Graphene, electrode, secondary battery, vehicle, and electronic equipment

JPWO2022106950A5Active Publication Date: 2024-11-11SEMICON ENERGY LAB CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022563252
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-17
Filing Date
2021-11-05
Publication Date
2024-11-11
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face challenges in maintaining high cycle characteristics and energy density due to electrode deterioration, particularly at high temperatures and during rapid charging, which affects their performance in electric vehicles and portable devices.

Method used

The use of graphene with multi-membered rings, preferably terminated with fluorine, as an active material in electrodes to enhance conductivity and stability, forming a three-dimensional conductive path that covers active material particles, thereby improving charge/discharge rates and reducing electrode degradation.

Benefits of technology

The graphene-enhanced electrodes result in secondary batteries with increased energy density, improved safety, and the ability to operate effectively across a wide temperature range, supporting high-rate charging and extended cycle life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a novel graphene. Also provided is a novel graphene compound. Also provided is an electrode having a high output. Also provided is a novel electrode. Also provided is a secondary battery with little deterioration. Also provided is a secondary battery having high safety. The graphene has pores formed by multi-membered rings of at least 9-membered rings composed of carbon atoms. In addition, at least one of the carbon atoms constituting the multi-membered ring is terminated by fluorine.
Need to check novelty before this filing date? Find Prior Art

Description

Graphene, electrodes, secondary batteries, vehicles and electronic devices

[0001] The present invention relates to a secondary battery using a negative electrode active material and a manufacturing method thereof, or a secondary battery using a positive electrode active material and a manufacturing method thereof, or a secondary battery using graphene and a manufacturing method thereof, or an electronic device such as a portable information terminal, a vehicle, or the like having a secondary battery.

[0002] One embodiment of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, or a manufacturing method thereof.

[0003] In this specification, the term "electronic device" refers to any device having a power storage device, and includes electro-optical devices having a power storage device, information terminal devices having a power storage device, and the like.

[0004] In this specification, the term "power storage device" refers to all elements and devices having a power storage function, including, for example, power storage devices such as lithium ion secondary batteries (also called secondary batteries), lithium ion capacitors, and electric double layer capacitors.

[0005] In recent years, various types of power storage devices have been actively developed, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries. In particular, demand for high-power, high-energy-density lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they are now indispensable in the modern information society as a rechargeable energy source, as they are used in portable information terminals such as mobile phones, smartphones, and notebook computers, portable music players, digital cameras, medical devices, and next-generation clean-energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs).

[0006] Regarding lithium ion secondary batteries, research has been conducted on the crystal structure of positive electrode active materials (Non-Patent Document 1).

[0007] Furthermore, in order to improve the cycle characteristics and capacity of lithium ion secondary batteries, improvements to the negative electrode having a coating have been investigated (Patent Document 1).

[0008] Fluorine has a high electronegativity, and various studies have been conducted on its reactivity. Non-Patent Document 2 describes reactions of compounds containing fluorine.

[0009] Silicon-based materials have high capacity and are used as active materials in secondary batteries. Silicon materials can be characterized by chemical shift values ​​obtained from NMR spectra (Patent Document 2).

[0010] JP 2015-88482 A JP 2015-156355 A

[0011] Zhaohui Chen et al, “Staging Phase Transitions in LixCoO2”, Journal of The Electrochemical Society, 2002, 149(12) A1604-A1609W. E. Counts et al, “Flouride Model Systems: II, The Binary Systems CaF▲2▼−BeF▲2▼, MgF▲2▼−BeF▲2▼, and LiF-MgF▲2▼, “Journal of the American Ceramic Society, (1953) 36[1] 12-17. Fig. 01471

[0012] An object of one embodiment of the present invention is to provide a novel graphene.An object of one embodiment of the present invention is to provide a novel graphene compound.An object of one embodiment of the present invention is to provide an electrode having high output.An object of one embodiment of the present invention is to provide a novel electrode.

[0013] Another object of one embodiment of the present invention is to provide a novel method for manufacturing graphene, a novel method for manufacturing a graphene compound, or a novel method for manufacturing an electrode.

[0014] Another object of one embodiment of the present invention is to provide a secondary battery that is less susceptible to deterioration, a highly safe secondary battery, or a novel secondary battery.

[0015] Another object of one embodiment of the present invention is to provide a novel substance, active material particles, a secondary battery, a power storage device, or a manufacturing method thereof.

[0016] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description of the specification, drawings, and claims.

[0017] One embodiment of the present invention is graphene having holes formed from nine- or more-membered rings formed from carbon atoms.

[0018] In the graphene, it is preferable that one or more carbon atoms constituting the multi-membered ring are terminated with fluorine.

[0019] Furthermore, in the analysis of the graphene by Raman spectroscopy, −1 The first peak observed at or near 1360 cm −1 It is preferable that the peak be a peak having a peak number of 1 or a second peak observed in the vicinity of the peak number.

[0020] Another embodiment of the present invention is an electrode including active material particles and graphene, in which the graphene has pores formed by nine- or more-membered rings each composed of carbon atoms, and the graphene covers at least a part of a surface of the active material particles.

[0021] In addition, in the graphene of the electrode, one or more carbon atoms constituting the multi-membered ring are preferably terminated with fluorine.

[0022] In addition, in the electrode, graphene has a Raman spectroscopic analysis of 1580 cm −1 The first peak observed at or near 1360 cm −1It is preferable that the peak be a peak having a peak number of 1 or a second peak observed in the vicinity of the peak number.

[0023] In the above-described configuration, the active material particles are preferably positive electrode active material particles.

[0024] In the above-described configuration, the active material particles are preferably negative electrode active material particles.

[0025] Another embodiment of the present invention is a secondary battery including any one of the above electrodes and an electrolyte.

[0026] Another embodiment of the present invention is an electronic device including any of the above secondary batteries.

[0027] Another embodiment of the present invention is a vehicle including the above-described secondary battery.

[0028] According to one embodiment of the present invention, a novel graphene can be provided. According to another embodiment of the present invention, a novel graphene compound can be provided. According to another embodiment of the present invention, an electrode having high output can be provided. According to another embodiment of the present invention, a novel electrode can be provided.

[0029] According to one embodiment of the present invention, a novel method for forming graphene, a novel method for forming a graphene compound, and a novel method for forming an electrode can be provided.

[0030] According to one embodiment of the present invention, a secondary battery with little deterioration can be provided. According to one embodiment of the present invention, a secondary battery with high safety can be provided. According to one embodiment of the present invention, a novel secondary battery can be provided.

[0031] According to one embodiment of the present invention, a novel substance, active material particles, a secondary battery, a power storage device, or a manufacturing method thereof can be provided.

[0032] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.

[0033] FIGS. 1A, 1B, and 1C are diagrams illustrating an example of a cross section of an electrode. FIGS. 2A and 2B are diagrams illustrating an example of a cross section of an electrode. FIG. 3 is a diagram illustrating a crystal structure of a positive electrode active material. FIG. 4 is a diagram illustrating a crystal structure of a positive electrode active material. FIG. 5 is a phase diagram. FIGS. 6A and 6B are diagrams illustrating an example of a manufacturing method. FIG. 7 is a diagram illustrating an example of a manufacturing method of an electrode of one embodiment of the present invention. FIGS. 8A and 8B are diagrams illustrating an example of a manufacturing method of a positive electrode active material of one embodiment of the present invention. FIG. 9 is a diagram illustrating an example of a manufacturing method of a positive electrode active material of one embodiment of the present invention. FIG. 10 is a diagram illustrating an example of a manufacturing method of a positive electrode active material of one embodiment of the present invention. FIG. 11 is a diagram illustrating an example of a manufacturing method of a positive electrode active material of one embodiment of the present invention. FIGS. 12A and 12B are cross-sectional views of a secondary battery. FIGS. 13A and 13B are diagrams illustrating an example of the external appearance of a secondary battery. FIGS. 14A and 14B are diagrams illustrating a manufacturing method of a secondary battery. 15A and 15B are diagrams illustrating a method for manufacturing a secondary battery. FIG. 16 is a diagram illustrating an example of the appearance of a secondary battery. FIG. 17 is a top view illustrating an example of a manufacturing apparatus for a secondary battery. FIG. 18 is a cross-sectional view illustrating an example of a method for manufacturing a secondary battery. FIGS. 19A to 19C are perspective views illustrating an example of a method for manufacturing a secondary battery. FIG. 19D is a cross-sectional view corresponding to FIG. 19C. FIGS. 20A to 20F are perspective views illustrating an example of a method for manufacturing a secondary battery. FIG. 21 is a cross-sectional view illustrating an example of a secondary battery. FIG. 22A is a diagram illustrating an example of a secondary battery. FIGS. 22B and 22C are diagrams illustrating an example of a method for manufacturing a stack. FIGS. 23A to 23C are diagrams illustrating an example of a method for manufacturing a secondary battery. FIGS. 24A and 24B are cross-sectional views illustrating an example of a stack. FIG. 24C is a cross-sectional view illustrating an example of a secondary battery. FIGS. 25A and 25B are diagrams illustrating an example of a secondary battery. FIG. 25C is a diagram illustrating the interior of a secondary battery. FIGS. 26A to 26C are diagrams illustrating an example of a secondary battery. Fig. 27A is a perspective view showing an example of a battery pack. Fig. 27B is a block diagram showing an example of a battery pack. Fig. 27C is a block diagram showing an example of a vehicle having a motor. Figs. 28A to 28E are diagrams showing an example of a transportation vehicle.FIG. 29A is a diagram showing an electric bicycle, FIG. 29B is a diagram showing a secondary battery for the electric bicycle, and FIG. 29C is a diagram explaining an electric motorcycle. FIGS. 30A and 30B are diagrams showing an example of a power storage device. FIGS. 31A to 31E are diagrams showing an example of an electronic device. FIGS. 32A to 32H are diagrams explaining an example of an electronic device. FIGS. 33A to 33C are diagrams explaining an example of an electronic device. FIG. 34 is a diagram explaining an example of an electronic device. FIGS. 35A to 35C are diagrams explaining an example of an electronic device. FIGS. 36A to 36C are diagrams explaining an example of an electronic device. FIG. 37 is an optical microscope photograph. FIGS. 38A, 38B, and 38C show evaluation results of Raman spectroscopy. FIG. 39 is a Raman spectrum. FIG. 40 is a TEM image. FIGS. 41A and 41B are FFT filtered images of the TEM image. FIGS. 42A and 42B are FFT filtered images of the TEM image. Figure 42C is a TEM image obtained by calculation, Figure 43A is a STEM image, and Figure 43B is an EDX analysis result.

[0034] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.

[0035] Furthermore, in this specification and the like, crystal planes and directions are indicated using Miller indices. In crystallography, crystal planes and directions are represented by a superscript bar after the number, but in this specification and the like, due to limitations on application notation, numbers may be represented by a minus sign (-) before them instead of a bar above them. Furthermore, individual orientations indicating directions within a crystal are represented by [ ], collective orientations indicating all equivalent directions are represented by < >, individual planes indicating crystal planes are represented by ( ), and collective planes with equivalent symmetry are represented by {}.

[0036] In this specification and the like, segregation refers to a phenomenon in which a certain element (for example, B) is spatially distributed non-uniformly in a solid composed of a plurality of elements (for example, A, B, C).

[0037] In this specification, the surface layer of particles of active material or the like is, for example, preferably a region within 50 nm from the surface, more preferably within 35 nm, and even more preferably within 20 nm. Surfaces formed by cracks and fissures may also be referred to as the surface. The region deeper than the surface layer is referred to as the interior.

[0038] In this specification and the like, the depth of charge when all of the intercalable and deintercalable lithium is intercalated into the positive electrode active material is defined as 0, and the depth of charge when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated is defined as 1.

[0039] In this specification, charging refers to the transfer of lithium ions from the positive electrode to the negative electrode within a battery and the transfer of electrons from the positive electrode to the negative electrode in an external circuit. Regarding a positive electrode active material, charging refers to the removal of lithium ions. A positive electrode active material with a charge depth of 0.7 to 0.9 is sometimes referred to as a positive electrode active material charged at a high voltage.

[0040] Similarly, discharging refers to the transfer of lithium ions from the negative electrode to the positive electrode within the battery and the transfer of electrons from the negative electrode to the positive electrode in an external circuit. For a positive electrode active material, discharging refers to the insertion of lithium ions. A positive electrode active material with a charge depth of 0.06 or less, or a positive electrode active material that has been discharged to 90% or more of its charge capacity from a high-voltage charged state, is referred to as a fully discharged positive electrode active material.

[0041] In this specification, a non-equilibrium phase change refers to a phenomenon that causes a non-linear change in a physical quantity. For example, a non-equilibrium phase change occurs around the peak in a dQ / dV curve obtained by differentiating capacitance (Q) with voltage (V) (dQ / dV), and it is believed that the crystal structure changes significantly.

[0042] A secondary battery has, for example, a positive electrode and a negative electrode. A material constituting the positive electrode is a positive electrode active material. The positive electrode active material is, for example, a substance that undergoes a reaction that contributes to the charge / discharge capacity. Note that the positive electrode active material may partially contain a substance that does not contribute to the charge / discharge capacity.

[0043] In this specification and the like, the positive electrode active material of one embodiment of the present invention may be referred to as a positive electrode material, a positive electrode material for a secondary battery, or the like. Also, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a compound. Also, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composition. Also, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composite.

[0044] The discharge rate is the relative ratio of the current during discharge to the battery capacity, and is expressed in units of C. For a battery with a rated capacity of X (Ah), the current equivalent to 1C is X (A). When a battery is discharged at a current of 2X (A), it is said to have been discharged at 2C, and when a battery is discharged at a current of X / 5 (A), it is said to have been discharged at 0.2C. The same is true for the charge rate; when a battery is charged at a current of 2X (A), it is said to have been charged at 2C, and when a battery is charged at a current of X / 5 (A), it is said to have been charged at 0.2C.

[0045] Constant current charging, for example, refers to a method of charging at a constant charge rate. Constant voltage charging, for example, refers to a method of charging at a constant voltage once the upper voltage limit is reached. Constant current discharging, for example, refers to a method of discharging at a constant discharge rate.

[0046] Embodiment 1 In this embodiment, graphene and an electrode according to one embodiment of the present invention will be described.

[0047] Graphene according to one embodiment of the present invention has holes formed by multi-membered rings composed of carbon. The multi-membered rings are preferably 9- or more-membered rings. Examples of the 9- or more-membered rings include 12-, 18-, and 22-membered rings.

[0048] The holes in the graphene of one embodiment of the present invention are preferably formed by mixing a material that becomes graphene as a first material, a compound that contains a halogen as a second material, and a compound that undergoes a eutectic reaction with the second material as a third material, and then heating the mixture. For example, graphene oxide can be used as the material that becomes graphene.

[0049] The graphene of one embodiment of the present invention preferably contains a halogen. One or more carbon atoms constituting the poly-membered ring are preferably terminated with a halogen atom. Fluorine is particularly preferred as the halogen.

[0050] The graphene of one embodiment of the present invention preferably has a functional group. Examples of the functional group included in the graphene of one embodiment of the present invention include a hydroxy group, an epoxy group, and a carboxy group. The functional group included in the graphene of one embodiment of the present invention may be bonded to carbon that constitutes a multi-membered ring included in the graphene of one embodiment of the present invention.

[0051] Graphene according to one embodiment of the present invention has a sheet shape. Graphene has a two-dimensional structure formed of six-membered carbon rings. In other words, graphene is a sheet having a two-dimensional structure formed of six-membered carbon rings, and graphene according to one embodiment of the present invention has holes formed by multiple-membered carbon rings in parts of the sheet.

[0052] An electrode of one embodiment of the present invention includes active material particles and graphene, and it is preferable that the graphene cover at least part of the surface of the active material particles.

[0053] An electrode of one embodiment of the present invention includes active material particles and a plurality of graphenes. At least a portion of the surface of the active material particles may be covered with the plurality of graphenes. The plurality of graphenes may have overlapping regions and non-overlapping regions. By partially overlapping the plurality of graphenes, a sheet having a larger area can be formed. For example, a first graphene has a first region overlapping with an active material particle and a second graphene. The first region is disposed on the surface of the active material particle. The first region is sandwiched between the active material particle and the second graphene. By overlapping the second graphene with the first region of the first graphene, for example, the first graphene and the second graphene can be partially overlapped with each other. Furthermore, the first graphene and the second graphene may be bonded to each other in the overlapping region. Furthermore, the overlapping region may be attracted to each other by intermolecular force.

[0054] The graphene is provided so as to cling to the surfaces of the active material particles, and preferably has a region in surface contact with the active material particles, and preferably is provided so as to adhere to the surfaces of the active material.

[0055] An electrode of one embodiment of the present invention includes a plurality of active material particles and graphene. The graphene preferably covers at least a part of the surface of each of the plurality of active material particles. The graphene preferably clings to the plurality of active material particles.

[0056] An electrode according to one embodiment of the present invention includes a plurality of active material particles and a plurality of graphenes. The plurality of graphenes have overlapping regions, thereby forming a sheet having a larger area. The sheet preferably covers at least a portion of each of the surfaces of the plurality of active material particles. Furthermore, the sheet preferably clings to the plurality of active materials.

[0057] In the electrode of one embodiment of the present invention, the graphene forms a bag-shaped region. The bag-shaped region may be formed of a plurality of graphenes. For example, the plurality of graphenes have a region where they overlap with each other, thereby forming the bag-shaped region. A plurality of active material particles are enclosed in the bag-shaped region.

[0058] In the electrode of one embodiment of the present invention, the plurality of graphenes can form a three-dimensional conductive path. In addition, in the electrode of one embodiment of the present invention, the plurality of graphenes may form a three-dimensional mesh structure.

[0059] An electrode of one embodiment of the present invention includes, for example, a current collector and an active material layer. The active material layer is provided over the current collector. The active material layer includes an active material and graphene. The active material layer may also include a binder.

[0060] The current collector can be made of a material that is highly conductive and does not alloy with carrier ions such as lithium, such as metals such as stainless steel, gold, platinum, zinc, iron, copper, aluminum, and titanium, and alloys thereof. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, and molybdenum, can also be used. The current collector can also be made of a metal element that reacts with silicon to form a silicide. Examples of metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be in a sheet, mesh, punched metal, expanded metal, or other shape. It is preferable to use a current collector with a thickness of 10 μm to 30 μm.

[0061] It is preferable to use a material that does not alloy with carrier ions such as lithium as the current collector used in the negative electrode.

[0062] A titanium compound may be provided as a current collector by being laminated on the metal element shown above. Examples of titanium compounds include titanium nitride, titanium oxide, titanium nitride in which part of the nitrogen is substituted with oxygen, titanium oxide in which part of the oxygen is substituted with nitrogen, and titanium oxynitride (TiO z N w , 0 < z < 2, 0 < w < 1), or a mixture or stack of two or more of these can be used. Among these, titanium nitride is particularly preferred because of its high conductivity and excellent oxidation suppression function. By providing a titanium compound on the surface of the current collector, for example, the reaction between the material of the active material layer formed on the current collector and the metal can be suppressed. When the active material layer contains an oxygen-containing compound, the oxidation reaction between the metal element and oxygen can be suppressed. For example, when aluminum is used as the current collector and the active material layer is formed using graphene oxide (described later), there may be a concern about the oxidation reaction between the oxygen in the graphene oxide and aluminum. In such a case, the oxidation reaction between the current collector and graphene oxide can be suppressed by providing a titanium compound on the aluminum.

[0063] In an electrode according to one embodiment of the present invention, a plurality of graphenes are distributed in the electrode so as to spread three-dimensionally and cover the active material, thereby increasing the strength of the active material layer. For example, increasing the strength of the active material layer can suppress collapse of the active material layer. Furthermore, for example, peeling of the active material layer from the current collector can be suppressed by contacting a portion of each of the plurality of graphenes with the current collector. In the electrode, graphene functions as a conductive agent that provides a conductive path and may also function as a binder that increases the strength of the active material layer and the electrode.

[0064] In the vertical cross section of the active material layer, sheet-like graphene is dispersed substantially uniformly in the inner region of the active material layer. The plurality of graphenes are formed so as to partially cover the plurality of granular active material particles or to adhere to the surfaces of the plurality of granular active material particles, and are therefore in surface contact with each other. Here, the vertical cross section of the active material layer refers to, for example, a surface substantially perpendicular to the current collector.

[0065] Here, a three-dimensional conductive path can be formed by bonding multiple graphenes together. Hereinafter, the three-dimensional conductive path formed by bonding multiple graphenes together will be referred to as a graphene net. When an active material is covered with a graphene net, the graphene net can also function as a binder that binds the active material together. Therefore, the amount of binder can be reduced or eliminated, thereby increasing the ratio of active material to the electrode volume and electrode weight. In other words, the charge / discharge capacity of a secondary battery can be increased.

[0066] The active material layer can be fabricated using, for example, graphene oxide and an active material. Here, in fabricating the active material layer, it is preferable to mix graphene oxide with an active material to form a layer that will become the active material layer, and then reduce the graphene oxide to obtain graphene. That is, the completed active material layer preferably contains reduced graphene oxide. In fabricating the active material layer, by using graphene oxide with extremely high dispersibility in a polar solvent, it is possible to uniformly disperse graphene oxide in a slurry containing graphene oxide and an active material. Therefore, in the fabricated active material layer, graphene can be approximately uniformly dispersed in the inner region of the active material layer. Since the solvent is volatilized and removed from the dispersion medium containing uniformly dispersed graphene oxide and the graphene oxide is reduced, the graphene remaining in the active material layer partially overlaps and is dispersed to such an extent that it is in surface contact with each other, thereby forming a three-dimensional conductive path. The graphene oxide may be reduced, for example, by heat treatment or using a reducing agent. The slurry is, for example, a mixture of raw materials for the active material layer and a solvent.

[0067] Alternatively, a spray dryer may be used to form a coating of graphene, a conductive agent, in advance, covering at least a portion of the surface of the active material, and the active materials on which the graphene coating has been formed may be electrically connected by the graphene to form a conductive path.

[0068] In this specification and the like, graphene may include, for example, graphene, multilayer graphene, multi-graphene, graphene oxide, multilayer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, etc. Graphene refers to a substance that contains carbon, has a shape such as a plate or sheet, and has a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings may also be called a carbon sheet. Graphene may have a functional group. Graphene preferably has a curved shape. Graphene may also be rolled up to resemble a carbon nanofiber.

[0069] In this specification and the like, graphene oxide refers to, for example, a material that contains carbon and oxygen, has a sheet-like shape, and has a functional group, in particular, an epoxy group, a carboxy group, or a hydroxy group.

