Method for verifying a photosensitive composition and method for manufacturing a photosensitive composition

A method using acid-degradable resins and specific solvents to measure defects in resist films simplifies the assessment of Line Width Roughness in photosensitive compositions, ensuring consistent performance across manufacturing lots.

KR103044623B1Active Publication Date: 2026-11-06FUJIFILM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
KR1020247009744
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-20
Publication Date
2026-11-06
Estimated Expiration
2042-09-20

AI Technical Summary

Technical Problem

Existing methods for determining the Line Width Roughness (LWR) of photosensitive compositions in semiconductor manufacturing are cumbersome and lack a simple, effective way to ensure consistency across manufacturing lots.

Method used

A method involving the formation of resist films on substrates using acid-degradable resins and photo-generating agents, followed by treatment with a specific solvent solution to measure defects, allowing comparison of reference and measurement data to assess LWR consistency.

Benefits of technology

Enables easy and accurate determination of whether a photosensitive composition exhibits a predetermined LWR, reducing variability and ensuring consistent performance across batches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024032452309-PCT00021_ABST
    Figure 112024032452309-PCT00021_ABST
Patent Text Reader

Abstract

A method for testing a photosensitive composition and a method for manufacturing a photosensitive composition that can easily test whether or not a photosensitive composition exhibits a predetermined LWR. The method for testing a photosensitive composition comprises: a process 1 in which a resist film is formed on a substrate 1 using a reference photosensitive composition comprising an acid-degradable resin having a group that decomposes by the action of an acid to generate a polar group, and a photogenerator, the resist film on the substrate 1 is removed using a treatment solution, and the number of defects on the substrate 1 from which the resist film on the substrate 1 has been removed is measured to obtain reference data; a process 2 in which a resist film is formed on a substrate 2 using a measurement photosensitive composition comprising a component of the same type as that included in the reference photosensitive composition, the resist film on the substrate 2 is removed using a treatment solution, and the number of defects on the substrate 2 from which the resist film on the substrate 2 has been removed is measured to obtain measurement data; and a process 3 in which the reference data and the measurement data are compared to determine whether or not they are within an allowable range, wherein the treatment solution contains a predetermined component.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for testing a photosensitive composition comprising a photogenerator and an acid-degradable resin having a group that decomposes by the action of an acid to generate a polar group, and a method for manufacturing a photosensitive composition. Background Technology

[0002] Conventionally, in the manufacturing process of semiconductor devices such as ICs (Integrated Circuits) and LSIs (Large Scale Integrated Circuits), microfabrication by lithography using photosensitive compositions is performed. Recently, with the increasing integration of integrated circuits, the formation of ultra-fine patterns in the sub-micron or quarter-micron range has become required. Accordingly, there is a trend toward shorter wavelengths, such as from the g-line to the i-line, and from ArF excimer laser light to KrF excimer laser light. Furthermore, currently, in addition to excimer laser light, lithography using electron beams and EUV (Extreme Ultra Violet) light is also being developed.

[0003] For example, Patent Document 1 discloses a resist composition comprising a photo-generating agent used in photolithography using high-energy rays such as ArF excimer laser light, KrF excimer laser light, electron beams, and extreme ultraviolet rays as a light source. Prior art literature

[0004] Patent Document 1: Japanese Published Patent Application No. 2020-126143 The problem to be solved

[0005] It is desirable for photosensitive compositions to have minimal performance differences between manufacturing lots. For this reason, conventionally, when manufacturing photosensitive compositions, attempts were made to produce a photosensitive composition that exhibits the same performance as other manufacturing lots in any manufacturing lot. At that time, in order to determine whether the newly manufactured photosensitive composition exhibits the same performance as the photosensitive composition of a previous manufacturing lot, a resist pattern was formed and its LWR (Line Width Roughness) was measured.

[0006] Meanwhile, in order to measure LWR, it is necessary to form a resist pattern after forming a resist film as described above. Since measuring LWR in this manner involves a cumbersome procedure, there has been a desire for a method that can more simply determine whether a photosensitive composition exhibits a predetermined LWR.

