Method for producing olefin dimer, and olefin dimerization catalyst
Patent Information
- Application Number
- JP2024512651
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-03-29
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing olefin dimerization catalysts face challenges with catalyst powdering during liquid phase reactions, leading to reduced catalyst life and reaction selectivity, and current methods to prevent this complicate the manufacturing process and increase costs.
An olefin dimerization catalyst with a specific range of alkali metal content (3.0% to 12.5% by mass) and pore characteristics (pore diameter of 0.05 μm to 10 μm and pore volume of 0.01 to 0.12 mL/g) is used, which suppresses catalyst powdering and enhances reaction selectivity.
The method effectively stabilizes the catalyst during long-term liquid phase reactions, maintaining reaction selectivity and extending catalyst life without increasing manufacturing complexity or costs.
Abstract
Description
Olefin dimer production method, olefin dimerization catalyst
[0001] The present disclosure relates to a process for producing olefin dimers, and an olefin dimerization catalyst.
[0002] Olefin dimers (including co-dimers; the same applies hereinafter) typified by 4-methyl-1-pentene are used as monomers for producing polyolefins. Many basic catalysts have been proposed as catalysts for producing the corresponding dimers by the dimerization reaction of olefins (including co-dimerization reaction; the same applies hereinafter). In particular, catalysts obtained by supporting an alkali metal on a carrier mainly composed of an anhydrous potassium compound are widely used.
[0003] Research into these catalysts is ongoing to further improve their activity and selectivity to the target substance. Furthermore, because catalyst life is often insufficient even when initial activity is high, research into extending catalyst life is also ongoing. Furthermore, efforts have been made to improve activity, selectivity, and catalyst life by adjusting the physical properties of the anhydrous potassium compound used and the physical properties of the support. (See, for example, Patent Documents 1 to 6.) Patent Document 7, for example, discloses a porous molded body used as a support for an α-olefin dimerization catalyst. Such olefin dimerization catalysts can also be used to produce 3-methyl-1-pentene, for example, in the codimerization reaction of ethylene and butene. This 3-methyl-1-pentene yields a polymer with an extremely high melting point. When using olefins with a large carbon number, such as in the production of 3-methyl-1-pentene, the reaction system may become liquid. When olefin dimers are produced over a long period of time using the catalyst in a liquid reaction (hereinafter sometimes referred to as a "liquid-phase reaction"), catalyst particles may be prone to collapse (powdering). In order to solve these problems, the present inventors have proposed an embodiment in which a metal oxide is used in combination with the olefin dimerization catalyst (for example, Patent Document 8).
[0004] Japanese Patent Application Laid-Open No. 58-114737 Japanese Patent Application Laid-Open No. 3-42043 Japanese Patent Application Laid-Open No. 7-222927 Japanese Patent Application Laid-Open No. 2006-326418 Japanese Patent Application Laid-Open No. 2008-149275 U.S. Patent No. 5,081,094 International Publication No. WO 2015 / 093378 International Publication No. 2019 / 189636
[0005] The olefin dimerization catalyst described in Patent Document 8 has the performance to stably produce olefin dimers even in harsh environments prone to particle powdering, such as the liquid reaction system used to produce 3-methyl-1-pentene, but the use of additional components such as metal oxides complicates the catalyst production process, lengthens the time required for catalyst production, and can increase costs. If possible, a method for producing olefin dimers and an olefin dimerization catalyst using a catalyst that is less prone to powdering even in a liquid-phase reaction are desired.
[0006] An object of one embodiment of the present disclosure is to provide a method for producing an olefin dimer using a catalyst with a simpler configuration, which is capable of suppressing catalyst powdering during an olefin dimerization reaction, and also to provide an olefin dimerization catalyst suitable for the method for producing an olefin dimer, for example.
[0007] Through investigations by the present inventors, it has been found that the use of an olefin dimerization catalyst having an alkali metal content within a specific range suppresses catalyst powdering during the olefin dimerization reaction and also results in excellent reaction selectivity.
