LAMINATE, MANUFACTURING METHOD FOR LAMINATE, AND BATTERY CASE
Patent Information
- Application Number
- JP2024538959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-15
- Filing Date
- 2023-06-15
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-06-15
AI Technical Summary
【0015】 本発明によれば、軽量かつ薄肉でありながら耐燃性や強度に優れる特徴を有し、バッテリーケース等の成形品用途に好適に用いることができる積層体、及びこれを用いたバッテリーケースを提供することができる。
Description
[Technical Field]
[0001] The present invention relates to a laminate that is lightweight and thin, yet has excellent flame resistance and strength, and can be suitably used for a variety of molded product applications, and to a battery case using the same. [Background technology]
[0002] Because the lithium-ion batteries used in many electric vehicles have the risk of catching fire, their battery cases must be strong as well as highly flame-resistant and fire-resistant. At the same time, to realize vehicles with better fuel economy and a lower environmental impact, molding materials that can further reduce the weight and space of the battery case itself while fully maintaining the aforementioned performance are needed.
[0003] As a lightweight and high-strength molding material, a so-called FRP sandwich molded body is known, in which a resin foam is used as a core material and is sandwiched between fiber-reinforced plastics (see, for example, Patent Document 1). However, the resin foam used as the core material in such a sandwich molded body is generally flammable, and in order to impart a certain degree of flame resistance, a resin foam with a sufficient thickness must be used, which makes it unsuitable for applications such as battery cases, which require high flame resistance and fire resistance, as well as light weight and space saving. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 2022-80629 Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, the problem to be solved by the present invention is to provide a molding material that is lightweight and thin-walled yet has excellent flame resistance and strength, and that can be suitably used for molded products such as battery cases, and to provide a battery case using the same. [Means for solving the problem]
[0006] As a result of extensive research, the present inventors have found that a laminate comprising a core layer (A) formed by compressing a foam in the thickness direction and an outer layer (B) made of fiber-reinforced plastic is lightweight and thin, yet has excellent flame resistance and strength, and can be used for a variety of molded products, including battery cases, and have completed the present invention.
[0007] That is, the present invention relates to (I) a laminate comprising a core layer (A) formed by compressing a foam in the thickness direction and an outer layer (B) made of a fiber-reinforced plastic.
[0008] The present invention further relates to (II) the laminate according to (I) above, wherein the compressibility of the core layer (A) is 40% or more in terms of thickness.
[0009] The present invention further relates to (III) the laminate according to (I) or (II) above, wherein the aspect ratio of the foam cells of the core layer (A) is 2 or more.
[0010] The present invention further relates to (IV) the laminate according to any one of (I) to (III), wherein the outer layer (B) is obtained by hot molding a prepreg containing reinforcing fibers (f) and a matrix resin (r), and the matrix resin is a resin composition (1) containing a polyisocyanate compound (r1) and a polyhydroxy(meth)acrylate compound (r2), or a resin composition (2) containing a polyisocyanate compound (r1), a monohydroxy(meth)acrylate compound (r3), and a polyhydroxy compound (r4).
[0011] The present invention further relates to (V) a method for producing the laminate described in any one of (I) to (IV) above, which comprises heat-molding a precursor obtained by laminating a core layer (a) made of a foam and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r) under conditions in which the core layer (a) is compressed.
[0012] The present invention further relates to (VI) a method for producing the laminate described in any one of (I) to (IV), in which the core layer (A) and the outer layer (B) made of fiber-reinforced plastic are bonded together using an adhesive.
[0013] The present invention further relates to (VII) a method for producing the laminate according to any one of (I) to (IV), which comprises hot molding a precursor obtained by laminating the core layer (A) and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r).
[0014] The present invention further relates to (VIII) a battery case using the laminate according to any one of (I) to (IV) above. [Effects of the Invention]
[0015] According to the present invention, it is possible to provide a laminate that is lightweight and thin yet has excellent flame resistance and strength, and that can be suitably used for molded products such as battery cases, and a battery case using the laminate. DETAILED DESCRIPTION OF THE INVENTION
[0016] The present invention will be described in detail below.
[0017] The laminate of the present invention is characterized by comprising a core layer (A) formed by compressing a foam in the thickness direction, and an outer layer (B) made of a fiber-reinforced plastic.
[0018] The foam may be made of any of a variety of resin materials without particular limitations. Examples of the resin material include polyurethane resin, phenolic resin, melamine resin, acrylic resin, polyethylene resin, polypropylene resin, polyvinyl chloride resin, polystyrene resin, styrene-acrylic resin, ABS resin, polyphenylene ether resin, polyetherimide resin, polymethyl methacrylate resin, and polymethacrylimide resin. The foaming method and foaming agent used for these resin materials are not particularly limited, and foams made using known, commonly used foaming agents and foaming methods can be used. Among these, bead foams are preferred, and bead foams made of polystyrene resin are more preferred, as they provide a laminate with superior flame resistance.
[0019] The bead foam can be produced, for example, by a method in which a foaming gas is injected into particles made of the various resin materials and heated to pre-expand to obtain expandable beads, and the obtained expandable beads are then foam-molded under heat and pressure. The average particle size of the expandable beads is preferably in the range of 0.5 to 5 mm, since the resulting laminate will have better flame resistance and strength. Examples of the foaming gas include propane, butane, and pentane, and the amount of gas injected is preferably 5 to 7 mass % of the foamed beads. The expansion ratio is preferably 40 to 70 times, since the resulting laminate will have better flame resistance and strength. The density of the foam is preferably 0.01 to 0.07 g / cm, since the laminate will have an excellent balance of light weight, flame resistance, and strength. 3 It is preferable that the range is:
[0020] In the bead foam, a functional coating agent can be applied to the surface of the expandable beads, which are the raw material, to impart desired performance to the resulting foam. Examples of functional coating agents include flame-retardant coating agents and heat-resistant coating agents. Among these, resin bead foams coated with a flame-retardant coating agent on the surface are preferred, as this will result in the resulting laminate having superior flame resistance. Examples of the flame-retardant coating agent include flame retardants such as phosphorus-containing compounds, halogen-containing compounds, nitrogen-containing compounds, hydrated metal compounds, borates, metal oxides, and silicone compounds.
[0021] The core layer (A) of the present invention is obtained by compressing the foam in the thickness direction. The compression ratio of the core layer (A) is preferably 40% or more, more preferably 60% or more, and particularly preferably 85% or more, in terms of thickness, so that the resulting laminate has sufficient flame resistance despite its thin wall. It is also preferably 97% or less, and more preferably 95% or less. The aspect ratio of the foam cells of the core layer (A) is preferably 1.7 or more, more preferably 2.5 or more, and particularly preferably 6.7 or more, so that the resulting laminate has sufficient flame resistance despite its thin wall. It is also preferably 30 or less, and more preferably 20 or less. The aspect ratio of the foam cells may be either an actual value measured by observing the cross section of the foam under a microscope, or a calculated value calculated from the compression ratio. Aspect ratio = 1 / [1-compression ratio (%) / 100]
[0022] The thickness of the core layer (A) is preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, because the resulting laminate has an excellent balance of flame resistance, strength, and light weight. The core layer (A) may be formed of only one layer, or may be formed of multiple layers. When the core layer (A) is multilayered, each layer may be formed of the same type of foam, or each layer may be formed of a different type of foam. Even when the core layer (A) is multilayered, the total thickness of the core layer (A) is preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm.
