Method for manufacturing carbon support, carbon support produced by the same, and electrode catalyst of fuel cell uses thereof

By extracting aromatic carbon materials from hydrocarbon raw materials and heat-treating at lower temperatures, the method enhances the crystallinity and durability of carbon supports, addressing the inefficiencies of high-temperature processes and improving fuel cell catalyst performance.

KR103042149B1Active Publication Date: 2026-11-06KOREA INST OF SCI & TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230105536
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2026-11-06
Estimated Expiration
2043-08-11

AI Technical Summary

Technical Problem

Existing methods for manufacturing crystalline carbon supports for fuel cells are costly and inefficient due to the use of high-temperature processes, leading to reduced catalytic activity and durability issues.

Method used

A method involving the extraction of aromatic carbon materials from aromatic hydrocarbon raw materials using organic solvents, followed by mixing with a carbon support and heat-treating at lower temperatures to improve crystallinity, thereby enhancing the carbon support's durability and catalytic activity.

Benefits of technology

The method improves the crystallinity of carbon supports at lower temperatures, preventing degradation and increasing the durability of fuel cell catalysts, making them more commercially viable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure R1020230105536_ABST
    Figure R1020230105536_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a crystalline carbon support, a crystalline carbon support according to the same, and a fuel cell catalyst comprising the same. The manufacturing method of the present invention can improve the crystallinity of the carbon support even at relatively low temperatures, thereby solving the problem of the surface of the carbon support becoming smooth, which is not only limited to commercialization due to conventional high-temperature heat treatment. In addition, the crystalline carbon support according to the present invention can improve the durability of the electrode catalyst and the lifespan of the fuel cell using it by preventing the degradation of the electrode catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a crystalline carbon support, a crystalline carbon support according to the same, and a catalyst for a fuel cell comprising the same. Background Technology

[0002] Polymer Electrolyte Membrane Fuel Cells (PEMFCs) are power generation systems that produce electricity through the electrochemical reaction of hydrogen and oxygen using a catalyst. They feature a structure in which a cation exchange membrane is inserted between the oxidation electrode (hereinafter anode) and the reduction electrode (hereinafter cathode), and as they can be applied to transportation vehicles, high demand is predicted for them in the future.

[0003] However, commercialization is difficult for fuel cells used in transportation because they require durability capable of operating for at least 8,000 hours. Accordingly, there have been attempts to overcome the low catalytic activity and durability of the oxygen reduction reaction.

[0004] Fuel cell catalysts are important factors determining the performance of fuel cells, and their activity is reduced due to the degradation of metal particles, such as platinum alone, platinum-based alloys, and non-platinum, and carbon supports (see Fig. 1). Accordingly, there have been many attempts to use (highly)crystalline carbon supports to suppress the degradation related to carbon.

[0005] Conventionally, to manufacture crystalline carbon supports, chemical vapor deposition of aromatic carbon materials (carbon precursors) performed at high temperatures or methods of growing carbon structures on pre-formed nanoparticles via arc discharge were used. However, these methods require expensive equipment and are uneconomical due to low yields, which limits their commercialization.

[0006] In addition, a method was used to manufacture a crystalline carbon support by mixing a metal catalyst with an aromatic carbon material (carbon precursor) and removing the metal catalyst after polymerization and carbonization processes; however, this method has the disadvantage of lowering the crystallinity of the carbon support, as it not only uses aromatic carbon materials (carbon precursors) that are harmful to the human body but also requires post-treatment in strong acids to remove the metal catalyst.

[0007] Against this backdrop, the inventors endeavored to develop a method for manufacturing a crystalline carbon support in an environmentally friendly and economical manner. As a result, they confirmed that the crystallinity of the carbon support can be improved even at relatively low temperatures when the carbon support is heat-treated together with an aromatic carbon material (carbon precursor) extracted from an aromatic hydrocarbon raw material, thereby completing the present invention. Prior art literature

[0008] (Patent Document 0001) KR 10-2034635 B The problem to be solved

[0009] The problem to be solved by the present invention is to provide a method for manufacturing a highly crystalline carbon support and a highly crystalline carbon support according to the same.

[0010] In addition, another problem to be solved by the present invention is to provide a highly durable fuel cell catalyst using the crystalline carbon support. means of solving the problem

[0011] The present invention, for achieving the above-mentioned purpose, relates to a method for manufacturing a crystalline carbon support comprising: (a) a step of extracting an aromatic carbon material by adding an organic solvent to an aromatic hydrocarbon raw material; (b) a step of forming an aromatic carbon material-carbon support composite by mixing a solution containing the aromatic carbon material and the organic solvent with a carbon support; and (c) a step of heat-treating the aromatic carbon material-carbon support composite.

[0012] In one embodiment of the present invention, the aromatic hydrocarbon raw material may be one or more selected from petroleum residue oil, petroleum pitch, coal residue oil, coal pitch, coal tar, coconut, and waste plastic.

[0013] In one embodiment of the present invention, the organic solvent may be one or more selected from hexane, toluene, tetrahydrofuran (THF), N-methyl-2-pyrrolidone (NMP), and dimethylformamide (DMF).

[0014] In one embodiment of the present invention, the aromatic carbon material may be a mixture of polycyclic aromatic hydrocarbons.

[0015] In one embodiment of the present invention, the aromatic carbon material may comprise a polycyclic aromatic hydrocarbon compound having a molecular weight of 10 to 10,000 m / z as measured by Matrix Assisted Laser Desorption Ionization Time of Flight (MALDI-TOF) mass spectrometry.

[0016] In one embodiment of the present invention, the carbon support may be one or more selected from carbon black, Ketjen black, carbon nanotube, graphene, graphene oxide, carbon nanofiber, and carbon nanospheres.

[0017] In one embodiment of the present invention, the heat treatment may be performed at 80 to 1600 ℃.

[0018] In one embodiment of the present invention, the aromatic hydrocarbon raw material is petroleum pitch, the organic solvent is dimethylformamide (DMF), the aromatic carbon material comprises a polycyclic aromatic hydrocarbon compound having a molecular weight of 10 to 10,000 m / z as measured by MALDI-TOF mass spectrometry, the carbon support is carbon black, and the heat treatment can be performed at 80 to 1600 ℃.

