AI Technical Summary

Technical Problem

Electrical contact materials with silver plating face issues of wear resistance due to adhesive wear, with existing solutions either restricting the thickness of the silver plating layer or relying on base material properties for evaluation, which can affect wear resistance.

Method used

An electrical contact material with a silver-containing layer having a controlled GOS value of 1.00° or less and a proportion of KAM values of 1.00° or more at 20% or more, along with specific crystal grain size and thickness ranges, and optionally an intermediate nickel layer, to enhance wear resistance independently of the base material characteristics.

Benefits of technology

The solution provides excellent wear resistance that is not influenced by the base material properties, maintaining high hardness and improving sliding properties while controlling strain and material costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This electric contact material comprises an electroconductive substrate and a silver-containing layer that contains silver and is disposed at least on a portion of the surface of the electroconductive layer. In a cross section of the electric contact material, the average GOS value of the silver-containing layer is 1.00° or less and the percentage of the silver-containing layer having a KAM value of 1.00° or more is 20% or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Electrical contact material, and contacts, terminals and connectors using the same

[0001] The present disclosure relates to an electrical contact material, and a contact, terminal, and connector using the same.

[0002] In recent years, automobiles have been increasingly adopting electrified drivetrains in order to achieve fuel economy. While this trend has dramatically increased the amount of current passing through the electrical wires between the battery, inverter, and motor, heat generated by electrical contacts and connectors has become a problem. For this reason, materials used for contacts and connectors are made of highly conductive pure copper, dilute copper alloys, or Corson alloys, with a nickel underplating applied to the surface, and then a silver or silver alloy plating applied over the underplating. However, because silver is a metal prone to adhesive wear, the silver plating is easily scraped off during sliding. This has the drawback of increasing the contact resistance of silver-plated materials due to wear of the silver plating.

[0003] To address these drawbacks, for example, Patent Document 1 describes a silver-plated terminal for connectors in which the surface of a copper or copper alloy base material is coated with a silver plating layer, the silver plating layer consisting of a first silver plating layer below the first silver plating layer and a second silver plating layer above the first silver plating layer, with the crystal grain size of the first silver plating layer being larger than the crystal grain size of the second silver plating layer. Patent Document 1 addresses the problem that the crystal grain size of the silver plating layer is likely to increase due to recrystallization, which reduces hardness and wear resistance, by specifying the crystal grain size of the silver plating layer to ensure good wear resistance. However, the size of the crystal grain size depends on the thickness of the plating layer. Therefore, Patent Document 1 requires a limit on the thickness of the silver plating layer to achieve good wear resistance.

[0004] Patent Document 2 also describes a method for producing a silver-plated product, in which a silver plating film with a purity of 99.9% by mass or higher is formed on a substrate by electroplating in a silver plating solution containing predetermined concentrations of silver, potassium cyanide, and selenium, where y is the product of the potassium cyanide concentration and the current density in the silver plating solution, and x is the solution temperature, such that y and x satisfy a predetermined relationship. Patent Document 2 exemplifies a method for producing a silver-plated product in which an increase in contact resistance is suppressed while maintaining high hardness by incorporating elements such as selenium into the silver plating film, and the Vickers hardness of the silver-plated product surface is used as the basis for wear resistance. Thus, Patent Document 2 uses the Vickers hardness of the silver-plated product, which depends on the characteristics of the substrate, to evaluate wear resistance. However, it is actually necessary to evaluate the wear resistance of the plating film itself, which is less affected by the characteristics of the substrate.

[0005] JP 2008-169408 A Japanese Patent No. 6611602 A

[0006] An object of the present disclosure is to provide an electrical contact material that has excellent abrasion resistance that is not easily affected by the characteristics of the base material, and a contact, a terminal, and a connector that use the same.

[0007] [1] An electrical contact material comprising a conductive substrate and a silver-containing layer containing silver provided on at least a portion of the surface of the conductive substrate, wherein, in a cross section of the electrical contact material, the silver-containing layer has an average GOS value of 1.00° or less and a proportion of KAM values ​​of 1.00° or more of 20% or more. [2] The electrical contact material according to [1] above, wherein the average crystal grain size in the silver-containing layer is 0.2 μm or more and 2.0 μm or less. [3] The electrical contact material according to [1] or [2] above, wherein the silver-containing layer is a pure silver layer. [4] The electrical contact material according to any one of [1] to [3] above, wherein the silver-containing layer has an average thickness of 0.5 μm or more and 5.0 μm or less. [5] The electrical contact material according to any one of [1] to [4] above, further comprising an intermediate layer made of nickel or a nickel alloy between the conductive substrate and the silver-containing layer. [6] The electrical contact material according to [5] above, wherein the average thickness of the intermediate layer is 0.01 μm or more and 3.00 μm or less. [7] A contact produced using the electrical contact material according to any one of [1] to [6] above. [8] A terminal produced using the electrical contact material according to any one of [1] to [6] above. [9] A connector produced using the electrical contact material according to any one of [1] to [6] above.

