resin composition containing the P3HA resin are mixed or blended (dry blended) is not particularly limited. In method (a2) above, the order in which the raw materials for the resin composition containing the P3HA resin are supplied to the melt kneading apparatus is not particularly limited.
[0028] In the method described in (a1) above, the mixing device is not particularly limited and includes ribbon blenders, flash blenders, tumbler mixers, super mixers, and the like.
[0029] In the methods described in (a1) and (a2) above, the melting and kneading apparatus is not particularly limited and includes extruders, kneaders, Banbar mixers, and rolls. Extruders are preferred as the melting and kneading apparatus due to their superior productivity and convenience, and twin-screw extruders are even more preferred.
[0030] In the melt-mixing process, the temperature at which the resin composition is melt-mixed cannot be specified in general terms, as it depends on the physical properties of P3HA (melting point, weight-average molecular weight, etc.) and the type of additives used. Regarding the temperature at which the resin composition is melt-mixed, for example, it is preferable that the temperature of the melt-mixed resin composition discharged from the discharge unit (hereinafter sometimes referred to as the composition temperature) be 140°C to 190°C, more preferably 150°C to 180°C, and even more preferably 160°C to 170°C. If the composition temperature is 150°C or lower, unmelted P3HA resin may be generated. On the other hand, if the composition temperature is 180°C or higher, the P3HA resin may undergo thermal decomposition.
[0031] Furthermore, in the resin supply process described above, the molten resin composition is supplied between the pair of molds by being discharged from the discharge unit. In the resin supply process described above, the molten resin composition is discharged from the discharge unit to the pair of molds while still in a molten state. This supplies the molten resin composition in a molten state between the pair of molds.
[0032] The method for supplying the molten resin composition between the molds is not particularly limited, as long as the molten resin composition discharged from the discharge unit can be supplied between the pair of molds. From the viewpoint of reliably supplying the molten resin composition between the pair of molds, it is preferable to first discharge the molten resin composition from the discharge unit to the lower mold, supply a predetermined amount of the molten resin composition to the lower mold, and then place the upper mold on the lower mold to supply the molten resin composition between the pair of molds.
[0033] Furthermore, in the resin supply process described above, the configuration of the discharge unit is not particularly limited as long as it is capable of discharging the molten resin composition, and conventionally known configurations can be adopted. From the viewpoint of improving the productivity of press-molded products, it is preferable that the discharge unit is capable of quantitatively discharging the molten resin composition. Examples of such discharge unit configurations include configurations equipped with a gear pump and configurations equipped with an automatic opening and closing nozzle. Specific examples of discharge units include plunger-type dischargers, pre-plunger-type dischargers, and screw-type dischargers.
[0034] Furthermore, in the press molding process described above, the pair of molds are closed and the flowable molten resin composition is press-molded and cooled. In the resin supply process described above, the molten resin composition is supplied between the pair of molds while still in a molten state, so even when the pair of molds is closed in the press molding process described above, the molten resin composition can flow through the space between the pair of molds.
[0035] In the resin supply step described above, the molten resin composition is supplied between the pair of molds. Then, in the press molding step described above, the pair of molds are subjected to hot pressing using a hot press molding machine. After the hot pressing is complete, the pair of molds are cooled to perform press molding. After press molding, the pair of molds are opened to obtain a press-molded body.
[0036] The hot press molding machine used in the above resin supply process is not particularly limited, as long as it is configured to hot press the pair of molds to which the molten resin composition is supplied. Conventional known devices can be used as the hot press molding machine.
[0037] Furthermore, it is preferable that the pair of molds be preheated in order to allow the molten resin composition supplied between them to flow. The heating temperature of the pair of molds should be such that it can maintain the composition temperature of the molten resin composition, preferably ±30°C of the composition temperature of the molten resin composition, and more preferably the same temperature as the composition temperature of the molten resin composition.
[0038] Furthermore, the pressing pressure of the pair of dies in the hot press molding machine is not particularly limited, but is preferably 50KN to 300KN, and more preferably 100KN to 200KN. Setting the above pressing pressure within the above numerical range has the advantage of making it easier to obtain a press-molded body with uniform thickness.
[0039] Furthermore, while the pressing time for a pair of molds in a hot press molding machine is not particularly limited, it is preferably 5 to 60 seconds, and more preferably 10 to 30 seconds. Setting the above pressing time within the above numerical range has the advantage of making it easier to obtain a press-molded body with uniform thickness.