[0008] That is, the means for solving the above problems include the following aspects. <1> B nA method for producing an olefin dimer, comprising a step of dimerizing olefins, including olefins having 4 to 10 carbon atoms, in the presence of an olefin dimerization catalyst containing a compound (B) represented by the formula X (wherein B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X), and an alkali metal (D), wherein the content of the alkali metal (D) is 3.0 to 12.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D). <2> A method for producing an olefin dimer according to <1>, wherein the content of the alkali metal (D) is 4.0 to 12.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D). <3> A method for producing an olefin dimer according to <1>, wherein the content of the alkali metal (D) is 4.8 to 12.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D). <4> The method for producing an olefin dimer according to <1>, wherein the content of the alkali metal (D) is 5.2 to 10.5% by mass relative to 100% by mass of the total amount of the compound (B) and the alkali metal (D). <5> The method for producing an olefin dimer according to any one of <1> to <4>, wherein the volume of pores in the compound (B) having a pore diameter in the range of 0.05 μm to 10 μm is in the range of 0.01 to 0.09 ml / g. <6> B nAn olefin dimerization catalyst comprising: a compound (B) represented by X (wherein B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X); and an alkali metal (D), wherein the compound (B) has a pore volume of 0.05 μm to 10 μm in the range of 0.01 to 0.12 mL / g, and the content of the alkali metal (D) is 5.2 to 12.5 mass% relative to 100 mass% of the total amount of the alkali metal (D) and the compound (B). <7> The olefin dimerization catalyst according to <6>, wherein the content of the alkali metal (D) is 6.2 to 12.5 mass%. <8> The olefin dimerization catalyst according to <6>, wherein the content of the alkali metal (D) is 6.2 to 10.5 mass%. <9> The olefin dimerization catalyst according to any one of <6> to <8>, wherein the pore volume of the compound (B) having a pore diameter of 0.05 μm to 10 μm is in the range of 0.01 to 0.09 mL / g. <10> The olefin dimerization catalyst according to any one of <6> to <8>, wherein the pore volume of the compound (B) having a pore diameter of 0.05 μm to 10 μm is in the range of 0.01 to 0.08 mL / g. <11> B n 7. The olefin dimerization catalyst according to <6>, comprising a compound (B) represented by X (wherein B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X), and an alkali metal (D), wherein the compound (B) has a pore volume in the range of 0.05 μm to 10 μm in pore diameter in the range of 0.01 to 0.09 mL / g, and a molar ratio [AB'] / [T'](mr) of the molar amount [T'] of all the alkali metals to the molar amount [AB'] of B in the compound (B) is 0.60 to 0.89 / (mr).
[0009] According to one embodiment of the present disclosure, there are provided a method for producing an olefin dimer, which suppresses catalyst powdering during an olefin dimerization reaction even under severe conditions such as a liquid-phase reaction, and which has excellent reaction selectivity, and an olefin dimer.
[0010] FIG. 1 is a graph showing the alkali metal content of the olefin dimerization catalyst and various reaction results in each of the examples and comparative examples.
[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the upper and lower limits. In numerical ranges described in stages in this specification, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in numerical ranges described in this specification, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0012] <Production Method of Olefin Dimer> The production method of an olefin dimer according to the present disclosure comprises the steps of: n The method includes a step of dimerizing olefins, including olefins having 4 to 10 carbon atoms, in the presence of an olefin dimerization catalyst containing a compound (B) represented by the formula X (wherein B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X), and an alkali metal (D), wherein the content of the alkali metal (D) is 3.0 to 12.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D). Since the method for producing an olefin dimer uses the above-described olefin dimerization catalyst, catalyst powdering during the olefin dimerization reaction is suppressed and the reaction selectivity is excellent. For example, when an olefin having 4 or more carbon atoms, such as butene, is used, the reaction of the olefin tends to be a liquid-phase reaction. In a liquid phase reaction, catalyst particles are prone to powdering and disintegration (powdering), but in the method for producing an olefin dimer of the present disclosure, catalyst particles are less likely to powder and disintegrate (powder) even in a liquid phase reaction involving an olefin having 4 to 10 carbon atoms, so olefin dimers can be produced stably over a long period of time. Each component used in the method for producing an olefin dimer will be described in detail below. The steps included in the method for producing an olefin dimer will be described in detail below.
[0013] <Olefin dimerization catalyst> The olefin dimerization catalyst, which is one component of the present disclosure, is B n The catalyst comprises a compound (B) represented by X (wherein B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X), and an alkali metal (D), and the content of the alkali metal (D) is 3.0 to 12.5% by mass relative to 100% by mass of the total amount of the compound (B) and the alkali metal (D). Each requirement of the olefin dimerization catalyst will be explained below.
[0014] <<Compound (B)>> Compound (B) is B n Represented by X. B n In the formula represented by X, B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X. That is, in the formula B n The compound (B) represented by X is a carbonate, sulfate, silicate, fluoride, chloride or bromide of sodium or potassium. Compound (B) is preferably sodium carbonate or potassium carbonate.
[0015] The compound (B) is n The compound may be one kind or two or more kinds of compounds represented by X. When two or more kinds are used, the mixing ratio thereof is not particularly limited.
[0016] Compound (B) may contain sodium or potassium carbonate and sodium or potassium sulfate, silicate, fluoride, chloride or bromide (hereinafter also referred to as "compound (B1)"). When compound (B) contains compound (B1), the content of compound (B1) is preferably more than 0 mass% and not more than 30 mass%, more preferably more than 0 mass% and not more than 20 mass%, and even more preferably more than 0 mass% and not more than 10 mass%, based on the total mass of compound (B). Compound (B) may contain sodium or potassium carbonate, sodium or potassium sulfate, silicate, fluoride, chloride or bromide (hereinafter also referred to as "compound (B1)"). When compound (B) contains compound (B1), the content of compound (B1) is preferably more than 0 mass% and not more than 30 mass%, more preferably more than 0 mass% and not more than 20 mass%, and even more preferably more than 0 mass% and not more than 10 mass%, based on the total mass of compound (B). n Y or K nY (wherein Y is SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of Y). That is, the compound (B1) is a sulfate, silicate, fluoride, chloride, or bromide of sodium or potassium. Examples of the compound (B1) include Na n Y or K n The compound (B1) may be any one of compounds represented by the formula Y, or a mixture of two or more of them. When the compound (B1) is a mixture of two or more of them, the mixing ratio of the mixture is not particularly limited. When the compound (B) or a composition thereof contains the compound (B1), the content of the compound (B1) is preferably more than 0 mass% and not more than 30 mass%, more preferably more than 0 mass% and not more than 20 mass%, and even more preferably more than 0 mass% and not more than 10 mass%.