[0007] The objective of the present invention is to provide a method for testing a photosensitive composition and a method for manufacturing a photosensitive composition, which can easily test whether or not a photosensitive composition exhibits a predetermined LWR. means of solving the problem

[0008] The inventors, after carefully examining the problems of the prior art, found that the above problem can be solved by the following configuration.

[0009] (1) A process 1 for obtaining reference data by forming a resist film on substrate 1 using a reference photosensitive composition comprising an acid-degradable resin having a group that decomposes by the action of an acid to generate a polar group, and a photo-generating agent, removing the resist film on substrate 1 using a treatment solution, and measuring the number of defects on substrate 1 from which the resist film on substrate 1 has been removed.

[0010] A process 2 for forming a resist film on substrate 2 using a photosensitive composition for measurement containing a component of the same type as a component included in a reference photosensitive composition, removing the resist film on substrate 2 using a treatment solution, measuring the number of defects on substrate 2 from which the resist film on substrate 2 has been removed, and acquiring measurement data;

[0011] It has process 3, which compares reference data and measurement data to determine whether or not it is within the allowable range,

[0012] The treatment solution comprises aromatic hydrocarbons, an organic solvent, and metal X, and

[0013] The content of aromatic hydrocarbons is 1 mass% or less with respect to the total mass of the treatment solution, and

[0014] The organic solvent does not contain aromatic hydrocarbons, and also contains aliphatic hydrocarbons,

[0015] Metal X is at least one metal selected from the group consisting of Al, Fe, and Ni, and

[0016] The mass ratio of aromatic hydrocarbon content to metal X content is 5.0×10 4 ~2.0×10 10 Phosphorus, method for testing a photosensitive composition.

[0017] (2) A method for verifying a photosensitive composition as described in claim 1, wherein, in process 3, if the measurement data falls outside the acceptable range, the components of the photosensitive composition for measurement are adjusted.

[0018] (3) A method for verifying a photosensitive composition described in (1) or (2), wherein in process 1 and process 2, the resist film on substrate 1 and the resist film on substrate 2 are each formed by performing pattern exposure on the resist film after forming the resist film.

[0019] (4) A method for verifying a photosensitive composition described in (3), wherein the pattern exposure in process 1 and process 2 uses any one of KrF excimer laser light, ArF excimer laser light, electron beam, and extreme ultraviolet light.

[0020] (5) A method for testing a photosensitive composition described in any one of (1) to (4), wherein the number of defects on substrate 1 with the resist film removed and the number of defects on substrate 2 with the resist film removed are each measured using a defect inspection device.

[0021] (6) A method for testing a photosensitive composition described in any one of (1) to (5), wherein the acid-degradable resin comprises repeating units having phenolic hydroxyl groups.

[0022] (7) Aliphatic hydrocarbons are undecanes, and

[0023] A method for testing a photosensitive composition described in any one of (1) to (6), wherein the organic solvent further comprises butyl acetate.

[0024] (8) A method for testing a photosensitive composition described in (7), wherein the ratio of the content of butyl acetate to the content of undecane is 65 / 35 to 99 / 1.

[0025] (9) A method for testing a photosensitive composition described in (8), wherein the ratio of the content of butyl acetate to the content of undecane is 90 / 10.

[0026] (10) An acid-degradable resin has repeating units derived from monomers that have groups that generate polar groups when decomposed by the action of acid, and

[0027] All monomers have a solubility index (R) based on the Hansen solubility parameter for the treatment solution, represented by Equation (1) described below, of 2.0 to 5.0 (MPa). 1 / 2 is, and also,

[0028] At least one of the monomers has a solubility index difference (△R) of 4.0 (MPa) before and after santalization. 1 / 2 A method for testing a photosensitive composition described in any one of (1) to (9), above.