[0040] The method for cooling a pair of molds after hot pressing is not particularly limited. For example, one method involves clamping the pair of molds after hot pressing with a pair of cooling plates and then performing a cooling press.
[0041] In this method, the press pressure during cooling press is not particularly limited, but is preferably 10KN to 100KN, and more preferably 30KN to 50KN. Setting the press pressure within the above numerical range has the advantage of producing a press-molded body with uniform thickness.
[0042] Furthermore, while there are no particular limitations on the pressing time during cooling press, it is preferably 60 to 600 seconds, and more preferably 120 to 300 seconds. Setting the above pressing time within the above numerical range has the advantage that the P3HA resin solidifies sufficiently, making it easier to remove the press-molded product.
[0043] Furthermore, while the temperature of the cooling plate used in the cooling press is not particularly limited, it is preferably between 10°C and 60°C, and more preferably between 20°C and 50°C. Setting the temperature of the cooling plate within the above numerical range has the advantage that the solidification of the P3HA resin proceeds sufficiently, making it easier to remove the press-molded product.
[0044] Herein, the present manufacturing method is characterized in that the molded surface of the mold has an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm. The arithmetic mean roughness Ra of the molded surface of the mold is preferably 0.2 μm to 0.9 μm, and more preferably 0.3 μm to 0.8 μm. The maximum height Rz of the molded surface of the mold is preferably 1.0 μm to 8.0 μm, and more preferably 2.0 μm to 6.0 μm. The arithmetic mean roughness Ra and the maximum height Rz can be measured according to conventionally known methods, for example, JIS B 0601-2001.
[0045] As long as the arithmetic mean roughness Ra and maximum height Rz of the molded surface of the above-mentioned mold are within the above range, the press-molded articles produced by this manufacturing method will not exhibit the clouding phenomenon caused by the fine bubbles mentioned above, and will have excellent release properties. Here, "molded surface" refers to the surface of the pair of molds that comes into contact with the molten resin composition, and can also be said to be the opposing surfaces of the pair of molds facing each other.
[0046] The above-mentioned molding surface exists in each of the pair of molds. In this manufacturing method, the molding surface exhibiting the arithmetic mean roughness Ra and the maximum height Rz within the above range may be the molding surface of at least one of the pair of molds, preferably both molding surfaces of the pair of molds. The molding surface exhibiting the arithmetic mean roughness Ra and the maximum height Rz within the above range may also be the molding surface of a concave mold (cavity).
[0047] Furthermore, the region on the molded surface that exhibits an arithmetic mean roughness Ra within the above range and a maximum height Rz within the above range is not particularly limited, as long as it includes the region of the molded surface corresponding to the area where the above-mentioned clouding phenomenon may occur in the press-molded body and the region of the molded surface that affects demolding.
[0048] For example, when a press-formed body has a concave shape with a recess or a cylindrical shape with no bottom hole, generally, in a pair of molds, the forming surface corresponding to the side wall of the press-formed body is a surface that rises with respect to the horizontal plane. In other words, in press forming, the side wall of a press-formed body is generally the portion that rises from the horizontal plane in the direction of pressing. The above-mentioned clouding phenomenon occurs particularly in the thin-walled portion of the side wall of the press-formed body. Furthermore, the side wall portion of a press-formed body has particularly poor release properties. The smaller the inclination angle of the side wall of the press-formed body with respect to the horizontal plane, the worse the release properties tend to be. Therefore, in the above-mentioned forming surface, the region showing the arithmetic mean roughness Ra and the maximum height Rz within the above range preferably includes at least the region corresponding to the thin-walled portion of the side wall of the press-formed body and the region corresponding to the side wall portion of the press-formed body, and more preferably the entire forming surface.
[0049] Furthermore, while there are no particular limitations on the press-molded articles suitable for this manufacturing method, they are articles in which the thickness of the rising portion (e.g., the side wall portion of the press-molded article) that rises in the direction of pressing is 0.1 mm to 0.4 mm, preferably 0.2 mm to 0.3 mm. By having the thickness of the rising portion within the above numerical range, the occurrence of the clouding phenomenon can be significantly suppressed.
[0050] Furthermore, by roughening the molded surface, a molded surface exhibiting an arithmetic mean roughness Ra and a maximum height Rz within the above range can be formed. This roughening treatment can be carried out using conventionally known methods, but preferably, it is at least one surface treatment selected from shot peening and blasting.
