Surface-treated steel sheet

JPWO2023190971A5Active Publication Date: 2024-11-08NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024512843
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-03-30
Publication Date
2024-11-08
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Conventional surface-treated steel sheets used in automobiles and other vehicles face issues with blistering and coating delamination during warm salt water immersion tests, leading to reduced corrosion resistance and inadequate adhesion of the electrodeposition coating.

Method used

A surface-treated steel sheet with a Zn-containing plating layer and a surface treatment layer containing a coating film with specific compositions and thicknesses, including a binder resin, oil absorbing agent, and conductive agent, where the oil absorbing agent has a particle size greater than half the average film thickness and a certain oil absorption capacity, enhancing adhesion and corrosion resistance.

Benefits of technology

The solution effectively suppresses blistering and coating peeling during electrodeposition coating, maintaining excellent corrosion resistance and weldability, with improved adhesion and surface roughness enhancing the chemical and physical bonding between coating layers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application discloses a surface-treated steel sheet. [Background technology]

[0002] Surface-treated steel sheets are used as components in automobiles and other vehicles. A surface-treated steel sheet comprises, for example, a plated steel sheet having a Zn-containing plating layer and a surface treatment layer provided on at least one main surface of the plated steel sheet. In conventional technology, a coating is used as the surface treatment layer, and the weldability and corrosion resistance of the surface-treated steel sheet are improved by adjusting the type and content of the components that make up the coating.

[0003] For example, Patent Document 1 discloses a technique for improving the weldability and corrosion resistance of a surface-treated steel sheet having a coating on at least one side of a plated steel sheet, by including predetermined amounts of a binder resin, non-oxide ceramic particles containing V, and doped zinc oxide particles in the coating.

[0004] Furthermore, Patent Document 2 discloses a technique for improving the corrosion resistance of the end face of a painted steel sheet, which is made by forming two or more coating films on at least one side of a Zn-containing plated steel sheet, by setting the outermost layer of the coating film to a predetermined thickness, including a predetermined non-chromium compound in the outermost layer of the coating film, and devising the structure of the coating film so that the electrical conductivity of the immersion water when the painted steel sheet is immersed in deionized water under predetermined conditions is 30 μS / cm or more.

[0005] Furthermore, Patent Document 3 discloses a technique for improving the weldability and corrosion resistance of a painted metal material having an organic film on its surface, by incorporating a predetermined resin having urethane bonds and predetermined conductive particles into the organic film.

[0006] Furthermore, Patent Document 4 discloses a technique for improving the weldability and corrosion resistance of a coated metal plate having a coating layer on its surface, by including a predetermined amount of conductive particles of a predetermined particle size in the coating layer. [Prior art documents] [Patent Documents]

[0007] [Patent Document 1] International Publication No. 2018 / 092244 [Patent Document 2] Japanese Patent Publication No. 2012-136025 [Patent Document 3] Japanese Patent Publication No. 2004-042622 [Patent Document 4] Japanese Patent Publication No. 2004-183080 [Overview of the project] [Problems that the invention aims to solve]

[0008] Surface-treated steel sheets used as components in automobiles and other applications require not only the weldability and corrosion resistance described above, but also good adhesion of the coating after electrodeposition coating. For example, the warm salt water immersion test (SDT) is used to evaluate the adhesion of the coating after electrodeposition coating. According to the inventor's new findings, when SDT is performed on conventional surface-treated steel sheets after electrodeposition coating, blistering and coating delamination may occur on the surface after SDT. When blistering or coating delamination occurs on surface-treated steel sheets, it can cause red rust, making it difficult to ensure sufficient corrosion resistance. Conventional surface-treated steel sheets have not received sufficient consideration for suppressing the occurrence of blistering and coating delamination during SDT, and for improving corrosion resistance after SDT. As described above, a new technology is needed that can achieve both weldability, corrosion resistance, and good adhesion of the coating after electrodeposition coating in surface-treated steel sheets. [Means for solving the problem]

[0009] This application discloses several embodiments as one means of solving the above-mentioned problems. <Aspect 1> Surface-treated steel sheet, A plated steel sheet having a Zn-containing plating layer, and a surface treatment layer provided on at least one main surface of the plated steel sheet, the surface treatment layer has at least a coating film as an outer layer, the coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less, the coating film contains a binder resin, an oil absorbing agent, and a conductive agent, the binder resin contains an epoxy resin, the proportion of the epoxy resin in the binder resin is 25% by volume or more, the oil absorbing agent has an oil absorption of 50 ml / 100g or more, the oil absorbing agent has a particle size that is not less than half the average film thickness and not more than the average film thickness, the coating film contains 5% by volume or more of the oil absorbing agent, A surface-treated steel sheet. <Aspect 2> the surface-treated steel sheet has a 60° gloss of 1% or more and 20% or less, The surface-treated steel sheet according to Aspect 1. <Aspect 3> the oil absorbing agent is silica, The surface-treated steel sheet according to Aspect 1 or 2. <Aspect 4> the conductive agent is doped oxide particles, a Si alloy containing 50% by mass or more of Si, a Si compound containing 50% by mass or more of Si, or a composite thereof, the coating film contains 5% by volume or more and 30% by volume or less of the conductive agent, The surface-treated steel sheet according to any one of Aspects 1 to 3. <Aspect 5> the doped oxide particles are doped zinc oxide particles, The surface-treated steel sheet according to Aspect 4. <Aspect 6> the Si alloy or the Si compound is ferrosilicon containing 70% by mass or more of Si, The surface-treated steel sheet according to Aspect 4 or 5. <Aspect 7> the coating film contains 10% by volume or more of the oil absorbing agent, the surface-treated steel sheet has a 60° gloss of 1% or more and 15% or less, The surface-treated steel sheet according to any one of aspects 1 to 6. <Aspect 8> The surface treatment layer has an inorganic or organic-inorganic composite film as an inner layer between the coating film and the plated steel sheet, The film has an average thickness of 0.1 μm or more and 1.0 μm or less, The surface-treated steel sheet according to any one of aspects 1 to 7. <Aspect 9> A surface-treated steel sheet, comprising a plated steel sheet having a Zn-containing plating layer, and a surface treatment layer provided on at least one main surface of the plated steel sheet, wherein the surface treatment layer has at least a coating film as an outer layer, the coating film has an average thickness of 1.0 μm or more and 10.0 μm or less, the coating film contains a binder resin, an oil absorbing agent, and a conductive agent, the binder resin contains an epoxy resin, the proportion of the epoxy resin in the binder resin is 25% by volume or more, the oil absorbing agent has a particle size that is not less than half and not more than the full size of the average film thickness, the coating film contains the oil absorbing agent in an amount of 5% by volume or more, the surface-treated steel sheet has a 60° gloss of 1% or more and 20% or less, The surface-treated steel sheet. [Effects of the Invention]

[0010] The surface-treated steel sheet of the present disclosure is excellent in weldability, corrosion resistance, and coating adhesion after electrodeposition coating. For example, the occurrence of blisters and coating peeling in SDT after electrodeposition coating is suppressed, and excellent corrosion resistance is maintained even after SDT. [Brief Description of the Drawings]

[0011] [Figure 1]This is a schematic diagram illustrating the action and effects of oil absorbents having an oil absorption capacity of 50 ml / 100 g or more. (A) shows the case where an oil absorbent with an oil absorption capacity of 50 ml / 100 g or more is present in the coating film, and (B) shows the case where a non-oil absorbent with an oil absorption capacity of less than 50 ml / 100 g is present in the coating film. [Modes for carrying out the invention]

[0012] The embodiments of the present invention will be described below. These descriptions are intended to be merely illustrative of embodiments of the present invention, and the present invention is not limited to the following embodiments.

