Method and apparatus for treating metallic member

JPWO2022107753A5Active Publication Date: 2024-11-22PARKER NETSUSHORI KOGYO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022563760
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2021-11-16
Publication Date
2024-11-22
Estimated Expiration
2041-11-16

AI Technical Summary

Technical Problem

Current surface activation methods for metal parts prior to nitriding or nitrocarburizing, such as those using chloride or fluorine compounds, face challenges in automation, control of gas production, and compatibility with mass flow controllers, leading to inconsistent results and potential corrosion issues.

Method used

A method and apparatus that utilize a liquid organic solvent, intermittently introduced into the processing furnace, to activate the metal surface, suppressing vaporization and allowing precise control of the solvent's addition, thereby enhancing the activation process and reducing manual labor and equipment complexity.

Benefits of technology

The method effectively activates the metal surface, ensuring consistent and optimal nitriding or nitrocarburizing treatments by controlling the solvent's introduction, reducing manual intervention, and minimizing equipment complexity, while preventing solvent vaporization and backflow.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention is a method for treating a metallic member using a treatment furnace, the method comprising a step for introducing an activation atmosphere gas into the treatment furnace, a step for heating the activation atmosphere gas in the treatment furnace to a first temperature, a step for introducing a nitriding atmosphere gas or a soft nitriding atmosphere gas into the treatment furnace, and a step for heating the nitriding atmosphere gas or the soft nitriding atmosphere gas in the treatment furnace to a second temperature. The activation atmosphere gas can be introduced into the treatment furnace through an activation atmosphere gas introduction pipe. An organic solvent in a liquid form is introduced into the activation atmosphere gas introduction pipe, which is in a state where the introduction of the activation atmosphere gas has been continued, several times intermittently.
Need to check novelty before this filing date? Find Prior Art

Description

METHOD AND APPARATUS FOR TREATING METAL COMPONENTS

[0001] The present invention relates to a method and apparatus for treating a metal member, which activates the surface of the metal member prior to subjecting the metal member to gas nitriding or gas soft nitriding.

[0002] Among the surface hardening treatments for steel, there is a high demand for nitriding, which is a low-heat-strain treatment, and recently, interest in gas nitriding or gas soft-nitriding in particular has been growing.Gas nitriding or gas soft-nitriding is widely used in automobile parts, molds, and other stainless steel parts to improve fatigue resistance, wear resistance, and corrosion resistance.

[0003] When these treatments are applied to the surface of a component made of alloy steel, particularly high-alloy steel such as stainless steel, the passivation film (oxide or the like) present on the surface of the component prevents nitrogen and carbon from penetrating and diffusing into the surface of the metal component, resulting in poor or uneven treatment of the component. For this reason, prior to these diffusion and penetration treatments, the surface of the metal component is subjected to an activation treatment.

[0004] Known surface activation methods include, for example, malcomizing, which uses chloride compounds (activators). Examples of chlorides used include vinyl chloride resin, ammonium chloride, and methylene chloride.

[0005] The chloride is placed in a treatment furnace together with the metal component and heated. This heating decomposes the chloride to generate HCl. The generated HCl destroys (denatures) the passivation film on the surface of the metal component, activating the surface. This ensures that the subsequent diffusion treatments, such as nitriding and carburizing, will be more reliable.

[0006] However, the surface activation of metal components using chlorides as described above requires the chlorides to be placed around the metal components in a processing furnace beforehand. This process is difficult to automate and requires manual labor by an operator. Furthermore, it is difficult to control the amount of HCl generated, so the optimal effect is not always obtained.

[0007] Furthermore, the generated HCl reacts with ammonia contained in the atmospheric gas during gas nitriding or gas soft nitriding to generate ammonium chloride, which not only accumulates in the treatment furnace or exhaust system and can cause problems, but also remains on the surface of the metal member (workpiece), resulting in a decrease in corrosion resistance and fatigue strength.

[0008] A method for activating the surface of a metal component using a fluorine compound (NF3), which belongs to the same halogen group as chloride, instead of chlorides, has also been put to practical use (for example, JP-A-3-44457 (Patent Document 1)). NF3 decomposes when heated to produce fluorine. The generated fluorine converts the passivation film on the surface of the metal component into a fluoride film, activating the surface.

[0009] However, the surface activation of metal components using the above-mentioned fluorine compound (NF3) requires advanced treatment to render harmless the NF3 and HF that may be contained in the exhaust gas, which has hindered the widespread use of this method.

[0010] As a pretreatment method that does not use chlorides or fluorine compounds, a method that uses a carbon compound has also been put into practical use (for example, Japanese Patent No. 4861703 (Patent Document 2), Japanese Patent Application Publication No. 9-38341 (Patent Document 3), and Japanese Patent Laid-Open Publication No. 10-219418 (Patent Document 4)). Specifically, acetylene is introduced into a furnace, and HCN generated in the reaction process starting from its thermal decomposition reduces the passivation film on the surface of the metal member, activating the surface (Japanese Patent No. 4861703 (Patent Document 2)). Alternatively, acetone vapor is introduced into a furnace, and HCN generated in the reaction process starting from its thermal decomposition reduces the passivation film on the surface of the metal member, activating the surface (Japanese Patent Application Publication No. 9-38341 (Patent Document 3), and Japanese Patent Laid-Open Publication No. 10-219418 (Patent Document 4)).

[0011] Furthermore, a method for activating a metal surface using a carbon-nitrogen compound is described in Japanese Patent No. 5826748 (Patent Document 5). In addition to a method using urea or acetamide, which are solid at room temperature, Japanese Patent No. 5826748 (Patent Document 5) also mentions a method using formamide, which is liquid at room temperature.

[0012] It has been known since the 1970s that CO gas forms HCN in a furnace (Heat Treatment, Vol. 18, No. 5, pp. 255-262 (Otomo Kiyomitsu) (Non-Patent Document 1)). Based on this knowledge, it is believed that carbon compounds and carbon-nitrogen compounds have been selected and studied as compounds that generate CO gas in a furnace during the reaction process.

[0013] However, it is known that for SUS-based materials (such as SUS310S, which contain a lot of Cr and Ni) with stronger passivation films, the method using HCN (carbon compound, carbon-nitrogen compound) is less effective at activating than the method using HCl (chloride).For this reason, it is necessary to use either the method using HCN (carbon compound, carbon-nitrogen compound) or the method using HCl (chloride) depending on the grade of the steel.

[0014] Japanese Patent Application Publication No. 9-38341 Japanese Patent Application Publication No. 10-219418 Japanese Patent No. 5826748 "Heat Treatment", Vol. 18, No. 5, pp. 255-262 (Kiyomitsu Otomo)

[0015] Carbon compounds and carbon-nitrogen compounds that are solid at room temperature must be placed in advance around the metal members in the treatment furnace. This process is difficult to automate and requires manual work by an operator. In addition, it is difficult to control the amount of HCN produced, so optimal effects are not always obtained.

[0016] Carbon compounds and carbon-nitrogen compounds, which are gases at room temperature, have the advantage that they can be introduced into the furnace in an appropriate amount controlled using a mass flow controller. However, gas cylinders are difficult to handle and take up space, and measures must be taken to prevent the risk of gas leaks from the piping. Furthermore, some types of carbon compounds and carbon-nitrogen compounds (especially types of activated species) are not compatible with mass flow controllers (making it difficult to properly control the amount introduced).

[0017] Carbon compounds and carbon-nitrogen compounds that are liquid at room temperature are generally gasified before being introduced into the furnace so that the appropriate amount can be controlled (see paragraph 0010 of Japanese Patent No. 4861703 (Patent Document 2): "Since acetone, which is liquid at room temperature and normal pressure, is used, a device for introducing acetone vapor is required.").

[0018] Japanese Patent No. 5826748 (Patent Document 5) describes the direct introduction of liquid formamide into the hot zone of a tubular furnace (a small experimental furnace) using a probe (see paragraph 0081 of Patent No. 5826748 (Patent Document 5)). However, this method is difficult to apply to a general production furnace. This is because, in a configuration in which a probe is directly connected to a general production furnace, the formamide in the probe vaporizes due to the high heat dissipation of the production furnace, causing a backflow, preventing the desired amount of formamide from being introduced into the furnace. Furthermore, there is a concern that the backflowing formamide may precipitate in unwanted piping, causing pipe clogging.

[0019] The present inventors have discovered that by introducing an organic solvent that is liquid at room temperature (carbon compounds, carbon-nitrogen compounds, or chlorides are also acceptable) into the activation atmosphere gas inlet pipe while the activation atmosphere gas is being continuously introduced into the processing furnace, it is possible to effectively prevent the organic solvent from evaporating and flowing back even when the processing furnace is at a high temperature.

