Electromagnetic wave absorbing particle dispersion, electromagnetic wave absorbing laminate, electromagnetic wave absorbing transparent substrate

Cesium tungsten oxide particles, produced by reducing cesium tungsten oxide precursors, address the color limitations of existing materials by achieving neutral tones and improved near-infrared absorption, suitable for automotive glass and photothermal conversion materials.

KR103044615B1Active Publication Date: 2026-11-06SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020227020075
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-31
Filing Date
2021-01-28
Publication Date
2026-11-06
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

Existing electromagnetic wave absorbing materials, particularly those containing tungsten oxide, exhibit strong blue coloring and limited ability to achieve neutral or yellow-based colors, which restricts their application in automotive glass and photothermal conversion materials, and they struggle to provide pure white colors.

Method used

The use of cesium tungsten oxide particles, produced by reducing cesium tungsten oxide precursors nCs2O·mWO3 (3.6≤m/n≤9.0) at specific temperatures, adjusts the band gap and electron distribution to achieve a neutral color tone while enhancing near-infrared absorption.

Benefits of technology

The resulting electromagnetic wave absorbing particles provide a neutral color tone with reduced solar transmittance, suitable for applications requiring neutral or white hues without blue tint, and enhance near-infrared absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022061736641-PCT00003_ABST
    Figure 112022061736641-PCT00003_ABST
Patent Text Reader

Abstract

General formula CsxW1-yO3-z(0.2≤x≤0.4, 0 <y≤0.4, 0<z≤0.46)로 표시되고, 사방정 또는 육방정의 결정 구조를 구비한 세슘텅스텐산화물을 함유하는 전자파 흡수 입자와, 고체 매체를 포함하고, 상기 전자파 흡수 입자가 상기 고체 매체 중에 분산되어 있는 전자파 흡수 입자 분산체를 제공한다.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electromagnetic wave absorbing particle dispersion, an electromagnetic wave absorbing laminate, and an electromagnetic wave absorbing transparent substrate. Background Technology

[0002] According to the 5th edition of the Dictionary of Physical and Chemical Sciences, "electromagnetic waves with wavelengths in the range of about 1 nm to 1 mm are called light." This wavelength range includes the visible light region and the infrared region.

[0003] Near-infrared rays contained in sunlight penetrate window materials and enter the interior, raising the surface temperatures of walls and floors, as well as the indoor air temperature. Conventionally, to maintain a comfortable indoor thermal environment, it has been practiced to prevent the indoor air temperature from rising by blocking near-infrared rays entering through windows, such as by using shading materials on window materials.

[0004] As a light-blocking material used for windows, etc., Patent Document 1 proposes a light-blocking film containing black fine powder containing inorganic pigments such as carbon black and titanium black, or organic pigments such as aniline black.

[0005] In addition, Patent Document 2 discloses a thermal sheet formed as a knitted fabric using a strip-shaped film having infrared reflectivity and a strip-shaped film having infrared absorbivity as warp or weft threads, respectively. It also describes using a synthetic resin film laminated with an aluminum deposition process and a synthetic resin film as the strip-shaped film having infrared reflectivity.

[0006] The applicant proposed in Patent Document 3 an infrared shielding material fine particle dispersion in which infrared material fine particles are dispersed in a medium, wherein the infrared material fine particles contain tungsten oxide fine particles or / and composite tungsten oxide fine particles, and the dispersion particle size of the infrared material fine particles is 1 nm or more and 800 nm or less. Prior art literature

[0007] Japanese Patent Publication No. 2003-029314, Japanese Patent Publication No. Hei 9-107815, International Publication No. 2005 / 037932

[0008] K. Adachi and T. Asahi, "Activation of plasmons and polarons in solar control cesium tungsten bronze and reduced tungsten oxide nanoparticles, "Journal of Material Research, Vol. 27, 965-970(2012)S. Yoshio and K. Adachi, "Polarons in reduced cesium tungsten bronzes studied using the DFT+U method, "Materials Research Express, Vol. 6, 026548(2019)K. Machida, M. Okada, and K. Adachi, "Excitations of free and localized electrons at nearby energies in reduced cesium tungsten bronze nanocrystals, "Journal of Applied Physics, Vol. 125, 103103(2019)S. F. Solodovnikov, N.V. Ivannikova, Z.A. Solodovnikova, E.S. Zolotova, "Synthesis and X-ray diffraction study of potassium, rubidium, and cesium polytungstates with defect pyrochlore and hexagonal tungsten bronze structures, "Inorganic Materials, Vol. 34, 845-853(1998)M. Okada, K. Ono, S. Yoshio, H. Fukuyama and K.Adachi, “Oxygen vacancies and pseudo Jahn-Teller destabilization in cesium-doped hexagonal tungsten bronzes,” Journal of American Ceramic Society, Vol. 102, 5386-5400(2019)S. Yoshio, M. Okada, K. Adachi, “Destabilization of Pseudo Jahn-Teller Distortion in Cesium-doped Hexagonal Tungsten Bronzes”, J. Appl. Phys., vol. 124, 063109-1-8 (2018). The problem to be solved

[0009] In the aforementioned patent document 3, tungsten oxide microparticles or / and composite tungsten oxide microparticles are disclosed as infrared shielding material microparticles. The transparent film in which these tungsten oxides are dispersed is accompanied by blue coloring, and the degree of blueness becomes stronger as the amount added increases.

[0010] However, in recent years, for applications such as automotive glass or photothermal conversion materials, there is a demand for a neutral color that increases near-infrared absorption—that is, lowers solar transmittance—while having no coloring such as blue in the transmitted color.

[0011] When based on a blue material such as the transparent film with dispersed tungsten oxide mentioned above, the colors obtained when coloring glass with various pigments or dyes are limited. In particular, it is difficult to obtain a yellow-based transparent color, which is a complementary color.

[0012] In addition, for photothermal conversion materials, specifically for applications such as bonding transparent resin members by photothermal conversion, a pure white color is required, but it is difficult to achieve a pure white color with materials such as the tungsten oxide mentioned above.

[0013] In this regard, for example, if the transmitted color of a transparent film in which a composite tungsten oxide is dispersed is neutral, that is, a transparent hue, its applications can be expanded. However, there have been no reports to date of a composite tungsten oxide that can achieve a neutral color while lowering the solar transmittance when used as a dispersion.

[0014] Therefore, in one aspect of the present invention, the purpose is to provide an electromagnetic wave absorbing particle dispersion having a more neutral hue for the transmitted color while suppressing solar radiation transmittance. means of solving the problem

[0015] In one aspect of the present invention, the general formula Cs x W 1-y O 3-z (0.2≤x≤0.4, 0 <y≤0.4, 0<z≤0.46)로 표시되고, 사방정 또는 육방정의 결정 구조를 구비한 세슘텅스텐산화물을 함유하는 전자파 흡수 입자와, 고체 매체를 포함하고,

[0016] The above electromagnetic wave absorbing particles are dispersed in the above solid medium to provide an electromagnetic wave absorbing particle dispersion. Effects of the invention

[0017] In one aspect of the present invention, an electromagnetic wave absorbing particle dispersion having a more neutral color tone while suppressing solar radiation transmittance can be provided. Brief explanation of the drawing

[0018] Fig. 1a shows cesium tungsten oxide (Cs4W 11 O 35 This is an explanatory diagram of the crystal structure of ). Fig. 1b shows cesium tungsten oxide (Cs4W 12 O 36 This is an explanatory diagram of the crystal structure of ). FIG. 2a shows cesium tungsten oxide (Cs4W 11 O 35 It is the energy band structure of ). Fig. 2b shows cesium tungsten oxide (Cs4W 12 O 36It is the energy band structure of ). FIG. 2c shows cesium tungsten oxide (Cs4W 11 O 36 It is the energy band structure of ). FIG. 2d shows cesium tungsten oxide (Cs6W 17 O 54 It is the energy band structure of ). Figure 3a is the dielectric function of cesium tungsten oxide. Figure 3b is the dielectric function of cesium tungsten oxide. Figure 4 is an electron beam diffraction image taken from the c-axis direction of powder A' obtained in Example 1. FIG. 5 is

[0001] of the pseudo-hexagonal particles of powder A obtained in Example 1. HEX It is an electron beam diffraction pattern along the normal axis. Figure 6 is a STEM-HAADF phase observed from the

[0221] normal axis of the pseudo-hexagonal particles of powder A obtained in Example 1. FIG. 7 shows the

[0001] pseudo-hexagonal particles of powder B obtained in Example 2. HEX It is an electron beam diffraction pattern along the normal axis. FIG. 8 is

[0001] of the pseudo-hexagonal particles of powder C obtained in Example 3 HEX It is an electron beam diffraction pattern along the normal axis. FIG. 9a is the molar absorption coefficient of the dispersion prepared in Examples 14 to 20 and Comparative Example 1. FIG. 9b shows the molar absorption coefficients of the dispersions prepared in Examples 14 to 20 and Comparative Example 1. FIG. 9c is the molar absorption coefficient of the dispersion prepared in Examples 15, 16, 18, 22, 23 and Comparative Example 1. FIG. 10a is a transmittance profile of the dispersion prepared in Examples 15, 16, 19 and Comparative Examples 1 to 3, derived such that VLT becomes constant. FIG. 10b is a transmittance profile of the dispersion prepared in Examples 15, 16, 19 and Comparative Examples 1 to 3, derived so that VLT becomes constant. FIG. 11a is an explanatory diagram of the change in near-infrared absorption characteristics of dispersions related to Comparative Examples 1 to 3, Example 15, Example 16, and Example 19 over reduction time. FIG. 11b is an explanatory diagram of the changes accompanying the color index and reduction time of the dispersions related to Comparative Examples 1 to 3, Example 15, Example 16, and Example 19. FIG. 11c is an explanatory diagram of the changes accompanying the color index and reduction time of the dispersions related to Comparative Examples 1 to 3, Example 15, Example 16, and Example 19. Specific details for implementing the invention

[0019] Hereinafter, embodiments for carrying out the present invention will be described with reference to the drawings, but the present invention is not limited to the following embodiments, and various modifications and substitutions can be made to the following embodiments without departing from the scope of the present invention.

[0020] [Electromagnetic wave absorbing particles, method for manufacturing electromagnetic wave absorbing particles]

[0021] Before describing the electromagnetic wave absorbing particle dispersion of the present embodiment, electromagnetic wave absorbing particles suitable for use as the electromagnetic wave absorbing particle dispersion of the present embodiment and a method for manufacturing electromagnetic wave absorbing particles will be described.

[0022] (1) Electromagnetic wave absorbing particles

[0023] The transmission color of cesium-doped hexagonal tungsten bronze nanoparticles, which have been used as electromagnetic wave absorbing particles in the past, is determined by their dielectric function hub (ε2) (ε2 obtained from experiments is disclosed in Non-Patent Literature 1), and band structure (Non-Patent Literature 2).

[0024] In the energy range of visible light (1.6 eV to 3.3 eV), cesium-doped hexagonal tungsten bronze (hereinafter abbreviated as Cs-HTB) has a sufficiently large band gap. Furthermore, since electron transitions between dd orbitals of tungsten are prohibited by the Fermi golden ratio, the probability of electron transitions is reduced, and ε2 takes a small value. Since ε2 represents the absorption of photons by electrons, visible light transmittance occurs when ε2 is small at visible wavelengths. However, near the blue wavelength, which is the shortest wavelength in the visible light region, absorption due to inter-band transitions exists, and near the red wavelength, which is the longest wavelength, localized surface plasmon resonance (LSPR) absorption and polaric electron transition absorption exist (Non-patent Literature 3). For this reason, light transmittance is constrained in each case.

[0025] As described above, in Cs-HTB, the band gap is sufficiently large, so the inter-band transition becomes greater than the energy of blue wavelength light, resulting in high blue transmittance. Conversely, on the red wavelength side, Cs-HTB has many conduction electrons, so LSPR absorption and polaronic absorption become strong, and at the same time, since the absorption wavelength approaches the red wavelength side, transmittance is low. Therefore, the transmitted color of the Cs-HTB nanoparticle dispersion film appears blue.

[0026] In other words, to neutralize the transmission color of the blue spectrum of Cs-HTB, it is necessary to strengthen the absorption on the blue side and strengthen the transmission on the red side. To do this, it is desirable to shift the absorption position of the inter-band transition to a low energy, and also to weaken the LSPR absorption and polaronic absorption to shift them to the low energy side.

[0027] To weaken LSPR absorption or polaronic absorption, it is effective to reduce the amount of free electrons and bound electrons contained in the material.

[0028] The aforementioned increase in absorption on the blue side is realized by using a material with a different energy band structure having a band gap at a low energy as a base. In addition, transmission on the red side is due to cesium ions (Cs₂), which are the source of free or bound electrons. + ) or oxygen vacancies (V O The amount of ) can be controlled by adding or subtracting.

[0029] Based on the above considerations, the inventors of the present invention have discovered that when electromagnetic wave absorbing particles containing cesium tungsten oxide, which is an oxide containing cesium (Cs) and tungsten (W), are used after various investigations of cesium tungsten oxide, obtained by reducing a crystal powder of nCs2O·mWO3 (n, m are integers, 3.6≤m / n≤9.0), a cesium tungsten oxide precursor containing Cs and W, the color tone of the transparent film, which is an electromagnetic wave absorbing particle dispersion, is reduced in blueness and neutralized.

[0030] The above electromagnetic wave absorbing particle starts from a blue compound with low transmittance and a band gap narrower than hexagonal Cs-HTB, and by reducing this, V O It is thought that the hue was neutralized by gradually increasing the LSPR absorption and polaronic absorption within an acceptable range to optimize the red transmittance.

[0031] In the above cesium tungsten oxide precursor nCs2O·mWO3 containing Cs, the charges of the positive elements Cs and W are neutralized by O, making it a non-conductive material. Cs2W7O 22 , Cs6W 20 O 63 , Cs2W6O 19 , Cs4W 11 O 35 , Cs6W 11 O 36 , Cs2W3O 10 For compounds listed in the WO3-Cs2O line, since the valence is balanced, the Fermi energy E FIt exists between the valence band and the conduction band and is nonconductive. When the Cs / W ratio (molar ratio) is 0.2 or greater, in order to accommodate Cs with a large ionic radius, the basic framework formed by the WO octahedron is either a hexagonal symmetric structure with large hexagonal vacancies, or a crystal structure in which plane defects containing W defects (tungsten defects) are formed in the atomic arrangement of hexagonal or cubic (pyrochlore structure) with large hexagonal vacancies, resulting in orthorhombic or monoclinic symmetry.