[0013] The surface-treated steel sheet according to the embodiment comprises a plated steel sheet having a Zn-containing plating layer and a surface treatment layer provided on at least one main surface of the plated steel sheet. The surface treatment layer has at least a coating film as an outer layer. The coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less. The coating film contains a binder resin, an oil absorbent, and a conductive agent. The binder resin contains an epoxy resin. The proportion of the epoxy resin in the binder resin is 25 volume% or more. The oil absorbent has an oil absorption capacity of 50 ml / 100 g or more. The oil absorbent has a particle size of more than half the average film thickness and less than or equal to it. The coating film contains 5 volume% or more of the oil absorbent.

[0014] 1. Plated steel sheet A plated steel sheet comprises, for example, a base steel sheet and a Zn-containing plating layer provided on at least one main surface of the base steel sheet. In this application, "main surface" refers to the surface corresponding to the front or back side of the sheet. The Zn-containing plating layer may be provided on only one main surface of the base steel sheet, or on both main surfaces. Furthermore, the Zn-containing plating layer may be provided on the entire main surface of the base steel sheet, or on a part of the main surface.

[0015] Various types of steel sheets with different chemical compositions and microstructures can be used as the base material. The base material may be ordinary steel sheet or steel sheet containing additive elements such as chromium, and the chemical composition and microstructure of the base material should be adjusted considering the desired mechanical properties and formability. Furthermore, the thickness of the base material is not particularly limited; for example, it may be 0.2 mm or more, or 6.0 mm or less.

[0016] The Zn-containing plating layer may have a chemical composition known to those skilled in the art. For example, the Zn-containing plating layer may contain additive elements other than Zn, such as Al, and may also contain Fe if an alloying treatment has been performed. As an example, the Zn-containing plating layer may be a Zn-Al-Mg alloy plating layer containing at least Al and Mg, or a Zn-Al-Mg-Si alloy plating layer further containing Si. The content (concentration) of these elements may be, in mass%, Al: 0-60%, Mg: 0-10%, Si: 0-2%, Mn: 0-1%, Ni: 0-1%, Sb: 0-1%, Fe: 0-20%. The Zn-containing plating layer may be an alloyed hot-dip galvanized layer, a hot-dip galvanized layer, or an electro-galvanized layer. The amount of zinc-containing plating layer adhering to the base steel sheet is not particularly limited and may be a general amount. For example, the thickness of the Zn-based alloy plating layer may be 1-30 μm.

[0017] 2. Surface treatment layer The surface treatment layer is provided on at least one main surface of the plated steel sheet. The surface treatment layer may be provided on only one main surface of the plated steel sheet, or on both main surfaces. Furthermore, the surface treatment layer may be provided on the entire main surface of the plated steel sheet, or on a part of the main surface. The surface treatment layer can be laminated on the surface of the Zn-containing plating layer of the plated steel sheet.

[0018] The surface treatment layer has at least a coating as an outer layer. The surface treatment layer may consist only of a coating, or it may have a two-layer structure consisting of a coating as an outer layer and a chemical conversion treatment coating as an inner layer. When the surface treatment layer has the two-layer structure, it can exhibit superior corrosion resistance, etc. On the other hand, when the surface treatment layer does not have a chemical conversion treatment coating as an inner layer, it can exhibit superior spot weldability.

[0019] 2.1 Coating film In the surface-treated steel sheet according to this embodiment, the coating film includes a binder resin, an oil absorbent, and a conductive agent.

[0020] (Binder resin) The binder resin includes an epoxy resin. The inclusion of an epoxy resin as a binder in the coating film improves adhesion to the electrodeposited coating film. The epoxy resin may be an aromatic epoxy resin, an aliphatic epoxy resin, or an epoxy resin such as an amine. Specific examples of epoxy resins include, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, and triphenylmethane type epoxy resin. The epoxy resin may be combined with a curing agent. Various epoxy curing agents, such as phenolic resins, can be used as the curing agent.

[0021] The binder resin may contain resins other than epoxy resin in addition to epoxy resin. Examples of resins other than epoxy resin include various thermosetting resins and thermoplastic resins. For example, at least one resin selected from polyester resin, urethane resin, acrylic resin, nylon resin, and olefin resin. When polyester resin is used as the binder resin, it may have a glass transition temperature (Tg) of -20 to 70°C and a number average molecular weight of 3,000 to 30,000. When urethane resin is used as the binder resin, it may have a Tg of 0 to 50°C and a number average molecular weight of 5,000 to 25,000. When acrylic resin is used as the binder resin, it may have a Tg of 0 to 50°C and a number average molecular weight of 3,000 to 25,000. The binder resin may contain curing agents other than epoxy curing agents. For example, melamine resin or isocyanate resin may be used.

[0022] It is important that the proportion of epoxy resin in the binder resin is 25% by volume or more. That is, with the total binder resin being 100% by volume, the proportion of epoxy resin is 25% by volume or more. The proportion of epoxy resin may be 30% by volume or more, 40% by volume or more, 50% by volume or more, 60% by volume or more, 70% by volume or more, 80% by volume or more, or 90% by volume or more. If the proportion of epoxy resin in the binder resin is too low, the adhesion between the coating film and the electrodeposition coating film may be insufficient, and the corrosion resistance after SDT may be insufficient. There is no particular upper limit to the proportion of epoxy resin in the binder resin, and the proportion of epoxy resin may be 100% by volume.

[0023] The binder resin content in the coating film is not particularly limited and may be, for example, 50% by volume or more, 60% by volume or more, 90% by volume or less, 80% by volume or less, or 70% by volume or less.

[0024] (Oil absorbent) The oil absorbent has the function of absorbing resin, and may have an oil absorption capacity of, for example, 50 ml / 100 g or more. Examples of materials having an oil absorption capacity of 50 ml / 100 g or more include oxide-based materials such as silica, iron oxide, and titanium oxide, and barium-based materials such as barium carbonate and barium sulfate. These can also function as pigments. In other words, the oil absorbent may be an oil-absorbing pigment. Furthermore, among these oil absorbents, those that also function as rust inhibitors may be used. In other words, the oil absorbent may be an oil-absorbing rust inhibitor. In particular, when the oil absorbent is silica, the silica exhibits high rust prevention properties, making it easier to further improve the corrosion resistance of the surface-treated steel sheet. In this embodiment, the oil absorbent has a particle size of more than half of the average film thickness of the coating film and equal to or less than half of that thickness. Also, the oil absorbent accounts for 5 volume% or more of the coating film.