[0020] Furthermore, the present inventors have discovered that by intermittently adding an organic solvent that is liquid at room temperature in multiple batches, it is possible to add an appropriate amount of organic solvent at a timing that is appropriate for the conditions inside the processing furnace.

[0021] The present invention was devised based on the above findings, and an object of the present invention is to provide a method and apparatus for treating metal members that can practically activate the surfaces of metal members using a liquid organic solvent.

[0022] The present invention provides a method for treating metal members using a treatment furnace, comprising: a metal member charging step of charging the metal members into the treatment furnace; an activation atmosphere gas introducing step of introducing an activation atmosphere gas into the treatment furnace; a first heating step of heating the activation atmosphere gas in the treatment furnace to a first temperature; a main atmosphere gas introducing step of introducing a nitriding atmosphere gas or a soft-nitriding atmosphere gas into the treatment furnace after the first heating step; and a second heating step of heating the nitriding atmosphere gas or the soft-nitriding atmosphere gas in the treatment furnace to a second temperature to nitride or soft-nitridize the metal members, wherein in the activation atmosphere gas introducing step, the activation atmosphere gas is introduced into the treatment furnace via an activation atmosphere gas piping, and the activation atmosphere gas introducing step is performed simultaneously during at least a portion of the first heating step, and during the first heating step, a liquid organic solvent is intermittently introduced into the activation atmosphere gas introducing piping multiple times.

[0023] According to the present invention, by introducing a liquid organic solvent (which may be a chloride in addition to a carbon compound or a carbon-nitrogen compound) into the activation atmosphere gas introduction pipe while the introduction of the activation atmosphere gas into the processing furnace is continuing, it is possible to effectively prevent the organic solvent from evaporating and flowing back even if the temperature (first temperature) of the processing furnace is high.

[0024] Furthermore, according to the present invention, by intermittently adding the liquid organic solvent in multiple batches, it is possible to add an appropriate amount of organic solvent at a timing that is appropriate for the conditions inside the processing furnace.

[0025] For example, the first heating temperature is 400°C to 500°C.

[0026] Within this temperature range, the activation treatment of the metal member proceeds favorably, while the occurrence of a situation in which the organic solvent evaporates and flows back is effectively suppressed.

[0027] Furthermore, for example, the activation atmosphere gas contains ammonia gas, and the organic solvent is a compound containing at least one type of hydrocarbon.

[0028] According to this, HCN generated during the reaction process starting from the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal member, thereby effectively activating the surface.

[0029] More specifically, the organic solvent is, for example, any one of formamide, xylene, and toluene.

[0030] In this case, the present inventors have confirmed in an actual production furnace that it is effective to add the organic solvent at a substantially uniform rate over a period of 1 second to 2 minutes (preferably 10 seconds to 2 minutes) in an amount of 10 to 80 ml per addition, and to add the organic solvent 2 to 6 times at intervals of 10 minutes or more.

[0031] Alternatively, for example, the activation atmosphere gas contains ammonia gas, and the organic solvent is at least one type of compound containing chlorine.

[0032] According to this, HCl generated during the reaction process starting from the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal member, thereby effectively activating the surface.

[0033] More specifically, the organic solvent is, for example, any one of trichloroethylene, tetrachloroethylene, and tetrachloroethane.

[0034] In this case, the present inventors have confirmed in an actual production furnace that it is effective to add the organic solvent at a substantially uniform rate over a period of 1 second to 2 minutes (preferably 10 seconds to 2 minutes) in an amount of 10 to 80 ml per addition, and to add the organic solvent 2 to 6 times at intervals of 10 minutes or more.

[0035] At least at the time of filing, the present patent also protects inventions that do not require the introduction of a liquid organic solvent into the activating atmosphere gas introduction pipe.

[0036] That is, the present invention is a method for treating metal members using a treatment furnace, comprising: a metal member charging step of charging metal members into the treatment furnace; an activation atmosphere gas introducing step of introducing an activation atmosphere gas into the treatment furnace; a first heating step of heating the activation atmosphere gas in the treatment furnace to a first temperature; a main atmosphere gas introducing step of introducing a nitriding atmosphere gas or a soft-nitriding atmosphere gas into the treatment furnace after the first heating step; and a second heating step of heating the nitriding atmosphere gas or the soft-nitriding atmosphere gas in the treatment furnace to a second temperature in order to nitride or soft-nitrid the metal members, wherein a liquid organic solvent is intermittently charged into the treatment furnace a plurality of times during the first heating step.

[0037] According to the present invention, by intermittently adding the liquid organic solvent in multiple batches, it is possible to add an appropriate amount of organic solvent at a timing that suits the conditions inside the processing furnace.

[0038] The present invention also provides a metal member processing apparatus comprising: a processing furnace; a metal member charging mechanism for charging metal members into the processing furnace; an atmospheric gas introduction pipe arranged to communicate with the processing furnace and for introducing atmospheric gas into the processing furnace; an organic solvent introduction device for intermittently introducing a liquid organic solvent into the atmospheric gas introduction pipe multiple times; and a heating device for heating the atmospheric gas in the processing furnace to a predetermined temperature.

[0039] According to the present invention, by introducing a liquid organic solvent (which may be a chloride in addition to a carbon compound or a carbon-nitrogen compound) into the atmosphere gas introduction pipe while the introduction of an activated atmosphere gas into the processing furnace is continuing, it is possible to effectively prevent the organic solvent from vaporizing and flowing back even when the temperature of the processing furnace is high.

[0040] Furthermore, according to the present invention, by intermittently adding the liquid organic solvent in multiple batches, it is possible to add an appropriate amount of organic solvent at a timing that is appropriate for the conditions inside the processing furnace.

[0041] The organic solvent introduction device preferably has a check valve on the upstream side of the atmospheric gas introduction pipe.

[0042] This prevents backflow of the organic solvent, allowing for more accurate injection of the appropriate amount of organic solvent. Furthermore, because undesired evaporation of the organic solvent is suppressed, a general-purpose check valve can be used.

[0043] It is also preferable that a dehumidifying device be provided midway along the atmospheric gas introduction pipe.

[0044] This effectively prevents the performance of the metal member from deteriorating due to moisture that may be contained in the atmospheric gas.

[0045] It is also preferable that the metal member feeding mechanism is configured to feed the metal members into and out of the processing furnace in a horizontal direction.

[0046] This is preferable because even if precipitation of the organic solvent occurs, there is a relatively small risk of the precipitate coming into contact with the metal member (in a mode in which the metal member is loaded and unloaded from above the furnace, there is a relatively large risk of the metal member coming into contact with the precipitate that has formed around the furnace opening).

[0047] It is also preferable that the atmospheric gas is an activated atmospheric gas, and that a second treatment furnace for nitriding or nitrocarburizing is provided separately from the treatment furnace.

[0048] According to this, since the activation treatment and the nitriding treatment or soft nitriding treatment can be performed in separate treatment furnaces, there is absolutely no risk of organic solvent precipitation during the nitriding treatment or soft nitriding treatment. Furthermore, since the nitriding treatment or soft nitriding treatment and the subsequent activation treatment of the metal member can be performed simultaneously, productivity is also increased (compared to simply preparing two treatment devices, there is no need to add an organic solvent to the treatment furnace for the nitriding treatment or soft nitriding treatment, which reduces costs accordingly).

[0049] At least at the time of filing, the present patent also protects inventions that do not require the introduction of a liquid organic solvent into the activating atmosphere gas introduction pipe.

[0050] That is, the present invention provides a metal member processing apparatus comprising: a processing furnace; a metal member introduction mechanism for introducing metal members into the processing furnace; an atmospheric gas introduction pipe arranged to communicate with the processing furnace and for introducing atmospheric gas into the processing furnace; an organic solvent introduction device that intermittently introduces a liquid organic solvent into the processing furnace multiple times; and a heating device that heats the atmospheric gas in the processing furnace to a predetermined temperature.

[0051] According to the present invention, by intermittently adding the liquid organic solvent in multiple batches, it is possible to add an appropriate amount of organic solvent at a timing that suits the conditions inside the processing furnace.

[0052] According to the present invention, by intermittently adding the liquid organic solvent in multiple batches, it is possible to add an appropriate amount of organic solvent at a timing that is appropriate for the conditions inside the processing furnace.

[0053] Furthermore, according to one aspect of the present invention, by introducing a liquid organic solvent (which may be a chloride in addition to a carbon compound or a carbon-nitrogen compound) into the activation atmosphere gas inlet pipe while the introduction of the activation atmosphere gas into the processing furnace is continuing, it is possible to effectively prevent the organic solvent from evaporating and flowing back even when the temperature of the processing furnace is high.