[0017] The compound (B) is preferably in a granular shape to be used as an olefin dimerization catalyst. When the compound (B) is granular, the particle size is preferably 5 μm to 600 μm, more preferably 20 μm to 500 μm, even more preferably 50 μm to 450 μm, and particularly preferably 50 μm to 300 μm, in terms of the median diameter (d50) of the volume statistics. Even when other optional components are contained, the same range is preferred. Powders having a median diameter in the range of 5 μm to 600 μm have good fluidity, making it possible to stably produce molded products.
[0018] In addition, in the compound (B), the content of particles having a particle diameter of 40 μm or less is preferably 3% by mass to 30% by mass relative to the total mass of the compound (B). It is generally known that small particles are desirably excluded due to poor particle movement during tableting, and it is preferable to set the content of particles having a particle diameter of 40 μm or less within the above range. If the content of particles having a particle diameter of 40 μm or less is within the above range, the fluidity of the raw material is ensured, blocking is less likely to occur when the raw material is molded, and uniform filling is facilitated.
[0019] Compound (B) may be a molded body. The molding method of compound (B) is not particularly limited, and methods such as extrusion molding, compression molding, and granulation molding are used. Among these, preferred molding methods for compound (B) include extrusion molding and compression molding, and tablet molding is also preferred. It is preferable to remove as much water as possible from the compound (B) or a composition containing compound (B). Among the above molding methods, in terms of the properties of the raw materials, it is preferable to mold the raw materials by compression molding, and more preferably by tablet molding. When molding the raw materials by compression molding, the raw materials are usually filled into a die that serves as a mold and compressed with a pestle to form a mold. Furthermore, when molding the raw materials by tablet molding, if the raw materials are used, the raw materials are uniformly filled into the die, so that a molded body with small density variation tends to be obtained.
[0020] When the raw material is shaped by extrusion, a liquid is added to the raw material to give it a viscosity sufficient to maintain its shape, and the shaped raw material is then passed through a mold for molding. When the olefin dimerization catalyst contains a hydrogen carbonate compound (A) described below, the hydrogen carbonate compound (A) dissolves in water. Therefore, when the raw material is shaped by extrusion, it is preferable to use an organic solvent in which the hydrogen carbonate compound (A) does not dissolve. When the raw material is shaped by tableting, the density of the tablet is preferably 1.6 g / mL to 2.3 g / mL, more preferably 1.8 g / mL to 2.2 g / mL. The density of the tablet can be adjusted by controlling the compression strength.
[0021] When the compound (B) is a molded body, there is no particular limitation on the size and shape of the molded body. The shape of the molded body can be selected depending on the conditions of the molding device, etc., and can be any of noodle-shaped, cylindrical, convex, ring-shaped, and spherical. When the raw material is molded by tableting, the shape of the molded body is preferably cylindrical, convex, or ring-shaped, and more preferably cylindrical from the viewpoint of ease of molding and strength.
[0022] Commercially available tablet presses can be used, and they may be rotary or press type. An optimal scale of equipment can be selected depending on the production volume. When raw materials are formed into cylindrical shapes using a tablet press, the resulting compacts are typically 2 mm to 5 mm in diameter and 2 mm to 6 mm in height. When the size of the compacts is within the above range, excessively small compacts can be prevented, thereby suppressing an increase in the number of tablet presses. This improves productivity and reduces costs. Furthermore, when the compacts are heat-treated and then used as a support for an olefin dimerization catalyst, for example, the diffusion of raw materials and products within the reaction system is likely to be improved, and the reaction activity and reaction selectivity of the olefin dimerization reaction are likely to be improved.