[0025] When the oil absorbent has a particle size that is more than half but less than or equal to the average thickness of the coating film, and accounts for 5% by volume of the coating film, the following effects can be expected. That is, as shown in Figure 1(A), when a coating film is formed using paint containing an oil absorbent, during the heating process for drying and solidifying the paint, the oil absorbent containing the solvent in the paint releases the solvent, and then the oil absorbent absorbs surrounding resin, etc. (as shown by the white arrows in the figure, the resin, etc. moves towards the oil absorbent), resulting in a state where there is a shortage of resin, etc. around the oil absorbent. As a result, irregularities are formed on the surface of the coating film. The formation of irregularities on the surface of the coating film increases the surface area of ​​the coating film, which can improve the physical adhesion between the coating film and the electrodeposited coating film. In addition, the frequency of contact between the chemical components contained in the coating film and the electrodeposited coating film increases, which can also improve the chemical adhesion between the coating film and the electrodeposited coating film. In contrast, if the coating does not contain an oil absorbent (or if a non-oil absorbent is included instead), if the particle size of the oil absorbent is too small, and / or if the oil absorbent content is too low, the surface irregularities formed on the coating will be small (Figure 1(B)), making it difficult to ensure high adhesion to the electrodeposited coating. Furthermore, if the particle size of the oil absorbent is too large relative to the average thickness of the coating, the oil absorbent is more likely to protrude significantly from the surface of the coating, causing it to detach from the coating and reducing corrosion resistance. Additionally, the oil absorbent is more likely to come into contact with the tip of the electrode during spot welding, hindering contact between the electrode and the conductive agent, which may reduce spot weldability.

[0026] As described above, the oil absorption capacity of the oil absorbent is, for example, 50 ml / 100 g or more. The oil absorption capacity of the oil absorbent may be 60 ml / 100 g or more, 70 ml / 100 g or more, 80 ml / 100 g or more, 90 ml / 100 g or more, or 100 ml / 100 g or more, and may also be 500 ml / 100 g or less, 450 ml / 100 g or less, 400 ml / 100 g or less, 350 ml / 100 g or less, or 300 ml / 100 g or less. In this application, the "oil absorption capacity" of the oil absorbent before it is incorporated into the coating film can be measured in accordance with "JIS K5101-13-1:2004 Pigment Test Methods - Part 13: Oil Absorption Capacity - Section 1: Refined Linseed Oil Method". On the other hand, the "oil absorption capacity" of the oil absorbent after it is incorporated into the coating film can be measured as follows (1) to (3). Furthermore, the following example illustrates how to measure the amount of oil absorbed when "silica" is used as the oil absorbent. If an oil absorbent containing element M is used instead of element Si, the amount of oil absorbed by the oil absorbent can be measured by analyzing element M instead of element Si in the elemental analysis described below. (1) Using SEM-EDX (JEOL Ltd. JSM-7200F (SEM), JED-2300 / F (EDS)), the cross-section of the coating film is observed to identify the silica particles contained in the coating film, and the atomic percentages of elements C, O, and Si contained in those silica particles are determined. Here, regions with a particle size of 1 μm or more where elements Si and O are distributed at 80 atomic percentage or more are identified as silica particles, and the atomic percentages of elements C, O, and Si are determined by region analysis of the part of that region excluding the outer edge 0.2 μm (central part), or by point analysis of the central part. Cross-sectional observation is performed after resin embedding, polishing, and Au deposition. (2) Based on atomic%, the mass ratio of silica to resin is determined. In this case, the O in the resin is the remainder (remainder O) obtained by subtracting the silica (SiO2) from the O content determined by SEM-EDX. That is, the resin content is C and the remainder O. (3) Determine the volume of resin per 100g of silica from the mass ratio of silica to resin, and determine the oil absorption amount (ml / 100g). Assume the specific gravity of the resin is 1.2.

[0027] The particle size of the oil absorbent described above is more than half (50% or more) of the average film thickness of the coating film, and less than or equal to (100% or less). The particle size of the oil absorbent may be 55% or more, 60% or more, or 65% or more of the average film thickness of the coating film, and may be less than 100%, 95% or less, 90% or less, or 85% or less. In this application, the "particle size" of the oil absorbent contained in the coating film is determined as follows: A surface-treated steel plate on which the coating film is formed is cut, the cross-section is exposed and polished, and the polished cross-section obtained in this way is observed with a scanning electron microscope to obtain an observation image. The shape of the oil absorbent particles present in the field of view of the observation image is determined. The ferret diameter in the direction along the film thickness direction of the coating film is determined for the shape of the oil absorbent. The determined ferret diameter is considered to be the "particle size" of the oil absorbent. It can be easily determined whether or not the particles in the observation image are oil absorbent by performing elemental analysis, etc.

[0028] The oil absorbent content in the coating film is 5% by volume or more. The upper limit of the oil absorbent content may be determined considering the durability and conductivity of the coating film. If the oil absorbent content in the coating film is too high, the content of the binder resin and conductive agent will be relatively low, which may relatively reduce the durability and conductivity of the coating film. The oil absorbent content in the coating film may be 10% by volume or more, 15% by volume or more, or 20% by volume or more, and may also be 40% by volume or less, 35% by volume or less, or 30% by volume or less.

[0029] (Rust inhibitor) The coating may contain a rust inhibitor. The rust inhibitor may be an inorganic rust inhibitor or an organic rust inhibitor. The rust inhibitor may contain at least one of the elements P and V, which exhibit rust-preventive properties. Examples of rust inhibitors containing P include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid; ammonium salts such as triammonium phosphate and diammonium hydrogen phosphate; metal phosphates with Na, Mg, Al, K, Ca, Mn, Ni, Zn, Fe, etc.; phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid) and their salts; organic phosphoric acids such as phytic acid and their salts. Furthermore, examples of rust inhibitors containing V include vanadium pentoxide, HVO3 metavanadate, ammonium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3)3, vanadium acetylacetonate V(OC(=CH2)CH2COCH3)3, and vanadium trichloride VCl3. The rust inhibitor may also be a guanidino group-containing compound, a biguanidino group-containing compound, a thiocarbonyl group-containing compound, etc. The rust inhibitor may take the form of, for example, particulate matter. The rust inhibitor may be water-soluble or non-water-soluble. If the rust inhibitor is water-soluble, for example, when the coating film is exposed to a humid environment, the rust inhibitor may dissolve and leach in water, exhibiting a rust-preventive function that suppresses corrosion of the plating layer. The content of the rust inhibitor in the coating film is not particularly limited. The amount of rust inhibitor may be greater than, less than, or the same as the amount of oil absorbent mentioned above. For example, the amount of rust inhibitor in the coating film may be 0% by volume or more, 0.5% by volume or more, 1.0% by volume or more, or 5.0% by volume or more, or 15% by volume or less, or 10% by volume or less.