[0054] FIG. 1 is a schematic diagram of a metal member treatment apparatus according to a first embodiment of the present invention. FIG. 2 is a schematic cross-sectional view of a circulation type treatment furnace (horizontal gas nitriding furnace). FIG. 3 is an image diagram showing an example of control for the introduction of an organic solvent. FIG. 4 is a schematic diagram of a modified example of a metal member treatment apparatus according to the first embodiment. FIG. 5 is a photograph of a circular stain. FIG. 6 is a schematic diagram of a further modified example of a metal member treatment apparatus according to the first embodiment. FIG. 7 is a schematic diagram of a metal member treatment apparatus according to a second embodiment of the present invention. FIG. 8 is a schematic diagram of a modified example of a metal member treatment apparatus according to the second embodiment. FIG. 9 is a schematic diagram of a further modified example of a metal member treatment apparatus according to the second embodiment.

[0055] [First embodiment] Fig. 1 is a schematic diagram of a metal member treatment apparatus 1 (nitriding treatment apparatus) according to a first embodiment of the present invention. As shown in Fig. 1, the treatment apparatus 1 of this embodiment is equipped with a circulation type treatment furnace 2, and only two types of gases, namely ammonia and ammonia decomposition gas, are introduced into the circulation type treatment furnace 2. The ammonia decomposition gas is a gas also called AX gas, and is a mixed gas consisting of nitrogen and hydrogen in a ratio of 1:3.

[0056] (Overview of Treatment Furnace 2) An example of the cross-sectional structure of the circulating treatment furnace 2 is shown in FIG. 2. In FIG. 2, a cylinder 202 called a retort is disposed within a furnace wall (also called a bell) 201 incorporating a heater (heating device) 201h. Further inside the retort, a cylinder 204 (φ700 mm × 1000 mm) called an inner retort is disposed (the heater 201h is conceptually illustrated in FIG. 2, and actual arrangements vary). As indicated by the arrows in the figure, the gas introduced through a gas introduction pipe 205 passes around the metal member serving as the workpiece, and then circulates through the space between the two cylinders 202 and 204 by the action of a stirring fan 203. Reference numeral 206 denotes a gas exhaust device with a flare, 207 denotes a thermocouple, 208 denotes a lid for cooling, and 209 denotes a fan for cooling. The circulating treatment furnace 2 is also called a horizontal gas nitriding furnace, and its structure is known.

[0057] (Outline of Metal Member S) The metal member S is, for example, stainless steel or heat-resistant steel, and is, for example, a unison ring or internal crank, which are turbocharger parts for automobiles, or an engine valve for automobiles, etc. However, in the following examples, SUS304 plate material (50 mm x 50 mm x 1 mm) and SUS301S plate material (50 mm x 50 mm x 1 mm) are used.

[0058] (Basic Configuration of Processing Apparatus 1) As shown in FIG. 1 , the processing furnace 2 of the processing apparatus 1 of this embodiment is provided with a furnace opening / closing lid 7 (metal member introduction mechanism), an agitation fan 8, an agitation fan drive motor 9, an atmospheric gas concentration detection device 3, a nitriding potential regulator 4, a programmable logic controller 31, and an in-furnace gas supply unit 20.

[0059] The agitating fan 8 is disposed in the processing furnace 2 and rotates within the processing furnace 2 to agitate the atmosphere within the processing furnace 2. The agitating fan drive motor 9 is connected to the agitating fan 8 and is configured to rotate the agitating fan 8 at a desired rotation speed.

[0060] The atmospheric gas concentration detection device 3 is composed of a sensor capable of detecting the hydrogen concentration or ammonia concentration in the process furnace 2 as the furnace atmospheric gas concentration. The detection body of the sensor is in communication with the interior of the process furnace 2 via an atmospheric gas detection pipe 12. In this embodiment, the atmospheric gas detection pipe 12 is formed as a path that directly connects the sensor body of the atmospheric gas concentration detection device 3 with the process furnace 2, and is connected midway to an in-furnace gas waste pipe 40 that leads to an exhaust gas combustion decomposition device 41. As a result, the atmospheric gas is divided into a gas that is to be disposed of and a gas that is to be supplied to the atmospheric gas concentration detection device 3.

[0061] After detecting the atmospheric gas concentration in the furnace, the atmospheric gas concentration detector 3 outputs an information signal including the detected concentration to the nitriding potential regulator 4 .

[0062] The nitriding potential regulator 4 includes an in-furnace nitriding potential calculation device 13 and a gas flow rate output adjustment device 30. The programmable logic controller 31 includes a gas introduction amount control device 14 and a parameter setting device 15.

[0063] The in-furnace nitriding potential calculation device 13 calculates the nitriding potential in the processing furnace 2 based on the hydrogen concentration or ammonia concentration detected by the atmospheric gas concentration detection device 3. Specifically, a calculation formula for the nitriding potential programmed according to the actual gas introduced into the furnace is incorporated, and the nitriding potential is calculated from the value of the atmospheric gas concentration in the furnace.

[0064] The parameter setting device 15 is configured, for example, by a touch panel, and is capable of setting and inputting the total flow rate of gas introduced into the furnace, the gas type, the processing temperature, the target nitriding potential, etc. The set and input parameter values ​​are transmitted to the gas flow rate output adjusting device 30.

[0065] The gas flow rate output adjusting device 30 performs control using the nitriding potential calculated by the in-furnace nitriding potential calculating device 13 as an output value, the target nitriding potential (set nitriding potential) as a target value, and the respective amounts of ammonia gas and ammonia decomposition gas introduced as input values. More specifically, for example, control can be performed in which the total flow rate of the introduced amounts of ammonia gas and ammonia decomposition gas is kept constant and the introduction ratio of each is changed. The output value of the gas flow rate output adjusting device 30 is transmitted to the gas introduction rate control device 14.

[0066] The gas introduction amount control device 14 is configured to send control signals to a first supply amount control device 22 (specifically, a mass flow controller) for ammonia gas and a second supply amount control device 26 (specifically, a mass flow controller) for ammonia decomposition gas, respectively, in order to realize the introduction amount of each gas.

[0067] The furnace introduction gas supply unit 20 of this embodiment has a first furnace introduction gas supply unit 21 for ammonia gas, a first supply amount control device 22, and a first supply valve 23. The furnace introduction gas supply unit 20 of this embodiment also has a second furnace introduction gas supply unit 25 for ammonia decomposition gas (AX gas), a second supply amount control device 26, and a second supply valve 27.

[0068] In this embodiment, the ammonia gas and the ammonia decomposition gas are mixed in the furnace gas introduction pipe 29 before entering the processing furnace 2 .

[0069] The first furnace introduction gas supply unit 21 is formed of, for example, a tank filled with the first furnace introduction gas (ammonia gas in this example).

[0070] The first supply amount control device 22 is formed by a mass flow controller and is interposed between the first furnace introduction gas supply unit 21 and the first supply valve 23. The opening degree of the first supply amount control device 22 changes in response to a control signal output from the gas introduction amount control device 14. The first supply amount control device 22 detects the supply amount from the first furnace introduction gas supply unit 21 to the first supply valve 23 and outputs an information signal including this detected supply amount to the gas introduction amount control device 14. This control signal can be used to correct the control by the gas introduction amount control device 14, etc.

[0071] The first supply valve 23 is formed by an electromagnetic valve that switches between an open and closed state in response to a control signal output from the gas introduction amount control device 14 , and is provided downstream of the first supply amount control device 22 .

[0072] The second furnace introduction gas supply unit 25 is formed, for example, by a tank filled with the second furnace introduction gas (ammonia decomposition gas in this example). Alternatively, the second furnace introduction gas supply unit 25 may be a pipe provided from a pyrolysis furnace that thermally decomposes ammonia gas to generate ammonia decomposition gas.

[0073] The second supply amount control device 26 is formed by a mass flow controller and is interposed between the second furnace introduction gas supply unit 25 and the second supply valve 27. The opening degree of the second supply amount control device 26 changes in response to a control signal output from the gas introduction amount control device 14. The second supply amount control device 26 also detects the supply amount from the second furnace introduction gas supply unit 25 to the second supply valve 27 and outputs an information signal including the detected supply amount to the gas introduction amount control device 14. The control signal can be used to correct the control by the gas introduction amount control device 14, etc.

[0074] The second supply valve 27 is formed by an electromagnetic valve that switches between an open and closed state in response to a control signal output from the gas introduction amount control device 14 , and is provided downstream of the second supply amount control device 26 .

[0075] The processing apparatus 1 of this embodiment is configured to introduce a first furnace introduction gas (ammonia gas) and a second furnace introduction gas (ammonia decomposition gas) into the processing furnace 2 as activation atmosphere gases as a pretreatment for nitriding to activate the surface of the metal member S. Furthermore, during the pretreatment, the heater 201h is configured to heat the activation atmosphere gas in the processing furnace 2 to a first temperature (a specific example will be described later, for example, 350°C to 550°C).