[0019] In addition, the present invention relates to a crystalline carbon support manufactured according to the above method.

[0020] In one embodiment of the present invention, the crystalline carbon support may have a specific surface area of ​​100 to 600 m² / g.

[0021] In one embodiment of the present invention, the crystalline carbon support may be a support for a fuel cell.

[0022] In addition, the present invention relates to a catalyst for a fuel cell comprising: the crystalline carbon support; and an active metal supported on the crystalline carbon support.

[0023] In one embodiment of the present invention, the active metal may be one or more selected from platinum, palladium, gold, silver, rhodium, iridium, ruthenium, osmium, cobalt, manganese, nickel, iron, chromium, molybdenum, and titanium. Effects of the invention

[0024] The manufacturing method of the present invention can improve the crystallinity of the carbon support even at relatively low temperatures, thereby solving the problem of the surface of the carbon support becoming smooth, which is not only limited to commercialization due to conventional high-temperature heat treatment.

[0025] In addition, the crystalline carbon support according to the present invention can improve the durability of the electrode catalyst and the lifespan of the fuel cell using it by preventing the degradation of the electrode catalyst. Brief explanation of the drawing

[0026] Figure 1 is a schematic diagram briefly illustrating the process of reduced activity and durability of a fuel cell catalyst due to the deterioration (corrosion) of a conventional carbon support. FIG. 2 is a schematic diagram briefly illustrating a method for controlling defects in existing commercial carbon supports using an aromatic carbon material (carbon precursor) extracted from an aromatic hydrocarbon raw material according to the present invention. FIG. 3 is a photograph showing a solution containing an aromatic carbon material extracted from an aromatic hydrocarbon raw material (petroleum pitch) and its respective solvent, according to one embodiment of the present invention. Here, “PCH” refers to a solution containing an aromatic carbon material in which the solvent is hexane, “PCT” refers to a solvent in which the solvent is toluene, “PCTe” refers to a solvent in which the solvent is tetrahydrofuran, “PCN” refers to a solvent in which the solvent is N-methyl-2-pyrrolidone, and “PCD” refers to a solvent in which the solvent is dimethylformamide. FIG. 4 is a photograph showing PCH extracted with hexane, a mixture (PCH-V) of the PCH and a commercial carbon support carbon black (Vulcan XC-72) mixed together, and a crystalline carbon support (PCH-Vh) prepared by heat-treating the PCH-V, according to one embodiment of the present invention. Figure 5 shows the results of electrochemical specific surface area (Initial EDLC) analysis of each ACM-carbon support composite ((a) PCH-V, (b) PCT-V, (c) PCTe-V, (d) PCN-V, and (e) PCD-V) prepared according to one embodiment of the present invention. Figure 6 shows the results of the electrochemical stability (EDLC change rate) analysis of each ACM-carbon support composite ((a) PCH-V, (b) PCT-V, (c) PCTe-V, (d) PCN-V, and (e) PCD-V) prepared according to one embodiment of the present invention. Figure 7 shows the results of electrochemical specific surface area (Initial EDLC) analysis of crystalline carbon supports prepared according to one embodiment of the present invention, PCH-Vh (Example 1), PCT-Vh (Example 2), PCTe-Vh (Example 3), PCN-Vh (Example 4) and PCD-Vh (Example 5). Figure 8 shows the results of the electrochemical stability (EDLC change rate) analysis of crystalline carbon supports prepared according to one embodiment of the present invention, PCH-Vh (Example 1), PCT-Vh (Example 2), PCTe-Vh (Example 3), PCN-Vh (Example 4) and PCD-Vh (Example 5). Figure 9 shows the BET analysis results of crystalline carbon supports prepared according to one embodiment of the present invention, namely PCH-Vh (Example 1), PCT-Vh (Example 2), PCTe-Vh (Example 3), PCN-Vh (Example 4) and PCD-Vh (Example 5). FIG. 10a is the XRD analysis result of PCD-Vh (Example 5), PCD-V, VC1000 (Comparative Example 2), and VC (Comparative Example 1) prepared according to one embodiment of the present invention, and FIG. 10b is the Raman analysis result of PCD-Vh (Example 5), PCD-V, VC1000 (Comparative Example 2), and VC (Comparative Example 1). FIG. 11 is a graph showing the results of comparing the change in electrical double layer capacitance (EDLC) calculated by performing NEDO protocol-based ADT on carbon black (Vulcan XC-72), carbon black heat-treated at 1000 ℃ (Vulcan XC-72 1000 ℃), the ACM-carbon support composite, and the heat-treated ACM-carbon support composite (crystalline carbon support) for each ACM sample ((a) PCH-V, (b) PCT-V, (c) PCTe-V, (d) PCN-V, and (e) PCD-V) prepared according to one embodiment of the present invention. Figure 12 is a TGA (thermogravimetric analysis) graph (left side of Figure 12) and a DTG (differential thermogravimetric analysis) graph (right side of Figure 12) for PCD-Vh prepared according to Example 5 of the present invention. Figure 13 is a graph showing the results of a comparative analysis of thermal oxidation resistance characteristics by performing TGA (thermogravimetric analysis) on PCD-Vh prepared according to Example 5 of the present invention and various commercial carbon supports. FIG. 14 is the result of analyzing the molecular weight (Mw) and molecular weight size distribution through Maldi-TOF analysis for each ACM sample ((Fig. 14a) PCH, (Fig. 14b) PCT, (Fig. 14c) PCTe, (Fig. 14d) PCN, and (Fig. 14e) PCD) extracted in one embodiment of the present invention. Figure 15 is the result of confirming structural characteristics by performing FT-IR analysis on a solution containing aromatic carbon materials (PCH, PCT, PCTe, PCN, and PCD) extracted from an aromatic hydrocarbon raw material (petroleum pitch) and their respective solvents, according to one embodiment of the present invention. FIG. 16 is a graph showing the change in the specific surface area (ECSA) and the change in the electric double layer capacitance (EDLC) of the platinum particles, observed according to an accelerated deactivation cycle, for a catalyst prepared by supporting platinum particles on PCD-Vh (PCD-V1000) prepared according to one embodiment of the present invention. Specific details for implementing the invention

[0027] The present invention will be described in detail below.