[0032] For example, in 2Cs2O·11WO3, in the model of Solodovnikov 1998 (non-patent document 4), in the hexagonal arrangement of WO octahedra similar to hexagonal tungsten bronze, a plane with W and O missing at a b / 8 pitch of the orthorhombic unit cell is inserted into the hexagonal (110) plane (=orthorhombic (010) plane), so the whole is orthorhombic. In these cesium tungsten oxide precursors nCs2O·mWO3 (n and m are integers, 3.6≤m / n≤9.0), the band gap is narrower than that of Cs-HTB, and therefore the transmittance of blue is low. However, it was found that when this is heated and reduced, the whole gradually changes into the hexagonal structure of tungsten bronze, and in the process, the band structure changes and the band gap widens, so the absorption of blue weakens, and thus the transmittance of blue becomes stronger. Furthermore, at this time, as reduction proceeds, electrons are gradually injected into the conduction band to become a conductor, and the band gap gradually widens due to the Burstein-Moss effect, so the transmission of blue light becomes stronger.

[0033] When the orthorhombic crystal becomes hexagonal by heat reduction, the plane defects containing W defects in the orthorhombic crystals gradually disappear, and a hexagonal framework of WO octahedrons is formed. The plane defects containing W defects are (010) ORTH It exists on a plane, which is a hexagonal prism plane {100} HEX , that is, [(100) HEX ,(010) HEX ,(110)HEX Since it is inherited from ], gradually {100} with heating and reduction HEX It becomes a hexagon containing defects on the face. The hexagon in this case is {100} HEX Because it contains defects in the planes, it deviates from perfect hexagonal symmetry and is in a state that can also be called pseudo-hexagonal. In this way, with heating and reduction, the crystal structure changes from orthorhombic to pseudo-hexagonal, and further to hexagonal. At this time, (010) containing the W defect that was contained in the orthorhombic structure ORTH The surface defect of the surface is, {100} HEX It is thought that it will be inherited by surface defects, gradually decrease, and eventually disappear.

[0034] Along with changes in crystal structure during thermal reduction, the electronic structure also changes. The disappearance of W defects results in the injection of a large amount of electrons into the material. In orthorhombic crystals, Cs outer shell electrons are consumed for the neutralization of O, making the material overall charge-neutral; however, when W defects are reduced to form a pseudo-hexagonal crystal, six outer shell electrons per W atom are consumed for the neutralization of O, causing Cs outer shell electrons to enter the W-5d orbital below the conduction band and become free electrons. These free electrons cause the absorption of near-infrared radiation through LSPR absorption. Meanwhile, thermal reduction simultaneously V O There is a function that generates. V O The generation of is carried out at a random site. V O When this occurs, the W atoms on either side become charged excess, and W 5+Localized electrons are generated that are bound (Non-patent Literature 2). These localized electrons transition to voids in the upper conduction band, causing polaronic absorption, and some are excited into free electron orbits, causing LSPR absorption (Non-patent Literature 3). Since the peak wavelengths of both these free electrons and bound electrons are near-infrared, the ends of the absorption fall within the red wavelength range, thereby lowering red transmittance. As the amount of free electrons and bound electrons increases—that is, as the degree of reduction increases—the wavelengths of LSPR absorption and polaronic absorption shift to higher wavelengths, and the amount of absorption increases, so red transmittance decreases.

[0035] Therefore, by reducing the crystal powder of the cesium tungsten oxide precursor nCs2O·mWO3 (n, m are integers, 3.6≤m / n≤9.0) and adjusting the degree of reduction at that time, the blue transmitted color can be neutralized.

[0036] The electromagnetic wave absorbing particles suitable for use in the electromagnetic wave absorbing particle dispersion of the present embodiment described above can be produced by heating a crystal powder of a cesium tungsten oxide precursor nCs2O·mWO3 containing Cs and W in a reducing atmosphere of 650°C or higher and 950°C or lower. In the formula for the cesium tungsten oxide, n and m are integers, and it is preferable that 3.6 ≤ m / n ≤ 9.0 is satisfied.

[0037] That is, as electromagnetic wave absorbing particles, particles obtained by heating and reducing a crystal powder of a cesium tungsten oxide precursor nCs2O·mWO3 (n, m are integers, 3.6≤m / n≤9.0) containing cesium and tungsten in a reducing gas atmosphere at a temperature of 650°C or higher and 950°C or lower can be used.

[0038] In order for all or part of the material to become hexagonal tungsten bronze by heating and reduction, the value of m / n must be in the range of 3.6 ≤ m / n ≤ 9.0 as described above. If it is less than 3.6, it becomes a cubic pyrochlore phase after heating and reduction, exhibiting strong coloration and no near-infrared absorption. Furthermore, if it is greater than 9.0, it undergoes phase separation into hexagonal tungsten bronze and tungsten trioxide after heating and reduction, and the near-infrared absorption effect is significantly reduced. The above cesium tungsten oxide precursor is Cs4W with m / n = 5.5. 11 O 35 It is more desirable that it be Cs4W as an electromagnetic wave absorbing particle, as a columnar phase. That is, as an electromagnetic wave absorbing particle, as a columnar phase 11 O 35 It is more preferable to use particles obtained by heating and reducing a cesium tungsten oxide precursor containing a phase at a temperature of 650°C or higher and 950°C or lower in a reducing gas atmosphere. Cs4W 11 O 35 By using electromagnetic wave absorbing particles obtained by high-temperature reduction as a dispersion of electromagnetic wave absorbing particles, a large near-infrared absorption effect is obtained while having a transmitted color with suppressed blue tint. In addition, the term "main phase" as used here refers to the phase that is contained in the largest amount by mass ratio.

[0039] As described above, the heating temperature for reducing cesium tungsten oxide is preferably 650°C or higher and 950°C or lower. By setting the temperature to 650°C or higher, the structural change from orthorhombic to hexagonal is sufficiently carried out, thereby enhancing the near-infrared absorption effect. Furthermore, by setting the temperature to 950°C or lower, the speed of the crystal structure change is appropriately maintained, allowing for easy control into appropriate crystalline and electronic states. Additionally, if the heating temperature is higher than 950°C and reduction is carried out too excessively, lower oxides such as W metal or WO2 may be generated, which is also undesirable from a related perspective.

[0040] And, the electromagnetic wave absorbing particles suitable for use in the electromagnetic wave absorbing particle dispersion of the present embodiment are of the general formula Cs x W 1-y O 3-z (0.2≤x≤0.4, 0 <y≤0.4, 0<z≤0.46)로 표시되고, 사방정 또는 육방정의 결정 구조를 구비한 세슘텅스텐산화물을 함유할 수 있다.

[0041] When the cesium tungsten oxide contained in the electromagnetic wave absorbing particles satisfies the above general formula such that the degree of W deficiency or oxygen vacancy Vo is within an appropriate range, and is used as an electromagnetic wave absorbing particle dispersion, it is possible to obtain an electromagnetic wave absorbing particle dispersion that has a more neutral color tone while suppressing solar radiation transmittance.

[0042] In addition, the electromagnetic wave absorbing particles may include the above-mentioned composite tungsten oxide. However, even in this case, it is not excluded that they contain unavoidable impurities that are mixed in during the manufacturing process, etc.

[0043] Conventionally known tungsten bronze for electromagnetic wave absorption has a hexagonal structure. Meanwhile, the composite tungsten oxide having electromagnetic wave absorbing particles used in the electromagnetic wave absorbing particle dispersion of the present embodiment may have an orthorhombic or hexagonal crystal structure. Furthermore, the hexagonal structure described herein includes pseudo-hexagonal structures.

[0044] The composite tungsten oxide containing the electromagnetic wave absorbing particles preferably has linear or planar defects on one or more selected planes, such as the orthorhombic (010) plane, the hexagonal prism plane {100} plane, and the hexagonal bottom plane (001). The defects include stacking irregularities based on misalignment between planes, or confusion in the arrangement or atomic positions of Cs atoms or W atoms within the planes, and thus sometimes involve streaks in the electron beam diffraction spots. The hexagonal prism plane {100} plane refers to the (100) plane, the (010) plane, and the (110) plane. The defects associated with the composite tungsten oxide, namely lattice defects, involve at least a W defect, specifically a partial W defect, and this W defect causes a loss of electrons in the crystal, which, as previously explained, acts as one of the essential causes for the neutralization of the blue tone.

[0045] Cesium tungsten oxide has defects, and the related defects may include tungsten defects as described above.

[0046] Furthermore, it is also possible for some of the oxygen atoms in the WO octahedra, which constitute the orthorhombic or hexagonal crystals that form the basic structure of cesium tungsten oxide, to be more randomly missing. These vacancies of octahedral oxygen, V O As mentioned above, it is introduced randomly, and the known hexagonal tungsten bronze Cs 0.32 WO 3-y In this case, it is known that y=0.46 or O reaches up to 15% of the electric charge point (Non-patent Literature 5). General formula Cs representing the cesium tungsten oxide contained in the electromagnetic wave absorbing particles used in the electromagnetic wave absorbing particle dispersion of the present embodiment. x W 1-y O 3-z In this case, the maximum amount V of z=0.46 O It can include. That is, z can be 0.46 or less.

[0047] The lattice constant of the cesium tungsten composite oxide corresponds to the amount of defects, composition, and crystallinity within the crystal lattice. While the value of the a-axis shows variation with respect to these variables, the value of the c-axis corresponds relatively well to the amount of lattice defects or optical properties. Consequently, it is preferable that the cesium tungsten oxide contained in the electromagnetic wave absorbing particles used in the electromagnetic wave absorbing particle dispersion of the present embodiment has a c-axis length in hexagonal form of 7.560 Å or more and 7.750 Å or less. By setting the c-axis length in hexagonal form of the cesium tungsten oxide to the above range, the near-infrared absorption effect is sufficiently enhanced, and the visible light transmittance is particularly enhanced. Furthermore, if the cesium tungsten oxide is hexagonal, the conversion is unnecessary, and the c-axis length in that hexagonal form becomes the c-axis length in hexagonal form.

[0048] The cesium tungsten oxide contained in the electromagnetic wave-absorbing particles used in the electromagnetic wave-absorbing particle dispersion of the present embodiment is often identified as a mixed phase of orthorhombic and hexagonal phases when the diffraction pattern of the sample is measured by X-ray powder diffraction. For example, Cs4W 11 O 35 If the raw material is reduced, orthorhombic Cs4W 11 O 35 and hexagonal Cs 0.32 It is identified with the mixed phase of WO3. In this case, the lattice constants of each phase can be determined using Rietveld analysis or the like, and converted into hexagonal equivalent values. As previously explained, since the orthorhombic phase is a hexagonal phase with lattice defect planes, the orthorhombic lattice constants can be converted into hexagonal lattice constants by an appropriate lattice correspondence model. If the correspondence of lattice changes between orthorhombic and hexagonal phases is assumed to be the model of Solodovnikov 1998 (Non-patent Literature 4), from the geometric relationship for this model, 4a orth 2 +b orth 2 =64a hex 2 =64b hex2 , c orth =c hex Since the relationship is extracted, all hexagonal converted lattice constants can be obtained using these equations. In addition, a in the above equation orth , b orth , c orth represents the lengths of the a-axis, b-axis, and c-axis of an orthorhombic shape. Also, a hex , b hex , c hex represents the lengths of the a-axis, b-axis, and c-axis of the hexagon.

[0049] The cesium tungsten oxide contained in the electromagnetic wave absorbing particles used in the electromagnetic wave absorbing particle dispersion of the present embodiment may have a portion of Cs substituted by an additive element. In this case, it is preferable that the additive element be one or more selected from Na, Tl, In, Li, Be, Mg, Ca, Sr, Ba, Al, and Ga.

[0050] The above-mentioned additive elements are electron-donating and assist in electron donation to the conduction band of the WO octahedral framework at the Cs site.

[0051] The average particle size of the electromagnetic wave absorbing particles of the present embodiment is not particularly limited, but it is preferably 0.1 nm or larger and 200 nm or smaller. This is because by making the average particle size of the electromagnetic wave absorbing particles 200 nm or smaller, localized surface plasmon resonance is expressed more prominently, which can particularly enhance near-infrared absorption characteristics, that is, particularly suppress solar radiation transmittance. In addition, by making the average particle size of the electromagnetic wave absorbing particles 0.1 nm or larger, it can be easily manufactured industrially. Furthermore, the particle size is closely related to the color of the dispersion-transmitting film, that is, the dispersion of the electromagnetic wave absorbing particles, and in the particle size range where Mie scattering is dominant, short-wavelength scattering in the visible light region decreases as the particle size becomes smaller. Therefore, increasing the particle size has the effect of suppressing the blue tint, but if it exceeds 100 nm, the film haze accompanying light scattering becomes too large to be ignored, and if it exceeds 200 nm, in addition to the increase in film haze, the generation of surface plasmons is suppressed, so the LSPR absorption becomes excessively small.

[0052] Here, the average particle size of the electromagnetic wave absorbing particles can be determined from the median diameter of a plurality of electromagnetic wave absorbing particles measured from a transmission electron microscope, or from the dispersion particle size measured by a particle size measuring device based on the dynamic light scattering method of the dispersion.

[0053] In addition, when applied to applications where transparency in the visible light region is particularly important, such as the front glass of an automobile, it is desirable to additionally consider scattering reduction by electromagnetic wave absorbing particles. When such scattering reduction is important, it is particularly desirable that the average particle size of the electromagnetic wave absorbing particles be 30 nm or less.

[0054] The average particle size refers to the particle size at 50% of the accumulated value in the particle size distribution, and the average particle size has the same meaning in other parts of this specification. As a method for measuring the particle size distribution to calculate the average particle size, direct measurement of the particle size of each particle using, for example, a transmission electron microscope may be used. In addition, the average particle size may be measured by a particle size measuring device based on the dynamic light scattering method of a dispersion as described above.

[0055] In addition, the electromagnetic wave absorbing particles may be surface-treated for purposes such as surface protection, improved durability, prevention of oxidation, and improved water resistance. Although the specific details of the surface treatment are not particularly limited, for example, the surface of the electromagnetic wave absorbing particles of the present embodiment may be modified with a compound containing one or more atoms selected from Si, Ti, Zr, and Al. In this case, one or more compounds selected from oxides, nitrides, carbides, etc., may be examples of compounds containing one or more atoms (elements) selected from Si, Ti, Zr, and Al.