[0076] After the pretreatment, the processing apparatus 1 of this embodiment is configured to introduce the first furnace introduction gas (ammonia gas) and the second furnace introduction gas (AX gas) into the processing furnace 2 as nitriding atmosphere gas under feedback control in order to nitride and harden the surface of the metal member S. During the pretreatment, the heater 201h is configured to heat the nitriding atmosphere gas in the processing furnace 2 to a second temperature (for example, 520°C to 650°C, a specific example of which will be described later).

[0077] (New Features of the Processing Apparatus 1) The processing apparatus 1 of this embodiment has a new feature in that it is equipped with an organic solvent introduction device 300 that intermittently introduces a liquid organic solvent into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) multiple times.

[0078] The organic solvent introduction device 300 includes a tank 301 filled with an organic solvent (specific examples will be described later), an organic solvent introduction pipe 302 extending from the container 301 to the inside of the furnace gas introduction pipe 29, a pump 303 provided midway along the organic solvent introduction pipe 302 to send the organic solvent in the container 301 toward the furnace gas introduction pipe 29, and a check valve 304 provided downstream of the pump 303.

[0079] The pump 303 is configured to deliver a predetermined amount of organic solvent (e.g., 0 to 100 ml) per delivery toward the furnace gas introduction pipe 29 intermittently multiple times at a predetermined interval (e.g., 0 to 120 minutes) at a predetermined delivery rate (e.g., 0 to 5000 ml / min).

[0080] The operating conditions of the pump 303 are controlled by an organic solvent feeding control device 305. Specifically, in this embodiment, the organic solvent is fed at a substantially uniform rate over a period of 1 second to 2 minutes (preferably 10 to 2 minutes) in an amount of 10 to 80 ml per feed, 2 to 6 times at intervals of 10 minutes or more.

[0081] The tip of the organic solvent introduction pipe 302 (e.g., a cylindrical pipe with a diameter of 3 mm) penetrates the pipe wall of the in-furnace gas introduction pipe 29 (e.g., a cylindrical pipe with a diameter of 27 mm) at a substantially right angle and extends into the in-furnace gas introduction pipe 29 (for example, protruding toward the central axis by approximately 300 mm (the exemplified dimensions may vary depending on the size of the processing furnace 2)). The in-furnace gas introduction pipe 29 extends into the processing furnace 2, and its tip forms an inclined surface (a slope of approximately 45°) (with the shorter side facing downward and the pointed tip facing upward), and the tip of the organic solvent introduction pipe 302 has a shape that is cut along a plane perpendicular to the axis of the organic solvent introduction pipe 302.

[0082] The check valve 304 is a general-purpose check valve for a liquid medium. In this embodiment, there is very little risk of the liquid organic solvent undesirably evaporating, so no special specifications are required.

[0083] (Operation of the Processing Apparatus 1: Pretreatment) Next, the operation of the processing apparatus 1 of this embodiment will be described. First, metal members S as the articles to be processed are loaded horizontally into the circulating processing furnace 2 through the furnace opening / closing lid 7 (metal member loading mechanism). Then, the circulating processing furnace 2 is heated by the heater 201h.

[0084] Thereafter, ammonia gas and ammonia decomposition gas are introduced as activated atmospheric gases at a set flow rate from the furnace introduction gas supply unit 20 through the furnace introduction gas introduction pipe 29 (atmospheric gas introduction pipe) into the processing furnace 2. The set flow rates can be set and input in the parameter setting device 15, and are controlled by a first supply amount control device 22 (mass flow controller) and a second supply amount control device 26 (mass flow controller). In addition, the stirring fan drive motor 9 is driven to rotate the stirring fan 8, thereby stirring the atmosphere in the processing furnace 2.

[0085] Meanwhile, the organic solvent feeding device 300 intermittently feeds a liquid organic solvent multiple times into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) while continuing to introduce the activated atmospheric gas (ammonia gas and ammonia decomposition gas) into the processing furnace 2. Here, the conditions for feeding the organic solvent by the organic solvent feeding device 300 can be set and input in the parameter setting device 15 and are controlled by the pump 303.

[0086] The liquid organic solvent introduced into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) is pushed out by the activated atmospheric gas (ammonia gas and ammonia decomposition gas) while remaining in the liquid state, and reaches the processing furnace 2. Then, the organic solvent is vaporized and thermally decomposed in the processing furnace 2.

[0087] The above-described pretreatment can activate the surface of the metal member S. Specifically, when the organic solvent is a compound containing at least one type of hydrocarbon, HCN produced during the reaction process starting from the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal member S, effectively activating the surface. Alternatively, when the organic solvent is a compound containing at least one type of chlorine, HCl produced during the reaction process starting from the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal member S, effectively activating the surface.

[0088] In particular, by adding the organic solvent intermittently multiple times, additional organic solvent is added during the progress of the pretreatment, which significantly enhances the effect of adding the organic solvent and significantly enhances the effect of activating the surface of the metal component S.

[0089] (Function of the Processing Apparatus 1: Nitriding Treatment) Thereafter, the heater 201h heats the circulation type processing furnace 2 to the desired nitriding treatment temperature. Meanwhile, in this embodiment, the introduction of the activated atmosphere gas (ammonia gas and ammonia decomposition gas) into the processing furnace 2 continues as the introduction of the nitriding atmosphere gas (the gas species continue, but the introduction amount can be changed). Specifically, a mixed gas of ammonia gas and ammonia decomposition gas is introduced into the processing furnace 2 from the furnace introduction gas supply unit 20 at a set initial flow rate for the nitriding treatment. This set initial flow rate can also be set and input in the parameter setting device 15 and is controlled by the first supply amount control device 22 and the second supply amount control device 26 (both mass flow controllers). In addition, the stirring fan drive motor 9 is driven to rotate the stirring fan 8, stirring the atmosphere in the processing furnace 2.

[0090] The in-furnace nitriding potential calculation device 13 of the nitriding potential regulator 4 calculates the nitriding potential in the furnace (which is initially an extremely high value (because there is no hydrogen in the furnace) but decreases as the decomposition of ammonia gas (hydrogen generation) progresses), and determines whether or not it has fallen below the sum of the target nitriding potential and a reference deviation value. This reference deviation value can also be set and input in the parameter setting device 15.

[0091] When it is determined that the calculated value of the nitriding potential in the furnace falls below the sum of the target nitriding potential and the reference deviation value, the nitriding potential regulator 4 starts to control the amount of gas introduced into the furnace via the gas introduction amount control device 14.

[0092] The in-furnace nitriding potential calculation device 13 of the nitriding potential regulator 4 calculates the in-furnace nitriding potential based on the input hydrogen concentration signal or ammonia concentration signal. The gas flow rate output adjustment device 30 then performs PID control with the nitriding potential calculated by the in-furnace nitriding potential calculation device 13 as an output value, the target nitriding potential (set nitriding potential) as a target value, and the amount of gas introduced into the furnace as an input value. Specifically, in this PID control, for example, control is performed to change the introduction ratio of the amount of ammonia gas introduced and the amount of ammonia decomposition gas introduced, while keeping the total flow rate of these gases constant. In this PID control, each setting parameter value set and input by the parameter setting device 15 is used. For example, different values ​​are prepared as the setting parameter values ​​depending on the value of the target nitriding potential.

[0093] Then, as a result of PID control, the gas flow rate output adjusting device 30 controls the amount of each gas introduced into the furnace. Specifically, the gas flow rate output adjusting device 30 determines the flow rate of each gas, and the output value is transmitted to the gas introduction rate control device 14.

[0094] The gas introduction amount controller 14 sends control signals to a first supply amount controller 22 for ammonia gas and a second supply amount controller 26 for ammonia decomposition gas, respectively, to realize the introduction amounts of each gas.

[0095] By the above-described control, the nitriding potential in the furnace can be stably controlled to be close to the target nitriding potential, thereby enabling the nitriding treatment of the surface of the metal member S to be carried out with extremely high quality.

[0096] (Specific Examples) Using the treatment device 1 of this embodiment, the practical effects of adding the following six types of organic solvents were verified. Formamide, xylene, and toluene are examples of liquid compounds containing hydrocarbons. Trichloroethylene, tetrachloroethylene, and tetrachloroethane are examples of liquid compounds containing chlorine.

[0097]

[0098] As the metal members S, five sheets of SUS316 plate material (50 mm x 50 mm x 1 mm) and five sheets of SUS310S plate material (50 mm x 50 mm x 1 mm) were loaded in a vertical position.