[0023] <<Pore Volume>> The compound (B) preferably has a pore volume in the range of 0.05 μm to 10 μm in diameter in the range of 0.01 mL / g to 0.12 mL / g. The lower limit of the pore volume is preferably 0.02 mL / g, more preferably 0.025 mL / g. On the other hand, the upper limit of the pore volume is preferably 0.10 mL / g, more preferably 0.09 mL / g, even more preferably 0.085 mL / g, and particularly preferably 0.080 mL / g. If the pore volume is within this range, the olefin dimerization reaction described below tends to proceed stably for a long period of time. The pore diameter of the compound (B) is preferably such that the median pore diameter of pores in the range of 0.001 μm to 10 μm is greater than 0.05 μm and not more than 0.35 μm. When the above requirements are satisfied, for example, when the catalyst of the present invention is used by packing it into a fixed bed, this is often preferable from the viewpoints of suppressing powdering of catalyst particles (one requirement for extending the catalyst's life) and handling during packing and discharging. The pore diameter can be adjusted, for example, by the proportion of hydrogen carbonate compound (A) used, which will be described later, or by the calcination conditions. The above catalyst shape requirements also apply to olefin dimerization catalysts containing olefins having 4 to 10 carbon atoms, which will be described later. The production method of an olefin dimerization catalyst often depends strongly on the shape of compound (B), although it depends on the production method and conditions.
[0024] <Alkali Metal (D)> The alkali metal (D) is preferably a metal selected from the group consisting of sodium and potassium, and more preferably sodium. Here, the alkali metal (D) is a non-ionized zero-valent metal. When the purity of the alkali metal (D) is 90% or more, the alkali metal may contain components other than the alkali metal. Examples of components other than the alkali metal include various oxides or hydroxides of elements other than Group 1 elements of the periodic table, such as lithium and potassium, and metal elements other than Group 1 elements of the periodic table. The content of the alkali metal (D) in the olefin dimerization catalyst of the present disclosure (sometimes referred to as h) is 3.0% by mass to 12.5% by mass, relative to 100% by mass of the total amount of the alkali metal (D) and compound (B).
[0025] The lower limit of the alkali metal (D) content is preferably 4.0 mass%, more preferably 4.8 mass%, even more preferably 5.2 mass%, even more preferably 5.5 mass%, even more preferably 5.9 mass%, particularly preferably 6.2 mass%, especially preferably 6.3 mass%, and most preferably 6.4 mass%. On the other hand, the upper limit of the alkali metal (D) content is preferably 11.0 mass%, more preferably 10.5 mass%, even more preferably 9.5 mass%, particularly preferably 9.0 mass%, and most preferably 8.5 mass%.
[0026] The olefin dimerization catalyst of the present disclosure may function as a suitable dimerization catalyst from the viewpoint of reaction durability, etc., not only when an olefin having 4 to 10 carbon atoms is contained, but also in other embodiments. In such cases, the content of the alkali metal (D) is 5.2 to 12.5 mass%, relative to 100 mass% of the total amount of the alkali metal (D) and compound (B). The preferred lower limit of the alkali metal (D) content is preferably 5.5 mass%, more preferably 5.9 mass%, even more preferably 6.2 mass%, particularly preferably 6.3 mass%, and most preferably 6.4 mass%. On the other hand, the preferred upper limit of the alkali metal (D) content is preferably 11.0 mass%, more preferably 10.5 mass%, even more preferably 9.5 mass%, particularly preferably 9.0 mass%, and most preferably 9.0 mass%.
[0027] The olefin dimerization catalyst of the present disclosure may contain components other than the compound (B) and the alkali metal (D), such as an alkali metal hydrogen carbonate compound (A) and graphite (C), as long as the components are within the scope of the object of the present disclosure.
[0028] - Hydrogencarbonate Compound (A) - Suitable examples of the hydrogencarbonate compound (A) of an alkali metal (hereinafter also simply referred to as "hydrogencarbonate compound (A)") include compounds represented by the formula AHCO3 (wherein A represents an alkali metal). In the formula, A is preferably Na or K. Examples of such hydrogencarbonate compound (A) include at least one compound of sodium hydrogencarbonate (NaHCO3) and potassium hydrogencarbonate (KHCO3). When the hydrogencarbonate compound (A) contains both sodium hydrogencarbonate (NaHCO3) and potassium hydrogencarbonate (KHCO3), the mixing ratio thereof is not particularly limited.
[0029] When the olefin dimerization catalyst contains the hydrogen carbonate compound (A), the proportion of the hydrogen carbonate compound (A) is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, and particularly preferably 5 parts by mass or less, per 100 parts by mass of the total of the hydrogen carbonate compound (A) and the compound (B).
[0030] From the viewpoint of adjusting the pore size of the olefin dimerization catalyst of the present disclosure to a larger value, the hydrogen carbonate compound (A) is more preferably potassium hydrogen carbonate (KHCO3), where A in the above formula is K.
[0031] -Graphite (C)- The olefin dimerization catalyst may further contain graphite (C). When the olefin dimerization catalyst further contains graphite (C), molding of a raw material containing graphite (C) is carried out, for example, by compression molding (tabletting molding, etc.) described below, which facilitates smooth movement of the mortar and pestle and makes the density of the molded body more stable. There are no particular restrictions on the properties of the graphite (C), and any graphite commonly used as a lubricant during molding may be used. Graphite (C) commonly used has a median diameter (d50) in the volume statistics range of 5 μm to 500 μm and a specific surface area measured by the BET method of 0.1 m 2 / g to 300m 2 The graphite (C) may be natural graphite or artificial graphite.