[0023] Specifically, the outer layer (B) made of fiber reinforced plastic is obtained by hot molding a prepreg containing reinforcing fibers (f) and a matrix resin (r).
[0024] Examples of the reinforcing fibers (f) include carbon fibers, glass fibers, silicon carbide fibers, alumina fibers, boron fibers, metal fibers, and organic fibers such as aramid fibers, vinylon fibers, and tetron fibers. These may be used alone or in combination of two or more. Among these, carbon fibers and glass fibers are preferred because they can provide a laminate with higher strength.
[0025] As the carbon fiber, various types such as polyacrylonitrile-based, pitch-based, and rayon-based fibers can be used, but among these, polyacrylonitrile-based fibers are preferred because they can provide carbon fibers with higher strength.
[0026] The shape of the reinforcing fibers (f) is not particularly limited, and examples thereof include reinforcing fiber tows in which reinforcing fiber filaments are bundled, unidirectional materials in which reinforcing fiber tows are aligned in one direction, woven fabrics, short-cut reinforcing fibers, and nonwoven fabrics or papers made of short-cut reinforcing fibers. When the reinforcing fibers (f) are woven fabrics, examples include sheets in which fiber bundles are aligned in one direction, such as plain weave, twill weave, satin weave, or non-crimped fabrics, or stitched sheets in which sheets stacked at different angles are stitched to prevent unraveling. When short-cut reinforcing fibers (f) are used, it is preferable to use fibers cut to a length of 2.5 to 50 mm, as this improves flowability in the mold during molding and the appearance of the molded product. Among these, it is preferable to use unidirectional materials or woven fabrics as reinforcing fibers, as these result in a stronger outer layer (B). When using a prepreg using unidirectional materials as reinforcing fibers, a stronger outer layer (B) can be obtained by stacking multiple sheets in order to form a quasi-isotropic structure, for example, with the fiber directions alternating between 0° and 90°.
[0027] For the same reasons as above, the length of the short cut reinforcing fibers is more preferably 8 to 50 mm, and particularly preferably 10 to 30 mm.
[0028] Weight of reinforced fiber (f) (fiber 1m 2 There are no particular restrictions on the weight per unit area, and a wide variety of weights can be used. The optimum value also differs depending on the reinforcing fiber (f). In general, a weight of 30 to 650 g / m is used because it provides an excellent balance between the uniformity of the fiber width of the reinforcing fiber (f) and the impregnation of the matrix resin (r). 2 When the reinforcing fiber (f) is a glass fiber, the thickness is preferably in the range of 50 g / m 2 It is preferable that the content is 100 g / m or more. 2 More preferably, it is 600 g / m or more. 2 Preferably, it is 350 g / m or less. 2 When the reinforcing fiber (f) is a carbon fiber, it is more preferable that the reinforcing fiber (f) is 50 g / m or less. 2 It is preferable that the weight is 80 g / m or more.2 More preferably, it is 300 g / m or more. 2 Preferably, it is 200 g / m or less. 2 More preferably, it is:
[0029] The basis weight of the short cut reinforcing fibers is set to 250 to 1500 g / m from the viewpoint of achieving both favorable impregnation property and high strength. 2 is preferable, and 300 to 1400 g / m 2 More preferably, 400 to 1300 g / m 2 is particularly preferred.
[0030] The content of the reinforcing fibers (f) in the prepreg is preferably 40% by mass or more, more preferably 50% by mass or more, since this results in a stronger outer layer (B), and is preferably 90% by mass or less, more preferably 80% by mass or less.
[0031] The matrix resin (r) can be impregnated into the reinforcing fibers (f) and can be molded by heating or other means, and a wide variety of resins can be used without particular limitation. Among these, a thermosetting resin composition is preferred for ease of handling. Furthermore, since the resulting outer layer (B) is a prepreg that is high in strength, easy to handle, and easily moldable into various shapes, it is preferred that the resin composition contain a urethane reaction component formed by an isocyanate group and a hydroxyl group, and that a polymerizable unsaturated group is present in the resin composition. Examples of such resin compositions include a resin composition (1) containing a polyisocyanate compound (r1) and a polyhydroxy(meth)acrylate compound (r2), and a resin composition (2) containing a polyisocyanate compound (r1), a monohydroxy(meth)acrylate compound (r3), and a polyhydroxy compound (r4).
[0032] In the present invention, the (meth)acrylate compound refers to a compound having either or both of an acryloyl group and a methacryloyl group, the (meth)acryloyl group refers to either or both of an acryloyl group and a methacryloyl group, and the (meth)acrylic acid refers to either or both of acrylic acid and methacrylic acid.
[0033] Examples of the polyisocyanate compound (r1) include aliphatic diisocyanate compounds such as butane diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and dimer acid diisocyanate; alicyclic diisocyanate compounds such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate; tolylene diisocyanate, Examples of suitable isocyanate compounds include aromatic diisocyanate compounds such as xylylene diisocyanate, tetramethylxylylene diisocyanate, lysine diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate; and modified isocyanurate compounds, biuret modified compounds, allophanate modified compounds, carbodiimide modified compounds, urethane imine modified compounds, and polyol modified compounds with polyols such as diethylene glycol and dipropylene glycol. These compounds may be used alone or in combination. Among these, aromatic diisocyanate compounds and their various modified compounds are preferred because they provide an outer layer (B) with excellent heat resistance. When multiple types of polyisocyanate compounds (r1) are used in combination, the proportion of aromatic diisocyanate compounds and their various modified products relative to the total mass of polyisocyanate compounds (r) is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0034] The polyhydroxy(meth)acrylate compound (r2) may be, for example, a (meth)acrylate compound obtained by reacting an epoxy resin with (meth)acrylic acid.
[0035] Examples of the epoxy resin include diglycidyloxybenzene, diglycidyloxynaphthalene, aliphatic epoxy resins, biphenol-type epoxy resins, bisphenol-type epoxy resins, novolac-type epoxy resins, alicyclic epoxy resins, glycidylamine-type epoxy resins, heterocyclic epoxy resins, glycidyl ester-type epoxy resins, triphenolmethane-type epoxy resins, phenol or naphthol aralkyl-type epoxy resins, phenylene or naphthylene ether-type epoxy resins, oxodoridone-modified epoxy resins, and brominated epoxy resins thereof. The epoxy resin may be an epoxy resin obtained by elongating the above-mentioned specific examples with an elongator.