[0030] (Conductive agent) The conductive agent has the function of improving the conductivity of the coating film and thereby improving the weldability of the surface-treated steel sheet. In this application, for example, the volume resistivity is 1.0 × 10 3 Materials having a conductivity of Ω / cm or less can be used as conductive agents. Examples of conductive agents include metals and metal compounds. Specifically, these may be metals such as magnesium, aluminum, silicon, calcium, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, germanium, strontium, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, silver, cadmium, indium, and tin; alloys such as magnesium, aluminum, silicon, phosphorus, calcium, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, germanium, arsenic, strontium, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, silver, cadmium, indium, tin, antimony, and tellurium; or compounds such as oxides of the above-mentioned metal elements. Among these, magnesium, aluminum, silicon, chromium, iron, nickel, zinc, tin, zinc-aluminum alloys, zinc-aluminum-magnesium alloys, zinc-aluminum-magnesium-silicon alloys, zinc-iron alloys, zinc-chromium alloys, zinc-nickel alloys, iron-nickel alloys, iron-chromium alloys, stainless steel, ferrosilicon, ferromanganese, ferrophosphor, and zinc oxide are readily available. The content of conductive agents in the coating is not particularly limited and should be determined appropriately considering the desired weldability and corrosion resistance.

[0031] In particular, when the conductive agent is doped oxide particles, a Si alloy containing 50% by mass or more of Si, a Si compound containing 50% by mass or more of Si, or a composite thereof, it is easier to improve conductivity (weldability) as well as the adhesion of the electrodeposited coating film to the outer layer. In this case, the content of the conductive agent in the coating film may be 5% by volume or more and 30% by volume or less.

[0032] When the conductive agent is doped oxide particles, a specific example of such doped oxide particles is doped zinc oxide particles. Examples of doped zinc oxide particles include those obtained by doping zinc oxide particles with at least one doping element selected from the group consisting of Group 13 elements of the periodic table such as B, Al, Ga, and In, and Group 15 elements of the periodic table such as P and As, thereby improving conductivity. When the doping element is Al or Ga, it is easier to further improve conductivity. The content of the doped element may be, for example, 0.05 atom% or more, or 0.1 atom% or more, and may be 5 atom% or less, relative to undoped zinc oxide particles.

[0033] When the conductive agent is a Si alloy or Si compound, a specific example of such Si alloy or Si compound is ferrosilicon containing 70% by mass or more Si. By incorporating ferrosilicon as a conductive agent into the coating film, it is easy to improve both the conductivity and corrosion resistance of the coating film. In particular, ferrosilicon containing 70% by mass or more Si has excellent corrosion resistance and moldability.

[0034] The conductive agent may be in particulate form, for example. When the conductive agent is in particulate form, its average particle size is not particularly limited and should be selected to be of an appropriate size considering the thickness of the coating film, etc. If the particle size of the conductive agent is too small relative to the thickness of the coating film, the conductivity is likely to decrease. On the other hand, if the particle size of the conductive agent is too large relative to the thickness of the coating film, the conductive agent is likely to detach from the coating film. In this regard, the particle size of the conductive agent may be 1 / 10 or more, or 1 / 5 or more, of the thickness of the coating film, and may also be 2 times or less, or the same as or less. The average particle size of the conductive agent may be, for example, 0.1 μm or more, 0.3 μm or more, 0.5 μm or more, or 1.0 μm or more, and may also be 20 μm or less, 10 μm or less, 8.0 μm or less, 6.0 μm or less, 5.0 μm or less, 4.0 μm or less, or 2.5 μm or less. Furthermore, the "average particle diameter" of a conductive agent refers to the average primary particle diameter when the particles present in the coating film exist as primary particles, and the average secondary particle diameter when they exist in aggregate form. The average particle diameter is measured as follows: A surface-treated steel plate with a coating film is cut, the cross-section is exposed and polished, and the resulting polished cross-section is observed with a scanning electron microscope to obtain an observation image. Several conductive particles are arbitrarily selected from the field of view of the observation image, the equivalent circle diameter of each particle is determined, and the average value of these is taken as the average particle diameter. Whether or not the particles in the observation image are conductive agents can be easily determined by performing elemental analysis, etc.

[0035] (Other ingredients) The coating film may contain components other than those described above. These other components include various additives. For example, pigments other than the oil absorbents and conductive agents mentioned above (such as glossy pigments for improving aesthetics), lubricants, defoamers, and thickeners. The amount of these other components in the coating film is not particularly limited.

[0036] (Average film thickness) In this embodiment, the coating film has an average film thickness of 1.0 μm or more and 10.0 μm. If the coating film is too thin, sufficient corrosion resistance may not be obtained. On the other hand, if the coating film is too thick, spot weldability may decrease. The average film thickness of the coating film may be 2.0 μm or more or 3.0 μm or more, or 9.0 μm or less, 7.0 μm or less, or 5.0 μm or less. The average film thickness of the coating film is measured as follows: The surface-treated steel sheet on which the coating film is formed is cut, the cross-section is exposed and polished, and the polished cross-section obtained in this way is observed with a scanning electron microscope to obtain an observation image. The thickness of the coating film present in the field of view of the observation image is measured at 10 or more points at 1.0 μm intervals in the plane direction of the plated steel sheet, and the average value is taken as the average film thickness. Alternatively, the average film thickness of the coating film may be determined by calculating the density of the coating film from the components contained in the coating film and then measuring the weight of the coating film. In this embodiment, the average film thickness characterized by either method is sufficient as long as it is between 1.0 μm and 10.0 μm.

[0037] (Amount of adhesion) The amount of coating film adhering is not particularly limited. For example, the amount of coating film adhering is 2.0 g / m². 2 More than 3.5g / m 2 or more, or 5.0 g / m 2 It may be greater than or equal to 20g / m 2 Below 15g / m 2 The following or 10g / m² 2 The following methods may also be used. Furthermore, the amount of coating on surface-treated steel sheets can be measured by gravimetric methods or cross-sectional observation. For gravimetric measurement, the initial weight of a steel sheet cut to a predetermined size is measured. Then, the coating is removed using a solvent or specialized chemical capable of dissolving the binder resin, or by blast treatment using resin beads or alumina beads. The weight of the steel sheet after removing the coating is then measured, and the difference between these two weights is calculated to determine the amount of coating.

[0038] 2.2 Chemical conversion coating In the surface-treated steel sheet according to this embodiment, the surface treatment layer may have an inorganic or organic-inorganic composite film as an inner layer between the coating and the steel sheet, and the film may have an average film thickness of 0.1 μm or more and 1.0 μm or less. This film may also be called a chemical conversion treatment film. That is, the surface treatment layer may have a two-layer structure consisting of a coating as an outer layer and a chemical conversion treatment film as an inner layer.

[0039] (Components) By providing a chemical conversion coating as an inner layer on the surface of a plated steel sheet, and further providing the aforementioned coating on the surface of the chemical conversion coating, the adhesion of the coating to the plated steel sheet is improved. The chemical conversion coating may be a layer that is substantially free of chromium (chromate-free layer). Examples of chromate-free treatment solutions used in chemical conversion include silica-based treatment solutions mainly composed of silicon compounds such as liquid-phase silica, gas-phase silica, and silicates, zircon-based treatment solutions mainly composed of zircon compounds, and mixtures thereof. The chemical conversion coating may contain a binder resin. For example, the chemical conversion coating may contain at least one of the binder resins exemplified as capable of constituting the aforementioned coating. The content of binder resin and other components in the chemical conversion coating is not particularly limited. For example, the binder resin content in the chemical conversion coating may be 0% to 50% by volume, and the content of components other than the binder resin may be 50% to 100% by volume. The chemical conversion coating as the inner layer may be an inorganic coating containing inorganic components as a binder, or an organic-inorganic composite coating. The chemical conversion coating may contain various additives. For example, these may include brightening pigments, lubricants, defoamers, and thickeners for the purpose of improving aesthetics. The content of other components in the chemical conversion coating is not particularly limited.