[0032] The content of graphite (C) in the olefin dimerization catalyst can be set arbitrarily as long as it allows molding, such as compression molding and granulation molding. The content of graphite (C) is preferably 0.3 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total of the optional hydrogen carbonate compound (A) and the essential compound (B). When the amount of graphite (C) added is 10 parts by mass or less, the strength of the olefin dimerization catalyst of the present disclosure tends to be less likely to decrease. When the amount of graphite (C) added is 0.3 parts by mass or more, as described above, for example, when the raw materials are molded by tableting, excessive friction between the mortar and pestle can be suppressed. This facilitates smooth operation of the device and stabilizes the density of the molded body. Therefore, when the amount of graphite (C) added is within the above range, the molded body is easily molded well. This makes it easier to ensure the strength of the porous molded body obtained by heat-treating the molded body.
[0033] The olefin dimerization catalyst may further contain components other than the hydrogen carbonate compound (A), graphite (C), and alkali metal (D). An example of such other compound is ammonium hydrogen carbonate. When the raw material contains ammonium hydrogen carbonate, the pore volume of the porous molded body can be further increased.
[0034] The alkali metal atoms in the olefin dimerization catalyst of the present disclosure may include atoms derived from the alkali metal (D) and atoms derived from an alkali metal salt of the aforementioned component (B) or the optional component (A) (corresponding to B and A in the above formula).
[0035] More preferred embodiments of the olefin dimerization catalyst of the present disclosure include: n An example of an olefin dimerization catalyst is one which contains a compound (B) represented by X (wherein B is Na or K, X is CO3, SO4, SiO3, F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X) and an alkali metal (D), wherein the pore volume of compound (B) having pore diameters in the range of 0.05 μm to 10 μm is in the range of 0.01 to 0.09 mL / g, and the molar ratio [AB'] / [T'] (mr) of the molar amount [T'] of all alkali metals to the molar amount [AB'] of B in compound (B) is 0.60 to 0.89 / (mr). The above (mr) means a molar ratio.
[0036] However, [AB'] is an index that includes not only the amount of B in the compound (B) but also the amounts of Na and K contained in salts such as A in the optional compound (A). A more preferred lower limit is 0.63, even more preferably 0.65, and particularly preferably 0.67. On the other hand, a preferred upper limit is 0.88, even more preferably 0.87, and particularly preferably 0.86. Within the above numerical range, an excellent balance is achieved between the resistance to particle collapse and olefin dimerization reaction performance. The reason for this estimation will be described later.
[0037] The above parameters can be calculated from the elemental analysis value of the alkali metal in the olefin dimerization catalyst of the present disclosure and the elemental analysis value of the alkali metal in a state in which the alkali metal (D) has been removed from the olefin dimerization catalyst. Of course, they can also be calculated from the ratio of the amounts of each component charged during the preparation of the olefin dimerization catalyst. As described above, the olefin dimerization catalyst of the present disclosure contains an alkali metal (D). However, this alkali metal (D) is believed to exist in the form of the alkali metal itself, rather than in the form of a compound such as a salt. As is well known, alkali metals tend to melt and vaporize relatively easily and have lower melting points and boiling points than salt compounds. For this reason, the alkali metal (D) can be removed from the olefin dimerization catalyst by heating the olefin dimerization catalyst to a temperature above the melting point of the alkali metal (D) and below the melting point of a salt compound such as compound (B). Separation methods utilizing the difference in boiling points between the components can also be used. As the elemental analysis method, known methods such as ICP analysis (inductively coupled plasma atomic emission spectroscopy) can be used without limitation.
[0038] <<Method for Producing an Olefin Dimerization Catalyst>> The olefin dimerization catalyst can be obtained, for example, by contacting the compound (B) with an alkali metal (D). This can be considered as a method for supporting the alkali metal (D) on a carrier called compound (B).
[0039] As a method for contacting the compound (B) with the alkali metal (D) to obtain an olefin dimerization catalyst, any known method can be used without limitation. Specific conditions will be explained below, taking the contact support method as an example. The temperature during the support treatment is usually in the range of 150°C to 400°C. From the viewpoint of obtaining a catalyst excellent in catalytic activity, catalyst life, and selectivity to olefin dimerization products, the temperature during the support treatment is preferably in the range of 200°C to 350°C, more preferably in the range of 200°C to 300°C. The atmosphere during the support treatment may be a reducing atmosphere or an inert atmosphere, as long as it is not a moisture-containing or oxidizing atmosphere. In consideration of safety and economy, the support treatment is preferably performed in a nitrogen atmosphere.
[0040] During the loading treatment, the support made of a porous molded body is preferably vibrated, rotated, or stirred in order to uniformly load the alkali metal (D). It is known that the loaded alkali metal (D) undergoes an exchange reaction with the alkali metal in the support when it comes into contact with the support under heating.