[0028] One aspect of the present invention relates to a method for manufacturing a crystalline carbon support comprising: (a) adding an organic solvent to an aromatic hydrocarbon raw material to extract an aromatic carbon material; (b) mixing a solution containing the aromatic carbon material and the organic solvent with a carbon support to form an aromatic carbon material-carbon support composite; and (c) heat-treating the aromatic carbon material-carbon support composite.

[0029] Conventionally, crystalline carbon supports are manufactured by high-temperature heat treatment of at least 1600°C or higher, which not only limits their commercialization but also causes a problem where the surface of the crystalline carbon support becomes smooth (a problem of a small specific surface area). When the surface of the crystalline carbon support is smooth in this way, it is difficult to disperse the active metal (catalyst) within the carbon support, and consequently, the active metal (catalyst) with a large particle size is supported, resulting in lower catalytic activity.

[0030] The method for manufacturing a crystalline carbon support according to the present invention can solve the problem of limited commercialization and the smoothing of the surface as described above by performing heat treatment at a relatively low temperature during the process of improving the crystallinity of the carbon support. The present invention can improve the crystallinity of the carbon support even at low temperatures by heat treating the carbon support together with an aromatic hydrocarbon compound extracted from an aromatic hydrocarbon raw material.

[0031] (a) Aromatic carbon material extraction step

[0032] (a) Step is to extract aromatic carbon materials by adding an organic solvent to the aromatic hydrocarbon raw material.

[0033] In the present invention, the term “aromatic hydrocarbon raw material” may be one or more selected from petroleum residue oil, petroleum pitch, coal residue oil, coal pitch, coal tar, coconut, and waste plastic as a feedstock for aromatic hydrocarbon compounds, preferably petroleum residue oil, petroleum pitch or coal pitch, and more preferably petroleum pitch.

[0034] In one embodiment, the petroleum residue oil may be one or more selected from pyrolysis fuel oil (PFO), heavy oil, extract heavy oil, vacuum redisue, atmospheric residue oil, naphtha cracking bottom oil (NCB), ethylene bottom oil (EBO), fluid catalytic cracking decanter oil (FCC-DO), residue fluid catalytic cracking decanter oil (RFCC-DO), aromatic extract (AE), and petroleum residue oil that has undergone hydrogenation treatment.

[0035] In one embodiment, the organic solvent may be a protic solvent such as IPA, acetone, or ethanol among polar solvents, or a non-protic solvent such as THF, DMF, or DMSO, or a non-polar solvent such as hexane, toluene, or benzene. The solvent of the present invention may be one or more selected from the above solvents.

[0036] In one embodiment, the amount of the organic solvent added may be 1 part by weight or more, preferably 1 to 500 parts by weight, and more preferably 1 to 300 parts by weight, per 100 parts by weight of the aromatic hydrocarbon raw material.

[0037] The more the amount of organic solvent added to the above aromatic hydrocarbon raw material, the greater the amount of aromatic carbon material extracted tends to be. If the amount is below the lower limit, the aromatic carbon material is not sufficiently extracted, and if the amount exceeds the upper limit, it is not economical.

[0038] In one embodiment, after adding the organic solvent to the aromatic hydrocarbon raw material, the aromatic carbon material can be extracted by heating in a water bath for 10 to 40 hours, preferably 15 to 35 hours, more preferably 20 to 30 hours, while stirring at 100 to 500 rpm, preferably 150 to 350 rpm, at a temperature of 20 to 40 ℃, preferably 25 to 35 ℃, more preferably 28 to 32 ℃.

[0039] In the present invention, the “aromatic carbon material” may also be referred to as an aromatic carbon component, an aromatic hydrocarbon component, an aromatic carbon fragment, an aromatic carbon residue, polycyclic aromatic hydrocarbons (PAHs), polycyclic aromatic hydrocarbon extracts, carbon dots, “aromatic carbon moiety (ACM),” or ACM. The ACM refers to a nanoscale carbon material having an aromatic ring in which the C=C and CC bonds of carbon atoms are hybridized.

[0040] In one embodiment, the ACM may be a mixture of polycyclic aromatic hydrocarbons.

[0041] The ACM mentioned above may vary depending on the type of aromatic hydrocarbon raw material and / or the organic solvent. In particular, the molecular weight of the extracted ACM varies depending on the type of organic solvent.

[0042] For example, if the organic solvent is hexane, a mixture of polycyclic aromatic hydrocarbons containing 6 to 13 carbon rings, preferably a mixture of polycyclic aromatic hydrocarbons containing 10 to 11 carbon rings (hereinafter referred to as 'PCH') may be extracted; if the organic solvent is toluene, a mixture of polycyclic aromatic hydrocarbons containing 5 to 17 carbon rings, preferably a mixture of polycyclic aromatic hydrocarbons containing 9 to 15 carbon rings (hereinafter referred to as 'PCT') may be extracted; if the organic solvent is tetrahydrofuran, a mixture of polycyclic aromatic hydrocarbons containing 7 to 18 carbon rings, preferably a mixture of polycyclic aromatic hydrocarbons containing 9 to 14 carbon rings (hereinafter referred to as 'PCTe') may be extracted; and if the organic solvent is N-methyl-2-pyrrolidone, 6 to A mixture of polycyclic aromatic hydrocarbons containing 18 carbon rings, preferably a mixture of polycyclic aromatic hydrocarbons containing 9 to 15 carbon rings (hereinafter referred to as 'PCN') can be extracted, and if the organic solvent is dimethylformamide, a mixture of polycyclic aromatic hydrocarbons containing 6 to 18 carbon rings, preferably a mixture of polycyclic aromatic hydrocarbons containing 9 to 15 carbon rings (hereinafter referred to as 'PCD') can be extracted.

[0043] In one embodiment, the ACM may comprise a polycyclic aromatic hydrocarbon compound having a molecular weight of 10 to 10,000 m / z, preferably 10 to 5,000 m / z, more preferably 10 to 2,000 m / z, more preferably 200 to 1,000 m / z, more preferably 300 to 700 m / z, more preferably 400 to 600 m / z, and more preferably 400 to 500 m / z as measured by Matrix Assisted Laser Desorption Ionization Time of Flight (MALDI-TOF) mass spectrometry.

