AI Technical Summary
Existing inkjet recording methods fail to effectively suppress the occurrence of cracks when image recording materials are folded, particularly due to uneven water evaporation and differences in absorption spectra among various inks.
An inkjet recording method involving the application of ink containing a colorant and water on one side of a paper base material, followed by infrared irradiation and the application of a post-treatment liquid with a surfactant on the opposite side, which includes a pulp layer and a coating layer with specific dry coating amounts and compositions to control water evaporation and ink absorption.
The method significantly reduces the occurrence of cracks when the image recording material is folded by controlling water evaporation and ink absorption, ensuring the integrity and durability of the recorded image.
Abstract
Description
Inkjet recording method
[0001] The present disclosure relates to an inkjet recording method.
[0002] BACKGROUND ART In recent years, in a method of recording an image using a water-based ink containing water, improvements in various properties of the resulting image recording have been investigated.
[0003] For example, Japanese Patent Application Laid-Open No. 2017-124561 describes an image forming method for forming an image by ejecting droplets onto a recording medium, the image forming method comprising ejecting a post-treatment liquid onto at least the image on the recording medium on which the image has been formed, identifying an area of the recording medium that overlaps with the area on which the image is to be formed, and ejecting the post-treatment liquid into the identified area. Japanese Patent Application Laid-Open No. 2020-164333 describes a post-processing device including a post-processing unit that performs post-processing on a recording medium recorded with aqueous ink, a mounting unit on which the recording medium to be post-processed in the post-processing unit is mounted, a deformation suppression unit that suppresses deformation of the recording medium in the mounting unit due to predetermined parameters related to the recording process on the recording medium, and a control unit that controls the deformation suppression unit based on the predetermined parameters, wherein the control unit receives the predetermined parameters from a printer control unit that controls the recording and changes the suppression strength of the deformation suppression unit for the recording medium based on the predetermined parameters, and the predetermined parameters include information based on the conditions under which the recording was performed on the recording medium.
[0004] However, there are cases where it is required to prevent cracks from occurring when the image-recorded material is folded.
[0005] The present disclosure has been made in consideration of the above circumstances, and according to one embodiment of the present invention, an inkjet recording method is provided that can suppress the occurrence of cracks when an image-recorded product is folded.
[0006] The present disclosure includes the following aspects.
[0007] <1> A method for producing a paper substrate, comprising the steps of: applying an ink containing a colorant and water onto side A, which is one side of the paper substrate, by an inkjet recording method; irradiating side A to which the ink has been applied with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm; and applying a post-treatment liquid containing water and a surfactant onto side B, which is the other side of the paper substrate, in this order; the paper substrate comprises a pulp layer and a coating layer disposed on at least one side of the pulp layer; the coating layer comprises at least one white pigment selected from the group consisting of calcium carbonate and kaolin, and a binder; the coating layer is disposed on the side A side, and the dry coating weight of the coating layer disposed on the side A side is 15 g / m 2 ~50g / m 2 No coating layer is disposed on the B-side, or if a coating layer is disposed on the B-side, the dry coating amount of the coating layer disposed on the B-side is 10 g / m 2 <2> The inkjet recording method according to <1>, wherein the infrared rays are near-infrared rays having a maximum wavelength in the range of 800 nm to 1,400 nm. <3> The inkjet recording method according to <1> or <2>, wherein the post-treatment liquid has a surface tension of 22.5 mN / m to 40.0 mN / m. <4> In the step of applying the post-treatment liquid, the post-treatment liquid is applied in an amount of 10 g / m per unit area. 2 ~55g / m 2 <5> The inkjet recording method according to any one of <1> to <4>, wherein the surfactant includes a nonionic surfactant. <6> The inkjet recording method according to any one of <1> to <5>, wherein the surfactant has an HLB value of 8.0 to 14.0. <7> The paper substrate has a basis weight of 180 g / m 2 ~600g / m 2<8> The inkjet recording method according to any one of <1> to <7>, further comprising a step of applying a pretreatment liquid onto side A before a step of applying the ink, wherein in the step of applying the ink, the ink is applied onto side A to which the pretreatment liquid has been applied. <9> The inkjet recording method according to <8>, wherein the pretreatment liquid contains an organic acid.
[0008] According to one embodiment of the present invention, there is provided an inkjet recording method that can suppress the occurrence of cracks when an image recorded product is folded.
[0009] The inkjet recording method of the present disclosure will be described in detail below.
[0010] In this specification, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.
[0011] As used herein, the amount of each component in a composition refers to the total amount of the components in the composition unless otherwise specified, when the composition contains multiple substances corresponding to each component. In this specification, a combination of two or more preferred aspects is a more preferred aspect. As used herein, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0012] In this specification, the term "image" refers to a film in general, and "image recording" refers to the formation of an image (i.e., a film). The concept of "image" in this specification also includes a solid image.
[0013] In this specification, "(meth)acrylate" is a concept that encompasses both acrylate and methacrylate, "(meth)acryloyl group" is a concept that encompasses both acryloyl group and methacryloyl group, and "(meth)acrylic acid" is a concept that encompasses both acrylic acid and methacrylic acid.
[0014] [Inkjet Recording Method] The inkjet recording method according to the present disclosure comprises, in this order, a step of applying an ink containing a colorant and water onto side A, which is one side of a paper substrate, by an inkjet recording system; a step of irradiating side A to which the ink has been applied with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm; and a step of applying a post-treatment liquid containing water and a surfactant onto side B, which is the other side of the paper substrate; the paper substrate comprises a pulp layer and a coating layer disposed on at least one side of the pulp layer, the coating layer comprising at least one white pigment selected from the group consisting of calcium carbonate and kaolin, and a binder; the coating layer is disposed on the side A side, and the dry coating weight of the coating layer disposed on the side A side is 15 g / m 2 ~50g / m 2 No coating layer is disposed on the B-side, or if a coating layer is disposed on the B-side, the dry coating amount of the coating layer disposed on the B-side is 10 g / m 2 The following is the result.
[0015] As a result of extensive research, the present inventors have found that the inkjet recording method according to the present disclosure can suppress the occurrence of cracks when an image-recorded product is folded. The reason for this effect is presumed to be as follows.
[0016] Infrared rays have a high energy density and high drying efficiency. However, when infrared rays are applied to the ink-applied side (side A) of a paper substrate, even the water contained in the paper substrate volatilizes, making the image recording itself brittle and prone to cracking in the coating layer and the underlying pulp layer when the image recording is folded. Water volatilization is particularly likely to progress in areas of the paper substrate where no ink is applied. Furthermore, when multiple inks of different hues are applied, differences in the ink absorption spectra result in differences in the degree of drying for each ink. For example, compared to inks of hues such as yellow, magenta, and cyan, black ink absorbs more infrared rays, so water volatilization is more likely to progress in areas where black ink is applied. Cracking tends to occur more easily in areas where no ink is applied and in areas where black ink is applied when the image recording is folded.
[0017] In contrast, in the inkjet recording method according to the present disclosure, a post-treatment liquid containing water and a surfactant is applied to the surface (side B) of the paper substrate opposite to the surface (side A) to which the ink has been applied. The post-treatment liquid penetrates into the surface B of the paper substrate, thereby preventing cracks from occurring when the image-recorded product is folded.
[0018] In the image forming method described in JP 2017-124561 A, a post-treatment liquid is ejected onto an image formed on a recording medium. JP 2020-164333 A does not describe a post-treatment liquid containing water and a surfactant. Neither JP 2017-124561 A nor JP 2020-164333 A assumes that the image-recorded product will be folded.
[0019] The paper substrate used in the inkjet recording method according to the present disclosure and each step will be described in detail below.
[0020] <Paper substrate> The inkjet recording method according to the present disclosure includes the steps of applying an ink containing a pigment and water onto side A, which is one side of a paper substrate, by an inkjet recording method, and applying a post-treatment liquid containing water and a surfactant onto side B, which is the other side of the paper substrate. That is, side A of the paper substrate is the side to which the ink is applied, and side B of the paper substrate is the side to which the post-treatment liquid is applied.
[0021] The paper substrate used in the inkjet recording method according to the present disclosure includes a pulp layer and a coating layer disposed on at least one surface of the pulp layer.
[0022] The pulp layer may be a single layer or two or more layers may be overlapped.