[0051] Shot peening is a surface treatment that creates irregularities on the molding surfaces of a pair of molds by projecting and impacting them with spherical particles using air pressure. Shot peening evens out the surface roughness of the molding surfaces and imparts compressive residual stress. In shot peening, various conditions such as the material and diameter of the spherical particles, the projection angle and speed (i.e., air pressure) of the spherical particles, and the processing time are not particularly limited, as long as the molding surfaces exhibit an arithmetic mean roughness Ra and a maximum height Rz within the specified range, and can be appropriately set according to the set values of the arithmetic mean roughness Ra and the maximum height Rz within the specified range.
[0052] Blasting is a surface treatment that forms irregularities on the molding surfaces of a pair of molds by projecting and impacting them with, for example, polygonal particles using air pressure. In this manufacturing method, blasting is similar to the shot peening treatment described above in that it forms irregularities on the molding surface, but it differs from the shot peening treatment in that it does not impart compressive residual stress to the molding surface. In blasting, various conditions such as the material and diameter of the polygonal particles, the projection angle and speed (i.e., air pressure) of the spherical particles, and the processing time are not particularly limited, as long as the molding surface exhibits an arithmetic mean roughness Ra and a maximum height Rz within the above range, and can be appropriately set according to the set values of the arithmetic mean roughness Ra and the maximum height Rz within the range.
[0053] Furthermore, in this manufacturing method, it is preferable that the molding surface of the mold is surface-treated with a fluororesin. Specifically, it is preferable that the molding surface of the mold is subjected to both a surface roughening treatment (hereinafter sometimes simply referred to as surface roughening treatment) and a surface treatment with a fluororesin (hereinafter sometimes referred to as fluorosurface treatment) so that it exhibits an arithmetic mean roughness Ra and a maximum height Rz within the above range relative to the molding surface. Due to the fluorosurface treatment of the molding surface, the press-molded articles manufactured by this manufacturing method will not exhibit the whitening phenomenon caused by the fine bubbles described above. The molding surface of the mold may be (1) a surface that has been surface-treated with fluorosurface treatment before the surface roughening treatment, or (2) a surface that has been surface-treated with fluorosurface treatment after the surface roughening treatment. In the case of (1), partial peeling of the fluorosurface treatment layer may occur due to the surface roughening treatment, and in the case of (2), the adhesion of the fluorosurface treatment layer is improved when the surface roughening treatment is performed before the fluorosurface treatment, so (2) is more preferable.
[0054] In this manufacturing method, the fluorine surface treatment only needs to be applied to the molding surface of at least one of the pair of molds, and preferably, it is applied to both of the pair of molds.
[0055] Furthermore, the area on the molded surface to which the fluorine surface treatment is applied is not particularly limited, as long as it is an area of the molded surface corresponding to the area in the press-molded body where the above-mentioned clouding phenomenon may occur. For example, when the press-molded body has a concave shape with recesses or a cylindrical shape with no bottom hole, generally, in a pair of molds, the molded surface corresponding to the side wall of the press-molded body is a surface that rises from the horizontal plane. In other words, in press molding, the side wall of the press-molded body is generally the part that rises from the horizontal plane in the direction of pressing. The above-mentioned clouding phenomenon occurs particularly in the thin-walled portion of the side wall of the press-molded body. Therefore, it is preferable that the area on the molded surface to which the fluorine surface treatment is applied includes at least the area corresponding to the thin-walled portion of the side wall of the press-molded body, and more preferably the entire molded surface.
[0056] Furthermore, the fluorine-based resin used in the above-mentioned fluorine surface treatment is not particularly limited, but examples include perfluoroalkoxyalkanes (PFA), ethylene-tetrafluoroethylene copolymers (ETFE), and polytetrafluoroethylene (PTFE).
[0057] Furthermore, the above-mentioned fluorine surface treatment may be used in combination with a metal surface coating treatment. That is, the coating formed by the above surface treatment may be a composite film of a metal coating and a fluorine-based resin coating. The metal constituting the above-mentioned metal coating is not particularly limited, but examples include nickel-based metals, chromium-based metals, iron-based metals, alumina-based metals, etc.
[0058] [Manufacturing equipment for press-formed products] A press-formed article manufacturing apparatus (hereinafter sometimes referred to as "this manufacturing apparatus") according to one embodiment of the present invention is configured to realize this manufacturing method. Figure 1 is a schematic diagram showing the general configuration of this manufacturing apparatus. Figure 2 is a schematic diagram showing the general configuration of the molding section of this manufacturing apparatus.