[0070] In this specification and the like, reduced graphene oxide refers to, for example, a material containing carbon and oxygen, having a sheet-like shape, and having a two-dimensional structure formed by six-membered carbon rings. It may also be called a carbon sheet. Although a single sheet of reduced graphene oxide can function, multiple sheets may also be stacked. Reduced graphene oxide preferably has a portion where the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % or more and 15 atomic % or less. By achieving such a carbon concentration or such an oxygen concentration, or by achieving such a concentration for at least one of the carbon and oxygen, or both, the reduced graphene oxide can function as a highly conductive agent even in small amounts.

[0071] By reducing graphene oxide, it may be possible to provide holes in the graphene.

[0072] Furthermore, the edges of the graphene may be terminated with halogen atoms, particularly fluorine atoms.

[0073] When graphene is analyzed by Raman spectroscopy, a peak called the G band may be observed. The G band is located at 1580 cm −1 The G band indicates the presence of sp2 bonds in carbon. When graphene has defects such as holes, a peak called the D band may be observed. The D band is located at 1360 cm in the Raman spectrum. −1 It refers to a peak near that peak.

[0074] For example, a low defect density in graphene is suggested when the ratio of the peak intensity of the D band to that of the G band (D / G) is less than 1. Furthermore, when graphene has defects such as holes, D / G may be 1 or more, for example, 1 or more and 3 or less, or 1 or more and 2 or less.

[0075] ToF-SIMS may be able to observe the bonds that form the pores in graphene or the functional groups that bond to the atoms that form the pores. TEM observation may also be able to observe the pores in graphene.

[0076] When graphene is observed using a high-resolution TEM image, pores composed of multi-membered rings can sometimes be observed.

[0077] In the graphene of one embodiment of the present invention, it is preferable that pores composed of multi-membered rings are observed by TEM observation.Furthermore, in the graphene of one embodiment of the present invention, it is preferable that pores composed of multi-membered rings, particularly 9- or more-membered rings, are observed by TEM observation.

[0078] Graphene can be observed, for example, by an FFT-filtered image of a TEM. The FFT-filtered image refers to an image obtained by performing an FFT (Fast Fourier Transform) process on a TEM image, followed by an IFFT (Inverse Fast Fourier Transform) process.

[0079] The electrode of one embodiment of the present invention can be suitably used for lithium-ion secondary batteries. In the electrode of one embodiment of the present invention, graphene has pores, which allow lithium ions, which are carrier ions, to pass through the pores. Therefore, even when graphene covers the surface of an active material, it does not inhibit lithium insertion and desorption into and from the active material, thereby achieving excellent secondary battery characteristics. For example, graphene preferably has pores formed of nine- or more-membered rings, which allow lithium ions to easily pass through the pores. In a ring having fewer than nine members, the distance between the carbon atom forming the pore and the lithium ion is short, which may increase the barrier energy for the lithium ion to pass through the pore.

[0080] In a nine- or more-membered ring, the distance between the carbon atom constituting the hole and the lithium ion is adequate, stabilizing the energy and lowering the barrier energy for the lithium ion to pass through the hole. Furthermore, halogens, especially fluorine, have high electronegativity and tend to be negatively charged. Therefore, when the carbon atom constituting the hole is terminated by a halogen, positively charged lithium ions approach, causing an interaction, stabilizing the energy and lowering the barrier energy for the lithium ion to pass through the hole.

[0081] Halogen, particularly fluorine, can form a hydrogen bond with a hydrogen atom. When the graphene of one embodiment of the present invention contains a halogen and the active material has a hydrogen-terminated region or a region terminated by a functional group having a hydrogen atom, the graphene can form a hydrogen bond and be attached to the active material.

[0082] The electrode of one embodiment of the present invention can be used for a positive electrode and a negative electrode of a secondary battery. The secondary battery of one embodiment of the present invention includes a positive electrode including the graphene of one embodiment of the present invention and a negative electrode including the graphene of one embodiment of the present invention.

[0083] When the electrode of one embodiment of the present invention is used as a positive electrode, a positive electrode active material may be used as an active material.When the electrode of one embodiment of the present invention is used as a negative electrode, a negative electrode active material may be used as an active material.

[0084] 1A is a schematic cross-sectional view illustrating an electrode of one embodiment of the present invention. An electrode 570 shown in FIG. 1A can be used for a positive electrode and a negative electrode of a secondary battery. The electrode 570 includes at least a current collector 571 and an active material layer 572 formed in contact with the current collector 571.

[0085] 1B, 1C, 2A, and 2B are enlarged views of a square region 570b surrounded by a dashed line in Fig. 1A. The active material layer 572 includes an electrolyte 581, particles 582, and graphene 583.

[0086] 1B includes particles 582 covered with graphene 583. In FIG. 1B, graphene 583 may cover the surfaces of a plurality of particles 582.

[0087] 1C , a portion of the surface of a particle 582 is covered with graphene 583. In some cases, the surfaces of a plurality of particles 582 are covered with graphene 583. In addition, the graphene 583 is distributed so as to form a three-dimensional conductive path in the electrode.

[0088] 2A , a plurality of particles 582 are aggregated. Some of the aggregated particles 582 are covered with graphene 583. The graphene 583 is distributed so as to form a three-dimensional conductive path within the electrode.

[0089] In the active material layer 572 shown in FIG. 2B , a plurality of graphenes 583 form a three-dimensional mesh structure, and particles 582 are arranged between the plurality of graphenes 583 .

[0090] The particles 582 preferably function as an active material. A material that functions as an active material can be used as the particles 582. Alternatively, the particles 582 preferably have, for example, a material that functions as an active material. In this specification and the like, the particles 582 are referred to as active material particles. Various materials can be used as the particles 582. Materials that can be used as the particles 582 will be described later.

[0091] The active material layer 572 includes graphene 583. The graphene 583 can function as a conductive agent.

[0092] Furthermore, the active material layer 572 preferably contains, in addition to graphene, a carbon-based material such as carbon black, graphite, carbon fiber, or fullerene. Examples of carbon black that can be used include acetylene black (AB). Examples of graphite that can be used include natural graphite and artificial graphite such as mesocarbon microbeads. These carbon-based materials have high conductivity and can function as a conductive agent in the active material layer. These carbon-based materials may also function as an active material. FIGS. 1B and 1C show an example in which the active material layer 572 contains acetylene black 584.

[0093] Examples of carbon fibers that can be used include mesophase pitch-based carbon fibers and isotropic pitch-based carbon fibers. Carbon nanofibers and carbon nanotubes can also be used as carbon fibers. Carbon nanotubes can be produced by vapor phase growth, for example.

[0094] The active material layer may also contain, as a conductive agent, one or more selected from metal powders such as copper, nickel, aluminum, silver, and gold, metal fibers, and conductive ceramic materials.

[0095] The content of the conductive additive relative to the total amount of the active material layer is preferably 1 wt % to 10 wt %, more preferably 1 wt % to 5 wt %. When the active material layer contains graphene and graphene oxide is used as the material to form the graphene, the content of the graphene oxide in the slurry for forming the active material layer is preferably 1 wt % to 10 wt %, more preferably 1 wt % to 5 wt %, relative to the total amount of the active material, graphene oxide, and binder.

[0096] Unlike granular conductive agents such as carbon black, which make point contact with the active material, graphene allows for surface contact with the active material with low contact resistance, so that a smaller amount of graphene than a conventional conductive agent can improve the electrical conductivity between the granular active material and graphene. This allows for an increased ratio of the active material in the active material layer, thereby increasing the discharge capacity of the secondary battery.

[0097] Furthermore, lithium easily passes through the graphene of one embodiment of the present invention, so that the charge / discharge rate of the secondary battery can be increased.

[0098] Particulate carbon-containing compounds such as carbon black and graphite, and fibrous carbon-containing compounds such as carbon nanotubes, easily enter microscopic spaces. Microscopic spaces refer to, for example, the regions between multiple active materials. By combining a carbon-containing compound that easily enters microscopic spaces with a sheet-like carbon-containing compound such as graphene, which can impart conductivity across multiple particles, the density of the electrode can be increased and an excellent conductive path can be formed. Furthermore, by including an electrolyte according to one embodiment of the present invention in a secondary battery, the operational stability of the secondary battery can be improved. That is, the secondary battery according to one embodiment of the present invention can achieve both high energy density and stability, making it effective as an in-vehicle secondary battery. Increasing the number of secondary batteries increases the vehicle weight, which in turn reduces the cruising range due to the increased energy required for movement. Using high-density secondary batteries can increase the cruising range without significantly changing the total weight of a vehicle equipped with the same weight of secondary batteries.

[0099] Furthermore, since a large amount of charging power is required when a vehicle's secondary battery has a high capacity, it is desirable to charge the battery under high-rate charging conditions in order to complete charging in a short time. Furthermore, charging is performed under high-rate charging conditions in so-called regenerative charging, in which temporary power is generated when the vehicle brakes are applied and the battery is charged with that power, so good rate characteristics are required for vehicle secondary batteries.

[0100] Because graphene has high conductivity, its proportion in the electrode can be reduced. Therefore, the surface area of ​​the conductive agent in the electrode can be reduced, thereby suppressing decomposition of the electrolyte. Decomposition of the electrolyte may occur significantly, particularly at high temperatures. Therefore, a secondary battery using an electrode of one embodiment of the present invention can suppress deterioration at high temperatures. Furthermore, because graphene has high conductivity, the secondary battery can operate with high output even at low temperatures. Therefore, by using the electrode of one embodiment of the present invention, a secondary battery for vehicle use having a wide operating temperature range can be obtained. Furthermore, by using an ionic liquid as the electrolyte, decomposition of the electrolyte at high temperatures can be suppressed, resulting in a secondary battery that can operate at high temperatures.

[0101] Furthermore, the secondary battery of one embodiment of the present invention has a high energy density, which allows for miniaturization, and has high conductivity, which allows for rapid charging. Therefore, the structure of the secondary battery of one embodiment of the present invention is also effective in portable information terminals.

[0102] The active material layer 572 preferably includes a binder (not shown). The binder binds or fixes, for example, the electrolyte and the active material. The binder can also bind or fix the electrolyte and a carbon-based material, the active material and another carbon-based material, multiple active materials together, multiple carbon-based materials, etc.

[0103] As the binder, it is preferable to use a material such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, or nitrocellulose.

[0104] Polyimide has excellent thermal, mechanical, and chemical stability. Furthermore, when polyimide is used as a binder, a dehydration reaction and a cyclization (imidization) reaction occur. These reactions can be performed, for example, by heat treatment. In an electrode according to one embodiment of the present invention, when graphene having an oxygen-containing functional group is used as the graphene and polyimide is used as the binder, the heat treatment can also reduce the graphene, thereby simplifying the process. Furthermore, because polyimide has excellent heat resistance, the heat treatment can be performed at a heating temperature of, for example, 200° C. or higher. By performing heat treatment at a heating temperature of 200° C. or higher, the reduction reaction of graphene can be sufficiently performed, and the conductivity of the electrode can be further increased.

[0105] A fluorine-containing polymer material, such as a fluoropolymer, can be used. PVDF is a resin with a melting point in the range of 134°C to 169°C, and is a material with excellent thermal stability.

[0106] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. As the binder, fluororubber can also be used.

[0107] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include one or more selected from cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, as well as starch. It is even more preferable to use these water-soluble polymers in combination with the rubber material described above.

[0108] The binder may be used in combination with two or more of the above.

[0109] Furthermore, graphene 583 is flexible and can cling to particles 582 like natto (fermented soybeans). For example, particles 582 can be compared to soybeans, and graphene 583 can be compared to a sticky component, such as polyglutamic acid. By disposing graphene 583 between materials contained in active material layer 572, such as an electrolyte, multiple active materials, and multiple carbon-based materials, not only can a good conductive path be formed within active material layer 572, but these materials can also be bound or fixed using graphene 583. For example, multiple graphenes 583 can be used to form a three-dimensional mesh structure, a polygonal array structure, such as a honeycomb structure in which hexagons are arranged in a matrix, and materials such as an electrolyte, multiple active materials, and multiple carbon-based materials are arranged in the mesh. This allows graphene to form a three-dimensional conductive path and prevent the electrolyte from falling off the current collector. Furthermore, in the polygonal array structure, polygons with different numbers of sides may be arranged intermingled. Therefore, the graphene 583 functions as a conductive agent and also as a binder in the active material layer 572 in some cases.

[0110] The particles 582 may have various shapes, such as a rounded shape or a shape with corners. Furthermore, in the cross section of the electrode, the particles 582 may have various cross-sectional shapes, such as a circle, an ellipse, a curved figure, a polygon, etc. For example, FIG. 2A shows an example in which the cross section of the particles 582 has a rounded shape, but the cross-sectional shape of the particles 582 may have corners. Furthermore, the cross-sectional shape of the particles 582 may be partially rounded and partially angular.

[0111] <Example of Negative Electrode Active Material> When the electrode 570 is a negative electrode, particles having a negative electrode active material can be used as the particles 582. As the negative electrode active material, it is preferable to use a material capable of reacting with carrier ions of a secondary battery, a material capable of inserting and desorbing carrier ions, a material capable of alloying with a metal that becomes a carrier ion, a material capable of dissolving and precipitating a metal that becomes a carrier ion, or the like.

[0112] The negative electrode active material can be silicon. The electrode 570 preferably uses silicon-containing particles as the particles 582.

[0113] As the negative electrode active material, a metal or a compound containing one or more elements selected from tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, and indium can be used. Examples of alloy compounds using such elements include Mg 2 Si, Mg 2 Ge, Mg 2 Sn, SnS 2 , V 2 Sn 3 , FeSn 2 , CoSn 2 , Ni 3 Sn 2 , Cu 6 Sn 5 , Ag 3 Sn, Ag 3 Sb, Ni 2 MnSb, CeSb 3 , LaSn 3 , La 3 Co 2 Sn 7 , CoSb 3 , InSb, SbSn, etc.

[0114] Alternatively, a material having low resistance may be used by adding impurity elements such as phosphorus, arsenic, boron, aluminum, or gallium to silicon. A silicon material pre-doped with lithium may also be used. Pre-doping methods include mixing silicon with lithium fluoride or lithium carbonate and annealing the mixture, or mechanical alloying of lithium metal and silicon. After forming the electrode, the material may be combined with an electrode such as lithium metal to dope the material with lithium through a charge-discharge reaction. The doped electrode may then be combined with a counter electrode (e.g., a positive electrode for a pre-doped negative electrode) to produce a secondary battery.

[0115] For example, silicon nanoparticles can be used as the particles 582. The average diameter of the silicon nanoparticles is, for example, preferably 5 nm or more and less than 1 μm, more preferably 10 nm or more and 300 nm or less, and even more preferably 10 nm or more and 100 nm or less.

[0116] The silicon nanoparticles may be crystalline, or may have a crystalline region and an amorphous region.

[0117] Examples of silicon-containing materials include SiO z (z is preferably smaller than 2, more preferably 0.5 or more and 1.6 or less) can be used.

[0118] The silicon-containing material may have, for example, a plurality of crystal grains within a single particle. For example, a single particle may have one or more silicon crystal grains within it. The single particle may have silicon oxide around the silicon crystal grain. The silicon oxide may be amorphous. The material may also be a particle in which graphene is attached to a secondary silicon particle.

[0119] Examples of compounds containing silicon include Li 2 SiO 3 and Li 4 SiO 4 Li can be used. 2 SiO 3 and Li 4 SiO 4 may each be crystalline or amorphous.

[0120] The silicon-containing compound can be analyzed using NMR, XRD, Raman spectroscopy, SEM, TEM, EDX, or the like.

[0121] As the negative electrode active material, for example, carbon-based materials such as graphite, graphitizable carbon, non-graphitizable carbon, carbon nanotubes, carbon black, and graphene can be used.

[0122] Furthermore, as the negative electrode active material, for example, an oxide containing one or more elements selected from titanium, niobium, tungsten, and molybdenum can be used.

[0123] As the negative electrode active material, a combination of the above-mentioned metals, materials, compounds, etc. can be used.

[0124] Examples of the negative electrode active material include SnO, SnO 2 , titanium dioxide (TiO 2 ), lithium titanium oxide (Li 4 Ti 5 O 12 ), lithium-graphite intercalation compound (Li z C 6 ), niobium pentoxide (Nb 2 O 5 ), tungsten oxide (WO 2 ), molybdenum oxide (MoO 2 ) and other oxides can be used.

[0125] In addition, as the negative electrode active material, a composite nitride of lithium and a transition metal, Li 3 Li with N-type structure 3−z M z N (M=Co, Ni, Cu, z is 0 or more and less than 3) can be used. For example, Li 2.6 Co 0.4 N 3 exhibits a large charge / discharge capacity (900 mAh / g) and is therefore preferred.

[0126] When a composite nitride of lithium and transition metals is used as the negative electrode material, V containing no lithium ions can be used as the positive electrode material. 2 O 5 , Cr 3 O 8 It is preferable that the composite nitride of lithium and a transition metal be used as the negative electrode material, even when a material containing lithium ions is used as the positive electrode material, by first removing the lithium ions contained in the positive electrode material.

[0127] Furthermore, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, a transition metal oxide that does not undergo an alloying reaction with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), or iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include Fe 2 O 3 ,CuO,Cu 2 O, RuO 2 , Cr 2 O 3 oxides such as CoS 0.89 , sulfides such as NiS and CuS, Zn 3 N 2 , Cu 3 N, Ge 3 N 4 Nitrides such as NiP 2 , FeP 2 , CoP 3 Phosphides such as FeF 3 , BiF 3 The above fluorides have a high potential, and therefore may be used as a positive electrode material.

[0128] Furthermore, although the volume of the particles 582 may change during charging and discharging, by disposing a fluorine-containing electrolyte between the particles 582 in the electrode, the particles can slide easily even when volume changes during charging and discharging, and the generation of cracks is suppressed, which has the effect of dramatically improving cycle characteristics. It is important that a fluorine-containing organic compound exists between the multiple active materials that make up the electrode.

[0129] <Example of Positive Electrode Active Material> When the electrode 570 is a positive electrode, particles having a positive electrode active material can be used as the particles 582. Examples of the positive electrode active material include composite oxides having an olivine-type crystal structure, a layered rock salt-type crystal structure, or a spinel-type crystal structure. For example, LiFePO 4 , LiFeO 2 , LiNiO 2 , LiMn 2 O 4 , V 2 O 5 , Cr 2 O 5 , MnO 2The following compounds are exemplified:

[0130] In addition, LiMn 2 O 4 Lithium-containing materials having a spinel-type crystal structure containing manganese, such as lithium nickel oxide (LiNiO 2 or LiNi 1−z Mj z O 2 It is preferable to mix (0<z<1) (Mj=Co, Al, etc.) This configuration can improve the characteristics of the secondary battery.

[0131] In addition, as the positive electrode active material, a Mn b Mk c O d A lithium-manganese composite oxide that can be expressed by the formula: Mk is preferably a metal element selected from among lithium and manganese, silicon, or phosphorus, and more preferably nickel. When measuring the entire lithium-manganese composite oxide particle, it is preferable that 0<a / (b+c)<2, c>0, and 0.26≦(b+c) / d<0.5 are satisfied during discharge. The composition of metals, silicon, phosphorus, etc. in the entire lithium-manganese composite oxide particle can be measured, for example, using an inductively coupled plasma mass spectrometer (ICP-MS). The oxygen composition in the entire lithium-manganese composite oxide particle can be measured, for example, using energy dispersive X-ray spectroscopy (EDX). The composition can also be determined by valence evaluation using fusion gas analysis and XAFS (X-ray absorption fine structure) analysis in combination with ICP-MS analysis. The lithium manganese composite oxide refers to an oxide containing at least lithium and manganese, and may contain at least one element selected from the group consisting of chromium, cobalt, aluminum, nickel, iron, magnesium, molybdenum, zinc, indium, gallium, copper, titanium, niobium, silicon, phosphorus, and the like.

[0132] In addition, particles containing a plurality of the above-listed positive electrode active materials may be used as the positive electrode active material. For example, one of the above-listed positive electrode active materials may be used with another positive electrode active material to form particles having a structure in which at least a portion of one of the positive electrode active materials is covered by the other. Such particles having a structure in which at least a portion of one of the positive electrode active materials is covered by the other may be called a positive electrode active material composite. As the composite treatment, for example, any one or more of the following composite treatments can be performed: composite treatments using mechanical energy such as mechanochemical methods, mechanofusion methods, and ball milling methods; composite treatments using liquid-phase reactions such as coprecipitation methods, hydrothermal methods, and sol-gel methods; and composite treatments using gas-phase reactions such as barrel sputtering methods, ALD (Atomic Layer Deposition) methods, vapor deposition methods, and CVD (Chemical Vapor Deposition) methods. In addition, it is preferable to perform a heat treatment after the composite treatment. The composite treatment may also be called a surface coating treatment or a coating treatment.

[0133] Note that the positive electrode active material particles may form secondary particles. For example, in the structures shown in Figures 1B and 1C, particles 582 may be replaced with secondary particles formed by the positive electrode active material particles.

[0134] [Structure of positive electrode active material] Lithium cobalt oxide (LiCoO 2 Materials having a layered rock salt type crystal structure, such as LiMO, are known to have a high discharge capacity and are excellent as positive electrode active materials for secondary batteries. 2 Examples of the composite oxides include those represented by the formula (1). The element M is, for example, one or more elements including a transition metal. The element M is, for example, one or more metals including cobalt. The element M may further include, for example, one or more elements selected from magnesium, calcium, zirconium, lanthanum, barium, copper, potassium, sodium, and zinc in addition to one or more metals including cobalt.

[0135] Alternatively, the positive electrode active material of one embodiment of the present invention includes lithium, an element M, and an additional element X. Examples of the additional element X include magnesium, calcium, zirconium, lanthanum, barium, copper, potassium, sodium, zinc, titanium, yttrium, nickel, aluminum, cobalt, manganese, vanadium, iron, chromium, niobium, hafnium, silicon, sulfur, phosphorus, boron, arsenic, chlorine, and fluorine.

[0136] It is known that the strength of the Jahn-Teller effect in transition metal compounds varies depending on the number of electrons in the d orbital of the transition metal.

[0137] In compounds containing nickel, distortion may easily occur due to the Jahn-Teller effect. 2 When LiCoO is charged and discharged at a high voltage, there is a concern that the crystal structure may be destroyed due to distortion. 2 It is suggested that the influence of the Jahn-Teller effect is small in this case, and the durability of charge and discharge at high voltages may be superior, which is preferable.

[0138] Here, LiMO 2 The composition of the lithium composite oxide represented by the formula is not limited to Li:M:O=1:1:2. 2 Examples of the lithium composite oxide represented by the formula (I) include lithium cobalt oxide, lithium nickel-cobalt-manganese oxide, lithium nickel-cobalt-aluminate, and lithium nickel-cobalt-manganese-aluminate.