[0041] In some cases, the method for producing an olefin dimerization catalyst preferably includes a step of heat-treating the compound (B) at a temperature in the range of 100°C to 500°C. The heat treatment time (i.e., heat treatment time) is preferably 0.3 hours or more. For example, when the hydrogen carbonate compound (A) is used in combination, the above treatment is preferably carried out. The atmosphere at this time is not limited, and may be air or an inert gas. Furthermore, for the purpose of adjusting the porosity or pore volume, the atmosphere may contain other gases such as water vapor. When water vapor is used in combination, the concentration is preferably 1.0 g / m. 3 ~750,000g / m 3 and more preferably 10.0 g / m 3 ~750,000g / m 3 is.
[0042] The content of the alkali metal (D) in the olefin dimerization catalyst (hereinafter sometimes referred to as the "support rate") is 3.0% by mass to 12.5% by mass, relative to 100% by mass of the total amount of the alkali metal (D) and compound (B). The preferred lower limit of the alkali metal (D) content is 4.0% by mass, more preferably 4.8% by mass, even more preferably 5.2% by mass, particularly preferably 6.2% by mass, and most preferably 6.4% by mass. On the other hand, the preferred upper limit of the alkali metal (D) content is 11.0% by mass, more preferably 10.5% by mass. It is still more preferably 9.5% by mass, particularly preferably 9.0% by mass, and most preferably 8.5% by mass.
[0043] It is readily expected that increasing the alkali metal (D) content tends to increase catalytic activity, but when the content reaches a certain range, this improvement effect may decrease. The olefin dimerization catalyst used in the olefin dimer production method according to the present disclosure exhibits a relatively high level of reactivity and selectivity balance when the alkali metal (D) content is in the range of 3.0% by mass to 12.5% by mass, and this performance balance tends to be less affected by the alkali metal (D) content. Furthermore, surprisingly, when the alkali metal content is increased, the catalyst has the unexpected excellent characteristic of being less prone to powdering, even when used under liquid-phase reaction conditions that are unfavorable for maintaining the catalyst shape. The inventors believe that this is because part or all of the alkali metal (D) functions as a binder in addition to its function as a catalytic active site, thereby suppressing powdering of catalyst particles. To achieve such a high alkali metal (D) content, it is desirable for the olefin dimerization catalyst of the present disclosure to have as high a pore volume value as possible. On the other hand, if the pore volume value becomes too high, the catalyst tends to be more fragile. The pore volume range of the olefin dimerization catalyst of the present disclosure has been selected taking into consideration the above-mentioned points. As such, the present disclosure has a simple configuration as an olefin dimerization catalyst, exhibits the unexpected effect of suppressing powdering, and can produce olefin dimers using a catalyst with excellent selectivity and reactivity. Therefore, olefin dimers can be produced stably and efficiently over a long period of time.
[0044] The olefin dimerization catalyst of the present disclosure preferably has a pore volume in the range of 0.05 μm to 10 μm in diameter in the range of 0.01 mL / g to 0.12 mL / g. The preferred lower limit of the pore volume of the olefin dimerization catalyst is 0.02 mL / g, more preferably 0.025 mL / g. On the other hand, the preferred upper limit of the pore volume of the olefin dimerization catalyst is 0.10 mL / g, more preferably 0.09 mL / g, even more preferably 0.085 mL / g, particularly preferably 0.08 mL / g, and especially preferably 0.07 mL / g. When the pore volume of the olefin dimerization catalyst is within this range, the olefin dimerization reaction involving an olefin having 4 to 10 carbon atoms, as described below, tends to proceed stably for a long period of time.
[0045] <Dimerization Reaction Step> The method for producing an olefin dimer according to the present disclosure includes a step (dimerization reaction step) of dimerizing olefins including olefins having 4 to 10 carbon atoms in the presence of an olefin dimerization catalyst. The olefin dimerization catalyst used in the dimerization reaction step is as described above. In the dimerization reaction step, the reaction temperature in the olefin dimerization reaction is usually 0°C to 300°C, preferably 50°C to 200°C. The reaction pressure is usually atmospheric pressure or 19.6 MPa (200 kg / cm 2 -G), and preferably 1.96 MPa to 14.7 MPa (20 kg / cm 2 -G~150kg / cm 2 -G).
[0046] The state of the olefin in the olefin dimerization reaction step is preferably a liquid phase. The liquid phase may be in a critical state as long as it is liquid. The olefin dimerization reaction can be carried out in a fixed bed system or a fluidized bed system. Among these, the fixed bed system is preferred. When the dimerization reaction is carried out in a fixed bed system, the liquid hourly space velocity (LHSV) of the olefin is usually 0.1 hr -1 ~10 hours -1 and preferably 0.5 hr -1 ~5 hours -1After the dimerization reaction is completed, the unreacted olefin and the product are separated from the mixture in accordance with a conventional method, and the unreacted olefin can be recycled and reused in the reaction.