[0008] According to the present disclosure, it is possible to provide an electrical contact material that has excellent abrasion resistance and is not easily affected by the characteristics of the base material, as well as a contact, a terminal, and a connector that use the same.

[0009] Fig. 1 is a cross-sectional view showing an example of an electrical contact material according to an embodiment, and Fig. 2 is a cross-sectional view showing another example of an electrical contact material according to an embodiment.

[0010] Hereinafter, a detailed description will be given based on an embodiment.

[0011] As a result of extensive research, the present inventors have focused on the amount of strain in a silver-containing layer provided on at least a part of the surface of a conductive substrate and have found that by controlling the GOS value and KAM value of the silver-containing layer, the abrasion resistance of an electrical contact material is excellent, independent of the properties of the conductive substrate, and have completed the present disclosure based on this finding.

[0012] An electrical contact material according to an embodiment includes a conductive substrate and a silver-containing layer containing silver provided on at least a part of the surface of the conductive substrate, wherein, in a cross section of the electrical contact material, the silver-containing layer has an average GOS value of 1.00° or less and a proportion of KAM values ​​of 1.00° or more of the silver-containing layer.

[0013] 1 is a cross-sectional view showing an example of an electrical contact material according to an embodiment. As shown in FIG. 1, the electrical contact material 1 includes a conductive substrate 10 and a silver-containing layer 20.

[0014] The conductive substrate 10 constituting the electrical contact material 1 is a conductive rolled material obtained by rolling. From the viewpoints of the rolling workability of the conductive substrate 10 and the high electrical conductivity of the electrical contact material 1, the conductive substrate 10 is preferably made of a copper-based material including pure copper and copper alloys, or an iron-based material including pure iron and iron alloys. Among these, Cu-Zn-based, Cu-Ni-Si-based, Cu-Sn-Ni-based, Cu-Cr-Mg-based, and Cu-Ni-Si-Zn-Sn-Mg-based copper alloys are preferred.

[0015] The electrical conductivity of the conductive substrate 10 is preferably 60% IACS or more, more preferably 80% IACS or more. When the electrical conductivity of the conductive substrate 10 is 60% IACS or more, the electrical contact material 1 has good electrical conductivity.

[0016] The shape of the conductive substrate 10 may be appropriately selected depending on the application of the electrical contact material 1, but is preferably strip-like, plate-like, rod-like or wire-like.

[0017] The silver-containing layer 20 constituting the electrical contact material 1 is provided on at least a portion of the surface of the conductive substrate 10 and contains silver. The silver-containing layer 20 covering the surface of the conductive substrate 10 is made of pure silver or a silver alloy, and preferably made of pure silver, i.e., it is preferred that the silver-containing layer 20 is a pure silver layer. From the viewpoints of providing the electrical contact material 1 with excellent abrasion resistance and making the abrasion resistance of the electrical contact material 1 less susceptible to the properties of the conductive substrate 10, it is preferred that the silver-containing layer 20 be formed by plating, i.e., that the silver-containing layer 20 be a plated film.

[0018] 1 , the average GOS value of the silver-containing layer 20 is 1.00° or less, and the proportion of KAM values ​​of 1.00° or more is 20% or more. The cross section of the electrical contact material 1 is a cross section parallel to the rolling direction of the conductive substrate 10.

[0019] With respect to the silver-containing layer 20 in the cross section of the electrical contact material 1, when the average GOS value is 1.00° or less, the amount of strain remaining in the crystal grains in the silver-containing layer 20 is low, and when the proportion of KAM values ​​of 1.00° or more is 20% or more, the amount of strain remaining in the silver-containing layer 20 can be maintained high, and the hardness increases, thereby improving the wear resistance.

[0020] From this viewpoint, the average GOS value of the silver-containing layer 20 in the cross section of the electrical contact material 1 is 1.00° or less, preferably 0.75° or less, and more preferably 0.50° or less. Furthermore, in the cross section of the electrical contact material 1, the proportion of the KAM value of the silver-containing layer 20 that is 1.00° or more is 20% or more, and more preferably 25% or more.