[0023] The pulp layer is a layer containing pulp as a main component. Here, the main component refers to a component that accounts for 50% by mass or more of the components that make up the pulp layer.
[0024] Although the type of pulp is not particularly limited, from the viewpoint of strength, the pulp layer preferably contains chemical pulp. Examples of chemical pulp include hardwood kraft pulp (LKP) and softwood kraft pulp (NKP). The pulp may be bleached pulp or unbleached pulp. LKP and NKP may each be bleached pulp or unbleached pulp.
[0025] Examples of pulps other than the above-mentioned NKP and LKP include mechanical pulps such as stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), thermoground pulp (TGP), chemiground pulp (CGP), groundwood pulp (GP), and thermomechanical pulp (TMP); disintegrated recycled paper pulp (DIP) produced from used brown paper, kraft envelope paper, magazine paper, newspaper paper, flyer paper, office paper, cardboard paper, white paper, Kent paper, imitation paper, and land certificate paper; and pulps produced chemically or mechanically from non-wood fibers such as kenaf, hemp, and reed.
[0026] The coating layer may be disposed on both sides of the pulp layer, or may be disposed on only one side of the pulp layer.
[0027] In the paper substrate, a coating layer is disposed on the A-side, and the dry coating amount of the coating layer disposed on the A-side is 15 g / m 2 ~50g / m 2 No coating layer is disposed on the B-side, or if a coating layer is disposed on the B-side, the dry coating amount of the coating layer disposed on the B-side is 10 g / m 2 The following is the relationship between the surface area of the pulp layer and the surface area of the ink-applied ink. Therefore, when coating layers are disposed on both surfaces of the pulp layer, the surface on which the coating layer with a larger dry coating weight is disposed is surface A (i.e., the surface to which ink is applied), and the surface on which the coating layer with a smaller dry coating weight is disposed is surface B (i.e., the surface to which post-treatment liquid is applied). Furthermore, when a coating layer is disposed on only one surface of the pulp layer, the surface on which the coating layer is disposed is surface A (i.e., the surface to which ink is applied), and the surface on which the coating layer is not disposed is surface B (i.e., the surface to which post-treatment liquid is applied).
[0028] In the inkjet recording method according to the present disclosure, the dry coating amount of the coating layer disposed on the B-side is 10 g / m 2 Since the thickness is less than 100 nm, the post-treatment liquid can easily penetrate the image recording material, and the occurrence of cracks when the image recording material is folded is suppressed.
[0029] The dry coating amount of the coating layer disposed on the A-side is 15 g / m from the viewpoint of vividness of the finished image recording material. 2 ~40g / m 2 It is preferable that the thickness is 15 g / m 2 ~30g / m 2 It is more preferable that:
[0030] The dry coating amount of the coating layer arranged on the B side is 7 g / m from the viewpoint of suppressing cracking when folded. 2 Preferably, the amount is 4 g / m or less. 2 The dry coating amount of the coating layer disposed on the B-side is preferably 0 g / m or less. 2 The dry coating amount of the coating layer disposed on the B-side may be 0 g / m 2 This means that the coating layer is disposed on only one side of the pulp layer.
[0031] The coating layer contains at least one white pigment selected from the group consisting of calcium carbonate and kaolin, and a binder.
[0032] The type of binder contained in the coating layer is not particularly limited, and examples thereof include starch, styrene-butadiene copolymer, acrylic resin, polyvinyl acetate, and polyvinyl alcohol.
[0033] The content of the white pigment is not particularly limited, and is, for example, 50% by mass to 95% by mass relative to the total amount of the coating layer.
[0034] The content of the binder is not particularly limited, and is, for example, 5% by mass to 50% by mass relative to the total amount of the coating layer.
[0035] The basis weight of the paper substrate is not particularly limited, but is preferably 180 g / m 2 ~600g / m 2 It is preferable that the thickness is 250 g / m 2 ~400g / m 2 It is more preferable that:
[0036] Typically, the greater the basis weight of the paper substrate, the thicker it is. There are no particular limitations on the thickness of the paper substrate, but it is preferably 150 μm to 750 μm, and more preferably 200 μm to 500 μm. The thicker the paper substrate, the more likely it is to crack when the image-recorded product is folded. According to the inkjet recording method of the present disclosure, even if the basis weight of the paper substrate is within the above range, i.e., even if the thickness of the paper substrate is thick, the occurrence of cracks is suppressed when the image-recorded product is folded.
[0037] Basis weight is the weight of 1 m of paper substrate. 2 Basis weight means the mass per unit area. Basis weight is measured by the method described in JIS P8124:2011.
[0038] Commercially available products can be used as the paper substrate. Examples of commercially available products include "OK Ball", "UF Coat", and "NEW Pigeon" manufactured by Oji Materia Co., Ltd.; "NEW Ultra H", "Bilight Card", "NEW Refine", "JET Ace", "JET STAR F", and "Frosh White Card SF" manufactured by Nippon Paper Industries Co., Ltd.; "NEW Tough Ivory", "High Clean Coat", "NEW Clean Coat V", "NEW-DV-F", and "Maricoat-F" manufactured by Hokuetsu Corporation; "Crescendo", "TANGO", "Reliant Coated Cover", and "Carolina Coated Cover" manufactured by WestRock; and "UPM UniquePack" and "UPM" manufactured by UPM Specialty Papers. and "CrownBoard" and "Liquid FC" manufactured by BillerudKorsnas.
[0039] <Ink Application Step> The inkjet recording method according to the present disclosure includes a step of applying an ink containing a colorant and water onto side A, which is one surface of a paper substrate, by an inkjet recording method (hereinafter also referred to as the "ink application step").
[0040] (Ink) The ink applied in the ink application step contains water.
[0041] The water content of the ink is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more, relative to the total amount of the ink. The upper limit of the water content is not particularly limited, but is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less.
[0042] The ink applied in the ink application step contains at least one colorant.
[0043] The colorant may be a dye or a pigment, and from the viewpoint of durability such as heat resistance, light resistance, and water resistance, the colorant is preferably a pigment.
[0044] When a pigment is used as a colorant, the pigment can be contained in the ink as a pigment dispersion. The pigment dispersion is a liquid obtained by dispersing the pigment in a liquid medium using a pigment dispersant, and contains at least a pigment, a dispersant, and a liquid medium. Details of the dispersant will be described later. The liquid medium may be water or an organic solvent.
[0045] The pigment may be an organic pigment or an inorganic pigment.
[0046] Examples of organic pigments include azo pigments, polycyclic pigments, dye chelates, nitro pigments, nitroso pigments, and aniline black. Among these, azo pigments or polycyclic pigments are preferred. Examples of azo pigments include azo lakes, insoluble azo pigments, condensed azo pigments, and chelate azo pigments. Examples of polycyclic pigments include phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments. Examples of dye chelates include basic dye chelates and acid dye chelates.
[0047] Examples of inorganic pigments include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, and carbon black.
[0048] Examples of the pigment include those described in "Encyclopedia of Pigments" edited by Seijiro Ito (published in 2000), "Industrial Organic Pigments" by W. Herbst and K. Hunger, and JP-A Nos. 2002-12607, 2002-188025, 2003-26978, and 2003-342503.
[0049] The volume average particle diameter of the pigment in the ink is preferably 10 nm to 200 nm, more preferably 20 nm to 180 nm, and even more preferably 30 nm to 150 nm. When the volume average particle diameter is 200 nm or less, color reproducibility is improved and ejection properties are improved when recording images using an inkjet recording method. Furthermore, when the volume average particle diameter is 10 nm or more, light resistance is improved.
[0050] The particle size distribution of the pigment is not particularly limited, and may be either a broad particle size distribution or a monodisperse particle size distribution. Two or more pigments having a monodisperse particle size distribution may be mixed and used.
[0051] The volume average particle size and particle size distribution of the pigment are values measured using a particle size distribution measuring device (for example, Microtrac UPA (registered trademark) EX150 manufactured by Nikkiso Co., Ltd.).
[0052] The content of the colorant is preferably 1% by mass to 20% by mass, and more preferably 1% by mass to 10% by mass, based on the total amount of the ink.