[0047] <<Olefins Containing Olefins Having 4 to 10 Carbon Atoms>> The olefins containing 4 to 10 carbon atoms may contain only olefins having 4 to 10 carbon atoms, or may contain olefins having 4 to 10 carbon atoms and olefins other than those having 4 to 10 carbon atoms. Specific examples of olefins having 4 to 10 carbon atoms include 1-butene, cis-2-butene, trans-2-butene, isobutylene, 1-pentene, 1-hexene, 1-octene, and 1-decene. Preferred olefins other than those having 4 to 10 carbon atoms are ethylene having 2 carbon atoms and propylene having 3 carbon atoms. A method of producing an olefin co-dimer by co-dimerizing such an olefin with the above-mentioned olefin having 4 to 10 carbon atoms is an example of a suitable embodiment of the present disclosure. A particularly preferred embodiment of the method for producing an olefin dimer according to the present disclosure is the co-dimerization reaction of 1-butene or a 2-butene with ethylene or propylene, and in particular, a method for producing 3-methyl-1-pentene by the co-dimerization reaction of 1-butene or a 2-butene with ethylene. The ethylene and olefins having 3 to 10 carbon atoms used in the present disclosure may be not only olefins derived from fossil resources such as petroleum, but also so-called bio-derived olefins such as plant-derived olefins.
[0048] The method for producing an olefin dimer may include other steps in addition to the above steps, as long as the effects of the present disclosure are achieved. Examples of such other steps include a step of preparing an olefin dimerization catalyst.
[0049] The present disclosure will be specifically described below using examples, but the present disclosure is not limited to these examples.
[0050] [Measurement of pore volume and median pore diameter] For the KCO powders used in Examples 1 to 7 and Comparative Example 1, the pore volumes of pores having diameters (i.e., pore diameters) in the range of 0.05 μm to 10 μm were measured by mercury intrusion using a mercury porosimeter (manufactured by Micrometrics, model number: Auto Pore IV). The results are shown in Table 1.
[0051] [Method of calculating the powdering rate] After the completion of the 120-hour reaction in each of the Examples and Comparative Examples, the total mass of the catalyst removed from the reactor was measured. The catalyst was then separated using a sieve with a mesh size of 500 μm, and the catalyst powdering rate (mass%) was calculated using the following formula. The smaller the powdering rate, the more the catalyst was suppressed from powdering during the olefin dimerization reaction. Powdering rate (mass%) = Mass of powder that passed through the sieve / Total mass of the catalyst × 100
[0052] Ethylene conversion and 3-methyl-1-pentene selectivity were determined by a conventional method using a GC 2014 gas chromatograph manufactured by Shimadzu Corporation. The column used was a DB-5 column manufactured by Agilent Technologies (inner diameter 0.25 mm, length 60 m, membrane pressure 1.0 μm, catalog number 122-5063).
[0053] [Measurement of Crushing Strength of Porous Molded Body] Using a digital hardness tester (manufactured by Fujiwara Seisakusho, model number: KHT-40N), the crushing strength of the porous molded body in the radial direction (i.e., toward the barrel of a cylindrical molded body) was measured according to the method described in JIS Z8841 (1993) "Granulated materials - Strength test method." The crushing strength is measured by placing the cylindrical porous molded body to be measured on a stationary sample stage, and then measuring the strength when a movable pressure surface is lowered from above at a constant speed and pressed against the cylindrical porous molded body to break it.
[0054] Example 1 (Reference Example for Claim 6) (1) Preparation of Catalyst 100 parts by mass of K2CO3 powder (manufactured by AGC Corporation, purity 99%) and 1.2 parts by mass of graphite (manufactured by Nippon Graphite Industries Co., Ltd., purity 98%) were uniformly mixed, compressed into tablets, and formed into cylindrical shapes with a diameter of 3.2 mm and a height of 3.2 mm to prepare a molded body. The pore volume of the molded body was 0.18 mL / g. 96.5 parts by mass of the molded body was dried in a nitrogen stream at 300°C for 2 hours, and then 3.5 parts by mass of sodium was added under a nitrogen stream. The mixture was stirred at 240°C for 4.0 hours to prepare an olefin dimerization catalyst. Since no adhesion of the added sodium to the carrier container was observed, it was determined that the entire amount of sodium was supported on the molded body. The support rate at this time was 5.0% by mass. The strength in the barrel direction after catalyst preparation was 2.4 kgf. (2) Dimerization Reaction 2.5 g of the catalyst prepared in (1) above was packed into a single-tube reactor with a diameter of 18 mm, and a 10 wt % ethylene (diluted with 1-butene) mixed solution was continuously fed to the catalyst layer at a flow rate of 7.2 g / h under conditions of 85°C reactor internal temperature and 9.3 MPa reaction pressure. The 3MP1 (3-methyl-1-pentene) synthesis reaction was carried out by the co-dimerization reaction of ethylene and 1-butene. Under the above temperature and pressure conditions, the reaction system was in a liquid phase. After 120 hours of flow reaction, the ethylene conversion, 3MP1 selectivity, and attrition rate were determined by the above method to be 67.7%, 65.9%, and 18.9%, respectively.