[0056] Here, the band structures of cesium tungsten oxide and cesium tungsten oxide precursors are described.

[0057] As explained above, it was shown that reducing nCs2O·mWO3 (n, m are integers, 3.6≤m / n≤9.0) at high temperatures yields a solar radiation shielding material with a transmittance color closer to neutral. During high-temperature reduction, hexagonalization including the elimination of W defects and V O It is thought that electrons are injected into the conduction band through the generation of [this], which is the source of near-infrared absorption, and this change in electronic structure is supported by first-principles calculations.

[0058] Cs4W in Fig. 1a 11 O 35 The crystal structure of is illustrated. Also, Cs in Fig. 1b 0.33 WO3 in Cs4W12 O 36 The crystal structure of is illustrated. In FIGS. 1a and 1b, cesium (11) and oxygen (12) are illustrated. Additionally, atoms of the same type are given the same hatching. Tungsten is not illustrated in FIGS. 1a and 1b because it is placed within an octahedron formed of oxygen (12). FIG. 1b is Cs 0.33 WO3, Cs4W of FIG. 1a 11 O 35 It is a structure that takes a new axis in a four-sided shape to allow for comparison.

[0059] Cs4W in Fig. 1a 11 O 35 The structure is the Cs4W in Fig. 1b 12 O 36 In the crystal structure of, W and O are regularly missing.

[0060] The band structures of the cesium tungsten oxide crystal structures of FIGS. 1a and 1b are illustrated in FIGS. 2a and 2b, respectively. In addition, the Cs4W of FIG. 1b 12 O 36 Based on, Cs4W with 1 W missing 11 O 36 Cs6W with a band structure, and 1.5 times the cell size in the b-axis direction, with one W missing 17 O 54 The structure of each band is illustrated in Fig. 2c and Fig. 2d, respectively.

[0061] Cs4W illustrated in FIGS. 2a and 2b 11 O 35 band structure, and Cs4W 12 O 36 The band structure is similar, but the Fermi energy (E F The former is within the band gap, and the latter is below the conduction band. Therefore, Cs4W 11 O 35 is an insulator, and Cs4W 12 O 36 It is a conductor. Cs4W 11 O35 In Cs4W 12 O 36 Based on this, there is a shortage of 1 unit each of W and O in the unit cell. Cs4W is full of W and O. 12 O 36 In this case, it is interpreted that a hexagonal WO3 network is formed and Cs electrons are injected into the W-5d orbital to become a conductor (Non-patent Literature 6).

[0062] Cs4W in Fig. 2c 11 O 36 Silver, Cs4W in Fig. 2b 12 O 36 It is a structure obtained by subtracting 1 from W.

[0063] Cs6W in Fig. 2d 17 O 54 , that is, 3Cs2O·17WO3 is Cs4W in Fig. 2b 12 O 36 , that is, Cs6W 18 O 54 From the perspective, it is a structure that maintains charge neutrality while subtracting one W.

[0064] The amount of W defect decreases in the order of Fig. 2a, Fig. 2d, and Fig. 2b, and E F The electrons are rising sequentially to the bottom side of the conductor, and as W electrons are injected into the W-5d orbital, the number of conduction electrons increases, supporting the increase in near-infrared absorption.

[0065] Cs4W 12 O 36 In the case where O is missing, detailed calculation examples have already been reported, and it is known that free electrons and localized electrons increase significantly along with the introduction of localized orbitals at the bottom of the conduction band (Non-patent document 2).

[0066] In experimentally obtained pseudo-hexagonal structures (intermediate structures during the phase transition between orthorhombic and hexagonal), the electronic state is considered to be a mixture of the above elements. That is, accompanying reduction, hexagonalization involving the disappearance of the W deficiency and V ODue to the generation of, electrons are gradually injected into the conduction band, and Fermi energy E F It rises from the band gap to the lower part of the conduction band.

[0067] Based on these band structures, the results of calculating the dielectric function including the Drude term are shown in FIGS. 3a and 3b. Focusing on the position of ε1=0 in the dielectric function ε1 shown in FIG. 3b, the shielded plasma frequency (Ω SP ) is Cs4W 11 O 35 , Cs6W 17 O 54 , Cs4W 12 O 36 , Cs4W 12 O 35 It can be seen that it increases in this order. Near-infrared absorption is expected to increase in this order, and this trend is consistent with the observation results.

[0068] From the dielectric function ε2 plot shown in FIG. 3a, it can be seen that the ε2 in the visible region is generally small for cesium tungsten oxide. At 3.3 eV in the blue region indicated by the dashed line (31), the band gap is narrow, defined by the inter-band transition, for Cs4W 11 O 35 I'm Cs6W 17 O 54 The absorption of increases. Meanwhile, at 1.6 eV in the red region indicated by the dotted line (32), influenced by the end of surface plasmon absorption, Cs4W 12 O 35 It can be seen that the absorption is large. The transmitted light in the red region is Ω SPIt is expected to decrease in the order of decreasing. The profile of ε2 in the visible light region illustrated in Fig. 3a basically corresponds to the experimentally observed Fig. 9b and accurately reproduces that trend. That is, compared to the conventionally used cesium tungsten oxide, the reason for the decrease in blueness in the cesium tungsten oxide containing electromagnetic wave absorbing particles suitable for use in the electromagnetic wave absorbing particle dispersion of this embodiment is that nCs2O·mWO3 (3.6≤m / n≤9.0), which has deficiencies in W and O, was used as a raw material, thereby reducing the Cs containing W deficiencies. 0.33 W 1-y O 3-z It is thought that this is because a phase is formed, and absorption on the high-energy side increases. By controlling the high-temperature reduction of nCs2O·mWO3 (3.6≤m / n≤9.0), the band gap and the amount of electrons injected into the conduction band are controlled, allowing for the control of a bluish tint. In addition, it was confirmed that the near-infrared absorption effect at that time is maintained at a relatively high state.

[0069] (Method for manufacturing electromagnetic wave absorbing particles)

[0070] The method for manufacturing electromagnetic wave absorbing particles described above is not particularly limited, and any method capable of manufacturing electromagnetic wave absorbing particles that satisfy the characteristics described above may be used without specific limitation. Here, an example of a method for manufacturing electromagnetic wave absorbing particles is described.

[0071] A method for manufacturing electromagnetic wave absorbing particles may, for example, have the following process.

[0072] A process for synthesizing a cesium tungsten oxide precursor, which is a tungstate containing cesium.

[0073] A heating and reduction process for heating and reducing a cesium tungsten oxide precursor in a reducing gas atmosphere at a temperature of 650°C or higher and 950°C or lower.

[0074] The following describes each process.

[0075] (1) Cesium tungsten oxide precursor synthesis process

[0076] In the process of synthesizing a cesium tungsten oxide precursor, a cesium tungsten oxide precursor containing cesium, namely cesium tungsten, can be synthesized. If a cesium tungsten oxide precursor has already been synthesized, the method for manufacturing electromagnetic wave absorbing particles according to the present embodiment may be initiated from a heating reduction process.

[0077] In addition, the cesium tungstate oxide precursor, which is a cesium tungstate, is preferably a crystalline powder of nCs2O·mWO3 (n, m is an integer, 3.6≤m / n≤9.0). As for the cesium tungstate oxide precursor, it is more preferable that it be a stable cesium tungstate. As for a stable cesium tungstate, Cs4W 11 O 35 , Cs2W6O 19 , Cs6W 20 O 63 , Cs2W7O 22 , Cs6W 11 O 36 One or more types selected from the above may be cited. The cesium tungsten oxide precursor is particularly Cs4W as the main phase. 11 O 35 It is more preferable that the cesium tungsten oxide precursor contains a phase.

[0078] These cesium tungstates can be prepared, for example, by calcining a mixture of raw material powders containing cesium or tungsten in the atmosphere at a temperature of 700°C or higher and 1000°C or lower. In addition, the method of manufacturing cesium tungstates is not limited to the above forms, and other methods such as the sol-gel method or complex polymerization method may also be used.

[0079] In addition, as cesium tungstate used as a starting material, non-equilibrium tungstate obtained by vapor phase synthesis, etc., may be used. This includes powders produced by the thermal plasma method or powders produced by electron beam melting.

[0080] (2) Heating and reducing process

[0081] A cesium tungsten oxide precursor as the above-mentioned starting material, specifically, a cesium tungstate having one or more crystal structures selected from, for example, orthorhombic, monoclinic, and pseudo-hexagonal, can be provided to a heating reduction process.

[0082] In the heating and reduction process, the above-described cesium tungsten oxide precursor can be heated and reduced in a reducing gas atmosphere at a temperature of 650°C or higher and 950°C or lower. By carrying out the heating and reduction process, electromagnetic wave absorbing particles containing cesium tungsten oxide of a desired composition are obtained.

[0083] When performing a heat reduction treatment, it is preferable to perform it under a stream of reducing gas. As the reducing gas, a mixed gas containing a reducing gas such as hydrogen and one or more inert gases selected from nitrogen, argon, etc. may be used. In addition, heating in a steam atmosphere or vacuum atmosphere, or other mild heating and reduction conditions may be used in combination.

[0084] In addition, the method for manufacturing electromagnetic wave absorbing particles of the present embodiment is not particularly limited to the above form. As a method for manufacturing electromagnetic wave absorbing particles, various methods capable of forming a predetermined structure including a defective microstructure can be used. Examples of methods for manufacturing electromagnetic wave absorbing particles include a method of reducing tungstate obtained by a solid-phase method, a liquid-phase method, or a gas-phase method, or a method of reducing WO3 in molten alkali halide.

[0085] The method for manufacturing electromagnetic wave absorbing particles may also have any process.

[0086] (3) Grinding process

[0087] As previously explained, it is desirable for the electromagnetic wave absorbing particles to be micronized and become fine particles. For this reason, the method for manufacturing electromagnetic wave absorbing particles may include a grinding process for grinding the powder obtained by a heating reduction process.

[0088] The specific means for grinding and micronizing are not particularly limited, and various means capable of mechanical grinding may be used. As for the mechanical grinding method, a dry grinding method using a jet mill or the like may be used. In addition, mechanical grinding may be performed in a solvent during the process of obtaining the electromagnetic wave absorbing particle dispersion described later.

[0089] (4) Formula process

[0090] As previously explained, the electromagnetic wave absorbing particle may have its surface modified with a compound containing one or more atoms selected from Si, Ti, Zr, and Al. Thus, the method for manufacturing the electromagnetic wave absorbing particle may further include, for example, a modification process in which the electromagnetic wave absorbing particle is modified with a compound containing one or more atoms selected from Si, Ti, Zr, and Al.

[0091] In the modification process, the specific conditions for modifying the electromagnetic wave absorbing particles are not particularly limited. For example, a modification process may be performed in which an alkoxide containing one or more atoms selected from the above atomic group (metal group) is added to the electromagnetic wave absorbing particles to be modified, and a film is formed on the surface of the electromagnetic wave absorbing particles.

[0092] [Electromagnetic wave absorbing particle dispersion]

[0093] Next, an example of the composition of the electromagnetic wave absorbing particle dispersion of the present embodiment will be described.

[0094] The electromagnetic wave absorbing particle dispersion of the present embodiment may include the electromagnetic wave absorbing particles described above and one or more liquid media selected from water, organic solvents, oils and fats, liquid resins, and liquid plasticizers. It is preferable that the electromagnetic wave absorbing particle dispersion has a composition in which electromagnetic wave absorbing particles are dispersed in a liquid medium.

[0095] As for the liquid medium, one or more types selected from water, organic solvents, oils and fats, liquid resins, and liquid plasticizers can be used, as previously explained.

[0096] As organic solvents, various types can be selected, such as alcohol-based, ketone-based, hydrocarbon-based, glycol-based, and water-based solvents. Specifically, alcohol-based solvents such as isopropyl alcohol, methanol, ethanol, 1-propanol, isopropanol, butanol, pentanol, benzyl alcohol, diacetone alcohol, and 1-methoxy-2-propanol; ketone-based solvents such as dimethyl ketone, acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, cyclohexanone, and isophorone; ester-based solvents such as 3-methyl methoxy-propionate and butyl acetate; and glycol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol isopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, and propylene glycol ethyl ether acetate; One or more types selected from amides such as formamide, N-methylformamide, dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene and xylene; and halogenated hydrocarbons such as ethylene chloride and chlorbenzene may be cited.

[0097] However, among these, organic solvents with low polarity are preferred, and in particular, isopropyl alcohol, ethanol, 1-methoxy-2-propanol, dimethyl ketone, methyl ethyl ketone, methyl isobutyl ketone, toluene, propylene glycol monomethyl ether acetate, n-butyl acetate, etc. are more preferred. One or more of these organic solvents may be used.

[0098] As for the oil, one or more types selected from drying oils such as linseed oil, sunflower oil, and tung oil; semi-drying oils such as sesame oil, cottonseed oil, rapeseed oil, soybean oil, and rice bran oil; non-drying oils such as olive oil, coconut oil, palm oil, and dehydrated castor oil; fatty acid monoesters obtained by directly esterifying a fatty acid of vegetable oil with a monoalcohol; ethers; and petroleum-based solvents such as Isofa (registered trademark) E, Exol (registered trademark) Hexane, Heptane, E, D30, D40, D60, D80, D95, D110, and D130 (all manufactured by ExxonMobil).

[0099] As for the liquid resin, one or more types selected from, for example, liquid acrylic resin, liquid epoxy resin, liquid polyester resin, liquid urethane resin, etc. may be used.

[0100] As a liquid plasticizer, for example, a liquid plasticizer for plastics can be used.

[0101] The components contained in the electromagnetic wave absorbing particle dispersion are not limited to the aforementioned electromagnetic wave absorbing particles and liquid medium. The electromagnetic wave absorbing particle dispersion may additionally contain any other components as necessary.

[0102] For example, acid or alkali may be added to the electromagnetic wave absorbing particle dispersion as needed to adjust the pH of the dispersion.

[0103] In addition, in order to further improve the dispersion stability of the electromagnetic wave absorbing particles in the aforementioned electromagnetic wave absorbing particle dispersion and to avoid coarsening of the dispersed particle size due to re-aggregation, various surfactants, coupling agents, etc., may be added to the electromagnetic wave absorbing particle dispersion as dispersants.

[0104] The dispersant, such as the surfactant or coupling agent, can be selected according to the application, and it is preferable that the dispersant has one or more functional groups selected from amine-containing groups, hydroxyl groups, carboxyl groups, and epoxy groups. These functional groups adsorb to the surface of electromagnetic wave-absorbing particles to prevent aggregation and have the effect of uniformly dispersing the electromagnetic wave-absorbing particles even within an infrared shielding film formed using the electromagnetic wave-absorbing particles. A polymer-based dispersant having one or more selected from the above functional groups (functional group groups) in its molecule is even more preferable.