[0139] When cobalt is used as the element M in an amount of 75 atomic % or more, preferably 90 atomic % or more, and more preferably 95 atomic % or more, it has many advantages such as being relatively easy to synthesize and handle, and having excellent cycle characteristics.

[0140] On the other hand, when nickel is used as the element M in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more, the raw material may be cheaper than when cobalt is used in large amounts, and the charge / discharge capacity per weight may increase, which is preferable.

[0141] Furthermore, the particle size may become small when nickel is used in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more as the element M. Therefore, for example, it is preferable that the third particles described above contain nickel in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more as the element M.

[0142] Furthermore, when nickel is present in part along with cobalt as element M, it may suppress the deviation of the layered structure consisting of octahedra of cobalt and oxygen. This is preferable because the crystal structure may become more stable, particularly in the charged state at high temperatures. This is because nickel easily diffuses deep into the lithium cobalt oxide, and while it is present on the cobalt site during discharge, it is thought to be able to be located on the lithium site through cation mixing during charge. The nickel present on the lithium site during charge is thought to function as a pillar supporting the layered structure consisting of octahedra of cobalt and oxygen, contributing to the stabilization of the crystal structure.

[0143] The element M does not necessarily have to contain manganese, nickel, or cobalt.

[0144] During charging, lithium is released from the surface of the particles, so the lithium concentration in the surface layer of the particles tends to be lower than in the interior, and the crystalline structure tends to collapse.

[0145] The particles of one embodiment of the present invention contain lithium, an element M, and oxygen. 2The particle of one embodiment of the present invention includes a lithium composite oxide represented by the formula:

[0023] Furthermore, the particle of one embodiment of the present invention has one or more elements selected from magnesium, fluorine, aluminum, and nickel in the surface layer portion. By having one or more of these elements in the surface layer portion of the particle of one embodiment of the present invention, structural changes accompanying charge and discharge can be reduced in the surface layer portion of the particle, and crack formation can be suppressed. Furthermore, irreversible structural changes in the surface layer portion of the particle can be suppressed, and capacity loss accompanying repeated charge and discharge can be suppressed. Furthermore, the concentration of these elements in the surface layer portion is preferably higher than the concentration of these elements in the entire particle. Furthermore, the particle of one embodiment of the present invention may have a structure in the surface layer portion in which, for example, part of the atoms in the lithium composite oxide are substituted with one or more elements selected from magnesium, fluorine, aluminum, and nickel.

[0146] The positive electrode active material will be described with reference to FIGS. 3 and 4. FIG.

[0147] In this specification, the layered rock-salt type crystal structure belonging to the space group R-3m, which is possessed by a composite oxide containing lithium and a transition metal such as cobalt, refers to a crystal structure having a rock-salt type ion arrangement in which cations and anions are alternately arranged, and in which the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Defects such as vacancies of cations or anions may also be present. Furthermore, strictly speaking, the layered rock-salt type crystal structure may have a structure in which the lattice of the rock-salt type crystal is distorted.

[0148] In this specification and the like, the term "rock salt type crystal structure" refers to a structure having a cubic crystal structure such as the space group Fm-3m, in which cations and anions are arranged alternately. Note that there may be a deficiency of cations or anions.

[0149] The fact that the crystal orientations of the two regions roughly coincide can be determined from TEM (Transmission Electron Microscope) images, STEM (Scanning Transmission Electron Microscope) images, HAADF-STEM (High-angle Annular Dark Field Scanning TEM) images, ABF-STEM (Annular Bright-Field Scanning Transmission Electron Microscope) images, etc. X-ray diffraction (XRD), electron diffraction, neutron diffraction, etc. can also be used to make this determination. High-resolution TEM images, etc., provide contrast derived from crystal planes. Due to electron diffraction and interference, for example, when an electron beam is incident perpendicular to the c-axis of a layered rock-salt composite hexagonal lattice, the contrast derived from the (0003) plane appears as a repetition of bright and dark bands (bright strips). Therefore, when the angle between bright lines in a TEM image is between 0 and 5 degrees, or between 0 and 2.5 degrees, it can be determined that the crystal planes are roughly aligned, i.e., the crystal orientation is roughly aligned. Similarly, when the angle between dark lines is 5 degrees or less, or 2.5 degrees or less, it can also be determined that the crystal orientation is roughly aligned.

[0150] The positive electrode active material manufactured in one embodiment of the present invention has a high reproducibility of CoO 2 The layer misalignment can be reduced. Furthermore, the change in volume can be reduced. Therefore, the compound can achieve excellent cycle characteristics. Furthermore, the compound can have a stable crystal structure in a high-voltage charged state. Therefore, the compound may be less likely to cause a short circuit when maintained in a high-voltage charged state. In such cases, safety is further improved, which is preferable.

[0151] In this compound, the change in crystal structure and the difference in volume between a fully discharged state and a high-voltage charged state are small when compared per the same number of transition metal atoms.

[0152] An example of the crystal structure of a positive electrode active material before and after charge and discharge is shown in Figure 3. The positive electrode active material shown in Figure 3 preferably has a layered rock-salt crystal structure belonging to the space R-3m in the discharged state. Furthermore, the surface layer of the positive electrode active material may have, in addition to or instead of the region represented by the layered rock-salt structure, a crystal represented by a structure different from the layered rock-salt structure, containing titanium, magnesium, and oxygen. For example, the surface layer may have a crystal represented by a spinel structure containing titanium, magnesium, and oxygen.

[0153] The theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated. For example, LiCoO 2 The theoretical capacity of LiNiO is 274 mAh / g. 2 The theoretical capacity of LiMn is 274mAh / g. 2 O 4 The theoretical capacity of the battery is 148 mAh / g.

[0154] The amount of lithium remaining in the positive electrode active material that can be inserted or removed can be determined by x in the composition formula, for example, Li x CoO 2 x in, or Li x MO 2 In this specification, Li x CoO 2 Li as appropriate x MO 2 In the case of a positive electrode active material in a secondary battery, x can be expressed as x = (theoretical capacity - charging capacity) / theoretical capacity. For example, LiCoO 2 When a secondary battery using as a positive electrode active material is charged at 219.2 mAh / g, Li 0.2 CoO 2 Or we can say x = 0.2. x CoO 2 The small value of x in the formula means, for example, 0.1<x≦0.24.

[0155] When properly synthesized lithium cobalt oxide is used in the positive electrode, the stoichiometric ratio is approximately satisfied. 2 The occupancy rate of Li on the lithium site is x = 1. The secondary battery after discharge also has LiCoO 2 In this case, x = 1. The end of discharge here refers to the state where the voltage is 2.5 V (lithium counter electrode) or less at a current of 100 mA / g, for example. In a lithium ion secondary battery, when the occupancy rate of lithium in the lithium site reaches x = 1 and no more lithium can enter, the voltage drops sharply. At this point, discharge can be said to be complete. Generally, LiCoO 2 In the case of a lithium ion secondary battery using the above method, the discharge voltage drops rapidly until it reaches 2.5 V, so it is assumed that the discharge is completed under the above conditions.

[0156] For example, a charge depth of 0 refers to the state where x = 1 in the above example. Also, an increase in charge depth refers to a decrease in the value of x in the above example.

[0157] Li x CoO 2 It is preferable that the charge capacity and / or discharge capacity used to calculate x in the above should be measured under conditions where there is no or minimal influence of short circuit and / or electrolyte decomposition. For example, data from a secondary battery that has experienced a sudden change in capacity that is considered to be due to a short circuit should not be used to calculate x.

[0158] The crystal structure at a charge depth of 0 (the state where discharge is completed) in Fig. 3 is the same as that in Fig. 4, which is R-3m(O3). On the other hand, when the positive electrode active material shown in Fig. 3 is at a fully charged charge depth, for example, when x is 0.24 or less, for example, about 0.2 or about 0.12, the positive electrode active material has a crystal structure different from the H1-3 type crystal structure. This structure is in the space group R-3m, and CoO 2The symmetry of the layers is the same as that of the O3 type. Therefore, this structure is referred to as the O3' type crystal structure in this specification. In the diagram of the O3' type crystal structure shown in FIG. 3, when x = 0.2, lithium can exist at any lithium site with a probability of about 20%, but this is not limited to this. It may exist only at a specific part of the lithium sites. In both the O3 type crystal structure and the O3' type crystal structure, CoO 2 Magnesium is preferably present dilutely between the layers, i.e., at the lithium sites. Also, halogens such as fluorine may be present randomly and dilutely at the oxygen sites.

[0159] The O3' type crystal structure is in the space group R-3m, and ions of cobalt, magnesium, etc. occupy hexacoordinated oxygen positions. Light elements such as lithium may occupy tetracoordinated oxygen positions.

[0160] The O3' type crystal structure has randomly interlayered Li atoms, but the CdCl 2 It can be said that this crystal structure is similar to that of the CdCl type. 2 A crystal structure similar to the type was observed when lithium nickel oxide was charged to a charge depth of 0.94 (Li 0.06 NiO 2 ), but it is known that pure lithium cobaltate or layered rock salt-type positive electrode active materials containing a large amount of cobalt do not usually have this crystal structure.

[0161] The layered rock salt-type crystal and the anions in the rock salt-type crystal have a cubic close-packed structure (face-centered cubic lattice structure). It is presumed that the anions in the O3'-type crystal also have a cubic close-packed structure. Therefore, when the layered rock salt-type crystal and the rock salt-type crystal come into contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, since the space group of the layered rock salt-type crystal and the O3'-type crystal is R-3m, which is different from the space group Fm-3m (the space group of a general rock salt-type crystal) of the rock salt-type crystal, the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt-type crystal and the O3'-type crystal and the rock salt-type crystal. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in the layered rock salt-type crystal, the O3'-type crystal, and the rock salt-type crystal, the crystal orientation may be said to be approximately aligned.

[0162] In the positive electrode active material shown in Figure 3, the change in the crystal structure when a large amount of lithium is released by charging at a high voltage is further suppressed compared to the positive electrode active material shown in Figure 4. For example, as shown by the dotted line in Figure 3, in these crystal structures, CoO 2 There is almost no layer misalignment.

[0163] More specifically, the cathode active material shown in FIG. 3 has high structural stability even at high charging voltages. For example, even at charging voltages where the H1-3 crystal structure is formed in FIG. 4 , such as a voltage of about 4.6 V relative to the potential of lithium metal, the cathode active material shown in FIG. 3 can maintain the R-3m(O3) crystal structure. Even at higher charging voltages, such as a voltage of about 4.65 V to 4.7 V relative to the potential of lithium metal, the cathode active material shown in FIG. 3 has a region where it can adopt the O3′ crystal structure. Furthermore, when the charging voltage is increased above 4.7 V, the H1-3 crystal may be observed in the cathode active material shown in FIG. 3 . Furthermore, even at lower charging voltages (for example, when the charging voltage is 4.5 V or more but less than 4.6 V relative to the potential of lithium metal), the cathode active material shown in FIG. 3 may adopt the O3′ crystal structure. In addition, when graphite is used as the negative electrode active material in a secondary battery, the voltage of the secondary battery drops by the amount of the graphite's potential compared to the voltage based on the lithium metal potential. The potential of graphite is approximately 0.05 V to 0.2 V based on the lithium metal potential. Therefore, even when the voltage of a secondary battery using graphite as the negative electrode active material is 4.3 V or higher and 4.5 V or lower, the positive electrode active material shown in FIG. 3 can maintain the R-3m(O3) crystal structure. Furthermore, even when the charge voltage is higher, for example, when the voltage of the secondary battery is higher than 4.5 V and lower than 4.6 V, there is a region in which the O3'-type crystal structure can be formed. Furthermore, when the charge voltage is lower, for example, when the voltage of the secondary battery is 4.2 V or higher but lower than 4.3 V, the positive electrode active material shown in FIG. 3 can sometimes form the O3'-type crystal structure.

[0164] Therefore, in the positive electrode active material shown in FIG. 3, the crystal structure is not easily broken even when charging and discharging are repeated at a high voltage.

[0165] The crystal structure shown in FIG. 4 is labeled R-3m(O3), which means Li x CoO 2 This is the crystal structure of lithium cobalt oxide with x=1 in the figure. In this crystal structure, lithium occupies octahedral sites and there is CoO 2 There are three layers. Therefore, this crystal structure is sometimes called an O3 type crystal structure. 2The layer is defined as a structure in which octahedral structures in which oxygen is six-coordinated to cobalt are connected in a plane with edge sharing. This is sometimes called a layer consisting of cobalt and oxygen octahedra.

[0166] It is known that the lithium cobalt oxide shown in Figure 4 has a crystal structure that has high lithium symmetry when x = 0.5 or so and belongs to the monoclinic space group P2 / m. This structure has CoO 2 There is one layer, so it is sometimes called O1 type or monoclinic O1 type.

[0167] When x = 0, the positive electrode active material has a crystal structure of the trigonal space group P-3m1, and also contains CoO 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal O1 type. In addition, when the trigonal crystal is converted into a composite hexagonal lattice, it is sometimes called hexagonal O1 type.

[0168] When x is about 0.12, the lithium cobalt oxide shown in FIG. 4 has a crystal structure of the space group R-3m. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m(O3). 2 It can also be said that the structure of and the structure of are stacked alternately. Therefore, this crystal structure is sometimes called an H1-3 crystal structure. Note that, since actual lithium insertion and extraction can be uneven, the H1-3 crystal structure is experimentally observed from about x = 0.25. In fact, the number of cobalt atoms per unit cell in the H1-3 crystal structure is twice that of other structures. However, in this specification and the like, to make it easier to compare with other crystal structures, the c-axis of the H1-3 crystal structure may be shown in a diagram where the c-axis is half the unit cell.

[0169] As an example of the H1-3 type crystal structure, as described in Non-Patent Document 1, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), and O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are each oxygen atoms. Which unit cell should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of the XRD pattern. In this case, it is sufficient to adopt a unit cell that results in a small GOF (goodness of fit) value.

[0170] The positive electrode active material shown in FIG. x CoO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less is even smaller than that in Figure 4. More specifically, the change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less is even smaller than that in Figure 4. 2 The layer misalignment can be reduced, and the volume change per cobalt atom can be reduced.

[0171] Furthermore, in the positive electrode active material shown in FIG. 3, the difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the O3′-type crystal structure is 2.5% or less, more specifically 2.2% or less, and typically 1.8%.

[0172] In the O3'-type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed within the ranges of Co(0,0,0.5), O(0,0,x), 0.20≦x≦0.25. Regarding the lattice constant of the unit cell, the a-axis is preferably 0.2797≦a≦0.2837 (nm), more preferably 0.2807≦a≦0.2827 (nm), and typically a=0.2817 (nm). The c-axis is preferably 1.3681≦c≦1.3881 (nm), more preferably 1.3751≦c≦1.3811 (nm), and typically c=1.3781 (nm).

[0173] CoO 2 Magnesium, which exists randomly and dilutely between the layers, i.e., at the lithium sites, dissolves in CoO when charged at a high voltage. 2This has the effect of suppressing layer misalignment. 2 When magnesium is present between the layers, the O3' type crystal structure is easily formed.

[0174] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that magnesium will enter the cobalt site. Magnesium present at the cobalt site may have little effect on maintaining the R-3m structure during high-voltage charging. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as cobalt being reduced to divalent and lithium transpiration.

[0175] Therefore, it is preferable to add a halogen compound such as a fluorine compound to the lithium cobalt oxide before the heat treatment to distribute magnesium throughout the particles. Adding the halogen compound lowers the melting point of the lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium throughout the particles at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte.

[0176] Note that if the magnesium concentration is increased above a desired value, the effect on stabilizing the crystal structure may be reduced. This is thought to be because magnesium enters the cobalt site in addition to the lithium site. The number of magnesium atoms in the positive electrode active material produced according to one embodiment of the present invention is preferably 0.001 to 0.1 times the number of cobalt atoms, more preferably more than 0.01 to less than 0.04 times, and even more preferably about 0.02 times. The magnesium concentration shown here may be, for example, a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using ICP-MS or the like, or may be based on the value of the raw material composition in the process of producing the positive electrode active material.

[0177] The number of nickel atoms in the positive electrode active material is preferably 7.5% or less of the number of cobalt atoms, preferably 0.05% to 4%, and more preferably 0.1% to 2%. The nickel concentration shown here may be a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.

[0178] <Particle size> If the particle size of the positive electrode active material is too large, problems such as difficulty in diffusing lithium and excessive roughness of the surface of the active material layer when applied to a current collector occur. On the other hand, if the particle size is too small, problems such as difficulty in supporting the active material layer when applied to a current collector and excessive reaction with the electrolyte occur. Therefore, the average particle size (D50: also referred to as median diameter) is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less.

[0179] <Analysis Method> Whether a certain positive electrode active material exhibits an O3'-type crystal structure when charged at a high voltage can be determined by analyzing the positive electrode charged at a high voltage using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferred in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when measuring a positive electrode obtained by disassembling a secondary battery as is.

[0180] As mentioned above, positive electrode active materials are characterized by minimal change in crystal structure between the high-voltage charged and discharged states. Materials with a crystal structure that exhibits significant changes between the high-voltage charged and discharged states at 50 wt % or more are undesirable because they cannot withstand high-voltage charging and discharging. It should be noted that simply adding impurity elements may not result in the desired crystal structure. For example, even if lithium cobalt oxide containing magnesium and fluorine has the same characteristics, there are cases in which the O3'-type crystal structure accounts for 60 wt % or more when charged at a high voltage, and cases in which the H1-3-type crystal structure accounts for 50 wt % or more. Furthermore, at a certain voltage, the O3'-type crystal structure may be nearly 100 wt %, and further increasing the voltage may result in the H1-3-type crystal structure. Therefore, it is preferable to analyze the crystal structure of positive electrode active materials using XRD or other methods. By combining these methods with measurements such as XRD, even more detailed analysis can be performed.

[0181] However, when a positive electrode active material is charged or discharged at a high voltage, its crystal structure may change when exposed to air. For example, it may change from an O3'-type crystal structure to an H1-3-type crystal structure. Therefore, it is preferable to handle all samples in an inert atmosphere, such as an argon-containing atmosphere.

[0182] The positive electrode active material shown in FIG. 4 is lithium cobalt oxide (LiCoO 2 The crystal structure of the lithium cobalt oxide shown in Figure 4 changes depending on the depth of charge.

[0183] As shown in FIG. 4, lithium cobalt oxide at a charge depth of 0 (discharged state) has a region having a crystal structure of the space group R-3m, and CoO 2 There are three layers. Therefore, this crystal structure is sometimes called an O3 type crystal structure. 2 The layer refers to a structure in which an octahedral structure in which cobalt is six-coordinated with oxygen atoms is continuous on a plane in an edge-sharing state.

[0184] At a charge depth of 1, the crystal structure has a space group of P-3m1, and the unit cell contains CoO 2There is one layer, and therefore this crystal structure is sometimes called an O1-type crystal structure.

[0185] Furthermore, lithium cobalt oxide at a charge depth of about 0.8 has a crystal structure of the space group R-3m. This structure is similar to CoO such as P-3m1(O1). 2 and LiCoO such as R-3m(O3). 2 It can also be said that this crystal structure is a structure in which the structure of and the structure of are stacked alternately. For this reason, this crystal structure is sometimes called an H1-3 crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 crystal structure is twice that of other structures. However, in Figure 4 and other parts of this specification, the c-axis of the H1-3 crystal structure is shown as half the unit cell to make it easier to compare with other structures.

[0186] As an example of the H1-3 type crystal structure, the coordinates of cobalt and oxygen in the unit cell are Co(0, 0, 0.42150±0.00016), O 1 (0, 0, 0.27671±0.00045), O 2 It can be expressed as (0, 0, 0.11535±0.00045). 1 and O 2 are oxygen atoms. In this way, the H1-3 crystal structure is represented by a unit cell using one cobalt and two oxygen atoms. On the other hand, the O3' crystal structure of one embodiment of the present invention is preferably represented by a unit cell using one cobalt and one oxygen atom. This indicates that the symmetry between cobalt and oxygen differs between the O3' crystal structure and the H1-3 structure, and the O3' crystal structure exhibits a smaller change from the O3 structure than the H1-3 structure. The unit cell that is more preferably used to represent the crystal structure of the positive electrode active material may be selected, for example, so that the GOF (good of fitness) value is smaller in Rietveld analysis of the XRD pattern.

[0187] When lithium cobalt oxide is repeatedly charged and discharged at a high voltage of 4.6 V or higher based on the redox potential of lithium metal, or when it is charged to a deep depth of charge of 0.8 or higher, the crystal structure of the lithium cobalt oxide changes repeatedly between the H1-3 crystal structure and the R-3m(O3) structure in the discharged state (i.e., a non-equilibrium phase change).

[0188] However, these two crystal structures are different from CoO 2 As shown by the dotted line and double arrows in FIG. 4, in the H1-3 type crystal structure, CoO 2 The layers deviate significantly from R-3m(O3). Such dynamic structural changes can adversely affect the stability of the crystal structure.

[0189] Furthermore, the difference in volume is large: when compared per the same number of cobalt atoms, the difference in volume between the H1-3 type crystal structure and the O3 type crystal structure in a discharged state is 3.0% or more.

[0190] In addition, the H1-3 type crystal structure has CoO such as P-3m1(O1). 2 A structure with continuous layers is likely to be unstable.

[0191] Therefore, repeated high-voltage charging and discharging causes the crystalline structure of lithium cobalt oxide to collapse, which leads to a deterioration in cycle characteristics. This is thought to be because the collapse of the crystalline structure reduces the number of sites where lithium can exist stably and makes it difficult for lithium to be inserted and extracted.

[0192] <Example of Method for Producing Graphene> An example of a method for producing graphene of one embodiment of the present invention will be described below.

[0193] The graphene 583 can be manufactured by mixing a material that becomes graphene as the material 801 and a compound having a halogen as the material 802, and performing heat treatment on the mixture. Here, for example, graphene oxide can be used as the material 801.

[0194] In addition to the material 802, a material that undergoes a eutectic reaction with the material 802 may be mixed as the material 803. The eutectic point of the eutectic reaction is preferably lower than at least one of the melting points of the material 802 and the material 803. The lowering of the melting point due to the eutectic reaction may make the material 802 and the material 803 more likely to react with the material 801 during heat treatment. Furthermore, the material 802 and the material 803 may more easily cover the surface of the material 801 during heat treatment, thereby improving the coverage.

[0195] Furthermore, by using a compound having a metal whose ions function as carrier ions in a reaction of a secondary battery as the materials 802 and 803, when the metal is contained in a negative electrode active material, the metal may contribute to charge and discharge as a carrier ion. A detailed example of a manufacturing method using the materials 801, 802, and 803 will be described later with reference to FIG.