[0053] When the ink applied in the ink application step contains a pigment, the ink preferably contains a pigment dispersant to disperse the pigment in water. In the present disclosure, a pigment dispersant is a compound that has the function of dispersing a pigment. The pigment dispersant adsorbs to the surface of the pigment, covering at least a portion of the surface of the pigment, thereby enabling the pigment to be dispersed in water. Note that when a self-dispersing pigment that can be dispersed in water even without a pigment dispersant is used as the pigment, the ink does not need to contain a pigment dispersant.
[0054] The form of the pigment dispersant contained in the ink is not particularly limited, and may be any of a random polymer, a block polymer, and a graft polymer. The pigment dispersant may also be a polymer having a crosslinked structure. In particular, the pigment dispersant is preferably a polymer having a crosslinked structure. When the pigment dispersant is a polymer having a crosslinked structure, it is thought that the pigment dispersant is less likely to detach from the surface of the pigment, and the dispersion stability of the pigment is high.
[0055] In this disclosure, a polymer refers to a compound having a weight average molecular weight of 1000 or more.
[0056] In this disclosure, the weight average molecular weight refers to a value measured by gel permeation chromatography (GPC). Measurements by gel permeation chromatography (GPC) are performed using an HLC (registered trademark)-8020GPC (manufactured by Tosoh Corporation) as a measuring device, three TSKgel (registered trademark) Super Multipore HZ-H columns (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), and THF (tetrahydrofuran) as an eluent. Measurements are performed using an RI detector at a sample concentration of 0.45% by mass, a flow rate of 0.35 ml / min, a sample injection volume of 10 μl, and a measurement temperature of 40°C. The calibration curve is prepared from eight samples of "Standard Sample TSK Standard, Polystyrene" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".
[0057] From the viewpoint of dispersion stability, the ratio of the content of the dispersant to the content of the pigment in the ink is preferably 0.5 to 3.0 by mass, and more preferably 1.0 to 2.0.
[0058] The ink applied in the ink application step preferably contains at least one organic solvent, from the viewpoint of improving the ejection properties.
[0059] Examples of organic solvents include polyhydric alcohols such as glycerin, 1,2,6-hexanetriol, trimethylolpropane, alkanediols (e.g., ethylene glycol, 1,2-propanediol), 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2-butene-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, 1,2-octanediol, 1,2-hexanediol, 1,2-pentanediol, 4-methyl-1,2-pentanediol, etc.), polyalkylene glycols (e.g., diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, dipropylene glycol, polyoxyethylene polyoxypropylene glycol, etc.); polyalkylene glycol ethers (e.g., diethylene glycol monoalkyl ether, triethylene glycol monoalkyl ether, tripropylene glycol monoalkyl ether, polyoxypropylene glyceryl ether, etc.); Examples include alkyl alcohols having 1 to 4 carbon atoms, 2-pyrrolidone, and N-methyl-2-pyrrolidone.
[0060] The content of the organic solvent is preferably 0.5% by mass to 30% by mass, more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 15% by mass, based on the total amount of the ink.
[0061] The ink applied in the ink application step preferably contains at least one water-soluble resin from the viewpoint of improving the ejection properties.
[0062] In the present disclosure, the term "water-soluble" in the context of a water-soluble resin means that the amount of the resin that dissolves in 100 g of water at 25°C is 1 g or more.
[0063] The water-soluble resin preferably contains a water-soluble resin X1 containing an alkyl group having 1 to 3 carbon atoms, an anionic group, and a cyclic structure.
[0064] When the water-soluble resin contains the water-soluble resin X1, the proportion of the water-soluble resin X1 in the total amount of the water-soluble resin is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass.
[0065] The alkyl group having 1 to 3 carbon atoms in the water-soluble resin X1 is a methyl group, an ethyl group, or a propyl group (i.e., an n-propyl group or an i-propyl group), preferably a methyl group or an ethyl group, more preferably a methyl group. The water-soluble resin X1 may contain only one type of alkyl group having 1 to 3 carbon atoms, or may contain two or more types.
[0066] The alkyl group having 1 to 3 carbon atoms in the water-soluble resin X1 may be introduced into the structure of the water-soluble resin X1 by polymerizing a polymerizable monomer containing an alkyl group having 1 to 3 carbon atoms. That is, the water-soluble resin X1 may contain a structural unit derived from a polymerizable monomer containing an alkyl group having 1 to 3 carbon atoms.
[0067] The polymerizable monomer containing an alkyl group having 1 to 3 carbon atoms is preferably a (meth)acrylic acid alkyl ester in which the alkyl group in the alkyl ester structure has 1 to 3 carbon atoms [hereinafter also referred to as "(meth)acrylic acid C1-3 alkyl ester"].
[0068] Specific examples of the (meth)acrylic acid C1-3 alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and i-propyl (meth)acrylate. The (meth)acrylic acid C1-3 alkyl ester is preferably methyl (meth)acrylate or ethyl (meth)acrylate, and more preferably methyl (meth)acrylate. Furthermore, the (meth)acrylic acid C1-3 alkyl ester is preferably methacrylic acid C1-3 alkyl ester.
[0069] When the water-soluble resin X1 contains a (meth)acrylic acid C1-3 alkyl ester unit, the water-soluble resin X1 may contain only one type of (meth)acrylic acid C1-3 alkyl ester unit or two or more types of (meth)acrylic acid C1-3 alkyl ester units. The content of the (meth)acrylic acid C1-3 alkyl ester units in the water-soluble resin X1 is preferably 3% by mass to 80% by mass, more preferably 3% by mass to 50% by mass, and even more preferably 5% by mass to 50% by mass, relative to the total amount of the water-soluble resin X1.
[0070] -Anionic Group- Examples of the anionic group in the water-soluble resin X1 include acid groups (e.g., carboxy groups, sulfo groups, phosphate groups, etc.) and salts of acid groups (e.g., salts of carboxy groups, salts of sulfo groups, salts of phosphate groups). The anionic group contained in the water-soluble resin X1 may be of one type only, or may be of two or more types. The water-soluble resin X1 may contain both an acid group and a salt of an acid group as the anionic group.
[0071] Salts of acid groups (e.g., salts of carboxy groups, salts of sulfo groups, and salts of phosphate groups) can be formed by neutralizing acid groups (e.g., carboxy groups, sulfo groups, and phosphate groups) with a neutralizing agent. The neutralization of the acid groups may be performed before or after polymerizing the polymerizable monomer containing an acid group. Neutralizing agents for neutralizing acid groups include inorganic bases such as hydroxides of alkali metals and hydroxides of alkaline earth metals, and organic bases such as organic amines. Examples of alkali metals include potassium (K) and sodium (Na). Examples of alkaline earth metals include calcium (Ca) and magnesium (Mg). Examples of alkali metal hydroxides include potassium hydroxide and sodium hydroxide. Examples of alkaline earth metal hydroxides include calcium hydroxide and magnesium hydroxide. Examples of organic amines include ammonia, primary amines (e.g., ethylamine, monoethanolamine, etc.), secondary amines (e.g., diethylamine, ethylenediamine, etc.), tertiary amines (e.g., triethylamine, triethanolamine, isopropylethylamine, pyrrolidine, piperidine, etc.), and quaternary ammonium salts. Among these, from the viewpoint of storage stability, organic amines having a boiling point of 80°C or higher are preferred. From the viewpoint of storage stability, alkali metal hydroxides or organic amines are preferred as neutralizing agents, and alkali metal hydroxides or organic amines having a boiling point of 80°C or higher are more preferred. Examples of organic amines having a boiling point of 80°C or higher include ethylenediamine (117°C), triethylamine (90°C), monoethanolamine (170°C), triethanolamine (208°C), isopropylethylamine (127°C), pyrrolidine (87°C), and piperidine (106°C).
[0072] The water-soluble resin X1 preferably contains at least one of a carboxy group and a salt of a carboxy group as an anionic group. In this case, the ratio of the salt of a carboxy group to the total of the carboxy group and the salt of a carboxy group (mol %; hereinafter, also referred to as the degree of neutralization) is preferably 40 mol % or more, preferably 50 mol % or more, more preferably 60 mol % or more, and even more preferably 80 mol % or more. The upper limit of the degree of neutralization can be 100 mol %.
[0073] The anionic group that can be contained in the water-soluble resin X1 may be introduced into the structure of the water-soluble resin X1 by polymerizing a polymerizable monomer containing an anionic group (and, if necessary, neutralizing it with a neutralizing agent). That is, the water-soluble resin X1 may contain a structural unit derived from a polymerizable monomer containing an anionic group. As the polymerizable monomer containing an anionic group, (meth)acrylic acid is particularly preferred.