[0055] [Example 2] (This is a reference example for claim 6.) (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that the amount of the molded body was 95.0 parts by mass and the amount of sodium was 5.0 parts by mass. The results of the ethylene conversion rate, 3MP1 selectivity, and powdering rate are shown in Table 1. The strength of the catalyst was 1.4 kgf.
[0056] Example 3 (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that the amount of the molded body was 93.5 parts by mass and the amount of sodium was 6.5 parts by mass. The strength of the catalyst was 2.0 kgf. The results are shown in Table 1.
[0057] Example 4 (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that the amount of the molded body was 92.5 parts by mass and the amount of sodium was 7.5 parts by mass. The strength of the catalyst was 1.4 kgf. The results are shown in Table 1.
[0058] Example 5 (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that the amount of the molded body was 91.5 parts by mass and the amount of sodium was 8.5 parts by mass. The strength of the catalyst was 1.0 kgf. The results are shown in Table 1.
[0059] Example 6 (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that the amount of the molded body was 90.0 parts by mass and the amount of sodium was 10.0 parts by mass. The strength of the catalyst was 1.2 kgf. The results are shown in Table 1.
[0060] Example 7 (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that the amount of the molded body was 88.0 parts by mass and the amount of sodium was 12.0 parts by mass. The strength of the catalyst was 1.0 kgf. The results are shown in Table 1.
[0061] Comparative Example 1 (1) A catalyst was prepared and a dimerization reaction was carried out in the same manner as in Example 1, except that 98.0 parts by mass of the molded body and 2.0 parts by mass of sodium were used in the preparation of the catalyst. The strength of the catalyst was 2.4 kgf. The results are shown in Table 1.
[0062]
[0063] It can be seen that the olefin dimer production methods of Examples 1 to 7 according to the present disclosure suppress catalyst powdering during the olefin dimerization reaction and have excellent reaction selectivity, compared to the olefin dimer production method of Comparative Example 1. It can also be seen that the catalysts of Examples 3 to 7 according to the present disclosure are less susceptible to powdering and have excellent selectivity for the 3MP-1 synthesis reaction. It can also be seen that the catalysts used in the olefin dimer production method according to the present disclosure have sufficient strength. On the other hand, it can also be seen that particle strength and powdering rate are not necessarily related indicators.
Claims
1. B n X (wherein B is Na or K, and X is CO 3 , S.O. 4 , SiO 3 , F, Cl, or Br, and n is an integer of 1 or 2 determined depending on the valence of X, and an alkali metal (D), wherein the pore volume of compound (B) having a pore diameter of 0.05 μm to 10 μm is in the range of 0.01 to 0.09 mL / g, and the content of alkali metal (D) is 3.0 to 12.5 mass% relative to 100 mass% of the total amount of compound (B) and alkali metal (D).
2. The method for producing an olefin dimer according to claim 1, wherein the content of the alkali metal (D) is 4.0 to 12.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D).
3. The method for producing an olefin dimer according to claim 1, wherein the content of the alkali metal (D) is 4.8 to 12.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D).
4. The method for producing an olefin dimer according to claim 1, wherein the content of the alkali metal (D) is 5.2 to 10.5 mass% relative to 100 mass% of the total amount of the compound (B) and the alkali metal (D).
5. (delete)
6. B n X (wherein B is Na or K and X is CO 3 , S.O. 4 , SiO 3 , F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X; and an alkali metal (D), The pore volume of the compound (B) having a pore diameter in the range of 0.05 μm to 10 μm is in the range of 0.01 to 0.12 mL / g; The olefin dimerization catalyst has a content of the alkali metal (D) of 5.2 to 12.5 mass % relative to 100 mass % of the total amount of the alkali metal (D) and the compound (B).
7. The olefin dimerization catalyst according to claim 6, wherein the content of the alkali metal (D) is 6.2 to 12.5 mass%.
8. The olefin dimerization catalyst according to claim 6, wherein the content of the alkali metal (D) is 6.2 to 10.5 mass%.
9. The olefin dimerization catalyst according to claim 6, wherein the volume of pores having a pore diameter in the range of 0.05 μm to 10 μm of the compound (B) is in the range of 0.01 to 0.09 mL / g.
10. The olefin dimerization catalyst according to claim 6, wherein the compound (B) has a pore volume in the range of 0.05 μm to 10 μm in pore diameter in the range of 0.01 to 0.08 mL / g.
11. B n X (wherein B is Na or K and X is CO 3 , S.O. 4 , SiO 3 , F, Cl, or Br, and n is an integer of 1 or 2 determined by the valence of X; and The pore volume of the compound (B) having a pore diameter in the range of 0.05 μm to 10 μm is in the range of 0.01 to 0.09 mL / g; The olefin dimerization catalyst according to claim 6, wherein the molar ratio [AB'] / [T'] (m.r.) of the molar amount [T'] of all alkali metals to the molar amount [AB'] of B in the compound (B) is 0.60 to 0.89 / (m.r.).