[0021] Furthermore, it is preferable that the proportion of KAM values ​​of 1.00° or more is 50% or less in the silver-containing layer 20 in the cross section of the electrical contact material 1. When the proportion of KAM values ​​of 1.00° or more in the silver-containing layer 20 is 50% or less, deterioration of bending workability due to excessive strain in the silver-containing layer 20 can be suppressed.

[0022] The GOS (Grain Orientation Spread) value is the average value of the misorientation between a certain measurement point i and all measurement points (including measurement point i) within a crystal grain, and is a parameter that reflects the overall change in the crystal orientation of the crystal grain, and is a value obtained by integrating the local misorientation. In contrast to the KAM value, which is a value that reflects the local amount of strain within the silver-containing layer 20, the GOS value is a value that reflects the average amount of strain within the silver-containing layer 20. The GOS value can be expressed by the following formula (1):

[0023]

[0024] α ij : Crystal orientation difference n between measurement point i and measurement point j g : Number of measurement points within a grain

[0025] The GOS value is a parameter that reflects the overall change in the crystal orientation of the grains and corresponds to the integral of the local misorientation (KAM value). The GOS value also depends on the grain size, and is thought to increase as the grain size increases.

[0026] The KAM (Kernel Average Misorientation) value at a measurement point i is the average value of the misorientation between a certain measurement point i and a measurement point j adjacent to the measurement point i, and is a value that reflects the amount of strain in the silver-containing layer 20. The KAM value can be expressed by the following formula (2).

[0027]

[0028] α ij : Crystal orientation difference between measurement point i and measurement point j n: Number of measurement points j adjacent to measurement point i

[0029] The KAM value is calculated for all measurement points within the field of view, and the average value is used as the representative value for that field of view. The KAM value tends to be large in areas with large strain and near grain boundaries.

[0030] The GOS and KAM values ​​can be obtained from crystal orientation analysis data calculated using analysis software (OIM Analysis, manufactured by TSL Solutions) from crystal orientation data continuously measured using an EBSD detector (OIM5.0 HIKARI, manufactured by TSL Solutions) attached to a high-resolution scanning analytical electron microscope (JSM-7001FA, manufactured by JEOL Ltd.). The measurement object is the surface of the silver-containing layer 20 on a surface where a cross section of the electrical contact material 1 parallel to the rolling direction of the conductive substrate 10 has been mirror-finished with a cross-section polisher (manufactured by JEOL Ltd.), and the measurement magnification is 30,000 times. Measurements are performed at measurement intervals of 50 nm or less, and measurement points where the CI value analyzed by the analysis software is 0.1 or less are excluded (noise removal). Boundaries where the orientation difference between adjacent pixels is 5.00° or more are considered to be grain boundaries, and the GOS and KAM values ​​are obtained. This measurement is performed multiple times (in multiple different measurement areas of the same sample) and the average values ​​are calculated to obtain the average GOS value and average KAM value. Furthermore, the percentage of KAM values ​​of 1.00° or more can be obtained from the KAM value. Thus, the average GOS value and average KAM value are the average values ​​of the GOS values ​​and KAM values ​​in the measurement area of ​​the silver-containing layer measured at 30,000x magnification, and the percentage of KAM values ​​of 1.00° or more is the percentage of KAM values ​​of 1.00° or more relative to the KAM values ​​in the measurement area of ​​the silver-containing layer measured at 30,000x magnification.

[0031] The average crystal grain size in the silver-containing layer 20 is preferably 0.2 μm or more, more preferably 0.4 μm or more, and even more preferably 0.6 μm or more. When the average crystal grain size in the silver-containing layer 20 is 0.2 μm or more, the abrasion resistance can be further improved.

[0032] The average crystal grain size in the silver-containing layer 20 is preferably 2.0 μm or less, more preferably 1.5 μm or less, and even more preferably 1.0 μm or less. When the average crystal grain size in the silver-containing layer 20 is 2.0 μm or less, wear resistance can be stably maintained.

[0033] The silver-containing layer 20 may also contain one or more elements (hereinafter also referred to as "second elements") selected from the group consisting of Sn, Zn, In, Ni, Cu, Se, Sb, and Co. The presence of the second element in the silver-containing layer 20 can improve slidability. In particular, from the viewpoint of improving the electrical connectivity of the electrical contact material 1, the silver-containing layer 20 preferably contains less than 15.0 at% in total of one or more elements selected from the group consisting of Sn, Zn, In, Ni, Cu, Se, Sb, and Co. Furthermore, from the viewpoint of efficiently improving slidability and reducing material costs by adding the second element, the silver-containing layer 20 preferably contains 0.1 at% or more in total of one or more elements selected from the group consisting of Sn, Zn, In, Ni, Cu, Se, Sb, and Co.