[0059] As shown in Figure 1, a press-molded article manufacturing apparatus 10 according to one embodiment of the present invention includes a pair of molds for filling with a molten resin composition containing a P3HA-based resin. In Figure 1, the lower mold of the pair of molds is shown. The manufacturing apparatus 10 includes a molten resin generation unit 1 and a supply unit 2.
[0060] The molten resin production unit 1 generates a molten resin composition by heating a P3HA-based resin composition. The molten resin production unit 1 is equipped with a raw material input unit for inputting the raw materials of the P3HA-based resin composition. The molten resin production unit 1 is equipped with a molten kneading device for molten and kneading the raw materials input from the raw material input unit. The molten resin production unit 1 may also be equipped with a mixing device for mixing the raw materials as needed. The molten kneading device and mixing device can be exemplified by the equipment described above.
[0061] The supply unit 2 has a discharge unit 2a that discharges the molten resin composition produced in the molten resin generation unit 1. The discharge unit 2a can be exemplified by the configuration of the discharge unit described above. The supply unit 2 supplies the molten resin composition between the pair of molds by the discharge unit 2a. In the configuration shown in Figure 1, the supply unit 2 is configured to discharge the molten resin composition from the discharge unit 2a to the lower mold. After a predetermined amount of molten resin composition is supplied to the lower mold, the upper mold is placed on the lower mold, thereby supplying the molten resin composition between the pair of molds.
[0062] Furthermore, as shown in Figure 2, the manufacturing apparatus 10 includes a molding section 30. The molding section 30 closes a pair of molds 31 and press-moldes and cools the flowable molten resin composition. The molding section 30 includes a hot press molding machine that heat-presses the pair of molds 31, and a cooling device that cools the pair of molds 31 after the heat-pressing is complete. The hot press machine and the cooling device can be any device used in press molding. For example, the cooling device may include a pair of cooling plates that sandwich the pair of molds 31, and the cooling plates may be used to cool and press the pair of molds 31.
[0063] The mold 31 shown in Figure 2 is a mold for forming a press-formed body that has a concave shape with a recess. The pair of molds 31 comprises a lower mold 32 and an upper mold 33.
[0064] In the manufacturing apparatus 10, the molding surfaces 32A and / or 33A of the pair of molds 31 have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm. Because the arithmetic mean roughness Ra and maximum height Rz of the molding surfaces of the molds 31 are within the above range, the press-molded articles produced by the manufacturing apparatus 10 are free from the whitening phenomenon caused by the fine air bubbles mentioned above and have excellent release properties.
[0065] Here, the molding surfaces 32A and 33A can be said to be the surfaces that constitute the molding space formed by the lower mold 32 and the upper mold 33.
[0066] Furthermore, in this manufacturing apparatus, it is preferable that the molding surfaces 32A and / or 33A of the pair of molds 31 are surface-treated with a fluororesin. The surface treatment with a fluororesin only needs to be applied to the molding surface of at least one of the molds, namely the molding surface 32A of the lower mold 32 and the molding surface 33A of the upper mold 33, and preferably to both the lower mold 32 and the upper mold 33.
[0067] Furthermore, the molding surface of the lower mold 32 has rising surfaces 32b and 32c, and the molding surface of the upper mold 33 has rising surfaces 33b and 33c. Rising surfaces 32b and 33b and rising surfaces 32c and 33c are molding surfaces that constitute the thin-walled portion of the rising part that rises in the pressing direction in the press-formed body. In the molding surfaces 32A and 33A of the pair of molds 31, the area to which the above surface treatment is applied is preferably an area that includes at least one of the rising surfaces 32b and 32c and the rising surfaces 33b and 33c, and more preferably the entire area of the molding surface 32A and / or 33A.
[0068] Furthermore, in the pair of molds 31, the distance between the rising surface 32b and the rising surface 33b, and the distance between the rising surface 32c and the rising surface 33c, define the thickness of the thin-walled portion of the rising part of the press-formed body. In the pair of molds 31, the distance between these rising surfaces is defined so that the thickness of the rising part of the press-formed body is 0.1 mm to 0.4 mm, preferably 0.2 mm to 0.3 mm.