[0105] Commercially available dispersants suitable for use include Solspers (registered trademark) 9000, 12000, 17000, 20000, 21000, 24000, 26000, 27000, 28000, 32000, 35100, 54000, 250 (manufactured by Nihon Lubrizol Co., Ltd.), EFKA (registered trademark) 4008, 4009, 4010, 4015, 4046, 4047, 4060, 4080, 7462, 4020, 4050, 4055, 4400, 4401, 4402, 4403, 4300, 4320, 4330. 4340, 6220, 6225, 6700, 6780, 6782, 8503 (manufactured by F-Car Additives), Azisper (registered trademark) PA111, PB821, PB822, PN411, Feymex L-12 (manufactured by Ajinomoto Fine Techno Co., Ltd.), DisperBYK (registered trademark) 101, 102, 106, 108, 111, 116, 130, 140, 142, 145, 161, 162, 163, 164, 166, 167, 168, 170, 171, 174, 180, 182, 192, 193, 2000, 2001, 2020, 2025, 2050, 2070, 2155, 2164, 220S, 300, 306, 320, 322, 325, 330, 340, 350, 377, 378, 380N, 410, 425, 430 (Made by Big Chem Japan Co., Ltd.), Dispalon (Registered Trademark) 1751N, 1831, 1850, 1860, 1934, DA-400N, DA-703-50, DA-725, DA-705, DA-7301, DN-900, NS-5210, NVI-8514L (Kusumoto Kasei One or more types selected from (manufactured by Kabushiki Kaisha), Arpon (registered trademark) UC-3000, UF-5022, UG-4010, UG-4035, UG-4070 (manufactured by Doa Kose Kabushiki Kaisha), etc. may be cited.

[0106] The method for dispersing electromagnetic wave absorbing particles into a liquid medium is not particularly limited as long as it is a method capable of dispersing the electromagnetic wave absorbing particles in a liquid medium. At this time, it is preferable that the average particle size of the electromagnetic wave absorbing particles be 200 nm or less, and it is more preferable that the average particle size be 0.1 nm or more and 200 nm or less.

[0107] As a method for dispersing electromagnetic wave absorbing particles into a liquid medium, examples include dispersion methods using devices such as bead mills, ball mills, sand mills, paint shakers, and ultrasonic homogenizers. Among these, grinding and dispersing using a media-stirring mill, such as a bead mill, ball mill, sand mill, or paint shaker, which uses a media (beads, balls, Ottawa sand), is preferable from the perspective of reducing the time required to achieve a desired average particle size. Through grinding and dispersion treatment using a media-stirring mill, the electromagnetic wave absorbing particles are dispersed into the liquid medium, and simultaneously, micronization proceeds due to collisions between the electromagnetic wave absorbing particles or collisions between the media and the particles, thereby allowing the electromagnetic wave absorbing particles to be further micronized and dispersed. In other words, grinding and dispersion treatment is performed.

[0108] As described above, the average particle size of the electromagnetic wave absorbing particles is preferably 0.1 nm or more and 200 nm or less. This is because if the average particle size is small, the scattering of light in the visible light region with wavelengths of 400 nm to 780 nm or less due to geometric scattering or Mie scattering is reduced. Consequently, it is possible to avoid the electromagnetic wave absorbing particle dispersion, in which the particles are dispersed in a resin or the like and obtained using, for example, the electromagnetic wave absorbing particle dispersion of the present embodiment, becoming frosted like glass and failing to achieve clear transparency. In other words, when the average particle size is 200 nm or less, the light scattering mode of the geometric scattering or Mie scattering weakens and becomes the Rayleigh scattering mode. Since scattered light in the Rayleigh scattering region is proportional to the sixth power of the dispersed particle size, scattering is reduced and transparency is improved as the dispersed particle size decreases. Furthermore, it is preferable that the average particle size is 100 nm or less, as the scattered light becomes very small.

[0109] However, regarding the dispersion state of the electromagnetic wave absorbing particles within the electromagnetic wave absorbing particle dispersion obtained using the electromagnetic wave absorbing particle dispersion of the present embodiment, in which the electromagnetic wave absorbing particles are dispersed in a solid medium such as a resin, as long as a known method of adding the dispersion to the solid medium is performed, the dispersion will not aggregate beyond the average particle size of the electromagnetic wave absorbing particles of the said dispersion.

[0110] In addition, if the average particle size of the electromagnetic wave absorbing particles is 0.1 nm or more and 200 nm or less, it is possible to avoid the electromagnetic wave absorbing particle dispersion or the molded body (plate, sheet, etc.) manufactured having a monotonously reduced transmittance and becoming a grayish color.

[0111] The content of electromagnetic wave absorbing particles in the dispersion of electromagnetic wave absorbing particles of the present embodiment is not particularly limited, but, for example, it is preferably 0.01 mass% or more and 80 mass% or less. This is because sufficient solar radiation transmittance can be achieved by making the content of electromagnetic wave absorbing particles 0.01 mass% or more. In addition, by making it 80 mass% or less, the electromagnetic wave absorbing particles can be uniformly dispersed within the dispersion medium.

[0112] [Electromagnetic wave absorbing particle dispersion]

[0113] Next, an example of the composition of the electromagnetic wave absorbing particle dispersion of the present embodiment will be described.

[0114] The electromagnetic wave absorbing particle dispersion of the present embodiment comprises the electromagnetic wave absorbing particles previously described and a solid medium. Furthermore, in the electromagnetic wave absorbing particle dispersion of the present embodiment, it is preferable that the electromagnetic wave absorbing particles are dispersed within the solid medium.

[0115] In addition, the electromagnetic wave absorbing particles already explained are defined by the general formula Cs x W 1-y O 3-z (0.2≤x≤0.4, 0 <y≤0.4, 0<z≤0.46)로 표시되고, 사방정 또는 육방정의 결정 구조를 구비한 세슘텅스텐산화물을 함유하는 전자파 흡수 입자이다. 상세에 대해서는 이미 설명했기 때문에, 여기에서는 설명을 생략한다.

[0116] Hereinafter, regarding the electromagnetic wave absorbing particle dispersion related to the present embodiment, (1) solid medium, (2) manufacturing method, (3) additive, and (4) application example will be described in that order.

[0117] (1) solid media

[0118] Examples of solid media include medium resins such as thermoplastic resins, thermosetting resins, and UV-curing resins. In other words, resins can be suitably used as solid media.

[0119] The specific material of the medium resin is not particularly limited, but, for example, it is preferably one resin selected from the group of resins consisting of polyester resin, polycarbonate resin, acrylic resin, styrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, olefin resin, epoxy resin, polyimide resin, fluoropolymer, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and UV-curing resin, or a mixture of two or more resins selected from the said group of resins. In addition, polyethylene terephthalate resin can be suitably used as the polyester resin.

[0120] These media resins may contain a polymeric dispersant having one or more functional groups selected from amine-containing groups, hydroxyl groups, carboxyl groups, and epoxy groups in the main framework.

[0121] The solid medium is not limited to a medium resin, and a binder using a metal alkoxide can also be used as the solid medium. Representative examples of such metal alkoxides include alkoxides of Si, Ti, Al, and Zr. It is also possible to make the solid medium into a dispersion of electromagnetic wave-absorbing particles containing oxides by hydrolyzing and polycondensing the binder using these metal alkoxides through heating or the like.

[0122] The content ratio of electromagnetic wave absorbing particles in the electromagnetic wave absorbing particle dispersion related to the present embodiment is not particularly limited, but it is preferable that the electromagnetic wave absorbing particle dispersion contains 0.001 mass% or more and 80 mass% or less of electromagnetic wave absorbing particles.

[0123] Although the shape of the electromagnetic wave absorbing particle dispersion of the present embodiment is not particularly limited, it is preferable that the electromagnetic wave absorbing particle dispersion of the present embodiment have a sheet shape, a board shape, or a film shape. This is because the electromagnetic wave absorbing particle dispersion can be applied to various uses by making it a sheet shape, a board shape, or a film shape.

[0124] (2) Method for manufacturing an electromagnetic wave-absorbing particle dispersion

[0125] The method for manufacturing an electromagnetic wave-absorbing particle dispersion of the present embodiment is described below. Furthermore, this description merely illustrates an example of the configuration of the method for manufacturing an electromagnetic wave-absorbing particle dispersion, and the method for manufacturing an electromagnetic wave-absorbing particle dispersion described above is not limited to the following examples.

[0126] The electromagnetic wave absorbing particle dispersion of the present embodiment can be manufactured, for example, using a masterbatch. In this case, the method for manufacturing the electromagnetic wave absorbing particle dispersion of the present embodiment may, for example, include the following masterbatch manufacturing process.

[0127] Masterbatch production process for obtaining a masterbatch in which electromagnetic wave absorbing particles are dispersed in a solid medium.

[0128] In the masterbatch production process, a masterbatch in which electromagnetic wave absorbing particles are dispersed in a solid medium can be produced.

[0129] The specific method for producing the masterbatch is not particularly limited. For example, the masterbatch can be produced by dispersing an electromagnetic wave absorbing particle dispersion or electromagnetic wave absorbing particles in a solid medium and pelletizing the solid medium.

[0130] In addition, as electromagnetic wave absorbing particles, an electromagnetic wave absorbing particle dispersion powder obtained by removing the liquid medium from an electromagnetic wave absorbing particle dispersion may also be used.

[0131] For example, a mixture is prepared by uniformly mixing an electromagnetic wave absorbing particle dispersion, electromagnetic wave absorbing particles, an electromagnetic wave absorbing particle dispersion powder, a solid medium granule or pellet, and, if necessary, other additives. Then, a masterbatch can be manufactured by kneading the mixture using a vented single-screw or double-screw extruder and processing it into a pellet shape by cutting the melt-extruded strand. In this case, the pellet shape may be cylindrical or prismatic. Additionally, it is possible to employ the so-called hot-cut method, which involves directly cutting the melt-extruded material, when producing the pellets. In this case, it is common to take a shape close to spherical.

[0132] Furthermore, in the masterbatch manufacturing process, when an electromagnetic wave-absorbing particle dispersion is used as a raw material, it is desirable to reduce or remove the liquid medium originating from the electromagnetic wave-absorbing particle dispersion. In this case, the extent to which the liquid medium contained in the electromagnetic wave-absorbing particle dispersion is removed is not particularly limited. For example, it is desirable to remove the liquid medium from the electromagnetic wave-absorbing particle dispersion, etc., up to an amount that is permissible to remain in the said masterbatch. Additionally, if a liquid plasticizer is used as the liquid medium, the entire amount of said liquid plasticizer may remain in the electromagnetic wave-absorbing particle dispersion.

[0133] The method for reducing or removing the liquid medium contained in the electromagnetic wave-absorbing particle dispersion from the electromagnetic wave-absorbing particle dispersion or from the mixture of the electromagnetic wave-absorbing particle dispersion and the solid medium is not particularly limited. For example, it is preferable to dry the electromagnetic wave-absorbing particle dispersion, etc. under reduced pressure. Specifically, the electromagnetic wave-absorbing particle dispersion, etc. is dried under reduced pressure while stirring, and the components of the electromagnetic wave-absorbing particle-containing composition and the liquid medium are separated. As for the apparatus used for said reduced pressure drying, a vacuum stirring type dryer may be used, but any apparatus having the above function is acceptable and is not particularly limited. In addition, the pressure value during the reduced pressure of the drying process is appropriately selected.

[0134] By using the vacuum drying method described above, the removal efficiency of liquid media originating from the electromagnetic wave-absorbing particle dispersion is improved. Furthermore, since the electromagnetic wave-absorbing particle dispersion powder obtained after vacuum drying and the raw material electromagnetic wave-absorbing particle dispersion are not exposed to high temperatures for extended periods, it is desirable that aggregation of the electromagnetic wave-absorbing particles dispersed in the dispersion powder or the dispersion does not occur. Additionally, the productivity of the electromagnetic wave-absorbing particle dispersion powder is increased, and it is easy to recover solvents such as evaporated liquid media, which is also desirable from an environmental perspective.

[0135] In the electromagnetic wave absorbing particle dispersion powder obtained after the drying process, it is desirable to sufficiently remove solvent components with a boiling point of 120°C or lower. For example, it is desirable that the residual amount of the relevant solvent component be 2.5 mass% or less. This is because if the residual solvent component is 2.5 mass% or less, bubbles do not form when the electromagnetic wave absorbing particle dispersion powder is processed, for example, into an electromagnetic wave absorbing particle dispersion, and thus the appearance and optical properties are maintained in good condition. Furthermore, if the residual solvent component in the electromagnetic wave absorbing particle dispersion powder is 2.5 mass% or less, aggregation due to natural drying of the residual solvent component does not occur when the electromagnetic wave absorbing particle dispersion powder is stored for a long period, thereby maintaining long-term stability.

[0136] The obtained masterbatch can adjust its dispersion concentration while maintaining the dispersion state of the electromagnetic wave absorbing particles contained in the electromagnetic wave absorbing particle dispersion by adding a solid medium and mixing.

[0137] In addition, the method for manufacturing an electromagnetic wave absorbing particle dispersion of the present embodiment may include a molding process, if necessary, to mold the obtained masterbatch or the masterbatch to which a solid medium has been added as described above, into an electromagnetic wave absorbing particle dispersion of a desired shape.

[0138] The specific method for forming the electromagnetic wave absorbing particle dispersion is not particularly limited, but known methods such as extrusion molding and injection molding may be used.

[0139] In the forming process, for example, an electromagnetic wave absorbing particle dispersion in the form of a sheet, board, or film formed into a planar or curved surface can be manufactured. The method of forming into a sheet, board, or film shape is not particularly limited, and various known methods may be used. For example, the calender roll method, extrusion method, casting method, inflation method, etc., may be used.

[0140] The method for manufacturing an electromagnetic wave absorbing particle dispersion of the present embodiment is not limited to the form having the masterbatch manufacturing process described above.

[0141] For example, the method for manufacturing an electromagnetic wave absorbing particle dispersion of the present embodiment may be in the form having the following process.

[0142] A process for preparing a precursor liquid by mixing a monomer, oligomer, and an uncured, liquid solid medium precursor with electromagnetic wave absorbing particles (electromagnetic wave absorbing particle dispersion powder) or an electromagnetic wave absorbing particle dispersion liquid to prepare an electromagnetic wave absorbing particle dispersion precursor liquid.

