Electric wire and cable

JPWO2023218506A5Active Publication Date: 2024-10-01SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024520101
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-09
Filing Date
2022-05-09
Publication Date
2024-10-01
Estimated Expiration
2042-05-09

AI Technical Summary

Technical Problem

Conventional electric wires and cables experience increased conduction resistance and power loss due to rising conductor temperatures, which is not effectively managed by their low heat dissipation properties, leading to inefficiencies in information transmission and power supply.

Method used

An electric wire design featuring an insulating layer composed of an olefin resin and a resin incompatible with it, combined with graphite and metal oxide or hydroxide fillers, forming a sea-island structure, which enhances thermal conductivity, mechanical strength, and oil resistance, thereby improving heat dissipation and insulation properties.

Benefits of technology

The solution effectively suppresses conductor temperature rise, reduces power loss, and provides high insulation and mechanical strength, ensuring efficient information transmission and power supply while maintaining high oil resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The electric wire according to the present disclosure comprises a conductor formed from a single wire or a conductor formed from multiple intertwined strands and an insulating layer covering the outer periphery of the conductor, wherein: the insulating layer contains a resin component, a first filler, and a second filler; the resin component contains an olefinic resin and a resin incompatible with the olefinic resin; the olefinic resin and the resin incompatible with the olefinic resin form a sea-island structure; the first filler is formed from graphite; the second filler is formed from a metal oxide, a metal hydroxide, or a combination of these ingredients; the first filler has a mass ratio of 10 / 100 to 80 / 100 with respect to the resin component; and the insulating layer has a thermal conductivity of 0.5 W / m·K or greater at 25˚C and a volume resistivity of 1 x 1013 Ω·cm or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Wires and cables

[0001] FIELD OF THE DISCLOSURE The present disclosure relates to electrical wires and cables.

[0002] In recent years, there has been a demand for ever greater capacity and speed in information transmission for electric wires and cables. Conventional cables generally include a core material (core wire) formed by twisting together a plurality of insulated electric wires (core electric wires), and an outer jacket layer that covers the core material (see Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2018-139177

[0004] The electric wire of the present disclosure includes a conductor formed of a single wire or a conductor formed by twisting a plurality of wires together, and an insulating layer covering the outer periphery of the conductor, wherein the insulating layer contains a resin component, a first filler, and a second filler, the resin component includes an olefin-based resin and a resin incompatible with the olefin-based resin, the olefin-based resin and the resin incompatible with the olefin-based resin forming a sea-island structure, the first filler is made of graphite, and the second filler is made of a metal oxide, a metal hydroxide, or a combination thereof, a mass ratio of the first filler to the resin component is 10 / 100 or more and 80 / 100 or less, and the insulating layer has a thermal conductivity at 25°C of 0.5 W / m K or more and a volume resistivity of 1×10 13 It is Ω·cm or more.

[0005] Fig. 1 is a schematic cross-sectional view showing an electric wire according to one embodiment, Fig. 2 is a schematic cross-sectional view showing a cable according to one embodiment, and Fig. 3 is a schematic cross-sectional view showing a cable according to another embodiment.

[0006] [Problem to be Solved by the Present Disclosure] In recent years, the amount of power consumption has increased along with the increase in the amount of information. As a result, when a current flows through an electric wire or cable that supplies power, the temperature of the conductor rises, the conduction resistance increases, and power loss is likely to occur.

[0007] The present disclosure has been made in light of the above circumstances, and aims to provide an electric wire including an insulating layer that has excellent heat dissipation properties, as well as high insulation properties, mechanical strength, and high oil resistance.

[0008] Effect of the Present Disclosure According to the present disclosure, it is possible to provide an electric wire including an insulating layer that has excellent heat dissipation properties, as well as high insulation properties, mechanical strength, and high oil resistance.

[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described.

[0010] An electric wire according to one aspect of the present disclosure includes a conductor formed of a single wire or a conductor formed by twisting a plurality of wires together, and an insulating layer covering the outer periphery of the conductor, wherein the insulating layer contains a resin component, a first filler, and a second filler, the resin component includes an olefin-based resin and a resin incompatible with the olefin-based resin, the olefin-based resin and the resin incompatible with the olefin-based resin forming a sea-island structure, the first filler is made of graphite, and the second filler is made of a metal oxide, a metal hydroxide, or a combination thereof, a mass ratio of the first filler to the resin component is 10 / 100 or more and 80 / 100 or less, and the insulating layer has a thermal conductivity at 25°C of 0.5 W / m K or more and a volume resistivity of 1×10 13 It is Ω·cm or more.