[0069] Furthermore, in the molding surfaces 32A and 33A of the pair of molds 31 shown in Figure 2, the areas where the release properties of the press-formed body are poor are the side surfaces. Therefore, in the molding surfaces 32A and / or 33A, the areas showing the arithmetic mean roughness Ra within the above range and the maximum height Rz within the above range preferably include at least one of the rising surfaces 32b, 32c, 33b, and 33c, and at least the areas where the release properties of the press-formed body are poor (side surfaces), and more preferably the entire area of the molding surfaces 32A and / or 33A.
[0070] (P3HA resin) The resin composition used in this manufacturing method includes a P3HA-based resin. In this specification, "P3HA-based resin" refers to a 3-hydroxyalkanoic acid repeating unit represented by the general formula: [-CHR-CH2-CO-O-] (wherein R is C n H 2n+1 It is a polyhydroxyalkanoate containing an alkyl group represented by , where n is an integer between 1 and 15 (inclusive), as a repeating unit.
[0071] More specifically, P3HA resins preferably contain 3-hydroxybutyrate (3HB) units. Examples of P3HA resins containing 3HB units include poly(3-hydroxybutyrate) (P3HB), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (P3HB3HV), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (P3HB3HV3HH), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4HB), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), and poly(3-hydroxybutyrate-co-3-hydroxydecanoate).
[0072] The P3HA-based resin may contain only one type, or it may contain two or more types.
[0073] As for P3HA resins, P3HA resins produced by microorganisms (microbially produced P3HA resins) are preferred. Microbially produced P3HA resins are usually composed only of D-isomers (R-isomers) of polyhydroxyalkanoate monomer units. Among microbially produced P3HA resins, P3HB, P3HB3HH, P3HB3HV, P3HB3HV3HH, and P3HB4HB are preferred due to their ease of industrial production, and P3HB, P3HB3HH, P3HB3HV, and P3HB4HB are more preferred.
[0074] The microorganisms that produce microbially produced P3HA resins are not particularly limited as long as they are microorganisms capable of producing P3HA resins. For example, the first P3HB-producing bacterium was Bacillus megaterium, discovered in 1925, and other examples include natural microorganisms such as Cupriavidus necator (formerly classified as Alcaligenes eutrophus, Ralstonia eutropha) and Alcaligenes latus. It is known that P3HB accumulates within the cells of these microorganisms.
[0075] Furthermore, known microorganisms that produce copolymers of hydroxybutyrate and other hydroxyalkanoates include Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB. In particular, with respect to P3HB3HH, Alcaligenes eutrophus AC32 strain (FERM BP-6038) (T.Fukui, Y.Doi, J.Bateriol., 179, p4821-4830 (1997)), into which genes of the P3HA resin synthase group have been introduced, are more preferred in order to increase the productivity of P3HB3HH. Microbial cells that have accumulated P3HB3HH in their cells by culturing these microorganisms under appropriate conditions are used. In addition to the above, genetically modified microorganisms into which various P3HA resin synthesis-related genes can be introduced can be used, depending on the P3HA resin to be produced, or the culture conditions, including the type of substrate, can be optimized.
[0076] Furthermore, the P3HA resin contains at least one copolymer of 3HB units and other hydroxyalkanoate units, and the 3-hydroxybutyrate units in the poly(3-hydroxyalkanoate) resin are preferably 90.0 to 99.0 mol%, more preferably 91.0 to 98.5 mol%, more preferably 92.0 to 98.5 mol%, and even more preferably 93.0 to 98.0 mol%, of the total repeating units (100 mol%).
[0077] When the composition ratio of 3HB repeating units is 90.0 mol% or higher, the rigidity of the P3HA resin is further improved, the crystallization rate is increased, burrs are reduced, and productivity tends to improve. On the other hand, when the composition ratio of 3HB repeating units is 99.0 mol% or lower, the melting point is below the thermal decomposition temperature, enabling stable and continuous production. The monomer composition ratio of P3HA resin can be measured by gas chromatography, etc. (see, for example, International Publication No. 2014 / 020838).
[0078] The molecular weight of the P3HA resin is not particularly limited, as long as it exhibits substantially sufficient physical properties for the intended application. The weight-average molecular weight range of the P3HA resin is preferably 100,000 to 1,000,000, more preferably 150,000 to 700,000, even more preferably 200,000 to 500,000, and particularly preferably 250,000 to 450,000. A weight-average molecular weight of 100,000 or more provides adequate mechanical strength. Furthermore, a molecular weight of 1,000,000 or less suppresses the increase in melt viscosity and provides excellent moldability.