[0034] The lower limit of the average thickness of the silver-containing layer 20 is preferably 0.5 μm or more, more preferably 2.0 μm or more, and even more preferably 3.0 μm or more. The upper limit of the average thickness of the silver-containing layer 20 is preferably 5.0 μm or less. When the lower limit of the average thickness of the silver-containing layer 20 is 0.5 μm or more, the excellent abrasion resistance of the electrical contact material 1 can be maintained for a long period of time. When the upper limit of the average thickness of the silver-containing layer 20 is 5.0 μm or less, material costs can be reduced.

[0035] Fig. 2 is a cross-sectional view showing another example of an electrical contact material according to an embodiment. The electrical contact material 2 shown in Fig. 2 has basically the same structure as the electrical contact material 1 shown in Fig. 1, except that an intermediate layer 30 is added.

[0036] 2 , the electrical contact material 2 further includes an intermediate layer 30 made of nickel or a nickel alloy between the conductive substrate 10 and the silver-containing layer 20. When the intermediate layer 30 is provided between the surface of the conductive substrate 10 and the silver-containing layer 20, thermal diffusion of the elements constituting the conductive substrate 10 into the silver-containing layer 20 can be suppressed and the adhesion between the conductive substrate 10 and the silver-containing layer 20 can be improved.

[0037] From the viewpoint of suppressing the thermal diffusion and further improving the adhesiveness, the intermediate layer 30 is preferably made of pure nickel or a Ni--P based nickel alloy.

[0038] The lower limit of the average thickness of the intermediate layer 30 is preferably 0.01 μm or more, more preferably 0.10 μm or more, and even more preferably 0.30 μm or more. The upper limit of the average thickness of the intermediate layer 30 is preferably 3.00 μm or less, more preferably 2.00 μm or less, and even more preferably 1.00 μm or less. If the lower limit of the average thickness of the intermediate layer 30 is less than 0.01 μm, the above-mentioned suppression of thermal diffusion and improvement of adhesion cannot be achieved. If the upper limit of the average thickness of the intermediate layer 30 exceeds 3.00 μm, bending workability deteriorates. When the electrical contact material is used in a terminal, bending workability of R / t≧1 is required.

[0039] Furthermore, the above-described electrical contact materials 1 and 2 may further include a copper layer (not shown) directly below the silver-containing layer 20, which is the surface layer. The copper layer (not shown) is made of pure copper or a copper alloy. The thickness of the copper layer (not shown) is significantly smaller than the thickness of the conductive substrate 10. When the electrical contact materials 1 and 2 further include a copper layer (not shown) directly below the silver-containing layer 20, the adhesion and bending workability can be improved.

[0040] As described above, the electrical contact materials 1 and 2 have excellent abrasion resistance that is not easily affected by the properties of the conductive substrate 10, and therefore the electrical contact materials 1 and 2 can be suitably used for contacts, terminals, and connectors. Such contacts are contacts made using the electrical contact materials 1 and 2, the terminals are terminals made using the electrical contact materials 1 and 2, and the connectors are connectors made using the electrical contact materials 1 and 2.

[0041] Next, a method for producing the electrical contact materials 1 and 2 will be described.

[0042] First, a silver-containing layer is formed on at least a portion of the surface of a conductive substrate by plating or the like. Then, the substrate having the silver-containing layer on its surface is rolled. In this manner, the electrical contact material 1 can be produced.

[0043] Furthermore, an intermediate layer is formed on at least a portion of the surface of the conductive substrate by plating or the like. Subsequently, a silver-containing layer is formed on the intermediate layer by plating or the like. Subsequently, the substrate provided with the intermediate layer and the silver-containing layer is rolled. In this manner, the electrical contact material 2 can be produced.

[0044] Regarding the plating conditions for the silver-containing layer, the current density was 5 A / dm 2 10A / dm or more 2 Hereinafter, by setting the bath temperature (liquid temperature) to 25°C or higher and prioritizing nucleation, many crystal grains with different crystal orientations grow, and the difference in crystal orientation becomes larger, which further increases the internal stress of the silver-containing layer. By controlling the current density and temperature within the above ranges, the KAM value in the silver-containing layer can be controlled, and the proportion of KAM values ​​of 1.00° or more in the silver-containing layer can be controlled to 20% or more. Even when the temperature is 25°C or higher, the current density can be controlled to 5 A / dm 2 If the current density is less than 10 A / dm, the crystal grains become coarse, the number of crystal grains with different crystal orientations decreases, and the average KAM value in the silver-containing layer becomes small, so that the proportion of KAM values ​​of 1.00° or more becomes less than 20%. 2 If it exceeds this value, the proportion of KAM values ​​of 1.00° or more will be less than 20% due to excessively fine crystals, and the surface hardness will be too high, resulting in poor bending workability.