[0011] The inventors focused on the fact that the coating materials used in conventional electric wires have poor heat dissipation properties, preventing heat from rising in temperature from the conductor. Therefore, they conducted extensive research into improving the thermal conductivity of the coating material to suppress the temperature rise of the conductor, and completed the present invention. The insulating layer of the electric wire contains an olefin-based resin with a high crystalline content as the resin component, thereby achieving excellent tensile strength and oil resistance. The insulating layer also contains a first filler made of graphite and a second filler made of a metal oxide, metal hydroxide, or a combination thereof, with a mass ratio of the first filler to the resin component of 10 / 100 or more and 80 / 100 or less. The insulating layer has a thermal conductivity of 0.5 W / m·K or more at 25°C, providing high thermal conductivity, which allows heat from the conductor to be released to the outside, effectively suppressing the temperature rise of the conductor. Furthermore, the volume resistivity is 1×10 13By having a resistivity of Ω·cm or more, the insulating properties of the insulating layer can be improved. Furthermore, since the resin component contains an olefin-based resin and a resin incompatible with the olefin-based resin, which form a sea-island structure, the first filler, which is difficult to disperse in the olefin-based resin, can be unevenly distributed toward the incompatible resin side, thereby further improving the heat dissipation properties of the insulating layer. Therefore, in this electric wire, the insulating layer has excellent heat dissipation properties, which can suppress temperature rise in the conductor and reduce power loss, and also has high insulation properties, mechanical strength, and high oil resistance.

[0012] The "volume resistivity" refers to the electrical resistance value measured by the double ring electrode method in accordance with JIS-K6271:2008. The "resin incompatible with olefin-based resin" refers to a resin that is incompatible with olefin-based resin, and this can be confirmed, for example, by observing a cross section of the insulating layer perpendicular to the longitudinal direction of the electric wire using a transmission electron microscope (TEM). A resin incompatible with olefin-based resin exhibits a sea-island structure when the cross section is observed using an electron microscope. By achieving such a dispersed state of sea-island structure, the physical behaviors derived from both the olefin-based resin and the resin incompatible with this olefin-based resin appear independently, and the mutual incompatibility allows the properties of both resins to be fully exhibited.

[0013] The mass ratio of the second filler to the resin component is preferably 30 / 100 or more and 200 / 100 or less. In the electric wire, when the mass ratio of the second filler to the resin component is 30 / 100 or more and 200 / 100 or less, both insulation properties and tensile elongation can be favorably achieved.

[0014] The average particle size ratio of the first filler to the second filler is preferably 1.1 or more. By making the average particle size ratio of the first filler to the second filler 1.1 or more, the heat dissipation property of the insulating layer of the electric wire can be further improved.

[0015] The "average particle size" refers to the median diameter (D50), which is the value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2:2001 is 50%. Specifically, the median diameter (D50) can be measured using the following method. Measurement is performed using a laser diffraction particle size distribution analyzer. A scattering measurement mode is employed, and a laser beam is irradiated onto a wet cell in which a dispersion liquid in which particles of the sample to be measured are dispersed in a dispersion solvent is circulated, to obtain a scattered light distribution from the measurement sample. The scattered light distribution is then approximated by a log-normal distribution, and the particle diameter at which the cumulative degree is 50% (D50) is taken as the median diameter.

[0016] It is preferable that the incompatible resin is a styrene copolymer, the olefin resin is polypropylene, and the mass ratio of the styrene copolymer to the polypropylene is 20 / 80 or more and 80 / 20 or less. When the olefin resin is polypropylene, the tensile strength and oil resistance of the insulating layer of the electric wire can be further improved. When the incompatible resin is a styrene copolymer, the tensile elongation of the insulating layer of the electric wire can be improved, and the dispersibility of the first filler can be increased, thereby improving heat dissipation. When the mass ratio of the styrene copolymer to the polypropylene is 20 / 80 or more and 80 / 20 or less, the tensile properties, heat dissipation properties, and oil resistance of the insulating layer of the electric wire can be further improved.

[0017] The polypropylene is preferably a random polypropylene or a block polypropylene, which can further improve the tensile strength and oil resistance of the insulating layer.

[0018] The content of the structural units derived from styrene in the styrene copolymer is preferably 5% by mass or more and 40% by mass or less. On the other hand, when the content of the structural units derived from styrene in the styrene copolymer is 5% by mass or more and 40% by mass or less, the tensile elongation and oil resistance of the insulating layer can be further improved.