[0029] (11) In reference data, the number of defects on List 1 is 0.0001 to 10 pieces / cm 2 A method for testing a photosensitive composition described in any one of (1) to (10).

[0030] (12) A method for testing a photosensitive composition described in any one of (1) to (11), wherein the content of aromatic hydrocarbons is 1 mass% or less relative to the total mass of the treatment solution.

[0031] (13) A method for manufacturing a photosensitive composition comprising a method for testing a photosensitive composition as described in any one of (1) to (12). Effects of the invention

[0032] According to the present invention, a method for testing a photosensitive composition and a method for manufacturing a photosensitive composition can be provided, which can easily test whether or not a photosensitive composition exhibits a predetermined LWR. Brief explanation of the drawing

[0033] FIG. 1 is a flowchart showing a first example of a method for testing a photosensitive composition of an embodiment of the present invention. FIG. 2 is a flowchart showing a first example of a method for acquiring reference data for a method of verifying a photosensitive composition of an embodiment of the present invention. FIG. 3 is a flowchart showing a first example of a method for acquiring measurement data of a method for verifying a photosensitive composition of an embodiment of the present invention. FIG. 4 is a flowchart showing a second example of a method for acquiring reference data for a method of verifying a photosensitive composition of an embodiment of the present invention. FIG. 5 is a flowchart showing a second example of a method for acquiring measurement data of a method for verifying a photosensitive composition of an embodiment of the present invention. FIG. 6 is a flowchart showing a second example of a method for testing a photosensitive composition of an embodiment of the present invention. FIG. 7 is a flowchart showing an example of a method for manufacturing a photosensitive composition of an embodiment of the present invention. Specific details for implementing the invention

[0034] Hereinafter, based on the suitable embodiments shown in the attached drawings, a method for verifying the photosensitive composition of the present invention and a method for manufacturing the photosensitive composition will be described in detail.

[0035] Furthermore, the drawings described below are exemplary for explaining the present invention, and the present invention is not limited to the drawings shown below.

[0036] In addition, the "~" indicating a numerical range below includes the numerical values ​​listed on both sides. For example, ε = numerical value α ~ numerical value β, where the range of ε is a range that includes numerical values ​​α and β, and expressed in mathematical symbols as α≤ε≤β.

[0037] In addition, "identical" includes the generally accepted margin of error in the relevant technical field.

[0038] Regarding the notation of a group (atomic group) in this specification, unless it contradicts the spirit of the present invention, notations that do not specify substitution or non-substitution include groups having substituents along with groups not having substituents. For example, the term "alkyl group" includes not only alkyl groups not having substituents (non-substituted alkyl groups) but also alkyl groups having substituents (substituted alkyl groups). Furthermore, the term "organic group" in this specification refers to a group comprising at least one carbon atom.

[0039] Unless otherwise specified, monovalent substituents are preferred.

[0040] In this specification, "active light" or "radiation" means, for example, emission spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light: Extreme Ultraviolet), X-rays, and electron beams (EB: Electron Beam), etc. In this specification, "light" means active light or radiation.

[0041] Unless otherwise specifically explained, the term "exposure" in this specification includes not only exposure by emission spectra of mercury lamps, far ultraviolet rays represented by excimer lasers, extreme ultraviolet rays (EUV light), and X-rays, but also drawing by particle beams such as electron beams and ion beams.

[0042] The bonding direction of the divalent groups indicated in this specification is not limited unless specifically explained. For example, in a compound represented by the formula “XYZ”, if Y is -COO-, Y may be -CO-O- or -O-CO-. Also, the compound may be “X-CO-OZ” or “XO-CO-Z”.

[0043] In this specification, (meth)acrylate refers to acrylate and methacrylate, and (meth)acrylic refers to acrylic and methacrylic.

[0044] In this specification, the weight average molecular weight (Mw), number average molecular weight (Mn), and dispersion (also called molecular weight distribution) (Mw / Mn) of the resin are defined as polystyrene equivalent values ​​by GPC measurement using a Gel Permeation Chromatography (GPC) device (Dosoh HLC-8120GPC) (solvent: tetrahydrofuran, flow rate (sample injection amount): 10 μL, column: Dosoh TSK gel Multipore HXL-M, column temperature: 40°C, flow rate: 1.0 mL / min, detector: differential refractive index detector).