[0040] (Average film thickness) The average film thickness of the chemical conversion treatment film is not particularly limited. From the viewpoints of further improving the adhesion between the plated steel sheet and the coating film, further improving corrosion resistance and weldability, etc., the average film thickness of the chemical conversion treatment film is preferably 0.1 μm or more and 1.0 μm or less. The average film thickness of the chemical conversion treatment film can be measured in the same manner as the average film thickness of the coating film. That is, the surface-treated steel sheet on which the chemical conversion treatment film is formed is cut, its cross section is exposed and then polished, and the polished cross section thus obtained is observed with a scanning electron microscope to obtain an observation image. The thickness of the chemical conversion treatment film present in the field of view of the observation image is measured at 10 or more points at intervals of 1 μm in the surface direction of the plated steel sheet, and the average value thereof is taken as the average film thickness. Alternatively, the average film thickness of the chemical conversion treatment film may be specified by determining the density of the chemical conversion treatment film from the components contained in the chemical conversion treatment film and then measuring the weight of the chemical conversion treatment film.

[0041] (Adhesion amount) In the surface-treated steel sheet, the adhesion amount of the chemical conversion treatment film is not particularly limited. For example, the adhesion amount of the chemical conversion treatment film is 200mg / m 2 or more and 2000mg / m 2 or less, the corrosion resistance of the surface-treated steel sheet can be further improved easily. The adhesion amount of the chemical conversion treatment film on the surface-treated steel sheet can be measured by X-ray fluorescence and cross-sectional analysis. Specifically, a calibration curve plate is prepared for each chemical conversion treatment. The chemically treated plate and the calibration curve plate are measured by X-ray fluorescence, and the adhesion amount of the produced chemically treated plate is calculated from the X-ray intensity of the contained elements and the X-ray intensity of the calibration curve plate.

[0042] 3. Effects As described above, in the surface-treated steel sheet according to this embodiment, the inclusion of an oil absorbent in the coating film creates irregularities on the surface of the coating film. These irregularities on the surface of the coating film improve adhesion between the coating film and the electrodeposited coating film, suppressing blistering and coating peeling during SDT (Surface Deposition Testing), and ensuring excellent corrosion resistance even after SDT. Furthermore, by keeping the average thickness of the coating film below a certain level and the particle size of the oil absorbent in the coating film below a certain level, excellent weldability can also be ensured. Thus, the surface-treated steel sheet according to this embodiment exhibits excellent weldability, corrosion resistance, and coating adhesion after electrodeposition painting. For example, the occurrence of blistering and coating peeling during SDT after electrodeposition painting is suppressed, and excellent corrosion resistance is maintained even after SDT.

[0043] The surface-treated steel sheet according to this embodiment tends to have a 60° gloss within a certain range due to the irregularities formed on the surface of the coating film. That is, the surface-treated steel sheet according to this embodiment may have a 60° gloss of 1% to 20%. Thus, having a 60° gloss of 1% to 20% of the surface-treated steel sheet tends to result in even better adhesion between the coating film and the electrodeposited coating film. The 60° gloss of the surface-treated steel sheet can vary depending on the amount of the oil absorbent contained in the coating film. For example, the surface-treated steel sheet according to this embodiment may have a coating film containing 10% or more of the oil absorbent, and the surface-treated steel sheet may have a 60° gloss of 1% to 15%. The 60° gloss of the surface-treated steel sheet can be measured using a gloss meter (Gloss Meter GM-1 manufactured by Suga Test Instruments Co., Ltd.).

[0044] 4. Manufacturing method of surface-treated steel sheet The above-mentioned surface-treated steel sheet can be manufactured, for example, by the following method. That is, the method for manufacturing the surface-treated steel sheet is: To obtain a plated steel sheet having a zinc-containing plating layer, and A coating film is formed by applying a paint containing a binder resin, an oil absorbent, and a conductive agent to at least one main surface of the plated steel sheet. It may include.

[0045] Alternatively, the manufacturing method for surface-treated steel sheets is: To obtain a plated steel sheet having a zinc-containing plating layer, A chemical conversion treatment is applied to at least one main surface of the plated steel sheet to form a chemical conversion treatment film, and A coating is formed by applying a paint containing a binder resin, an oil absorbent, and a conductive agent to the surface of the aforementioned chemical conversion treated film. It may include.

[0046] 4.1 Fabrication of plated steel sheets A plated steel sheet having a Zn-containing plating layer can be obtained, for example, by obtaining a slab by continuous casting, hot rolling the slab to obtain a hot-rolled sheet, winding the hot-rolled sheet, cold rolling the hot-rolled sheet to obtain a cold-rolled sheet, annealing the cold-rolled sheet, applying a plating treatment to the sheet after annealing, and optionally performing a skin pass. The continuous casting conditions, hot rolling conditions, winding conditions, cold rolling conditions, annealing conditions, and plating conditions may be conventionally known general conditions.

[0047] 4.2 Chemical treatment In the manufacturing method of this disclosure, a chemical conversion treatment film may be formed as an inner layer by applying a chemical conversion treatment to at least one main surface of the plated steel sheet obtained as described above. The chemical conversion treatment can be carried out by applying the various treatment solutions described above to the surface of the steel sheet and drying it.

[0048] 4.3 Formation of the coating film In the manufacturing method of the present disclosure, a coating film as an outer layer may be formed by applying a paint containing a binder resin, an oil absorbent, and a conductive agent to the surface of the plated steel sheet obtained as described above, or to the surface of the chemical conversion coating film formed as described above, and then drying it. Here, by adjusting the type of oil absorbent contained in the coating film, the content of the oil absorbent, the thickness of the coating film, etc., a surface-treated steel sheet according to the above embodiment can be obtained. Furthermore, according to the inventor's new findings, it is possible to further improve the roughness of the coating film by rapidly heating it during drying after the coating film is formed. In general painted steel sheets, if the coating film is heated rapidly during drying, the surface of the coating film hardens before the solvent in the paint has completely evaporated, resulting in a coating film containing air bubbles, i.e., coating bubbling. For this reason, it is common to heat slowly until the solvent evaporates, and then increase the heating rate. In contrast, according to the inventor's new findings, when forming a coating film having an average film thickness of 1.0 μm or more and 10.0 μm or less, bubbling is less likely to occur even if rapid heating is performed during coating film drying. Rapid heating during coating drying allows the solvent contained in the oil absorbent to be quickly discharged from the system, increasing the amount of resin absorbed by the oil absorbent and further improving the roughness of the coating. In this regard, in the manufacturing method of this disclosure, the heating rate during coating drying is preferably 20°C / s or higher, and more preferably 40°C / s or higher. As far as the inventors have confirmed, when the heating rate during coating drying is 20°C / s or higher, the 60° gloss value of the surface-treated steel sheet is less than 20%, and when the heating rate during coating drying is 40°C / s or higher, the 60° gloss value of the surface-treated steel sheet is 17% or lower. There is no particular upper limit to the heating rate. From the viewpoint of suppressing the occurrence of coating defects such as coating edges, and from the viewpoint of allowing sufficient discharge of the solvent contained in the oil absorbent and absorption of resin by the oil absorbent, the practical upper limit of the heating rate is 100°C / s.