[0074] When the water-soluble resin X1 contains a structural unit derived from a polymerizable monomer containing an anionic group (for example, (meth)acrylic acid), the content of the structural unit derived from the polymerizable monomer containing an anionic group is preferably 5% by mass to 40% by mass, and more preferably 8% by mass to 20% by mass, based on the total amount of the water-soluble resin X1.
[0075] The cyclic structure in the water-soluble resin X1 preferably contains at least one of an aromatic ring and an aliphatic ring, and more preferably contains an aromatic ring. The water-soluble resin X1 may contain only one type of cyclic structure or two or more types of cyclic structures.
[0076] In the present disclosure, the term "aromatic ring" refers to a cyclic unsaturated ring having aromaticity. Examples of the aromatic ring include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, an anthracene ring, and a pyrene ring; and heteroaromatic rings such as a pyridine ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazolyl ring, and an acridone ring. Among these, the aromatic ring is preferably an aromatic hydrocarbon ring.
[0077] When the cyclic structure in the water-soluble resin X1 contains an aromatic ring, the aromatic ring can be introduced into the structure of the water-soluble resin X1 by polymerization of a polymerizable monomer containing an aromatic ring. As the polymerizable monomer containing an aromatic ring, a polymerizable monomer containing an aromatic ring and an ethylenically unsaturated double bond is preferred, and a vinyl polymerizable monomer containing an aromatic ring is more preferred. Examples of the polymerizable monomer containing an aromatic ring include styrene, methylstyrene, divinylbenzene, vinylpyridine, diallyl phthalate, and (meth)acrylates containing an aromatic ring (e.g., benzyl acrylate, phenoxyethyl acrylate, etc.).
[0078] The polymerizable monomer containing an aromatic ring may be unsubstituted, or may be a substituted polymerizable monomer substituted with a substituent. Examples of the substituent include a halogen atom, an alkyl group, a carboxylic acid group, and a hydroxyl group. Examples of the halogen atom include a chlorine atom, a bromine atom, and an iodine atom. The alkyl group is preferably an alkyl group having 1 to 12 carbon atoms (preferably 1 to 8 carbon atoms), and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, and a hexyl group. The alkyl group may be unsubstituted, or may have the same substituent as above.
[0079] Specific examples of structural units derived from polymerizable monomers having an aromatic ring that can be contained in the water-soluble resin X1 are the same as the specific examples of structural units derived from polymerizable monomers having an aromatic ring that can be contained in the pigment dispersion resin described above.
[0080] The content of the structural unit derived from a polymerizable monomer having a cyclic structure (e.g., an aromatic ring) in the water-soluble resin X1 is preferably 50% by mass to 85% by mass, more preferably 60% by mass to 80% by mass, based on the total amount of the water-soluble resin X1.
[0081] It is particularly preferred that the water-soluble resin X1 contains a structural unit derived from a C1-3 alkyl (meth)acrylate ester (i.e., a (meth)acrylate alkyl ester in which the alkyl group in the alkyl ester structure has 1 to 3 carbon atoms), a structural unit derived from (meth)acrylic acid, and a structural unit derived from a polymerizable monomer containing a cyclic structure. The preferred contents of each structural unit in this embodiment are as described above. In the above embodiment, the concept of a "structural unit derived from (meth)acrylic acid" encompasses both a structural unit obtained by polymerization of (meth)acrylic acid (i.e., a structural unit containing a carboxy group) and a structural unit obtained by polymerization and neutralization of (meth)acrylic acid (i.e., a structural unit containing a salt of a carboxy group) (here, neutralization may be carried out before or after polymerization).
[0082] The weight-average molecular weight of the water-soluble resin X1 is preferably 5,000 to 100,000. When the weight-average molecular weight of the water-soluble resin X1 is within this range, image bleeding and blocking are further suppressed. In addition, the ink ejection properties are further improved. From the viewpoint of ink ejection properties, the weight-average molecular weight of the water-soluble resin X1 is more preferably 10,000 to 80,000, and even more preferably 10,000 to 30,000.
[0083] The ink applied in the ink application step preferably contains a surfactant. The type of surfactant is not particularly limited, and may be any of anionic surfactants, cationic surfactants, betaine surfactants, and nonionic surfactants.
[0084] The content of the surfactant is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass, based on the total amount of the ink.
[0085] The ink applied in the ink application step may contain additives such as wax, colloidal silica, an antifoaming agent, a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, a conductive salt, and a basic compound, as necessary.
[0086] The surface tension of the ink applied in the ink application step is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 25 mN / m to 45 mN / m.
[0087] The surface tension of the ink is measured at a temperature of 25° C. using a surface tensiometer, for example, an automatic surface tensiometer (product name "DY-300") manufactured by Kyowa Interface Science Co., Ltd.
[0088] The viscosity of the ink applied in the ink application step is preferably 1.2 mPa·s to 15.0 mPa·s, more preferably 2.0 mPa·s to 13.0 mPa·s or less, and even more preferably 2.5 mPa·s to 10.0 mPa·s or less.
[0089] The viscosity of the ink is measured at a temperature of 30° C. using a rotational viscometer, for example, a product name "VISCOMETER TV-22" manufactured by Toki Sangyo Co., Ltd.
[0090] From the viewpoint of storage stability of the ink, the pH of the ink applied in the ink application step is preferably 6.0 to 11.0, more preferably 7.0 to 10.0, and even more preferably 7.0 to 9.0.
[0091] The pH of the ink is measured at a temperature of 25° C. using a pH meter, for example, a product name "WM-50EG" manufactured by Toa DDK Corporation.
[0092] (Inkjet Recording Method) The inkjet recording method is not particularly limited as long as it is a method capable of recording an image, and any known method can be used. Examples of inkjet recording methods include a charge control method that uses electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electric signal into an acoustic beam and irradiates the ink with it, thereby ejecting the ink using radiation pressure, and a thermal inkjet (Bubble Jet (registered trademark)) method that heats the ink to form bubbles and uses the resulting pressure.
[0093] Inkjet heads used in inkjet recording methods include a shuttle method in which a short serial head is used and recording is performed while the head is scanned in the width direction of the substrate, and a line method in which a line head is used in which recording elements are arranged corresponding to the entire area of one side of the substrate.
[0094] In the line method, a pattern can be formed over the entire surface of a substrate by scanning the substrate in a direction intersecting the arrangement direction of the recording elements, eliminating the need for a transport system such as a carriage for scanning a short head. Furthermore, the line method does not require complex scanning control of the carriage movement and the substrate, and only the substrate moves, making it possible to achieve faster recording speeds than the shuttle method.
[0095] The volume of ink droplets ejected from the inkjet head is preferably 1 pL (picoliter) to 100 pL, more preferably 1 pL to 10 pL, and even more preferably 1 pL to 5 pL.
[0096] <Infrared Irradiation Step> The inkjet recording method according to the present disclosure includes a step of irradiating the ink-applied side A with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm (hereinafter also referred to as the "infrared irradiation step").
[0097] By irradiating the ink with infrared rays, the ink applied in the ink application step is dried.
[0098] The maximum wavelength in infrared radiation refers to the wavelength at which the radiant energy density is greatest. The maximum wavelength is calculated from the radiator temperature according to Planck's law of radiation. For example, if the radiator is a filament, the maximum wavelength is 2,415 nm when the filament temperature is 1,200°C, and 828 nm when it is 3,500°C.
[0099] From the viewpoint of improving the scratch resistance of the image, the infrared rays are preferably near-infrared rays having a maximum wavelength in the range of 800 nm to 1,400 nm.
[0100] The irradiation energy of the infrared rays is not particularly limited, but from the viewpoint of drying property, it is preferably 50 kJ / m 2 ~500kJ / m 2Preferably, it is 60 kJ / m 2 ~400kJ / m 2 More preferably, it is 70 kJ / m 2 ~300 kJ / m 2 It is particularly preferred that:
[0101] The method of infrared irradiation is not particularly limited, and for example, irradiation can be performed using a device such as a normal infrared lamp, a xenon flash lamp, a xenon lamp, a xenon short arc lamp, a near-infrared halogen heater, an infrared LED, or an infrared laser.