[0019] A cable according to another aspect of the present disclosure includes the one or more electric wires and an outer jacket layer disposed around the one or more electric wires. The cable includes the above-described electric wire as a core wire constituting a core wire, and therefore has excellent heat dissipation properties, as well as high insulation properties, mechanical strength, and high oil resistance.

[0020] [Details of Embodiments of the Present Disclosure] Hereinafter, electric wires according to embodiments of the present disclosure will be described in detail with appropriate reference to the drawings.

[0021] <Electric wire> The electric wire includes a conductor made of a single wire or a conductor made of multiple stranded wires, and an insulating layer covering the outer periphery of the conductor. Fig. 1 shows an electric wire according to one embodiment of the present disclosure. The electric wire 1 in Fig. 1 includes a conductor 2 made of a single wire or a linear conductor made of multiple stranded wires, and an insulating layer 3 covering the outer periphery of the conductor 2. In the electric wire, an additional layer such as a primer treatment layer may be provided between the conductor and the insulating layer.

[0022] [Conductor] The conductor 2 is a metal linear body that is responsible for electrical conduction of the electric wire 1. Examples of the conductor 2 include a round wire having a circular cross section, a rectangular wire having a rounded square cross section, and a rectangular wire having a rounded rectangular cross section. The conductor 2 may be a single linear body as shown in Figs. 1 and 2, or may be a twisted wire body formed by twisting together a plurality of thin wires.

[0023] The conductor 2 may be made of a metal such as copper, aluminum, nickel, silver, or iron, or an alloy thereof, but copper or aluminum is preferred from the viewpoints of electrical conductivity and workability. The conductor 2 may also have a multilayer structure in which a coating made of another metal is laminated on the outer surface of a metal linear body.

[0024] The lower limit of the average cross-sectional area (including the gaps between the wires) of the conductor 2 is 2 mm 2 is preferable, and 8 mm 2 is more preferable, and 14 mm 2 On the other hand, the upper limit of the average cross-sectional area of ​​the conductor 2 is 600 mm 2 is preferable, and 500 mm 2 More preferably, 400 mm 2is more preferable. If the average cross-sectional area of ​​the conductor 2 is less than the above lower limit, there is a risk that a sufficient current will not flow. On the other hand, if the average cross-sectional area of ​​the conductor 2 exceeds the above upper limit, there is a risk that sufficient bending resistance will not be obtained. Here, the "average cross-sectional area" refers to the average value of values ​​measured at any 10 cross sections.

[0025] [Insulating Layer] The insulating layer 3 contains a resin component, a first filler, and a second filler.

[0026] The average thickness of the insulating layer 3 is not particularly limited, but the lower limit of the average thickness is preferably 0.8 mm, more preferably 1.0 mm. On the other hand, the upper limit of the average thickness of the insulating layer 4 is preferably 10 mm, more preferably 7 mm. If the average thickness of the insulating layer 4 is less than the above lower limit, the insulating properties of the insulating layer 4 may be insufficient. Furthermore, if the average thickness of the insulating layer 4 exceeds the above upper limit, flexibility may be impaired. Here, "average thickness" refers to the average value of thicknesses measured at any ten points. Note that the same definition is used below when referring to "average thickness" for other members, etc.

[0027] (Resin Component) The resin component contains an olefin resin and a resin incompatible with the olefin resin. The olefin resin and the resin incompatible with the olefin resin form a sea-island structure. The resin component contains an olefin resin and a resin incompatible with the olefin resin, and these form a sea-island structure, which allows the first filler, which is difficult to disperse in the olefin resin, to be unevenly distributed toward the incompatible resin, thereby further improving the heat dissipation properties of the insulating layer 3.

[0028] <Olefin-Based Resin> The insulating layer 3 contains an olefin-based resin as a resin component, which provides excellent tensile strength and oil resistance. Examples of olefin-based resins include polyethylene (PE) and polypropylene (PP).

[0029] Examples of polyethylene include high-density polyethylene (PE), very low-density polyethylene (VLDPE), low-density polyethylene, linear low-density polyethylene (LLDPE), ethylene-α-olefin copolymer, acid-modified polyethylene modified with unsaturated carboxylic acid or a derivative thereof, etc. Examples of ethylene-α-olefin copolymer include ethylene-vinyl acetate copolymer (EVA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate copolymer (EMA), ethylene-butyl acrylate copolymer (EBA), ethylene-methyl methacrylate copolymer, ethylene-acrylic acid copolymer, and ethylene-methacrylic acid copolymer.