[0036] Examples of the aliphatic epoxy resin include polyglycidyl ethers of various aliphatic polyol compounds and one or more of their alkylene oxide adducts with epihalohydrin. Examples of the aliphatic polyol compounds include ethylene glycol, propylene glycol, 1,3-propanediol, 2-methylpropanediol, 1,2,2-trimethyl-1,3-propanediol, 2,2-dimethyl-3-isopropyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 3-methyl-1,3-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1, Examples include aliphatic diol compounds such as 6-hexanediol, 1,4-bis(hydroxymethyl)cyclohexane, and 2,2,4-trimethyl-1,3-pentanediol; alicyclic diol compounds such as 2,2-bis(4-hydroxyphenyl)propane; and tri- or higher functional aliphatic polyol compounds such as trimethylolethane, trimethylolpropane, glycerin, hexanetriol, pentaerythritol, ditrimethylolpropane, and dipentaerythritol.
[0037] Examples of the biphenol-type epoxy resin include biphenol compounds such as biphenol and tetramethylbiphenol, and polyglycidyl ethers of one or more of these alkylene oxide adducts with epihalohydrin.
[0038] Examples of the bisphenol type epoxy resin include bisphenol compounds such as bisphenol A, tetrabromobisphenol A, bisphenol F, bisphenol S, bisphenol fluorene, and biscresol fluorene, and polyglycidyl ethers of one or more of these alkylene oxide adducts with epihalohydrin.
[0039] Examples of the novolac epoxy resin include polyglycidyl etherified novolac resins made of one or more phenolic compounds such as phenol, dihydroxybenzene, cresol, xylenol, naphthol, dihydroxynaphthalene, bisphenol, and biphenol with epihalohydrin.
[0040] Examples of the alicyclic epoxy resin include those obtained by hydrogenating the biphenol compounds or bisphenol compounds, and those obtained by polyglycidyl etherifying one or more of their alkylene oxide adducts with epihalohydrin, as well as 3,4-epoxy-6-methylcyclohexylmethyl-3,4-epoxy-6-methylcyclohexanecarboxylate and 1-epoxyethyl-3,4-epoxycyclohexane.
[0041] Examples of the glycidylamine type epoxy resin include N,N-diglycidylaniline, triglycidylaminophenol, tetraglycidylxylenediamine, and 4,4'-methylenebis[N,N-diglycidylaniline].
[0042] Examples of the heterocyclic epoxy resin include 1,3-diglycidyl-5,5-dimethylhydantoin and triglycidyl isocyanurate.
[0043] Examples of the glycidyl ester type epoxy resin include phthalic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, diglycidyl-p-oxybenzoic acid, and dimer acid glycidyl ester.
[0044] Examples of extenders for epoxy resins include the above-mentioned various biphenol compounds and hydrogenated products thereof, the above-mentioned various bisphenol compounds and hydrogenated products thereof, dibasic acid compounds, and acid group-containing polyester resins.
[0045] Among these, the bisphenol-type epoxy resin is preferred because it is excellent in impregnation into the reinforcing fibers (f) and in the strength of the resulting outer layer (B). In this case, the epoxy equivalent of the epoxy resin is preferably in the range of 150 to 600 g / equivalent, and more preferably in the range of 200 to 450 g / equivalent.
[0046] The reaction between the epoxy resin and (meth)acrylic acid can be carried out by heating at a temperature of about 60 to 140°C in the presence of an esterification catalyst. If necessary, a reaction solvent or a polymerization inhibitor may be added. The reaction ratio between the epoxy resin and (meth)acrylic acid is preferably such that the molar ratio of the functional groups of both [carboxy group / epoxy group] is in the range of 0.6 to 1.1.
[0047] When the bisphenol-type epoxy resin is used as the epoxy resin, the resulting (meth)acrylate compound preferably has a hydroxyl value of 50 to 200 mg / KOH, and a (meth)acryloyl group equivalent of 300 to 600 g / equivalent.
[0048] The polyhydroxy(meth)acrylate compound (r2) may be used singly or in combination of two or more. When two or more polyhydroxy(meth)acrylate compounds (r2) are used in combination, the proportion of the bisphenol type epoxy resin (meth)acrylate compound relative to the total mass of the polyhydroxy(meth)acrylate compound (r2) is preferably 50 mass% or more, more preferably 70 mass% or more, and particularly preferably 80 mass% or more.
[0049] Examples of the monohydroxy(meth)acrylate compound (r3) include hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxybutyl(meth)acrylate, trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, (poly)oxyalkylene(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of these compounds, and lactone-modified (meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of these compounds. These compounds may be used alone or in combination of two or more.
[0050] Among these, monohydroxymono(meth)acrylate compounds are preferred, and hydroxyethyl(meth)acrylate is more preferred, because they provide an excellent balance between the ability to impregnate the reinforcing fibers (f) and the strength of the resulting outer layer (B). When a plurality of monohydroxy(meth)acrylate compounds (r3) are used in combination, the proportion of hydroxyethyl(meth)acrylate to the total mass of the monohydroxy(meth)acrylate compounds (r3) is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0051] Examples of the polyhydroxy compound (r4) include dihydroxybenzene, dihydroxynaphthalene, the various aliphatic polyols mentioned above, biphenol compounds, bisphenol compounds, alkylene oxide adducts thereof, and lactone-modified compounds. These may be used alone or in combination. Among them, alkylene oxide adducts of bisphenol compounds are preferred because they provide an excellent balance between the impregnation of the reinforcing fibers (f) and the strength of the resulting outer layer (B). The average number of moles of alkylene oxide added is preferably in the range of 2 to 10 moles.
[0052] When multiple types of polyhydroxy compounds (r4) are used in combination, the proportion of alkylene oxide adducts of bisphenol compounds relative to the total mass of polyhydroxy compounds (r4) is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0053] In the resin composition (1), the molar ratio (NCO / OH) of the isocyanate groups contained in the polyisocyanate compound (r1) to the hydroxyl groups contained in the polyhydroxy(meth)acrylate compound (r2) is preferably in the range of 0.3 to 1.2, more preferably in the range of 0.4 to 1.1, and particularly preferably in the range of 0.5 to 1.0, in order to obtain a prepreg with excellent ease of handling and moldability.
[0054] In the resin composition (2), the molar ratio (NCO / OH) of the isocyanate groups contained in the polyisocyanate compound (r1) to the sum of the hydroxyl groups contained in the monohydroxy(meth)acrylate compound (r3) and the polyhydroxy compound (r4) is preferably in the range of 0.7 to 1.3, more preferably in the range of 0.8 to 1.1, and particularly preferably in the range of 0.8 to 1.0, in order to provide excellent ease of handling and moldability of the prepreg. Furthermore, the molar ratio (r3 / r4) of the monohydroxy(meth)acrylate compound (r3) to the polyhydroxy compound (r4) is preferably in the range of 40 / 60 to 80 / 20, more preferably in the range of 50 / 50 to 70 / 30, in order to provide further improved heat resistance and curability.