[0044] In one specific example, the molecular weights of the above ACMs were compared using MALDI-TOF mass spectrometry, and it was specifically confirmed that the order was PCD, PCN, PCTe, PCT, and PCH.

[0045] In one embodiment, the molecular weight distribution measured by MALDI-TOF mass spectrometry of the ACMs was confirmed, and it was found that the smaller the molecular weight (Mw) value of the ACM, the narrower the molecular weight distribution, and the larger the molecular weight (Mw) value, the wider the molecular weight distribution.

[0046] In one embodiment, functional groups were identified by FT-IR analysis of the above ACMs, and it was confirmed that -COO groups were observed in PCH and PCTe, -OH groups were observed in PCH, PCN, and PCD, and C=C bonds were observed only in PCD.

[0047] (b) Aromatic carbon material-carbon support composite formation step

[0048] (b) Step is to mix a solution containing the aromatic carbon material (ACM) and an organic solvent with a carbon support to form an aromatic carbon material-carbon support composite.

[0049] In one embodiment, the carbon support may be a commercial carbon support.

[0050] The optimal mixing ratio of the above ACM may vary depending on the characteristics of the carbon material (carbon support), such as bonding, micropores, and specific surface area.

[0051] In one embodiment, the ACM may be 5 to 80 parts by weight, preferably 10 to 40 parts by weight, and more preferably 10 to 20 parts by weight, with respect to 100 parts by weight of a carbon support.

[0052] If the ratio of ACM to the carbon support is below the lower limit, defects in the carbon support cannot be healed, and if it exceeds the upper limit, the excess ACM added may oxidize and reduce durability.

[0053] In one embodiment, after adding the carbon support to the ACM-containing solution, the mixture can be stirred at room temperature at 100 to 500 rpm, preferably 200 to 400 rpm, for 6 hours or more, preferably 6 to 40 hours, more preferably 6 to 24 hours to form an aromatic carbon material-carbon support composite.

[0054] (c) Heat treatment step

[0055] Step (c) is a step of heat-treating the aromatic carbon material-carbon support composite. In the manufacturing method of the present invention, the aromatic carbon material-carbon support composite obtained in step (b) may have improved crystallinity compared to the carbon support, but crystallinity may be further improved by additionally performing the heat treatment step (c).

[0056] In one embodiment, the heat treatment may be performed at 80 to 1600 ℃, preferably 100 to 1400 ℃, more preferably 150 to 1200 ℃, more preferably 700 to 1200 ℃, more preferably 800 to 1100 ℃, and more preferably 900 to 1050 ℃ for 30 minutes to 3 hours.

[0057] If the above heat treatment temperature is below the above lower limit, a reaction between the ACM and the carbon support may not occur. Furthermore, if the above heat treatment temperature exceeds the above upper limit, expensive equipment for high-temperature heat treatment is required, which is not only uneconomical but also causes the functional groups present on the surface of the carbon support to disappear, failing to act as anchoring sites, which can lead to the easy detachment of active metals (e.g., platinum). Additionally, the specific surface area of ​​the crystalline carbon support is significantly reduced, and the ECSA may be significantly reduced due to the decrease in the pore structure.

[0058] In addition, in the case of a crystalline carbon support prepared by forming an aromatic carbon material-carbon support composite according to the present invention and then performing heat treatment within the above range, the specific surface area is reduced relatively less, and only micropores that are unfavorable to mass transfer and three-phase interfaces are blocked, thereby maintaining a high dispersion of active metals (e.g., platinum, etc.) and improving initial performance.

[0059] The method for manufacturing a crystalline carbon support according to the present invention described above does not require expensive equipment and is highly economical, making commercialization relatively easy.

[0060] Furthermore, according to the method for manufacturing a crystalline carbon support of the present invention described above, the crystallinity of the carbon support can be effectively improved even at relatively low temperatures, thereby solving various problems caused by conventional high-temperature heat treatment. In addition, the crystalline carbon support of the present invention manufactured according to the above method can significantly improve the durability of the electrode catalyst by preventing the degradation of the electrode catalyst.

[0061] Meanwhile, although not explicitly stated in the following examples, in the method for manufacturing a crystalline carbon support according to the present invention, platinum particles were supported on a crystalline carbon support prepared by varying the type of aromatic hydrocarbon raw material, whether it is an aromatic carbon material extracted from the aromatic hydrocarbon raw material, the type of organic solvent, and the heat treatment conditions, and then the surface of the catalyst was observed using a high-magnification TEM before and after 30,000 cycles.

[0062] As a result, unlike other conditions and different numerical ranges, when all of the following conditions were satisfied, it was confirmed that metal particles exhibiting oxygen reduction activity were evenly supported within the catalyst without clumping, and that the number of pores or the volume of pores on the catalyst surface were further reduced. In addition, it was confirmed that the electrode coated with the catalyst exhibited a uniform and stable electrode surface state even after 30,000 cycles were performed in the same manner as the experimental example below (durability evaluation experiment).

[0063] However, if any of the following conditions are not satisfied, it was observed that some metal particles exhibiting oxygen reduction activity were aggregated and supported within the catalyst after 30,000 cycles.

[0064] A method for manufacturing a crystalline carbon support according to the present invention, wherein ① the aromatic hydrocarbon raw material is petroleum pitch, ② the organic solvent is dimethylformamide, ③ the aromatic carbon material comprises a polycyclic aromatic hydrocarbon compound having a molecular weight of 300 to 600 m / z as measured by MALDI-TOF mass spectrometry, ④ the carbon support is carbon black, and ⑤ the heat treatment is performed at 950 to 1050 ℃.

[0066] Another aspect of the present invention relates to a crystalline carbon support manufactured according to the above method.

[0067] In one embodiment, the crystalline carbon support may have a specific surface area of ​​100 to 600 m² / g, preferably 300 to 600 m² / g.

[0068] When the crystalline carbon support of the present invention is used as a support for a fuel cell, if its specific surface area is less than the lower limit, the dispersibility of the active metal supported on the carbon support is reduced, and as a result, the activity of the catalyst may be reduced, and if it exceeds the upper limit, the active metal supported in micropores where mass transfer is not easy increases, and the performance of the catalyst may decrease.