[0030] Examples of polypropylene include homopolypropylene, random polypropylene, block polypropylene, and acid-modified polypropylene modified with unsaturated carboxylic acid or a derivative thereof. Examples of random polypropylene include propylene-α-olefin copolymer, which is a copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms. Block polypropylene is a resin composed of homopolypropylene as the main component, a random copolymer elastomer as a copolymer component, and an ethylene polymer as an optional component.

[0031] Examples of unsaturated carboxylic acids used in the acid modification include acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, etc. Examples of derivatives of unsaturated carboxylic acids include maleic acid monoesters, maleic anhydride, itaconic acid monoesters, itaconic anhydride, fumaric acid monoesters, fumaric anhydride, etc. Among these, derivatives of unsaturated carboxylic acids are preferred, and maleic anhydride is more preferred.

[0032] Examples of the propylene-α-olefin copolymer include ethylene-propylene copolymer, propylene-acrylic acid copolymer, propylene-methacrylic acid copolymer, propylene-acrylate ester copolymer, and propylene-methacrylate ester copolymer.

[0033] The olefin-based resin is preferably polypropylene, and more preferably random polypropylene or block polypropylene. When the olefin-based resin is random polypropylene or block polypropylene, it is possible to improve tensile strength and oil resistance while suppressing a significant decrease in tensile elongation.

[0034] <Resin incompatible with olefin-based resin> By including a resin incompatible with the olefin-based resin in the resin component, the first filler, which is difficult to disperse in the olefin-based resin, can be unevenly distributed toward the resin incompatible with the olefin-based resin, thereby further improving the heat dissipation properties of the insulating layer. Examples of resins incompatible with the olefin-based resin include styrene-based copolymers, polyvinyl chloride resins, polyurethanes, fluororesins, fluororubbers, and silicones. Among these, styrene-based copolymers are more preferred because they have good dispersibility of the first filler and can improve the tensile elongation of the insulating layer. The incompatible resin may include one or more types.

[0035] Examples of styrene copolymers include styrene-ethylene block copolymers (SE), styrene / ethylene-butylene / ethylene block copolymers (SEBC) or hydrogenated products thereof, styrene / ethylene-butylene / styrene block copolymers (SEBS) or hydrogenated products thereof, styrene / ethylene-propylene / styrene block copolymers (SEPS), styrene / ethylene-ethylene-propylene-styrene block copolymers (SEEPS), and hydrogenated styrene-butadiene rubber (HSBR).

[0036] The lower limit of the content of the structural units derived from styrene relative to the styrene-based copolymer is preferably 5% by mass, more preferably 8% by mass. The upper limit of the content of the structural units derived from styrene is preferably 40% by mass, more preferably 38% by mass. By setting the content of the structural units derived from styrene within the above range, the tensile elongation and oil resistance of the insulating layer can be further improved.

[0037] When the incompatible resin is a styrene copolymer and the olefin resin is polypropylene, the lower limit of the mass ratio of the styrene copolymer to the polypropylene is preferably 20 / 80, more preferably 30 / 70. The upper limit of the mass ratio of the styrene copolymer to the polypropylene is preferably 80 / 20 or less, more preferably 70 / 30. When the mass ratio of the styrene copolymer to the polypropylene is within the above range, the tensile properties, heat dissipation properties, and oil resistance of the insulating layer of the electric wire can be further improved.

[0038] The insulating layer 3 may contain a resin other than the olefin-based resin and the resin incompatible with the olefin-based resin, such as polyvinyl chloride resin, polyurethane, fluororesin, fluororubber, silicone, or polyester resin.

[0039] (First Filler) The first filler is made of graphite. When the insulating layer contains the first filler made of graphite, the electrical conductivity of the insulating layer can be increased, and the heat dissipation properties can be improved.

[0040] The lower limit of the mass ratio of the first filler to the resin component is 10 / 100, preferably 20 / 100, and more preferably 25 / 100. The upper limit of the mass ratio of the first filler to the resin component is 80 / 100, preferably 75 / 100, and more preferably 70 / 100. When the mass ratio of the first filler to the resin component is within the above range, both heat dissipation and insulation properties in the insulating layer can be achieved satisfactorily.

[0041] The lower limit of the average particle size of the graphite is preferably 0.5 μm, more preferably 1 μm, and more preferably 5 μm. On the other hand, the upper limit of this average particle size is preferably 100 μm, more preferably 50 μm, and more preferably 30 μm. If the average particle size of the graphite is less than 0.5 μm, the thermal conductivity at 25° C. may decrease. On the other hand, if the average particle size of the graphite is more than 100 μm, the tensile elongation may decrease. By having the average particle size of the graphite in the above range, heat dissipation properties can be further improved.