[0045] In this specification, the acid dissociation constant (pKa) refers to the pKa in an aqueous solution, and specifically, it is a value obtained by calculation based on a database of Hamette substituent constants and known literature values ​​using the following software package 1. All pKa values ​​described in this specification represent values ​​obtained by calculation using this software package.

[0046] Software Package 1: Advanced Chemistry Development (ACD / Labs) Software V8.14 for Solaris (1994-2007 ACD / Labs).

[0047] Meanwhile, pKa is also determined by molecular orbital calculations. Specifically, this method involves H₂ in an aqueous solution based on thermodynamic cycles. + One method is to calculate it by calculating the dissociation free energy. H + Regarding the method for calculating the dissociation free energy, it can be calculated, for example, by the Density Functional Path (DFT); however, various other methods have been reported in the literature and are not limited thereto. Additionally, while there are multiple software programs capable of performing DFT, Gaussian 16 can be cited as an example.

[0048] In this specification, pKa refers to a value obtained by calculation based on a database of Hammett substituent constants and known literature values ​​using software package 1 as described above. However, if pKa cannot be calculated by this method, a value obtained by Gaussian 16 based on the DFT (density functional method) is adopted.

[0049] Additionally, as described above, pKa in this specification refers to "pKa in an aqueous solution," but if pKa in an aqueous solution cannot be calculated, "pKa in a dimethyl sulfoxide (DMSO) solution" shall be adopted.

[0050] In this specification, examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.

[0051] The inventors have discovered that for two photosensitive compositions containing the same type of components, by using a predetermined treatment solution and comparing the predetermined data on the number of defects, it is possible to determine whether the photosensitive compositions exhibit the same degree of performance regarding LWR performance.

[0052] Specifically, it was discovered that when a treatment solution containing aliphatic hydrocarbons and aromatic hydrocarbons / metal impurities within a predetermined range is used, there is a correlation between the difference in the number of defects as described above and the difference in LWRs. That is, it was found that when the number of defects is of the same degree, the performance of the LWR is of the same degree, whereas when the number of defects is different, the performance of the LWR is also different.

[0053] For two photosensitive compositions containing the same type of components, when a conventional treatment solution is used, the range of variation in the result of the number of defects is large, and also the range of variation in the result of LWR is large.

[0054] In this regard, it was found that when the treatment solution of the present invention is used for two photosensitive compositions containing the same type of components, the range of variation in the result of the number of defects and the range of variation in the result of LWR are both small, and when comparing the result of the number of defects, LWR also exhibits the same level of performance.

[0055] Below, a method for verifying a photosensitive composition will be explained in detail.

[0056] [First Example of a Method for Testing a Photosensitive Composition]

[0057] FIG. 1 is a flowchart showing a first example of a method for verifying a photosensitive composition according to an embodiment of the present invention. FIG. 2 is a flowchart showing a first example of a method for acquiring reference data according to a method for verifying a photosensitive composition according to an embodiment of the present invention, and FIG. 3 is a flowchart showing a first example of a method for acquiring measurement data according to a method for verifying a photosensitive composition according to an embodiment of the present invention.

[0058] A first example of a method for verifying a photosensitive composition has, as shown in FIG. 1, a process 1 (step S10) for acquiring reference data, a process 2 (step S12) for acquiring measurement data, and a process 3 (step S14) for comparing the reference data and the measurement data to determine whether or not it is within an acceptable range.

[0059] In process 3 (step S14), if it is within the allowable range, it is determined to be a photosensitive composition exhibiting a predetermined LWR.

[0060] Meanwhile, in process 3 (step S14), if it falls outside the allowable range, it is determined to be a photosensitive composition that does not exhibit a predetermined LWR.