[0102] <Post-treatment liquid application step> The inkjet recording method according to the present disclosure includes a step of applying a post-treatment liquid containing water and a surfactant onto side B, which is the other side of the paper substrate (hereinafter also referred to as a "post-treatment liquid application step").
[0103] The post-treatment liquid applied in the post-treatment liquid application step contains water.
[0104] The water content is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more, based on the total amount of the post-treatment liquid. The upper limit of the water content is not particularly limited, and is, for example, 99.95% by mass.
[0105] The post-treatment liquid applied in the post-treatment liquid application step contains at least one surfactant.
[0106] The type of surfactant is not particularly limited, and may be any of anionic surfactants, cationic surfactants, betaine surfactants, and nonionic surfactants.
[0107] Examples of anionic surfactants include fatty acid salts, alkyl sulfate ester salts, alkylbenzene sulfonates, alkylnaphthalene sulfonates, dialkyl sulfosuccinates, alkyl phosphate ester salts, naphthalene sulfonate-formalin condensates, and polyoxyethylene alkyl sulfate ester salts.
[0108] Examples of cationic surfactants include alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkylpyridinium salts, alkyl quaternary ammonium salts, alkyldimethylbenzylammonium salts, alkylisoquinolinium salts, dialkylmorphonium salts, polyoxyethylene alkylamines, alkylamine salts, polyamine fatty acid derivatives, amyl alcohol fatty acid derivatives, benzalkonium chloride, and benzethonium chloride.
[0109] Examples of betaine surfactants include coconut alkyl dimethylamine oxide and fatty acid amidopropyl dimethylamine oxide.
[0110] Examples of nonionic surfactants include polyoxyethylene higher alkyl ethers, polyoxyethylene higher alkyl phenyl ethers, higher fatty acid diesters of polyoxyethylene glycol, acetylene glycol surfactants, silicone surfactants, and fluorine surfactants.
[0111] Among these, the surfactant is preferably a nonionic surfactant. When the post-treatment liquid contains a nonionic surfactant, the post-treatment liquid easily penetrates into side B of the paper substrate, which is highly effective in suppressing cracks when the image-recorded product is folded.
[0112] The surfactant preferably has an HLB (Hydrophile-Lipophile Balance) value of 8.0 to 14.0, more preferably 9.0 to 13.0. When the HLB value of the surfactant is within the above range, the post-treatment liquid easily penetrates into side B of the paper substrate, which is highly effective in suppressing cracks when the image-recorded product is folded.
[0113] When the post-treatment liquid contains two or more surfactants, it is preferable that the weighted average value of the HLB values of the surfactants is within the above range.
[0114] The HLB value is calculated by the Kawakami formula below: HLB = 7 + 11.7 log (Mw / Mo), where Mw is the molecular weight of the hydrophilic group and Mo is the molecular weight of the hydrophobic group. In the present disclosure, when a catalog value can be confirmed for the HLB value, the catalog value is used as a priority.
[0115] The post-treatment liquid applied in the post-treatment liquid application step may contain additives such as a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, a conductive salt, a basic compound, etc., as required.
[0116] The surface tension of the post-treatment liquid applied in the post-treatment liquid application step is preferably 20.0 mN / m to 45.0 mN / m, more preferably 22.5 mN / m to 40.0 mN / m, and even more preferably 25.0 mN / m to 35.0 mN / m. The method for measuring the surface tension of the post-treatment liquid is the same as the method for measuring the surface tension of the ink.
[0117] When the surface tension of the post-treatment liquid is within the above range, the post-treatment liquid easily penetrates into side B of the paper substrate, and is therefore highly effective in preventing cracks from occurring when the image-recorded product is folded.
[0118] The method for applying the post-treatment liquid is not particularly limited, and examples thereof include known methods such as coating, dipping, flexographic printing, and inkjet recording.
[0119] The amount of post-treatment liquid applied per unit area was 3 g / m 2 ~70g / m 2 It is preferable that the density is 10 g / m 2 ~55g / m 2 It is more preferable that the application amount is 3 g / m 2 When the amount of application is 70 g / m or more, the occurrence of cracks when the image-recorded product is folded is further suppressed. 2 If it is equal to or less than this, the breaking strength of the image recording material is high, and it is possible to prevent the image recording material from breaking inside the device.
[0120] In the inkjet recording method according to the present disclosure, since the post-treatment liquid is allowed to penetrate into the paper substrate, thereby suppressing the occurrence of cracks when the image recording material is folded, it is preferable not to provide a step of heating and drying the post-treatment liquid after the post-treatment liquid application step.
[0121] <Pretreatment Liquid Application Step> In the inkjet recording method according to the present disclosure, from the viewpoint of improving the scratch resistance of the image, it is preferable to include, before the ink application step, a step of applying a pretreatment liquid onto side A (hereinafter also referred to as a "pretreatment liquid application step"). When the pretreatment liquid application step is included, in the ink application step, ink is applied onto side A to which the pretreatment liquid has been applied.
[0122] The pretreatment liquid applied in the pretreatment liquid application step preferably contains a flocculant. The flocculant is not particularly limited as long as it is a component that aggregates components in the ink. The flocculant is preferably at least one selected from the group consisting of polyvalent metal compounds, organic acids, metal complexes, and cationic polymers, and more preferably contains an organic acid.
[0123] -Polyvalent Metal Compound- Examples of polyvalent metal compounds include salts of alkaline earth metals of Group 2 of the periodic table (e.g., magnesium, calcium), transition metals of Group 3 of the periodic table (e.g., lanthanum), metals of Group 13 of the periodic table (e.g., aluminum), and lanthanides (e.g., neodymium).
[0124] The salts of these metals are preferably salts of organic acids, nitrates, chlorides, or thiocyanates, as described below.
[0125] Among these, the polyvalent metal compound is preferably a calcium salt or magnesium salt of an organic acid (e.g., formic acid, acetic acid, benzoic acid, etc.); a calcium salt or magnesium salt of nitric acid; calcium chloride, magnesium chloride, or a calcium salt or magnesium salt of thiocyanic acid.
[0126] It is preferable that the polyvalent metal compound is at least partially dissociated into polyvalent metal ions and counter ions in the pretreatment liquid.
[0127] Organic Acids Examples of organic acids include organic compounds having an acidic group.
[0128] Acidic groups include phosphate groups, phosphonate groups, phosphinate groups, sulfate groups, sulfonate groups, sulfinate groups, and carboxy groups.
[0129] Among these, from the viewpoint of the aggregation speed of the ink, the acidic group is preferably a phosphate group or a carboxy group, and more preferably a carboxy group.
[0130] It is preferable that at least a portion of the acidic groups is dissociated in the pretreatment liquid.
[0131] Examples of organic compounds having a carboxy group include (meth)acrylic acid, poly(meth)acrylic acid, acetic acid, formic acid, benzoic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, citric acid, tartaric acid, phthalic acid, 4-methylphthalic acid, lactic acid, pyrrolidonecarboxylic acid, pyronecarboxylic acid, pyrrolecarboxylic acid, furancarboxylic acid, pyridinecarboxylic acid, coumaric acid, thiophenecarboxylic acid, and nicotinic acid.
[0132] Among these, from the viewpoint of the aggregation speed of the ink, the organic compound having a carboxy group is preferably a divalent or higher carboxylic acid (hereinafter also referred to as a polycarboxylic acid), and more preferably a dicarboxylic acid.
[0133] Specifically, the polycarboxylic acid is preferably malonic acid, malic acid, maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, tartaric acid, 4-methylphthalic acid, or citric acid, and more preferably malonic acid, malic acid, tartaric acid, succinic acid, glutaric acid, pimelic acid, adipic acid, or citric acid.
[0134] The organic acid preferably has a low pKa (for example, 1.0 to 5.0), which reduces the surface charge of particles such as pigments and resin particles in the ink, which are stabilized by weakly acidic functional groups such as carboxyl groups, by contacting them with an organic acid having an even lower pKa, thereby lowering dispersion stability.
[0135] The organic acid preferably has a low pKa, high solubility in water, and a valence of at least 2. Furthermore, the organic acid more preferably has a high buffering capacity in a pH range lower than the pKa of the functional group (e.g., carboxy group) that stabilizes the dispersion of the particles in the ink.