[0042] (Second Filler) The insulating layer 3 contains a second filler made of a metal oxide, a metal hydroxide, or a combination thereof. When the insulating layer 3 contains a second filler made of a metal oxide, a metal hydroxide, or a combination thereof, the heat dissipation property and insulating property of the insulating layer can be improved.

[0043] Examples of the metal oxide include magnesium oxide, zinc oxide, aluminum oxide, titanium oxide, and calcium oxide.

[0044] Examples of the metal hydroxide include magnesium hydroxide, aluminum hydroxide, and calcium hydroxide.

[0045] The lower limit of the mass ratio of the second filler to the resin component is preferably 30 / 100, more preferably 50 / 100. The upper limit of the mass ratio of the second filler to the resin component is preferably 200 / 100, more preferably 180 / 100. In the electric wire, when the mass ratio of the second filler to the resin component is within the above range, both insulation properties and tensile elongation can be achieved satisfactorily.

[0046] The lower limit of the average particle size ratio of the first filler to the second filler is preferably 1.1, more preferably 5. When the average particle size ratio of the first filler to the second filler is 1.1 or more, the heat dissipation properties of the insulating layer of the electric wire can be further improved. The upper limit of the average particle size ratio of the first filler to the second filler is not particularly limited, but may be, for example, 100 or less, from the viewpoint that if the particle size of graphite is too large, the tensile elongation decreases.

[0047] The insulating layer 3 may contain other additives as needed, such as a flame retardant, a flame retardant assistant, an antioxidant, a lubricant, a colorant, a reflectivity imparting agent, a masking agent, a processing stabilizer, and a plasticizer.

[0048] The lower limit of the thermal conductivity of the insulating layer 3 at 25° C. is 0.5 W / m·K, preferably 0.6 W / m·K, and more preferably 0.7 W / m·K. By setting the lower limit of the insulating layer 3 to 0.5 W / m·K, the heat dissipation properties of the insulating layer 3 can be improved.

[0049] The lower limit of the volume resistivity of the insulating layer 3 is 1×10 13 Ω cm, and 1×10 14 Ω cm is preferred, and 1×10 15 It is more preferable that the volume resistivity of the insulating layer 3 is 1×10 13 By making the resistivity Ω·cm or more, the insulating properties and voltage resistance of the insulating layer 3 can be improved.

[0050] [Method for Producing Electric Wire] The method for producing the electric wire is not particularly limited, but may include, for example, the following steps: (1) a step of preparing an insulating layer-forming resin composition (hereinafter also referred to as a resin composition) for forming an insulating layer (resin composition preparation step); and (2) a step of coating a conductor with the insulating layer-forming resin composition (resin composition coating step).

[0051] (1) Resin Composition Preparation Step In the resin composition preparation step, the resin components of the resin composition for forming an insulating layer, the first filler, the second filler, and other additives as necessary are mixed using a melt mixer or the like to prepare a resin composition for forming an insulating layer. As the melt mixer, a known mixer such as an open roll, a Banbury mixer, a pressure kneader, a single-screw mixer, or a multi-screw mixer can be used. The resin composition of the present disclosure may be crosslinked by chemical crosslinking, silane crosslinking, or radiation crosslinking.

[0052] (2) Resin Composition Coating Step The resin composition coating step can be carried out by, for example, extruding the resin composition for forming an insulating layer onto a conductor using a melt extruder. This produces an extrusion-molded product corresponding to the insulating layer. The dimensions of the extrusion-molded product can be designed depending on the application, etc.

[0053] <Cable> A cable according to another aspect of the present disclosure includes one or more of the electric wires and an outer jacket layer disposed around the one or more electric wires.

[0054] The outer diameter of the cable is appropriately designed depending on the application, but the lower limit of the outer diameter is preferably 10 mm, more preferably 15 mm, while the upper limit of the outer diameter of the cable is preferably 80 mm, more preferably 60 mm, and even more preferably 50 mm.

[0055] [First embodiment] A cable according to a first embodiment of the present disclosure is shown in Fig. 2. A coaxial cable 5 according to the first embodiment includes an electric wire 1 including a conductor 2 and an insulating layer 3 covering the outer periphery of the conductor 2, and an outer jacket layer 4 disposed around the electric wire 1. That is, the coaxial cable 5 has a cross-sectional configuration in which the conductor 2, the insulating layer 3, and the outer jacket layer 4 are concentrically stacked. The cable being a coaxial cable 5 enables a reduction in diameter. The electric wire 1, the conductor 2, and the insulating layer 3 are the same as those of the electric wire 1 in Fig. 1, and therefore the same reference numerals are used and description thereof will be omitted.