[0055] The resin compositions (1) and (2) may contain a polymerizable unsaturated group-containing compound other than the polyhydroxy(meth)acrylate compound (r2) and the monohydroxy(meth)acrylate compound (r3). Specific examples thereof include aliphatic mono(meth)acrylate compounds such as methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, isodecyl(meth)acrylate, lauryl(meth)acrylate, isotridecyl(meth)acrylate, n-stearyl(meth)acrylate, ethylene glycol(meth)acrylate alkyl ether, and propylene glycol(meth)acrylate alkyl ether; alicyclic mono(meth)acrylate compounds such as cyclohexyl(meth)acrylate, isobornyl(meth)acrylate, adamantyl mono(meth)acrylate, dicyclopentenyloxyethyl(meth)acrylate, and dicyclopentanyl methacrylate; glycidyl(meth)acrylate, tetrahydrofurfuryl acrylate, and the like. heterocycle-containing mono(meth)acrylate compounds such as acrylate; aromatic ring-containing mono(meth)acrylate compounds such as benzyl (meth)acrylate, phenyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenoxy (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethoxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, phenoxybenzyl (meth)acrylate, benzyl benzyl (meth)acrylate, and phenylphenoxyethyl (meth)acrylate; (poly)oxyalkylene-modified mono(meth)acrylate compounds in which a polyoxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the above-mentioned various mono(meth)acrylate monomers; lactone-modified mono(meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of the above-mentioned various mono(meth)acrylate compounds;Aliphatic di(meth)acrylate compounds such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate; 1,4-cyclohexanedimethanol di(meth)acrylate, norbornane di(meth)acrylate, norbornane dimethanol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate. alicyclic di(meth)acrylate compounds such as; aromatic ring-containing di(meth)acrylate compounds such as biphenol di(meth)acrylate and bisphenol di(meth)acrylate; polyoxyalkylene-modified di(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the above-mentioned various di(meth)acrylate compounds; lactone-modified di(meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of the above-mentioned various di(meth)acrylate compounds. Meth)acrylate compounds; aliphatic tri(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate and glycerin tri(meth)acrylate; (poly)oxyalkylene-modified tri(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the aliphatic tri(meth)acrylate compounds; lactone-modified compounds in which a (poly)lactone structure has been introduced into the molecular structure of the aliphatic tri(meth)acrylate compounds Tri(meth)acrylate compounds; tetrafunctional or higher aliphatic poly(meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; tetrafunctional or higher (poly)oxyalkylene-modified poly(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the aliphatic poly(meth)acrylate compounds;Examples of the poly(meth)acrylate compound include tetrafunctional or higher lactone-modified poly(meth)acrylate compounds in which a (poly)lactone structure is introduced into the molecular structure of the aliphatic poly(meth)acrylate compound. These may be used alone or in combination of two or more types.
[0056] Among these, preferred are difunctional or higher functional (meth)acrylate compounds having a molecular weight in the range of 150 to 600, as they provide an excellent balance between the ability to impregnate the reinforcing fibers (f) and the strength of the resulting outer layer (B).When a plurality of types of other polymerizable unsaturated group-containing compounds are used in combination, the proportion of difunctional or higher functional (meth)acrylate compounds having a molecular weight in the range of 150 to 600 relative to the total mass of the other polymerizable unsaturated group-containing compounds is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0057] When other polymerizable unsaturated group-containing compounds are used in the resin composition (1), the amount thereof is preferably 40% by mass or less, more preferably 30% by mass or less, based on the total mass of the polyisocyanate compound (r1) and the polyhydroxy(meth)acrylate compound (r2), in order to achieve an excellent balance between the impregnation property into the reinforcing fiber (f) and the strength of the resulting outer layer (B). When other polymerizable unsaturated group-containing compounds are used in the resin composition (2), the amount thereof is preferably 40% by mass or less, more preferably 30% by mass or less, based on the total mass of the polyisocyanate compound (r1), the monohydroxy(meth)acrylate compound (r3), and the polyhydroxy compound (r4).
[0058] The resin compositions (1) and (2) may contain a polymerization initiator. While common polymerization initiators can be used without particular limitation, organic peroxides are particularly preferred. Examples of organic peroxides include diacyl peroxide compounds, peroxyester compounds, hydroperoxide compounds, ketone peroxide compounds, alkyl perester compounds, percarbonate compounds, and peroxyketals. These may be used alone or in combination. Among these, those having a 10-hour half-life temperature of 60°C or higher are preferred because they shorten the molding time. Furthermore, when producing a laminate by the below-described production methods 1 and 3, particularly when the core layer (a) or core layer (A) is a polystyrene foam, those having a 10-hour half-life temperature of 90°C or lower are preferred, more preferably 80°C or lower, and particularly preferably 70°C or lower are preferred, in order to avoid molding defects due to swelling of the polystyrene foam. Examples of such polymerization initiators include 1,6-bis(t-butylperoxycarbonyloxy)hexane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-amylperoxy)cyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, t-butylperoxydiethyl acetate, t-butylperoxyisopropyl carbonate, t-butylperoxy2-ethylhexyl carbonate, t-amylperoxyisopropyl carbonate, and t-amylperoxy2-ethylhexyl Examples of the polymerization initiator include butyl peroxycarbonate, t-hexylperoxyisopropyl carbonate, di-tert-butylperoxyhexahydroterephthalate, t-amylperoxytrimethylhexanoate, t-amylperoxyisonononaate, t-hexylperoxy-2-ethylhexanoate, n-butyl 4,4-di(t-butylperoxy)valerate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, and t-butylperoxypivalate. The amount of the polymerization initiator added is preferably in the range of 0.5 to 3 mass% relative to the total mass of the polymerizable unsaturated group-containing compound in the resin composition.
[0059] The resin compositions (1) and (2) may contain other components in addition to the various compounds described above, such as thermoplastic resins, polymerization inhibitors, curing accelerators, fillers, low-shrinkage agents, mold release agents, thickeners, viscosity reducers, pigments, antioxidants, plasticizers, flame retardants, antibacterial agents, UV stabilizers, reinforcing materials, and photocuring agents.
[0060] Examples of the thermoplastic resin include polyamide resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polycarbonate resin, urethane resin, polypropylene resin, polyethylene resin, polystyrene resin, acrylic resin, polybutadiene resin, polyisoprene resin, and resins obtained by modifying these by copolymerization, etc. These may be used alone or in combination of two or more.
[0061] Examples of the polymerization inhibitor include hydroquinone, trimethylhydroquinone, pt-butylcatechol, t-butylhydroquinone, toluhydroquinone, p-benzoquinone, naphthoquinone, hydroquinone monomethyl ether, phenothiazine, copper naphthenate, copper chloride, etc. These may be used alone or in combination of two or more.