[0196] For example, a compound containing oxygen and carbon can be used as the material 803. For example, a carbonate can be used as the compound containing oxygen and carbon. Alternatively, for example, an organic compound can be used as the compound containing oxygen and carbon.

[0197] Alternatively, the material 803 may be a hydroxide.

[0198] Carbonates, hydroxides, etc. are preferred because they are inexpensive and highly safe materials. Carbonates, hydroxides, etc. are also preferred because they may form a eutectic point with compounds containing halogens.

[0199] A more specific example of the material 802 and the material 803 will be described. When lithium fluoride is used as the material 802, it may be difficult for the lithium fluoride to melt when mixed with the material 801 and heated, and it may be difficult for the lithium fluoride to react with the material 801. In such a case, by using a compound that undergoes a eutectic reaction with lithium fluoride as the material 803, the eutectic reaction between the lithium fluoride and the material 803 makes it easier for the fluorine contained in the lithium fluoride to react with the material 801.

[0200] As an example of the material 803 that undergoes a eutectic reaction with lithium fluoride, lithium carbonate will be described.

[0201] Figure 5 shows LiF and Li 2 CO 3 Figure 5 is a phase diagram showing the relationship between the ratio of LiF and temperature. Figure 5 is based on data from FACT Salt Phase Diagrams. As shown in Figure 5, the melting point of LiF is approximately 850°C, but the melting point of LiF is approximately 850°C. 2 CO 3 Therefore, for example, at the same heating temperature, the melting point of LiF and Li is lower than that of LiF alone. 2 CO 3 The mixed solution is more easily dissolved and therefore more likely to react with the material 801. In addition, the heating temperature can be lowered.

[0202] Furthermore, by using a eutectic reaction, it is possible to increase the affinity with the surface of the material 801. For example, when graphene is used as the material 801, the C—H bond of graphene may have low affinity with, for example, fluorine. 2 CO 3 The eutectic reaction improves the affinity between the C—H bond and the material containing fluorine, thereby increasing the reactivity.

[0203] Also, at point P shown in FIG. 2 CO 3 The molar amount of LiF relative to the total molar amount of [LiF / (Li 2 CO 3 + LiF)] is approximately 0.48, and the melting point is the lowest. 2 CO 3 The molar ratio of LiF:Li 2 CO 3 If a1 = a1: (1 - a1), the melting point can be minimized by setting a1 to around 0.48. The temperature at point P is approximately 615°C.

[0204] a1 is preferably, for example, greater than 0.2, and more preferably 0.3 or greater. In particular, by setting a1 to a value greater than 0.48, the fluorine content of graphene can be increased. However, if the fluorine content is too high, the melting point may increase, resulting in poor coverage. a1 is, for example, preferably less than 0.9, and more preferably 0.8 or less.

[0205] An example of a method for manufacturing graphene of one embodiment of the present invention will be described with reference to a flow diagram in FIG. 6A.

[0206] In step S21, a material 801 is prepared. The material 801 is a raw material of graphene of one embodiment of the present invention. For example, the material 801 is graphene before fluorine addition. For example, the material 801 is graphene before reduction. Graphene oxide is used as the material 801 here.

[0207] In step S22, a compound containing a halogen is prepared as the material 802. A halogen compound containing a metal A1 can be used as the halogen compound. For example, the metal A1 can be one or more elements selected from lithium, magnesium, aluminum, sodium, potassium, calcium, barium, lanthanum, cerium, chromium, manganese, iron, cobalt, nickel, zinc, zirconium, titanium, vanadium, and niobium. For example, a fluoride or a chloride can be used as the halogen compound. The halogen contained in the halogen compound is referred to as element Z. Examples of Z include fluorine and chlorine.

[0208] Here, lithium fluoride is prepared as an example.

[0209] In step S23, a compound containing oxygen and carbon is prepared as material 803. For example, a carbonate containing metal A2 can be used as the compound containing oxygen and carbon. For example, one or more elements selected from lithium, magnesium, aluminum, sodium, potassium, calcium, barium, lanthanum, cerium, chromium, manganese, iron, cobalt, and nickel can be used as metal A2.

[0210] Here, lithium carbonate is prepared as an example.

[0211] Next, in step S31, materials 801, 802, and 803 are mixed, in step S32 the mixture is collected, and in step S33 a mixture 804 is obtained.

[0212] It is preferable that material 802 and material 803 are mixed in a ratio of (material 802):(material 803)=a1:(1-a1) [unit: mol], where a1 is preferably greater than 0.2 and less than 0.9, and more preferably greater than 0.3 and less than 0.8.

[0213] Furthermore, the material 801 and the material 802 are preferably mixed in a ratio of (material 801):(material 802)=1:b1 (unit: mol), and b1 is preferably 0.001 or more and 0.2 or less.

[0214] Next, in step S51, the mixture 804 is heated.

[0215] Heating in a reducing atmosphere is preferable because it can suppress oxidation of the surface of the material 801. The reducing atmosphere may be, for example, a nitrogen atmosphere or a rare gas atmosphere. Alternatively, a mixture of two or more types of nitrogen and rare gas may be used. Heating may also be performed under reduced pressure.

[0216] The melting point of the material 802 is M 2 When expressed as [K], the heating temperature is, for example, (M 2 -550) [K] higher (M 2 +50) [K], and (M 2 -400) [K] or more M 2 It is more preferable that it is [K] or less.

[0217] Furthermore, solid-state diffusion of a compound is likely to occur at temperatures equal to or higher than the Tammann temperature. For example, the Tammann temperature is 0.757 times the melting point of an oxide. Therefore, for example, the heating temperature is preferably 0.757 times the eutectic point or higher, or a temperature close to that temperature.

[0218] Furthermore, in the case of lithium fluoride, which is a typical example of the material 802, the amount of evaporation increases rapidly above the melting point. Therefore, for example, the heating temperature is preferably equal to or lower than the melting point of the material 802.

[0219] The eutectic point of the material 802 and the material 803 is M 23 When expressed as [K], the heating temperature is, for example, (M 23 ×0.7) [K] higher (M 2 +50) [K], and (M 23 ×0.75) [K] or more (M 2 +20) [K] or less, and M 23 [K] higher (M 2 +10) [K], and (M 23 ×0.8) [K] or more M 2 It is more preferable that the value is equal to or less than [K], and M 23 [K] or more M 2 It is more preferable that it is [K] or less.

[0220] When lithium fluoride is used as the material 802 and lithium carbonate is used as the material 803, the heating temperature is, for example, preferably greater than 350°C and less than 900°C, more preferably 390°C or higher and 850°C or lower, even more preferably 520°C or higher and 910°C or lower, still more preferably 570°C or higher and 860°C or lower, and even more preferably 610°C or higher and 860°C or lower.

[0221] The heating time is, for example, preferably 1 hour or more and 60 hours or less, and more preferably 3 hours or more and 20 hours or less.

[0222] Next, in step S52, the heated mixture is recovered, and in step S53, graphene 583 is obtained. The graphene 583 produced in the example shown here is, for example, graphene doped with fluorine. The graphene 583 produced in the example shown here is, for example, reduced graphene oxide, or graphene doped with fluorine.

[0223] Through the above steps, graphene of one embodiment of the present invention can be obtained.

[0224] <Example of Particle Production Method> Alternatively, as shown in Fig. 6B , particles 582 may be used in step S24, and particles 582 may be further added to and mixed with materials 801, 802, and 803 in step S31b, and the materials may be collected in step S32b, and mixture 804b may be obtained in step S33b. By using the flow shown in Fig. 6B , particles covered with graphene can be produced. Steps S31 and S32 can be referred to for steps S31b and S32b, respectively.

[0225] In step S51b, the mixture 804b is heated, the heated mixture is recovered in step S52b, and particles 582 covered with graphene (hereinafter, particles 582b) are obtained in step S53b. Steps S51 and S52 can be referred to, respectively, for steps S51b and S52b. In addition, in step S53b, particles 582 not covered with graphene and graphene not covering particles 582 may be obtained along with particles 582b. The particles 582b are, for example, particles 582 covered with graphene to which fluorine has been added. In addition, the particles 582b are, for example, particles 582 covered with graphene and contain fluorine.

[0226] <Method for Manufacturing Electrode> FIG. 7 is a flowchart illustrating an example of a method for manufacturing an electrode according to one embodiment of the present invention.

[0227] First, in step S71, particles 582 are prepared. Here, particles containing silicon are prepared. Alternatively, particles 582b, the manufacturing method of which has been described above, may be used instead of particles 582.

[0228] Next, in step S72, a solvent is prepared. The solvent may be, for example, one or a mixture of two or more of water, methanol, ethanol, acetone, tetrahydrofuran (THF), dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).

[0229] Next, in step S73, the particles 582 prepared in step S71 are mixed with the solvent prepared in step S72, the mixture is recovered in step S74, and mixture E-1 is obtained in step S75. A kneader or the like can be used for mixing. For example, a planetary centrifugal mixer or the like can be used as the kneader.

[0230] Next, in step S80, a material 584b that will later become graphene is prepared. Graphene oxide can be used as the material 584b. Alternatively, graphene 583 produced using the flow shown in FIG. 6 can be used.

[0231] Next, in step S81, the mixture E-1 is mixed with the material 584b prepared in step S80, and in step S82, the mixture is recovered to obtain a mixture E-2 (step S86). Note that the mixing may involve stiff kneading (kneading at high viscosity). If stiff kneading is performed, a solvent may be added after stiff kneading to lower the viscosity, and further mixing may be performed.

[0232] Next, in step S87, a binder is prepared. The above-described materials can be used as the binder. In this example, polyimide is used. Note that in step S87, a precursor of the material used as the binder may be prepared. For example, a polyimide precursor is prepared.

[0233] Next, in step S88, mixture E-2 is mixed with the binder or binder precursor prepared in step S87. Next, in step S89, viscosity is adjusted. Specifically, for example, the same type of solvent as the solvent prepared in step S72 is prepared and added to the mixture obtained in step S88. By adjusting the viscosity, for example, it may be possible to adjust the thickness, density, etc. of the electrode obtained in the subsequent step S97.

[0234] Next, the mixture whose viscosity has been adjusted in step S89 is mixed in step S90 and recovered in step S91 to obtain mixture E-3 (step S92). The mixture E-3 obtained in step S92 is called, for example, a slurry.

[0235] Next, in step S93, a current collector is prepared.

[0236] Next, in step S94, the mixture E-3 is applied to the current collector prepared in step S93. For application, a slot die method, a gravure method, a blade method, or a combination thereof can be used. Alternatively, a continuous coater or the like can be used for application.

[0237] Next, in step S95, the first heating is performed. The first heating volatilizes the solvent. The first heating is performed at a temperature in the range of 50° C. to 200° C., preferably 60° C. to 150° C.

[0238] For example, heat treatment may be performed on a hot plate in an air atmosphere at 30°C or higher and 70°C or lower for 10 minutes or longer, and then heat treatment may be performed in a reduced pressure environment at room temperature or higher and 100°C or lower for 1 hour or longer and 10 hours or shorter.

[0239] Alternatively, the heat treatment may be performed using a drying furnace, etc. When a drying furnace is used, the heat treatment may be performed at a temperature of 30° C. or higher and 120° C. or lower for 30 seconds or longer and 2 hours or shorter.

[0240] Alternatively, the temperature may be increased stepwise. For example, after heat treatment at 60° C. or lower for 10 minutes or less, heat treatment may be further performed at 65° C. or higher for 1 minute or more.

[0241] Next, in step S96, a second heating is performed. When polyimide is used as the binder, it is preferable that a cyclization addition reaction of the polyimide occurs during the second heating. Furthermore, a dehydration reaction of the polyimide may occur during the second heating. Alternatively, a dehydration reaction of the polyimide may occur during the first heating. Furthermore, a cyclization reaction of the polyimide may occur during the first heating. Furthermore, it is preferable that a reduction reaction of the material 584b occurs during the second heating.

[0242] In step S97, an electrode is obtained in which an active material layer is provided on a current collector. The electrode obtained in step S97 is an electrode including graphene.

[0243] The thickness of the active material layer thus formed is preferably, for example, 5 μm or more and 300 μm or less, more preferably 10 μm or more and 150 μm or less. The amount of active material carried in the active material layer is preferably, for example, 2 mg / cm. 2 50mg / cm or more 2 The following is fine.

[0244] The active material layer may be formed on both sides of the current collector, or on only one side thereof, or both sides may have regions where the active material layer is partially formed.

[0245] After the solvent is evaporated from the active material layer, pressing may be carried out by a compression method such as a roll press method or a plate press method, etc. Heat may be applied during pressing.

[0246] By manufacturing an electrode using the manufacturing method of one embodiment of the present invention, a three-dimensional conductive path using a plurality of graphenes can be formed in an active material layer of the electrode. In addition, a plurality of graphenes can be formed in a mesh-like shape in the electrode.

[0247] <Regarding Graphene> Graphene according to one embodiment of the present invention can be obtained in step S53 of FIG. 6A , step S53b of FIG. 6B , and step S97 of FIG. 7 . The graphene obtained in each step may have different fluorine concentrations and different pore frequencies. Furthermore, the graphene obtained in each step may have different oxygen concentrations.

[0248] At least a portion of the graphene of one embodiment of the present invention obtained in step S53b of FIG. 6B covers, for example, particle 582.

[0249] The graphene according to one embodiment of the present invention obtained in step S97 of Fig. 7 is contained inside the electrode. At least a portion of the graphene according to one embodiment of the present invention obtained in step S97 of Fig. 7 covers, for example, particles 582. A plurality of the graphene according to one embodiment of the present invention obtained in step S97 of Fig. 7 constitute a three-dimensional structure within the electrode.

[0250] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0251] Embodiment 2 In this embodiment, an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described.

[0252] The following materials have a layered rock salt crystal structure, and are listed below as examples: LiMO 2 The following shows an example of a method for producing a material represented by the formula (1): The metal M includes a metal Me1. The metal Me1 is one or more metals including cobalt. The metal M may further include a metal X in addition to the metal Me1. The metal X is one or more metals selected from magnesium, calcium, zirconium, lanthanum, barium, copper, potassium, sodium, and zinc.

[0253] 8A, a lithium source and a transition metal source are prepared as materials for lithium and transition metal. Note that in the drawing, the transition metal source is illustrated as a Me1 source.

[0254] As the lithium source, for example, lithium carbonate, lithium fluoride, etc. can be used.

[0255] The transition metal source may be, for example, at least one of manganese, cobalt, and nickel. For example, the transition metal source may be a combination of cobalt alone, nickel alone, cobalt and manganese, cobalt and nickel, or cobalt, manganese, and nickel.

[0256] It is preferable to use a high-purity material as the transition metal source used in the synthesis. Specifically, the purity of the material is 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N (99.995%) or higher, and even more preferably 5N (99.999%) or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.

[0257] In addition, it is preferable that the transition metal source has high crystallinity. For example, it is preferable that the transition metal source has single crystal grains. The crystallinity of the transition metal source can be evaluated, for example, from a TEM (transmission electron microscope) image, a STEM (scanning transmission electron microscope) image, a HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) image, an ABF-STEM (annular bright-field scanning transmission electron microscope) image, etc. Furthermore, X-ray diffraction (XRD), electron diffraction, neutron diffraction, etc. can also be used to evaluate the crystallinity of the transition metal source. Note that the above-mentioned crystallinity evaluation can be applied not only to the transition metal source, but also to the evaluation of the crystallinity of primary particles or secondary particles.

[0258] Furthermore, when using metals capable of forming a layered rock-salt composite oxide, it is preferable to set the mixing ratio of cobalt, manganese, and nickel within a range that allows a layered rock-salt crystal structure to be formed. Furthermore, an additional element X may be added to these transition metals within a range that allows a layered rock-salt crystal structure to be formed. An example of the process of adding the additional element X is shown in FIG. 8B. In step S11, a lithium source, a transition metal source, and an additional element X source are prepared, and then step S12 is performed.

[0259] The additive element X can be one or more selected from magnesium, calcium, zirconium, lanthanum, barium, titanium, yttrium, nickel, aluminum, cobalt, manganese, vanadium, iron, chromium, niobium, copper, potassium, sodium, zinc, chlorine, fluorine, hafnium, silicon, sulfur, phosphorus, boron, and arsenic. In addition to the above elements, bromine and beryllium may also be used as the additive element X. However, since bromine and beryllium are toxic to living organisms, it is preferable to use the additive element X described above.

[0260] The transition metal source may be an oxide or hydroxide of the metals exemplified above, and the cobalt source may be, for example, cobalt oxide or cobalt hydroxide.

[0261] As the manganese source, manganese oxide, manganese hydroxide, etc. can be used. As the nickel source, nickel oxide, nickel hydroxide, etc. can be used. As the aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.

[0262] <Step S12> Next, in step S12, the lithium source and transition metal source are crushed and mixed. Crushing and mixing can be performed by dry or wet methods. It is particularly preferable to perform crushing using dehydrated acetone with a purity of 99.5% or higher, in which the water content is reduced to 10 ppm or less. Note that, in this specification, the term "crushing" may be interpreted as "pulverization." Mixing can be performed using, for example, a ball mill or a bead mill. When using a ball mill, it is preferable to use zirconia balls as the media. When using a ball mill or a bead mill, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media or materials. For example, the process may be performed at a peripheral speed of 838 mm / s (rotation speed: 400 rpm, ball mill diameter: 40 mm). Furthermore, using the dehydrated acetone described above in crushing and mixing can reduce impurities that may be mixed into the materials.

[0263] <Step S13> Next, in step S13, the mixed materials are heated. The heating temperature in this step is preferably 800°C or higher and lower than 1100°C, more preferably 900°C or higher and 1000°C or lower, and even more preferably about 950°C. If the temperature is too low, the decomposition and melting of the lithium source and transition metal source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to factors such as lithium transpiration from the lithium source and / or excessive reduction of the metal used as the transition metal source. For example, when cobalt is used as the transition metal, defects may occur in which cobalt becomes divalent.

[0264] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an atmosphere with little water, such as dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). For example, the heating may be carried out in an atmosphere with a dew point of -93°C. The heating may also be carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.

[0265] For example, when heating at 1000°C for 10 hours, it is preferable to increase the temperature by 200°C / h and to supply dry air at a flow rate of 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable to set the cooling time from the specified temperature to room temperature to 10 hours or more and 50 hours or less. However, cooling to room temperature in step S13 is not essential.

[0266] The crucible used for heating in step S13 is preferably made of a material that does not easily release impurities. For example, a crucible made of alumina with a purity of 99.9% may be used.

[0267] Furthermore, when recovering the material after heating in step S13, it is preferable to transfer the material from the crucible to a mortar and then recover it, since this prevents impurities from being mixed into the material. It is also preferable that the mortar be made of a material that does not easily release impurities. Specifically, it is preferable to use a mortar made of alumina with a purity of 90% or more, preferably 99% or more. Note that conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.

[0268] <Step S14> Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be manufactured (Step S14). Note that the positive electrode active material 100 is a composite oxide containing lithium, a transition metal, and oxygen (LiMO). 2 However, the positive electrode active material of one embodiment of the present invention may be represented by LiMO. 2 The composition is not strictly limited to Li:M:O=1:1:2, so long as it has a crystalline structure of a lithium composite oxide represented by the formula:

[0269] By using a high-purity transition metal source material for synthesis and preparing a cathode active material through a synthesis process with minimal impurity contamination, a material with a low impurity concentration, in other words, a highly purified material, can be obtained. Furthermore, the cathode active material obtained by this method for preparing a cathode active material has high crystallinity. Furthermore, the cathode active material obtained by the method for preparing a cathode active material according to one embodiment of the present invention can increase the capacity and / or reliability of a secondary battery.

[0270] [Method 2 for Manufacturing Positive Electrode Active Material] Next, another example of a method for manufacturing a positive electrode active material according to one embodiment of the present invention will be described with reference to FIGS.

[0271] 9, steps S11 to S14 are performed in the same manner as in FIG. 8A to obtain a composite oxide containing lithium, a transition metal, and oxygen (LiMO 2 ) to prepare.

[0272] It is also possible to use a pre-synthesized composite oxide in step S14. In this case, steps S11 to S13 can be omitted. When preparing a pre-synthesized composite oxide, it is preferable to use a high-purity material. The purity of the material is 99.5% or more, preferably 99.9% or more, and more preferably 99.99% or more.

[0273] A heating step may be provided between step S14 and the next step S20. This heating can smooth the surface of the composite oxide, for example. For example, the heating may be performed under the same atmosphere and temperature conditions as step S33, with a treatment time shorter than that of step S33. A smooth surface refers to a surface with few irregularities, a rounded overall surface, and rounded corners. Furthermore, a smooth surface refers to a state in which there is little foreign matter adhering to the surface. Foreign matter is considered to be a cause of irregularities, so it is preferable that it does not adhere to the surface.

[0274] <Step S20> In step S20 of Fig. 9, a source of the additive element X is prepared. The materials described above can be used as the source of the additive element X. Furthermore, a plurality of elements may be used as the additive element X. The additive element X can be added by a method such as a solid-phase method, a liquid-phase method including a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, or a PLD (pulsed laser deposition) method.

[0275] Here, a magnesium source (Mg source) and a fluorine source (F source) are prepared as sources of the additional element X. A lithium source may also be prepared in addition to the magnesium source and the fluorine source.

[0276] As the magnesium source, for example, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used.

[0277] Examples of fluorine sources include lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 2 ), lanthanum fluoride (LaF 3 ) Sodium aluminum hexafluoride (Na 3 AlF 6 The fluorine source is not limited to a solid, and may be, for example, fluorine (F 2 ), fluorocarbon, sulfur fluoride, oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 2 F), etc., may be used and mixed into the atmosphere in the heating step described below. A mixture of multiple fluorine sources may also be used. Among these, lithium fluoride is preferred because it has a relatively low melting point of 848°C and is easily melted in the heating step described below.

[0278] Examples of lithium sources that can be used include lithium fluoride and lithium carbonate. That is, lithium fluoride can be used as both a lithium source and a fluorine source. Magnesium fluoride can be used as both a fluorine source and a magnesium source.

[0279] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 Lithium fluoride (LiF) and magnesium fluoride (MgF) 2 is LiF:MgF 2Mixing lithium fluoride (LiF) and magnesium fluoride (MgF) in a molar ratio of about 65:35 results in the greatest effect of lowering the melting point (Non-Patent Document 2). On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, 2 The molar ratio of LiF:MgF 2 =k:1 (0≦k≦1.9), and LiF:MgF 2 =k:1 (0.1≦k≦0.5) is more preferable, and LiF:MgF 2 = k: 1 (k = 0.33 or its vicinity) is more preferable. In this specification, "k = 0.33 or its vicinity" refers to a value that is greater than 0.9 times and smaller than 1.1 times the value.