[0056] The main component of the outer layer 4 is not particularly limited as long as it is a synthetic resin with excellent abrasion resistance, and examples thereof include polyvinyl chloride, polyethylene, cross-linked polyethylene, chloroprene, etc. The outer layer 4 may also be cross-linked.

[0057] The outer covering layer 4 may contain the additives exemplified for the insulating layer 3 .

[0058] The average thickness of the outer covering layer 4 is preferably 0.5 mm or more and 3.0 mm or less.

[0059] Second Embodiment A cable according to a second embodiment of the present disclosure is shown in Fig. 3. The cable 20 according to the second embodiment is a cable including a core wire formed by twisting together two of the electric wires 1 shown in Fig. 1, an inner coating layer 7 (intervening) disposed around the core wire, and an outer coating layer 10 disposed around the inner coating layer 7. The core wire is formed by twisting two electric wires 1 of the same diameter together. As shown in Fig. 3, the cable 20 may have a tape member 8 such as paper wound between the outer coating layer 10 and the inner coating layer 7 as a restraining member. The cable 20 can be suitably used, for example, as a power supply cable in the field of information and communications.

[0060] The main component of the inner coating layer 7 is, for example, PP yarn, paper, jute, or the like.

[0061] The lower limit of the outer diameter of the inner coating layer 7 is preferably 9.0 mm, more preferably 10 mm, while the upper limit of the outer diameter of the inner coating layer 7 is preferably 75 mm, more preferably 60 mm.

[0062] The outer layer 10 has the same configuration as the outer layer 4 in FIG. 2, and therefore a description thereof will be omitted.

[0063] <Cable Manufacturing Method> The cable can be obtained by a manufacturing method including a step of covering one or more electric wires with an outer covering layer (outer covering layer covering step). When the cable includes multiple electric wires, the manufacturing method may include a step of twisting the multiple electric wires. Furthermore, when the cable includes an inner covering layer or a tape member around one or more electric wires, the manufacturing method may include a step of forming an inner covering layer or a step of winding a tape member.

[0064] In the outer covering layer covering step, a resin composition for forming an outer covering layer is extruded onto the outside of one or more electric wires formed using, for example, a melt extrusion molding machine, thereby coating the outside of one or more electric wires with an outer covering layer.

[0065] After coating with the jacket layer, the wire or wires are cooled to harden the jacket layer, and the cable is obtained. The cable is then wound and collected.

[0066] The method for producing the cable may further include a step of crosslinking the resin component of the jacket layer (crosslinking step). This crosslinking step may be performed before or after coating the exterior of one or more electric wires with the composition that forms the jacket layer (after the jacket layer is formed).

[0067] The cable includes the above-described electric wire as a core electric wire constituting the core wire, and therefore has excellent heat dissipation properties, as well as high insulation properties, mechanical strength, and high oil resistance.

[0068] [Other Embodiments] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is not limited to the configurations of the above-described embodiments, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0070] <Insulating Layers No. 1 to No. 31> Insulating layers No. 1 to No. 31, each consisting of a single layer, were formed by the following procedure.

[0071] [Resin Component] 1. Olefin-Based Resin The following polypropylenes were used as the olefin-based resin in the resin component. (1) Random Polypropylene (Random PP) MFR 1.3 (g / 10 min), Flexural Modulus 950 MPa (2) Block Polypropylene (Block PP) MFR: 2.0 (g / 10 min), Flexural Modulus 790 MPa The melt flow rate (MFR) is a value measured using a melt indexer at a measurement temperature of 230°C and a load of 2.16 kg according to a method in accordance with JIS-K7210-1:2014 (Method A: Mass Measurement Method). The flexural modulus is a value measured according to a method in accordance with JIS-K7171:2016. 2. Styrene-Based Copolymer The following styrene-based copolymer was used as a resin incompatible with the olefin-based resin in the resin component. (1) Styrene / ethylene-butylene / styrene block copolymer (SEBS) (styrene structural unit content: 12% by mass) Shore A hardness: 42 (2) SEBS (styrene structural unit content: 18% by mass) Shore A hardness: 67 (3) SEBS (styrene structural unit content: 35% by mass) Shore A hardness: 49 (4) SEBS (styrene structural unit content: 43% by mass) Shore A hardness: 96 (5) Hydrogenated styrene butadiene rubber (HSBR) (styrene structural unit content: 10% by mass) Shore A hardness: 42 Note that "Shore A hardness" refers to the hardness measured using a Type A durometer based on JIS-K6253:2012. "Styrene structural unit content" refers to the content of structural units derived from styrene relative to the styrene-based copolymer.