[0069] In one embodiment, the crystalline carbon support may be a support for a fuel cell.

[0071] Another aspect of the present invention relates to a catalyst for a fuel cell comprising: the crystalline carbon support above; and an active metal supported on the crystalline carbon support.

[0072] The catalyst for a fuel cell according to the present invention is formed by efficiently dispersing active metal particles, such as platinum particles of appropriate size, on a crystalline carbon support of the present invention, so the catalytic activity is improved, and the overall characteristics of the fuel cell using the same can be improved.

[0073] In one embodiment, the active metal may be one or more selected from platinum, palladium, gold, silver, rhodium, iridium, ruthenium, osmium, cobalt, manganese, nickel, iron, chromium, molybdenum, and titanium.

[0075] Another aspect of the present invention relates to an electric device comprising a catalyst comprising the crystalline carbon support; and an active metal supported on the crystalline carbon support.

[0076] In one embodiment, the electric device may be any one selected from an electric vehicle, a fuel cell drone, a fuel cell for power generation, a fuel cell for mobility, a water electrolysis fuel cell, and a hydrogen / electric power device for aerospace.

[0078] The present invention will be described in detail below by way of examples, but the present invention is not limited by the following examples.

[0079] Example 1: Preparation of Crystalline Carbon Support - PCH-Vh

[0080] (1) A mixed solution of 1 g of petroleum pitch and 100 mL of hexane was stirred at 30 °C for 24 hours to obtain a solution (PCH) in which aromatic carbon substances were precipitated (Fig. 3).

[0081] (2) 20 parts by weight of the aromatic carbon material dispersed in the above solution (PCH) was added to 100 parts by weight of carbon black (Vulcan XC-72) and stirred for 6 hours. Afterward, the mixture was filtered to obtain a precipitate (Fig. 4). The obtained precipitate was washed with hexane and dried in a vacuum oven at 150°C to obtain an aromatic carbon material-carbon support composite (PCH-V).

[0082] (3) A crystalline carbon support (PCH-Vh) was prepared by heat-treating 100 mg of the above aromatic carbon material-carbon support composite (PCH-V) at 1,000 °C for 1 hour under an argon (inert gas) atmosphere.

[0084] Example 2: Preparation of Crystalline Carbon Support - PCT-Vh

[0085] A crystalline carbon support (PCT-Vh) was prepared in the same manner as in Example 1, but using toluene instead of hexane.

[0087] Example 3: Preparation of Crystalline Carbon Support - PCTe-Vh

[0088] A crystalline carbon support (PCTe-Vh) was prepared in the same manner as in Example 1, but using tetrahydrofuran instead of hexane.

[0090] Example 4: Preparation of Crystalline Carbon Support - PCN-Vh

[0091] A crystalline carbon support (PCN-Vh) was prepared in the same manner as in Example 1, but using N-methyl-2-pyrrolidone instead of hexane.

[0093] Example 5: Preparation of Crystalline Carbon Support - PCD-Vh

[0094] A crystalline carbon support (PCD-Vh) was prepared in the same manner as in Example 1, but using dimethylformamide instead of hexane.

[0096] Example 6: Preparation of a Crystalline Carbon Support - Using Graphene Oxide

[0097] The same procedure as in Example 1 was carried out, but a crystalline carbon support was prepared using graphene oxide instead of carbon black.

[0099] Comparative Example 1: Commercial carbon support

[0100] A commercial carbon support, carbon black (Vulcan XC-72), was prepared.

[0102] Comparative Example 2: Heat-treated commercial carbon support

[0103] 100 mg of commercial carbon support carbon black (Vulcan XC-72) was heat-treated at 1,000 ℃ for 1 hour under an argon atmosphere to prepare heat-treated carbon black (Vulcan XC-72 1,000 ℃).

[0105] <Test Example>

[0106] Test Example 1: Characteristics of ACM-Carbon Support Composite and Crystalline Carbon Support

[0107] ACM (aromatic carbon material)-carbon support composite obtained in step (2) of the example

[0108] The electrochemical specific surface area (Initial EDLC) of the ACM-carbon support composite obtained in step (2) of the example was measured and compared, and it was specifically confirmed that the order was PCD-V (Example 5) > PCN-V (Example 4) > PCH-V (Example 1) > PCTe-V (Example 3) > PCT-V (Example 2) (Fig. 5).

[0109] In addition, as a result of confirming the electrochemical stability (EDLC change rate) of the ACM-carbon support composite obtained in step (2) of the above example, it was specifically confirmed that the electrochemical stability, i.e., durability, increased in the order of PCH-V (Example 1), PCD-V (Example 5), PCT-V (Example 2), PCN-V (Example 4), and PCTe-V (Example 3) (Fig. 6).

[0110] Crystalline carbon support obtained in step (3) of the example

[0111] In addition, the initial specific surface area (Initial EDLC) of the crystalline carbon supports prepared in the examples was measured and compared, and it was confirmed that the order was PCH-Vh (Example 1) > PCD-Vh (Example 5) > PCT-Vh (Example 2) > PCN-Vh (Example 4) and PCTe-Vh (Example 3) (Fig. 7).

[0112] In addition, as a result of confirming the electrochemical stability (EDLC change rate) of the crystalline carbon supports prepared in the examples, it was specifically confirmed that electrochemical stability, i.e., durability, increased in the order of PCH-V (Example 1), PCD-V (Example 5), PCTe-V (Example 3), PCN-V (Example 4), and PCT-V (Example 2). Specifically, PCH-Vh of Example 1 was found to be similar to commercial carbon black (Comparative Example 1) and had a larger electric double layer capacitance (EDLC) compared to heat-treated commercial carbon black (Comparative Example 2). In addition, PCT-Vh of Example 2 was similar to heat-treated commercial carbon black (Comparative Example 2), PCTe-Vh of Example 3 and PCN-Vh of Example 4 were similar to commercial carbon black (Comparative Example 1) but showed lower electric double layer capacitance (EDLC), and PCD-Vh of Example 5 showed a similar trend to commercial carbon black (Comparative Example 1) and PCD-V, and showed a larger EDLC and higher stability compared to heat-treated commercial carbon black (Comparative Example 2) (Fig. 8).

[0113] In addition, BET analysis of the crystalline carbon supports prepared in the examples confirmed that the specific surface area was in the order of PCH-Vh (Example 1), PCD-Vh (Example 5), PCTe-Vh (Example 3), PCT-Vh (Example 2), and PCN-Vh (Example 4) (Fig. 9 and Table 1).

[0114] division Specific Surface Area (㎡ / g) Micropore volume (cm³ / g) Example 1 (PCH-Vh) 165.45 0.014490 Example 2 (PCT-Vh) 121.29 0.015023 Example 3 (PCTe-Vh) 130.78 0.012805 Example 4 (PCN-Vh) 95.99 0.006656 Example 5 (PCD-Vh) 157.04 0.016200 Comparative Example 2 (VC1000) 235.77 0.035622

[0116] In addition, FIG. 10a shows the XRD analysis results of PCD-Vh (Example 5), PCD-V, VC1000 (Comparative Example 2), and VC (Comparative Example 1), and FIG. 10b and Table 2 show the Raman analysis results of PCD-Vh (Example 5), PCD-V, VC1000 (Comparative Example 2), and VC (Comparative Example 1). Through FIG. 10a, FIG. 10b, and Table 2, the Lc value (Z-axis direction) and La value (X, Y-axis direction) can be confirmed.

[0117] division Lc(Å) La(Å) Example 5 (PCD-Vh)_10wt% 14.22 39.3 PCD-V_10wt% 14.36 36.6 Comparative Example 1 (VC) 15.42 37.6 Comparative Example 2 (VC1000) 15.30 37.9

[0118] Looking at Figures 10a and 10b and Table 2 above, it can be seen that the Lc value of the crystalline carbon support according to Example 5 is similar to that of Comparative Examples 1 and 2, while the La value shows growth of about 2 Å. From these results, it can be seen that the size of the X and Y axis planes grew as defects in the carbon crystal planes were healed.

[0120] Test Example 2: EDLC (Electric Double Layer Capacitance) Analysis

[0121] The Electric Double Layer Capacitance (EDLC) of the crystalline carbon support according to the examples and comparative examples was confirmed by performing an Accelerated Degradation Test (ADT) based on the NEDO protocol (Fig. 11). The NEDO protocol is a durability test for polymer electrolyte fuel cells (PEMFC) proposed by Japan NEDO. It is a method for evaluating the performance degradation of a fuel cell during operation / stopping by accelerating the corrosion of the catalyst-supported carbon support through cyclic voltammetry performed repeatedly at 500 mV / s between 1.0 V and 1.5 V.

[0122] The above-mentioned accelerated duralability test (ADT) was performed in accordance with the NEDO protocol. Specifically, after performing the ADT for 1,000 cycles (1.0 V to 1.5 V 1,000 times), EDLC results as shown in FIG. 5 or FIG. 7 were obtained using cyclic voltammetry from 0 V to 1.2 V. Subsequently, the EDLC of the crystalline carbon support of the present invention was determined by calculating the area between the oxidation current and the reduction current within a specific voltage range. The determination of whether the structure of the carbon support is well maintained is based on the change values ​​of the EDLC values ​​over a total of four cycles at 0K, 1K, 2K, and 3K.

[0123] FIG. 11 shows the EDLC of each crystalline carbon support according to the examples and comparative examples compared with carbon black (Vulcan XC-72), carbon black heat-treated at 1000°C (Vulcan XC-72 1000°C), and carbon support composites of the examples and comparative examples that were not heat-treated.

[0124] Looking at Fig. 11, it can be seen that the PCD-Vh of Example 5 shows the least change in the EDLC. These results indicate that the PCD-Vh of Example 5 has the highest durability and is most suitable for use as a fuel cell catalyst.

[0126] Test Example 3: Evaluation of Thermal Oxidation Resistance

[0127] It is known that carbon materials with higher crystallinity undergo weight loss at higher temperatures in an oxygen atmosphere.

[0128] The thermal oxidation resistance characteristics of the crystalline carbon support according to Example 5 and the Comparative Example were evaluated through thermogravimetric analysis (TGA) and derivative thermogravimetry (DTG) based on said TGA (Figs. 12 and 13). In the present invention, thermogravimetric analysis (TGA) is a method of measuring the rate of mass change of a sample as a function of temperature or time according to a change in temperature, and the oxidation resistance of carbon can be confirmed through TGA in an oxygen atmosphere. It is known that the oxidation resistance characteristics are better when the mass loss occurs more gradually in the higher temperature range.

[0129] TGA measurements were performed in an air atmosphere by increasing the temperature at a rate of 10 degrees / min up to 500 degrees and at a rate of 5 degrees / min from 500 degrees to 1000 degrees.

[0130] Figure 12 and Table 3 are the results of confirming the thermal oxidation resistance of a crystalline carbon support according to Example 5 of the present invention through thermogravimetric analysis (TGA).

[0131] division Onset temp. of weight loss(℃) Onset temp. of Deriv. weight peak (℃) PCD-V_10wt% 643.70 598.25 PCD-Vh_10wt% (Example 5) 650.50 616.29 Comparative Example 1 643.90 601.63 Comparative Example 2 641.30 610.88

[0133] Looking at Figure 12 and Table 3, it can be seen that the crystalline carbon support (PCD-Vh) according to Example 5 of the present invention has a significantly increased onset temperature of weight loss compared to PCD-V and the comparative example, and thus its thermal oxidation resistance is greatly improved.

[0134] In addition, the minimum temperature of the differential thermogravimetric analysis of the crystalline carbon support (PCD-Vh) according to Example 5 of the present invention is 600 to 700 ℃, specifically 600 to 650 ℃, more specifically 610 to 630 ℃, and even more specifically 610 to 620 ℃, so it exhibits excellent thermal oxidation resistance, which minimizes carbon degradation when applied to a catalyst for a fuel cell, thereby ultimately ensuring stability and durability.

[0135] In addition, Figure 13 and Table 4 are the results of a comparative analysis of thermal oxidation resistance characteristics by performing TGA (thermogravimetric analysis) on PCD-Vh prepared according to Example 5 of the present invention and various commercial carbon supports.