[0079] The weight-average molecular weight can be determined using gel permeation chromatography (GPC) (Shodex GPC-101, Showa Denko Corporation), with a polystyrene gel column (Shodex K-804, Showa Denko Corporation) and chloroform as the mobile phase, expressed as the molecular weight in polystyrene equivalent. Calibration curves are created using polystyrene with weight-average molecular weights of 31,400, 197,000, 668,000, and 1,920,000. Any column suitable for measuring the aforementioned molecular weights can be used in the GPC.
[0080] The resin composition in this manufacturing method may contain a second P3HA-based resin in addition to the P3HA-based resin. The second P3HA-based resin contains at least one copolymer of 3HB units and other hydroxyalkanoate units, and the 3HB units in the poly(3-hydroxyalkanoate)-based resin are preferably 65.0 to 90.0 mol%, more preferably 68.0 to 88.0 mol%, and even more preferably 70.0 to 85.0 mol% of the total repeating units (100 mol%). The inclusion of the second P3HA-based resin in the resin composition results in superior toughness of the molded article.
[0081] The second P3HA-based resin is not particularly limited, as long as it is different from the aforementioned P3HA-based resin. Examples of the second P3HA-based resin include the resins exemplified above as the aforementioned P3HA-based resin.
[0082] The content of the second P3HA resin is not particularly limited, but is preferably 50 parts by weight or less, more preferably 45 parts by weight or less, and even more preferably 40 parts by weight or less, per 100 parts by weight of the total P3HA resin. The lower limit of the content of the second P3HA resin is not particularly limited and may be 0 parts by weight. The P3HA resin described above can be used as the second P3HA resin. In this specification, "total P3HA resin" refers to all P3HA resin contained in the resin composition in this manufacturing method.
[0083] The resin composition may contain other resins besides P3HA resins, as long as they do not impair the effects of the present invention. Examples of such other resins include aliphatic polyester resins such as polybutylene succinate adipate, polybutylene succinate, polycaprolactone, and polylactic acid, and aliphatic aromatic polyester resins such as polybutylene adipate terephthalate, polybutylene sebatate terephthalate, and polybutylene azelate terephthalate. The other resin may consist of only one type or two or more types.
[0084] The content of the other resins is not particularly limited, but is preferably 50 parts by weight or less, more preferably 40 parts by weight or less, per 100 parts by weight of the total P3HA resin. Even more preferably 30 parts by weight or less. The lower limit of the content of the other resins is not particularly limited and may be 0 parts by weight.
[0085] The resin composition does not necessarily have to contain an inorganic filler, but it is preferable that it further contains an inorganic filler. The inclusion of an inorganic filler in the resin composition improves the crystallization rate, resulting in effects such as reduced burrs and improved production cycles.
[0086] The inorganic filler is not particularly limited, but examples include talc, diatomaceous earth, white clay, clay, calcium carbonate, manganese carbonate, magnesium carbonate, barium sulfate, mica, silica, alumina, zircon, iron oxide, zinc oxide, titanium oxide, silicon nitride, boron nitride, aluminum nitride, silicon carbide, graphite, carbon black, ferrite, graphite, quartz, glass fiber, and glass particles. These may be used individually or in combination of two or more types.
[0087] The inorganic filler content is, for example, 0 to 60 parts by weight, preferably 5 to 50 parts by weight, more preferably 10 to 40 parts by weight, and particularly preferably 15 to 35 parts by weight, based on 100 parts by weight of the total P3HA resin. When the inorganic filler content is within the above range, it is possible to achieve both a sufficient crystallization rate and toughness.
[0088] Furthermore, the resin composition may contain additives that can be used together with the P3HA resin, to the extent that they do not impair the effects of the present invention. Examples of such additives include colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolites, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather-resistant modifiers, ultraviolet absorbers, crystal nucleating agents, lubricants, mold release agents, water repellents, antibacterial agents, and sliding properties modifiers. Only one type of additive may be included, or two or more types may be included. The content of these additives can be appropriately determined by those skilled in the art depending on the intended use.