[0072] [First Filler] The following three types of graphite were used as the first filler: (1) Thin graphite (average particle size: 22 μm) (2) Spherical graphite (average particle size: 20 μm) (3) Thin graphite (average particle size: 5 μm)

[0073] [Second Filler] The following five types of fillers were used as the second filler: (1) Magnesium hydroxide (average particle size: 0.8 μm) (2) Aluminum hydroxide (average particle size: 1.5 μm) (3) Aluminum hydroxide (average particle size: 10.0 μm) (4) Zinc oxide type 1 (average particle size: 0.75 μm) (5) Magnesium oxide (average particle size: 4.5 μm)

[0074] A resin composition for forming an insulating layer was prepared using the above resin component, first filler, and second filler. The composition and content of the insulating layer are shown in Tables 1 to 3. "-" indicates that the corresponding component was not used.

[0075] [Production of insulating layer] The insulating layer was produced by extrusion molding using the resin composition for forming the insulating layer. An extrusion die was used for extrusion molding. The extrusion molding was carried out at a die temperature of 180°C and a linear speed of 5 m / min to obtain insulating layers No. 1 to No. 31 with an average thickness of 2.5 mm. The insulating layers were used to produce insulating layers with a cross-sectional area of ​​14 mm. 2 An electric wire was prepared by covering the outer periphery of a (14SQ) conductor.

[0076] [Evaluation] Insulating layers No. 1 to No. 31 were evaluated for thermal conductivity, volume resistivity, tensile strength, tensile elongation, tensile strength and tensile elongation after an oil resistance test, conductor temperature during current application, withstand voltage, and the presence or absence of a sea-island structure in the cross section of the insulating layer.

[0077] (Thermal Conductivity) A press sheet measuring φ150 mm x thickness 0.5 mm was prepared as a test sample from the resin composition for forming an insulating layer using a heat press machine, and the thermal conductivity at 25°C was measured in accordance with ISO-22007-3 (temperature wave method). A higher value of the thermal conductivity [W / (m K)] indicates higher heat dissipation properties of the insulating layer. A thermal conductivity of 0.50 [W / (m K)] or higher at 25°C can be said to have excellent heat dissipation properties.

[0078] (Volume Resistivity (Insulating Property)) A press sheet measuring φ150 mm x 1 mm thick was prepared as a test sample from the resin composition for forming an insulating layer using a heat press machine, and electrical resistance was measured using the double ring electrode method specified in JIS-K6271:2008. The volume resistivity value was calculated from the measured value. A larger value of volume resistivity [Ω cm] means higher insulating property of the insulating layer. The volume resistivity is calculated as 1×10 13 In the above cases, it can be said that the insulating layer has excellent insulating properties.

[0079] (Tensile Strength and Tensile Elongation) The tensile strength [MPa] and tensile elongation [%] of each insulating layer were measured in accordance with JIS-K-7162: 1994. When the tensile strength is 10 MPa or more and the tensile elongation is 200% or more, it can be said that the mechanical strength of the insulating layer is excellent.

[0080] (Tensile strength and tensile elongation after oil resistance test) After immersion for 4 hours at 70°C using JIS No. 2 test oil according to JIS-C3005:2014, the tensile strength [MPa] and tensile elongation [%] were measured to evaluate the oil resistance. The tensile elongation [%] of the insulating layer was measured in accordance with JIS-K-7162:1994. The higher the tensile strength retention and tensile elongation retention after the oil resistance test, the better the oil resistance. When the tensile strength retention is 80% or more and the elongation retention is 60% or more, it can be said that the oil resistance of the insulating layer is excellent.

[0081] (Conductor Temperature During Current Flow) To measure the conductor temperature during current flow, a current of 140 A was passed through each of electric wires having an outer diameter of 9.4 mm and a length of 3 m, each of which had an insulating layer No. 1 to No. 31 with an average thickness of 2.5 mm coated on the outer periphery of a 14SQ conductor with a conductor diameter of 4.4 mm, and the temperature of the conductor surface at the center of the electric wire was measured.