[0062] Examples of the curing accelerator include metal soaps such as cobalt naphthenate, cobalt octenate, vanadyl octenate, copper naphthenate, and barium naphthenate, and metal chelate compounds such as vanadyl acetylacetate, cobalt acetylacetate, and iron acetylacetonate. Examples of amines include N,N-dimethylamino-p-benzaldehyde, N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyl-p-toluidine, N-ethyl-m-toluidine, triethanolamine, m-toluidine, diethylenetriamine, pyridine, phenylmorpholine, piperidine, and diethanolaniline. These may be used alone or in combination of two or more.
[0063] The fillers are broadly classified into inorganic compounds and organic compounds. Fillers are components added mainly for the purpose of adjusting the physical properties of molded products, such as strength, elastic modulus, impact strength, and fatigue durability.
[0064] Examples of inorganic compounds include calcium carbonate, magnesium carbonate, barium sulfate, mica, talc, kaolin, clay, celite, asbestos, barite, baryta, silica, silica sand, dolomite limestone, gypsum, aluminum fine powder, hollow balloons, alumina, glass powder, aluminum hydroxide, kansuiite, zirconium oxide, antimony trioxide, titanium oxide, molybdenum dioxide, and iron powder. Examples of organic compounds include powders of natural polysaccharides such as cellulose and chitin, and synthetic resin powders. Examples of synthetic resin powders include organic powders composed of hard resins, soft rubbers, elastomers, or polymers (copolymers), and particles having a multilayer structure such as a core-shell structure. Specific examples of synthetic resin powders include particles composed of butadiene rubber, acrylic rubber, urethane rubber, silicone rubber, and the like, polyimide resin powder, fluororesin powder, and phenolic resin powder. These may be used alone or in combination.
[0065] Examples of the release agent include zinc stearate, calcium stearate, paraffin wax, polyethylene wax, carnauba wax, etc. Preferred examples include paraffin wax, polyethylene wax, carnauba wax, etc. These may be used alone or in combination of two or more.
[0066] Examples of the thickener include metal oxides and hydroxides such as magnesium oxide, magnesium hydroxide, calcium oxide, and calcium hydroxide, acrylic resin-based fine particles, etc. These thickeners can be used alone or in combination of two or more.
[0067] Examples of the flame retardant include phosphorus atom-containing compounds, halogen atom-containing compounds, nitrogen atom-containing compounds, hydrated metal compounds, borates, metal oxides, silicone compounds, etc. These flame retardants can be used alone or in combination of two or more.
[0068] The method for producing the prepreg is not particularly limited, but examples thereof include a method in which the components of the matrix resin (r) are mixed using a known mixer such as a static mixer, a power mixer, a planetary mixer, or a kneader, and then the mixed material is impregnated into the reinforcing fibers (f), which are then sandwiched between release films and rolled using a rolling mill. When the matrix resin (r) is impregnated into the reinforcing fibers (f), the mixture may be heated as appropriate.
[0069] When the resin compositions (1) and (2) are used as the matrix resin (r), a prepreg with excellent storage stability and ease of handling can be obtained by allowing the rolled sheet to stand at room temperature to 50°C to cause a urethane reaction between the isocyanate groups and hydroxyl groups in the resin composition. When the resin compositions (1) and (2) are used as the matrix resin (r), the urethane reaction may be partially carried out during the preparation of the resin composition.
[0070] The thickness of the prepreg is preferably 0.02 mm or more, more preferably 0.05 mm or more, for ease of handling and excellent moldability, and is preferably 1.0 mm or less, more preferably 0.5 mm or less.
[0071] The outer layer (B) can be obtained by hot molding the prepreg. One example of a hot molding method is to place a plurality of prepreg layers into a mold preheated to 110°C to 160°C, clamp the mold using a compression molding machine, and then cure the layer while maintaining a molding pressure of 0.1 to 10 MPa. A preferred production method involves using a mold with a shear edge, maintaining a mold temperature of 130°C to 160°C and a molding pressure of 1 to 8 MPa, and performing hot compression molding for 1 to 3 minutes per mm of molded product thickness. The number of prepreg layers can be arbitrarily determined based on the balance between moldability and the strength of the resulting outer layer (B). However, a range of 1 to 20 layers is preferred for achieving excellent lightweight properties. The orientation of the prepregs during lamination can be arbitrarily determined taking into account the desired strength, but it is preferable to laminate them so that they are quasi-isotropic. For example, it is preferable to stack the prepregs in order so that the fiber directions alternate between 0° and 90°. The thickness of the outer layer (B) is preferably 0.1 mm or more, more preferably 0.4 mm or more, and particularly preferably 0.6 mm or more, in order to balance the strength and lightness of the resulting laminate, and is preferably 2.0 mm or less, more preferably 1.5 mm or less.
[0072] The laminate of the present invention may include the core layer (A) and the outer layer (B). As described above, the core layer (A) may be multilayered, or the outer layer (B) may be multilayered. The laminate of the present invention may also include layers other than these. The other layers may be arranged on both sides of the core layer (A) or on only one side. The other layers are preferably located intermediate the core layer (A) and the outer layer (B). Examples of the other layers include a metal layer, a resin layer, and an adhesive layer. In this case, the combined thickness of the core layer (A) and the outer layer (B) preferably accounts for 80% or more, more preferably 85% or more, of the total thickness of the laminate.
[0073] The method for producing the laminate of the present invention is not particularly limited, and the laminate can be produced by a wide variety of methods depending on the application and desired shape of the laminate. Specific examples include the following three production methods. These production methods will be described below. (Production Method 1) A method for producing a laminate in which a precursor obtained by laminating a core layer (a) made of a foam and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r) is heat-molded under conditions in which the core layer (a) is compressed. (Production Method 2) A method for producing a laminate in which the core layer (A) and the outer layer (B) made of fiber-reinforced plastic are bonded together using an adhesive. (Production Method 3) A method for producing a laminate, which comprises hot molding a precursor obtained by laminating the core layer (A) and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r).
[0074] The manufacturing method 1 involves heat-molding a precursor formed by laminating a core layer (a) made of a foam and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r) under conditions that compress the core layer (a). As described above, the outer layer (b) is preferably formed by stacking multiple prepregs, specifically 1 to 20 prepregs. The stacking direction of the prepregs can be set arbitrarily taking into account the desired strength, but it is preferable to stack them so that they are quasi-isotropic. For example, it is preferable to stack them in order so that the fiber directions alternate between 0° and 90°. The core layer (a) and the outer layer (b) may be directly laminated, or another layer such as an adhesive layer may be provided between them. When manufacturing a laminate using the manufacturing method 1, the moldable temperature of the prepreg forming the outer layer (b) is preferably 140°C or lower, and more preferably 110°C or lower, to prevent further foaming of the foam forming the core layer (a) during the heat-molding step.