[0045] In addition, the rolling processing ratio is 5% or more and 15% or less. When the processing ratio is 5% or more, the amount of strain in the silver-containing layer is increased, thereby improving wear resistance. When the processing ratio is 15% or less, the deterioration of bending workability due to excessive strain in the silver-containing layer can be suppressed. The rolling processing ratio is the percentage obtained by dividing the difference between the cross-sectional area of ​​the sample before rolling and the cross-sectional area of ​​the sample after rolling by the cross-sectional area of ​​the sample before rolling. By controlling the rolling processing ratio within the above range, the KAM value in the silver-containing layer can be controlled, and the proportion of KAM values ​​of 1.00° or more in the silver-containing layer can be controlled to 20% or more. When the rolling processing ratio is less than 5% or rolling is not performed, the amount of strain at the grain boundary is small, the number of measurement points with KAM values ​​of 1.00° or more is reduced, and the proportion of KAM values ​​of 1.00° or more in the silver-containing layer is reduced, so that the proportion of KAM values ​​of 1.00° or more becomes less than 20%.

[0046] Furthermore, after forming the silver-containing layer and before rolling, a heat treatment is performed at 300°C to 600°C for 5 to 60 seconds. This heat treatment can homogenize the strain introduced by plating. By performing heat treatment within the above range, strain within the crystal grains is released, thereby controlling the average GOS value of the silver-containing layer to 1.00° or less. Furthermore, by releasing strain within the crystal grains through heat treatment, strain within the silver-containing layer is largely present at the crystal grain boundaries, and measurement points showing KAM values ​​of 1.00° or more can be concentrated near the grain boundaries, thereby controlling the proportion of KAM values ​​of 1.00° or more to 20% or more. Regarding heat treatment, if the heat treatment temperature is less than 300°C or the heat treatment time is less than 5 seconds, the strain within the crystal grains cannot be sufficiently released, and measurement points showing KAM values ​​of 1.00° or more cannot be concentrated near the grain boundaries, making it impossible to achieve an average GOS value of 1.00° or less and a proportion of KAM values ​​of 1.00° or more of 20% or more. Regarding heat treatment, even if the heat treatment temperature exceeds 600°C and / or the heat treatment time exceeds 60 seconds, it is not possible to achieve an average GOS value of 1.00° or less and a proportion of KAM values ​​of 1.00° or more of 20% or more. Furthermore, excessive heat treatment reduces the material strength, making it impossible to maintain sufficient strength when used in contacts, terminals, and connectors.

[0047] Furthermore, when manufacturing the electrical contact materials 1 and 2 having the silver-containing layer 20 containing the second element, the silver-containing layer containing the second element may be directly formed by, for example, a plating method using a plating bath containing a silver component and a second element component, as described above. Alternatively, the silver-containing layer containing the second element may be formed by alternately depositing the silver-containing layer and the second element layer by, for example, a plating method, followed by a heat treatment. In this case, the rolling processing ratio is preferably 5% or more and 15% or less, from the same viewpoint as above. The heat treatment in this case may be substituted by a heat treatment performed after the silver-containing layer is formed and before the rolling processing.

[0048] According to the embodiment described above, by focusing on the amount of strain in the silver-containing layer provided on the surface of the conductive substrate and controlling the GOS value and KAM value of the silver-containing layer, it is possible to obtain an electrical contact material that has excellent abrasion resistance that is not easily affected by the characteristics of the substrate.

[0049] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects encompassed by the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure.

[0050] Next, examples and comparative examples will be described, but the present disclosure is not limited to these examples.

[0051] (Examples 1 to 5) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, a silver-containing layer was formed by plating (current density 10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50 g / L, potassium cyanide 100 g / L) at a bath temperature of 25°C. 2 ) on the surface of the substrate, followed by a heat treatment at 300°C to 600°C for 5 to 60 seconds. Subsequently, rolling was performed at the working ratio shown in Table 1 to produce electrical contact materials having a silver-containing layer (pure silver layer) shown in Table 1.