[0089] The present invention is not limited to the embodiments described above, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0090] In other words, one embodiment of the present invention is as follows: <1> A heating step involves heating a resin composition containing a poly(3-hydroxyalkanoate) resin to form a molten resin composition, A resin supply step of supplying the molten resin composition between a pair of molds by discharging it from a discharge section, A molding step comprising closing the pair of molds, press-molding the flowable molten resin composition, and cooling it, A method for manufacturing a press-formed article, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm. <2> The molding surfaces of the pair of molds are subjected to at least one surface treatment selected from shot peening and blasting. <1> A method for manufacturing a press-molded body. <3> The molding surfaces of the pair of molds are treated with a fluororesin surface treatment. <1> or <2> A method for manufacturing a press-molded body. <4> The aforementioned press-formed body has a thickness of 0.1 mm to 0.4 mm in the rising portion that rises in the pressing direction. <1> ~ <3> A method for manufacturing a press-molded body. <5> The aforementioned poly(3-hydroxyalkanoate) resin is one or more selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), and poly(3-hydroxybutyrate-co-3-hydroxydecanoate). <1> ~ <4> A method for manufacturing a press-molded body. <6> A press-molded body manufacturing apparatus comprising a pair of molds for filling with a molten resin composition containing a poly(3-hydroxyalkanoate) resin, A molten resin production unit that heats a poly(3-hydroxyalkanoate) resin composition to produce a molten resin composition, A supply unit having a discharge unit for dispensing the molten resin composition, and supplying the molten resin composition between the pair of molds by the discharge unit, The system includes a molding section that closes the pair of molds, press-moldes the flowable molten resin composition, and cools it, A press-formed body manufacturing apparatus, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm. [Examples]
[0091] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0092] (Example 1) Using a tabletop plunger-type melting and dispensing machine (manufactured by Nakatsuji Mold Industry Co., Ltd.), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (sometimes referred to as P3HB3HH) (weight-average molecular weight Mw 400,000, 3HH ratio 6 mol%) was heated to 160°C to produce a molten resin. The molten P3HB3HH resin was then dispensed into a lower mold that had been preheated to 150°C, supplying the molten P3HB3HH resin to the lower mold. Next, the lower mold containing the P3HB3HH resin was closed by an upper mold, also heated to 150°C, thereby supplying the molten resin between the pair of molds. The pair of molds containing the P3HB3HH resin were then subjected to hot pressing using a hot press molding device (Mikado Technos Co., Ltd., VS38-2525) at a press pressure of 125 KN for a pressing time of 20 seconds. The pair of molds, which had just been heat-pressed, were immediately sandwiched between upper and lower cooling plates heated to 25°C, and press molding was performed by cooling press at a press pressure of 30KN for 300 seconds. After press molding, the molds were opened and the molded product was removed.
[0093] A pair of molds 31, as shown in Figure 2, were used. The upper and lower molds were made of aluminum alloy (A7075). The pair of molds used had blast treatment applied to the entire molding surface of both the upper and lower molds.
[0094] For the molding surfaces of both the upper and lower molds described above, the arithmetic mean roughness Ra and maximum height Rz were measured over multiple intervals in accordance with JIS B 0601-2001. As a result, the arithmetic mean roughness Ra was 0.40 μm and the maximum height Rz was 2.91 μm.
[0095] (Example 2) Press molding was performed in the same manner as in Example 1, except that a pair of molds were used in which the arithmetic mean roughness Ra and maximum height Rz measured over multiple sections of both the upper and lower mold surfaces were 0.76 μm and 5.09 μm, respectively.
[0096] (Example 3) The molds used had blast treatment applied to the entire molding surface of both the upper and lower molds, followed by a 5 μm layer of nickel-PTFE composite plating (PTFE content 30 wt%), which is a fluorine surface treatment. Press forming was performed in the same manner as in Example 1, except that a pair of molds were used in which the arithmetic mean roughness Ra and maximum height Rz measured over multiple sections of both the upper and lower molds were 0.44 μm and 3.18 μm, respectively.
[0097] (Comparative Example 1) Press molding was performed in the same manner as in Example 1, except that a pair of molds were used in which the arithmetic mean roughness Ra and maximum height Rz measured over multiple sections of both the upper and lower mold surfaces were 1.97 μm and 12.66 μm, respectively.
[0098] (Evaluation method) <Bubble generation evaluation> The press-molded bodies of Examples 1, 2, and 3, and Comparative Example 1 were visually inspected to determine whether or not air bubbles were present, and evaluated as follows. ○: No air bubbles, ×: There are air bubbles.