[0082] (Voltage resistance) In accordance with JIS-C3605:2002, 2000 V was applied to each of the wires coated with the insulating layer No. 1 to No. 31, and the presence or absence of dielectric breakdown was evaluated. The evaluation was based on the following two levels. A rating of A indicates good effectiveness. A: No dielectric breakdown occurred. B: Dielectric breakdown occurred.

[0083] (Presence or absence of sea-island structure in insulating layer) The presence or absence of sea-island structure in the cross section of the insulating layer was determined by preparing thin film sections from the insulating layer taken from each electric wire using a freezing microtome method, staining the samples with ruthenium tetroxide, osmium tetroxide, tungsten phosphate, or the like, and observing the stained samples with a transmission electron microscope to visually judge.

[0084] The evaluation results of each of the insulating layers are shown in Tables 1 to 3.

[0085]

[0086]

[0087]

[0088] From the results in Tables 1 to 3, it can be seen that the insulating layer contains an olefin resin and a resin incompatible with the olefin resin as resin components, the olefin resin and the incompatible resin forming a sea-island structure, the insulating layer contains graphite as a first filler and a metal oxide or metal hydroxide as a second filler, the mass ratio of the first filler to the resin components is 10 / 100 or more and 80 / 100 or less, the insulating layer has a thermal conductivity of 0.5 W / m K or more at 25°C, and a volume resistivity of 1×10 13 The insulating layers of Tests No. 1 to No. 22, which had a resistivity of Ω·cm or more, obtained good results in all of heat dissipation, insulation, mechanical strength, and oil resistance.

[0089] On the other hand, the insulating layer of No. 24, which did not contain an olefin-based resin, showed a decrease in tensile elongation. The insulating layer of No. 23, which did not contain a resin incompatible with the olefin-based resin, showed a decrease in tensile strength and tensile strength retention rate after the oil resistance test. 13 The insulation layer of No. 25, which had a volume resistivity of less than 1×10 Ω cm, experienced dielectric breakdown in the withstand voltage test. 13The insulating layer No. 26, which had a resistivity of less than Ω·cm, experienced dielectric breakdown in the withstand voltage test. The insulating layers No. 27, No. 30, and No. 31, which had a mass ratio of the first filler to the resin component of less than 10 / 100 and a thermal conductivity at 25°C of less than 0.5 W / m·K, experienced a high conductor temperature when current was applied. The insulating layer No. 28, which had a thermal conductivity at 25°C of less than 0.5 W / m·K, experienced a high conductor temperature when current was applied. The insulating layer No. 29, which did not contain a second filler, experienced dielectric breakdown in the withstand voltage test.

[0090] The above results demonstrate that the electric wire has excellent heat dissipation properties, as well as high insulation properties, mechanical strength, and high oil resistance.

[0091] REFERENCE SIGNS LIST 1 Electric wire 2 Conductor 3 Insulating layer 4, 10 Outer covering layer 5, 20 Cable 7 Inner covering layer 8 Tape member

Claims

1. A conductor made of a single wire or a conductor made of a plurality of stranded wires; an insulating layer covering the outer periphery of the conductor; Equipped with the insulating layer contains a resin component, a first filler and a second filler, the resin component includes an olefin-based resin and a resin incompatible with the olefin-based resin, the olefin-based resin and a resin incompatible with the olefin-based resin form a sea-island structure, The first filler is made of graphite, The second filler is made of a metal oxide, a metal hydroxide, or a combination thereof; a mass ratio of the first filler to the resin component is 10 / 100 or more and 80 / 100 or less; The insulating layer has a thermal conductivity of 0.5 W / m K or more at 25° C. and a volume resistivity of 1×10 13 An electric wire having a resistance of Ω·cm or more.

2. The electric wire according to claim 1 , wherein a mass ratio of the second filler to the resin component is equal to or greater than 30 / 100 and equal to or less than 200 / 100.

3. 2. The electric wire according to claim 1, wherein an average particle size ratio of the first filler to the second filler is 1.1 or more.

4. the incompatible resin is a styrene-based copolymer, The olefin resin is polypropylene, 2. The electric wire according to claim 1, wherein a mass ratio of the styrene-based copolymer to the polypropylene is 20 / 80 or more and 80 / 20 or less.

5. The electric wire according to claim 4, wherein the polypropylene is a random polypropylene or a block polypropylene.

6. The electric wire according to claim 4, wherein the content of the structural unit derived from styrene in the styrene-based copolymer is 5% by mass or more and 40% by mass or less.

7. One or more electric wires according to any one of claims 1 to 6; a jacket layer disposed around the one or more electric wires; A cable that is provided with: