Multilayer films and packaging materials

JPWO2024075352A5Active Publication Date: 2024-10-03DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023572172
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-06
Filing Date
2023-07-06
Publication Date
2024-10-03
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

Existing multilayer films used for packaging are difficult to recycle due to the mixture of polyethylene and polypropylene, leading to quality deterioration and inaccurate composition analysis, especially when high-density polyethylene is used, which affects transparency and impact resistance.

Method used

A multilayer film structure comprising a surface layer, intermediate layer, and sealing layer, with a composition of 90% polyethylene, 5-40% high-density polyethylene, and 28-72% medium-density polyethylene, ensuring easy recyclability and accurate compositional analysis by IR.

Benefits of technology

The film maintains excellent packaging suitability, impact resistance at low temperatures, and reduces environmental load by being easily recyclable, while allowing precise determination of polyethylene ratio in recycled materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a mono-material multilayer film comprising at least a surface layer (A), an intermediate layer (B) and a sealing layer (C) laminated in this order, characterized in that 90% by mass or more of the components contained in the multilayer film are polyethylene resins, the content of high-density polyethylene in the entire multilayer film is 5 to 40% by mass, and the content of medium-density polyethylene in the entire multilayer film is 28 to 72% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer film used as a packaging material for food, medical products, etc. [Background technology]

[0002] Of all the plastics produced, only a very small amount is separated, collected and recycled worldwide. It is said that the majority of plastic waste is incinerated, disposed of in landfills, or leaks into the environment. It is difficult to turn recycled plastic products back into the same products from a cost perspective, and since plastics basically deteriorate every time they are recycled, they have no choice but to be reborn as products of lower quality.

[0003] Reasons for the deterioration of quality of recycled plastics include the fact that many plastic products currently in circulation are made using polymeric compounds (sometimes called resins or polymers) with multiple different structures, and that impurities are mixed into the plastic, causing it to become discolored. In particular, packaging materials used for food and beverages are often multifunctional, such as durable weather resistance during distribution and refrigeration, functions to protect the contents from processes such as heat sterilization, and long-term storage (gas barrier properties), and these are given many functions by combining various raw materials with each function. Conversely, the quality of recycled plastics deteriorates due to the multifunctional nature of these materials. In order to prevent the deterioration of quality of recycled plastics, recycled materials are sometimes mixed with virgin materials (newly synthesized polymeric compounds that are not recycled).

[0004] As a way to improve the quality of recycled plastics without compromising the functionality of the packaging material as much as possible, there is a movement to "use packaging materials from as single a type of raw material as possible" (sometimes referred to as "mono-materialization"), and proposals have begun to use multi-layer films (sometimes referred to as mono-material films) made by laminating multiple layers of only polyethylene film as the main plastic raw material.

[0005] On the other hand, polypropylene film, which is often used as packaging material along with polyethylene, has a specific gravity close to that of polyethylene, so it cannot be easily separated by specific gravity, and as a result, polyethylene and polypropylene end up mixed together in recycled materials. Mono-material films laminated with polyethylene have been disclosed (see, for example, Patent Documents 1 and 2). However, even in the case of such mono-material films, when they are collected after use and mixed with polypropylene to become recycled materials, their composition (the ratio of polyethylene to polypropylene) becomes unknown, making it difficult to produce stably or to obtain the desired physical properties when re-filming, and there is a concern that the quality may decline.

[0006] In order to know the composition ratio of polyethylene and polypropylene in the recycled material, it is necessary to measure it by nuclear magnetic resonance spectroscopy (NMR). However, NMR is expensive and complicated, which leads to high costs for recycled materials. Therefore, composition analysis by simple quantitative methods such as infrared spectroscopy (IR) and differential scanning calorimetry (DSC) has been proposed (see Non-Patent Documents 1 and 2). However, when determining the blend ratio of polyethylene and polypropylene using IR, it has been pointed out that the accuracy of composition analysis decreases when a large amount of polyethylene with many branches, such as low-density polyethylene, is included.

[0007] Furthermore, the inventors conducted extensive research into determining the polyethylene ratio in a recycled material consisting of a mixture of polyethylene and polypropylene, and found that the calculation formulas described in Non-Patent Documents 1 and 2 had a large measurement error for the recycled material with a high polyethylene ratio. [Prior art documents] [Non-patent literature]

[0008] [Non-Patent Document 1] Adachi, Kurita, Asakura, Gifu Prefectural Industrial Technology Center Research Report No. 13, pp10-13, 2019 [Non-Patent Document 2] Adachi, Kurita, Asakura, Gifu Prefectural Industrial Technology Center Research Report No.1, pp37-40, 2020 [Patent documents]

[0009] [Patent Document 1] JP 2020-55176 A [Patent Document 2] International Publication No. WO2022 / 168867 Summary of the Invention [Problem to be solved by the invention]

[0010] It is considered that polyethylene with few short chain branches is less likely to affect the polypropylene peak when a mixture with a polypropylene resin is measured by infrared spectroscopy (IR). Therefore, from the viewpoint of the accuracy of measuring the polyethylene ratio by IR of a recycled material in which a polypropylene resin and a polyethylene resin are mixed, it is preferable to use polyethylene with few short chain branches, especially high density polyethylene. On the other hand, high density polyethylene film is difficult to use for packaging applications where the contents need to be visually confirmed due to its poor transparency, and may not be suitable for packaging frozen foods or chilled foods that are stored in a low temperature environment due to its poor impact resistance at low temperatures.

[0011] The inventors conducted extensive research to develop a multilayer film that is an easily recyclable mono-material film, has good accuracy in measuring the polyethylene ratio by IR for recycled materials in which polypropylene-based resin and polyethylene-based resin are mixed, can be used in low-temperature environments such as for frozen foods, and has excellent packaging suitability, and as a result, they arrived at the multilayer film of the present invention. That is, they discovered that these problems can be solved by setting the contents of high-density polyethylene and medium-density polyethylene in the entire multilayer film to specific ranges.

[0012] In other words, an object of the present invention is to provide a multilayer film which has excellent performance as a packaging material, is a mono-material, and has excellent composition analysis accuracy by IR. [Means for solving the problem]

[0013] The present invention solves the above-mentioned problems by providing a multilayer film comprising at least a surface layer (A), an intermediate layer (B) and a sealing layer (C) laminated in this order, characterized in that 90% by mass or more of the components contained in the multilayer film are polyethylene resins, the content of high-density polyethylene in the entire multilayer film is 5 to 40% by mass, and the content of medium-density polyethylene in the entire multilayer film is 28 to 72% by mass. Effect of the Invention

[0014] The multilayer film of the present invention is a polyethylene mono-material film, so it is easy to recycle and contributes to reducing the environmental load. Furthermore, when recycled, the composition of the recycled material is easily clarified because the accuracy of the composition analysis of the recycled material is not reduced, making it easier to obtain the desired physical properties, and therefore the amount of virgin material mixed with the recycled material can be reduced, contributing to the realization of a recycling-oriented society.

[0015] The multilayer film of the present invention is also excellent in suitability for packaging machines and is suitable as a packaging material. In particular, the multilayer film of the present invention is excellent in impact resistance at a very low temperature of -20°C, and therefore can be suitably used for packaging frozen foods, chilled foods, etc. that are transported or managed at low temperatures, and for packaging medical products. Furthermore, since suitable impact resistance can be achieved without bonding to a stretched substrate, the weight of the packaging material can be reduced, thereby reducing the environmental load and the cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The multilayer film of the present invention is a multilayer film having at least a surface layer (A), an intermediate layer (B) and a seal layer (C) laminated in this order, characterized in that 90% by mass or more of the components contained in the multilayer film are polyethylene-based resins, the content of high-density polyethylene in the entire multilayer film is 5 to 40% by mass, and the content of medium-density polyethylene in the entire multilayer film is 28 to 72% by mass.

[0017] [Surface layer (A)] The surface layer (A) of the multilayer film of the present invention is preferably a layer containing a polyethylene resin as the main resin component, although other co-extrudable resins may be used in combination therewith within the scope of not impairing the effects of the present invention. "Main resin component" specifically means that 70% by mass or more of the resin components used in the surface layer (A) is a polyethylene-based resin, preferably 80% by mass or more is a polyethylene-based resin, and more preferably 90% by mass or more is a polyethylene-based resin.

[0018] As the polyethylene-based resin, for example, polyethylene resins such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), and the like can be used.

[0019] The low density polyethylene (LDPE) is 0.935g / cm 3 By "ethylene" is meant a homopolymer of ethylene having a density less than 1000 MPa. The linear low-density polyethylene (LLDPE) is a copolymer of ethylene and α-olefin polymerized using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst, and has a density of 0.925 g / cm. 3 It refers to polyethylene having less than 100% carbon atoms. Therefore, it is distinguished from low-density polyethylene (LDPE), which is a homopolymer of ethylene. The α-olefins that serve as comonomers for linear low-density polyethylene are those having 3 or more carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 4-methylpentene, 3,3-dimethylbutene, and mixtures thereof. The above medium density polyethylene (MDPE) is 0.925g / cm 3 More than 0.942g / cm 3 It means a copolymer of ethylene and α-olefin having a density of less than 10 ... The above high density polyethylene (HDPE) is 0.942g / cm 3 It may be a homopolymer of ethylene or a copolymer of ethylene and an α-olefin, but since an increase in the amount of the α-olefin serving as a comonomer reduces the density, it is preferable to have a small amount of comonomer, and specifically, the comonomer ratio is preferably 0.5% or less. In commercially available products, the comonomer ratio may not be disclosed, so linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene are distinguished by density, and low-density polyethylene and medium-density polyethylene are distinguished by whether they are homopolymers of ethylene or not. In the present invention, even if a product is commercially available as linear low-density polyethylene, a product having a density of 0.925 g / cm3 may be used. 3 The above is treated as medium density polyethylene. For example, the density is 0.926g / cm 3If there is a polyethylene of this type, if it is an ethylene homopolymer it is treated as low density polyethylene, and if it is an ethylene and α-olefin copolymer it is treated as medium density polyethylene.

[0020] As the polyethylene resin, biomass-derived polyethylene may be used, for example, biomass-derived low-density polyethylene (product name: SBC818, density: 0.918 g / cm) manufactured by Braskem. 3 , MFR: 8.1 g / 10 min), and biomass-derived low-density polyethylene manufactured by Braskem (product name: SPB681, density: 0.922 g / cm 3 , MFR: 3.8g / 10min), Braskem biomass-derived linear low-density polyethylene (product name: SLL118, density: 0.916g / cm 3 , MFR: 1.0 g / 10 min.)

[0021] As described later, the surface layer (A) of the multilayer film of the present invention needs to have a higher melting point than the seal layer (C) of the multilayer film. Therefore, the surface layer (A) of the multilayer film of the present invention is preferably a layer in which a medium density polyethylene (a1) and a high density polyethylene (a2) are used in combination, and the ratio of the medium density polyethylene (a1) to the high density polyethylene (a2) is more preferably 30:70 to 85:15, and even more preferably 40:60 to 70:30. When the surface layer (A) is such a layer, it can exhibit impact resistance in a very low temperature (e.g., -20°C) environment while maintaining suitable packaging suitability, and also has good resistance to puncture by frozen foods. The medium-density polyethylene (a1) and the high-density polyethylene (a2) may be used in combination of two or more kinds. In that case, for example, when two kinds (a1-1 and a1-2) of the medium-density polyethylene (a1) are used, it is preferable that the ratio of (a1-1)+(a1-2):(a2) is within the above range.

[0022] In addition, the surface layer (A) of the multilayer film of the present invention may further contain a polyethylene resin other than the medium density polyethylene (a1) and the high density polyethylene (a2). In particular, in the case of applications requiring transparency, it is preferable to further use low density polyethylene (LDPE). By further using the low density polyethylene (LDPE), the crystallization of the surface layer (A) can be delayed and the transparency can be improved.

[0023] The surface layer (A) of the multilayer film of the present invention preferably has a melting point of 110 to 150°C, more preferably 115 to 145°C. By setting the melting point of the surface layer (A) within the above range, adhesion to a seal bar during packaging can be suppressed, and suitable packaging machine suitability can be easily achieved. Also, suitable impact resistance and heat resistance can be achieved. The melting point of the resin refers to the melting peak measured by a differential scanning calorimeter. When the surface layer (A) is a resin layer containing a mixture of multiple resins, it is preferable to determine the blending ratio so that the melting point of the mixed resin composition falls within the range. The melting point of the mixed resin composition is a melting point calculated from the content of each resin component and the melting point of each resin, and is calculated as (TaWa+TbWb+TcWc···) / (Wa+Wb+Wc···) when the resins used in each layer are resin a, resin b, resin c···, and the melting points of these resins are Ta, Tb, Tc···, and the masses of the resins used in the layers are Wa, Wb, Wc···.

[0024] The surface layer (A) of the multilayer film of the present invention has a density of 0.925 to 0.955 g / cm 3 and preferably 0.930 to 0.950 g / cm 3 It is more preferable that: By setting the density of the surface layer (A) within the above range, it becomes easier to realize suitable impact resistance and packaging machine suitability, and also suitable heat resistance can be realized. The density is a value measured in accordance with JIS K7112.

[0025] The MFR (190°C, 21.18N) of the polyethylene resin used in the surface layer (A) is 0.5 to 50g / 10min (190°C, 21.18N), preferably 1 to 30g / 10min (190°C, 21.18N), and more preferably 2 to 20g / 10min (190°C, 21.18N). It is preferable for the MFR to be within this range in terms of obtaining good film-forming properties.

[0026] The surface layer (A) of the multilayer film of the present invention may be made of various resins used in packaging films other than the polyethylene resin, and among these, olefin resins such as polypropylene resins are preferably used. As the polypropylene resin, a propylene homopolymer, a propylene-α-olefin random copolymer, a propylene-α-olefin block copolymer, etc. may be used. These may be used alone or in combination.

[0027] When an olefin-based resin other than the above-mentioned polyethylene-based resin is used as the resin component used in the surface layer (A), its content is preferably 30 mass % or less of the resin components contained in the surface layer (A), more preferably 10 mass % or less, and even more preferably 5 mass % or less.

[0028] In addition, a cyclic polyolefin resin may be used as the olefin resin other than the above-mentioned polyethylene resin, but the content of the cyclic polyolefin resin in the resin components contained in the surface layer (A) is preferably 10 mass% or less, more preferably 5 mass% or less, and it is also preferable that no cyclic polyolefin resin is used at all. Examples of the cyclic olefin resin include norbornene polymers, vinyl alicyclic hydrocarbon polymers, and cyclic conjugated diene polymers. Of these, norbornene-based polymers are preferred. Furthermore, examples of norbornene-based polymers include ring-opening polymers (COP) of norbornene-based monomers, and norbornene copolymers (COC) obtained by copolymerizing norbornene-based monomers with olefins such as ethylene. Also particularly preferred are hydrogenated products of COP and COC. The weight average molecular weight of the cyclic olefin resin is preferably from 5,000 to 500,000, and more preferably from 7,000 to 300,000.

[0029] The norbornene monomer used as the raw material for the norbornene polymer is an alicyclic monomer having a norbornene ring. Examples of such norbornene-based monomers include norbornene, tetracyclododecene, ethylidenenorbornene, vinylnorbornene, ethylidetetracyclododecene, dicyclopentadiene, dimethanotetrahydrofluorene, phenylnorbornene, methoxycarbonylnorbornene, and methoxycarbonyltetracyclododecene. These norbornene monomers may be used alone or in combination of two or more kinds.

[0030] The norbornene-based copolymer is a copolymer of the norbornene-based monomer and a copolymerizable olefin. Examples of such olefins include olefins having 2 to 20 carbon atoms, such as ethylene, propylene, and 1-butene; cycloolefins, such as cyclobutene, cyclopentene, and cyclohexene; and non-conjugated dienes, such as 1,4-hexadiene.

[0031] In the surface layer (A) used in the present invention, resins other than those mentioned above may be used in combination. Examples of the other resins include thermoplastic elastomers such as polyethylene-based elastomers, such as ethylene-vinyl acetate copolymer (EVA) and ethylene-α-olefin copolymer, polypropylene-based elastomers, and butene-based elastomers; ethylene-based copolymers such as ethylene-methyl methacrylate copolymer (EMMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate (EMA) copolymer, ethylene-ethyl acrylate-maleic anhydride copolymer (E-EA-MAH), ethylene-acrylic acid copolymer (EAA), and ethylene-methacrylic acid copolymer (EMAA); and further ionomers of ethylene-acrylic acid copolymer and ionomers of ethylene-methacrylic acid copolymer.

[0032] When the above-mentioned other resins are used, their content is preferably 30 mass % or less of the resin components contained in the surface layer (A), more preferably 20 mass % or less, even more preferably 10 mass % or less, and even more preferably 5 mass % or less.

[0033] In the surface layer (A) of the multi-layer film of the present invention, various additives may be appropriately used in addition to the above resin components. Examples of the additives include antioxidants, weather stabilizers, antistatic agents, antifogging agents, antiblocking agents, lubricants, nucleating agents, pigments, and biodegradability-promoting additives. When these additives are used, they are used in an amount of preferably 5 parts by mass or less, and more preferably about 0.01 to 3 parts by mass, per 100 parts by mass of the resin component used in the surface layer (A).

[0034] The thickness ratio of the surface layer (A) of the multilayer film of the present invention to the total thickness of the multilayer film is preferably in the range of 10 to 45%, particularly preferably in the range of 15 to 30%, since this makes it easy to obtain suitable heat resistance and excellent impact resistance at low temperatures.

[0035] [Middle layer (B)] The intermediate layer (B) of the multilayer film of the present invention is preferably a layer containing a polyethylene resin as a main resin component, similar to the surface layer (A) of the multilayer film of the present invention, but may be used in combination with other co-extrudable resins within the scope of not impairing the effects of the present invention.

[0036] The intermediate layer (B) of the multilayer film of the present invention is preferably a layer in which a medium density polyethylene (b1) and a high density polyethylene (b2) are used in combination, and the ratio of the medium density polyethylene (b1) to the high density polyethylene (b2) is more preferably 50:50 to 90:10, and further preferably 70:30 to 80:20. When the intermediate layer (B) is such a layer, it is easy to exhibit impact resistance in a very low temperature (e.g., −20° C.) environment. A plurality of types of medium-density polyethylene (b1) and high-density polyethylene (b2) may be used in combination. In that case, for example, when two types of medium-density polyethylene (b1) (b1-1 and b1-2) are used, it is preferable that the ratio of (b1-1)+(b1-2):(b2) is within the range.

[0037] In addition, the intermediate layer (B) of the multilayer film of the present invention may further contain a polyethylene resin other than the medium density polyethylene (b1) and the high density polyethylene (b2). In particular, in the case of applications requiring transparency, it is preferable to further use low density polyethylene (LDPE). By further using the low density polyethylene (LDPE), the crystallization of the intermediate layer (B) can be delayed and the transparency can be improved.

[0038] The intermediate layer (B) of the multilayer film of the present invention has a melting point of preferably 110 to 150°C, more preferably 115 to 140°C. By setting the melting point of the intermediate layer (B) within the above range, it becomes easier to realize suitable impact resistance and packaging machine suitability, and also suitable heat resistance can be realized. The melting point of the resin refers to the melting peak measured by a differential scanning calorimeter. When the intermediate layer (B) is composed of one type of resin, the melting point of the intermediate layer (B) is the melting point of the resin. When the intermediate layer (B) is a resin layer in which multiple types of resins are mixed, it is preferable to determine the blending ratio so that the melting point of the mixed resin composition is within the range. The melting point of the mixed resin composition is a melting point calculated from the content of each resin component and the melting point of each resin, and is calculated as (TaWa+TbWb+TcWc···) / (Wa+Wb+Wc···), where the resins used in each layer are resin a, resin b, resin c···, and the melting points of these resins are Ta, Tb, Tc···, and the masses of the resins used in the layers are Wa, Wb, Wc···.

[0039] The intermediate layer (B) of the multilayer film of the present invention has a density of 0.925 to 0.955 g / cm 3 and preferably 0.930 to 0.950 g / cm 3 It is more preferable that: By setting the density of the intermediate layer (B) within this range, the film has suitable impact resistance and also improves interlayer adhesion. The density is a value measured in accordance with JIS K7112.

[0040] The MFR (190°C, 21.18N) of the polyethylene resin used in the intermediate layer (B) is 0.5 to 50g / 10min (190°C, 21.18N), preferably 1 to 30g / 10min (190°C, 21.18N), and more preferably 2 to 20g / 10min (190°C, 21.18N). It is preferable for the MFR to be within this range in terms of obtaining good film-forming properties.

[0041] In the intermediate layer (B) used in the present invention, resins other than those mentioned above may be used in combination. Examples of the other resins include polypropylene-based resins such as propylene homopolymers, propylene-α-olefin random copolymers, and propylene-α-olefin block copolymers, cyclic olefin-based resins, thermoplastic elastomers such as ethylene-vinyl acetate copolymers (EVA), polyethylene-based elastomers, polypropylene-based elastomers, and butene-based elastomers; ethylene-based copolymers such as ethylene-methyl methacrylate copolymers (EMMA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methyl acrylate (EMA) copolymers, ethylene-ethyl acrylate-maleic anhydride copolymers (E-EA-MAH), ethylene-acrylic acid copolymers (EAA), and ethylene-methacrylic acid copolymers (EMAA); and further ionomers of ethylene-acrylic acid copolymers and ionomers of ethylene-methacrylic acid copolymers.

[0042] When the other resins are used, the content of the other resins is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, of the resin components contained in the intermediate layer (B). Within this range, the multilayer film as a whole is easily made mono-material, and recyclability is improved.

[0043] In the intermediate layer (B) of the multi-layer film of the present invention, various additives may be appropriately used in addition to the above resin components. Examples of the additives include antioxidants, weather stabilizers, antistatic agents, antifogging agents, antiblocking agents, lubricants, nucleating agents, pigments, and biodegradability-promoting additives. When these additives are used, they are used in an amount of preferably 5 parts by mass or less, and more preferably about 0.01 to 3 parts by mass, per 100 parts by mass of the resin component used in the intermediate layer (B).

[0044] The thickness ratio of the intermediate layer (B) to the total thickness of the multilayer film is preferably 30 to 70%, and more preferably 35 to 55%, from the viewpoints of good packaging machine suitability and low-temperature impact resistance.

[0045] Sealing layer The sealing layer (C) of the multilayer film of the present invention is preferably a layer containing linear low density polyethylene as the main resin component. By providing the sealing layer (C), good impact resistance and heat sealability can be achieved.

[0046] The melting point of the seal layer (C) of the multilayer film of the present invention is preferably 75 to 125°C, more preferably 80 to 120°C, further preferably 80 to 100°C, and particularly preferably 83 to 97°C. By setting the melting point of the sealing layer (C) within this range, good sealing strength can be obtained. The melting point of a resin refers to the melting peak measured by a differential scanning calorimeter. When there are two peaks, the peak with the largest amount of endotherm is taken as the melting point. When the seal layer (C) is composed of one type of resin, the melting point of the seal layer (C) is the melting point of the resin. When the seal layer (C) is a resin layer in which multiple types of resins are mixed, it is preferable to determine the blending ratio so that the melting point of the mixed resin composition is within the range. The melting point of the mixed resin composition is a melting point calculated from the content of each resin component and the melting point of each resin, and is calculated as (TaWa+TbWb+TcWc···) / (Wa+Wb+Wc···), where the resins used in each layer are resin a, resin b, resin c···, and the melting points of these resins are Ta, Tb, Tc···, and the masses of the resins used in the layers are Wa, Wb, Wc···.

[0047] The density of the linear low density polyethylene is 0.880 to 0.924 g / cm because it is easy to obtain good sealing properties and impact resistance. 3 It is preferable that the density is 0.890 to 0.920 g / cm 3 When the density is in this range, it can be assumed that the number of short chain branches in the polyethylene is relatively small, and even when it is mixed with polypropylene as a recycled material, the blend ratio can be easily identified by infrared spectroscopy (IR).

[0048] The linear low density polyethylene has an MFR of 0.5 to 50 g / 10 min (190° C., 21.18 N), preferably 1 to 30 g / 10 min (190° C., 21.18 N), and more preferably 2 to 20 g / 10 min (190° C., 21.18 N). It is preferable for the MFR to be within this range in terms of obtaining good film-forming properties.

[0049] By making the content of linear low-density polyethylene in the sealing layer (C) of the multilayer film of the present invention 70 mass% or more of the resin components contained in the sealing layer (C), it becomes easier to obtain suitable sealing properties and excellent impact resistance at low temperatures. The content is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, of the resin component contained in the seal layer (C). Furthermore, 100% by mass of the resin component contained in the seal layer (C) may be linear low-density polyethylene. In addition, two or more linear low density polyethylenes having different densities, MFRs, etc. may be used in combination, so long as the total content is within the above range.

[0050] In the sealing layer (C) of the multi-layer film of the present invention, resins other than the linear low density polyethylene may be used in combination within the range that does not impair the effects of the present invention. Examples of other resins that can be used in combination include polyethylene resins other than the linear low-density polyethylene resins exemplified for the surface layer (A) above, olefin resins such as polypropylene resins, and other resins. When the olefin resin is used as the resin other than the linear low-density polyethylene, its content is preferably 30 mass% or less of the resin components contained in the seal layer (C), more preferably 10 mass% or less, and even more preferably 5 mass% or less.

[0051] In addition, a cyclic polyolefin resin may be used as the olefin resin, but the content of the cyclic polyolefin resin in the resin components contained in the sealing layer (C) of the multilayer film of the present invention is preferably 10 mass% or less, more preferably 5 mass% or less, and it is also preferable that no cyclic polyolefin resin is used at all.

[0052] In addition, the sealing layer (C) of the multilayer film of the present invention may contain resins other than those mentioned above. Examples of such resins include the thermoplastic elastomers, ethylene-based copolymers, ionomers, etc. exemplified for the surface layer (A). When such other resins are used, their content is preferably 30 mass% or less of the resin components contained in the sealing layer (C), more preferably 10 mass% or less, and even more preferably 5 mass% or less.

[0053] In the sealing layer (C) of the multi-layer film of the present invention, various additives may be appropriately used in addition to the above resin components. Examples of the additives include antioxidants, weather stabilizers, antistatic agents, antifogging agents, antiblocking agents, lubricants, nucleating agents, pigments, and biodegradability-promoting additives. When these additives are used, they are used in an amount of preferably 15 parts by mass or less, more preferably about 0.01 to 10 parts by mass, per 100 parts by mass of the resin component used in the sealing layer (C).

[0054] The thickness ratio of the sealing layer (C) of the multilayer film of the present invention to the total thickness of the multilayer film is preferably 10 to 45%, more preferably 20 to 40%, from the viewpoint of low-temperature impact resistance and sufficient seal strength when a heavy object is enclosed. If the thickness ratio of the sealing layer (C) to the total thickness of the multilayer film is 10% or more, sufficient seal strength can be obtained, and if the thickness ratio is 20% or more, it is more preferable because seal strength that can withstand the enclosure of a heavy object can be easily obtained. In addition, if the thickness ratio is 45% or less, when mixed with a polypropylene film as a recycled material, the polyethylene / polypropylene ratio can be specified with a practical accuracy by simple measurement using IR, and if the thickness ratio is 40% or less, it is more preferable because the accuracy is improved.

[0055] The sealing layer (C) of the multilayer film of the present invention may be composed of multiple layers. When the sealing layer (C) is composed of multiple layers, the linear low-density polyethylene contained in each of the multiple sealing layers (C) is preferably 70% by mass or more, more preferably 75% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the sealing layer (C) is made of multiple layers, each layer may have the same or different composition, or may have different additives, as long as the composition is within the range. When the sealing layer (C) is made of multiple layers, the total thickness of the sealing layer (C) is preferably 10 to 45%, more preferably 20 to 40%, of the total thickness of the multilayer film.

[0056] [Multi-layer film] The multilayer film of the present invention is a multilayer film in which the surface layer (A), intermediate layer (B) and seal layer (C) are laminated in the order of (A) / (B) / (C). In addition, within the scope of the effects of the present invention, another layer (e.g., including a plurality of seal layers (C), other intermediate layers, adhesive layers, adhesive layers, etc.) may be included between the surface layer (A), intermediate layer (B) and seal layer (C). In that case, it is sufficient that the layers are laminated in the order of (A) / (B) / (C), such as (A) / (B) / (C) / (C), (A) / (B) / (other layers) / (C), (A) / (other layers) / (B) / (C), etc. When another layer is added to make a mono-material film, it is preferable that all layers, including the other layer, have a polyethylene resin as the main resin component. Due to the above-described constitution, the multilayer film of the present invention can achieve suitable impact resistance even at low temperatures, particularly at temperatures as low as -20°C, which is significantly below 0°C. In addition, it has good film-forming properties, and can achieve favorable sealing properties and suitability for packaging machines.

[0057] The multilayer film of the present invention is such that 90% by mass or more of the components contained in the multilayer film are polyethylene-based resins. By making 90% by mass or more of the components contained in the multilayer film polyethylene-based resins, the multilayer film becomes a mono-material film, and recyclability is improved. Note that the components contained in the multilayer film include not only resins but also additives, adhesives, etc. From the viewpoint of recyclability, it is more preferable that 95% by mass or more of the components contained in the multilayer film is a polyethylene resin.

[0058] The multilayer film of the present invention preferably has a total thickness of 15 to 100 μm, more preferably 20 to 90 μm. If the total thickness of the film is within this range, it becomes easier to obtain excellent impact resistance, rigidity, sealability, suitability for packaging heavy items, suitability for use with packaging machines, and the like at low temperatures.

[0059] The thickness of each layer is not particularly limited, but for example, the thickness of the surface layer (A) is preferably from 2 to 25 μm, and more preferably from 4 to 20 μm. The thickness of the intermediate layer (B) is preferably from 10 to 40 μm, and more preferably from 12 to 38 μm. The thickness of the sealing layer (C) is preferably from 5 to 35 μm, and more preferably from 7 to 30 μm.

[0060] In addition, when the sealing layer (C) is made up of multiple layers, preferably when it has a configuration such as surface layer (A) / intermediate layer (B) / sealing layer (C1) / sealing layer (C2), it is preferable that the total thickness of the sealing layers (C1 and C2) is within the thickness range of the above-mentioned sealing layer (C).

[0061] From the viewpoint of protecting the contents, the multilayer film of the present invention preferably has a seal strength of 5 N / 15 mm or more, and more preferably 10 N / 15 mm or more, when the seal layers (C) of the multilayer film are combined and heat-sealed under conditions of 100°C, 0.2 MPa, and 1 second with a seal width of 10 mm.

[0062] The multilayer film of the present invention preferably has an impact resistance of 0.5 J or more, more preferably 0.7 J or more, as measured by a film impact method. The impact strength is measured after conditioning a 40 μm multilayer film at −20° C.

[0063] The multilayer film of the present invention has a rigidity of preferably 200 to 400 MPa, and more preferably 220 to 380 MPa or more, because suitable flexibility can be easily obtained from the multilayer film.

[0064] In the multilayer film of the present invention, the difference between the melting point of the surface layer (A) and the melting point of the seal layer (C) is preferably 10° C. or more, more preferably 20° C. or more. By ensuring the melting point difference, it becomes easier to obtain suitable packaging suitability. The melting points of the surface layer (A), intermediate layer (B), and seal layer (C) are melting points calculated from the content and melting point of each resin component used in each layer. When the resins used in each layer are resin a, resin b, resin c, etc., where the melting points of these resins are Ta, Tb, Tc, etc., and the masses of the resins used in the layers are Wa, Wb, Wc, etc., the melting points are calculated as (TaWa+TbWb+TcWc...) / (Wa+Wb+Wc...).

[0065] When the melting point of the surface layer (A) of the multilayer film of the present invention is A°C, the melting point of the intermediate layer (B) is B°C, and the melting point of the seal layer (C) is C°C, the multilayer film of the present invention satisfies the following calculation formula. A≧B>C By adjusting the melting point of each layer as described above, it is possible to create a difference in melting point between the surface layer (A) and the sealing layer (C), improving suitability for packaging machines. In addition, the interlayer adhesion between the surface layer (A), the intermediate layer (B), and the sealing layer (C) is improved, improving low temperature resistance and sealing strength.

[0066] The multilayer film of the present invention has a high density polyethylene content of 5 to 40% by mass relative to the entire multilayer film. This range of high density polyethylene content is preferable because suitable seal strength and packaging suitability can be obtained. The high density polyethylene content of the entire multilayer film is preferably 7 to 35% by mass, more preferably 8 to 31% by mass, and even more preferably 10 to 26% by mass.

[0067] The multilayer film of the present invention has a medium-density polyethylene content of 28 to 72% by mass relative to the entire multilayer film. This range of medium-density polyethylene content is preferable because suitable seal strength, packaging suitability, and impact resistance can be obtained. The medium-density polyethylene content of the entire multilayer film is preferably 31 to 64% by mass, more preferably 34 to 56% by mass, and even more preferably 34 to 52% by mass.

[0068] The multilayer film of the present invention can maintain a low amount of short-chain branching of polyethylene while controlling the melting point and rigidity by setting the content of high-density polyethylene and medium-density polyethylene in the entire multilayer film within a specific range, which improves the performance of the packaging material, such as seal strength, packaging suitability, and impact resistance, as well as the accuracy of measuring the polyethylene ratio by IR for a recycled material in which a polypropylene resin and the multilayer film are mixed.

[0069] The method for producing the multilayer film of the present invention is not particularly limited, but examples thereof include a coextrusion method in which each resin or resin mixture used for the surface layer (A), intermediate layer (B), and seal layer (C) is heated and melted in a separate extruder, and laminated in the molten state in the order of, for example, (A) / (B) / (C) by a method such as a coextrusion multilayer die method or a feed block method, and then formed into a film by an inflation method, a T-die chill roll method, or the like. This co-extrusion method is preferable because it allows relatively free adjustment of the thickness ratio of each layer, and it can provide a multi-layer film that is excellent in hygiene and cost performance.

[0070] In addition, for applications in which transparency is not required or where a luxurious design is required, the multilayer film of the present invention may be a matte multilayer film in which an uneven structure is formed on the film surface by pressure molding using a chill roll having an uneven structure in the above-mentioned coextrusion method. For example, each resin or resin mixture used for the surface layer (A), intermediate layer (B), and seal layer (C) is heated and melted in a separate extruder, and the thermoplastic resin extruded in a molten state from a T-die in the order of (A) / (B) / (C) by a method such as a multilayer coextrusion die method or a feed block method is pressure molded by a chill roll having a concave-convex structure to form a concave-convex structure on the film surface, thereby forming a multilayer film having a concave-convex structure. This method imparts a matte design to the multilayer film while simplifying the manufacturing process and reducing costs by performing shaping simultaneously with film molding, with little environmental impact.

[0071] When the multilayer film of the present invention is a multilayer film having a concave-convex structure, the specific surface area of ​​the surface of the seal layer (C) side of the multilayer film is preferably 1.02 or more. By making such a multilayer film, a high-class matte design can be obtained even though it is a mono-material film. Here, the specific surface area refers to the average value of the S / A specific surface area measured three times under the following measurement conditions using a non-contact surface / layer cross-sectional shape measurement system VertScan (registered trademark) 2.0 (model number: R3300G Lite, manufactured by Ryoka Systems Co., Ltd.). -Measurement conditions- Camera: XC-HR50, equipped with 1 / 3-inch IT progressive scan CCD (Manufactured by Sony Corporation) Objective lens: 5x - Tube: Monocular tube Wavelength filter: 520nm Surface measurement mode: Phase Field of view size: 640×480 pixels

[0072] The specific surface area of ​​the seal layer (C) side surface of the multilayer film is preferably 1.02 or more, more preferably 1.03 or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 1.30 or less, more preferably 1.10 or less. If the specific surface area is within the above range, pressure molding using a chill roll having an uneven structure may be performed on the seal layer (C) side surface of the multilayer film or on the surface layer (A) side surface of the multilayer film.

[0073] The multilayer film of the present invention can be obtained as a substantially unstretched multilayer film by the above-mentioned production method, and therefore can be subjected to secondary forming such as deep drawing by vacuum forming.

[0074] Furthermore, in order to improve adhesion to printing ink and lamination suitability when used as a sealant film for lamination, it is preferable to subject the resin layer (A) to a surface treatment. Examples of such surface treatments include surface oxidation treatments such as corona treatment, plasma treatment, chromic acid treatment, flame treatment, hot air treatment, and ozone / ultraviolet treatment, as well as surface roughening treatments such as sandblasting, with corona treatment being preferred.

[0075] [Packaging material] Examples of packaging materials made of the multilayer film of the present invention include packaging bags and packaging containers used for food, medicines, industrial parts, miscellaneous goods, magazines, etc. In particular, since the film has excellent impact resistance at very low temperatures, it can be suitably used for packaging materials for frozen foods, frozen lunches, refrigerated foods, and medical products that are distributed at low temperatures.

[0076] The packaging bag is preferably a packaging bag formed by overlapping and sealing the seal layers (C) of the multilayer film of the present invention. It is also preferable that the packaging bag is a packaging bag formed by overlapping and sealing the seal layer (C) and the surface layer (A) of the multilayer film of the present invention. For example, two sheets of the multilayer film can be cut to the desired size of a packaging bag, stacked on top of each other and sealed on three sides to form a bag, after which the contents can be filled in through the unsealed side and the unsealed side can be sealed to use as a packaging bag. Furthermore, it is also possible to form a packaging bag by sealing the ends of a rolled film into a cylindrical shape using an automatic packaging machine, and then sealing the top and bottom. The sealing method is not particularly limited, and may be heat sealing or ultrasonic sealing. The method of ultrasonic sealing is not particularly limited, and may be appropriately selected from known ultrasonic sealing methods and methods using known ultrasonic sealing devices according to the purpose.

[0077] It is also possible to form a packaging bag or container by overlapping and sealing another sealable film with the sealing layer (C). In this case, the other film to be used may be a film of LDPE, EVA or the like, which has a relatively low mechanical strength.

[0078] The multilayer film of the present invention can also be used by laminating it to another substrate. The other substrate that can be used in this case is not particularly limited, but from the viewpoint of easily realizing the effects of the present invention, it is preferable to use a plastic substrate having high rigidity and high gloss, in particular a stretched resin film. In addition, for applications where transparency is not required, aluminum foil can be used alone or in combination.

[0079] Examples of the stretched resin film include biaxially oriented polyester (PET), easily tearable biaxially oriented polyester (PET), biaxially oriented polypropylene (OPP), biaxially oriented polyamide (PA), coextruded biaxially oriented polypropylene with an ethylene-vinyl alcohol copolymer (EVOH) as the central layer, biaxially oriented ethylene-vinyl alcohol copolymer (EVOH), and coextruded biaxially oriented polypropylene coated with polyvinylidene chloride (PVDC). These may be used alone or in combination.

[0080] Examples of the lamination method when the multilayer film of the present invention obtained by the above-mentioned production method is laminated with the above-mentioned substrate to form a laminate film include dry lamination, wet lamination, non-solvent lamination, extrusion lamination, etc. In this case, the layer of adhesive located between the multilayer film and the substrate is called an adhesive layer.

[0081] Examples of adhesives used in the dry lamination include solvent-based two-component curing adhesives, etc. The term "solvent-based" adhesive refers to a form used in a so-called dry lamination method, in which the adhesive is applied to a substrate, heated in an oven or the like to volatilize the organic solvent in the coating, and then laminated to another substrate, and includes a polyisocyanate composition, a polyol composition, and an organic solvent capable of dissolving (diluting) them.

[0082] In the above two-component curing adhesive, in consideration of the creation of a recycling-based society that should develop in a sustainable manner (sustainability), it is preferable to use plant-derived raw materials (biomass raw materials) as raw materials for the polyisocyanate composition or polyol composition. The biomass degree can be increased by appropriately using a biomass raw material. Examples of the biomass raw material include castor oil-based polyols such as castor oil, dehydrated castor oil, hydrogenated castor oil, and 5-50 mol alkylene oxide adducts of castor oil, as well as aliphatic polybasic acids such as succinic acid, succinic anhydride, glutaric acid, adipic acid, azelaic acid, sebacic acid, and itaconic acid, and alkyl esters of the acids, and dimer acids.

[0083] Commercially available biomass adhesives may be used, such as adhesives listed in the Japan Organic Resources Association, such as DIC Dry BM (DIC Corporation) and Takenate BM (Mitsui Chemicals, Inc.).

[0084] The weight of the adhesive layer after drying is 0.1 to 10 g / m 2 is preferably 1 to 6 g / m 2 More preferably, the thickness is 2 to 5 g / m 2 The thickness of the adhesive layer is preferably from 0.1 to 10 μm, more preferably from 1 to 7 μm, and even more preferably from 2 to 5 μm.

[0085] In addition, various adhesives can be used for the adhesive layer, but it is preferable to use a pressure-sensitive adhesive. Examples of pressure-sensitive adhesives include rubber-based adhesives obtained by dissolving polyisobutylene rubber, butyl rubber, or mixtures thereof in organic solvents such as benzene, toluene, xylene, or hexane; or these rubber-based adhesives blended with tackifiers such as abiethylene acid rosin ester, terpene-phenol copolymer, or terpene-indene copolymer; and acrylic-based adhesives obtained by dissolving acrylic copolymers with a glass transition point of -20°C or less, such as 2-ethylhexyl acrylate-n-butyl acrylate copolymer or 2-ethylhexyl acrylate-ethyl acrylate-methyl methacrylate copolymer, in an organic solvent.

[0086] In packaging materials using the multilayer film of the present invention, it is preferable to form any tear initiation portion such as a V notch, an I notch, a perforation, or a microhole in the sealed portion in order to weaken the initial tear strength and improve the ease of opening.

[0087] The multilayer film of the present invention may further have a printing layer on the surface layer (A). The printing layer is a layer on which a desired pattern is formed by liquid printing ink in order to impart cosmetic properties, various information related to the contents, and functionality to the printed material. The printing layer is formed by printing a gravure printing ink or a flexographic printing ink (hereinafter referred to as liquid printing ink) containing a binder resin and a colorant, or an inkjet ink. The printing layer may be a single layer or may have multiple printing layers. When there are multiple printing layers, the liquid printing ink used for each printing layer may be the same, may have the same composition but only the colorant is different, or may have different compositions. In addition, printing using a combination of liquid printing ink and inkjet ink may be used.

[0088] The liquid printing inks are used as gravure printing inks or flexographic printing inks, and are roughly divided into organic solvent-based liquid printing inks that use organic solvents as the main solvent, and water-based liquid printing inks that use water as the main solvent. The printing layer formed on the multilayer film of the present invention is preferably a general-purpose organic solvent-based liquid printing ink.

[0089] The organic solvent-based liquid printing ink is prepared by dispersing a mixture of pigment, binder resin, organic solvent medium, dispersant, defoamer, etc., in a dispersing machine to obtain a pigment dispersion. The pigment dispersion is then mixed with resin, aqueous medium, and, if necessary, additives such as a leveling agent, and then stirred. The ink is produced using a dispersing machine such as a bead mill, Eiger mill, sand mill, gamma mill, or attritor, which are commonly used in the production of gravure and flexographic printing inks.

[0090] Examples of the binder resin include cellulose-based resins such as cellulose nitrate, cellulose acetate propionate (CAP) and cellulose acetate butyronate (CAB), and other cellulose-based resins; polyamide-based resins, urethane-based resins, acrylic-based resins, vinyl chloride-vinyl acetate copolymer resins, chlorinated polypropylene resins, ethylene-vinyl acetate copolymer resins, vinyl acetate resins, polyvinyl chloride resins, and other vinyl chloride resins; polyester resins, alkyd resins, rosin-based resins, rosin-modified maleic acid resins, ketone resins, cyclized rubber, chlorinated rubber, butyral, and petroleum resins.

[0091] Examples of the pigment include inorganic pigments and organic pigments that are used in general inks, paints, and recording agents, etc. Examples of the organic pigment include soluble azo-based, insoluble azo-based, azo-based, phthalocyanine-based, halogenated phthalocyanine-based, anthraquinone-based, anthanthrone-based, dianthraquinonyl-based, anthrapyrimidine-based, perylene-based, perinone-based, quinacridone-based, thioindigo-based, dioxazine-based, isoindolinone-based, quinophthalone-based, azomethine azo-based, flavanthrone-based, diketopyrrolopyrrole-based, isoindoline-based, indanthrone-based, carbon black-based, and other pigments. In addition, for example, carmine 6B, lake red C, permanent red 2B, disazo yellow, pyrazolone orange, carmine FB, chromophthalic yellow, chromophthalic red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, aniline black, diketopyrrolopyrrole red, daylight fluorescent pigments, etc. can be mentioned. In addition, both non-acid-treated pigments and acid-treated pigments can be used. Examples of inorganic pigments include white inorganic pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silica, litbon, antimony white, and gypsum. Among inorganic pigments, the use of titanium oxide is particularly preferred. Titanium oxide is white in color and is preferred from the standpoints of coloring power, hiding power, chemical resistance, and weather resistance, and from the standpoint of printing performance, the titanium oxide is preferably treated with silica and / or alumina.

[0092] Examples of inorganic pigments other than white include aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, and zircon. Aluminum is in powder or paste form, but it is preferable to use it in paste form from the standpoint of handleability and safety. Whether leafing or non-leafing aluminum is used is appropriately selected from the standpoint of brightness and concentration.

[0093] The organic solvent-based liquid printing ink has excellent adhesion to various substrates and can be used for printing on paper, synthetic paper, thermoplastic resin films, plastic products, steel plates, etc., and is useful as an ink for gravure printing using a gravure printing plate made by electronic engraving or the like, or for flexographic printing using a flexographic printing plate made by a resin plate or the like. The thickness of the liquid printing ink formed by the gravure printing method or the flexographic printing method using the organic solvent-based liquid printing ink is preferably 0.1 to 10 μm, more preferably 1 to 5 μm, and even more preferably 1 to 3 μm. The weight of the printed layer after drying is 0.1 to 10 g / m 2 is preferably 1 to 5 g / m 2 More preferably, it is 1 to 3 g / m 2 It is even more preferable that:

[0094] In the above liquid printing ink, in consideration of the establishment of a recycling-based society that should develop in a sustainable manner (sustainability), it is preferable to use a liquid printing ink that uses raw materials derived from plants (biomass raw materials). Examples of plant-derived raw materials include cellulose resins such as cellulose acetate propionate resin and nitrocellulose; polyamide resins using dimer acids or polymerized fatty acids derived from natural oils such as soybean oil, palm oil, and rice bran oil; polycarboxylic acids such as succinic acid, succinic anhydride, adipic acid, azelaic acid, sebacic acid, dimer acid, glutaric acid, and malic acid; polyols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, pentylene glycol, 1,10-dodecanediol, dimer diol, and isosorbide; and polyisocyanates such as 1,5-pentamethylene diisocyanate and dimer diisocyanate. These polycarboxylic acids include biomass polyurethanes synthesized from plant-derived raw materials, rosin resins, dammar resins, and polylactic acid.

[0095] The liquid printing ink using the above-mentioned plant-derived raw materials can be a commercially available product. Examples of commercially available products include inks listed in the Japan Organic Resources Association, such as Glossa BM, Raizin, Ultima, Finart BM (all manufactured by DIC Corporation), Rotobio (manufactured by Sakata Inx Corporation), PANNECO, Real NEX BO, FB King X (all manufactured by Toyo Ink Co., Ltd.), NT-VESTA, and PULPTECC (both manufactured by Tokyo Ink Co., Ltd.).

[0096] The above-mentioned printed layer may be printed directly onto the surface layer (A) of the multilayer film of the present invention, a so-called surface printing method, or may be printed onto another substrate, a so-called reverse printing method, and then the substrate and the multilayer film of the present invention are laminated by dry lamination.

[0097] [Recycled materials] Even if the multilayer film of the present invention is collected as a recycled material and mixed with a polypropylene-based resin film, the mixing ratio with the polypropylene-based resin can be easily and accurately determined by composition analysis using a simple quantitative method such as infrared spectroscopy (IR) or differential scanning calorimetry (DSC). Therefore, it is possible to promote the advanced use of recycled materials and contribute to the realization of a recycling-oriented society.

[0098] The mixed ratio of the recycled material in which the multilayer film of the present invention and the polypropylene resin are mixed can be determined by measuring with infrared spectroscopy (IR). Specifically, the polyethylene (multilayer film of the present invention) ratio of the recycled material can be calculated by the following procedure based on the method described in Gifu Prefectural Industrial Technology Center Research Report No. 13 pp10-13 (2019).

[0099] Infrared spectroscopy: Measured using FT / IR-4100 manufactured by JASCO Corporation. -1 The peak height of 841 cm was determined as the polyethylene peak. -1 The peak height of this peak is taken as the peak derived from polypropylene. Here, in the literature, "719 cm -1 Peak height: 841cm -1 The polyethylene mixing ratio is calculated based on a calibration curve of "(intensity ratio) = 0.0444 × (polyethylene mixing ratio)" using "peak height of the peak at the peak of the polyethylene mixed ratio" as an intensity ratio. However, the inventors' investigations revealed that this calibration curve has a large error when the polyethylene ratio is relatively high. Therefore, the inventors investigated a calibration curve with good accuracy and found that -1 Peak height / (841cm -1 Peak height +719cm -1 The polyethylene mixing ratio calculated from this formula is the polyethylene ratio of the recycled material.

[0100] The linear approximation formula described in Gifu Prefectural Industrial Technology Center Research Report No. 13 pp10-13 (2019) has been verified when the polyethylene ratio in a mixture of polyethylene and polypropylene is 5 to 50 mass%, but has not been verified when the polyethylene ratio exceeds 50 mass%. Furthermore, the inventors have found through their studies that the accuracy drops significantly when the polyethylene ratio is 70 mass% or more. On the other hand, the exponential approximation equation discovered by the inventors can specify the polyethylene ratio with good accuracy even when the polyethylene ratio is low, and can specify the polyethylene ratio with good accuracy even when the polyethylene ratio is 70 mass% or more.

[0101] The multilayer film of the present invention uses a small amount of low-density polyethylene, which reduces the accuracy of measuring the polyethylene ratio of recycled materials mixed with polypropylene-based resins, and therefore the accuracy of measuring the polyethylene ratio of the recycled materials is relatively good. Moreover, the multilayer film can achieve both packaging suitability and interlayer adhesive strength as well as excellent accuracy of measuring the polyethylene ratio by adjusting physical properties such as melting point and rigidity using a combination of high-density polyethylene and medium-density polyethylene. EXAMPLES

[0102] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the contents of the examples. Unless otherwise specified, "parts" and "%" below are based on mass.

[0103] Example 1 The following resins were used as the resin components forming the surface layer (A), intermediate layer (B) and seal layer (C) to prepare resins and resin mixtures forming each layer. These resins and resin mixtures were fed to three extruders and melted at 250°C. The molten resin was fed into a T-die / chill roll method coextrusion multilayer film manufacturing apparatus equipped with a feed block (feed block and T-die temperature: 250°C) and co-melt extrusion was carried out to obtain a multilayer film having a three-layer structure of surface layer (A) / middle layer (B) / seal layer (C), with thicknesses of 10 μm / 23 μm / 17 μm (total 50 μm).

[0104] Surface layer (A): Medium density polyethylene (density: 0.933 g / cm 3 , MFR (190°C, 21.18N): 4g / 10min, melting point: 122°C) (hereinafter referred to as "MDPE (1)") 60 parts by mass, high-density polyethylene (density: 0.960g / cm 3 , MFR (190°C, 21.18N): 8g / 10min, melting point: 134°C) (hereinafter referred to as "HDPE") 40 parts by mass Intermediate layer (B): 70 parts by mass of MDPE, 30 parts by mass of HDPE Sealing layer (C): Linear low-density polyethylene (density: 0.905 g / cm 3 , MFR (190°C, 21.18N): 4g / 10min, melting point (peak with largest endothermic amount): 89°C) (hereinafter referred to as "LLDPE") 100 parts by mass

[0105] (Examples 2 to 6) Multilayer films of Examples 2 to 6 were obtained in the same manner as in Example 1, except that the compounding ratio and layer thickness of each layer were changed as shown in Table 1.

[0106] Example 7 After co-melt extrusion was carried out in the same manner as in Example 1, the film was pressurized and cooled using a chill roll having an uneven structure at 40°C to obtain a matte multilayer film having a three-layer structure of a surface layer (A) / middle layer (B) / sealing layer (C), with average thicknesses of the layers being 10 μm / 23 μm / 17 μm (total 50 μm).

[0107] (Examples 8 to 10) Matte multilayer films of Examples 8 to 10 were obtained in the same manner as in Example 7, except that the compounding ratio and layer thickness of each layer were changed as shown in Table 2.

[0108] (Comparative Examples 1 to 2) A multilayer film of Comparative Example 1 was obtained in the same manner as in Example 1, except that the compounding ratio and layer thickness of each layer were changed as shown in Table 2.

[0109] [Surface roughness measurement] For the obtained coextruded film, the surface roughness (RzJIS) of the surface of the seal layer (A) was measured (unit: μm) using a non-contact surface / layer cross-sectional shape measuring system VertScan (registered trademark) 2.0 (model number: R3300G Lite, manufactured by Ryoka Systems Co., Ltd.).