[0136] -Metal Complex- The metal complex preferably contains, as a metal element, at least one selected from the group consisting of zirconium, aluminum, and titanium.
[0137] The metal complex is preferably a metal complex containing, as a ligand, at least one selected from the group consisting of acetate, acetylacetonate, methylacetoacetate, ethylacetoacetate, octylene glycolate, butoxyacetylacetonate, lactate, lactate ammonium salt, and triethanolamine.
[0138] The metal complex may be a commercially available product. Various organic ligands, particularly various polydentate ligands capable of forming metal chelate catalysts, are commercially available. Therefore, the metal complex may be a metal complex prepared by combining a commercially available organic ligand with a metal.
[0139] Examples of the metal complex include zirconium tetraacetylacetonate (e.g., "Orgatix ZC-150" manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium monoacetylacetonate (e.g., "Orgatix ZC-540" manufactured by Matsumoto Fine Chemical Co., Ltd.), and zirconium bisacetylacetonate (e.g., "Orgatix ZC-540" manufactured by Matsumoto Fine Chemical Co., Ltd.)."Orgatix ZC-550"), zirconium monoethylacetoacetate (for example, "Orgatix ZC-560" manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium acetate (for example, "Orgatix ZC-115" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium diisopropoxybis(acetylacetonate) (for example, "Orgatix TC-100" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium tetraacetylacetonate (for example, "Orgatix TC-401" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium dioctyloxybis(octylene glycolate) (for example, "Orgatix TC-200" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium diisopropoxybis(ethylacetoacet ... TC-750"), zirconium tetraacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix ZC-700"), zirconium tributoxymonoacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix ZC-540"), zirconium monobutoxyacetylacetonate bis(ethylacetoacetate) (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix ZC-570")), zirconium dibutoxy bis(ethylacetoacetate) (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix ZC-580"), aluminum trisacetylacetonate (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix AL-80"), titanium lactate ammonium salt (e.g., Matsumoto Fine Chemical Co., Ltd.'s "Orgatix Examples of suitable anti-oxidizing agents include titanium triethanolamine (e.g., "Orgatix TC-300" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium lactate (e.g., "Orgatix TC-310, 315" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium triethanolamine (e.g., "Orgatix TC-400" manufactured by Matsumoto Fine Chemical Co., Ltd.), and zirconyl chloride compounds (e.g., "Orgatix ZC-126" manufactured by Matsumoto Fine Chemical Co., Ltd.).
[0140] Among these, the metal complex is preferably a titanium lactate ammonium salt (e.g., "Orgatix TC-300" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium lactate (e.g., "Orgatix TC-310, 315" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium triethanolamine (e.g., "Orgatix TC-400" manufactured by Matsumoto Fine Chemical Co., Ltd.), or a zirconyl chloride compound (e.g., "Orgatix ZC-126" manufactured by Matsumoto Fine Chemical Co., Ltd.).
[0141] -Cationic Polymer- The pretreatment liquid may also contain one or more cationic polymers as a flocculating component. The cationic polymer is preferably a homopolymer of a cationic monomer having a primary to tertiary amino group or a quaternary ammonium salt group, or a copolymer or condensation polymer of a cationic monomer and a non-cationic monomer. The cationic polymer may be used in the form of either a water-soluble polymer or water-dispersible latex particles. Examples of cationic polymers include polyvinylpyridine salts, polyalkylaminoethyl acrylates, polyalkylaminoethyl methacrylates, polyvinylimidazole, polyethyleneimines, polybiguanides, polyguanides, polyallylamine, and derivatives thereof.
[0142] The weight-average molecular weight of the cationic polymer is preferably small from the viewpoint of the viscosity of the pretreatment liquid. When the pretreatment liquid is applied to a recording medium by an inkjet recording method, the weight-average molecular weight is preferably 1,000 to 500,000, more preferably 1,500 to 200,000, and even more preferably 2,000 to 100,000. A weight-average molecular weight of 1,000 or more is advantageous from the viewpoint of aggregation speed. A weight-average molecular weight of 500,000 or less is advantageous from the viewpoint of ejection reliability. However, this does not apply when the pretreatment liquid is applied to a recording medium by a method other than inkjet recording.
[0143] The pretreatment liquid may contain only one type of flocculant, or two or more types.
[0144] The content of the flocculant is preferably 0.1% by mass to 40% by mass, more preferably 0.1% by mass to 30% by mass, even more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 10% by mass, relative to the total amount of the pretreatment liquid.
[0145] The pretreatment liquid applied in the pretreatment liquid application step preferably contains water. The water content is not particularly limited, and is, for example, 40% by mass to 70% by mass.
[0146] The pretreatment liquid applied in the pretreatment liquid application step may contain other components in addition to the flocculant and water, as necessary. Examples of other components that may be contained in the pretreatment liquid include known additives such as organic solvents, resin particles, surfactants, solid wetting agents, colloidal silica, inorganic salts, anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, antifungal agents, pH adjusters, viscosity adjusters, rust inhibitors, chelating agents, and water-soluble polymer compounds (for example, the water-soluble polymer compounds described in paragraphs 0026 to 0080 of JP 2013-001854 A).
[0147] From the viewpoint of the aggregation rate of the ink, the pH of the pretreatment liquid is preferably 0.1 to 4.5, and more preferably 0.2 to 4.0. The method for measuring the pH of the pretreatment liquid is the same as the method for measuring the pH of the ink.
[0148] From the viewpoint of the aggregation speed of the ink, the viscosity of the pretreatment liquid is preferably 0.5 mPa·s to 10 mPa·s, and more preferably 1 mPa·s to 5 mPa·s. The viscosity is a value measured at 25°C using a viscometer. The method for measuring the viscosity of the pretreatment liquid is the same as the method for measuring the viscosity of the ink.
[0149] The surface tension of the pretreatment liquid is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The method for measuring the surface tension of the pretreatment liquid is the same as the method for measuring the surface tension of the ink.
[0150] The method for applying the pretreatment liquid is not particularly limited, and examples thereof include known methods such as a coating method, a dipping method, and an inkjet recording method.
[0151] Examples of the coating method include known coating methods using a bar coater, extrusion die coater, air doctor coater, blade coater, rod coater, knife coater, squeeze coater, reverse roll coater, and the like.
[0152] After the pretreatment liquid is applied, the pretreatment liquid applied to the paper substrate may be dried by heating. Examples of means for drying the pretreatment liquid by heating include known heating means such as a heater, known air blowing means such as a dryer, and a combination of these.
[0153] Examples of methods for heating and drying the pretreatment liquid include a method of applying heat using a heater or the like from the side opposite to the side of the paper substrate to which the pretreatment liquid has been applied, a method of applying warm or hot air to the side of the paper substrate to which the pretreatment liquid has been applied, a method of applying heat using an infrared heater from the side of the paper substrate to which the pretreatment liquid has been applied or the side opposite to the side to which the pretreatment liquid has been applied, and a combination of these methods.
[0154] The heating temperature during the heating and drying of the pretreatment liquid is preferably 35° C. or higher, and more preferably 40° C. or higher. The upper limit of the heating temperature is not particularly limited, and is, for example, 120° C.
[0155] The time for heat drying is not particularly limited, but is preferably 0.5 to 60 seconds, more preferably 0.5 to 20 seconds, and even more preferably 0.5 to 10 seconds.
[0156] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the present disclosure is not limited to these examples.
[0157] [Ink Preparation] The components shown in Table 1 were mixed to the contents (% by mass) shown in Table 1. After that, coarse particles were removed using a 1 μm filter, and cyan ink C1, magenta ink M1, yellow ink Y1, and black ink K1 were obtained. The average pigment particle size, pH, viscosity, surface tension, and electrical conductivity of each ink are shown in Table 1.
[0158] Details of each component listed in Table 1 are as follows.