[0143] A process for producing an electromagnetic wave absorbing particle dispersion by curing a solid medium precursor, such as the above monomer, through a chemical reaction such as condensation or polymerization.

[0144] For example, when using acrylic resin as a solid medium, an electromagnetic wave absorbing particle dispersion precursor can be obtained by mixing an acrylic monomer or an acrylic-based UV-curing resin with electromagnetic wave absorbing particles.

[0145] Next, if the precursor liquid of the electromagnetic wave absorbing particle dispersion is filled into a predetermined mold or the like and radical polymerization is performed, an electromagnetic wave absorbing particle dispersion using acrylic resin is obtained.

[0146] Even when using a resin that hardens by crosslinking as a solid medium, a dispersion can be obtained by performing a crosslinking reaction on the electromagnetic wave absorbing particle dispersion precursor liquid, just as in the case where the acrylic resin described above is used.

[0147] (3) Additives

[0148] When a medium resin is used as the solid medium, the electromagnetic wave absorbing particle dispersion of the present embodiment may contain known additives (additives), such as plasticizers, flame retardants, anti-coloring agents, and fillers, which are typically added to these resins. Above all, as previously explained, the solid medium is not limited to a medium resin, and a binder using a metal alkoxide can also be used.

[0149] The shape of the electromagnetic wave absorbing particle dispersion related to the present embodiment is not particularly limited, but as previously explained, it may take the form of, for example, a sheet shape, a board shape, or a film shape.

[0150] When an electromagnetic wave-absorbing particle dispersion in the form of a sheet, board, or film is used as an intermediate layer for a transparent substrate such as laminated glass, the solid medium contained in said electromagnetic wave-absorbing particle dispersion may not possess sufficient flexibility or adhesion to the transparent substrate as is. In this case, it is preferable for the electromagnetic wave-absorbing particle dispersion to contain a plasticizer. Specifically, for example, if said solid medium is polyvinyl acetal resin and is used for the above-mentioned application, it is also preferable for the electromagnetic wave-absorbing particle dispersion to contain a plasticizer.

[0151] As the plasticizer described above, a material used as a plasticizer in the solid medium used in the electromagnetic wave absorbing particle dispersion of the present embodiment may be used. For example, as a plasticizer used in an electromagnetic wave absorbing particle dispersion composed of polyvinyl acetal resin, examples include a plasticizer that is a compound of a monohydric alcohol and an organic acid ester, an ester-based plasticizer such as a polyhydric alcohol organic acid ester compound, and a phosphate-based plasticizer such as an organic phosphate-based plasticizer. Any plasticizer is preferably in a liquid state at room temperature. Among these, a plasticizer that is an ester compound synthesized from a polyhydric alcohol and a fatty acid is preferred.

[0152] (4) Application example

[0153] The electromagnetic wave absorbing particle dispersion of the present embodiment can be used in various forms, and its use and application modes are not particularly limited. Below, an electromagnetic wave absorbing transparent substrate, an electromagnetic wave absorbing intermediate film, and an electromagnetic wave absorbing laminate are described as application examples of the electromagnetic wave absorbing particle dispersion of the present embodiment.

[0154] (4-1) Electromagnetic wave absorbing transparent substrate

[0155] The electromagnetic wave absorbing transparent substrate of the present embodiment comprises a transparent substrate and an electromagnetic wave absorbing layer on at least one side of the transparent substrate, and the electromagnetic wave absorbing layer can be an electromagnetic wave absorbing particle dispersion as previously described.

[0156] The electromagnetic wave absorbing transparent substrate of the present embodiment may have a transparent substrate as described above. As the transparent substrate, one or more types selected from, for example, a transparent film substrate and a transparent glass substrate may be preferably used.

[0157] The film substrate is not limited to a film shape and may, for example, be in the shape of a board or a sheet. As the material of the film substrate, one or more types selected from polyester resin, acrylic resin, urethane resin, polycarbonate resin, polyethylene resin, ethylene vinyl acetate copolymer, vinyl chloride resin, fluoropolymer, etc., may be suitably used and can be used for various purposes. Above all, as the material of the film substrate, it is preferable that it be polyester resin, and in particular, it is more preferable that it be polyethylene terephthalate resin (PET resin). That is, the film substrate is preferably a polyester resin film, and more preferably a polyethylene terephthalate resin film.

[0158] When using a film substrate as a transparent substrate, it is desirable that the surface of the film substrate be surface-treated to facilitate the adhesion of the electromagnetic wave absorption layer.

[0159] In addition, to improve the adhesion between the glass substrate or film substrate and the electromagnetic wave absorption layer, it is also a desirable configuration to form an intermediate layer on the glass substrate or film substrate and to form an electromagnetic wave absorption layer on the intermediate layer. The composition of the intermediate layer is not particularly limited and can be composed of, for example, a polymer film, a metal layer, an inorganic layer (e.g., an inorganic oxide layer such as silica, titania, or zirconia), an organic / inorganic composite layer, etc.

[0160] Since the electromagnetic wave absorbing particle dispersion has already been explained, a description thereof is omitted here. Additionally, while the shape of the electromagnetic wave absorbing particle dispersion is not particularly limited, it is preferable to have, for example, a sheet shape, a board shape, or a film shape.

[0161] A method for manufacturing an electromagnetic wave-absorbing transparent substrate of the present embodiment is described.

[0162] The electromagnetic wave absorbing transparent substrate of the present embodiment can be manufactured by forming an electromagnetic wave absorbing layer on a transparent substrate, which is an electromagnetic wave absorbing particle dispersion in which electromagnetic wave absorbing particles are dispersed in a solid medium, using, for example, the electromagnetic wave absorbing particle dispersion liquid previously described.

[0163] Therefore, the method for manufacturing an electromagnetic wave-absorbing transparent substrate of the present embodiment may have, for example, the following process.

[0164] A coating process for applying a coating solution containing the previously described electromagnetic wave absorbing particle dispersion to the surface of a transparent substrate.

[0165] Electromagnetic wave absorption layer formation process, in which an electromagnetic wave absorption layer is formed after evaporating the liquid medium in the coating solution.

[0166] The coating solution used in the coating process can be prepared, for example, by adding and mixing a solid medium, such as a resin or a metal alkoxide, or a solid medium precursor to the electromagnetic wave absorbing particle dispersion solution already described.

[0167] As previously explained, a solid medium precursor refers to one or more types selected from monomers, oligomers, and uncured solid media of the solid medium.

[0168] When an electromagnetic wave absorption layer, which is a coating film, is formed on a transparent substrate, the electromagnetic wave absorption layer becomes a state in which cesium tungsten oxide particles are dispersed in a solid medium. Therefore, the electromagnetic wave absorption layer becomes a dispersion of electromagnetic wave-absorbing particles. In this way, by providing a dispersion of electromagnetic wave-absorbing particles on the surface of a transparent substrate, an electromagnetic wave-absorbing transparent substrate can be manufactured.

[0169] As for solid media or solid media precursors, they have already been explained in (1) electromagnetic wave absorbing particle dispersions and (2) the method for manufacturing electromagnetic wave absorbing particle dispersions, so they will be omitted here.

[0170] In order to provide an electromagnetic wave absorption layer on a transparent substrate, the method of applying a coating solution onto the transparent substrate is any method capable of uniformly applying the coating solution to the surface of the transparent substrate and is not particularly limited. Examples include bar coating, gravure coating, spray coating, dip coating, spin coating, screen printing, roll coating, pour coating, etc.

[0171] Here, the procedure for manufacturing an electromagnetic wave absorption layer on the surface of a transparent substrate is explained, using an example where a UV-curing resin is used as the medium resin and the layer is formed by applying it using a bar coating method.

[0172] A coating solution, with the concentration and additives appropriately adjusted to have suitable leveling properties, is applied onto a transparent substrate using a wire bar of a number that satisfies the purpose of the thickness of the electromagnetic wave absorption layer and the content of electromagnetic wave absorption particles. Then, after removing a solvent, such as a liquid medium, contained in the coating solution by drying, a coating layer that is an electromagnetic wave absorption layer can be formed on the transparent substrate by curing it through irradiation with ultraviolet light.

[0173] The drying conditions of the coating film vary depending on the type and ratio of each component and solvent, but typically, they are at a temperature of 60°C or higher and 140°C or lower for 20 seconds or more and 10 minutes or less. There are no particular restrictions on ultraviolet irradiation, and, for example, ultraviolet exposure devices such as ultra-high pressure mercury lamps can be suitably used.

[0174] Additionally, the adhesion between the substrate and the electromagnetic wave absorption layer, the smoothness of the coating film during coating, and the drying properties of the organic solvent may be manipulated by the preceding and succeeding processes (pre-process, post-process) for the formation of the electromagnetic wave absorption layer. Examples of the preceding and succeeding processes include a surface treatment process of the substrate, a pre-bake (pre-heating of the substrate) process, and a post-bake (post-heating of the substrate) process, and can be appropriately selected. It is preferable that the heating temperature in the pre-bake or post-bake process be, for example, 80°C or higher and 200°C or lower, and the heating time be 30 seconds or higher and 240 seconds or lower.

[0175] The method for manufacturing the electromagnetic wave-absorbing transparent substrate of the present embodiment is not limited to the above method. As another example of the method for manufacturing the electromagnetic wave-absorbing transparent substrate of the present embodiment, a form having the following process may also be cited.

[0176] Electromagnetic wave absorbing particle dispersion coating and drying process, wherein the previously described electromagnetic wave absorbing particle dispersion is applied to the surface of a transparent substrate and dried.

[0177] A binder application and curing process in which a binder using a solid medium such as a resin or a metal alkoxide, or a solid medium precursor, is applied and cured on a surface coated with an electromagnetic wave absorbing particle dispersion.

[0178] In this case, a film in which electromagnetic wave-absorbing particles are dispersed is formed on the surface of a transparent substrate by the application and drying process of the electromagnetic wave-absorbing particle dispersion. Additionally, the electromagnetic wave-absorbing particle dispersion can be applied by the same method as described for the application process of the previously described method for manufacturing an electromagnetic wave-absorbing transparent substrate.

[0179] In addition, by applying a binder onto a film in which the electromagnetic wave absorbing particles are dispersed and curing it, the cured binder is positioned between the electromagnetic wave absorbing particles, thereby forming an electromagnetic wave absorbing layer.

[0180] The electromagnetic wave absorbing transparent substrate may additionally have a coating layer on the surface of the electromagnetic wave absorbing particle dispersion. That is, it may be provided with a multilayer film.

[0181] The coating layer may be a coating film of an oxide containing, for example, one or more types selected from Si, Ti, Zr, and Al. In this case, the coating layer may be formed by applying a coating solution containing one or more types selected from an alkoxide containing one or more types selected from Si, Ti, Zr, and Al, and a partially hydrolyzed condensation polymer of said alkoxide, onto an electromagnetic wave absorption layer, for example, and then heating.

[0182] By forming a coating layer, the coated component fills the gaps where electromagnetic wave absorbing particles are deposited in the first layer and forms a film, thereby suppressing the refraction of visible light. Consequently, the haze value of the film is further reduced, and the transmittance of visible light can be improved. Additionally, the adhesion of the electromagnetic wave absorbing particles to the substrate can be improved.

[0183] Here, as a method for forming a coating film containing an alkoxide containing one or more of Si, Ti, Zr, and Al, or a partially hydrolyzed condensation compound thereof, on a film containing electromagnetic wave absorbing particles or a film containing electromagnetic wave absorbing particles, a coating method is preferred in terms of ease of film formation operation and cost.

[0184] As a coating solution used in the above coating method, it is suitably possible to use one or more alkoxides containing one or more of Si, Ti, Zr, and Al, or one or more partially hydrolyzed condensation compounds of said alkoxides, in a solvent such as water or alcohol. The content of said alkoxides, etc. in the coating solution is not particularly limited, but, for example, it is preferably 40 mass% or less in terms of oxides in the coating obtained after heating. In addition, if necessary, an acid or an alkali may be added to adjust the pH.

[0185] By applying the coating solution as a second layer onto a film composed mainly of electromagnetic wave absorbing particles and heating it, an oxide film comprising one or more types selected from Si, Ti, Zr, and Al can be easily formed as the coating layer. It is also preferable to use an organosilazan solution as a binder component or a component of the coating solution used in the coating solution related to the present embodiment.

[0186] As an inorganic binder or coating film, the heating temperature of the substrate after application of an electromagnetic wave absorbing particle dispersion or coating solution comprising one or more types of metal alkoxides among Si, Ti, Zr, and Al, and a hydrolyzed polymer thereof is not particularly limited. For example, the substrate heating temperature is preferably 100°C or higher, and more preferably is higher than the boiling point of the solvent in the coating solution such as the electromagnetic wave absorbing particle dispersion.

[0187] This is because if the substrate heating temperature is 100°C or higher, the polymerization reaction of the metal alkoxide or the hydrolysis polymer of said metal alkoxide contained in the film can be completed. In addition, if the substrate heating temperature is 100°C or higher, water or organic solvents, which are solvents, hardly remain in the film, so these solvents do not cause a reduction in visible light transmittance in the film after heating.

[0188] The thickness of the electromagnetic wave absorption layer on the transparent substrate of the present embodiment is not particularly limited, but for practical purposes, it is preferable to be 10 μm or less, and more preferable to be 6 μm or less. This is because if the thickness of the electromagnetic wave absorption layer is 10 μm or less, it exhibits sufficient pencil hardness and abrasion resistance, and in addition, it can avoid process abnormalities such as warping of the substrate film during the volatilization of the solvent and curing of the binder in the electromagnetic wave absorption layer.

[0189] (4-2) Intermediate membrane for electromagnetic wave absorption, electromagnetic wave absorption laminate

[0190] The electromagnetic wave absorbing laminate of the present embodiment may have a laminated structure comprising the previously described electromagnetic wave absorbing particle dispersion and a transparent substrate. The electromagnetic wave absorbing laminate of the present embodiment may be a laminate having the previously described electromagnetic wave absorbing particle dispersion and a transparent substrate as elements, and having them laminated.

[0191] As an electromagnetic wave absorbing laminate, for example, two or more transparent substrates and the electromagnetic wave absorbing particle dispersion described above can be laminated. In this case, the electromagnetic wave absorbing particle dispersion can be placed between, for example, the transparent substrates and used as an intermediate film for electromagnetic wave absorption.