[0280] When the subsequent mixing and crushing steps are performed in a wet system, a solvent is prepared. As the solvent, it is preferable to use a protic solvent that does not easily react with lithium, such as a ketone such as acetone, an alcohol such as ethanol or isopropanol, ether, dioxane, acetonitrile, or N-methyl-2-pyrrolidone (NMP).

[0281] Next, the above materials are mixed and crushed. Mixing can be performed by dry or wet methods, but wet methods are preferred because they allow for smaller crushing. For example, a ball mill or a bead mill can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. The conditions for the ball mill or bead mill can be the same as those for step S12.

[0282] Next, the crushed and mixed material is recovered to obtain the source of the additional element X. Note that this source of the additional element X may be called a mixture because it is made of a plurality of materials.

[0283] The mixture preferably has a D50 (median diameter) of 600 nm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less. Such a finely divided mixture facilitates uniform adhesion of the mixture to the surface of the composite oxide particles when mixed with a composite oxide containing lithium, a transition metal, and oxygen in a subsequent process. Uniform adhesion of the mixture to the surface of the composite oxide particles is preferred because it facilitates thorough distribution of halogen and magnesium near the surface of the composite oxide particles after heating. If there are regions near the surface that do not contain halogen and magnesium, the above-mentioned O3'-type crystal structure may be difficult to obtain in a charged state.

[0284] Although the above example illustrates a method of mixing two types of materials, the present invention is not limited to this. For example, the additive element X source may be prepared by mixing four types of materials (a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source)). Alternatively, the additive element X source may be prepared using a single material, i.e., one type of material. Nickel oxide, nickel hydroxide, etc. may be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. may be used as the aluminum source.

[0285] <Step S31> Next, in step S31 of FIG. 9, the LiMO obtained in step S14 is 2 and a source of the additional element X. The ratio of the number of transition metal atoms M in the composite oxide containing lithium, transition metal, and oxygen to the number of magnesium atoms Mg in the additional element X is preferably M:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).

[0286] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the composite oxide particles. For example, it is preferable to use conditions with a lower rotation speed or a shorter time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media.

[0287] In this embodiment, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.

[0288] <Step S32> Next, in step S32 of FIG. 9, the mixed materials are collected to obtain a mixture 903.

[0289] Although this embodiment describes a method of adding a mixture of lithium fluoride and magnesium fluoride to lithium cobalt oxide with few impurities, one embodiment of the present invention is not limited thereto. Instead of the mixture 903 in step S32, a starting material for lithium cobalt oxide to which a magnesium source, a fluorine source, and the like have been added and heated may be used. In this case, there is no need to separate the steps S11 to S14 from the steps S21 to S23, which simplifies the process and increases productivity.

[0290] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be used. If lithium cobalt oxide to which magnesium and fluorine have been added is used, the steps up to step S32 can be omitted, which is simpler.

[0291] Alternatively, a magnesium source and a fluorine source may be further added to lithium cobalt oxide to which magnesium and fluorine have been added in advance.

[0292] <Step S33> Next, in step S33, the mixture 903 is heated in an atmosphere containing oxygen. The heating is preferably performed in such a manner that the particles of the mixture 903 do not stick to each other.

[0293] It is preferable that the additive be added uniformly across the entire surface of the particle. However, if the particles of the mixture 903 stick together during heating, the additive may be added unevenly to only a portion of the entire surface. Furthermore, even though the surface of the particle is preferably smooth and has few irregularities, if the particles stick together, the surface may become more irregular, potentially increasing defects such as cracks and / or fissures. This is thought to be due to the fact that the adhesion of the mixture 903 to each other reduces the contact area with oxygen in the atmosphere and blocks the route for the additive to diffuse.

[0294] The heating in step S33 may be performed using a rotary kiln. The heating in a rotary kiln may be performed while stirring, whether it is a continuous or batch type. The heating in step S33 may be performed using a roller hearth kiln.

[0295] The heating temperature in step S33 is LiMO 2 The temperature must be equal to or higher than the temperature at which the reaction between LiMO and the source of the added element X proceeds. 2 The temperature may be lower than the melting point of these materials. For example, in the case of oxides, the melting point T m 0.757 times [K] (Tammann temperature T d ) or more, solid-phase diffusion occurs. Therefore, the heating temperature in step S33 may be, for example, 500° C. or more.

[0296] However, if the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts, the reaction proceeds more easily, which is preferable. For example, LiF and MgF are used as the source of the additive element X. 2 When LiF and MgF 2 Since the eutectic point of is around 742°C, it is preferable to set the heating temperature in step S33 to 742°C or higher.

[0297] Also, LiCoO 2 :LiF:MgF 2In the mixture 903 in which the molar ratio is 100:0.33:1, an endothermic peak is observed around 830° C. in differential scanning calorimetry (DSC measurement). Therefore, the heating temperature is preferably 830° C. or higher.

[0298] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.

[0299] However, the heating temperature is LiMO 2 Decomposition temperature of LiCoO 2 In addition, at temperatures close to the decomposition temperature, a small amount of LiMO 2 Therefore, the heating temperature in step S33 is preferably less than 1130°C, more preferably 1000°C or less, even more preferably 950°C or less, and even more preferably 900°C or less.

[0300] Therefore, the heating temperature in step S33 is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and even more preferably 500°C or higher and 900°C or lower. Also, the heating temperature is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, the heating temperature is preferably 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower.

[0301] Furthermore, when the mixture 903 is heated, it is preferable to control the partial pressure of fluorine or fluoride in the atmosphere within an appropriate range.

[0302] In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. 2 The temperature can be lowered to a temperature below the decomposition temperature of the compound, for example, 742° C. to 950° C., and additives such as magnesium can be distributed near the surface, making it possible to produce a positive electrode active material with good characteristics.

[0303] However, since LiF has a lower specific gravity in a gaseous state than oxygen, when LiF volatilizes due to heating, the amount of LiF in the mixture 903 decreases. This weakens the function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiMO 2 There is also a possibility that Li and F on the surface may react to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, it is still necessary to suppress volatilization.

[0304] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903.

[0305] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln to heat the mixture 903. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln.

[0306] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by, for example, placing a lid on a container containing the mixture 903 .

[0307] It is preferable that the heating is performed for an appropriate time. The heating time depends on the heating temperature, the LiMO 2 The temperature and time required for the reaction may vary depending on the particle size, composition, etc. Small particles may be more suitable at lower temperatures or for shorter times than large particles.

[0308] For example, when the average particle size (D50) of the composite oxide in step S14 of Fig. 9 is about 12 µm, the heating temperature is preferably, for example, 600°C or higher and 950°C or lower. The heating time is, for example, preferably 3 hours or longer, more preferably 10 hours or longer, and even more preferably 60 hours or longer.

[0309] On the other hand, when the average particle size (D50) of the composite oxide in step S14 is about 5 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 2 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.

[0310] <Step S34> Next, the heated material is recovered to produce the positive electrode active material 100. At this time, it is preferable to further sieve the recovered particles. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced (Step S34).

[0311] [Method 3 for Manufacturing Positive Electrode Active Material] Next, another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.

[0312] In FIG. 10, steps S11 to S14 are performed in the same manner as in FIG. 8A to obtain a composite oxide containing lithium, a transition metal, and oxygen (LiMO 2 ) to prepare.

[0313] Alternatively, a composite oxide containing lithium, a transition metal, and oxygen that has been synthesized in advance may be used in step S14, in which case steps S11 to S13 can be omitted.

[0314] 9, a heating step may be provided between step S14 and step S20. The heating may be performed using the same atmosphere and temperature conditions as step S33, but for a shorter processing time than step S33.

[0315] <Step S20a> In step S20a of Fig. 10, a source of the additive element X1 is prepared. The source of the additive element X1 can be selected from the additive elements X described above. For example, one or more selected from magnesium, fluorine, and calcium can be suitably used as the additive element X1. The additive element X1 can be added by a solid-phase method, a liquid-phase method such as a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, a PLD (pulsed laser deposition) method, or the like.

[0316] Here, a magnesium source (Mg source) and a fluorine source (F source) are prepared as the first additional element X1. Next, referring to step S20 shown in Fig. 9, the magnesium source and the fluorine source are appropriately subjected to pulverization, mixing, heating, etc., to obtain an additional element source (X1 source).

[0317] 9. Steps S31 to S33 shown in FIG. 10 can be fabricated in the same manner as steps S31 to S33 shown in FIG.

[0318] <Step S34a> Next, the material heated in step S33 is recovered to produce a composite oxide.

[0319] <Step S40> In step S40 of FIG. 10 , a source of the additive element X2 is prepared. The source of the additive element X2 can be selected from the additive elements X described above. For example, one or more elements selected from nickel, titanium, boron, zirconium, and aluminum can be suitably used as the additive element X2. In this embodiment, nickel and aluminum are used as the additive element X2. The additive element X2 can be added by a solid-phase method, a liquid-phase method such as a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, a PLD (pulsed laser deposition) method, or the like.

[0320] For step S40 shown in FIG. 10, refer to step S20 shown in FIG. 9, and grinding, mixing, heating, etc. can be appropriately performed to obtain the additive element source (X2 source).

[0321] Furthermore, when a plurality of elements are used as the second additive element source, each element may be prepared by independently pulverizing the elements, resulting in the independent preparation of a plurality of second additive element sources (X2 sources) in step S40.

[0322] Here, when the sol-gel method is used to add the additive element X2, a solvent to be used in the sol-gel method is prepared in addition to the additive element X2 source. For example, a metal alkoxide can be used as the metal source for the sol-gel method, and alcohol can be used as the solvent. For example, when aluminum is added, aluminum isopropoxide can be used as the metal source, and isopropanol (2-propanol) can be used as the solvent. For example, when zirconium is added, zirconium (IV) tetrapropoxide can be used as the metal source, and isopropanol can be used as the solvent.

[0323] <Steps S51 to S53> Next, step S51 in FIG. 10 is a step of mixing the composite oxide produced in step S34a with the additive element X2 source produced in step S40. Note that step S51 in FIG. 10 can be processed in a manner similar to step S31 shown in FIG. 9. Also, step S52 in FIG. 10 can be processed in a manner similar to step S32 shown in FIG. 9. Note that the material produced in step S52 in FIG. 10 is a mixture 904. Mixture 904 contains the material of mixture 903 as well as the additive element X2 source added in step S40. Also, step S53 in FIG. 10 can be processed in a manner similar to step S33 shown in FIG. 9.

[0324] <Step S54> Next, the heated material is recovered to produce the positive electrode active material 100. At this time, it is preferable to further sieve the recovered particles. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced (Step S54).

[0325] As shown in Figure 10, by separating the steps of introducing the transition metal, the additive element X1, and the additive element X2, it may be possible to change the depth profile of each element. For example, the concentration of the additive can be increased near the surface compared to the interior of the particle. Furthermore, using the number of transition metal atoms as a reference, the ratio of the number of atoms of the additive element to the reference can be made higher near the surface than in the interior.

[0326] Furthermore, by using a high-purity material as the transition metal source for synthesis, and employing a process with minimal impurity contamination during synthesis, thoroughly eliminating impurity contamination from the transition metal source and during synthesis, and controlling and introducing a desired additive element (additive element X, additive element X1, or additive element X2) into the positive electrode active material, a positive electrode active material can be obtained in which regions with low impurity concentrations and regions with the additive element introduced are controlled. Furthermore, a positive electrode active material with high crystallinity can be obtained. Furthermore, the positive electrode active material obtained by the method for manufacturing a positive electrode active material according to one embodiment of the present invention can increase the capacity and / or reliability of a secondary battery.

[0327] [Method 4 for Producing Positive Electrode Active Material] Next, a method for carrying out the present invention, which is different from Methods 1 to 3 for Producing Positive Electrode Active Material, will be described.

[0328] As described above, the additive element X may be added to the composite oxide within a range that allows a layered rock salt type crystal structure to be formed, and in Fig. 11, steps S11 to S34a are performed in the same manner as in Fig. 10. In this production method 4, a step of adding the second additive element (X2) in two or more separate steps will be described.

[0329] 11, one of the second additive element sources (hereinafter referred to as the X2a source) is prepared. The X2a source can be selected from the additive elements X described in step S20 shown in FIG. 9. For example, the additive element X2a can be one or more selected from nickel, titanium, boron, zirconium, and aluminum.

[0330] The additive element X2a can be added by a solid phase method, a liquid phase method such as a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, a PLD (pulsed laser deposition) method, or the like.

[0331] FIG. 11 illustrates an example in which nickel is used as the additional element X2a.

[0332] In step S40a shown in Fig. 11, the second additional element source (X2a source) can be obtained by appropriately performing pulverization, mixing, heating, etc. with reference to step S20 shown in Fig. 9. For example, a nickel source is obtained as the second additional element source (X2a source) using a solid-phase method.

[0333] When a plurality of additive element sources are prepared, they may be crushed independently.

[0334] <Step S40b> Step S40b shown in FIG. 11 allows obtaining a source of the second additive element (hereinafter referred to as the X2b source). For example, the second additive element source (X2b source) is obtained using a sol-gel method. Unlike step S40a, when preparing the source using the sol-gel method, it is preferable to prepare the source as an independent process. The manufacturing process of the second additive element source (X2b source) using the sol-gel method will be described.

[0335] When using the sol-gel method, in addition to the second additive element (X2b), a solvent to be used in the sol-gel method is prepared. For example, a metal alkoxide can be used as the metal source for the sol-gel method, and for example, alcohol can be used as the solvent. When preparing an aluminum source, aluminum isopropoxide can be used as the aluminum alkoxide, and when preparing a zirconium source, zirconium isopropoxide can be used as the zirconium alkoxide, and isopropanol can be used as the solvent.

[0336] Next, aluminum alkoxide, zirconium alkoxide, and isopropanol are mixed (stirred). A sol-gel reaction may be allowed to proceed here, or the sol-gel reaction may be allowed to proceed in the next step. If the sol-gel reaction is allowed to proceed, heating may be applied during mixing. In this way, a mixture (also referred to as a mixed liquid) containing an aluminum source and a zirconium source is prepared as a second additive element source (X2b source).

[0337] 11 can be performed under the same conditions as those of steps S31 to S33 shown in Fig. 9. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced in step S54. The sol-gel reaction can be promoted in step S53.

[0338] This embodiment can be used in combination with other embodiments.

[0339] 12A , an example of a secondary battery according to one embodiment of the present invention will be described. The secondary battery includes an outer casing (not shown), a positive electrode 503, a negative electrode 506, a separator 507, and an electrolyte containing a lithium salt or the like. The separator 507 is provided between the positive electrode 503 and the negative electrode 506.

[0340] The positive electrode 503 includes a positive electrode active material. The positive electrode 503 also includes a positive electrode active material layer 502 provided over a positive electrode current collector 501. The positive electrode active material layer 502 includes, for example, a positive electrode active material, a conductive agent, and a binder. The electrode described in the above embodiment can be used as the positive electrode of one embodiment of the present invention.

[0341] The negative electrode 506 includes a negative electrode active material. The negative electrode 506 also includes a negative electrode active material layer 505 provided over a negative electrode current collector 504. The negative electrode active material layer 505 includes, for example, a negative electrode active material, a conductive agent, and a binder. The electrode described in the above embodiment can be used as the negative electrode of one embodiment of the present invention.

[0342] [Electrolyte] The electrolyte preferably contains a solvent and a metal salt that serves as a carrier ion. The solvent for the electrolyte is preferably an aprotic organic solvent, and examples thereof include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, and sultone, or any combination and ratio of two or more of these.

[0343] Furthermore, by using one or more flame-retardant and non-volatile ionic liquids (room-temperature molten salts) as the electrolyte solvent, it is possible to prevent the secondary battery from exploding or catching fire even if the internal temperature rises due to an internal short circuit or overcharging of the secondary battery. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of organic cations used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, imidazolium cations, and aromatic cations such as pyridinium cations. Examples of anions used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.

[0344] The salt to be dissolved in the solvent is, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4, LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO 2 ), LiN(C 2 F 5 SO 2 ) 2 These lithium salts may be used alone or in any combination and ratio of two or more of them.

[0345] The electrolyte used in the secondary battery is preferably a highly purified electrolytic solution with low content of granular dust and elements other than the constituent elements of the electrolyte (hereinafter simply referred to as "impurities"). Specifically, it is preferable that the weight ratio of impurities to the electrolyte be 1% or less, preferably 0.1% or less, and more preferably 0.01% or less.

[0346] In addition, additives such as vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), or dinitrile compounds such as succinonitrile and adiponitrile may be added to the electrolyte. The concentration of the added material may be, for example, 0.1 wt % to 5 wt % of the total solvent. VC and LiBOB are particularly preferred because they easily form a good coating.

[0347] A solution containing a solvent and a salt that serves as carrier ions may be called an electrolyte.

[0348] A polymer gel electrolyte in which a polymer is swollen with an electrolytic solution may also be used.

[0349] The use of a polymer gel electrolyte improves safety against leakage, etc. It also enables the secondary battery to be made thinner and lighter.

[0350] Examples of polymers that can be used to form gels include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel.

[0351] Examples of polymers that can be used include polymers having a polyalkylene oxide structure, such as polyethylene oxide (PEO), PVDF, and polyacrylonitrile. Copolymers containing these can also be used. For example, PVDF-HFP, a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The polymer formed may also have a porous shape.

[0352] In addition, solid electrolytes containing inorganic materials such as sulfides and oxides, and solid electrolytes containing polymeric materials such as polyethylene oxide (PEO) can be used. When a solid electrolyte is used, the installation of one or more separators and spacers is unnecessary. Furthermore, since the entire battery can be solidified, the risk of leakage is eliminated, dramatically improving safety.

[0353] [Separator] The separator 507 may be made of, for example, paper, nonwoven fabric, glass fiber, ceramics, etc. Alternatively, it may be made of nylon (polyamide), vinylon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, polyurethane, polypropylene, polyethylene, etc. The separator is preferably processed into an envelope shape and disposed so as to encase either the positive electrode or the negative electrode.

[0354] Furthermore, a polymer film containing, for example, polypropylene, polyethylene, polyimide, etc. can be used for the separator 507. Polyimide has good wettability with ionic liquids, and may be a more preferable material for the separator 507 in some cases.

[0355] Polymer films containing polypropylene, polyethylene, etc. can be produced by either the dry method or the wet method. The dry method involves heating and stretching a polymer film containing polypropylene, polyethylene, polyimide, etc., to create gaps between the crystals and create fine holes. The wet method involves mixing a solvent into the resin beforehand, forming it into a film, and then extracting the solvent to create holes.

[0356] The left diagram of Fig. 12B shows an enlarged view of region 507a as an example of separator 507 (when produced by a wet method). In this example, a structure in which multiple holes 587 are formed in polymer film 588 is shown. The right diagram of Fig. 12B shows an enlarged view of region 507b as another example of separator 507 (when produced by a dry method). In this example, a structure in which multiple holes 585 are formed in polymer film 586 is shown.

[0357] The pore diameter of the separator may differ between the surface layer portion of the surface facing the positive electrode and the surface layer portion of the surface facing the negative electrode after charge and discharge. In this specification, the surface layer portion of the separator is preferably, for example, a region within 5 μm, more preferably within 3 μm, from the surface.

[0358] The separator may have a multi-layer structure, for example, a structure in which two types of polymer materials are laminated.

[0359] Alternatively, a structure can be used in which a ceramic material, a fluorine material, a polyamide material, or a mixture thereof is coated on a polymer film having, for example, polypropylene, polyethylene, polyimide, etc. Alternatively, a structure can be used in which a ceramic material, a fluorine material, a polyamide material, or a mixture thereof is coated on a nonwoven fabric, for example. Polyimide has good wettability with ionic liquids and may be more preferable as a coating material.

[0360] As the fluorine-based material, for example, PVDF, polytetrafluoroethylene, etc. can be used.

[0361] Examples of polyamide-based materials that can be used include nylon and aramid (meta-aramid, para-aramid).

[0362] [Exterior Body] The exterior body of the secondary battery can be made of one or more materials selected from a metal material such as aluminum and a resin material. A film-like exterior body can also be used. Examples of the film include a three-layer structure film in which a thin, flexible metal film such as aluminum, stainless steel, copper, or nickel is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film such as a polyamide resin or polyester resin is further provided on the thin metal film as the outer surface of the exterior body.

[0363] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0364] Embodiment Mode 4 In this embodiment mode, a method for manufacturing a secondary battery will be described.

[0365] <Method 1 for manufacturing laminated secondary battery> Here, an example of a method for manufacturing a laminated secondary battery whose external views are shown in Figures 13A and 13B will be described with reference to Figures 14A and 14B and Figures 15A and 15B. A secondary battery 500 shown in Figures 13A and 13B has a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511. Note that, as a cross-sectional view of the laminated secondary battery shown in Figure 13A etc., for example, a structure in which a positive electrode, a separator, and a negative electrode are stacked and surrounded by an outer casing can be used, as shown in Figure 18 described later.

[0366] First, a positive electrode 503, a negative electrode 506, and a separator 507 are prepared. Fig. 14A shows an example of the positive electrode 503 and the negative electrode 506. The positive electrode 503 has a positive electrode active material layer 502 on a positive electrode current collector 501. The positive electrode 503 preferably has a tab region where the positive electrode current collector 501 is exposed. The negative electrode 506 has a negative electrode active material layer 505 on a negative electrode current collector 504. The negative electrode 506 preferably has a tab region where the negative electrode current collector 504 is exposed.

[0367] Next, negative electrodes 506, separators 507, and positive electrodes 503 are stacked. Fig. 14B shows the stacked negative electrodes 506, separators 507, and positive electrodes 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. This can also be called a stack consisting of negative electrodes, separators, and positive electrodes.

[0368] Next, the tab regions of the positive electrode 503 are joined together, and the positive electrode lead electrode 510 is joined to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for joining. Similarly, the tab regions of the negative electrode 506 are joined together, and the negative electrode lead electrode 511 is joined to the tab region of the outermost negative electrode.

[0369] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are arranged on the outer casing 509 .

[0370] Next, as shown in Fig. 15A, the exterior body 509 is folded at the portion indicated by the dashed line. Thereafter, the outer periphery of the exterior body 509 is joined. For example, thermocompression bonding or the like may be used for joining. At this time, an area (hereinafter referred to as an inlet 516) that is not joined is provided in a part (or one side) of the exterior body 509 so that the electrolyte 508 can be introduced later.

[0371] Next, as shown in Fig. 15B, electrolyte 508 is introduced into the inside of exterior body 509 through inlet 516 provided in exterior body 509. Introduction of electrolyte 508 is preferably performed under a reduced pressure atmosphere or an inert atmosphere. Finally, inlet 516 is joined. In this manner, laminated secondary battery 500 can be fabricated.