[0075] In the above-mentioned manufacturing method 1, the molding conditions are not particularly limited, but examples include a method in which molding is performed at a temperature of 80 to 140°C and a pressure of 0.1 to 6 MPa for several minutes to several tens of minutes. A mold release agent may be applied to the mold as needed, and the precursor is preferably filled in the center of the mold. Furthermore, the thickness of the laminate may be adjusted using a spacer or the like so that it has a predetermined thickness.
[0076] The manufacturing method 2 is a method of bonding the core layer (A) and the outer layer (B) made of the fiber-reinforced plastic together using an adhesive. The core layer (A) and outer layer (B) used in manufacturing method 2 are as described above. The adhesive used in manufacturing method 2 is not particularly limited and is selected depending on the application and desired shape of the laminate, etc., and examples include acrylic resin-based, urethane resin-based, rubber-based, polyester resin-based, epoxy resin-based, cyanoacrylate resin-based, silicone resin-based, and modified silicone resin-based adhesives. The adhesive may be in any form, such as a one-component liquid, a two-component liquid, a sheet, or a double-sided tape.
[0077] The manufacturing method 3 involves hot molding a precursor obtained by laminating the core layer (A) and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r). The core layer (A) used in manufacturing method 3 is as described above. As described above, the outer layer (b) is preferably made by laminating multiple prepregs, specifically, 1 to 20 prepregs. The direction in which the prepregs are laminated can be set arbitrarily taking into account the desired strength, but it is preferable to laminate them so that they are quasi-isotropic. For example, it is preferable to laminate them in order so that the fiber directions alternate between 0° and 90°. The core layer (A) and the outer layer (b) may be laminated directly, or another layer such as an adhesive layer may be provided between them. Furthermore, when producing a laminate by production method 3, in order to prevent the foam constituting the core layer (A) from further foaming during the heat-forming step, the moldable temperature of the prepreg constituting the outer layer (b) is preferably 140°C or lower, and more preferably 110°C or lower.
[0078] In the manufacturing method 3, the molding conditions are not particularly limited, but examples include a method in which molding is performed at a temperature of 80 to 140°C and a pressure of 0.1 to 6 MPa for several minutes to several tens of minutes. A mold release agent may be applied to the mold as needed, and the precursor is preferably filled in the center of the mold. Furthermore, the thickness of the laminate may be adjusted using a spacer or the like so that it has a predetermined thickness.
[0079] The laminate of the present invention is characterized by being lightweight yet having excellent flame resistance and strength, and therefore can be suitably used for a variety of applications, including battery cases, aerospace aircraft components, railway vehicle components, housing equipment components, electronic equipment components, medical equipment components, home appliance components, and automobile components. [Example]
[0080] The present invention will now be described in more detail with reference to examples and comparative examples, in which "parts" and "%" are by mass unless otherwise specified.
[0081] Production Example 1 Production of prepreg (1) A 1-L flask equipped with a thermometer, nitrogen and air inlet tubes, a cooling condenser, and a stirrer was charged with an epoxy resin (DIC Corporation's "Epiclon 152"), 365 parts by mass of tetrabromobisphenol A-type epoxy resin (epoxy equivalent: 365 g / equivalent, bromine content: 48.1% by mass), 84 parts by mass of methacrylic acid, and 0.18 parts by mass of t-butylhydroquinone as a polymerization inhibitor, and the flask was heated to 95°C under a gas flow of a 1:1 mixture of nitrogen and air. 0.9 parts by mass of triphenylphosphine was added as a catalyst, the temperature was raised to 105°C, and the reaction was carried out for 12 hours. When the acid value reached 1 or less, the reaction was terminated. After cooling to around 80°C, the flask was removed from the reactor, and epoxy methacrylate (1) was obtained. The hydroxyl value of this resin was 135 mgKOH / g. The (meth)acryloyl group equivalent of this resin was 450 g / equivalent.
[0082] 13 parts by mass of diphenylmethane diisocyanate ("Lupranate MI" manufactured by BASFINOAC Polyurethanes Co., Ltd.), 80 parts by mass of the epoxy (meth)acrylate resin (1) obtained above, 20 parts by mass of an ethylenically unsaturated monomer (butanediol dimethacrylate), and 11.3 parts by mass of a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide, 10-hour half-life temperature 87°C) were mixed to obtain a matrix resin (1). Using a prepreg manufacturing device, glass fibers ("ER1620F" manufactured by Nippon Electric Glass Co., Ltd., glass fiber basis weight 162 g / m) were mixed. 2 ) was impregnated with matrix resin (1) so that the resin mass content was 35%, to obtain prepreg (1) with a thickness of 0.13 mm.
[0083] Production Example 2: Production of prepreg (2) 13 parts by mass of diphenylmethane diisocyanate ("Lupranate MI" manufactured by BASFINOAC Polyurethanes Co., Ltd.), 80 parts by mass of the epoxy (meth)acrylate resin (1) obtained in Production Example 1, 20 parts by mass of an ethylenically unsaturated monomer (butanediol dimethacrylate), and 18.1 parts by mass of a polymerization initiator ("Trigonox 421-70" manufactured by Kayaku Akzo Co., Ltd., organic peroxide, 10-hour half-life temperature 65°C) were mixed to obtain a matrix resin (2). Using a prepreg manufacturing apparatus, glass fibers ("ER1620F" manufactured by Nippon Electric Glass Co., Ltd., glass fiber basis weight 162 g / m) were mixed. 2 ) was impregnated with matrix resin (2) so that the resin mass content was 35%, to obtain prepreg (2) with a thickness of 0.13 mm.
[0084] Production Example 3: Production of prepreg (3) A mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate MR-200" manufactured by Tosoh Corporation, polymethylene polyphenyl polyisocyanate content 55 to 65 mass parts), 100 mass parts of hydroxyethyl methacrylate, 59 mass parts of hydroxyethyl methacrylate, 24 mass parts of an ethylene oxide adduct of bisphenol A ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent 164 g / equivalent), 31 mass parts of an ethylene oxide adduct of bisphenol A ("Newpol BPE-40" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent 204 g / equivalent), and 2.1 mass parts of a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide) was mixed to obtain a matrix resin (2). Using a prepreg manufacturing device, glass fiber (Nippon Electric Glass Co., Ltd. "ER1620F", glass fiber basis weight 162 g / m 2 ) was impregnated with matrix resin (3) so that the resin mass content was 35%, to obtain a prepreg (3) with a thickness of 0.13 mm.
[0085] Production Example 4 Production of prepreg (4) A matrix resin (3) was obtained by mixing 100 parts by mass of a mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate MR-200" manufactured by Tosoh Corporation, polymethylene polyphenyl polyisocyanate content 55 to 65% by mass), 59 parts by mass of hydroxyethyl methacrylate, 24 parts by mass of an ethylene oxide adduct of bisphenol A ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent 164 g / equivalent), 31 parts by mass of an ethylene oxide adduct of bisphenol A ("Newpol BPE-40" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent 204 g / equivalent), and 2.1 parts by mass of a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide). A prepreg manufacturing apparatus was used to prepare a matrix resin (3). Carbon fiber ("T700SC" manufactured by Toray Industries, Inc., carbon fiber basis weight 100 g / m) was then mixed. 2 ) was impregnated with matrix resin (4) so that the resin mass content was 34%, to obtain a prepreg (4) with a thickness of 0.1 mm.
[0086] Production Example 5 Production of prepreg (5) A matrix resin (3) was obtained by mixing 100 parts by mass of a mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate MR-200" manufactured by Tosoh Corporation, polymethylene polyphenyl polyisocyanate content of 55 to 65% by mass), 59 parts by mass of hydroxyethyl methacrylate, 24 parts by mass of an ethylene oxide adduct of bisphenol A ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent 164 g / equivalent), 31 parts by mass of an ethylene oxide adduct of bisphenol A ("Newpol BPE-40" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent 204 g / equivalent), and 2.1 parts by mass of a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide). Using an SMC manufacturing machine, carbon fibers (Toray Industries, Inc. "T700SC", carbon fiber weight 1150 g / m) were cut into 1 / 2 inch pieces and randomly scattered. 2 ) was impregnated with matrix resin (4) so that the resin mass content was 43%, to obtain a prepreg (5) with a thickness of 1.6 mm.
[0087] Examples 1 to 4 and Comparative Example 1 The laminates (1) to (9) and the laminate (1') were produced in the following manner and subjected to various evaluation tests. The evaluation results of each laminate are shown in Tables 1 and 2.
[0088] Example 1: Production of laminate (1) The prepreg (1) obtained in Production Example 1 was cut into pieces measuring 298 mm x 218 mm and 298 mm x 218 mm, and eight pieces were stacked in order so that the fiber orientation of the prepreg alternated between the 0° and 90° directions. This was loaded into the center of a flat plate mold coated with a mold release agent and compression molded under conditions of 4 MPa pressure, upper mold temperature 140°C, lower mold temperature 135°C, and molding time 3 minutes to obtain an outer layer (B1) measuring 300 mm x 220 mm x 1 mm. The flexural modulus of the outer layer (B1) measured in accordance with JIS K 7017 was 24.6 GPa. A 4 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A1) of 300 mm x 220 mm x 2 mm. The compression ratio in the thickness direction of the core layer (A1) was 50%, and the specific gravity was 0.08 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 2. Using a flame-retardant double-sided tape (Nitto Denko "No. 5011N", thickness 0.15 mm), one outer layer (B1) was attached to each side of the core layer (A1) to obtain a laminate (1).
[0089] Example 2: Production of laminate (2) The thermosetting prepreg (1) obtained in Production Example 1 was cut into pieces measuring 298 mm x 218 mm and 298 mm x 218 mm, and four sheets were stacked in order so that the fiber orientation of the prepreg alternated between 0° and 90°. This was loaded into the center of a flat plate mold coated with a mold release agent and compression molded under conditions of 4 MPa pressure, upper mold temperature 140°C, lower mold temperature 135°C, and molding time 3 minutes to obtain an outer layer (B2) measuring 300 mm x 220 mm x 0.5 mm. The flexural modulus of the outer layer (B2) measured in accordance with JIS K 7017 was 24.6 GPa. A 10 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A2) of 300 mm x 220 mm x 2 mm. The compression ratio in the thickness direction of the core layer (A2) was 80%, and the specific gravity was 0.20 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 5. Using a flame-retardant double-sided tape (Nitto Denko "No. 5011N", thickness 0.15 mm), one outer layer (B2) was attached to each side of the core layer (A2) to obtain a laminate (2).
[0090] Example 3: Production of laminate (3) The thermosetting prepreg (1) obtained in Production Example 1 was cut into pieces measuring 298 mm x 218 mm and 298 mm x 218 mm, and three sheets were stacked in order so that the fiber orientation of the prepreg alternated between the 0° and 90° directions. The pieces were placed in the center of a flat plate mold coated with a mold release agent and compression molded in a compression molding machine under conditions of 4 MPa pressure, 140°C for the upper mold, 135°C for the lower mold, and a molding time of 3 minutes to obtain an outer layer (B3) measuring 300 mm x 220 mm x 0.35 mm. The flexural modulus of the outer layer (B3) measured in accordance with JIS K 7017 was 24.6 GPa. A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A3) of 300 mm x 220 mm x 2 mm. The compression ratio in the thickness direction of the core layer (A3) was 90%, and the specific gravity was 0.40 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 10. Using a flame-retardant double-sided tape (Nitto Denko "No. 5011N", thickness 0.15 mm), one outer layer (B3) was attached to each side of the core layer (A3) to obtain a laminate (3).
[0091] Example 4 Production of laminate (4) A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A4) of 300 mm x 220 mm x 1.5 mm. The compression ratio in the thickness direction of the core layer (A4) was 92.5%, and the specific gravity was 0.53 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 13.3. Using a flame-retardant double-sided tape (Nitto Denko "No. 5011N", thickness 0.15 mm), one outer layer (B2) obtained in Example 2 was attached to each side of the core layer (A4) to obtain a laminate (4).
[0092] Example 5 Production of laminate (5) The prepreg (2) obtained in Production Example 2 was cut into sizes of 298 mm × 218 mm and 298 mm × 218 mm, and eight sheets were laminated in order so that the fiber directions of the prepregs were alternately in the 0° direction and the 90° direction. These were then laminated on a 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a surface coated with a flame retardant, density 0.04 g / cm) cut into sizes of 298 mm × 218 mm. 3 After laminating the mixture to both sides of a sheet of plastic (expansion ratio: 60), the mixture was placed in the center of a flat plate mold coated with a release agent, a 4 mm spacer was placed, and the mixture was compression molded under the conditions of a pressure of 4 MPa, an upper mold temperature of 105°C, a lower mold temperature of 100°C, and a molding time of 5 minutes to obtain a laminate (5) of 300 mm x 220 mm x 4 mm. The flexural modulus of the outer layer measured in accordance with JIS K 7017 was 24.6 GPa.
[0093] Example 6 Production of laminate (6) A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3The prepreg (2) obtained in Production Example 2 was cut to a size of 298 mm x 218 mm and placed in the center of a flat plate mold. The prepreg (2) was compression molded at an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A4) measuring 300 mm x 220 mm x 4 mm. Eight prepregs were laminated on both sides of the core layer (A4) so that the fiber directions of the prepregs alternated between 0° and 90°. The prepreg was then placed in the center of a flat plate mold coated with a release agent. A 4 mm spacer was placed in the mold. The prepreg was compression molded at a pressure of 4 MPa, an upper mold temperature of 105°C, a lower mold temperature of 100°C, and a molding time of 5 minutes to obtain a laminate (6) measuring 300 mm x 220 mm x 4 mm. The flexural modulus of the outer layer measured in accordance with JIS K 7017 was 24.6 GPa.