[0099] The pretreatment temperature was 420°C, and the set flow rates of ammonia gas and ammonia decomposition gas introduced as activation atmosphere gases were 35 L / min (constant) and 5 L / min (constant), respectively. The pretreatment duration was 1 hour, and the organic solvent was added at a substantially uniform rate of 20 mL per addition over 1 minute, four times with 14-minute intervals. The first addition of the organic solvent began when the temperature inside the treatment furnace 2 reached 420°C, and the pretreatment was completed 14 minutes after the fourth addition of the organic solvent (see FIG. 3).

[0100] The nitriding temperature was set to 580° C., the set initial flow rate of ammonia gas introduced as the nitriding atmosphere gas was set to 17 L / min, and the set initial flow rate of ammonia decomposition gas introduced as the nitriding atmosphere gas was set to 23 L / min. The duration of the nitriding treatment was set to 5 hours, the target nitriding potential was set to 1.5, and the introduced flow rate of the nitriding atmosphere gas was feedback controlled.

[0101] Thereafter, the processing furnace 2 (and the metal member S) was cooled using a cooling lid 208 and a cooling fan 209 (see FIG. 2).

[0102] The thickness of the nitride layer formed on the surface of the metal member S was measured by observing the vicinity of the surface of the cut metal member S with an optical microscope. The average values ​​of the measured values ​​are shown in the table below.

[0103]

[0104] Next, as a comparative example, the addition of the organic solvent was changed to adding 80 ml of the organic solvent only once at a substantially uniform rate over one minute, and the timing for starting the addition was set to the timing when the temperature inside the processing furnace 2 reached 420°C. The other conditions were the same as those in the above example. The thickness of the nitride layer formed on the surface of the metal member S was measured by observing the vicinity of the surface of the cut metal member S with an optical microscope. The average values ​​of the measured values ​​are shown in the table below.

[0105]

[0106] As shown in Tables 2 and 3, for SUS316, excellent effects were observed when all six types of organic solvents were added intermittently multiple times.

[0107] Furthermore, as shown in Tables 2 and 3, for SUS310S, excellent effects were observed when three types of organic solvents containing chloride were added intermittently multiple times.

[0108] In the processing apparatus 1 of this embodiment, it can be said that it is effective to selectively use either a method using HCN (carbon compound, carbon-nitrogen compound) or a method using HCl (chloride) depending on the grade of the steel (see paragraph 0013).

[0109] (Verification of Suitable Pretreatment Temperature) Depending on the pretreatment temperature, the ease of nitriding (ease of penetration of nitrogen atoms) in the subsequent nitriding treatment may vary. For a pretreatment temperature (first temperature) of 300°C to 550°C, a SUS316 plate (50 mm x 50 mm x 1 mm) was used as the metal member S, and other conditions were the same as in the above example. The thickness of the nitride layer formed on the surface of the metal member S was measured by observing the surface vicinity of the cut metal member S with an optical microscope. The average values ​​of the measured values ​​are shown in the table below. As can be seen from the table, a pretreatment temperature in the range of 400°C to 500°C was suitable.

[0110]

[0111] (Effects of the Processing Apparatus 1) According to the processing apparatus 1 of the present embodiment as described above, the organic solvent feeding device 300 feeds a liquid organic solvent (chlorides are also possible in addition to carbon compounds and carbon-nitrogen compounds) into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) while the introduction of activated atmospheric gas (ammonia gas and ammonia decomposition gas) into the processing furnace 2 is continuing, thereby effectively preventing the organic solvent from vaporizing and flowing back even when the temperature of the processing furnace 2 is high.

[0112] According to the processing apparatus 1 of this embodiment, the organic solvent feeding device 300 feeds the liquid organic solvent intermittently in multiple divided doses, thereby realizing the feeding of an appropriate amount of organic solvent at a timing appropriate for the state inside the processing furnace 2. This allows additional organic solvent to be fed during the progress of preprocessing, significantly enhancing the effect of feeding the organic solvent and significantly enhancing the effect of activating the surfaces of the metal components S. Specifically, by controlling the pump 303, the organic solvent can be fed at a substantially uniform rate over a period of 1 second to 2 minutes, with 10 to 80 ml of organic solvent being fed two to six times at intervals of 10 minutes or more.

[0113] Furthermore, according to the processing apparatus 1 of this embodiment, the organic solvent feeding device 300 has a check valve 304 upstream of the furnace gas introduction pipe 29 (atmospheric gas introduction pipe), which prevents backflow of the organic solvent and enables the feeding of an appropriate amount of organic solvent with higher accuracy.

[0114] Furthermore, according to the processing apparatus 1 of this embodiment, the metal members S are horizontally loaded into and unloaded from the processing furnace 2 via the furnace opening / closing lid 7. As a result, even if precipitation of the organic solvent occurs, there is a relatively small risk of the precipitate coming into contact with the metal members S.

[0115] In the processing apparatus 1 of this embodiment, the pretreatment temperature (first heating temperature) is preferably set within a range of 400° C. to 500° C. This temperature range allows the activation treatment of the metal member S to proceed favorably, while effectively preventing the organic solvent from evaporating and flowing back.

[0116] In the processing apparatus 1 of this embodiment, for example, the activation atmosphere gas may contain ammonia gas, and the organic solvent may be a compound containing at least one type of hydrocarbon. In this case, HCN generated during the reaction process starting with the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal component S, effectively activating the surface. More specifically, the organic solvent may be, for example, formamide, xylene, or toluene. In these cases, the present inventors have confirmed in an actual production furnace that it is effective to add the organic solvent at a substantially uniform rate over a period of 1 second to 2 minutes, with 10 to 80 ml added 2 to 6 times at intervals of 10 minutes or more.

[0117] Furthermore, in the processing apparatus 1 of this embodiment, for example, the activation atmosphere gas may contain ammonia gas, and the organic solvent may be a compound containing at least one type of chlorine. In this case, HCl generated during the reaction process starting with the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal component S, effectively activating the surface. More specifically, the organic solvent may be, for example, trichloroethylene, tetrachloroethylene, or tetrachloroethane. In these cases, the present inventors have confirmed in an actual production furnace that it is effective to add the organic solvent at a substantially uniform rate over a period of 1 second to 2 minutes, with 10 to 80 ml of the organic solvent added 2 to 6 times at intervals of 10 minutes or more.

[0118] (Modification of Processing Apparatus 1) Fig. 4 is a schematic diagram of a modification of the processing apparatus 1. As shown in Fig. 4, in this modification, a dehumidifier 331 is provided upstream of the first supply amount control device 22 for ammonia gas (an example of a location along the atmospheric gas introduction piping), and a dehumidifier 335 is provided upstream of the second supply amount control device 26 for ammonia decomposition gas (an example of a location along the atmospheric gas introduction piping). When the second furnace introduction gas supply unit 25 is a piping installed from a pyrolysis furnace that thermally decomposes ammonia gas to produce ammonia decomposition gas, a dehumidifier may be provided upstream of the pyrolysis furnace (the ammonia gas, which is the raw material for the ammonia decomposition gas, is dehumidified). Furthermore, when ammonia gas dehumidified by a dehumidifier upstream of the first supply amount control device 22 is distributed and supplied to the pyrolysis furnace, only this one dehumidifier is sufficient.

[0119] This effectively prevents performance degradation of the metal member S due to moisture that may be contained in the activation atmosphere gas (ammonia gas and ammonia decomposition gas). (According to the knowledge of the present inventors, if the moisture content is high, circular stains may appear on the metal member S after nitriding treatment (impairing the appearance). See FIG. 5.)

[0120] 6 is a schematic diagram of a further modified example of the processing device 1. In the modified example shown in FIG. 6, two processing devices 1' and 1'' are arranged to cooperate with each other.

[0121] The first processing apparatus 1' is used for activation processing, and compared to the processing apparatus 1 described above, the atmospheric gas detection pipe 12, the atmospheric gas concentration detection device 3, and the in-furnace nitriding potential calculation device 13 can be omitted.

[0122] The second treatment apparatus 1 ″ is used for nitriding treatment, and compared to the treatment apparatus 1 described above, the organic solvent feeding apparatus 300 can be omitted.

[0123] In addition, in this modified example, a mobile furnace 400 (vacuum furnace or atmospheric furnace) for transporting the metal components S that have been pre-processed by the first processing device 1' to the second processing device 1" is provided so as to be movable from the area near the furnace opening / closing cover 7 of the first processing device 1' to the area near the furnace opening / closing cover 7 of the second processing device 1".

[0124] In addition, as shown in FIG. 6, the first furnace introduction gas supply unit 21 (tank) for ammonia gas and the second furnace introduction gas supply unit 25 (tank or piping) for ammonia gas decomposition gas are shared between the two processing apparatuses 1′ and 1″.

[0125] According to this modified example, after the activation treatment is performed in the treatment furnace 2 of the first treatment device 1', the nitriding treatment can be performed in a separate treatment furnace 2 of the second treatment device 1'', so there is no risk of organic solvents precipitating during the nitriding treatment in the treatment furnace 2 of the second treatment device 1''.

[0126] Furthermore, according to this modified example, the nitriding treatment in the treatment furnace 2 of the second treatment apparatus 1'' and the activation treatment of the next metal member S in the treatment furnace 2 of the first treatment apparatus 1' can be carried out simultaneously, thereby increasing productivity.

[0127] [Second embodiment] Fig. 7 is a schematic diagram of a treatment apparatus 501 (nitrocarburizing treatment apparatus) for metal members according to a second embodiment of the present invention. As shown in Fig. 7, the treatment apparatus 501 of this embodiment also includes a circulation type treatment furnace 2 similar to the treatment apparatus 1 of the first embodiment, but uses three types of gases, namely ammonia, ammonia decomposition gas, and carbon dioxide gas, as the gases introduced into the circulation type treatment furnace 2.

[0128] Specifically, in the processing apparatus 501 of this embodiment, a third furnace introduction gas supply unit 561 for carbon dioxide gas, a third supply amount control device 562, and a third supply valve 563 are added to the furnace introduction gas supply unit 520.

[0129] The third furnace introduction gas supply unit 561 is formed of, for example, a tank filled with the third furnace introduction gas (carbon dioxide gas in this example).

[0130] The third supply amount control device 562 is also formed by a mass flow controller, and is interposed between the third furnace introduction gas supply unit 561 and the third supply valve 563. The opening degree of the third supply amount control device 562 changes in response to a control signal output from the gas introduction amount control device 14. The third supply amount control device 562 detects the supply amount from the third furnace introduction gas supply unit 561 to the third supply valve 563, and outputs an information signal including this detected supply amount to the gas introduction amount control device 14. This control signal can be used to correct the control by the gas introduction amount control device 14, etc.

[0131] The third supply valve 563 is formed by an electromagnetic valve that switches between an open and closed state in response to a control signal output from the gas introduction amount controller 14 , and is provided downstream of the third supply amount controller 562 .

[0132] In this embodiment, the ammonia gas, the ammonia decomposition gas, and the carbon dioxide gas are mixed in the furnace gas introduction pipe 29 before entering the processing furnace 2 .

[0133] The gas flow rate output adjusting device 30 is configured to perform control using the nitriding potential calculated by the in-furnace nitriding potential calculating device 13 of the nitriding potential adjuster 4 as an output value, the target nitriding potential (set nitriding potential) as a target value, and the respective amounts of ammonia gas and ammonia decomposition gas introduced as input values ​​(the amount of carbon dioxide gas introduced is kept constant). More specifically, for example, it is possible to perform control such that the total flow rate of the amount of ammonia gas introduced and the amount of ammonia decomposition gas introduced is kept constant and the introduction ratio of these gases is changed. The output value of the gas flow rate output adjusting device 30 is transmitted to the gas introduction amount control device 14.

[0134] The gas introduction amount control device 14 is configured to send control signals to a first supply amount control device 22 (specifically, a mass flow controller) for ammonia gas, a second supply amount control device 26 (specifically, a mass flow controller) for ammonia decomposition gas, and a third supply amount control device 562 (specifically, a mass flow controller) for carbon dioxide gas, in order to realize the introduction amount of each gas.

[0135] Also, in the processing apparatus 501 of this embodiment, as a pretreatment for the soft nitriding treatment, the first furnace introduction gas (ammonia gas) and the second furnace introduction gas (ammonia decomposition gas) can be introduced into the processing furnace 2 as activation atmosphere gases in order to activate the surface of the metal member S. Furthermore, during the pretreatment, the heater 201h can heat the activation atmosphere gas in the processing furnace 2 to a first temperature (a specific example will be described later, but for example, 350°C to 550°C).

[0136] After the pretreatment, the processing apparatus 1 of this embodiment is configured to introduce, as a soft nitriding atmosphere gas, the first furnace introduction gas (ammonia gas) and the second furnace introduction gas (AX gas) into the processing furnace 2 under feedback control (variable control) while controlling the third furnace introduction gas (carbon dioxide gas) to a constant amount, in order to soft-nitriding and harden the surface of the metal member S. During the pretreatment, the heater 201h is configured to heat the nitriding atmosphere gas in the processing furnace 2 to a second temperature (for example, 520°C to 650°C, a specific example of which will be described later).

[0137] Other configurations of the processing apparatus 501 of this embodiment are substantially the same as those of the processing apparatus 1 of the first embodiment. In Fig. 7, parts that are the same as those of the first embodiment are denoted by the same reference numerals. Further, detailed description of parts of this embodiment that are the same as those of the first embodiment will be omitted.

[0138] (Outline of Metal Member S) The metal member S to be soft-nitrided in this embodiment is also, for example, stainless steel or heat-resistant steel, and is, for example, a unison ring or internal crank, which are turbocharger parts for automobiles, or an engine valve for automobiles, etc. In the following example, a SUS304 plate material (50 mm x 50 mm x 1 mm) and a SUS301S plate material (50 mm x 50 mm x 1 mm) are used.

[0139] (Function of the Processing Apparatus 501: Pretreatment) Next, the function of the processing apparatus 501 of this embodiment will be described. First, metal members S as the articles to be processed are loaded horizontally into the circulating processing furnace 2 through the furnace opening / closing lid 7 (metal member loading mechanism). Then, the circulating processing furnace 2 is heated by the heater 201h.

[0140] Thereafter, ammonia gas and ammonia decomposition gas are introduced as activated atmospheric gases at set flow rates from the furnace introduction gas supply unit 520 through the furnace introduction gas introduction pipe 29 (atmospheric gas introduction pipe) into the processing furnace 2. The set flow rates can be set and input in the parameter setting device 15, and are controlled by the first supply amount control device 22 (mass flow controller) and the second supply amount control device 26 (mass flow controller). In addition, the stirring fan drive motor 9 is driven to rotate the stirring fan 8, thereby stirring the atmosphere in the processing furnace 2.

[0141] Meanwhile, the organic solvent feeding device 300 intermittently feeds a liquid organic solvent multiple times into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) while continuing to introduce the activated atmospheric gas (ammonia gas and ammonia decomposition gas) into the processing furnace 2. Here, the conditions for feeding the organic solvent by the organic solvent feeding device 300 can be set and input in the parameter setting device 15 and are controlled by the pump 303.

[0142] The liquid organic solvent introduced into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) is pushed out by the activated atmospheric gas (ammonia gas and ammonia decomposition gas) while remaining in the liquid state, and reaches the processing furnace 2. Then, the organic solvent is vaporized and thermally decomposed in the processing furnace 2.

[0143] The above-described pretreatment can activate the surface of the metal member S. Specifically, when the organic solvent is a compound containing at least one type of hydrocarbon, HCN produced during the reaction process starting from the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal member S, effectively activating the surface. Alternatively, when the organic solvent is a compound containing at least one type of chlorine, HCl produced during the reaction process starting from the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal member S, effectively activating the surface.

[0144] In particular, by adding the organic solvent intermittently multiple times, additional organic solvent is added during the progress of the pretreatment, which significantly enhances the effect of adding the organic solvent and significantly enhances the effect of activating the surface of the metal component S.

[0145] (Function of the Treatment Device 501: Nitrocarburizing Treatment) Thereafter, the heater 201h heats the circulation type treatment furnace 2 to a desired nitriding temperature. Meanwhile, in this embodiment, the introduction of an activated atmosphere gas into the treatment furnace 2 is started. That is, the introduction of ammonia gas and ammonia decomposition gas continues as the introduction of a nitriding atmosphere gas, while the introduction of carbon dioxide gas is started. Specifically, a mixed gas of ammonia gas, ammonia decomposition gas, and carbon dioxide gas is introduced into the treatment furnace 2 from the furnace introduction gas supply unit 20 at a set initial flow rate for the nitriding treatment. This set initial flow rate can also be set and input in the parameter setting device 15 and is controlled by the first supply amount control device 22, the second supply amount control device 26, and the third supply amount control device 562 (all of which are mass flow controllers). In addition, the stirring fan drive motor 9 is driven to rotate the stirring fan 8, thereby stirring the atmosphere in the treatment furnace 2.

[0146] The in-furnace nitriding potential calculation device 13 of the nitriding potential regulator 4 calculates the nitriding potential in the furnace (which is initially an extremely high value (because there is no hydrogen in the furnace) but decreases as the decomposition of ammonia gas (hydrogen generation) progresses), and determines whether or not it has fallen below the sum of the target nitriding potential and a reference deviation value. This reference deviation value can also be set and input in the parameter setting device 15.