[0192] In this case, it is preferable that the intermediate film for electromagnetic wave absorption have a sheet shape, a board shape, or a film shape.

[0193] One or more types of transparent substrates selected from transparent plate glass, plate-shaped plastic, and film-shaped plastic in the visible light region can be suitably used.

[0194] When plastic is used as a transparent substrate, the material of the plastic is not particularly limited and can be selected according to the application. For example, one or more types selected from polycarbonate resin, acrylic resin, polyester resin, polyamide resin, vinyl chloride resin, olefin resin, epoxy resin, polyimide resin, ionomer resin, fluoropolymer resin, etc. may be used. In addition, polyethylene terephthalate resin can be suitably used as the polyester resin.

[0195] The transparent substrate may contain particles having a solar radiation shielding function. As particles having a solar radiation shielding function, electromagnetic wave absorbing particles having near-infrared shielding properties may be used.

[0196] By interposing the previously described electromagnetic wave absorbing particle dispersion as a component of an intermediate layer that is clamped between multiple transparent substrates, a solar radiation shielding customized structure, which is a type of electromagnetic wave absorbing laminate that transmits visible light while having a near-infrared shielding function, can be obtained.

[0197] In addition, multiple opposing transparent substrates can be joined by a known method and integrated to form the electromagnetic wave absorbing laminate described above.

[0198] When the previously described electromagnetic wave absorbing particle dispersion is used as an electromagnetic wave absorbing intermediate film, the solid medium may be the one described in the section on electromagnetic wave absorbing particle dispersion. However, from the perspective of increasing the adhesion strength between the electromagnetic wave absorbing intermediate film and the transparent substrate, it is preferable that the solid medium be a polyvinyl acetal resin.

[0199] The electromagnetic wave absorbing intermediate film of the present embodiment can be manufactured by the method for manufacturing an electromagnetic wave absorbing particle dispersion described above, and can be an electromagnetic wave absorbing intermediate film having any shape, such as a sheet shape, a board shape, or a film shape.

[0200] In addition, if the electromagnetic wave absorbing intermediate film does not possess sufficient flexibility or adhesion to the transparent substrate, it is desirable to add a liquid plasticizer for the medium resin. For example, if the medium resin used in the electromagnetic wave absorbing intermediate film is polyvinyl acetal resin, the addition of a liquid plasticizer for polyacetal resin is beneficial for improving adhesion to the transparent substrate.

[0201] As a plasticizer, a substance used as a plasticizer for the media resin may be used. For example, as a plasticizer used in an infrared shielding film composed of polyvinyl acetal resin, examples include plasticizers that are compounds of monohydric alcohols and organic acid esters, ester-based plasticizers such as polyhydric alcohol organic acid ester compounds, and phosphate-based plasticizers such as organic phosphate-based plasticizers. In any case, it is preferable that the plasticizer be in a liquid state at room temperature. Among these, a plasticizer that is an ester compound synthesized from a polyhydric alcohol and a fatty acid is preferred.

[0202] In addition, at least one selected from the group consisting of a silane coupling agent, a metal salt of a carboxylic acid, a metal hydroxide, and a metal carbonate may be added to the intermediate film for electromagnetic wave absorption. The metal constituting the metal salt of the carboxylic acid, the metal hydroxide, and the metal carbonate is not particularly limited, but it is preferable that it be at least one selected from sodium, potassium, magnesium, calcium, manganese, cesium, lithium, rubidium, and zinc. In the intermediate film for electromagnetic wave absorption, it is preferable that the content of at least one selected from the group consisting of a metal salt of a carboxylic acid, a metal hydroxide, and a metal carbonate is 1 mass% or more and 100 mass% or less with respect to the electromagnetic wave absorbing particles.

[0203] In addition, the electromagnetic wave absorbing intermediate film may, if necessary, contain at least one type of particle among oxide particles, complex oxide particles, and boride particles containing two or more elements selected from the group consisting of Sb, V, Nb, Ta, W, Zr, F, Zn, Al, Ti, Pb, Ga, Re, Ru, P, Ge, In, Sn, La, Ce, Pr, Nd, Gd, Tb, Dy, Ho, Y, Sm, Eu, Er, Tm, Tb, Lu, Sr, and Ca, in addition to the electromagnetic wave absorbing particles already described. The electromagnetic wave absorbing intermediate film may contain the related particles in a range of 5 mass% or more and 95 mass% or less when the total with the electromagnetic wave absorbing particles is 100 mass%.

[0204] The electromagnetic wave absorbing laminate may contain an ultraviolet absorber in at least one layer of an intermediate film disposed between transparent substrates. As for the ultraviolet absorber, one or more types selected from compounds having a malonic acid ester structure, compounds having an oxalate anilide structure, compounds having a benzotriazole structure, compounds having a benzophenone structure, compounds having a triazine structure, compounds having a benzoate structure, compounds having a hindered amine structure, etc.

[0205] In addition, the intermediate layer of the electromagnetic wave absorbing laminate may be composed solely of the electromagnetic wave absorbing intermediate film related to the present embodiment.

[0206] The electromagnetic wave absorbing intermediate film described herein is one embodiment of an electromagnetic wave absorbing particle dispersion. It goes without saying that the electromagnetic wave absorbing particle dispersion related to this embodiment can be used without being clamped onto two or more transparent substrates that transmit visible light. That is, the electromagnetic wave absorbing particle dispersion related to this embodiment can exist as an electromagnetic wave absorbing particle dispersion on its own.

[0207] The electromagnetic wave absorbing laminate related to the present embodiment is not limited to the form in which an electromagnetic wave absorbing particle dispersion is placed between transparent substrates as described above, and any configuration may be taken as long as it has a laminated structure including an electromagnetic wave absorbing particle dispersion and a transparent substrate.

[0208] Examples

[0209] The present invention will be described in more detail below with reference to the examples. However, the present invention is not limited to the following examples.

[0210] Here, the evaluation method in the following examples and comparative examples will first be explained.

[0211] (Chemical analysis)

[0212] Chemical analysis of the obtained electromagnetic wave absorbing particles was performed by atomic absorption analysis (AAS) for Cs and by ICP emission spectroscopy (1CP-OES) for W (tungsten). In addition, O was analyzed using a light element analysis device (LECO, model ON-836), by melting the sample in He gas and quantifying the CO gas that reacted with carbon in the crucible using IR absorption spectroscopy. Table 1 shows the composition ratio calculated with W (tungsten) set to 1, derived from the content ratio of each element obtained by chemical analysis. Furthermore, in the following Examples 1 to 13, a powder of electromagnetic wave absorbing particles containing a cesium-tungsten composite oxide having a W deficiency was obtained. For this reason, for powders A to M, which are electromagnetic wave absorbing particles obtained in Examples 1 to 13, the composition ratio obtained by multiplying the value corresponding to the W deficiency by the composition ratio when W is set to 1 as shown in Table 1 is all the general formula Cs x W 1-y O 3-z (0.2≤x≤0.4, 0 <y≤0.4, 0<z≤0.46)를 충족함을 확인할 수 있다.

[0213] (X-ray diffraction measurement)

[0214] X-ray diffraction measurements were performed by measuring the powder using Cu-Kα rays with the Spectris X'Pert-PRO / MPD instrument.

[0215] Measurements were performed after calibrating the diffraction angles with a standard sample (NIST640e). Then, Rietveld analysis was performed on the obtained XRD diffraction patterns to determine the lattice constants of the crystal phases. In addition, if orthorhombic is included, it is denoted as R in Table 1, and if hexagonal is included, it is denoted as H. In addition, if both orthorhombic and hexagonal are included, it is denoted as R+H in Table 1.

[0216] In the case of the mixed phase of orthorhombic and hexagonal phases, lattice constants for each phase were determined. Then, the orthorhombic lattice constants were converted into hexagonal lattice constants by the following lattice correspondence model. The correspondence of lattice changes between orthorhombic and hexagonal phases is given by Equation 4a, extracted from the model of Solodovnikov 1998 (Non-patent Literature 4). orth 2 +b orth 2 =64a hex 2 =64b hex 2 , c orth =c hex Using, the hexagonal converted lattice constant was calculated. In addition, a in the above equation orth , b orth , c orth represents the lengths of the a-axis, b-axis, and c-axis of an orthorhombic shape. Also, a hex , b hex , c hex represents the lengths of the a-axis, b-axis, and c-axis of the hexagon.

[0217] (Optical properties of electromagnetic wave-absorbing transparent substrates)

[0218] The visible light transmittance (VLT) and solar irradiance transmittance (ST) of the electromagnetic wave-absorbing transparent substrate were measured in accordance with ISO 9050 and JIS R 3106. Specifically, transmittance was measured using a spectrophotometer U-4100 manufactured by Hitachi Seisakusho Co., Ltd., and calculated by multiplying by a coefficient based on the spectrum of sunlight. For transmittance measurement, measurements were taken at 5 nm intervals over a wavelength range of 300 nm to 2100 nm. L * a * b * The color index was calculated by determining the tristimulus values ​​X, Y, and Z for a D65 standard light source and a light source angle of 10° in accordance with JIS Z8701, and then obtaining the color index from the tristimulus values ​​in accordance with JIS Z8729. The RGB color index was calculated from the tristimulus values ​​in the same manner.

[0219] [Example 1]

[0220] Cesium carbonate (Cs2CO3) and tungsten trioxide (WO3) were weighed, mixed, and kneaded in a molar ratio of Cs2CO3:WO3 = 2:11. The resulting mixture was placed in a carbon boat and heated twice at 850°C for 20 hours in an atmospheric tubular furnace to obtain powder A', which is an extremely thin, greenish-white powder. Additionally, when heating, after heating at 850°C for 20 hours, the mixture was removed, ground, and mixed, and then reheated under the same conditions.

[0221] The obtained white powder, Powder A', was evaluated as follows.

[0222] The X-ray powder diffraction pattern is slightly Cs6W 11 O 36 It's mixed, but almost Cs4W 11 O 35 It was identified as a single phase (ICDD 00-51-1891).

[0223] The lattice constants were measured as a=14.6733Å, b=52.3841Å, and c=7.7424Å. The related values ​​were very close to those of Solodovnikov (Non-patent Literature 4), a=14.6686Å, b=52.3971Å, and c=7.7356Å. The chemical analysis results of this white powder are Cs 0.36 WO 3.18 It became so that it almost matched the weighing composition.

[0224] Next, TEM observation was performed on the obtained white powder, powder A'. When the limited field electron diffraction pattern was taken, an orthorhombic spot pattern was obtained. Figure 4 shows the spot pattern taken from the c-axis direction of the orthorhombic. Periodicity of b / 8 periods was observed in the b-axis direction, confirming the existence of W and O defect planes. Additionally, from the streaks extending in the b-axis direction, it was found that some plane defects exist on the b-plane. Although this spot pattern from the c-axis is close to 6-fold symmetry, the angle between the (480) and (4-80) spots is 52.2°, which deviates from 60° in the case of 6-fold symmetry, and it is thought that the deviation from 6-fold symmetry is due to the W and O defect planes that entered the b / 8 period.

[0225] The obtained white powder, Cs4W 11 O 35 The powder was spread thinly and evenly in a carbon boat, placed inside a tubular furnace, and heated from room temperature to 800°C in an Ar gas stream. While maintaining the temperature at 800°C, the flow was switched to a mixture of 1 vol% H2 gas (hereinafter, vol% is simply indicated as %) using Ar gas as a carrier, and after reducing for 5 minutes, the H2 gas was stopped and the mixture was slowly cooled to 100°C using only the Ar gas stream. Afterward, the Ar gas stream was stopped and the mixture was slowly cooled to room temperature, and powder A was removed. The color of the removed powder A was aquatic.

[0226] The XRD pattern of powder A exhibited a mixed two-phase pattern of orthorhombic and hexagonal phases. Lattice constants for each phase were determined using the Rietveld method; for the orthorhombic phase, a=14.6609Å, b=52.4040Å, and c=7.7419Å (converted values ​​for hexagonal were a=7.5062Å and c=7.7419Å), and for the hexagonal phase, a=7.4170Å and c=7.5752Å. It was confirmed that the values ​​on the c-axis for both phases fell within the range of 7.560Å ≤ c ≤ 7.750Å.

[0227] Next, TEM observation of powder A was performed, and orthorhombic particles and pseudo-hexagonal particles were observed.

[0228] Here, the electron beam diffraction pattern of a pseudo-hexagonal particle is shown in FIG. 5. The pseudo-hexagonal particle is

[0001] of FIG. 5 HEX As indicated by the electron beam diffraction pattern of the normal axis, it exhibited a diffraction pattern close to hexagonal. Here (200) HEX Wow (110) HEX The interplanar angle was measured to be 59.2°, which was a value close to a hexagon.

[0229] Next, powder A was observed in STEM-HAADF mode (STEM: scanning transmission electron microscopy, HAADF: High-angle annular dark field).

[0230] Figure 6 shows the HAADF image observed from the

[0221] normal axis of a pseudo-hexagonal particle. In the HAADF mode, atomic particles are observed with brightness proportional to the atomic number and the probability of atomic existence in the projection direction, so the (110) that appears dark in Figure 6 HEX The linear region along the line was identified as a defect of W, which has the largest atomic number. The trace of this W defect region was observed from a different direction, (110) HEX It was confirmed that it is spread out in a planar shape. In addition, it is thought that some of the traces with thin contrast are contracted in a linear shape.

[0231] In this embodiment, the heat reduction treatment is performed for 5 minutes, which is shorter than the time described in other embodiments below, and at the beginning of the reduction at high temperature, orthorhombic (010) ORTH The W defect shrinks, causing a structural transition to a pseudo-hexagonal structure, and in the pseudo-hexagonal structure, {100} HEX Many W defect areas during shrinkage could be observed on the surface.

[0232] [Example 2]

[0233] Cs4W, which is powder A' obtained in Example 1 11 O 35 The powder was spread thinly and evenly in a carbon boat, placed inside a tubular furnace, and heated from room temperature to 800°C in an Ar gas stream. While maintaining the temperature at 800°C, the stream was switched to a mixture of 1% H2 gas with Ar gas as a carrier, and after reduction for 15 minutes, the H2 gas was stopped, and the mixture was slowly cooled to 100°C using only the Ar gas stream. Afterward, the Ar gas stream was stopped, and the mixture was slowly cooled to room temperature, and powder B was removed. The color of the removed powder B was blue.