[0094] Example 7 Production of laminate (7) The prepreg (3) obtained in Production Example 3 was cut into pieces measuring 298 mm x 218 mm and 298 mm x 218 mm, and eight pieces were stacked in order so that the fiber orientation of the prepreg alternated between 0° and 90°. This was loaded into the center of a flat plate mold coated with a mold release agent and compression molded under conditions of 4 MPa pressure, upper mold temperature 140°C, lower mold temperature 135°C, and molding time 3 minutes to obtain an outer layer (B4) measuring 300 mm x 220 mm x 1 mm. The flexural modulus of the outer layer (B4) measured in accordance with JIS K 7017 was 23.2 GPa. A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A3) of 300 mm x 220 mm x 2 mm. The compression ratio in the thickness direction of the core layer (A3) was 90%, and the specific gravity was 0.40 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 10. Using a flame-retardant double-sided tape (No. 5011N, manufactured by Nitto Denko Corporation), one outer layer (B4) was attached to each side of the core layer (A3) to obtain a laminate (7).
[0095] Example 8 Production of laminate (8) The prepreg (4) obtained in Production Example 4 was cut into pieces measuring 298 mm x 218 mm and 298 mm x 218 mm, and eight pieces were stacked in order so that the fiber orientation of the prepreg alternated between 0° and 90°. This was loaded into the center of a flat plate mold coated with a mold release agent and compression molded under conditions of 4 MPa pressure, upper mold temperature 140°C, lower mold temperature 135°C, and molding time 3 minutes to obtain an outer layer (B5) measuring 300 mm x 220 mm x 1 mm. The flexural modulus of the outer layer (B5) measured in accordance with JIS K 7017 was 61.5 GPa. A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A3) of 300 mm x 220 mm x 2 mm. The compression ratio in the thickness direction of the core layer (A3) was 90%, and the specific gravity was 0.40 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 10. Using a flame-retardant double-sided tape (Nitto Denko Corporation's "No. 5011N"), one outer layer (B5) was attached to each side of the core layer (A3) to obtain a laminate (8).
[0096] Example 9 Production of laminate (9) The prepreg (5) obtained in Production Example 5 was cut to a size of 290 mm x 212 mm. One of these sheets was placed in the center of a flat plate mold coated with a mold release agent and compression molded under conditions of a pressure of 10 MPa, an upper mold temperature of 145°C, a lower mold temperature of 145°C, and a molding time of 3 minutes to obtain an outer layer (B5) of 300 mm x 220 mm x 1.5 mm. The flexural modulus of the outer layer (B5) measured in accordance with JIS K 7017 was 29 GPa. A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of an upper mold temperature of 30°C, a lower mold temperature of 30°C, and a molding time of 5 minutes to obtain a core layer (A3) of 300 mm x 220 mm x 2 mm. The compression ratio in the thickness direction of the core layer (A3) was 80%, and the specific gravity was 0.20 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 5. Using a flame-retardant double-sided tape (Nitto Denko Corporation's "No. 5011N"), one outer layer (B5) was attached to each side of the core layer (A3) to obtain a laminate (9).
[0097] Comparative Example 1: Production of laminate (1') A 2 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm) 3 The foam (expansion ratio: 60 times) was cut into a size of 300 mm x 220 mm to form a core layer (A1'). Using a flame-retardant double-sided tape (Nitto Denko "No. 5011N", thickness 0.15 mm), one outer layer (B1) obtained in Example 1 was attached to each side of the core layer (A1') to obtain a laminate (1').
[0098] Evaluation of laminate thickness The total thickness of the core layer (A) and the outer layer (B) (two layers) was evaluated as the thickness of the laminate. Note that in this evaluation, the thickness of the laminate did not include the thickness of the double-sided tape used in the manufacturing process of the laminate.
[0099] Measurement of specific gravity of laminated material The specific gravity was evaluated by dividing the total weight of the core layer (A) and outer layer (B) (two layers) by the volume of the laminate. Note that in this evaluation, the weight and volume of the double-sided tape used in the manufacturing process of the laminate were not included in the weight and volume of the laminate.
[0100] Flame resistance evaluation Using a gas burner, the flame was applied to the center of one side of the laminate, and the position of the flame was adjusted so that the temperature of the direct flame in contact with the laminate was 1000°C, and the laminate was heated for 6 minutes. The surface temperature of the center of the side of the laminate that was not heated by the direct flame was measured, and the maximum temperature during heating was used for evaluation.
[0101] Evaluation of laminate strength The bending rigidity (D) was calculated as an index showing the strength of the laminate and evaluated. The bending stiffness (D) was calculated using the following formula: D = ((E1 × t1) × (E2 × t2) × (T + tc) 2 ) / 4λ(E1×t1+E2×t2) where E is the bending modulus of elasticity of the outer layer (B) [kN / mm 2 ] (upper layer E1, lower layer E2), t is the thickness of the outer layer (B) [mm] (upper layer t1, lower layer t2), tc is the thickness of the core layer (A) [mm], and T is the thickness of the laminate [mm]. λ is 1-(Poisson's ratio) 2 The coefficient for anisotropic materials is 0.99. The average value for steel plates is 4.5kN mm 2 Anything above that was rated as A, and anything below that was rated as B.
[0102] [Table 1]
[0103] [Table 2]
Claims
1. The foamed foam has a core layer (A) compressed in the thickness direction and an outer layer (B) made of a fiber-reinforced plastic, The foam is a polyethylene resin bead foam having a flame retardant coating applied to its surface, A laminate in which the core layer (A) has a compressibility of 40% or more in terms of thickness, and the aspect ratio of foam cells of the core layer (A), represented by the following formula, is 2 or more. Aspect ratio = 1 / [1 - compression ratio (%) / 100]
2. 2. The laminate according to claim 1, wherein the outer layer (B) is obtained by hot molding a prepreg containing reinforcing fibers (f) and a matrix resin (r), and the matrix resin is a resin composition (1) containing a polyisocyanate compound (r1) and a polyhydroxy(meth)acrylate compound (r2), or a resin composition (2) containing a polyisocyanate compound (r1), a monohydroxy(meth)acrylate compound (r3), and a polyhydroxy compound (r4).
3. 3. The method for producing a laminate according to claim 1 or 2, wherein a precursor obtained by laminating a core layer (a) made of a foam and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r) is heat-molded under conditions in which the core layer (a) is compressed.
4. A method for manufacturing a laminate, comprising bonding a core layer (A) formed by compressing a foam in the thickness direction and an outer layer (B) made of fiber-reinforced plastic using an adhesive to obtain a laminate comprising the core layer (A) and the outer layer (B).
5. A method for manufacturing a laminate, comprising: heat-molding a precursor formed by laminating a core layer (A) obtained by compressing a foam in the thickness direction and an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r) to obtain a laminate having the core layer (A) and an outer layer (B) made of fiber-reinforced plastic.
6. A battery case using the laminate according to claim 1 or 2.