[0136] division T 10 (℃) T 50 (℃) T 90 (℃) Comparative Example 1 578.4 688.1 737.4 Comparative Example 2 584.5 688.4 741.6 PCD-V_10wt% 567.3 677.9 720.0 PCD-Vh_10wt%(Example 5) 611.9 709.1 775.4 Vulcan XC72R 610 664 701 Graphite 671 740 784

[0138] Looking at FIG. 13 and Table 4, it can be seen that the crystalline carbon support (PCD-Vh) according to Example 5 of the present invention has significantly improved thermal oxidation resistance properties, with the temperature of weight loss increasing by 10 wt%, 50 wt%, and 90 wt% compared to PCD-V and the comparative example. In particular, it can be seen that the PCD-Vh of the present invention has high thermal oxidation resistance properties even compared to commercial carbon black (Vulcan XC72R) with high crystallinity.

[0140] Test Example 4: Analysis of Molecular Weight Size and Distribution of ACM

[0141] The molecular weight and distribution of each ACM (aromatic carbon material) extracted in the example were confirmed through Maldi-TOF analysis (Fig. 14).

[0142] MALDITOP analysis is a measurement method that allows determining the molecular weight of molecules contained in a sample. In particular, compared to gas chromatography, MALDITOP utilizes a laser to induce vaporization of the sample, which reduces the problem of sample molecules breaking down into smaller molecules due to heat. This allows for the determination of the sample's intrinsic molecular weight, and more accurate molecular weight analysis is possible by calculating the molecular weight based on the time of flight (TOF) and the time it takes to reach the detector. In the experiment of this invention, the extracted ACM solution was measured without a matrix.

[0143] Figure 14 shows the results of Maldi-TOF analysis for each ACM sample ((Fig. 14a) PCH, (Fig. 14b) PCT, (Fig. 14c) PCTe, (Fig. 14d) PCN, and (Fig. 14e) PCD) extracted from an embodiment of the present invention. Figure 14 represents the molecular weight size distribution based on the mass to charge values ​​of ACM, with darker colors indicating higher frequency.

[0144] Looking at Figure 14, it can be seen that although ACM is extracted from the same raw material (petroleum pitch), the molecular weight size and its distribution differ depending on the solvent.

[0145] Specifically, through FIG. 14a, PCH is C 34 H 10 (Molecular weight (Mw): 418.443) and C 38 H 12 It is a mixture of polycyclic aromatic hydrocarbons containing (molecular weight (Mw): 468.502),

[0146] Through Fig. 14b, PCT is C 34 H 10 (Molecular weight (Mw): 418.443), C 38 H 12 (Molecular weight (Mw): 468.502), C 38 H 22 (Molecular weight (Mw): 478.581) and C 40 H 12It is a mixture of polycyclic aromatic hydrocarbons containing (molecular weight (Mw): 492.523),

[0147] Through Fig. 14c, PCTe is C 38 H 12 (Molecular weight (Mw): 468.502) and C 38 H 22 It is a mixture of polycyclic aromatic hydrocarbons containing (molecular weight (Mw): 478.581),

[0148] Through Fig. 14d, PCN is C 38 H 12 (Molecular weight (Mw): 468.502), C 38 H 22 (Molecular weight (Mw): 478.581) and C 40 H 12 It is a mixture of polycyclic aromatic hydrocarbons containing (molecular weight (Mw): 492.523),

[0149] Through Fig. 14e, PCD is C 38 H 12 (Molecular weight (Mw): 468.502), C 38 H 22 (Molecular weight (Mw): 478.581) and C 40 H 12 It can be inferred that it is a mixture of polycyclic aromatic hydrocarbons containing (molecular weight (Mw): 492.523).

[0150] From the above results, it can be seen that the molecular weights of the ACMs are in the order of PCD > PCN > PCTe > PCT > PCH.

[0151] In addition, as a result of examining the molecular weight distribution of the above ACMs, it can be seen that the smaller the molecular weight of the ACM, the narrower the molecular weight distribution, and the larger the molecular weight, the wider the molecular weight distribution.

[0153] Test Example 5: Functional Group Analysis of ACM

[0154] The structural characteristics of each ACM (aromatic carbon material) extracted in the example were confirmed through FT-IR analysis, and each functional group was analyzed (Fig. 15).

[0155] FT-IR analysis is a measurement method that utilizes the property that when infrared light is irradiated onto a sample, the frequency of transmission or absorption differs depending on the bonding structure, thereby allowing for the identification of bonding present in the sample. In the present invention, ACM was measured in a solution state to confirm the differences in bonding present in different ACMs.

[0156] Looking at Fig. 15, it can be seen that although ACM is extracted from the same raw material (petroleum pitch), the oxygen functional groups present on the surface of ACM differ depending on the type of solvent. Specifically, it can be seen that PCH and PCD have both -COOH and -OH groups, PCTe has only -COOH groups, and PCN has only -OH groups. In particular, it was confirmed that C=C bonds are observed only in PCD.

[0158] Test Example 6: Evaluation of the durability of a catalyst using a crystalline carbon support

[0159] 6-1: Preparation of a catalyst using a crystalline carbon support

[0160] A catalyst was prepared by supporting platinum on a crystalline carbon support according to an example.

[0161] Specifically, 78 mg of a crystalline carbon support (PCD-Vh) prepared according to Example 5 was dispersed in a mixed solution of ethylene glycol (EG) and water (45 ml : 5 ml). A platinum precursor and a stabilizer were sequentially added to the dispersion solution. During this process, the concentration of the platinum precursor was 20 wt% and the weight was 51.89 mg. Subsequently, the pH of the mixed solution was adjusted to 10 using 1 M NaOH, and the solution was maintained at a temperature of 170°C for 3 hours to deposit platinum (Pt) particles on the surface of the crystalline carbon support. Afterward, the mixed solution was cooled to room temperature, the crystalline carbon support deposited with platinum (Pt) particles was filtered, thoroughly washed with distilled water, and dried in a 60°C oven for at least 12 hours to synthesize the catalyst.