[0099] <Evaluation of mold opening force (evaluation of mold release properties)> For the release properties of the press-formed articles in Examples 1, 2, and 3, and Comparative Example 1, the maximum force required to separate the upper and lower molds after press forming (mold opening force) was measured using a crane scale. The release properties were then evaluated based on the relative values of the mold opening forces in Examples 1, 2, and 3, with the mold opening force of Comparative Example 1 set to 100.
[0100] The evaluation results are shown in Table 1.
[0101] [Table 1]
[0102] Regarding the evaluation results for bubble formation, as is clear from the results shown in Table 1, the press-molded article of Comparative Example 1 had bubbles and a problem with its appearance. On the other hand, the press-molded articles of Examples 1, 2, and 3 did not show any bubbles and had a good appearance.
[0103] Regarding the evaluation results of the die opening force, as is clear from the results shown in Table 1, the die opening force of the press-formed article of Comparative Example 1 was 127 kgf (relative value 100). In contrast, the die opening force of the press-formed article of Example 1 was 6 kgf (relative value 4.7), the die opening force of the press-formed article of Example 2 was 10 kgf (relative value 7.9), and the die opening force of the press-formed article of Example 3 was 2 kgf (relative value).
[0104] In the method of Comparative Example 1, the mold opening force is large and the release properties are poor, so the press-molded article is prone to deformation during demolding. Therefore, it is difficult to stably manufacture press-molded articles using the method of Comparative Example 1.
[0105] In contrast, the methods of Examples 1, 2, and 3 involve a small mold opening force and excellent release properties, resulting in press-molded articles that are less prone to deformation during demolding. Therefore, the methods of Examples 1, 2, and 3 enable the stable production of press-molded articles. [Industrial applicability]
[0106] This invention can be suitably used in the field of manufacturing press-molded articles using P3HA resin, and in other fields. [Explanation of symbols]
[0107] 1. Molten resin generation section 2 Supply section 2a Discharge part 30 Molding section 31 pairs of molds 32 Lower mold 32A Molding surface 33 Upper mold 33A Molding surface 10. Manufacturing equipment (machinery for manufacturing press-formed products)
Claims
1. A heating step involves heating a resin composition containing a poly(3-hydroxyalkanoate) resin to form a molten resin composition, A resin supply step of supplying the molten resin composition between a pair of molds by discharging it from a discharge section, A molding step comprising closing the pair of molds, press-molding the flowable molten resin composition, and cooling it, A method for manufacturing a press-formed article, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm.
2. The method for manufacturing a press-formed article according to claim 1, wherein the molding surfaces of the pair of molds are subjected to at least one surface treatment selected from shot peening and blasting.
3. A method for manufacturing a press-molded article according to claim 1 or 2, wherein the molding surfaces of the pair of molds are subjected to a surface treatment with a fluororesin.
4. The method for manufacturing a press-formed article according to claim 1 or 2, wherein the press-formed article has a thickness of 0.1 mm to 0.4 mm for the rising portion that rises in the pressing direction.
5. The method for producing a press-molded article according to claim 1 or 2, wherein the poly(3-hydroxyalkanoate) resin is one or more selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), and poly(3-hydroxybutyrate-co-3-hydroxydecanoate).
6. A press-molded body manufacturing apparatus comprising a pair of molds for filling with a molten resin composition containing a poly(3-hydroxyalkanoate) resin, A molten resin generating unit that heats a poly(3-hydroxyalkanoate) resin composition to produce a molten resin composition, A supply unit having a discharge unit for dispensing the molten resin composition, and supplying the molten resin composition between the pair of molds by the discharge unit, The system includes a molding section that closes the pair of molds, press-moldes the flowable molten resin composition, and cools it, A press-formed body manufacturing apparatus, wherein the molding surfaces of the pair of molds have an arithmetic mean roughness Ra in the range of 0.1 μm to 1.0 μm and a maximum height Rz in the range of 0.5 μm to 10.0 μm.
Citation Information
Patent Citations
Environment-friendly molding process for notebook computer shell
CN112571715A
METHOD FOR MOLDING HYDROGENATED alpha-OLEFIN- DICYCLOPENTADIENE COPOLYMER AND MOLDING OBTAINED THEREFROM
JP2000006181A
Manufacturing equipment and manufacturing method for molded body
JP2007076178A
How to print 3D micro-optical images onto packaging systems
JP2020524097A
Thermoplastic resin molded member and its surface processing method, thermoplastic resin molding die and its surface processing method
JP2022053734A