[0049] 5. Variations The surface-treated steel sheet of the present disclosure may have the following configuration. That is, the modified surface-treated steel sheet comprises a plated steel sheet having a Zn-containing plating layer and a surface treatment layer provided on at least one main surface of the plated steel sheet. Here, the surface treatment layer has at least a coating film as an outer layer, the coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less, the coating film contains a binder resin, an oil absorbent and a conductive agent, the binder resin contains an epoxy resin, the proportion of the epoxy resin to the binder resin is 25 volume% or more, the oil absorbent has a particle size of more than half the average film thickness and less than or equal to it, the coating film contains 5 volume% or more of the oil absorbent, and the surface-treated steel sheet has a 60° gloss of 1% or more and 20% or less. In the modified surface-treated steel sheet, for example, by including an oil absorbent of a predetermined size relative to the film thickness, the resin surrounding the oil absorbent is absorbed by the oil absorbent, resulting in roughness and a 60° gloss of 1% to 20%. Surface-treated steel sheets with such a configuration have excellent weldability, corrosion resistance, and adhesion of the coating after electrodeposition coating. For example, the occurrence of blistering and coating peeling during SDT after electrodeposition coating is suppressed, and excellent corrosion resistance is maintained even after SDT. [Examples]

[0050] The present invention will be further described below with reference to examples, but the present invention is not limited to the following examples. The present invention allows for the adoption of various conditions as long as they do not depart from the spirit of the invention and achieve the objectives of the present invention.

[0051] 1. Manufacturing of surface-treated steel sheets 1.1 Preparation of alloyed hot-dip galvanized steel sheet The following five types of zinc-plated steel sheets and cold-rolled steel sheets were prepared. The surfaces were degreased by immersing them in an aqueous solution (2.5% by mass, 40°C) of a water-based alkaline degreasing agent (FC-301, manufactured by Nippon Parkerizing Co., Ltd.) for 2 minutes, then washed with water and dried to prepare base metal sheets for surface treatment.

[0052] GA: Alloyed hot-dip galvanized steel sheet (thickness 0.8 mm, 10% Fe by mass, plating adhesion 45 g / m²)2 ) ZA1: Zn-Al-Mg tripod-type hot-dip galvanized steel sheet (Zn-11%Al-3%Mg-0.2%Si) (Sheet thickness 0.8mm, 10% Fe by mass, plating adhesion 60g / m²) 2 ) ZA2: Zn-Al-Mg tripod-type hot-dip galvanized steel sheet (Zn-6%Al-3%Mg) (Sheet thickness 0.8mm, 10%Fe by mass, plating adhesion 60g / m²) 2 ) ZL: Electrolytic Zn-10 mass% Ni alloy plated steel sheet (thickness 0.8 mm, plating adhesion 40 g / m²) 2 ) GI: Hot-dip galvanized steel sheet (thickness 0.8 mm, plating thickness 60 g / m²) 2 ) EG: Electro-galvanized steel sheet (thickness 0.8 mm, plating thickness 40 g / m²) 2 ) CR: Cold-rolled steel sheet (0.8mm thickness, no plating)

[0053] 1.2 Formation of the inner layer (chemical conversion coating) Next, the following chemical conversion treatment solution S was prepared, and the solution was applied to the above-mentioned base metal plate while changing the grit of the bar coat so that the adhesion amount shown in Tables 3 and 4 was achieved. Then, the metal plate was dried in a hot air oven so that the temperature reached on the surface of the metal plate was 70°C, and then air-dried to form a chemical conversion treatment film on the surface of the metal plate. The average thickness of the chemical conversion treatment film was 0.2 μm.

[0054] A chemical conversion treatment solution consisting of S:Zr compound, silane coupling agent, silica microparticles, and polyester resin, with an Nv of 10%.

[0055] 1.3 Formation of the outer layer (coating film) Next, in order to form a coating film having the composition ratio (volume %) shown in Tables 1 and 2, each component was mixed to achieve the same solid content concentration as in Tables 1 and 2, and a coating composition for film formation was prepared. This composition was applied to a base metal plate or a chemical conversion treated film using a bar coater, while changing the bar coat grit and dilution ratio to achieve the adhesion amount shown in Tables 3 and 4, and dried in an oven under conditions where the maximum temperature reached was 200°C, thereby forming a coating film as the outer layer. The average film thickness of the coating film was the film thickness (μm) shown in Tables 3 and 4. The components contained in the coating composition are shown below.

[0056] (Oil-absorbing pigment) SC: Calcium ion exchange silica (Ca exchange rate 9%) (oil absorption capacity 300 ml / 100 g, particle size 2 μm) Si1: Silica (oil absorption 250ml / 100g, particle size 2μm) Si2: Silica (oil absorption capacity 100 ml / 100 g, particle size 1, 2, 3, 5, or 10 μm) Si3: Silica (oil absorption 50ml / 100g, particle size 2μm) FeO: Iron oxide (oil absorption 60ml / 100g, particle size 2μm)

[0057] (Non-oil absorbing pigment) PA: Aluminum tripolyphosphate (oil absorption capacity 10 ml / 100 g, particle size 2 μm) PM: Magnesium phosphate (oil absorption capacity 30 ml / 100 g, particle size 2 μm) Si4: Silica (oil absorption 30ml / 100g, particle size 2μm)

[0058] (Conductive pigment) FeSi: Ferrosilicon particles (average particle size 3 μm, containing 70% or more by mass of Si) SUS: SUS particles (average particle size 4μm) ZnO: Doped zinc oxide particles (23-Kt, manufactured by Hakusui Tech Co., Ltd., average particle size 0.5 μm)

[0059] (Binder resin) B1: Epoxy resin (ADEKA EP-4100) B2: Polyester resin (Byron 200, manufactured by Byron) B3: Epoxy resin (ADEKA EM-0461N) B4: Polyester resin (Byron MD1480, manufactured by Byron Co., Ltd.) B5: Urethane resin (Superflex 150, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) B6: Melamine resin (Allnex Cymel 325)

[0060] 2. Performance evaluation test The following performance evaluation tests were performed on each surface-treated steel sheet.