[0234] The XRD pattern of powder B exhibited a mixed two-phase pattern of orthorhombic and hexagonal phases. Lattice constants for each phase were determined using the Rietveld method, yielding a=14.6576Å, b=52.4315Å, and c=7.7412Å for the orthorhombic phase (converted values ​​for hexagonal were a=7.5088Å and c=7.7412Å), and a=7.4122Å and c=7.5940Å for the hexagonal phase. It was confirmed that the values ​​on the c-axis for both phases fell within the range of 7.560Å ≤ c ≤ 7.750Å.

[0235] Next, TEM observation of powder B was performed, and as with powder A obtained in Example 1, orthorhombic particles and pseudo-hexagonal particles were observed. The pseudo-hexagonal particles are

[0001] of FIG. 7 HEXAs indicated by the electron beam diffraction pattern of the normal axis, it exhibited a diffraction pattern close to hexagonal. Here (200) HEX Wow (110) HEX The interplanar angle was measured to be 59.5°, which was a value close to a hexagon.

[0236] [Example 3]

[0237] Cs4W, which is powder A' obtained in Example 1 11 O 35 The powder was spread thinly and evenly in a carbon boat, placed inside a tubular furnace, and heated from room temperature to 800°C in an Ar gas stream. While maintaining the temperature at 800°C, the stream was switched to a mixture of 1% H2 gas with Ar gas as a carrier, and after reduction for 30 minutes, the H2 gas was stopped, and the mixture was slowly cooled to 100°C using only the Ar gas stream. Afterward, the Ar gas stream was stopped, and the mixture was slowly cooled to room temperature, and the powder C was removed. The color of the removed powder C was deep blue.

[0238] The XRD pattern of powder C exhibited a mixed two-phase pattern of orthorhombic and hexagonal phases. Lattice constants for each phase were determined using the Rietveld method, yielding a=14.6649Å, b=52.4010Å, and c=7.7451Å for the orthorhombic phase (converted values ​​for hexagonal were a=7.5064Å and c=7.7451Å), and a=7.4076Å and c=7.6107Å for the hexagonal phase. It was confirmed that the values ​​on the c-axis for both phases fell within the range of 7.560Å ≤ c ≤ 7.750Å.

[0239] Next, TEM observation of powder C was performed, and as with powder A obtained in Example 1, orthorhombic particles and pseudo-hexagonal particles were observed. The pseudo-hexagonal particles exhibited a hexagonal diffraction pattern, as indicated by the electron beam diffraction pattern along the

[0001] axis in Fig. 8. Here (200) HEX Wow (110) HEX The interplanar angle was measured as 60.0°, which became a hexagonal value.

[0240] [Examples 4 to 7]

[0241] Cs4W, which is powder A' obtained in Example 1 11 O 35 The reduction time during the reduction treatment of the powder was changed to 35 to 90 minutes, as shown in Table 1. Except for the above, powders D, E, F, and G were prepared in the same manner as when powder A of Example 1 was prepared. The color tone of powders D to G is all deep blue, and the XRD lattice constants are as shown in the table.

[0242] In addition, as shown in Table 1, in Example 4, an orthorhombic phase was also observed, and the c-axis length converted to a hexagonal phase was 7.7440 Å (Example 4).

[0243] [Examples 8 to 11]

[0244] Cs4W, which is powder A' obtained in Example 1 11 O 35 The heating temperature and reduction time during the heat reduction treatment of the powder were changed as shown in Table 1. Specifically, in Example 8, the time was 650°C for 120 minutes; in Example 9, 700°C for 60 minutes; in Example 10, 900°C for 10 minutes; and in Example 11, 950°C for 20 minutes. Except for the above points, powders H, I, J, and K were prepared in the same manner as when powder A was prepared in Example 1. Water-colored, blue, dark blue, and dark blue powders were obtained, respectively. The lattice constants obtained from the XRD patterns of each obtained powder were as shown in Table 1.

[0245] In addition, as shown in Table 1, in Examples 8 and 9 and the following Examples 12 and 13, an orthorhombic phase was also observed, and the c-axis length converted to a hexagonal phase was 7.7428 Å (Example 8), 7.7471 Å (Example 9), 7.7449 Å (Example 12), and 7.7466 Å (Example 13).

[0246] [Example 12]

[0247] Cesium carbonate and tungsten trioxide were mixed in a molar ratio of Cs2CO3:WO3 = 3:11, spread thinly and evenly in a carbon boat, placed inside a tubular furnace, and heated at 850°C for 5 hours to obtain an extremely thin, greenish-white powder. The main phase of this white powder was Cs6W 11 O 36 Identified with (ICDD1-70-632), but Cs4W 11 O 35 It was a mixed image with.

[0248] The obtained white powder was heat-treated at 800°C for 30 minutes in a 1% H2-N2 stream to obtain a deep blue powder L.

[0249] The XRD pattern of powder L showed a mixed two-phase pattern of orthorhombic and hexagonal. The lattice constants obtained from the XRD pattern of the obtained powder L are as shown in Table 1.

[0250] [Example 13]

[0251] Cesium carbonate and tungsten trioxide were mixed in a molar ratio of Cs2CO3:WO3 = 1:6, spread thinly and evenly in a carbon boat, placed inside a tubular furnace, and heated at 850°C for 5 hours to obtain an extremely thin, greenish-white powder. The main phase of this white powder was Cs4W 11 O 35 and sympathized, but Cs2W6O 19 It was a mixed image with (ICDD00-045-0522).

[0252] The obtained white powder was heat-treated at 800°C for 30 minutes in a 1% H2-N2 stream to obtain a deep blue powder M.

[0253] The XRD pattern of powder M showed a two-phase mixed pattern of orthorhombic and hexagonal. The lattice constants obtained from the XRD pattern of the obtained powder M are as shown in Table 1.

[0254] As shown in Examples 1 to 13 above, white Cs4W 11 O 35 I'm Cs6W 11 O 36 , Cs2W6O 19 Cs4W including 11 O 35 When the powder was reduced at a high temperature, the color of the powder gradually changed from watery to blue and dark blue.

[0255] Also Cs4W 11 O 35 It was confirmed that lattice defects containing W defects exist in the phase, and the structure is orthorhombic; however, when this is reduced at high temperature, the lattice defects containing W defects disappear, and the orthorhombic structure changes into a hexagonal structure.

[0256] [Example 14]

[0257] 20 mass% of powder A prepared in Example 1, 10 mass% of an acrylic polymer dispersant having a group containing an amine as a functional group (hereinafter abbreviated as "dispersant a"), and 70 mass% of methyl isobutyl ketone (MIBK) as a solvent were weighed. These weighed materials were placed in a glass container together with silica beads of 0.3 mm diameter, and dispersed and ground using a paint shaker for 5 hours to obtain dispersion A.

[0258] Here, when measuring the average particle size of the electromagnetic wave absorbing particles in dispersion A (the dispersion particle size measured by the ELS-8000 manufactured by Otsuka Denshi Co., Ltd., a particle size measuring device based on dynamic light scattering), it was 26.4 nm.

[0259] 50 parts by mass of a hard coating UV-curing resin (Doa Gosei Aronix UV-3701) was mixed with 100 parts by mass of this dispersion A to form an electromagnetic wave absorbing particle coating solution. Then, the related electromagnetic wave absorbing coating solution was applied using a bar coater onto a polyethylene terephthalate (PET) resin film (Teijin HPE-50, hereinafter also referred to as "PET film") which is a transparent film substrate, to form a coating film. In addition, the same PET film was used as the transparent substrate in other embodiments as well.

[0260] Electromagnetic wave absorbing film A, having a coating layer containing electromagnetic wave absorbing particles, was prepared by drying a PET film with a coating film at 80°C for 5 minutes to evaporate an organic solvent, which is a liquid medium, and then curing it with a high-pressure mercury lamp. In addition, the coating layer is an electromagnetic wave absorbing layer, and the electromagnetic wave absorbing film is a form of an electromagnetic wave absorbing transparent substrate.

[0261] For the obtained dispersion A, the transmittance was measured using a Hitachi High-Tech U-4100 spectrophotometer, and the molar absorption coefficient was determined. The profiles are shown in FIGS. 9a and 9b. FIGS. 9a shows the molar absorption coefficients of the dispersions of Examples 14 to 20 and Comparative Example 1, prepared using electromagnetic wave absorbing particles prepared in Examples 1 to 7. FIGS. 9b is a partial enlarged view of FIGS. 9a. FIGS. 9c shows the molar absorption coefficients of the dispersions of Examples 15, 16, 18, 22, 23 and Comparative Example 1, prepared using electromagnetic wave absorbing particles prepared in Examples 2, 3, 5, 9, and 10.

[0262] According to the profile shown in Fig. 9, absorption in the near-infrared region from 0.6 eV to 1.6 eV and transmission in the visible region from 1.6 eV to 3.0 eV could be confirmed.

[0263] The visible light transmittance (VLT) and solar irradiance transmittance (ST) of electromagnetic wave absorbing film A were measured as VLT=72.3% and ST=55.3%, respectively, indicating that, similar to dispersion A, it is transparent in visible light and also possesses a near-infrared absorption effect. The color index of electromagnetic wave absorbing film A is L * =88.4, a * =-1.4, b * It became 8.8, and the blue color was very weak and close to a neutral color, that is, it displayed a neutral hue.

[0264] [Example 15]

[0265] Powder B prepared in Example 2 was dispersed and ground in the same manner as in Example 14 to obtain dispersion B. The dispersion particle size was 31.4 nm. The profile of the molar absorption coefficient of this dispersion B is shown in FIGS. 9a to 9c. In addition, the transmittance profile of dispersion B is shown in FIGS. 10a and 10b. Furthermore, in deriving the transmittance profile, the transmittance profile was derived from the molar absorption coefficient using the Lambert-Beer equation so that the VLT value was the same as the VLT value of the spectral transmittance of dispersion A obtained in Example 14. The same method was used to derive the transmittance profile for the following Comparative Examples 1 to 3, Example 16, and Example 19, as shown in FIGS. 10a and 10b.

[0266] Since the solar shielding effect and transmittance color change depending on the VLT value of the film, their evaluation needs to be performed at the same VLT. Therefore, coating solution B was prepared by adjusting the mixing ratio of dispersion solution B, UV-curing resin, and MIBK so that the VLT value of the spectral transmittance obtained from the electromagnetic wave absorbing film of Example 14 is approximately the same as the VLT range (72.0% to 73.0%). Electromagnetic wave absorbing film B was prepared by applying, drying, and curing coating solution B to a PET film in the same manner as in Example 14.

[0267] The optical properties of electromagnetic wave absorption film B were VLT=72.7% and ST=41.6%, respectively, indicating that it possesses extremely good solar radiation shielding characteristics.

[0268] In addition, the color index of electromagnetic wave absorbing film B is L * =88.5, a * =-3.9, b * = 5.4, and b * This is positive, and the blue color is weak, exhibiting a hue close to a neutral color. In the rarefaction film of the electromagnetic wave absorbing particles used in automobile windshields at VLT=70 to 80%, it can be said that the film is one that hardly gives off a blue tint.

[0269] [Comparative Example 1]

[0270] Cs4W, which is powder A' obtained in Example 1 11 O 35 The powder was subjected to grinding and dispersion treatment in the same procedure as in Example 14 to obtain dispersion N. The color of dispersion N was grayish-white, and the dispersion particle size of the particles in dispersion N was 30.3 nm. The transmittance profile of dispersion N is shown in FIG. 10a and FIG. 10b.

[0271] In the same procedure as in Example 15, a coating solution N was obtained by adjusting the mixing ratio of dispersion N, UV-curing resin, and MIBK, and then an electromagnetic wave absorbing film N was obtained. Meanwhile, as for the spectral characteristics of the electromagnetic wave absorbing film N, VLT=72.6% and ST=80.2% were obtained, indicating that there was almost no infrared absorption effect.

[0272] [Comparative Example 2]

[0273] A raw material mixture was prepared by weighing, mixing, and kneading an aqueous solution of cesium carbonate (Cs2CO3), tungstic acid (H2WO4), and tungsten dioxide powder (WO2) to a composition of Cs2O·5WO3·4WO2. After thorough mixing, the raw material mixture was spread thinly and evenly in a carbon boat and maintained at 550°C for 60 minutes under a 1% H2 gas stream using N2 as a carrier. Subsequently, the stream was switched to 100% N2 and maintained for 1 hour, then the temperature was raised to 800°C and maintained for 1 hour, and finally cooled slowly to room temperature to obtain powder O. The color of powder O was deep blue. As a result of chemical analysis, the composition Cs 0.33 WO 2.74 was obtained.

[0274] The XRD pattern of powder O exhibited a hexagonal single phase. Rietveld analysis yielded lattice constants a = 7.4088 Å and c = 7.6033 Å. The value of the lattice constant c-axis was within the desired range.

[0275] Next, TEM observations were performed, and no particularly noticeable lattice defects were observed. In STEM atomic observations as well, no noticeable lattice defects were observed, and no W defects were observed.

[0276] Powder O was subjected to grinding and dispersion treatment in the same procedure as in Example 15 to obtain dispersion O. The color of dispersion O was deep blue. The dispersion particle size of the electromagnetic wave absorbing particles in dispersion O was 25.8 nm. The transmittance profile of dispersion O is shown in FIGS. 10a and FIGS. 10b.

[0277] After obtaining a coating solution O by adjusting the mixing ratio of dispersion O, UV-curing resin, and MIBK in the same manner as in Example 15, an electromagnetic wave absorbing film O was obtained.

[0278] As for the spectral characteristics of the electromagnetic wave absorbing film O, VLT=72.5%, ST=37.5%, and color index L * =88.2, a * =-5.7, b *=-2.8 was obtained. Therefore, the powder and dispersion have a strong near-infrared absorption effect, but the electromagnetic wave absorbing film O containing the dispersion is b * Since the value has a negative value, it can be seen that the blue tint is clearly perceived.

[0279] [Comparative Example 3]

[0280] As a reference sample for color tone, a dispersion of In2O3:Sn (hereinafter abbreviated as ITO) with a neutral color tone was prepared. It is known that ITO fine particles possess a neutral color tone, but depending on the reduction or manufacturing method, various types exist ranging from slightly bluish to brownish. Here, among them, ITO powder (Powder P) manufactured by ENAM, which is close to purely transparent, was used.

[0281] Powder P was subjected to grinding and dispersion treatment in the same procedure as in Example 14 to obtain dispersion P. The color of dispersion P was light watery. The dispersion particle size of the electromagnetic wave absorbing particles in dispersion P was 35.4 nm. The transmittance profile of dispersion P is shown in FIGS. 10a and FIGS. 10b.