[0052] (Examples 6 to 14) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, a silver-containing layer was formed by plating (current density 10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50 g / L, potassium cyanide 100 g / L) at a bath temperature of 25°C. 2 ) on the surface of the substrate, and then a tin layer was plated (current density 10 A / dm) in a sulfuric acid bath (tin sulfate 80 g / L, sulfuric acid 80 g / L) at a bath temperature of 25°C. 2 ), followed by a heat treatment at 300°C to 600°C for 5 to 60 seconds. Subsequently, rolling was performed at the working ratio shown in Table 1 to produce electrical contact materials having a silver-containing layer (silver alloy layer) shown in Table 1.

[0053] (Examples 15 to 19) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, an intermediate layer was plated (current density 15 A / dm) in a nickel plating bath (nickel sulfate hexahydrate 500 g / L, nickel chloride 30 g / L, boric acid 30 g / L) at a bath temperature of 55°C. 2) on the surface of the substrate, and then a silver-containing layer was plated (current density 10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50 g / L, potassium cyanide 100 g / L) at a bath temperature of 25°C. 2 ) on the surface of the intermediate layer, followed by a heat treatment at 300°C to 600°C for 5 to 60 seconds. Next, rolling was performed at the working ratio shown in Table 1, thereby producing electrical contact materials having a silver-containing layer (pure silver layer) and an intermediate layer (pure nickel layer) shown in Table 1.

[0054] (Comparative Examples 1 to 3) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, an intermediate layer was plated (current density 15 A / dm) in a nickel plating bath (nickel sulfate hexahydrate 500 g / L, nickel chloride 30 g / L, boric acid 30 g / L) at a bath temperature of 55°C. 2 ) on the surface of the substrate, and then a silver-containing layer was plated (current density 10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50 g / L, potassium cyanide 100 g / L) at a bath temperature of 25°C. 2 ) on the surface of the intermediate layer, followed by a heat treatment at a temperature below 300°C or above 600°C for less than 5 seconds. Rolling was then performed at the working ratio shown in Table 1 to produce electrical contact materials having a silver-containing layer (pure silver layer) and an intermediate layer (pure nickel layer) as shown in Table 1. In Comparative Example 3, rolling was not performed.

[0055] (Examples 20 to 34) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, an intermediate layer was plated (current density 15 A / dm) in a nickel plating bath (nickel sulfate hexahydrate 500 g / L, nickel chloride 30 g / L, boric acid 30 g / L) at a bath temperature of 55°C. 2 ) on the surface of the substrate, and then a silver-containing layer is plated (current density 5-10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50-100 g / L, potassium cyanide 100-200 g / L) at a bath temperature of 25°C. 2 ) on the surface of the intermediate layer, and then a tin layer is plated (current density 10 to 20 A / dm) in a sulfuric acid bath (tin sulfate 80 g / L, sulfuric acid 80 g / L) at a bath temperature of 25°C. 2), followed by a heat treatment at 300°C to 600°C for 5 to 60 seconds. Subsequently, rolling was performed at the working ratio shown in Table 1, thereby producing electrical contact materials having a silver-containing layer (silver alloy layer) and an intermediate layer (pure nickel layer) shown in Table 1.

[0056] (Comparative Examples 4 to 9) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, an intermediate layer was plated (current density 15 A / dm) in a nickel plating bath (nickel sulfate hexahydrate 500 g / L, nickel chloride 30 g / L, boric acid 30 g / L) at a bath temperature of 55°C. 2 ) on the surface of the substrate, and then a silver-containing layer is plated (current density 5-10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50-100 g / L, potassium cyanide 100-200 g / L) at a bath temperature of 25°C. 2 ) on the surface of the intermediate layer, and then a tin layer is plated (current density 10 to 20 A / dm) in a sulfuric acid bath (tin sulfate 80 g / L, sulfuric acid 80 g / L) at a bath temperature of 25°C. 2 ), followed by a heat treatment at a temperature below 300°C or above 600°C for less than 5 seconds. Subsequently, rolling was performed at the working ratio shown in Table 1 to produce electrical contact materials having a silver-containing layer (silver alloy layer) and an intermediate layer (pure nickel layer) shown in Table 1. In Comparative Example 8, no intermediate layer was formed.