[0110] [Measurement of specific surface area] For the obtained coextruded film, the specific surface area (S / A) of the surface of the seal layer (A) was measured using a non-contact surface / layer cross-sectional shape measuring system VertScan (registered trademark) 2.0 (model number: R3300G Lite, manufactured by Ryoka Systems Co., Ltd.).

[0111] [Haze measurement] The haze of the films obtained in the above examples and comparative examples was measured using a haze meter (NDH5000) manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K7105.

[0112] [Gloss measurement] The gloss of the films obtained in the above examples and comparative examples was measured using a gloss meter (VG-2000) manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS Z8741.

[0113] [Measurement of stiffness] The films obtained in the examples and comparative examples were cut into a size of 300 mm length x 25.4 mm width (200 mm interval between marks) with the longitudinal direction being the flow direction of the film (machine direction) to obtain test pieces with a thickness of 30 μm. The 1% tangent modulus (unit: MPa) at 23°C was measured at a tensile speed of 500 mm / min in accordance with ASTM D-882 using a Tensilon tensile tester (manufactured by A&D Co., Ltd.).

[0114] [Heat seal strength] Using the films obtained in the Examples and Comparative Examples, test pieces were prepared by heat sealing at 100°C, 0.2 MPa, and 1 second to a seal width of 10 mm. These were then cut to a width of 15 mm, and the heat seal strength (unit: N / 15 mm) was measured using a tensile tester. The same evaluation was carried out three times, and the average value was used as the evaluation result. ○: Heat seal strength is 5N / 15mm or more ×: Heat seal strength is less than 5N / 15mm

[0115] [Impact resistance] The films obtained in the Examples and Comparative Examples were left to stand in a thermostatic chamber adjusted to -20°C for 4 hours to prepare test specimens. For each test piece, a BU-302 film impact tester manufactured by Tester Sangyo was used, with a 1.0 inch head attached to the tip of the pendulum, to measure the impact strength by the film impact method. ○: Impact strength is 0.70(J) or more ×: Impact strength is less than 0.70 (J)

[0116] [Packaging machine suitability] The multilayer films prepared in the Examples and Comparative Examples were wrapped in vertical pillow bags using an automatic packaging machine as described below, and the bags were evaluated as follows. Packaging machine: DAIKEN DK2400 Horizontal sealing: speed 32 bags / min, vertical heat seal temperature 140°C, horizontal heat seal temperature 100°C to 140°C changed in 10°C increments to seal the seal layers (C) together. The appearance of the sealed parts of the flat bags which had been horizontally (palm-seamed) sealed and vertically sealed at each horizontal heat seal temperature was observed and evaluated based on shrinkage, the state of fusion of the film to the heat seal bar, and the degree of wrinkling. ○: No shrinkage of the seal, adhesion to the seal bar, or wrinkles △: Some shrinkage of the seal area, adhesion to the seal bar, wrinkles, etc. ×: Shrinkage of the seal part, adhesion to the seal bar, wrinkles, etc.

[0117] [IR polyethylene ratio measurement results for multi-layer film and polypropylene mixed recycled material] The multilayer films obtained in the examples and comparative examples were crushed and melt-extruded pellets were mixed with polypropylene homopolymer pellets to prepare monolayer films (weight ratio of polypropylene = 50:50 and 70:30). The obtained monolayer film samples simulating the recycled materials were subjected to infrared spectroscopy. The infrared spectroscopy was performed using FT / IR-4100 manufactured by JASCO Corporation, and the film sample was measured five times at different locations. In the obtained absorbance spectrum, the peak intensity of polyethylene was determined as "peak height at 719 cm-1 / (peak height at 841 cm-1+peak height at 719 cm-1)", and the polyethylene mixing ratio was calculated based on "(polyethylene mixing ratio) = 4.2866 × exp (3.5636 × (peak intensity of polyethylene))", and the average value of the five measurements was used as the polyethylene ratio of the recycled material. Evaluation was performed according to the following criteria. Each peak height was calculated by setting a baseline. ◎: The measurement result of the polyethylene ratio of recycled materials is within ±3% by mass of the actual mixture ratio. 〇: The measurement result of the polyethylene ratio of recycled materials is within ±5% of the actual mixture ratio, exceeding ±3% by mass. △: The measurement result of the polyethylene ratio of recycled materials is within ±10% of the actual mixture ratio, exceeding ±5% by mass. ×: The measurement result of the polyethylene ratio of the recycled material is more than ±10% by mass of the actual mixture ratio. For example, when the actual mixing ratio of multilayer film:polypropylene was 50:50, the measurement result of the polyethylene ratio of the recycled material was 65 mass %, it was evaluated as Δ.

[0118] The results obtained above are shown in Tables 1 and 2.

[0119] [Table 1]

[0120] [Table 2]

[0121] The resins used in the table are shown below. MDPE (1) Medium density polyethylene (density: 0.933 g / cm 3 , MFR(190℃, 21.18N):4g / 10min, Melting point:122℃ MDPE (2) Medium density polyethylene (density: 0.931 g / cm 3 , MFR(190℃, 21.18N):4g / 10min, Melting point:123℃ HDPE: High density polyethylene (density: 0.960g / cm 3 , MFR(190℃, 21.18N):8g / 10min, Melting point:134℃ LLDPE: Linear low-density polyethylene (density: 0.905 g / cm 3 , MFR (190℃, 21.18N): 4g / 10min, Melting point (peak with largest endothermic heat): 89℃ LDPE: Low density polyethylene (density: 0.922 g / cm 3 , MFR(190℃, 21.18N):5g / 10min, Melting point:108℃

[0122] As is clear from the above table, the multilayer films of the present invention in Examples 1 to 10 had suitable rigidity, excellent impact resistance at a very low temperature of -20°C, and excellent suitability for packaging machines. In addition, since they are monomaterials of polyethylene resins, they are easy to recycle. Furthermore, the polyethylene ratios measured by IR for the recycled materials consisting of mixtures of the multilayer films and polypropylene in Examples 1 and 5 to 7 were close to the actual mixture ratios, and even when mixed with polypropylene, the polyethylene ratio was easily identified by infrared spectroscopy, which was advantageous for the advanced utilization of the recycled materials. On the other hand, the multilayer film of Comparative Example 1 was a low-density polyethylene film, and therefore had poor suitability for packaging machines. Also, the polyethylene ratio measured by IR was far from the actual mixing ratio, and even when mixed with polypropylene, the polyethylene ratio could not be accurately determined by infrared spectroscopy. Also, the multilayer film of Comparative Example 2 had a low content of high-density polyethylene, and therefore the polyethylene ratio measured by IR was somewhat far from the actual mixing ratio, and even when mixed with polypropylene, the polyethylene ratio could not be accurately determined by infrared spectroscopy.

Claims

1. A multilayer film having at least a surface layer (A), an intermediate layer (B) and a seal layer (C) laminated in this order, Among the components contained in the multilayer film, 90% by mass or more is a polyethylene-based resin, The content of high density polyethylene in the entire multilayer film is 5 to 40 mass%; The content of medium density polyethylene in the entire multilayer film is 28 to 72 mass%; A multilayer film that satisfies the following formula, where A°C is the melting point of the surface layer (A), B°C is the melting point of the intermediate layer (B), and C°C is the melting point of the seal layer (C). A ≧ B > C

2. The multilayer film according to claim 1, wherein the total thickness of the multilayer film is in the range of 20 to 90 μm.

3. 2. The multilayer film according to claim 1, wherein the multilayer film has an impact strength of 0.7 J or more at −20° C.

4. The multilayer film according to claim 1 , wherein the specific surface area of ​​the surface of the multilayer film on the side of the seal layer (C) is 1.02 or more.

5. A packaging material using the multilayer film according to any one of claims 1 to 4.