[0372] In the above, the positive electrode lead electrode 510 and the negative electrode lead electrode 511 are led out of the exterior of the outer casing from the same side to produce the secondary battery 500 shown in Fig. 13A. The positive electrode lead electrode 510 and the negative electrode lead electrode 511 can also be led out of the exterior of the outer casing from opposite sides to produce the secondary battery 500 shown in Fig. 13B.

[0373] <Method 2 for manufacturing laminated secondary battery> Next, an example of a method for manufacturing a laminated secondary battery 600 whose external view is shown in Fig. 16 will be described with reference to Fig. 17, Fig. 18, Fig. 19A to Fig. 19D, and Fig. 20A to Fig. 20F. The secondary battery 600 shown in Fig. 16 has a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511. The outer casing 509 is sealed in a region 514.

[0374] The laminated secondary battery 600 can be fabricated using, for example, the manufacturing apparatus shown in FIG. 17 . The manufacturing apparatus 670 shown in FIG. 17 includes a material input chamber 671, a transfer chamber 672, a treatment chamber 673, and a material removal chamber 676. Each chamber can be connected to various exhaust mechanisms depending on the intended use. Each chamber can also be connected to various gas supply mechanisms depending on the intended use. To prevent impurities from entering the manufacturing apparatus 670, an inert gas is preferably supplied to the manufacturing apparatus 670. The gas supplied to the manufacturing apparatus 670 is preferably highly purified using a gas purifier before being introduced into the manufacturing apparatus 670. The material input chamber 671 is a chamber for loading a positive electrode, a separator, a negative electrode, an outer casing, and the like into the manufacturing apparatus 670. The transfer chamber 672 includes a transfer mechanism 680. The treatment chamber 673 includes a stage and an electrolyte dripping mechanism. The component removal chamber 676 is a chamber for removing the fabricated secondary battery to the outside of the manufacturing apparatus 670 .

[0375] The laminated secondary battery 600 is fabricated as follows.

[0376] First, an exterior body 509b is placed on a stage 691 of a processing chamber 673, and then a positive electrode 503 is placed on the exterior body 509b ( FIGS. 19A and 19B ). Next, an electrolyte 515a is dropped onto the positive electrode 503 from a nozzle 694 ( FIGS. 19C and 19D ). FIG. 19D is a cross section corresponding to the dashed-dotted line A-B in FIG. 19C . Note that the illustration of the stage 691 may be omitted to avoid cluttering the drawings. The dropping method may be, for example, any one of a dispensing method, a spray method, an inkjet method, or the like. The electrolyte may be dropped using an ODF (One Drop Fill) method.

[0377] By moving the nozzle 694, the electrolyte 515a can be dropped over the entire surface of the positive electrode 503. Alternatively, by moving the stage 691, the electrolyte 515a may be dropped over the entire surface of the positive electrode 503.

[0378] The electrolyte is preferably dropped from a position at a shortest distance X from the receiving surface that is greater than 0 mm and equal to or less than 1 mm.

[0379] It is also preferable to appropriately adjust the viscosity of the electrolyte dropped from a nozzle, etc. The electrolyte can be dropped from a nozzle if the viscosity of the entire electrolyte is within the range of 0.3 mPa·s to 1000 mPa·s at room temperature (25°C).

[0380] In addition, since the viscosity of the electrolyte changes depending on the temperature of the electrolyte, it is preferable to appropriately adjust the temperature of the electrolyte to be dropped. The temperature of the electrolyte is preferably equal to or higher than the melting point and equal to or lower than the boiling point or flash point of the electrolyte.

[0381] Next, the separator 507 is placed on the positive electrode 503 so as to overlap the entire surface of the positive electrode 503 ( FIG. 20A ). Subsequently, the electrolyte 515b is dripped onto the separator 507 using a nozzle 694 ( FIG. 20B ). Thereafter, the negative electrode 506 is placed on the separator 507 ( FIG. 20C ). The negative electrode 506 is placed on top of the separator 507 so as not to protrude from the separator 507 in a top view. Subsequently, the electrolyte 515c is dripped onto the negative electrode 506 using a nozzle 694 ( FIG. 20D ). The stack of the positive electrode 503, the separator 507, and the negative electrode 506 is then further stacked to produce the stack 512 shown in FIG. 18 . Next, the positive electrode 503, the separator 507, and the negative electrode 506 are sealed with the exterior bodies 509a and 509b ( FIGS. 20E and 20F ).

[0382] In FIG. 18 , the positive electrode and the negative electrode are arranged such that the positive electrode active material layer and the negative electrode active material layer sandwich a separator. Note that in a secondary battery according to one embodiment of the present invention, it is preferable that the negative electrode active material layer has few or no regions that do not face the positive electrode active material layer. When the electrolyte contains an ionic liquid and the negative electrode active material layer has regions that do not face the positive electrode active material layer, the charge / discharge efficiency of the secondary battery may decrease. Therefore, in a secondary battery according to one embodiment of the present invention, for example, it is preferable that the edge of the positive electrode active material layer and the edge of the negative electrode active material layer are as aligned as possible. Therefore, it is preferable that the areas of the positive electrode active material layer and the negative electrode active material layer are aligned as much as possible when viewed from above. Alternatively, it is preferable that the edge of the positive electrode active material layer is located more inward than the edge of the negative electrode active material layer.

[0383] Multiple laminates 512 can be obtained by arranging multiple laminates 512 on exterior body 509b. After sealing exterior bodies 509a and 509b at region 514 so as to surround the active material layer, each laminate 512 is cut outside region 514, thereby separating the multiple secondary batteries into individual ones.

[0384] During sealing, first, a frame-shaped resin layer 513 is formed on the exterior body 509b. Next, at least a portion of the resin layer 513 is irradiated with light under reduced pressure to harden at least a portion of the resin layer 513. Next, sealing is performed in the region 514 by thermocompression bonding or welding under atmospheric pressure. Alternatively, only sealing by thermocompression bonding or welding may be performed without performing the above-described sealing by light irradiation.

[0385] Although Figure 16 shows an example in which the exterior body 509 is sealed on all four sides (sometimes called a four-sided seal), it may also be sealed on three sides (sometimes called a three-sided seal) as shown in Figures 13A and 13B.

[0386] Through the above steps, the laminated secondary battery 600 can be fabricated.

[0387] <Another Secondary Battery and Manufacturing Method 1> An example of a cross-sectional view of a stack of one embodiment of the present invention is shown in Fig. 21. A stack 550 shown in Fig. 21 is manufactured by placing one separator between a positive electrode and a negative electrode while folding the separator.

[0388] In the laminate 550, one separator 507 is folded multiple times so as to be sandwiched between the positive electrode active material layers 502 and the negative electrode active material layers 505. In Fig. 21, six layers of positive electrodes 503 and six layers of negative electrodes 506 are stacked, and therefore the separator 507 is folded at least five times. The separator 507 may not only be provided so as to be sandwiched between the positive electrode active material layers 502 and the negative electrode active material layers 505, but also may have its extending portion further folded so as to bind the plurality of positive electrodes 503 and negative electrodes 506 together with tape or the like.

[0389] In the method for manufacturing a secondary battery of one embodiment of the present invention, after the positive electrode 503 is disposed, an electrolyte can be dropped onto the positive electrode 503. Similarly, after the negative electrode 506 is disposed, an electrolyte can be dropped onto the negative electrode 506. Furthermore, in the method for manufacturing a secondary battery of one embodiment of the present invention, an electrolyte can be dropped onto the separator 507 before folding the separator or after folding the separator 507 and overlapping it with the negative electrode 506 or the positive electrode 503. By dropping the electrolyte onto at least one of the negative electrode 506, the separator 507, and the positive electrode 503, the negative electrode 506, the separator 507, or the positive electrode 503 can be impregnated with the electrolyte.

[0390] 22A has a stack 972 inside a housing 971. A terminal 973b and a terminal 974b are electrically connected to the stack 972. At least a portion of the terminal 973b and at least a portion of the terminal 974b are exposed to the outside of the housing 971.

[0391] The stack body 972 can have a structure in which a positive electrode, a negative electrode, and a separator are stacked. Alternatively, the stack body 972 can have a structure in which a positive electrode, a negative electrode, and a separator are wound, or the like.

[0392] For example, the laminate 972 may be a laminate having a structure in which separators are folded back as shown in FIG.

[0393] An example of a method for manufacturing the stacked body 972 will be described with reference to FIGS. 22B and 22C.

[0394] First, as shown in FIG. 22B , a strip-shaped separator 976 is placed on top of a positive electrode 975a, and then a negative electrode 977a is placed on top of the positive electrode 975a with the separator 976 sandwiched between them. Thereafter, the separator 976 is folded back and placed on top of the negative electrode 977a. Next, as shown in FIG. 22C , a positive electrode 975b is placed on top of the negative electrode 977a with the separator 976 sandwiched between them. In this way, by folding back the separator and arranging the positive electrode and negative electrode in order, a stack 972 can be produced. A structure including a stack produced in this way is sometimes called a "zigzag structure."

[0395] Next, an example of a method for manufacturing the secondary battery 970 will be described with reference to FIGS. 23A to 23C.

[0396] 23A , a positive electrode lead electrode 973a is electrically connected to the positive electrode of the laminate 972. Specifically, for example, a tab region may be provided on each positive electrode of the laminate 972, and each tab region may be electrically connected to the positive electrode lead electrode 973a by welding or the like. In addition, a negative electrode lead electrode 974a is electrically connected to the negative electrode of the laminate 972.

[0397] One stack 972 or a plurality of stacks 972 may be arranged inside the housing 971. Fig. 23B shows an example in which two sets of stacks 972 are prepared.

[0398] Next, as shown in FIG. 23C , the prepared laminate 972 is housed in a housing 971, terminals 973b and 974b are attached, and the housing 971 is sealed. It is preferable that a conductor 973c is electrically connected to each positive electrode lead electrode 973a of the plurality of laminates 972. It is also preferable that a conductor 974c is electrically connected to each negative electrode lead electrode 974a of the plurality of laminates 972. The terminal 973b is electrically connected to the conductor 973c, and the terminal 974b is electrically connected to the conductor 974c. The conductor 973c may have a conductive region and an insulating region. The conductor 974c may have a conductive region and an insulating region.

[0399] A metal material (for example, aluminum) can be used for the housing 971. In the case where a metal material is used for the housing 971, the surface of the housing 971 is preferably covered with resin or the like. Alternatively, a resin material can be used for the housing 971.

[0400] It is preferable to provide a safety valve, an overcurrent protection element, or the like in the housing 971. The safety valve is a valve that releases gas when the pressure inside the housing 971 reaches a predetermined level in order to prevent the battery from exploding.

[0401] <Another Secondary Battery and Manufacturing Method 2> Fig. 24C shows an example of a cross-sectional view of a secondary battery of another embodiment of the present invention. A secondary battery 560 shown in Fig. 24C is manufactured using the stack 130 shown in Fig. 24A and the stack 131 shown in Fig. 24B. Note that for clarity, Fig. 24C only shows the stack 130, the stack 131, and the separator 507.

[0402] As shown in FIG. 24A , the laminate 130 includes a positive electrode 503 having positive electrode active material layers on both sides of a positive electrode current collector, a separator 507, a negative electrode 506 having negative electrode active material layers on both sides of a negative electrode current collector, the separator 507, and a positive electrode 503 having positive electrode active material layers on both sides of a positive electrode current collector laminated in this order.

[0403] As shown in FIG. 24B , the laminate 131 includes a negative electrode 506 having a negative electrode active material layer on both sides of a negative electrode current collector, a separator 507, a positive electrode 503 having a positive electrode active material layer on both sides of a positive electrode current collector, the separator 507, and a negative electrode 506 having a negative electrode active material layer on both sides of a negative electrode current collector laminated in this order.

[0404] The method for manufacturing a secondary battery according to one embodiment of the present invention can be applied to manufacturing a stack. Specifically, when the negative electrode 506, the separator 507, and the positive electrode 503 are stacked to manufacture a stack, an electrolyte is dropped onto at least one of the negative electrode 506, the separator 507, and the positive electrode 503. By dropping multiple drops of the electrolyte, the negative electrode 506, the separator 507, or the positive electrode 503 can be impregnated with the electrolyte.

[0405] As shown in FIG. 24C, the plurality of stacks 130 and the plurality of stacks 131 are covered with a wound separator 507 .

[0406] In addition, in the method for manufacturing a secondary battery of one embodiment of the present invention, after the stack 130 is arranged, an electrolyte can be dropped onto the stack 130. Similarly, after the stack 131 is arranged, an electrolyte can be dropped onto the stack 131. Furthermore, before the separator 507 is folded, or after the separator 507 is folded and overlapped with the stack, an electrolyte can be dropped onto the separator 507. By dropping multiple drops of the electrolyte, the stack 130, the stack 131, or the separator 507 can be impregnated with the electrolyte.

[0407] <Another Secondary Battery and Manufacturing Method 3> A secondary battery of another embodiment of the present invention will be described with reference to Fig. 25 and Fig. 26. The secondary battery described here can be called a wound secondary battery, or the like.

[0408] The secondary battery 913 shown in FIG. 25A has a wound body 950 provided with terminals 951 and 952 inside a housing 930. The wound body 950 is immersed in an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 is not in contact with the housing 930 by using an insulating material or the like. Note that in FIG. 25A , for convenience, the housing 930 is shown separated, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a resin material.

[0409] 25B, the housing 930 shown in Fig. 25A may be formed from a plurality of materials. For example, the secondary battery 913 shown in Fig. 25B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housing 930a and the housing 930b.

[0410] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to suppress shielding of the electric field by the secondary battery 913. Note that if the shielding of the electric field by the housing 930a is small, the antenna may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.

[0411] 25C shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 sandwiched therebetween, and the laminated sheet is wound. Note that multiple layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.

[0412] In a method for manufacturing a secondary battery according to one embodiment of the present invention, when the negative electrode 931, the separator 933, and the positive electrode 932 are stacked, an electrolyte is dropped onto at least one of the negative electrode 931, the separator 933, and the positive electrode 932. That is, the electrolyte is preferably dropped onto at least one of the negative electrode 931, the separator 933, and the positive electrode 932 before the laminate sheet is wound. By dropping multiple drops of the electrolyte, the negative electrode 931, the separator 933, or the positive electrode 932 can be impregnated with the electrolyte.

[0413] 26A may be provided as a secondary battery 913 having a wound body 950a. The wound body 950a shown in Fig. 26A includes a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 includes a negative electrode active material layer 931a. The positive electrode 932 includes a positive electrode active material layer 932a.

[0414] The separator 933 has a width wider than the negative electrode active material layer 931 a and the positive electrode active material layer 932 a, and is wound so as to overlap the negative electrode active material layer 931 a and the positive electrode active material layer 932 a. From the standpoint of safety, it is preferable that the negative electrode active material layer 931 a be wider than the positive electrode active material layer 932 a. A wound body 950 a having such a shape is preferable because of its high safety and productivity.

[0415] 26B, the negative electrode 931 is electrically connected to a terminal 951. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 is electrically connected to a terminal 952. The terminal 952 is electrically connected to a terminal 911b.

[0416] 26C , the wound body 950a and the electrolyte are covered by the housing 930 to form the secondary battery 913. It is preferable to provide the housing 930 with a safety valve, an overcurrent protection element, etc. The safety valve opens temporarily only when the internal pressure of the housing 930 exceeds a predetermined value to prevent the battery from exploding.

[0417] 26B, the secondary battery 913 may have a plurality of wound bodies 950a. By using a plurality of wound bodies 950a, the secondary battery 913 can have a larger charge / discharge capacity.

[0418] This embodiment mode can be combined with other embodiment modes as appropriate.

[0419] Embodiment 5 In this embodiment, application examples of a secondary battery according to one embodiment of the present invention will be described with reference to FIGS.

[0420] [Vehicle] First, an example in which the secondary battery of one embodiment of the present invention is applied to an electric vehicle (EV) will be described.

[0421] 27C shows a block diagram of a vehicle having a motor. The electric vehicle is equipped with first batteries 1301a and 1301b as main driving secondary batteries, and a second battery 1311 that supplies power to an inverter 1312 that starts the motor 1304. The second battery 1311 is also called a cranking battery or starter battery. The second battery 1311 only needs to have high output, and does not need to have a large capacity, and the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.

[0422] For example, a secondary battery manufactured using a method for manufacturing a secondary battery according to one embodiment of the present invention can be used for one or both of the first batteries 1301a and 1301b.

[0423] In this embodiment, an example is shown in which two first batteries 1301a and 1301b are connected in parallel, but three or more batteries may be connected in parallel. Furthermore, if the first battery 1301a can store sufficient power, the first battery 1301b may be omitted. By configuring a battery pack having multiple secondary batteries, it is possible to extract large amounts of power. The multiple secondary batteries may be connected in parallel, in series, or in series after being connected in parallel. A plurality of secondary batteries is also called a battery pack.

[0424] In addition, in a secondary battery for vehicle use, a service plug or circuit breaker that can cut off high voltage without using tools is provided in the first battery 1301a in order to cut off power from multiple secondary batteries.

[0425] The power of the first batteries 1301a and 1301b is mainly used to rotate the motor 1304, but also supplies power to 42V system (high voltage system) on-board components (such as an electric power steering 1307, a heater 1308, and a defogger 1309) via a DCDC circuit 1306. When a rear motor 1317 is provided for the rear wheels, the first battery 1301a is also used to rotate the rear motor 1317.

[0426] In addition, the second battery 1311 supplies power to 14V (low voltage) in-vehicle components (audio 1313, power windows 1314, lamps 1315, etc.) via the DCDC circuit 1310.

[0427] The first battery 1301a will be described with reference to FIG. 27A.

[0428] 27A shows an example of a large battery pack 1415. One electrode of the battery pack 1415 is electrically connected to the control circuit unit 1320 by a wiring 1421. The other electrode is electrically connected to the control circuit unit 1320 by a wiring 1422. The battery pack may have a configuration in which a plurality of secondary batteries are connected in series.

[0429] A memory circuit including a transistor using an oxide semiconductor may be used for the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor may be referred to as a battery operating system (BTOS) or a battery oxide semiconductor (BTOS).

[0430] The control circuit 1320 detects the terminal voltage of the secondary battery and manages the charge / discharge state of the secondary battery. For example, to prevent overcharging, it can turn off both the output transistor and the cutoff switch of the charging circuit almost simultaneously.

[0431] FIG. 27B shows an example of a block diagram of the battery pack 1415 shown in FIG. 27A.

[0432] The control circuit 1320 includes a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging, a control circuit 1322 for controlling the switch unit 1324, and a voltage measurement unit for the first battery 1301a. The control circuit 1320 sets upper and lower voltage limits for the secondary battery used and limits the upper limit of external current or the upper limit of output current to the external device. The range between the lower and upper voltage limits for the secondary battery is within the recommended voltage range. If the secondary battery falls outside this range, the switch unit 1324 activates and functions as a protection circuit. The control circuit 1320 can also be called a protection circuit because it controls the switch unit 1324 to prevent overcharging or overdischarging. For example, if the control circuit 1322 detects a voltage that could cause overcharging, it turns off the switch unit 1324 to cut off the current. Furthermore, a PTC element may be provided in the charge / discharge path to provide a function for cutting off the current in response to an increase in temperature. The control circuit section 1320 also has an external terminal 1325 (+IN) and an external terminal 1326 (-IN).

[0433] The switch unit 1324 can be configured by combining one or both of an n-channel transistor and a p-channel transistor. The switch unit 1324 is not limited to a switch having a Si transistor using single crystal silicon, and can be configured by, for example, Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaO z The switch portion 1324 may be formed using a power transistor having gallium oxide (gallium oxide; z is a real number greater than 0). Furthermore, a memory element using an OS transistor can be freely arranged by stacking it on a circuit using a Si transistor, and therefore integration can be easily achieved. Furthermore, an OS transistor can be manufactured using the same manufacturing equipment as a Si transistor, and therefore can be manufactured at low cost. That is, a control circuit portion 1320 using an OS transistor can be stacked on the switch portion 1324 and integrated into a single chip. The volume occupied by the control circuit portion 1320 can be reduced, enabling miniaturization.

[0434] The first batteries 1301a and 1301b mainly supply power to in-vehicle devices of the 42V system (high voltage system), and the second battery 1311 supplies power to in-vehicle devices of the 14V system (low voltage system). A lead-acid battery is often used as the second battery 1311 because of its cost advantage.

[0435] In this embodiment, an example is shown in which lithium ion secondary batteries are used as both the first battery 1301a and the second battery 1311. The second battery 1311 may be a lead storage battery, an all-solid-state battery, or an electric double layer capacitor.

[0436] Furthermore, regenerative energy generated by the rotation of the tire 1316 is sent to the motor 1304 via the gear 1305, and is then sent from the motor controller 1303 or the battery controller 1302 via the control circuit unit 1321 to charge the second battery 1311. Alternatively, the first battery 1301a is charged from the battery controller 1302 via the control circuit unit 1320. Alternatively, the first battery 1301b is charged from the battery controller 1302 via the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is desirable that the first batteries 1301a and 1301b be capable of rapid charging.

[0437] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b. The battery controller 1302 can set charging conditions in accordance with the charging characteristics of the secondary battery used, and can perform rapid charging.

[0438] Although not shown, when an external charger is connected, the charger's outlet or the charger's connection cable is electrically connected to the battery controller 1302. Power supplied from the external charger is charged to the first batteries 1301a and 1301b via the battery controller 1302. Some chargers are provided with a control circuit, and although the functions of the battery controller 1302 may not be used, it is preferable to charge the first batteries 1301a and 1301b via the control circuit unit 1320 to prevent overcharging. The control circuit unit 1320 may also be provided in the connection cable or the charger's connection cable. The control circuit unit 1320 is sometimes called an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. The ECU includes a microcomputer. The ECU uses a CPU or a GPU.

[0439] Next, an example in which the secondary battery of one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.

[0440] When a secondary battery according to one embodiment of the present invention is installed in a vehicle, next-generation clean energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs) can be realized. Furthermore, the secondary battery can also be installed in agricultural machinery such as electric tractors, mopeds including electrically assisted bicycles, motorcycles, electric wheelchairs, electric carts, small or large ships, submarines, aircraft such as fixed-wing aircraft and rotary-wing aircraft, rockets, artificial satellites, space probes or planetary probes, and spacecraft. A large secondary battery can be fabricated by using the method for manufacturing a secondary battery according to one embodiment of the present invention. Therefore, the secondary battery according to one embodiment of the present invention can be suitably used in transportation vehicles.