[0057] (Examples 35 to 37) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, an intermediate layer was plated (current density 10 A / dm) in a nickel-phosphorus electrolytic bath (nickel sulfate hexahydrate 500 g / L, nickel chloride hexahydrate 30 g / L, boric acid 30 g / L, phosphorous acid 16 g / L) at a bath temperature of 55°C. 2 ) on the surface of the substrate, and then a silver-containing layer containing a second element is plated (current density 5-10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50-100 g / L, potassium cyanide 100-200 g / L, indium trichloride 15 g / L) at a bath temperature of 25°C. 2) on the surface of the intermediate layer, followed by a heat treatment at 300°C to 600°C for 5 to 60 seconds. Subsequently, rolling was performed at the working ratio shown in Table 1 to produce electrical contact materials having a silver-containing layer (silver alloy layer) and an intermediate layer (nickel alloy layer) shown in Table 1.

[0058] (Examples 38 to 55) A substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was subjected to electrolytic degreasing and then acid cleaning. Thereafter, an intermediate layer was plated (current density 15 A / dm) in a nickel plating bath (nickel sulfate hexahydrate 500 g / L, nickel chloride 30 g / L, boric acid 30 g / L) at a bath temperature of 55°C. 2 ), and then a silver-containing layer containing a second element was plated (current density 5 to 10 A / dm) in an alkaline cyanide silver bath (silver cyanide 50 to 100 g / L, potassium cyanide 100 to 200 g / L, zinc chloride 10 g / L (Examples 38 to 40), nickel chloride 10 g / L (Examples 41 to 46), copper chloride dihydrate 12 g / L (Examples 44 to 46), potassium selenocyanate 2.2 mg / L (Examples 47 to 49), antimony trichloride 12 g / L (Examples 50 to 52), cobalt chloride 10 g / L (Examples 53 to 55)) at a bath temperature of 25°C. 2 ) on the surface of the intermediate layer, followed by a heat treatment at 300°C to 600°C for 5 to 60 seconds. Next, rolling was performed at the working ratio shown in Table 1, thereby producing electrical contact materials having the silver-containing layer (silver alloy layer) and intermediate layer (pure nickel layer) shown in Table 1.

[0059] [Measurements and Evaluations] The electrical contact materials obtained in the above Examples and Comparative Examples were subjected to the following measurements and evaluations. The results are shown in Table 2.

[0060] [1] Average GOS value and proportion of KAM values ​​of 1.00° or more The GOS value and KAM value were obtained from crystal orientation analysis data calculated using analysis software (OIM Analysis, manufactured by TSL Solutions) from crystal orientation data continuously measured using an EBSD detector (OIM5.0 HIKARI, manufactured by TSL Solutions) attached to a high-resolution scanning analytical electron microscope (JSM-7001FA, manufactured by JEOL Ltd.).

[0061] Using a cross-section polisher (manufactured by JEOL Ltd.), the silver-containing layer surface was obtained on a mirror-finished cross section of an electrical contact material parallel to the rolling direction of the conductive substrate. The measurement magnification was 30,000x. Measurements were performed at intervals of 50 nm or less. Measurement points with a CI value of 0.1 or less analyzed by analysis software were excluded, and boundaries where the orientation difference between adjacent pixels was 5.00° or more were considered to be grain boundaries, and the GOS value and KAM value were obtained. This measurement was performed five times (at five different measurement areas on the same sample), and the average values ​​were calculated to obtain the average GOS value and average KAM value of the silver-containing layer. In addition, the proportion of KAM values ​​of 1.00° or more in the silver-containing layer was calculated from the KAM value.

[0062] [2] Average crystal grain size A cross section of an electrical contact material parallel to the rolling direction of the conductive substrate was mirror-finished with a cross-section polisher (manufactured by JEOL Ltd.), and the surface of the silver-containing layer on the surface was observed at a magnification of 30,000 times in an SEM image, and the average crystal grain size in the silver-containing layer was obtained by a cutting method using a line segment perpendicular to the plating thickness direction.

[0063] [3] Dynamic Friction Coefficient An electrical contact material was subjected to bulging to obtain a bulged material with a bulged portion having a curvature radius of 5 mm. The surface of the silver-containing layer side of the bulged material was subjected to 15 reciprocating slides using a friction and wear tester, Tribogear (surface property measuring instrument type: 14FW, manufactured by Shinto Scientific Co., Ltd.), at a contact load of 5 N, a sliding distance of 5 mm, and a sliding speed of 100 mm / min. The value after the 15th slide was taken as the dynamic friction coefficient. The dynamic friction coefficient was ranked as follows:

[0064] ◎: Coefficient of dynamic friction is less than 0.4 ○: Coefficient of dynamic friction is 0.4 or more and less than 0.6 ×: Coefficient of dynamic friction is 0.6 or more