[0061] 2.1 Warm Salt Immersion Test (SDT) (Preparation) Each surface-treated steel sheet was subjected to surface conditioning for 20 seconds at room temperature using the surface conditioning agent Preparen X (product name) manufactured by Nippon Parkerizing Co., Ltd. Furthermore, chemical conversion treatment (phosphate treatment) was performed using the chemical conversion treatment solution (zinc phosphate treatment solution) "Palbond 3020 (product name)" manufactured by Nippon Parkerizing Co., Ltd. The temperature of the chemical conversion treatment solution was set to 43°C, and the hot-pressed material was immersed in the chemical conversion treatment solution for 120 seconds, followed by rinsing with water and drying. After the above chemical conversion treatment (phosphate treatment), a cationic electrodeposition paint manufactured by Nippon Paint Co., Ltd. was electrodeposited using a slope current of 160V, and then baked at a baking temperature of 170°C for 20 minutes. The average thickness of the electrodeposited coating film after electrodeposition was 10 μm for all samples.

[0062] (Corrosion resistance under SDT) After the electrodeposition coating described above, the edges of the surface-treated steel sheet were sealed with tape and immersed in a 3% NaCl aqueous solution at 50°C for 500 hours. After the immersion test, the sample was removed, dried, and the area percentage of blisters present on the electrodeposited coating surface was visually measured. In this corrosion resistance test, a score of "3" was judged to indicate a certain degree of corrosion resistance, and a score of "4" or "5" was judged to indicate excellent corrosion resistance. The results are shown in Tables 3 and 4. 1: Blister area ratio from an evaluation perspective is 50% or more. 2: Blister area ratio from an evaluation perspective is 5% or more but less than 50% 3: Blister area ratio from an evaluation perspective is 1% or more but less than 5% 4. From an evaluation standpoint, blistering occurs, but less than 1% of cases. 5: No blistering occurred.

[0063] 2.2 Post-SDT Corrosion Resistance Test Surface-treated steel plates that had been subjected to electrodeposition coating after a hot salt water immersion test were subjected to 120 cycles of cyclic corrosion testing under the following cycle conditions.

[0064] (Cycle conditions) The experiment was conducted using a cycle consisting of salt spray (SST, 5% NaCl, 35°C atmosphere) for 2 hours, drying (60°C) for 2 hours, and wetting (50°C, 98% RH) for 4 hours.

[0065] Subsequently, the corrosion status from the flat surface was observed, and the following scores were assigned. In this corrosion resistance test, a score of "3", "4", or "5" indicated excellent corrosion resistance. The results are shown in Tables 3 and 4. 1: White rust is observed on 50% or more of the surface area from which the evaluation surface was taken, or red rust is observed from the evaluation surface. 2: White rust occurrence rate from the evaluation surface is 10% or more but less than 50% 3: White rust occurrence rate from the evaluation surface is 5% or more but less than 10% 4: White rust occurrence rate from the evaluation surface is 1% or more but less than 5% 5: White rust occurrence rate from the evaluation surface is less than 1%

[0066] 2.3 Spot weldability Each surface-treated steel plate was subjected to a continuous spot welding test using a CF-type Cr-Cu electrode with a tip diameter of 5 mm and radius of R40, with a pressing force of 1.96 kN, a welding current of 8 kA, and an energizing time of 12 cycles / 50 Hz. The number of spots just before the nugget diameter fell below 3√t (where t is the plate thickness) was determined. The superiority of the spot weldability was evaluated using the following evaluation points. In this weldability test, a score of "4", "5", or "6" was judged to indicate excellent weldability. The results are shown in Tables 3 and 4. 1: No nuggets are generated and no welding points can be performed, or the number of weld points is less than 10. 2: Number of RBIs: 10 or more but less than 50 3: Number of RBIs between 50 and 200 4: Number of RBIs between 200 and 1000 5: Number of RBIs between 1000 and 2000 6: Number of RBIs is 2000 or more

[0067] 2.4 60° Gloss The 60° gloss of each surface-treated steel sheet was measured using a BYK Microtrigloss. The measured 60° gloss values ​​(%) are shown in Tables 3 and 4.

[0068] [Table 1]

[0069] [Table 2]

[0070] [Table 3]

[0071] [Table 4]

[0072] 3. Results and Discussion The results shown in Tables 1-4 indicate the following:

[0073] Although samples No. 1 and 2 contained an oil-absorbing pigment with an oil absorption capacity of 50 ml / 100 g, its content was less than 5% by volume. As a result, the resin and other materials were not sufficiently absorbed by the oil-absorbing pigment during film formation, causing the surface of the coating to become smooth. Consequently, sufficient adhesion was not obtained between the coating and the electrodeposition coating, resulting in poor corrosion resistance after SDT (Surface-Defined Therapy).

[0074] In the case of No. 23, the Si4 contained in the coating film is a non-oil-absorbing pigment with an oil absorption capacity of less than 50 ml / 100 g. As a result, the resin and other materials were not absorbed into the non-oil-absorbing pigment during coating film formation, and the surface of the coating film became smooth. Consequently, sufficient adhesion was not obtained between the coating film and the electrodeposition coating film, resulting in poor corrosion resistance after SDT (Surface Deposition Testing).

[0075] For Nos. 25 and 26, the PA and PM contained in the coating film were non-oil-absorbing pigments with an oil absorption capacity of less than 50 ml / 100 g. As a result, resins and other materials were not absorbed into the non-oil-absorbing pigments during coating film formation, and the surface of the coating film became smooth. Consequently, a large amount of blistering occurred during SDT (Surface Deposition Testing), and the corrosion resistance after SDT was also poor.

[0076] In the case of No. 28, the binder resin constituting the coating film did not contain epoxy resin, resulting in poor adhesion between the coating film and the electrodeposition coating film. As a result, a large amount of blistering occurred during SDT (Surface Deposition Testing), and the corrosion resistance after SDT was also poor.

[0077] For Nos. 29 and 30, the proportion of epoxy resin in the binder resin constituting the coating film was too low, resulting in poor adhesion between the coating film and the electrodeposition coating film. As a result, a large amount of blistering occurred during SDT (Surface Deposition Testing), and the corrosion resistance after SDT was also poor.

[0078] In the case of No. 43, the particle size of the oil-absorbing pigment was less than half of the film thickness (0.33 times / 1 / 3), resulting in insufficient absorption of resin and other materials into the oil-absorbing pigment during film formation, causing the surface of the film to become smooth. As a result, sufficient adhesion could not be obtained between the paint film and the electrodeposition coating film, leading to the generation of a large amount of blisters during SDT and poor corrosion resistance after SDT.

[0079] For samples No. 45 and 46, the particle size of the oil-absorbing pigment was 1.67 times and 3.33 times the film thickness of the coating, respectively, which was greater than the film thickness, making it easy for the oil-absorbing pigment to detach from the coating. In addition, the oil-absorbing pigment excessively absorbed the resin in the coating, resulting in an excessively thin resin layer. As a result, a large amount of blistering occurred during SDT (Stand-Down Time). Furthermore, for sample No. 46, the tip of the electrode came into contact with the oil-absorbing pigment during spot welding, hindering conductivity to the conductive pigment and reducing spot weldability.

[0080] For No. 47, similar to No. 1, the volume percentage of oil-absorbing pigment contained in the coating film was less than 5%, resulting in significantly inferior corrosion resistance after SDT (Surface-Dependent Treatment).