[0163] 6-2: Durability Evaluation

[0164] Electrochemical experiments on the fuel cell catalyst prepared in Section 6-1 above were performed in a Rotating Disk Electrode (RDE) 3-Electrode Cell, using a 0.1M HClO4 solution as the electrolyte. An Ag / AgCl solution (saturated KCl, 3M) was used as the reference electrode, and a platinum wire was used as the counter electrode. To prepare the catalyst ink, the catalyst was added to distilled water, Nafion (5 wt%), and ethanol, and ultrasonically dispersed. The resulting ink was then applied to a glassy carbon RDE electrode (5 mm) using a micropipette at a concentration of 154 μg / cm² based on platinum. 2 After loading, it was dried.

[0165] Subsequently, changes in the chemically active surface (ECSA) and electric double layer capacitance (EDLC) of the above fuel cell catalyst were observed according to an accelerated deactivation cycle and are shown in Fig. 16 and Table 5.

[0166] Measurements were taken by performing cyclic voltammetry at a rate of 20 mV / s in the voltage range from 0 V to 1.2 V. The ECSA was calculated by determining the area of ​​the oxidation current peak between 0 V and 0.4 V from the measured graph and subtracting the area of ​​the oxidation current due to the EDLC from the result, then substituting this value into Equation 1 below. Additionally, the EDLC (C / cm²) was calculated by determining the area between the oxidation and reduction currents between 0.4 V and 0.44 V and dividing by 0.02.

[0167] [Equation 1]

[0168]

[0169] The above-mentioned electrochemical surface area (ECSA) represents the surface area of ​​platinum participating in electrochemical reactions. A decrease in the ECSA is a phenomenon caused by the loss or clumping of platinum particles, and a higher rate of decrease indicates lower durability of the catalyst.

[0170] In the above electric double layer capacitor (EDLC), when the carbon support is oxidized under electrochemical reaction conditions, oxygen functional groups are formed on the surface and then oxidized, increasing the electrochemical surface area. As the above EDLC increases, it means that the durability of the carbon support is lower.

[0171] division ECSA change rate EDLC change rate Pt / VC1000 (Comparative Example 2) -21.1% +102.2% Pt / PCD-Vh (Example) -16.7% +36.7%

[0172] Looking at Figure 16 and Table 5, it can be seen that the durability characteristics of the fuel cell catalyst using PCD-Vh of Example 5 of the present invention are significantly higher than those of the catalyst using heat-treated commercial carbon black of Comparative Example 2.

[0174] These results indicate that the catalyst using the crystalline carbon support according to the embodiment of the present invention possesses superior electrochemical properties, particularly durability, compared to the catalyst using the carbon support of the comparative example. It appears that the durability of the crystalline carbon support of the present invention is significantly improved due to defect healing of the commercial carbon support by an aromatic carbon material extracted from aromatic hydrocarbon raw materials such as petroleum pitch.

[0176] Although the present invention has been described as a preferred embodiment mentioned above, various modifications and variations are possible without departing from the essence and scope of the invention. Furthermore, the appended claims include such modifications and variations that fall within the essence of the invention.

Claims

Claim 1 A method for manufacturing a crystalline carbon support comprising: (a) a step of extracting an aromatic carbon material by adding an organic solvent to an aromatic hydrocarbon raw material; (b) a step of forming an aromatic carbon material-carbon support composite by mixing a solution containing the aromatic carbon material and the organic solvent with a carbon support; and (c) a step of heat-treating the aromatic carbon material-carbon support composite; wherein step (b) is performed without using an activator, a template material, or an inorganic salt, and the crystalline carbon support has a specific surface area of ​​100 to 600 m² / g. Claim 2 A method for manufacturing a crystalline carbon support according to claim 1, characterized in that the aromatic hydrocarbon raw material of step (a) is one or more selected from petroleum residue oil, petroleum pitch, coal residue oil, coal pitch, coal tar, coconut, and waste plastic. Claim 3 A method for manufacturing a crystalline carbon support according to claim 1, wherein the organic solvent in step (a) is one or more selected from hexane, toluene, tetrahydrofuran (THF), N-methyl-2-pyrrolidone (NMP), and dimethylformamide (DMF). Claim 4 A method for manufacturing a crystalline carbon support according to claim 1, wherein the aromatic carbon material in step (a) is a mixture of polycyclic aromatic hydrocarbons. Claim 5 A method for manufacturing a crystalline carbon support according to claim 1, characterized in that the aromatic carbon material in step (a) comprises a polycyclic aromatic hydrocarbon compound having a molecular weight of 10 to 10,000 m / z as measured by Matrix Assisted Laser Desorption Ionization Time of Flight (MALDI-TOF) mass spectrometry. Claim 6 A method for manufacturing a crystalline carbon support according to claim 1, wherein the carbon support in step (b) is one or more selected from carbon black, Ketjen black, carbon nanotube, graphene, graphene oxide, carbon nanofiber, and carbon nanospheres. Claim 7 A method for manufacturing a crystalline carbon support according to claim 1, characterized in that the heat treatment in step (c) is performed at 80 to 1600 ℃. Claim 8 A method for manufacturing a crystalline carbon support according to claim 1, wherein the aromatic hydrocarbon raw material is petroleum pitch, the organic solvent is dimethylformamide (DMF), the aromatic carbon material has a molecular weight of 10 to 10,000 m / z as measured by MALDI-TOF mass spectrometry, the carbon support is carbon black, and the heat treatment is performed at 80 to 1600 ℃. Claim 9 A crystalline carbon support for a fuel cell catalyst manufactured according to the method of any one of claims 1 to 8. Claim 10 delete Claim 11 A fuel cell catalyst characterized by having an active metal supported on a crystalline carbon support for a fuel cell catalyst according to claim 9. Claim 12 A catalyst for a fuel cell according to claim 11, characterized in that the active metal is one or more selected from platinum, palladium, gold, silver, rhodium, iridium, ruthenium, osmium, cobalt, manganese, nickel, iron, chromium, molybdenum, and titanium.

Citation Information

Patent Citations

  • Carbon-based calcined material and complex thereof as well as fuel cell using the carbon-based calcined material

    US20230238545A1

  • Method of preparing catalyst for fuel cell using electron beam

    KR102034635B1