[0065] [4] Wear Resistance The surface of the silver-containing layer of the electrical contact material was subjected to 50 reciprocating strokes using a friction and wear tester, Tribogear (surface property measuring instrument type: 14FW, manufactured by Shinto Scientific Co., Ltd.), at a contact load of 4 N, a sliding distance of 50 mm, and a sliding speed of 100 mm / min. The ratio of the depth from the reference surface (the surface that was not reciprocally slid) to the thickness of the silver-containing layer was measured using a laser roughness meter. The wear resistance was ranked as follows:

[0066] ◎: The ratio of the depth from the reference plane to the thickness of the silver-containing layer is less than 1 / 10. ○: The ratio of the depth from the reference plane to the thickness of the silver-containing layer is 1 / 10 or more but less than 1 / 5. ×: The ratio of the depth from the reference plane to the thickness of the silver-containing layer is 1 / 5 or more.

[0067] [5] Contact Resistance Value The contact resistance value of the surface of the silver-containing layer of the electrical contact material was measured 10 times using an electrical contact simulator (manufactured by Yamazaki Seiki Kenkyusho Co., Ltd.) at a current of 20 mA and a load of 1 N, and the average of the measured values ​​was used as the contact resistance value of the electrical contact material. The contact resistance values ​​were ranked as follows:

[0068] ◎: Contact resistance is less than 0.3 mΩ ○: Contact resistance is 0.3 mΩ or more but less than 0.8 mΩ ×: Contact resistance is 0.8 mΩ or more

[0069] [6] Heat Resistance The electrical contact materials were heated in an air atmosphere at 150°C for 1,000 hours. After heating, the contact resistance of the silver-containing layer side of the electrical contact material was measured 10 times using an electrical contact simulator (manufactured by Yamazaki Seiki Kenkyusho Co., Ltd.) at a current of 20 mA and a load of 1 N. The average of the measured values ​​was used as the contact resistance of the electrical contact material. The heat resistance was ranked as follows:

[0070] ◎: Contact resistance after heating is less than 1.0 mΩ ○: Contact resistance after heating is 1.0 mΩ or more but less than 5.0 mΩ ×: Contact resistance after heating is 5.0 mΩ or more

[0071] [7] Bending workability In accordance with the test method of Japan Copper and Brazing Association Technical Standard JCBA-T307:2007, five test pieces (n=5) each measuring 10 mm in width and 30 mm in length were taken from the electrical contact material so that the longitudinal direction of the test piece was parallel to the rolling direction. A bending test was performed on each test piece at a bending angle of 90 degrees and R / t=1 to determine the presence or absence of cracks.

[0072] ○: No cracks in five test pieces ×: Cracks in one or more test pieces

[0073]

[0074]

[0075] As shown in Tables 1 and 2, in Examples 1 to 55, the average GOS value in the silver-containing layer was 1.00° or less and the proportion of KAM values ​​of 1.00° or more was 20% or more, so the abrasion resistance of the electrical contact materials was not affected by the properties of the conductive substrate and was good. On the other hand, in Comparative Examples 1 to 9, the average GOS value in the silver-containing layer was 1.00° or less and the proportion of KAM values ​​of 1.00° or more was outside the range of 20% or more, so the abrasion resistance of the electrical contact materials was poor.

[0076] 1, 2 Electrical contact material 10 Conductive substrate 20 Silver-containing layer 30 Intermediate layer

Claims

1. A conductive substrate; a silver-containing layer that contains silver and is provided on at least a portion of the surface of the conductive substrate; An electrical contact material comprising: An electrical contact material, wherein in a cross section of the electrical contact material, the silver-containing layer has an average GOS value of 1.00° or less and a proportion of KAM values ​​of 1.00° or more of 20% or more.

2. 2. The electrical contact material according to claim 1, wherein the average crystal grain size in said silver-containing layer is 0.2 μm or more and 2.0 μm or less.

3. The electrical contact material of claim 1 , wherein the silver-containing layer is a pure silver layer.

4. 2. The electrical contact material according to claim 1, wherein the average thickness of the silver-containing layer is 0.5 μm or more and 5.0 μm or less.

5. 2. The electrical contact material of claim 1, further comprising an intermediate layer of nickel or a nickel alloy between the conductive substrate and the silver-containing layer.

6. 6. The electrical contact material according to claim 5, wherein the intermediate layer has an average thickness of 0.01 μm or more and 3.00 μm or less.

7. A contact made by using the electrical contact material according to any one of claims 1 to 6.

8. A terminal produced by using the electrical contact material according to any one of claims 1 to 6.

9. A connector produced by using the electrical contact material according to any one of claims 1 to 6.