[0441] 28A to 28E show transportation vehicles using a secondary battery of one embodiment of the present invention. The automobile 2001 shown in FIG. 28A is an electric automobile using an electric motor as a power source for traveling. Alternatively, it is a hybrid automobile that can appropriately select and use an electric motor or an engine as a power source for traveling. When a secondary battery is installed in a vehicle, the secondary battery is installed in one or more locations. The automobile 2001 shown in FIG. 28A includes the battery pack 1415 shown in FIG. 27A. The battery pack 1415 includes a secondary battery module. The battery pack 1415 preferably further includes a charge control device electrically connected to the secondary battery module. The secondary battery module includes one or more secondary batteries.

[0442] Furthermore, automobile 2001 can charge its secondary battery by receiving power from an external charging facility using a plug-in system, a contactless power supply system, or the like. Charging can be performed using a predetermined charging method or connector standard, such as CHAdeMO (registered trademark) or Combo, as appropriate. The charging device may be a charging station installed in a commercial facility or a household power source. For example, plug-in technology can be used to charge the secondary battery installed in automobile 2001 using an external power supply. Charging can be performed by converting AC power to DC power via a conversion device, such as an AC-DC converter.

[0443] Furthermore, although not shown, a power receiving device can be mounted on a vehicle and power can be supplied contactlessly from a ground-based power transmitting device to charge the vehicle. In the case of this contactless power supply method, by incorporating a power transmitting device into a road or an exterior wall, charging can be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method can also be used to transmit and receive power between two vehicles. Furthermore, a solar cell can be installed on the exterior of the vehicle to charge the secondary battery while the vehicle is stopped or moving. For such contactless power supply, an electromagnetic induction method or a magnetic field resonance method can be used.

[0444] 28B shows a large transport vehicle 2002 having an electrically controlled motor as an example of a transport vehicle. The secondary battery module of the transport vehicle 2002 is, for example, a four-cell unit of secondary batteries of 3.5 V to 4.7 V, with 48 cells connected in series for a maximum voltage of 170 V. Apart from the number of secondary batteries constituting the secondary battery module of the battery pack 2201, the transport vehicle 2002 has the same functions as those shown in FIG. 28A, and therefore a description thereof will be omitted.

[0445] FIG. 28C shows, as an example, a large transport vehicle 2003 having an electrically controlled motor. The secondary battery module of the transport vehicle 2003 has, for example, a maximum voltage of 600 V, which is obtained by connecting in series one hundred or more secondary batteries with a voltage of 3.5 V or higher and 4.7 V or lower. Therefore, secondary batteries with small variations in characteristics are required. By using the method for manufacturing a secondary battery according to one embodiment of the present invention, secondary batteries with stable battery characteristics can be manufactured, enabling low-cost mass production from the viewpoint of yield. Furthermore, except for the number of secondary batteries constituting the secondary battery module of the battery pack 2202, the same functions as those in FIG. 28A are provided, and therefore description thereof will be omitted.

[0446] Fig. 28D shows, as an example, an aircraft 2004 having an engine that burns fuel. Since the aircraft 2004 shown in Fig. 28D has wheels for takeoff and landing, it can also be said to be part of a transportation vehicle, and has a battery pack 2203 that includes a secondary battery module formed by connecting multiple secondary batteries and the secondary battery module and a charge control device.

[0447] The secondary battery module of the aircraft 2004 is, for example, eight 4 V secondary batteries connected in series to produce a maximum voltage of 32 V. Other than the number of secondary batteries constituting the secondary battery module of the battery pack 2203, the secondary battery module has the same functions as those shown in Fig. 28A, and therefore a description thereof will be omitted.

[0448] FIG. 28E shows an example of a transport vehicle 2005 for transporting cargo. The transport vehicle 2005 has an electrically controlled motor and performs various tasks by receiving power from a secondary battery constituting a secondary battery module of a battery pack 2204. The transport vehicle 2005 does not necessarily have to be driven by a human driver and can be unmanned via CAN communication or the like. While a forklift is shown in FIG. 28E , this is not a limitation, and a battery pack having a secondary battery according to one embodiment of the present invention can be mounted on industrial machinery that can be operated via CAN communication or the like, such as an automated transporter, a work robot, or a small construction machine.

[0449] 29A is an example of an electric bicycle using the secondary battery of one embodiment of the present invention. The secondary battery of one embodiment of the present invention can be applied to the electric bicycle 2100 shown in Fig. 29A. A power storage device 2102 shown in Fig. 29B includes, for example, a plurality of secondary batteries and a protection circuit.

[0450] The electric bicycle 2100 includes a power storage device 2102. The power storage device 2102 can supply electricity to a motor that assists a rider. The power storage device 2102 is portable and is shown in a state detached from the bicycle in FIG. 29B . The power storage device 2102 includes a plurality of secondary batteries 2101 of one embodiment of the present invention, and a display unit 2103 can display the remaining battery charge and other information. The power storage device 2102 also includes a control circuit 2104 that can control charging or detect an abnormality of the secondary battery, which is an example of one embodiment of the present invention. The control circuit 2104 is electrically connected to the positive electrode and negative electrode of the secondary battery 2101. A small solid-state secondary battery may be provided in the control circuit 2104. Providing a small solid-state secondary battery in the control circuit 2104 also allows power to be supplied to retain data in a memory circuit of the control circuit 2104 for a long period of time. Furthermore, a synergistic effect in terms of safety can be obtained by combining the positive electrode active material 100 of one embodiment of the present invention with a secondary battery using the positive electrode. The secondary battery and the control circuit 2104 in which the positive electrode active material 100 according to one embodiment of the present invention is used for a positive electrode can significantly contribute to preventing accidents such as fires caused by secondary batteries.

[0451] 29C illustrates an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. A scooter 2300 illustrated in FIG. 29C includes a power storage device 2302, a side mirror 2301, and a turn signal light 2303. The power storage device 2302 can supply electricity to the turn signal light 2303. Furthermore, the power storage device 2302, which includes a plurality of secondary batteries each using the positive electrode active material 100 of one embodiment of the present invention in its positive electrode, can have a high capacity and contribute to miniaturization. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery.

[0452] 29C is capable of storing a power storage device 2302 in under-seat storage 2304. The power storage device 2302 can be stored in under-seat storage 2304 even if the under-seat storage 2304 is small.

[0453] [Building] Next, an example in which the secondary battery of one embodiment of the present invention is mounted in a building will be described with reference to FIG.

[0454] 30A includes a power storage device 2612 including a secondary battery with stable battery characteristics obtained by using a manufacturing method for a secondary battery according to one embodiment of the present invention, and a solar panel 2610. The power storage device 2612 is electrically connected to the solar panel 2610 via wiring 2611 or the like. The power storage device 2612 may also be electrically connected to a ground-mounted charging device 2604. The power obtained by the solar panel 2610 can be charged to the power storage device 2612. The power stored in the power storage device 2612 can be charged to a secondary battery of the vehicle 2603 via the charging device 2604. The power storage device 2612 is preferably installed in an underfloor space. By installing the power storage device 2612 in the underfloor space, the space above the floor can be effectively utilized. Alternatively, the power storage device 2612 may be installed on the floor.

[0455] The power stored in the power storage device 2612 can also be supplied to other electronic devices in the house. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the power storage device 2612 can be used as an uninterruptible power supply, allowing the use of electronic devices.

[0456] 30B illustrates an application example of a power storage device according to one embodiment of the present invention. As illustrated in FIG. 30B , a large-sized power storage device 791 obtained by a method for manufacturing a secondary battery according to one embodiment of the present invention is installed in an underfloor space 796 of a building 799.

[0457] A control device 790 is installed in the power storage device 791, and the control device 790 is electrically connected to the distribution board 703, the power storage controller 705 (also called the control device), the display 706, and the router 709 by wiring.

[0458] Electric power is sent from commercial power source 701 to distribution board 703 via service line attachment portion 710. Electric power is also sent to distribution board 703 from power storage device 791 and commercial power source 701, and distribution board 703 supplies the sent electric power to general load 707 and power storage load 708 via outlets (not shown).

[0459] The general load 707 is, for example, an electrical appliance such as a television or a personal computer, and the power storage load 708 is, for example, an electrical appliance such as a microwave oven, a refrigerator, or an air conditioner.

[0460] The power storage controller 705 includes a measurement unit 711, a prediction unit 712, and a planning unit 713. The measurement unit 711 has a function of measuring the amount of power consumed by the general load 707 and the power storage load 708 during a day (e.g., from midnight to midnight). The measurement unit 711 may also have a function of measuring the amount of power of the power storage device 791 and the amount of power supplied from the commercial power source 701. The prediction unit 712 has a function of predicting the amount of power demand to be consumed by the general load 707 and the power storage load 708 during the next day based on the amount of power consumed by the general load 707 and the power storage load 708 during the previous day. The planning unit 713 has a function of creating a plan for charging and discharging the power storage device 791 based on the amount of power demand predicted by the prediction unit 712.

[0461] The amount of power consumed by the general load 707 and the power storage load 708 measured by the measurement unit 711 can be confirmed on the display 706. It can also be confirmed on an electrical device such as a television or a personal computer via the router 709. It can also be confirmed on a portable electronic device such as a smartphone or a tablet via the router 709. The amount of power demand for each time period (or each hour) predicted by the prediction unit 712 can also be confirmed on the display 706, the electrical device, or the portable electronic device.

[0462] The secondary battery of one embodiment of the present invention can be used in, for example, one or both of an electronic device and a lighting device, such as a mobile phone, a smartphone, a portable information terminal such as a laptop computer, a portable game console, a portable music player, a digital camera, or a digital video camera.

[0463] A personal computer 2800 shown in FIG. 31A includes a housing 2801, a housing 2802, a display unit 2803, a keyboard 2804, a pointing device 2805, and the like. A secondary battery 2807 is provided inside the housing 2801, and a secondary battery 2806 is provided inside the housing 2802. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 2807 may be electrically connected to the secondary battery 2807. A touch panel is applied to the display unit 2803. As shown in FIG. 31B, the housings 2801 and 2802 can be removed from the personal computer 2800, and the personal computer 2800 can be used as a tablet terminal using only the housing 2802.

[0464] A large secondary battery obtained by the method for manufacturing a secondary battery according to one embodiment of the present invention can be used as one or both of the secondary battery 2806 and the secondary battery 2807. The shape of the secondary battery obtained by the method for manufacturing a secondary battery according to one embodiment of the present invention can be freely changed by changing the shape of the exterior body. For example, by forming the secondary batteries 2806 and 2807 to match the shapes of the housings 2801 and 2802, the capacity of the secondary battery can be increased and the usage time of the personal computer 2800 can be extended. Furthermore, the weight of the personal computer 2800 can be reduced.

[0465] A flexible display is applied to the display portion 2803 of the housing 2802. A large-sized secondary battery obtained by the manufacturing method of a secondary battery according to one embodiment of the present invention is applied to the secondary battery 2806. A large-sized secondary battery obtained by the manufacturing method of a secondary battery according to one embodiment of the present invention can be made into a bendable secondary battery by using a flexible film for the exterior body. This allows the housing 2802 to be folded and used as shown in FIG. 31C . In this case, part of the display portion 2803 can also be used as a keyboard as shown in FIG. 31C .

[0466] The housing 2802 can be folded so that the display portion 2803 faces inward as shown in FIG. 31D, or can be folded so that the display portion 2803 faces outward as shown in FIG. 31E.

[0467] The secondary battery of one embodiment of the present invention can be applied to a bendable secondary battery and can be mounted in electronic devices. In addition, the secondary battery can be incorporated along the curved surface of the interior or exterior of a house or building, or the interior or exterior of a car.

[0468] 32A shows an example of a mobile phone. The mobile phone 7400 includes a display portion 7402 built into a housing 7401, operation buttons 7403, an external connection port 7404, a speaker 7405, a microphone 7406, and the like. Note that the mobile phone 7400 includes a secondary battery 7407. By using the secondary battery of one embodiment of the present invention as the secondary battery 7407, a lightweight mobile phone with a long life can be provided. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 7407 may be electrically connected to the secondary battery 7407.

[0469] FIG. 32B shows the mobile phone 7400 in a bent state. When the mobile phone 7400 is deformed by an external force and bent as a whole, the secondary battery 7407 installed therein is also bent. FIG. 32C shows the state of the bent secondary battery 7407 at that time. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is fixed in a bent state. The secondary battery 7407 has a lead electrode electrically connected to the current collector. For example, the current collector is copper foil, and a portion of the current collector is alloyed with gallium to improve adhesion with the active material layer in contact with the current collector, resulting in a configuration with high reliability when the secondary battery 7407 is bent.

[0470] FIG. 32D shows an example of a bangle-type display device. The portable display device 7100 includes a housing 7101, a display unit 7102, operation buttons 7103, and a secondary battery 7104. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 7104 may be electrically connected to the secondary battery 7104. FIG. 32E also shows a bent secondary battery 7104. When the secondary battery 7104 is worn on a user's wrist in a bent state, the housing deforms, causing a partial or complete change in curvature of the secondary battery 7104. The degree of bending at any point on the curve, expressed as the radius of the corresponding circle, is called the radius of curvature, and the reciprocal of the radius of curvature is called the curvature. Specifically, a partial or complete change in the main surface of the housing or secondary battery 7104 occurs within a radius of curvature range of 40 mm to 150 mm. High reliability can be maintained if the radius of curvature of the main surface of the secondary battery 7104 is within a range of 40 mm to 150 mm. By using the secondary battery of one embodiment of the present invention as the secondary battery 7104, a lightweight and long-life portable display device can be provided.

[0471] 32F shows an example of a wristwatch-type portable information terminal 7200. The portable information terminal 7200 includes a housing 7201, a display portion 7202, a band 7203, a buckle 7204, operation buttons 7205, an input / output terminal 7206, and the like.

[0472] The portable information terminal 7200 can execute various applications such as mobile phone calls, e-mail, document browsing and creation, music playback, internet communication, and computer games.

[0473] The display surface of the display portion 7202 is curved, and display can be performed along the curved display surface. The display portion 7202 also includes a touch sensor, and can be operated by touching the screen with a finger, a stylus, or the like. For example, an application can be started by touching an icon 7207 displayed on the display portion 7202.

[0474] The operation button 7205 can have various functions, such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / deactivation, power saving mode activation / deactivation, etc. For example, the functions of the operation button 7205 can be freely set by an operating system incorporated in the portable information terminal 7200.

[0475] The portable information terminal 7200 is also capable of performing standardized short-range wireless communication. For example, hands-free conversation is possible by communicating with a wirelessly enabled headset.

[0476] The portable information terminal 7200 also includes an input / output terminal 7206, and can directly exchange data with another information terminal via a connector. Charging can also be performed via the input / output terminal 7206. Note that charging may be performed by wireless power supply without using the input / output terminal 7206.

[0477] The display portion 7202 of the portable information terminal 7200 includes the secondary battery of one embodiment of the present invention. By using the secondary battery of one embodiment of the present invention, a lightweight portable information terminal with a long life can be provided. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. For example, the secondary battery 7104 shown in FIG. 32E can be installed in a curved state inside the housing 7201 or in a bendable state inside the band 7203.

[0478] The portable information terminal 7200 preferably has a sensor. For example, a fingerprint sensor, a pulse sensor, a human body sensor such as a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like is preferably mounted as the sensor.

[0479] 32G shows an example of a wristband-type display device. The display device 7300 includes a display portion 7304 and a secondary battery of one embodiment of the present invention. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. The display device 7300 may also include a touch sensor in the display portion 7304 and can function as a portable information terminal.

[0480] The display surface of the display portion 7304 is curved, and display can be performed along the curved display surface. The display state of the display device 7300 can be changed by short-range wireless communication according to a communication standard.

[0481] The display device 7300 also includes an input / output terminal, and can directly exchange data with another information terminal via a connector. Charging can also be performed via the input / output terminal. Note that charging may be performed by wireless power supply without using the input / output terminal.

[0482] By using the secondary battery of one embodiment of the present invention as the secondary battery included in the display device 7300, a lightweight display device with a long lifetime can be provided.

[0483] Furthermore, examples in which a secondary battery with good cycle characteristics according to one embodiment of the present invention is mounted on an electronic device will be described with reference to FIGS. 32H, 33, and 34. FIG.

[0484] By using the secondary battery of one embodiment of the present invention as a secondary battery in an electronic device, a lightweight product with a long life can be provided. For example, examples of daily electronic devices include electric toothbrushes, electric shavers, and electric beauty devices. For the secondary battery of these products, a small, lightweight, and large-capacity stick-shaped secondary battery is desired for ease of holding by users.

[0485] FIG. 32H is a perspective view of a device also known as a tobacco-containing smoking device (electronic cigarette). In FIG. 32H, the electronic cigarette 7500 includes an atomizer 7501 including a heating element, a secondary battery 7504 that supplies power to the atomizer, and a cartridge 7502 including a liquid supply bottle or a sensor. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 7504 may be electrically connected to the secondary battery 7504. The secondary battery 7504 shown in FIG. 32H has external terminals so that it can be connected to a charging device. Because the secondary battery 7504 is the tip portion when held, it is desirable that the total length be short and the weight be light. The secondary battery of one embodiment of the present invention has high capacity and good cycle characteristics, making it possible to provide a compact and lightweight electronic cigarette 7500 that can be used for a long period of time.

[0486] Next, an example of a foldable tablet terminal is shown in Figures 33A and 33B. The tablet terminal 7600 shown in Figures 33A and 33B includes a housing 7630a, a housing 7630b, a movable portion 7640 connecting the housings 7630a and 7630b, a display portion 7631 having display portions 7631a and 7631b, switches 7625 to 7627, a fastener 7629, and an operation switch 7628. Using a flexible panel for the display portion 7631 allows the tablet terminal to have a larger display area. Figure 33A shows the tablet terminal 7600 in an open state, and Figure 33B shows the tablet terminal 7600 in a closed state.

[0487] The tablet terminal 7600 also includes a power storage unit 7635 inside the housing 7630a and the housing 7630b. The power storage unit 7635 passes through the movable portion 7640 and is provided across the housing 7630a and the housing 7630b.

[0488] All or part of the display portion 7631 can be a touch panel area, and data can be input by touching an image including an icon, text, an input form, etc. displayed in the area. For example, keyboard buttons may be displayed on the entire surface of the display portion 7631a on the housing 7630a side, and information such as text and images may be displayed on the display portion 7631b on the housing 7630b side.

[0489] A keyboard may be displayed on the display portion 7631b of the housing 7630b, and information such as text and images may be displayed on the display portion 7631a of the housing 7630a. A keyboard display switch button of a touch panel may be displayed on the display portion 7631, and the keyboard may be displayed on the display portion 7631 by touching the button with a finger, a stylus, or the like.

[0490] In addition, touch input can be simultaneously performed on the touch panel area of ​​the display portion 7631a on the housing 7630a side and the touch panel area of ​​the display portion 7631b on the housing 7630b side.

[0491] Furthermore, the switches 7625 to 7627 may be interfaces capable of switching various functions in addition to interfaces for operating the tablet terminal 7600. For example, at least one of the switches 7625 to 7627 may function as a switch for turning the tablet terminal 7600 on and off. For example, at least one of the switches 7625 to 7627 may have a function for switching the display orientation, such as portrait or landscape, or a function for switching between black and white and color display. For example, at least one of the switches 7625 to 7627 may have a function for adjusting the brightness of the display unit 7631. The brightness of the display unit 7631 can be optimized depending on the amount of external light detected by an optical sensor built into the tablet terminal 7600 during use. The tablet terminal may also have built-in not only an optical sensor but also other detection devices, such as a gyroscope, an acceleration sensor, or other sensors for detecting tilt.

[0492] 33A shows an example in which the display areas of the display portion 7631a on the housing 7630a and the display portion 7631b on the housing 7630b are substantially the same, the display areas of the display portion 7631a and the display portion 7631b are not particularly limited, and the sizes of one and the other may be different, and the display qualities may also be different. For example, one display panel may be capable of displaying at a higher resolution than the other.

[0493] 33B shows a tablet terminal 7600 folded in half, and the tablet terminal 7600 includes a housing 7630, a solar cell 7633, and a charge / discharge control circuit 7634 including a DCDC converter 7636. In addition, a secondary battery of one embodiment of the present invention is used as a power storage unit 7635.

[0494] As described above, the tablet terminal 7600 can be folded in half, and thus can be folded so that the housing 7630a and the housing 7630b overlap when not in use. By folding, the display portion 7631 can be protected, thereby improving the durability of the tablet terminal 7600. Furthermore, the power storage unit 7635 using the secondary battery of one embodiment of the present invention has a high capacity and favorable cycle characteristics, and therefore the tablet terminal 7600 can be used for a long period of time. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery included in the power storage unit 7635 may be electrically connected to the secondary battery.

[0495] In addition, the tablet terminal 7600 shown in Figures 33A and 33B can have functions such as displaying various information (still images, videos, text images, etc.), displaying a calendar, date or time on the display unit, a touch input function for touch input operations or editing information displayed on the display unit, and controlling processing using various software (programs).

[0496] A solar cell 7633 attached to the surface of the tablet terminal 7600 can supply power to a touch panel, a display unit, a video signal processor, or the like. The solar cell 7633 can be provided on one or both surfaces of the housing 7630, and can be configured to efficiently charge the power storage unit 7635. Use of a lithium-ion battery as the power storage unit 7635 has the advantage of enabling miniaturization.

[0497] The configuration and operation of the charge / discharge control circuit 7634 shown in Fig. 33B are described with reference to a block diagram in Fig. 33C. Fig. 33C shows a solar cell 7633, a power storage unit 7635, a DC / DC converter 7636, a converter 7637, switches SW1 to SW3, and a display unit 7631. The power storage unit 7635, the DC / DC converter 7636, the converter 7637, and switches SW1 to SW3 correspond to the charge / discharge control circuit 7634 shown in Fig. 33B.

[0498] First, an example of operation when power is generated by the solar cell 7633 using external light will be described. The power generated by the solar cell is stepped up or down by a DC-DC converter 7636 to a voltage for charging the power storage unit 7635. When power from the solar cell 7633 is used to operate the display unit 7631, a switch SW1 is turned on, and the converter 7637 steps up or steps down the voltage to a voltage required for the display unit 7631. When no display is to be performed on the display unit 7631, the switch SW1 may be turned off and the switch SW2 may be turned on to charge the power storage unit 7635.

[0499] Note that the solar cell 7633 is shown as an example of a power generation means, but is not particularly limited thereto, and a configuration in which the power storage unit 7635 is charged by other power generation means such as a piezoelectric element (piezo element) or a thermoelectric conversion element (Peltier element) may be used. For example, a configuration in which a contactless power transmission module that transmits and receives power wirelessly (contactlessly) for charging, or a combination of other charging means may be used.