[0282] After obtaining a coating solution P by adjusting the mixing ratio of dispersion P, UV-curing resin, and MIBK in the same manner as performed in Example 15, an electromagnetic wave absorbing film P was obtained. As for the spectral characteristics of the electromagnetic wave absorbing film P, VLT=72.7%, ST=47.8%, and color index L * =88.3, ​​a * =-2.2, b * =12.4 was obtained. Therefore, the electromagnetic wave absorbing film P comprising a dispersion using ITO powder and a dispersion solution is b * Since the value is a large positive value, it can be seen that the blue tint is very small and it is perceived as a neutral color. However, regarding the near-infrared absorption effect, it was confirmed to be the same as Example 15 and lower than Comparative Example 2.

[0283] [Examples 16 to 20]

[0284] Powders C to G prepared in Examples 3 to 7 were dispersed and ground in the same manner as in Example 14 to obtain dispersions C to G. The profiles of the molar absorption coefficients of each dispersion are shown in FIG. 9. In addition, the dispersion particle sizes of each dispersion are shown in Table 2.

[0285] Then, coating solutions C to G were obtained by adjusting the mixing ratio of each dispersion and UV-curing resin with MIBK, in the same manner as in Example 15. Electromagnetic wave absorbing films C to G were obtained using each coating solution. The optical properties and color index of each electromagnetic wave absorbing film are shown in Table 2.

[0286] In these electromagnetic wave absorbing films, it was found that as the reduction time at 800°C increases, near-infrared absorption increases, while the transmitted color shows a strong tendency toward blue. However, in all cases, it was confirmed that a color tone close to a neutral color was exhibited.

[0287] As previously explained, the transmittance profiles of the dispersions related to Comparative Examples 1 to 3, Example 15, Example 16, and Example 19 are summarized and illustrated in FIG. 10a and FIG. 10b is a partially enlarged view of FIG. 10a.

[0288] In addition, the solar transmittance (ST) of the dispersions related to Comparative Examples 1 to 3, Examples 15, 16, and 19 is illustrated in FIG. 11a, and the color indices are illustrated in FIG. 11b and FIG. 11c. Furthermore, in FIG. 11a to 11c, t on the horizontal axis R represents the reduction time at 800°C. For this reason, although explanations are provided only for parts of Figures 11a to 11c, t R This same example becomes the same experimental example.

[0289] In FIG. 10a and FIG. 10b, it can be seen that Comparative Example 1 has a low transmittance of the blue wavelength, while having a high transmittance of the red wavelength, and appears as a transparent film overall when used as a dispersion film (dispersant). Conversely, in Comparative Example 2, while the transmittance of the blue wavelength is high, the transmittance of the red wavelength drops significantly, and appears as a blue film overall when used as a dispersion film (dispersant).

[0290] The dispersions of Examples 15, 16, and 19 are intermediate with the dispersions of Comparative Examples 1 and 2. As the reduction time at 800°C increases, the transmittance of the blue wavelength gradually increases, while conversely, the transmittance of the red wavelength tends to decrease rapidly along with absorption in the near-infrared region. In Example 19, where the reduction time at 800°C is 60 minutes, the transmittance profile approaches that of Comparative Example 2. It can be seen that even with the same VLT value, the electromagnetic wave absorption film of Example 19 has a similar transmittance at the red wavelength but a lower transmittance at the blue wavelength, indicating a more neutral hue.

[0291] In FIG. 11a, it was confirmed that the dispersions of Examples 16 and 19, in which the reduction time at 800°C exceeded 20 minutes, exhibited superior characteristics in terms of solar irradiation shielding effect compared to the dispersion of Comparative Example 3 using ITO. Furthermore, when the reduction time at 800°C was 60 minutes, the conventional Cs 0.33 It is at almost the same level as the dispersion of Comparative Example 2 using WO3.

[0292] Regarding the color tones illustrated in Figs. 11b and 11c, b is used when the reduction time at 800°C is up to about 30 minutes. * The value is, Cs 0.33 It can be seen that the value is significantly improved, as it is much more neutral than Comparative Example 2 using WO3.

[0293] [Examples 21 to 24]

[0294] Powders H to K prepared in Examples 8 to 11 were dispersed and ground in the same manner as in Example 14 to obtain dispersions H to K. The dispersion particle sizes of the dispersions are shown in Table 2. In addition, the profile of the molar absorption coefficient of the obtained dispersions is shown in FIG. 9c.

[0295] Then, in the same procedure as in Example 15, the mixing ratio of each dispersion, UV-curing resin, and MIBK was adjusted, and coating solution H to coating solution K was adjusted so that the VLT of the electromagnetic wave absorbing film obtained from each dispersion was 72% to 74%, and then electromagnetic wave absorbing film H to electromagnetic wave absorbing film K was obtained.

[0296] The optical properties and color index of these electromagnetic wave absorbing films are shown in Table 2.

[0297] In these electromagnetic wave absorbing films, although the reduction temperature and time at 650°C to 950°C differ, it can be seen that as the degree of high-temperature reduction of the particles increases, the absorption of near-infrared rays increases, while the transmitted color shows a strong tendency toward blue. However, in all cases, it was confirmed that a color tone close to a neutral color was exhibited.

[0298] It was confirmed that the blue tendency of the transmitted color and the near-infrared absorption effect have a trade-off relationship, and that it is desirable to select an appropriate degree of high-temperature reduction depending on the application.

[0299] [Examples 25, 26]

[0300] Powder L and Powder M prepared in Examples 12 and 13 were dispersed and ground in the same manner as in Example 14 to obtain dispersion L and dispersion M. The dispersion particle sizes of the dispersions are shown in Table 2.

[0301] Then, in the same procedure as in Example 15, the mixing ratio of each dispersion, UV-curing resin, and MIBK was adjusted, and coating solution L and coating solution M were adjusted so that the VLT of the electromagnetic wave absorbing film obtained from each dispersion was about 72%, and then electromagnetic wave absorbing film L and electromagnetic wave absorbing film M were obtained.

[0302] The optical properties and color indices of these electromagnetic wave absorbing films are shown in Table 2. In these electromagnetic wave absorbing films, the composition and structure of the raw material powder are Cs6W 11 O 36 , or Cs2W6O 19 Cs4W including 11 O 35 Although slightly different from the powder, the change from orthorhombic to hexagonal accompanied by high-temperature reduction basically contains the same content, and it is thought that the characteristics of the electromagnetic wave absorption film depend mainly on the reduction conditions at high temperatures.

[0303] In other words, even if the raw material powder is changed between tungsten oxide Cs2O·nWO3 (3.6≤n≤9.0) containing Cs and W, it can be seen that as the degree of high-temperature reduction of the particles increases, the near-infrared absorption increases, while the transmitted color shows a stronger blue tendency. The blue tendency of the transmitted color and the near-infrared absorption effect are in a trade-off relationship, and an appropriate degree of high-temperature reduction can be selected depending on the application.

[0304] [Example 27]

[0305] Coating solution A was prepared by mixing dispersion C prepared in Example 16 with UV-curing resin (Doa Gosei Aronix UV3701) and MIBK. The obtained coating solution was applied to a 3 mm thick soda-lime glass substrate using a bar coater (Imoto Seisakusho IMC-700) to form a coating film, and after evaporating the solvent from the coating film, the coating film was cured by irradiating it with ultraviolet light using a high-pressure mercury lamp to produce an electromagnetic wave-absorbing transparent substrate having an electromagnetic wave-absorbing layer.

[0306] Regarding the electromagnetic wave-absorbing transparent substrate related to Example 27, optical properties were measured in the same manner as in Example 14, and VLT=72.2%, ST=37.0%, L * =88.6, a * =-3.8, b * = It was 4.3.

[0307] [Example 28]

[0308] The dispersion C prepared in Example 16 was subjected to removing MIBK from the solvent using a vacuum dryer to obtain electromagnetic wave absorbing particle dispersion powder C. 100 parts by mass of polycarbonate resin pellets and 0.15 parts by mass of dispersion powder C were uniformly mixed, then melt-kneaded at 290°C using a twin-screw extruder (manufactured by Toyo Seiki Seisakusho), and the extruded strand with a diameter of 3 mm was cut and pelletized to obtain masterbatch C. The polycarbonate resin pellets and masterbatch C were blended so that the VLT was approximately 72% when molded into a 2 mm thick polycarbonate sheet, and after obtaining a mixture by uniformly mixing, the mixture was molded into a sheet of 10 cm × 5 cm with a thickness of 2.0 mm using an injection molding machine to produce an electromagnetic wave absorbing particle dispersion related to Example 28. Regarding the electromagnetic wave absorbing particle dispersion related to Example 28, optical properties were measured in the same manner as in Example 14, and VLT=72.4%, ST=39.1%, L * =88.3, ​​a * =-4.4,b * = It was 4.6.

[0309] [Example 29]

[0310] A plasticizer dispersion was prepared by mixing dispersion powder C prepared in Example 28 with a plasticizer, which is a compound of a monohydric alcohol and an organic acid ester. The plasticizer dispersion and polyvinyl acetal resin were blended at a ratio such that the VLT of the electromagnetic wave absorbing laminate related to Example 29 was approximately 72%, and the mixture was prepared to form a resin composition and loaded into a twin-screw extruder. The resin composition was then kneaded at 200°C and extruded from a T-die to obtain an intermediate film, which is a dispersion of electromagnetic wave absorbing particles with a thickness of 0.7 mm, using the calender roll method. The obtained intermediate film was sandwiched between two soda-lime glass substrates to laminate the electromagnetic wave absorbing laminate related to Example 29. Optical properties of the electromagnetic wave absorbing laminate related to Example 29 were measured in the same manner as in Example 14, resulting in VLT=72.3%, ST=36.7%, and L * =88.7, a * =-4.2, b * =4.1.

[0311]

[0312]

[0313] Although electromagnetic wave absorbing particle dispersions, electromagnetic wave absorbing laminates, and electromagnetic wave absorbing transparent substrates have been described above in the embodiments and examples, the present invention is not limited to the above embodiments and examples. Various modifications and changes are possible within the scope of the gist of the present invention as described in the patent claims.

[0314] This application claims priority based on Japanese Patent Application No. 2020-015746 filed with the Japan Patent Office on January 31, 2020, and incorporates the entire contents of Japanese Patent Application No. 2020-015746 into this international application.

Claims

Claim 1 General formula Cs x W 1-y O 3-z (0.2≤x≤0.4, 0 <y≤0.4, 0<z≤0.46)로 표시되고, 사방정 또는 육방정의 결정 구조를 구비한 세슘텅스텐산화물을 함유하는 전자파 흡수 입자와, 고체 매체를 포함하고,상기 전자파 흡수 입자가 상기 고체 매체 중에 분산되어 있는 전자파 흡수 입자 분산체이며,JIS Z8701에 준거하여, D65 표준 광원, 광원 각도 10°에 대한 삼자극값 X, Y, Z를 산출하고, 삼자극값으로부터 JIS Z 8729에 준거하여 구한 b*값이 정의 값인 전자파 흡수 입자 분산체. Claim 2 In claim 1, the cesium tungsten oxide is an electromagnetic wave absorbing particle dispersion having linear or planar defects on one or more selected planes, such as the (010) plane of the orthorhombic, the {100} plane of the hexagonal prism, and the (001) plane of the hexagonal bottom. Claim 3 An electromagnetic wave absorbing particle dispersion according to claim 1 or 2, wherein the cesium tungsten oxide has a defect, and the defect includes a tungsten defect. Claim 4 An electromagnetic wave absorbing particle dispersion according to claim 1 or 2, wherein a portion of the O of the WO octahedron constituting the orthorhombic or hexagonal crystal of the cesium tungsten oxide is randomly missing. Claim 5 In claim 1 or 2, the cesium tungsten oxide is an electromagnetic wave absorbing particle dispersion having a c-axis length in hexagonal form of 7.560 Å or more and 7.750 Å or less. Claim 6 An electromagnetic wave absorbing particle dispersion according to claim 1 or 2, wherein a portion of the Cs of the cesium tungsten oxide is substituted by an additive element, and the additive element is one or more selected from Na, Tl, In, Li, Be, Mg, Ca, Sr, Ba, Al, and Ga. Claim 7 An electromagnetic wave absorbing particle dispersion according to claim 1 or 2, wherein the average particle size of the electromagnetic wave absorbing particles is 0.1 nm or more and 200 nm or less. Claim 8 An electromagnetic wave absorbing particle dispersion according to claim 1 or 2, wherein the surface of the electromagnetic wave absorbing particle is modified by a compound comprising one or more atoms selected from Si, Ti, Zr, and Al. Claim 9 An electromagnetic wave absorbing particle dispersion according to claim 1 or 2, wherein the electromagnetic wave absorbing particles used are particles obtained by heating and reducing a crystal powder of a cesium tungsten oxide precursor nCs2O·mWO3 (n, m are integers, 3.6≤m / n≤9.0) in a reducing gas atmosphere at a temperature of 650°C or higher and 950°C or lower. Claim 10 In claim 1 or 2, as the electromagnetic wave absorbing particle, Cs4W as the main phase 11 O 35 An electromagnetic wave absorbing particle dispersion using particles obtained by heating and reducing a cesium tungsten oxide precursor containing a phase at a temperature of 650°C or higher and 950°C or lower in a reducing gas atmosphere. Claim 11 An electromagnetic wave absorbing particle dispersion in which the solid medium is a resin, as in claim 1 or 2. Claim 12 In claim 11, the above resin is an electromagnetic wave absorbing particle dispersion in which the resin is one resin selected from the group of resins consisting of polyester resin, polycarbonate resin, acrylic resin, styrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, olefin resin, epoxy resin, polyimide resin, fluoropolymer, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and UV-curing resin, or a mixture of two or more resins selected from the said group of resins. Claim 13 An electromagnetic wave absorbing particle dispersion having a sheet shape, a board shape, or a film shape in accordance with claim 1 or 2. Claim 14 An electromagnetic wave absorbing laminate having a laminated structure comprising an electromagnetic wave absorbing particle dispersion and a transparent substrate as described in claim 1 or 2. Claim 15 An electromagnetic wave absorbing transparent substrate comprising a transparent substrate and an electromagnetic wave absorbing layer having at least one side of the transparent substrate, wherein the electromagnetic wave absorbing layer is a dispersion of electromagnetic wave absorbing particles as described in claim 1 or 2.

Citation Information

Patent Citations

  • Electromagnetic wave-absorbing transparent substrate

    WO2019031246A1