[0147] When it is determined that the calculated value of the nitriding potential in the furnace falls below the sum of the target nitriding potential and the reference deviation value, the nitriding potential regulator 4 starts to control the amount of gas introduced into the furnace via the gas introduction amount control device 14.

[0148] The in-furnace nitriding potential calculation device 13 of the nitriding potential regulator 4 calculates the in-furnace nitriding potential based on the input hydrogen concentration signal or ammonia concentration signal. The gas flow rate output adjustment device 30 then performs PID control with the nitriding potential calculated by the in-furnace nitriding potential calculation device 13 as an output value, the target nitriding potential (set nitriding potential) as a target value, and the amount of gas introduced into the furnace as an input value. Specifically, in this PID control, for example, control is performed in which the introduction ratio of the amount of ammonia gas introduced and the amount of ammonia decomposition gas introduced is changed while keeping the total amount constant. In this PID control, each setting parameter value set and input by the parameter setting device 15 is used. For example, different values ​​are prepared as the setting parameter values ​​depending on the value of the target nitriding potential.

[0149] Then, as a result of PID control, the gas flow rate output adjusting device 30 controls the amount of each gas introduced into the furnace. Specifically, the gas flow rate output adjusting device 30 determines the flow rate of each gas, and the output value is transmitted to the gas introduction rate control device 14.

[0150] The gas introduction amount control device 14 sends control signals to the first supply amount control device 22 for ammonia gas, the second supply amount control device 26 for ammonia decomposition gas, and the third supply amount control device 562 for carbon dioxide gas, respectively, in order to realize the introduction amount of each gas.

[0151] By the above-described control, the nitriding potential in the furnace can be stably controlled to be close to the target nitriding potential, thereby enabling the nitriding treatment of the surface of the metal member S to be carried out with extremely high quality.

[0152] (Specific Example) Using the treatment device 501 of this embodiment, the practical effect of adding the six types of organic solvents shown in Table 1 above was verified.

[0153] As the metal members S, five sheets of SUS316 plate material (50 mm x 50 mm x 1 mm) and five sheets of SUS310S plate material (50 mm x 50 mm x 1 mm) were loaded in a vertical position.

[0154] The pretreatment temperature was 420°C, and the set flow rates of ammonia gas and ammonia decomposition gas introduced as activation atmosphere gases were 35 L / min (constant) and 5 L / min (constant), respectively. The pretreatment duration was 1 hour, and the organic solvent was added at a substantially uniform rate of 20 mL per addition over 1 minute, four times with 14-minute intervals. The first addition of the organic solvent began when the temperature inside the treatment furnace 2 reached 420°C, and the pretreatment was completed 14 minutes after the fourth addition of the organic solvent (see FIG. 3).

[0155] The soft nitriding temperature was set to 580°C, the set initial flow rate of ammonia gas introduced as the soft nitriding atmosphere gas was set to 17 L / min, the set initial flow rate of ammonia decomposition gas introduced as the soft nitriding atmosphere gas was set to 23 L / min, and the set flow rate (constant) of carbon dioxide gas introduced as the soft nitriding atmosphere gas was set to 2 L / min. The duration of the soft nitriding treatment was set to 5 hours, the target nitriding potential was set to 1.5, and the introduced flow rate of the soft nitriding atmosphere gas was feedback controlled.

[0156] Thereafter, the processing furnace 2 (and the metal member S) was cooled using a cooling lid 208 and a cooling fan 209 (see FIG. 2).

[0157] The thickness of the soft nitride layer formed on the surface of the metal member S was measured by observing the vicinity of the surface of the cut metal member S with an optical microscope. The average values ​​of the measured values ​​are shown in the following table.

[0158]

[0159] Next, as a comparative example, the addition of the organic solvent was changed to adding 80 ml of the organic solvent only once at a substantially uniform rate over one minute, and the timing for starting the addition was set to the timing when the temperature inside the treatment furnace 2 reached 420°C. The other conditions were the same as those in the above-mentioned example. Then, the thickness of the soft nitride layer formed on the surface of the metal member S was measured by observing the vicinity of the surface of the cut metal member S with an optical microscope. The average values ​​of the measured values ​​are shown in the table below.

[0160]

[0161] As shown in Tables 5 and 6, for SUS316, excellent effects were observed when all six types of organic solvents were added intermittently multiple times.

[0162] Furthermore, as shown in Tables 5 and 6, for SUS310S, excellent effects were observed when three types of organic solvents containing chloride were added intermittently multiple times.

[0163] In the processing apparatus 501 of this embodiment, it can be said that it is effective to selectively use either the method using HCN (carbon compound, carbon-nitrogen compound) or the method using HCl (chloride) depending on the grade of the steel type (see paragraph 0013).

[0164] (Effects of Treatment Device 501) With the treatment device 501 of the present embodiment as described above, the organic solvent feeding device 300 feeds a liquid organic solvent (chlorides are also possible in addition to carbon compounds and carbon-nitrogen compounds) into the furnace gas introduction pipe 29 (atmospheric gas introduction pipe) while the introduction of activated atmospheric gas (ammonia gas and ammonia decomposition gas) into the treatment furnace 2 is continuing, thereby effectively preventing the organic solvent from vaporizing and flowing back even when the temperature of the treatment furnace 2 is high.

[0165] Furthermore, in the treatment apparatus 501 of this embodiment, the organic solvent supply device 300 can supply the liquid organic solvent intermittently in multiple divided doses, thereby realizing supply of an appropriate amount of organic solvent at a timing appropriate for the state inside the treatment furnace 2. This allows additional organic solvent to be supplied during the progress of pretreatment, significantly enhancing the effect of supplying the organic solvent and significantly enhancing the effect of activating the surfaces of the metal components S. Specifically, by controlling the pump 303, the organic solvent can be supplied at a substantially uniform rate over a period of 1 second to 2 minutes, with 10 to 80 ml of organic solvent being supplied at each dose, 2 to 6 times at intervals of 10 minutes or more.

[0166] Also in the treatment apparatus 501 of this embodiment, the organic solvent feeding device 300 has a check valve 304 upstream of the furnace gas introduction pipe 29 (atmospheric gas introduction pipe), which prevents backflow of the organic solvent and enables the feeding of an appropriate amount of organic solvent with higher accuracy.

[0167] Furthermore, in the processing apparatus 501 of this embodiment, the metal members S are also loaded and unloaded horizontally into and from the processing furnace 2 via the furnace opening / closing lid 7. As a result, even if precipitation of the organic solvent occurs, there is a relatively small risk of the precipitate coming into contact with the metal members S.

[0168] In the treatment apparatus 501 of this embodiment, the pretreatment temperature (first heating temperature) is also preferably set within a range of 400° C. to 500° C. This temperature range allows the activation treatment of the metal member S to proceed favorably, while effectively suppressing the occurrence of a situation in which the organic solvent evaporates and flows back.

[0169] In the processing apparatus 501 of this embodiment, the activation atmosphere gas may contain ammonia gas, and the organic solvent may be a compound containing at least one type of hydrocarbon. In this case, HCN generated during the reaction process starting with the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal component S, effectively activating the surface. More specifically, the organic solvent may be, for example, formamide, xylene, or toluene. In these cases, the present inventors have confirmed in an actual production furnace that it is effective to add the organic solvent at a substantially uniform rate over a period of 1 second to 2 minutes, with 10 to 80 ml added 2 to 6 times at intervals of 10 minutes or more.

[0170] Furthermore, in the processing apparatus 501 of this embodiment, for example, the activation atmosphere gas may contain ammonia gas, and the organic solvent may be a compound containing at least one type of chlorine. In this case, HCl generated during the reaction process starting with the thermal decomposition of the organic solvent reduces the passivation film on the surface of the metal component S, effectively activating the surface. More specifically, the organic solvent may be, for example, trichloroethylene, tetrachloroethylene, or tetrachloroethane. In these cases, the present inventors have confirmed in an actual production furnace that it is effective to add the organic solvent at a substantially uniform rate over a period of 1 second to 2 minutes, in an amount of 10 to 80 ml, 2 to 6 times with an interval of 10 minutes or more.

[0171] (Modification of Treatment Apparatus 501) Fig. 8 is a schematic diagram of a modification of the treatment apparatus 501. As shown in Fig. 8, in this modification, a dehumidifier 331 is provided upstream of the first supply amount control device 22 for ammonia gas (an example of a location along the atmospheric gas introduction piping), and a dehumidifier 335 is provided upstream of the second supply amount control device 26 for ammonia decomposition gas (an example of a location along the atmospheric gas introduction piping). When the second in-furnace introduction gas supply unit 25 is a piping installed from a pyrolysis furnace that thermally decomposes ammonia gas to produce ammonia decomposition gas, a dehumidifier may be installed upstream of the pyrolysis furnace (the ammonia gas, which is the raw material for the ammonia decomposition gas, is dehumidified). Furthermore, when ammonia gas dehumidified by a dehumidifier upstream of the first supply amount control device 22 is distributed and supplied to the pyrolysis furnace, only this one dehumidifier is sufficient.