[0500] FIG. 34 illustrates an example of another electronic device. In FIG. 34 , a display device 8000 is an example of an electronic device using a secondary battery 8004 according to one embodiment of the present invention. Specifically, the display device 8000 corresponds to a display device for receiving TV broadcasts and includes a housing 8001, a display portion 8002, a speaker portion 8003, a secondary battery 8004, and the like. To enhance safety, a protection circuit for preventing overcharging and / or overdischarging of the secondary battery 8004 may be electrically connected to the secondary battery 8004. The secondary battery 8004 according to one embodiment of the present invention is provided inside the housing 8001. The display device 8000 can receive power from a commercial power source or can use power stored in the secondary battery 8004. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the display device 8000 can be used by using the secondary battery 8004 according to one embodiment of the present invention as an uninterruptible power source.

[0501] The display portion 8002 can be a liquid crystal display device, a light-emitting device having a light-emitting element such as an organic EL element in each pixel, an electrophoretic display device, a semiconductor display device such as a DMD (Digital Micromirror Device), a PDP (Plasma Display Panel), or an FED (Field Emission Display).

[0502] The display device includes all display devices for displaying information, such as those for receiving TV broadcasts, those for personal computers, and those for displaying advertisements.

[0503] In FIG. 34 , a stationary lighting device 8100 is an example of an electronic device using a secondary battery 8103 according to one embodiment of the present invention. Specifically, the lighting device 8100 includes a housing 8101, a light source 8102, a secondary battery 8103, and the like. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 8103 may be electrically connected to the secondary battery 8103. FIG. 34 illustrates the case where the secondary battery 8103 is provided inside a ceiling 8104 on which the housing 8101 and the light source 8102 are installed; however, the secondary battery 8103 may be provided inside the housing 8101. The lighting device 8100 can receive power from a commercial power source or can use power stored in the secondary battery 8103. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the lighting device 8100 can be used by using the secondary battery 8103 according to one embodiment of the present invention as an uninterruptible power supply.

[0504] Note that although Figure 34 illustrates an example of a stationary lighting device 8100 provided on the ceiling 8104, the secondary battery of one embodiment of the present invention can also be used in a stationary lighting device provided on a side wall 8105, a floor 8106, a window 8107, or the like other than the ceiling 8104, or can also be used in a tabletop lighting device.

[0505] Furthermore, an artificial light source that artificially obtains light using electric power can be used as the light source 8102. Specifically, examples of the artificial light source include a discharge lamp such as an incandescent lamp or a fluorescent lamp, an LED, and / or an organic EL element.

[0506] In FIG. 34 , an air conditioner including an indoor unit 8200 and an outdoor unit 8204 is an example of an electronic device using a secondary battery 8203 according to one embodiment of the present invention. Specifically, the indoor unit 8200 includes a housing 8201, an air outlet 8202, a secondary battery 8203, and the like. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 8203 may be electrically connected to the secondary battery 8203. Although FIG. 34 illustrates the case where the secondary battery 8203 is provided in the indoor unit 8200, the secondary battery 8203 may also be provided in the outdoor unit 8204. Alternatively, the secondary battery 8203 may be provided in both the indoor unit 8200 and the outdoor unit 8204. The air conditioner can receive power from a commercial power source or can use power stored in the secondary battery 8203. In particular, when a secondary battery 8203 is provided in both the indoor unit 8200 and the outdoor unit 8204, the air conditioner can be used by using the secondary battery 8203 of one embodiment of the present invention as an uninterruptible power supply even when power cannot be supplied from a commercial power source due to a power outage or the like.

[0507] Note that although a separate-type air conditioner including an indoor unit and an outdoor unit is illustrated in FIG. 34 , a secondary battery according to one embodiment of the present invention can also be used in an integrated air conditioner in which the functions of the indoor unit and the outdoor unit are combined in a single housing.

[0508] In FIG. 34 , an electric refrigerator-freezer 8300 is an example of an electronic device using a secondary battery 8304 according to one embodiment of the present invention. Specifically, the electric refrigerator-freezer 8300 includes a housing 8301, a refrigerator compartment door 8302, a freezer compartment door 8303, a secondary battery 8304, and the like. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 8304 may be electrically connected to the secondary battery 8304. In FIG. 34 , the secondary battery 8304 is provided inside the housing 8301. The electric refrigerator-freezer 8300 can receive power from a commercial power source or can use power stored in the secondary battery 8304. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the electric refrigerator-freezer 8300 can be used by using the secondary battery 8304 according to one embodiment of the present invention as an uninterruptible power supply.

[0509] Among the electronic devices described above, electronic devices such as microwave ovens and other high-frequency heating devices and electric rice cookers require a large amount of power for a short period of time. Therefore, by using a secondary battery according to one embodiment of the present invention as an auxiliary power source for supplementing the power that cannot be supplied by the commercial power source, it is possible to prevent the breaker of the commercial power source from tripping when the electronic device is in use.

[0510] Furthermore, by storing power in the secondary battery during times when electronic devices are not in use, particularly during times when the ratio of the amount of power actually used to the total amount of power that can be supplied by the commercial power supplier (referred to as the power usage rate) is low, it is possible to prevent the power usage rate from increasing outside of these times. For example, in the case of an electric refrigerator-freezer 8300, power is stored in the secondary battery 8304 during the night when the temperature is low and the refrigerator door 8302 and the freezer door 8303 are not opened or closed. Then, during the day when the temperature is high and the refrigerator door 8302 and the freezer door 8303 are opened and closed, the secondary battery 8304 is used as an auxiliary power source, thereby keeping the daytime power usage rate low.

[0511] According to one embodiment of the present invention, the cycle characteristics of the secondary battery can be improved, and the reliability can be improved. Furthermore, according to one embodiment of the present invention, a high-capacity secondary battery can be obtained, and therefore the characteristics of the secondary battery can be improved, and therefore the secondary battery itself can be made smaller and lighter. Therefore, by incorporating the secondary battery according to one embodiment of the present invention in the electronic device described in this embodiment, the electronic device can have a longer life and be lighter.

[0512] 35A shows an example of a wearable device. The wearable device uses a secondary battery as a power source. Furthermore, in order to improve splash-proof, water-resistant, or dust-proof performance when used at home or outdoors, there is a demand for a wearable device that can be charged wirelessly as well as via a wired connection with an exposed connector.

[0513] For example, a secondary battery according to one embodiment of the present invention can be mounted on an eyeglasses-type device 9000 as shown in FIG. 35A . The eyeglasses-type device 9000 includes a frame 9000a and a display unit 9000b. Mounting a secondary battery on the temples of the curved frame 9000a allows the eyeglasses-type device 9000 to be lightweight, well-balanced in weight, and have a long continuous use time. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including a secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.

[0514] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on a headset device 9001. The headset device 9001 includes at least a microphone unit 9001a, a flexible pipe 9001b, and an earphone unit 9001c. The secondary battery can be provided in the flexible pipe 9001b or the earphone unit 9001c. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.

[0515] Furthermore, a secondary battery according to one embodiment of the present invention can be mounted on a device 9002 that can be directly attached to the body. A secondary battery 9002b can be provided in a thin housing 9002a of the device 9002. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 9002b may be electrically connected to the secondary battery 9002b. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.

[0516] Furthermore, a secondary battery according to one embodiment of the present invention can be mounted on a device 9003 that can be attached to clothing. A secondary battery 9003b can be provided in a thin housing 9003a of the device 9003. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 9003b may be electrically connected to the secondary battery 9003b. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.

[0517] Furthermore, the secondary battery of one embodiment of the present invention can be mounted on a belt-type device 9006. The belt-type device 9006 has a belt portion 9006a and a wireless power receiving portion 9006b, and the secondary battery can be mounted inside the belt portion 9006a. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including the secondary battery of one embodiment of the present invention, a configuration that can accommodate space saving due to a miniaturized housing can be realized.

[0518] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on the wristwatch device 9005. The wristwatch device 9005 has a display portion 9005a and a belt portion 9005b, and the secondary battery can be provided on the display portion 9005a or the belt portion 9005b. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to a miniaturized housing can be realized.

[0519] The display portion 9005a can display not only the time but also various information such as incoming emails and / or phone calls.

[0520] Furthermore, since the wristwatch device 9005 is a wearable device that is worn directly on the arm, it may be equipped with sensors that measure the user's pulse, blood pressure, etc. Data on the user's exercise volume and health can be accumulated to manage the user's health.

[0521] FIG. 35B shows a perspective view of the wristwatch-type device 9005 removed from the wrist.

[0522] 35C shows a side view of the display device 9005. The display device 9005 includes a secondary battery 913 according to one embodiment of the present invention. The secondary battery 913 is small and lightweight and is provided so as to overlap with the display portion 9005a.

[0523] 36A shows an example of a cleaning robot. The cleaning robot 9300 includes a display unit 9302 arranged on the top surface of a housing 9301, multiple cameras 9303 arranged on the side surface, a brush 9304, operation buttons 9305, a secondary battery 9306, various sensors, and the like. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 9306 may be electrically connected to the secondary battery 9306. Although not shown, the cleaning robot 9300 is provided with tires, a suction port, and the like. The cleaning robot 9300 can move by itself, detect dust 9310, and suck up the dust through a suction port provided on the bottom surface.

[0524] For example, the cleaning robot 9300 can analyze an image captured by the camera 9303 to determine whether or not there is an obstacle such as a wall, furniture, or a step. Furthermore, if an object that may become entangled in the brush 9304, such as a wire, is detected through image analysis, the cleaning robot 9300 can stop the rotation of the brush 9304. The cleaning robot 9300 includes a secondary battery 9306 according to one embodiment of the present invention and a semiconductor device or electronic component therein. By using the secondary battery 9306 according to one embodiment of the present invention in the cleaning robot 9300, the cleaning robot 9300 can be a highly reliable electronic device with a long operating time.

[0525] Fig. 36B shows an example of a robot. The robot 9400 shown in Fig. 36B includes a secondary battery 9409, an illuminance sensor 9401, a microphone 9402, an upper camera 9403, a speaker 9404, a display unit 9405, a lower camera 9406, an obstacle sensor 9407, a movement mechanism 9408, a computing device, etc. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 9409 may be electrically connected to the secondary battery 9409.

[0526] The microphone 9402 has a function of detecting the user's voice, environmental sounds, etc. The speaker 9404 has a function of emitting sound. The robot 9400 can communicate with the user using the microphone 9402 and the speaker 9404.

[0527] The display portion 9405 has a function of displaying various information. The robot 9400 can display information desired by a user on the display portion 9405. The display portion 9405 may be equipped with a touch panel. The display portion 9405 may be a detachable information terminal, which can be installed in a fixed position on the robot 9400 to enable charging and data transfer.

[0528] The upper camera 9403 and the lower camera 9406 have the function of capturing images of the surroundings of the robot 9400. In addition, the obstacle sensor 9407 can detect the presence or absence of obstacles in the direction of travel when the robot 9400 moves forward using the movement mechanism 9408. The robot 9400 can recognize the surrounding environment and move safely using the upper camera 9403, the lower camera 9406, and the obstacle sensor 9407.

[0529] The robot 9400 includes a secondary battery 9409 according to one embodiment of the present invention and a semiconductor device or an electronic component inside the robot 9400. By using the secondary battery according to one embodiment of the present invention in the robot 9400, the robot 9400 can be a highly reliable electronic device with a long operating time.

[0530] Fig. 36C shows an example of an air vehicle. The air vehicle 9500 shown in Fig. 36C has a propeller 9501, a camera 9502, a secondary battery 9503, and the like, and has the function of flying autonomously. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 9503 may be electrically connected to the secondary battery 9503.

[0531] For example, image data captured by the camera 9502 is stored in the electronic component 9504. The electronic component 9504 can analyze the image data and detect the presence or absence of an obstacle when moving. Furthermore, the electronic component 9504 can estimate the remaining battery charge from a change in the storage capacity of the secondary battery 9503. The flying object 9500 includes the secondary battery 9503 according to one embodiment of the present invention therein. By using the secondary battery according to one embodiment of the present invention in the flying object 9500, the flying object 9500 can be an electronic device with a long operating time and high reliability.

[0532] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0533] In this example, graphene of one embodiment of the present invention was manufactured and its physical properties were evaluated.

[0534] <Preparation of Graphene> Fluorine-containing graphene was prepared with reference to the flow shown in FIG. 6 .

[0535] In step S21, graphene oxide was prepared as material 801. In step S22, lithium fluoride was used as material 802. In step S23, lithium carbonate was used as material 803.

[0536] In step S31, 0.25 g of graphene oxide, 0.0125 g of lithium fluoride, and 0.0125 g of lithium carbonate were mixed, and collected in step S32, and a mixture 804 was obtained in step S33.

[0537] In step S51, heating was performed under the conditions of 850° C. for 10 hours in a nitrogen atmosphere.

[0538] In step S52, the heated mixture was collected, and in step S53, graphene 583 was obtained. The graphene 583 obtained in this example is hereinafter referred to as sample Sm1.

[0539] <Raman spectroscopy> The Raman spectrum of sample Sm1 was obtained using an NRS-5500 manufactured by JASCO Corporation. The excitation wavelength was 532 nm. The measurement was performed in an air atmosphere at room temperature.

[0540] An optical microscope photograph of sample Sm1 is shown in Figure 37. In the Raman spectrum, the in-plane distribution of the D band peak intensity is shown in Figure 38A, the in-plane distribution of the G band peak intensity is shown in Figure 38B, and the ratio of the D band peak intensity to the G band peak intensity (D band peak intensity / G band peak intensity) is shown in Figure 38C. Furthermore, the Raman spectrum of an arbitrary location on sample Sm1 is shown in Figure 39.

[0541] The observation of the G-band suggested sp2 bonds of carbon, and suggested that the obtained sample Sm1 had graphene. The observation of the D-band suggested that the obtained graphene had defects.

[0542] <TEM Observation> Next, TEM observation was performed on sample Sm1. A JEM-ARM200F manufactured by JEOL Ltd. was used for the observation. The acceleration voltage was 80 kV. The obtained TEM image is shown in FIG. 40. Furthermore, FFT filtered images of region 91 indicated by a square in FIG. 40 are shown in FIGS. 41A and 42A. FIG. 41B is an enlarged view of the region surrounded by a square in FIG. 41A, and FIG. 42B is an enlarged view of the region surrounded by a square in FIG. 42A.

[0543] The FFT filtered image refers to an image obtained by performing IFFT processing on an image obtained by performing FFT processing on a TEM image.

[0544] As shown in Figure 41B, the presence of a seven-membered ring was suggested.

[0545] As shown in Figure 42B, the presence of a 12-membered ring was suggested. The presence of a 12-membered ring was suggested by consideration using an image obtained by first-principles calculations.

[0546] Figure 42C shows the results of calculation of a TEM image of graphene having 12-membered rings. The structure of graphene having 12-membered rings was calculated by first-principles calculation using a plane wave basis and pseudopotential. GGA-PBE was used as the exchange-correlation functional. Based on the graphene structure calculated by first-principles calculation, an image was calculated when the electron beam was defocused from the focal position using the aperture radius, convergence angle, and spherical aberration coefficient of the electron beam optical system. The acceleration voltage was 80 kV, and the objective aperture radius was 6 nm. −1 The convergence angle was set to 0.3 mrad, and the defocus value was set to -10 nm.

[0547] It was suggested that the graphene of one embodiment of the present invention obtained in this example had seven- or more-membered rings, and also had holes each composed of a 12-membered ring.

[0548] <EDX> Next, the STEM image of sample Sm1 was observed and EDX analysis was performed.

[0549] A JEM-ARM200F manufactured by JEOL Ltd. was used for the STEM observation and EDX analysis. The acceleration voltage was 80 kV. A JED-2300T manufactured by JEOL Ltd. was used as the EDX analysis device. Figure 43A shows a STEM image of region 92 shown in Figure 40. Figure 43B shows an EDX area analysis image corresponding to the observation location shown in Figure 43A. When the spectra were analyzed in regions A and B indicated by squares in the figure, fluorine was detected in each. Fluorine was also detected in other regions, suggesting that fluorine is widely distributed within the surface.

[0550] 91: region, 92: region, 100: positive electrode active material, 130: laminate, 131: laminate, 500: secondary battery, 501: positive electrode current collector, 502: positive electrode active material layer, 503: positive electrode, 504: negative electrode current collector, 505: negative electrode active material layer, 506: negative electrode, 507: separator, 507a: region, 507b: region, 508: electrolyte, 509: exterior body, 509a: exterior body, 509b: exterior body, 510: positive electrode lead electrode, 511: negative electrode lead electrode, 512: laminate, 513: resin layer, 514: region, 515a: electrolyte, 515b: electrolyte, 515c: electrolyte, 516: inlet, 550 : laminate, 560: secondary battery, 570: electrode, 570b: region, 571: current collector, 572: active material layer, 581: electrolyte, 582: particle, 582b: particle, 583: graphene, 584: acetylene black, 584b: material, 585: hole, 586: polymer film, 587: hole, 588: polymer film, 600: secondary battery, 670: manufacturing apparatus, 671: component input chamber, 672: transfer chamber, 673: treatment chamber, 676: component removal chamber, 680: transfer mechanism, 691: stage, 694: nozzle, 701: commercial power source, 703: distribution board, 705: power storage controller, 70 6: display, 707: general load, 708: power storage system load, 709: router, 710: service line attachment section, 711: measurement section, 712: prediction section, 713: planning section, 790: control device, 791: power storage device, 796: underfloor space section, 799: building, 801: material, 802: material, 803: material, 804: mixture, 804b: mixture, 903: mixture, 904: mixture, 911a: terminal, 911b: terminal, 913: secondary battery, 930: housing, 930a: housing, 930b: housing, 931: negative electrode, 931a: negative electrode active material layer, 932: positive electrode, 932a: positive electrode active material layer, 933: cell separator, 950: wound body, 950a: wound body, 951: terminal, 952: terminal, 970: secondary battery, 971: housing, 972: laminate, 973a: positive electrode lead electrode, 973b: terminal, 973c: conductor, 974a: negative electrode lead electrode, 974b: terminal, 974c: conductor, 975a: positive electrode, 975b: positive electrode, 976: separator, 977a: negative electrode, 1301a: battery, 1301b: battery, 1302: battery controller, 1303: motor controller, 1304: motor, 1305: gear, 1306: DCDC circuit, 1307: electric power steering,1308: heater, 1309: defogger, 1310: DCDC circuit, 1311: battery, 1312: inverter, 1313: audio, 1314: power window, 1315: lamps, 1316: tires, 1317: rear motor, 1320: control circuit section, 1321: control circuit section, 1322: control circuit, 1324: switch section, 1325: external terminal, 1326: external terminal, 1415: battery pack, 1421: wiring, 1422: wiring, 2001: automobile, 2002: transport vehicle, 2003: transport vehicle, 2004: aircraft, 2005: transport vehicle, 21 00: electric bicycle, 2101: secondary battery, 2102: power storage device, 2103: display unit, 2104: control circuit, 2201: battery pack, 2202: battery pack, 2203: battery pack, 2204: battery pack, 2300: scooter, 2301: side mirror, 2302: power storage device, 2303: turn signal light, 2304: under-seat storage, 2603: vehicle, 2604: charging device, 2610: solar panel, 2611: wiring, 2612: power storage device, 2800: personal computer, 2801: housing, 2802: housing, 2803: display unit, 2804: keyboard, 2 805: pointing device, 2806: secondary battery, 2807: secondary battery, 7100: portable display device, 7101: housing, 7102: display unit, 7103: operation button, 7104: secondary battery, 7200: portable information terminal, 7201: housing, 7202: display unit, 7203: band, 7204: buckle, 7205: operation button, 7206: input / output terminal, 7207: icon, 7300: display device, 7304: display unit, 7400: mobile phone, 7401: housing, 7402: display unit, 7403: operation button, 7404: external connection port, 7405: speaker, 7 406: microphone, 7407: secondary battery, 7500: electronic cigarette, 7501: atomizer, 7502: cartridge, 7504: secondary battery, 7600: tablet terminal, 7625: switch, 7627: switch, 7628: operation switch, 7629: fastener, 7630: housing, 7630a: housing, 7630b: housing, 7631: display unit, 7631a: display unit, 7631b: display unit, 7633: solar cell, 7634: charge / discharge control circuit, 7635: power storage unit, 7636: DCDC converter, 7637: converter, 7640: moving part, 8000: display device,8001: Housing, 8002: Display unit, 8003: Speaker unit, 8004: Secondary battery, 8100: Lighting device, 8101: Housing, 8102: Light source, 8103: Secondary battery, 8104: Ceiling, 8105: Side wall, 8106: Floor, 8107: Window, 8200: Indoor unit, 8201: Housing, 8202: Air outlet, 8203: Secondary battery, 8204: Outdoor unit, 8300: Electric refrigerator-freezer, 830 1: Housing, 8302: Refrigerator door, 8303: Freezer door, 8304: Secondary battery, 9000: Glasses-type device, 9000a: Frame, 9000b: Display unit, 9001: Headset-type device, 9001a: Microphone unit, 9001b: Flexible pipe, 9001c: Earphone unit, 9002: Device, 9002a: Housing, 9002b: Secondary battery, 9003: Device chair, 9003a: housing, 9003b: secondary battery, 9005: wristwatch-type device, 9005a: display unit, 9005b: belt unit, 9006: belt-type device, 9006a: belt unit, 9006b: wireless power supply receiving unit, 9300: cleaning robot, 9301: housing, 9302: display unit, 9303: camera, 9304: brush, 9305: operation button, 9306: secondary battery Battery, 9310: garbage, 9400: robot, 9401: illuminance sensor, 9402: microphone, 9403: upper camera, 9404: speaker, 9405: display unit, 9406: lower camera, 9407: obstacle sensor, 9408: movement mechanism, 9409: secondary battery, 9500: flying object, 9501: propeller, 9502: camera, 9503: secondary battery, 9504: electronic component,

Claims

1. having a hole formed of a 9- or more-membered ring formed of carbon atoms; Graphene in which one or more of the carbon atoms constituting the poly-membered ring are terminated with fluorine.

2. In claim 1, In Raman spectroscopy analysis, -1 The first peak observed at or near 1360 cm -1 or a second peak observed in the vicinity thereof.

3. The present invention relates to a method for producing an active material having an active material particle and a graphene. The graphene has holes formed of 9- or more-membered rings formed of carbon atoms, one or more of the carbon atoms constituting the poly-membered ring are terminated with fluorine; The graphene covers at least a portion of the surface of the active material particles.

4. In claim 3, The graphene has a Raman spectroscopy analysis of 1580 cm -1 The first peak observed at or near 1360 cm -1 and a second peak observed at or near the peak.

5. In claim 3 or claim 4, The active material particles are positive electrode active material particles.

6. In any one of claims 3 to 5, The active material particles are negative electrode active material particles.

7. A secondary battery comprising the electrode according to any one of claims 3 to 6 and an electrolyte.

8. An electronic device comprising the secondary battery according to claim 7.

9. A vehicle comprising the secondary battery according to claim 7.