[0159] Cyan pigment dispersion: Product name "Pro-jet Cyan APD1000", manufactured by FUJIFILM Imaging Colorants, pigment concentration 14.0% by mass Magenta pigment dispersion: Product name "Pro-jet Magenta APD1000", manufactured by FUJIFILM Imaging Colorants, pigment concentration 14.0% by mass Yellow pigment dispersion: Product name "Pro-jet Yellow TP APD1000", manufactured by FUJIFILM Imaging Colorants, pigment concentration 15.4% by mass Black pigment dispersion: Product name "Pro-jet Black APD1000", manufactured by FUJIFILM Imaging Colorants, pigment concentration 14.0% by mass
[0160] Aqueous solution of water-soluble resin PL-1: an aqueous solution of a water-soluble resin prepared by the following method 1,2-propanediol Acetylene glycol surfactant: product name "Olfine E1020", manufactured by Nissin Chemical Industry Co., Ltd. PEG 6000: product name "Polyethylene Glycol 6000", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Aqueous dispersion of ester wax: product name "Cellosol 524", manufactured by Chukyo Yushi Co., Ltd., solid content concentration 30 mass% Aqueous dispersion of colloidal silica: product name "Snowtex XS", manufactured by Nissan Chemical Industries, Ltd., solid content concentration 20 mass% Defoamer: product name "BYK-024", manufactured by BYK Japan
[0161] <Preparation of Aqueous Solution of Water-Soluble Resin PL-1> 1,2-propanediol (35 g) was charged into a 500 mL three-neck flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, and the temperature was raised to 90°C under a nitrogen stream. A mixed solution containing 5.55 g of dimethyl-2,2'-azobis(2-methylpropionate) (product name "V-601", Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, 10.7 g of methacrylic acid (MAA), 69.3 g of methyl methacrylate (MMA), 20.0 g of isobornyl methacrylate (IBOMA), 1.63 g of dodecyl mercaptan, and 65.00 g of 1,2-propanediol was added dropwise at a constant rate over 2 hours. After the dropwise addition of the mixed solution was completed, the mixture was stirred for 1 hour. Subsequently, a mixed solution of 1.85 g of V-601 and 24.62 g of 1,2-propanediol was added to the resulting reaction mixture, and the mixture was stirred for an additional 1.5 hours. After adding 120.21 g of 1,2-propanediol to the resulting reaction mixture, 8.56 g of a 50% by weight aqueous solution of sodium hydroxide was added dropwise using a dropping funnel to obtain an aqueous solution of water-soluble resin PL-1 (solids concentration: 30% by weight). The water-soluble resin PL-1 [MAA / MMA / IBOMA] had an acid value of 60 mgKOH / g and a weight-average molecular weight (Mw) of 15,000.
[0162]
[0163] [Preparation of Pretreatment Liquid 1] The following components were mixed and filtered using a 1 μm filter to obtain a pretreatment liquid 1 with a pH of 4.3. Malonic acid: 10.90% by mass Citric acid: 13.40% by mass Diethylene glycol monobutyl ether: 2.00% by mass Potassium hydroxide: 7.30% by mass Antifoaming agent (product name "BYK-038", manufactured by BYK Japan KK)... 0.05% by mass Polyacrylic acid having a weight average molecular weight of 25,000 (product name "Polyacrylic acid 25,000", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)... 0.95% by mass Ion-exchanged water... 65.40% by mass
[0164] [Preparation of Post-Treatment Liquid] The surfactants and water shown in Table 2 were mixed to the contents (mass %) shown in Table 2. The mixture was then filtered using a 1 μm filter to obtain post-treatment liquids PT-1 to PT-17. The type, classification, and HLB value of the surfactant are shown in Table 2.
[0165] Details of the surfactants listed in Table 2 are as follows:
[0166] ・Acetylene glycol surfactant 1: Product name "Olfine E1010", manufactured by Nissin Chemical Industry Co., Ltd. ・Acetylene glycol surfactant 2: Product name "Olfine E1020", manufactured by Nissin Chemical Industry Co., Ltd. ・Polyoxyethylene lauryl ether 1: Product name "Emulgen 102KG", manufactured by Kao Corporation ・Polyoxyethylene lauryl ether 2: Product name "Emulgen 103", manufactured by Kao Corporation ・Polyoxyethylene lauryl ether 3: Product name "Emulgen 105", manufactured by Kao Corporation ・Polyoxyethylene lauryl ether 4: Product name "Emulgen 108", manufactured by Kao Corporation ・Polyoxyethylene lauryl ether 5: Product name "Emulgen 109P", manufactured by Kao Corporation ・Polyoxyethylene lauryl ether 6: Product name "Emulgen 120", manufactured by Kao Corporation ・Polyoxyethylene lauryl ether 7: Product name "Emulgen 150", manufactured by Kao Corporation Silicone surfactant: Product name "BYK-347", manufactured by BYK Japan Alkylbenzene sulfonic acid: Product name "Paionin A-40", manufactured by Takemoto Yushi Co., Ltd. Lauryl trimethyl ammonium chloride: Product name "Paionin B-111", manufactured by Takemoto Yushi Co., Ltd. Fatty acid amidopropyl dimethylamine oxide: Product name "Paionin C-151", manufactured by Takemoto Yushi Co., Ltd.
[0167]
[0168] [Production of image recording material] In Examples 1 to 29 and Comparative Examples 1 and 2, single-sided coated paper (product name "UF Coat", manufactured by Oji Materia Co., Ltd.) was used as the paper substrate. The basis weight of the paper substrate used in each example is as shown in Table 3. In the paper substrate, the side on which the coating layer was disposed was designated "side A," and the side on which the coating layer was not disposed was designated "side B." The dry coating amount of the coating layer disposed on side A was approximately 18 g / m 2In Comparative Example 3, double-sided coated paper (product name "Bon Ivory+", manufactured by Oji Materia Co., Ltd., basis weight: 310 g / m) was used as the paper substrate. 2 The dry coating amount of each of the coating layers disposed on both sides was approximately 18 g / m 2 It was.
[0169] (1) Pretreatment liquid application process: A pretreatment liquid was applied to the A side of the paper substrate in an amount of 1.5 g / m 2 Pretreatment liquid 1 was applied using a coating bar so that the thickness of the coating became 1 / 4. Two seconds after application, hot air at a temperature of 100°C and a velocity of 15 m / sec was blown onto the coated surface from a height of 10 cm for 5 seconds to dry it. Note that in Example 29, the pretreatment liquid application step was not carried out.
[0170] (2) Ink Application Step Three seconds after the pretreatment liquid had dried, the black ink K1, cyan ink C1, magenta ink M1, and yellow ink Y1 were ejected in this order onto the surface of the paper substrate coated with the pretreatment liquid 1 (side A) under the conditions below by a single pass method, to record an image.
[0171] <Conditions> Inkjet head: 1,200 dpi (dots per inch) / 20-inch wide piezo full-line head arranged for four colors Droplet volume: 1.5 pL (picoliters) per pixel for each color Drive frequency: 60 kHz (substrate transport speed: 1,270 mm / sec)
[0172] (3) Infrared irradiation step: Two seconds after the ink is applied to side A, a near-infrared lamp with a maximum wavelength of 830 nm is used to irradiate side A with 250 kJ / m 2 In Example 24, an infrared lamp with a maximum wavelength of 2,400 nm was used instead of the near-infrared lamp.
[0173] (4) Post-treatment liquid application step Three seconds after irradiation with near-infrared rays or infrared rays, a post-treatment liquid shown in Table 3 was applied to side B of the paper substrate by flexographic printing in an amount shown in Table 3, thereby obtaining an image recorded matter. Note that in Comparative Example 1, the post-treatment liquid application step was not carried out.
[0174] [Evaluation and Measurement] The obtained image-recorded matter was evaluated for abrasion resistance, folding resistance, and strength. The evaluation methods are as follows. The evaluation results are shown in Table 3.
[0175] <Abrasion Resistance> An abrasion test was carried out using a Gakushin-type abrasion tester (manufactured by Yasuda Seiki Seisakusho). 30 seconds after the application of the post-treatment liquid was completed, the image recorded was fixed to the test piece table. An unused paper substrate (product name: UF Coat, basis weight: 310 g / m) was attached to the abrasion element. 2 A friction pad (manufactured by Oji Materia Co., Ltd.) was fixed so that the coating layer of the unused paper substrate faced the image-recorded surface of the image-recorded product. The friction pad was placed on the test piece, and a pressure of 240 g / cm was applied from above the friction pad. 2 The image of the rubbed portion was visually observed, and the rub resistance was evaluated based on the state of scratches and peeling on the image of the rubbed portion. The evaluation criteria are as follows: 3 or higher is a level that is not problematic in practical use.