[0081] For Nos. 54 and 55, similar to No. 28, the binder resin constituting the coating film did not contain epoxy resin, resulting in poor adhesion between the coating film and the electrodeposition coating film. As a result, a large amount of blistering occurred during SDT (Surface Deposition Testing), and the corrosion resistance after SDT was also poor.

[0082] For No. 63, a steel sheet without a Zn plating layer was used, resulting in a large amount of blistering during SDT (Surface Deposition Testing), and significantly inferior corrosion resistance after SDT.

[0083] In the case of No. 64, the coating film thickness was less than 1.0 μm, making it prone to oil-absorbing pigments detaching from the coating. Furthermore, the coating was too thin, making it difficult to ensure sufficient corrosion resistance. As a result, a large amount of blistering occurred during SDT (Surface Deposition Testing), and the corrosion resistance after SDT was also poor.

[0084] In the case of No. 67, similar to No. 43, the particle size of the oil-absorbing pigment was less than half of the film thickness (0.33 times / 1 / 3), resulting in insufficient absorption of resin and other materials into the oil-absorbing pigment during film formation, causing the surface of the film to become smooth. As a result, sufficient adhesion could not be obtained between the paint film and the electrodeposition coating film, and a large amount of blistering occurred during SDT (Stage Deposition Testing).

[0085] For No. 71, the coating thickness was too thick at 15.0 μm, resulting in poor spot weldability.

[0086] In contrast, for Nos. 3-22, 24, 27, 31-42, 44, 48-53, 56-62, 65, 66, 68-70, 72, and 73, (1) the coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less, (2) the coating film contains a binder resin, an oil absorbent, and a conductive agent, (3) the binder resin contains epoxy resin, (4) the proportion of epoxy resin in the binder resin is 25 volume% or more, (5) the oil absorbent has an oil absorption capacity of 50 ml / 100 g or more, (6) the oil absorbent has a particle size of more than half the average film thickness and less than or equal to it, and (7) the coating film contains 5 volume% or more of the oil absorbent. As a result, they have excellent weldability, can suppress blistering during SDT, and have excellent corrosion resistance after SDT.

[0087] Furthermore, binder resins B1 and B2 are solvent-based resins, while binder resins B3 to B5 are water-based resins. As is clear from the above results, the technology of this disclosure is applicable to both solvent-based resins and water-based resins.

[0088] Based on the above results, surface-treated steel sheets that meet the following requirements can be said to have excellent weldability and corrosion resistance, as well as excellent adhesion of the coating after electrodeposition coating.

[0089] Surface-treated steel sheet, A plated steel sheet having a Zn-containing plating layer, The plated steel sheet has a surface treatment layer provided on at least one main surface, The surface treatment layer has at least a coating film as an outer layer, The coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less. The aforementioned coating film comprises a binder resin, an oil absorbent, and a conductive agent. The binder resin comprises an epoxy resin, The proportion of the epoxy resin in the binder resin is 25% by volume or more. The oil absorbent has an oil absorption capacity of 50 ml / 100 g or more. The oil absorbent has a particle size that is more than half the average film thickness and less than or equal to it. The coating film contains 5% by volume or more of the oil absorbent, Surface-treated steel sheet.

[0090] 4. Examination of drying conditions for paint A chemical conversion coating was formed on the steel plate (GA mentioned above) in the same manner as described above. Then, a coating paint (paint No. 3 or 6 mentioned above) was applied to the chemical conversion coating using a bar coater, and the coating was dried in an oven under conditions that resulted in a maximum temperature of 200°C to form an outer coating. At this time, the effect of drying conditions on the roughness of the coating surface was confirmed by changing the drying conditions of the paint. Specifically, the heating rate during drying was controlled to 5.0°C / s, 10.0°C / s, 25.0°C / s, 50.0°C / s, or 100.0°C / s. Table 5 below shows the type of steel plate, the thickness of the chemical conversion coating, the type of paint, the thickness of the coating, the heating rate during paint drying, and the ratio of the particle size of the oil-absorbing pigment to the thickness of the coating.

[0091] The surface-treated steel sheets obtained as described above were subjected to the same performance evaluation as described above. The results are shown in Table 5 below.

[0092] [Table 5]

[0093] As is clear from the results shown in Table 5, the faster the heating rate during paint drying, the greater the roughness of the coating and the lower the 60° gloss value of the surface-treated steel sheet. As described above, by controlling not only the type of coating but also the drying conditions during coating formation, it is possible to further reduce the 60° gloss of the surface-treated steel sheet and further improve the adhesion of the coating after electrodeposition coating.

Claims

1. A surface-treated steel sheet, A plated steel sheet having a Zn-containing plating layer; A surface treatment layer is provided on at least one main surface of the plated steel sheet, the surface treatment layer has at least a coating film as an outer layer, The coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less, The coating film contains a binder resin, an oil absorbent, and a conductive agent, The binder resin includes an epoxy resin, The ratio of the epoxy resin in the binder resin is 25% by volume or more, The oil absorbing agent has an oil absorption of 50 ml / 100 g or more, The oil absorbing agent has a particle size of half or more and equal to or less than the average film thickness, The coating film contains 5% by volume or more of the oil absorbing agent. Surface treated steel sheet.

2. The surface-treated steel sheet has a 60° gloss of 1% or more and 20% or less. The surface-treated steel sheet according to claim 1.

3. The oil absorbing agent is silica. The surface-treated steel sheet according to claim 1.

4. the conductive agent is a doped oxide particle, a Si alloy containing 50% by mass or more of Si, a Si compound containing 50% by mass or more of Si, or a composite thereof; The coating film contains the conductive agent in an amount of 5% by volume or more and 30% by volume or less. The surface-treated steel sheet according to claim 1.

5. the doped oxide particles are doped zinc oxide particles; The surface-treated steel sheet according to claim 4.

6. The Si alloy or the Si compound is ferrosilicon containing 70 mass% or more of Si. The surface-treated steel sheet according to claim 4.

7. The coating film contains the oil absorbing agent in an amount of 10% by volume or more, The surface-treated steel sheet has a 60° gloss of 1% or more and 15% or less. The surface-treated steel sheet according to any one of claims 1 to 6.

8. the surface treatment layer has an inorganic or organic-inorganic composite coating as an inner layer between the coating film and the plated steel sheet, The coating has an average thickness of 0.1 μm or more and 1.0 μm or less. The surface-treated steel sheet according to any one of claims 1 to 6.

9. A surface-treated steel sheet, A plated steel sheet having a Zn-containing plating layer; A surface treatment layer is provided on at least one main surface of the plated steel sheet, the surface treatment layer has at least a coating film as an outer layer, The coating film has an average film thickness of 1.0 μm or more and 10.0 μm or less, The coating film contains a binder resin, an oil absorbent, and a conductive agent, The binder resin includes an epoxy resin, The ratio of the epoxy resin in the binder resin is 25% by volume or more, The oil absorbing agent has a particle size of half or more and equal to or less than the average film thickness, The coating film contains 5% by volume or more of the oil absorbing agent, The surface-treated steel sheet has a 60° gloss of 1% or more and 20% or less. Surface treated steel sheet.