[0172] This effectively prevents performance degradation of the metal component S due to moisture that may be contained in the activation atmosphere gas (ammonia gas and ammonia decomposition gas). (According to the knowledge of the present inventors, if the moisture content is high, circular stains may appear on the metal component S after soft nitriding (impairing the appearance). See FIG. 5.)

[0173] 9 is a schematic diagram of a further modified example of the processing device 501. In the modified example shown in FIG. 9, two processing devices 501' and 501'' are configured to work together.

[0174] The first treatment device 501′ is used for activation treatment, and compared to the aforementioned treatment device 501, the atmospheric gas detection piping 12, the atmospheric gas concentration detection device 3, the in-furnace nitriding potential calculation device 13, the third supply amount control device 562, and the third supply valve 563 can be omitted.

[0175] The second treatment device 501 ″ is used for soft nitriding treatment, and compared to the treatment device 501 described above, the organic solvent injection device 300 can be omitted.

[0176] In addition, in this modified example, a mobile furnace 400 (vacuum furnace or atmospheric furnace) for transporting metal components S that have been pre-processed by the first processing device 501' to the second processing device 501" is provided so as to be movable from the area near the furnace opening / closing cover 7 of the first processing device 501' to the area near the furnace opening / closing cover 7 of the second processing device 501".

[0177] In addition, as shown in FIG. 9, the first furnace introduction gas supply unit 21 (tank) for ammonia gas and the second furnace introduction gas supply unit 25 (tank or piping) for ammonia gas decomposition gas are shared between the two treatment devices 501′ and 501″.

[0178] According to this modified example, after the activation treatment is performed in the treatment furnace 2 of the first treatment device 501′, the soft nitriding treatment can be performed in a separate treatment furnace 2 of the second treatment device 501″, so there is absolutely no risk of organic solvents precipitating during the soft nitriding treatment in the treatment furnace 2 of the second treatment device 501″.

[0179] Furthermore, according to this modified example, the soft nitriding treatment in the treatment furnace 2 of the second treatment device 501″ and the activation treatment of the next metal member S in the treatment furnace 2 of the first treatment device 501′ can be carried out simultaneously, thereby increasing productivity.

[0180] 1 Processing device 1' First processing device 1" Second processing device 3 Atmospheric gas concentration detection device 4 Nitriding potential regulator 7 Furnace opening / closing lid 8 Stirring fan 9 Stirring fan drive motor 12 Atmospheric gas detection piping 13 In-furnace nitriding potential calculation device 14 Gas introduction amount control device 15 Parameter setting device 20 Furnace introduction gas supply unit 21 First furnace introduction gas supply unit 22 First supply amount control device 23 First supply valve 25 Second furnace introduction gas supply unit 26 Second supply amount control device 27 Second supply valve 29 Furnace introduction gas introduction piping 30 Gas flow rate output adjustment device 31 Programmable logic controller 40 Furnace gas waste piping 41 Exhaust gas combustion decomposition device 201h Heater 202 Cylinder 203 Stirring fan 204 Cylinder 205 Gas introduction pipe 206 Gas exhaust device 208 Lid 209 Fan 300 Organic solvent introduction device 301 Tank 302 Organic solvent introduction pipe 303 Pump 304 Check valve 305 Organic solvent introduction control device 331 Dehumidifier 335 Dehumidifier 400 Mobile furnace S Metal member 501 Treatment device 501' First treatment device 501" Second treatment device 561 Third furnace introduction gas supply section 562 Third supply amount control device 563 Third supply valve

Claims

1. A method for treating metal members using a treatment furnace, comprising the steps of: a metal member introduction step of introducing metal members into a treatment furnace; an activation atmosphere gas introduction step of introducing an activation atmosphere gas into the processing furnace; a first heating step of heating an activation atmosphere gas in the processing furnace to a first temperature; a main atmosphere gas introduction step of introducing a nitriding atmosphere gas or a soft nitriding atmosphere gas into the treatment furnace after the first heating step; a second heating step of heating the nitriding atmosphere gas or the nitrocarburizing atmosphere gas in the treatment furnace to a second temperature in order to nitride or nitrocarburize the metal member; Equipped with During the first heating step, a liquid organic solvent is intermittently introduced into the treatment furnace a plurality of times; The activation atmosphere gas contains ammonia gas, The organic solvent is a compound containing at least one type of hydrocarbon. A processing method comprising:

2. The organic solvent is any one of formamide, xylene, and toluene.

2. The method of claim 1.

3. A method for treating metal members using a treatment furnace, comprising the steps of: a metal member introduction step of introducing metal members into a treatment furnace; an activation atmosphere gas introduction step of introducing an activation atmosphere gas into the processing furnace; a first heating step of heating an activation atmosphere gas in the processing furnace to a first temperature; a main atmosphere gas introduction step of introducing a nitriding atmosphere gas or a soft nitriding atmosphere gas into the treatment furnace after the first heating step; a second heating step of heating the nitriding atmosphere gas or the nitrocarburizing atmosphere gas in the treatment furnace to a second temperature in order to nitride or nitrocarburize the metal member; Equipped with During the first heating step, a liquid organic solvent is intermittently introduced into the treatment furnace a plurality of times; The activation atmosphere gas contains ammonia gas, The organic solvent is a compound containing at least one type of chlorine. A processing method comprising:

4. The organic solvent is any one of trichloroethylene, tetrachloroethylene, and tetrachloroethane.

4. The method according to claim 3.

5. In the activation atmosphere gas introduction step, the activation atmosphere gas is introduced into the processing furnace through an activation atmosphere gas introduction pipe, During at least a part of the first heating step, the activation atmosphere gas introduction step is performed simultaneously, During the period, the organic solvent in a liquid state is intermittently introduced into the activation atmosphere gas introduction pipe multiple times.

5. The method according to claim 1, wherein the first and second electrodes are arranged in a first direction.

6. The organic solvent is added at a substantially uniform rate over a period of 1 second to 2 minutes, with an amount of 10 to 80 ml per addition, and is added 2 to 6 times with an interval of 10 minutes or more.

6. The method according to claim 5 .

7. The first temperature is between 400° C. and 500° C.

7. The method according to claim 1, wherein the first and second electrodes are arranged in a first direction.

8. A processing furnace; a metal member input mechanism for inputting metal members into the processing furnace; an atmospheric gas supply pipe that is arranged so as to communicate with the processing furnace and that introduces an atmospheric gas into the processing furnace; an organic solvent supplying device for supplying a liquid organic solvent into the treatment furnace intermittently a plurality of times; a heating device for heating the atmospheric gas in the processing furnace to a predetermined temperature; Equipped with The atmospheric gas is an activated atmospheric gas, The activation atmosphere gas contains ammonia gas, The organic solvent is a compound containing at least one type of hydrocarbon. A processing device for metal members comprising:

9. The organic solvent is any one of formamide, xylene, and toluene.

9. The processing device according to claim 8.

10. A processing furnace; a metal member input mechanism for inputting metal members into the processing furnace; an atmospheric gas supply pipe that is arranged so as to communicate with the processing furnace and that introduces an atmospheric gas into the processing furnace; an organic solvent supplying device for supplying a liquid organic solvent into the treatment furnace intermittently a plurality of times; a heating device for heating the atmospheric gas in the processing furnace to a predetermined temperature; Equipped with The atmospheric gas is an activated atmospheric gas, The activation atmosphere gas contains ammonia gas, The organic solvent is a compound containing at least one type of chlorine. A processing device for metal members comprising:

11. The organic solvent is any one of trichloroethylene, tetrachloroethylene, and tetrachloroethane. The processing device according to claim 10 .

12. The organic solvent supplying device is configured to supply a liquid organic solvent intermittently multiple times into the processing furnace via the atmospheric gas introduction pipe.

12. The method according to claim 8, wherein the first and second electrodes are arranged in a first direction.

13. The organic solvent supplying device has a check valve on the upstream side of the atmospheric gas introduction pipe.

13. The processing apparatus according to claim 8, wherein the processing apparatus is a processing apparatus for performing a processing operation.

14. A dehumidifier is provided in the atmospheric gas introduction pipe.

14. The processing device according to claim 8,

15. The metal member input mechanism is configured to horizontally insert and remove the metal member into and from the processing furnace.

15. The processing apparatus according to claim 8,