[0176] 5: No scratches were found on the image in the rubbed area. 4: Slight scratches were found on the image in the rubbed area. 3: The image in the rubbed area had peeled off slightly, and very thin scratches were found. 2: The image in the rubbed area had peeled off, and the scratches were noticeable. 1: The image in the rubbed area had peeled off, and part of the paper base was exposed.
[0177] <Folding Endurance> 30 seconds after the application of the post-treatment liquid was completed, the image-recorded product was folded 180° so that the side on which the image was recorded was facing outward. After returning the image-recorded product to its original state, the folded portion was visually inspected, and folding endurance was evaluated based on the state of cracks. The evaluation criteria are as follows: 3 or higher is a level that is acceptable for practical use. 5: No cracks were observed in the folded portion. 4: Slight cracks were observed in the folded portion. 3: Slight cracks were observed in the folded portion. 2: Noticeable cracks were observed in the folded portion. 1: The folded portion was completely cracked.
[0178] <Strength> Ten minutes after the application of the post-treatment liquid was completed, the breaking strength of the image-recorded product was measured using a Tensilon universal testing machine (product name "FTF-1250", manufactured by Orientec Co., Ltd.) in an environment of 22°C and relative humidity of 60%. The breaking strength of the paper substrate before image recording was also measured using the same method. The strength was calculated based on the following formula: Strength (%) = (breaking strength of image-recorded product / breaking strength of paper substrate) × 100. Note that if the strength is less than 50%, problems such as tearing of the image-recorded product within the device may occur.
[0179] In Table 3, the type and basis weight of the paper substrate are listed. Regarding the pre-treatment liquid application step, "Y" is listed if it was performed, and "N" if it was not performed. Regarding the infrared irradiation step, the type of irradiation light is listed. Regarding the post-treatment liquid application step, the type, amount applied, and surface tension of the post-treatment liquid, as well as the classification, HLB value, and content of the surfactant contained in the post-treatment liquid are listed. Note that in Comparative Example 1, the post-treatment liquid application step was not performed, so "-" is listed in the column for the post-treatment liquid application step. In Comparative Example 2, water was used as the post-treatment liquid in the post-treatment liquid application step, so "-" is listed in the column for the surfactant contained in the post-treatment liquid.
[0180]
[0181] As shown in Table 3, Examples 1 to 29 comprised, in this order, a step of applying an ink containing a colorant and water onto side A of a paper substrate by an inkjet recording method; a step of irradiating side A to which the ink has been applied with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm; and a step of applying a post-treatment liquid containing water and a surfactant onto side B of the paper substrate; the paper substrate comprised a pulp layer and a coating layer disposed on at least one side of the pulp layer, the coating layer comprising at least one white pigment selected from the group consisting of calcium carbonate and kaolin, and a binder; the coating layer was disposed on the side A, and the dry coating weight of the coating layer disposed on the side A was 15 g / m. 2 ~50g / m 2 Since no coating layer was disposed on the B-side, it was possible to suppress the occurrence of cracks when the image-recorded product was folded.
[0182] On the other hand, in Comparative Example 1, since the post-treatment liquid application step was not carried out, it was found that cracks occurred when the image-recorded product was folded.
[0183] In Comparative Example 2, since water was used as the post-treatment liquid, it was found that cracks occurred when the image-recorded product was folded.
[0184] In Comparative Example 3, the paper substrate was a paper substrate having a dry coating amount of the coating layer of 10 g / m 2 It was found that because double-sided coated paper of ultra-high hardness was used, cracks occurred when the image recording material was bent.
[0185] In Example 1, near-infrared rays were irradiated in the infrared ray irradiation step, and it was found that the scratch resistance of the image was superior to that of Example 24.
[0186] In Example 1, the surface tension of the post-treatment liquid was 22.5 mN / m or more, and therefore it was found that the effect of suppressing the occurrence of cracks when the image-recorded material was folded was higher than in Example 14. In Example 1, the surface tension of the post-treatment liquid was 40.0 mN / m or less, and therefore it was found that the effect of suppressing the occurrence of cracks when the image-recorded material was folded was higher than in Example 5.
[0187] In Example 1, the amount of post-treatment liquid applied per unit area was 10 g / m 2 As a result, it was found that the effect of suppressing the occurrence of cracks when the image-recorded product was folded was higher than that of Example 15. In Example 1, the amount of post-treatment liquid applied per unit area was 55 g / m 2 As a result, it was found that the strength of the image recorded product was superior to that of Example 20.
[0188] In Example 1, since the surfactant contains a nonionic surfactant, it was found that the effect of suppressing the occurrence of cracks when the image-recorded material is folded was higher than in Examples 21 to 23.
[0189] In Examples 8 to 11, the HLB values of the surfactants were 8.0 or more, and therefore, it was found that the effect of suppressing the occurrence of cracks when the image-recorded material was folded was higher than in Example 7. In Examples 8 to 11, the HLB values of the surfactants were 14.0 or more, and therefore, it was found that the effect of suppressing the occurrence of cracks when the image-recorded material was folded was higher than in Example 12.
[0190] In Example 1, the pretreatment liquid application step was carried out, and therefore it was found that the scratch resistance of the image was superior to that of Example 29.
[0191] [Preparation of Pretreatment Solution 2] The following components were mixed and filtered using a 1 μm filter to obtain a pretreatment solution 2 with a pH of 7.1: calcium formate 4.90% by mass calcium lactate pentahydrate 3.80% by mass Olfine E1010 0.20% by mass BYK-024 0.01% by mass ion-exchanged water 91.09% by mass
[0192] [Preparation of Pretreatment Solution 3] The following components were mixed and filtered using a 1 μm filter to obtain Pretreatment Solution 3 with a pH of 7.4: Calcium formate: 10.10% by mass; Calcium lactate pentahydrate: 8.10% by mass; Olfine E1010: 0.20% by mass; BYK-024: 0.01% by mass; Ion-exchanged water: 81.59% by mass.
[0193] Examples 30 and 31 Image records were obtained in the same manner as in Example 1, except that pre-treatment liquid 1 was changed to pre-treatment liquid 2 and pre-treatment liquid 3, respectively. Evaluations were carried out in the same manner as in Example 1. The evaluation results are shown in Table 4.
[0194]
[0195] In Examples 30 and 31, similarly to Example 1, the occurrence of cracks when the image-recorded material was folded could be suppressed.
[0196] The disclosure of Japanese Patent Application No. 2022-048836, filed on March 24, 2022, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.
Claims
1. A step of applying an ink containing a colorant and water onto one side (side A) of a paper substrate by an inkjet recording method; a step of irradiating the A side to which the ink has been applied with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm; applying a post-treatment liquid containing water and a surfactant onto the other surface B of the paper base material, The paper base material includes a pulp layer and a coating layer disposed on at least one surface of the pulp layer, The coating layer includes at least one white pigment selected from the group consisting of calcium carbonate and kaolin, and a binder, The coating layer is disposed on the A-side side, and the dry coating amount of the coating layer disposed on the A-side side is 15 g / m 2 ~50g / m 2 and The coating layer is not disposed on the B-side, or if it is disposed, the dry coating amount of the coating layer disposed on the B-side is 10 g / m 2 The inkjet recording method is as follows:
2. 2. The ink jet recording method according to claim 1, wherein the infrared ray is near infrared ray having a maximum wavelength in the range of 800 nm to 1,400 nm.
3. 3. The inkjet recording method according to claim 1, wherein the post-treatment liquid has a surface tension of 22.5 mN / m to 40.0 mN / m.
4. In the step of applying the post-treatment liquid, the post-treatment liquid is applied in an amount of 10 g / m 2 ~55g / m 2 The inkjet recording method according to claim 1 or 2, wherein the ink is applied in a range of
5. The inkjet recording method according to claim 1 or 2, wherein the surfactant includes a nonionic surfactant.
6. 3. The ink jet recording method according to claim 1, wherein the surfactant has an HLB value of 8.0 to 14.
0.
7. The paper base material has a basis weight of 180 g / m 2 Up to 600 g / m 2 The inkjet recording method according to claim 1 or 2, wherein
8. a step of applying a pretreatment liquid onto the A side prior to the step of applying the ink, The inkjet recording method according to claim 1 or 2, wherein in the step of applying the ink, the ink is applied onto the surface A to which the pretreatment liquid has been applied.