[0061] In this way, the method for verifying a photosensitive composition can easily verify whether or not it is a photosensitive composition exhibiting a predetermined LWR (Line Width Roughness).

[0062] Process 1 (step S10) for acquiring reference data has the following process.

[0063] Process 1 (step S10) shown in FIG. 2 forms a resist film on a substrate using a standard photosensitive composition comprising an acid-degradable resin having a group that decomposes by the action of an acid to generate a polar group, and a photo-generating agent (step S20).

[0064] The substrate is not particularly limited, and a semiconductor substrate such as a silicon substrate is used. It is preferable that the substrate be cleaned in advance to remove foreign matter from the substrate. There is no limit to the size of the foreign matter on the substrate, but for example, it may be 20 nm or larger.

[0065] The method of forming the resist film is not particularly limited and, for example, may be formed using a spin coater. In forming the resist film, after applying a reference photosensitive composition onto a substrate, a pre-bake treatment may be performed on the film of the reference photosensitive composition.

[0066] Next, the resist film on the substrate is removed using a treatment solution (Step S22). The method of removing the resist film is not particularly limited as long as the treatment solution is used; the resist film may be removed by applying the treatment solution in a mist form to the resist film, or by immersing the resist film in the treatment solution.

[0067] In addition, the various materials used in this process will be explained in detail in the following paragraph.

[0068] Next, the number of defects on the substrate from which the resist film has been removed is measured, for example, using a defect inspection device (Step S24). Reference data is obtained by measuring the number of defects (Step S10).

[0069] Furthermore, regarding the reference data, the number of defects may be the total number of defects on the surface, or the value obtained by dividing the number of defects by the surface area of ​​the surface, i.e., the number of defects per unit area, may be used as the reference data. In this case, the reference data is, for example, pieces / cm² 2 It is represented as follows. The number of defects is, for example, 0.0001 to 10 defects / cm². 2 It is desirable, and 0.0005~5 pieces / cm 2 is more desirable, and 0.001~1 piece / cm 2 is more desirable.

[0070] Here, the defects on the substrate from which the resist film has been removed refer to foreign substances, such as particles and residues, remaining on the substrate. These defect-causing components are primarily contained within the resist film. More specifically, when a resist film is formed on a substrate, components within the resist film that can become defects are adsorbed onto the substrate, and remain on the substrate even after the resist film is removed by a treatment solution, thereby becoming defects.

[0071] In addition, the number of defects can be measured by known methods, but for example, the number of defects can be measured using UVision 5 (manufactured by AMAT).

[0072] Process 2 (step S12) for acquiring measurement data has the process shown below.

[0073] Process 2 (step S12) shown in FIG. 3 forms a resist film on a substrate using a photosensitive composition for measurement that includes a component of the same type as the component included in the reference photosensitive composition (step S30).

[0074] The description is as explained in Step S20 above. The method for forming the resist film is as explained in Step S20 above.

[0075] Next, the resist film on the substrate is removed using a processing solution (Step S32). The resist film is removed in the same manner as in Step S22 described above.

[0076] Next, the number of defects on the substrate from which the resist film has been removed is measured using a defect inspection device (Step S34). The number of defects is measured in the same manner as in Step S24.

[0077] By the above method, the number of defects is measured and measurement data is obtained (Step S12).

[0078] In addition, as with the reference data, the number of defects may be the total number of defects on the surface, or the value obtained by dividing the number of defects by the surface area, i.e., the number of defects per unit area, may be used as the measurement data. In this case, the measurement data is, for example, pieces / cm 2 It appears as.

[0079] In Step S14 (Process 3), in order to compare the reference data and the measurement data, the reference data and the measurement data are made to have the same data format. By making the data formats the same, comparison can be easily made.

[0080] As described above, in Step S14 (Process 3), reference data and measurement data are compared to determine whether they fall within an acceptable range. The acceptable range is appropriately set according to, for example, the application. The acceptable range is defined by a ratio γ, expressed as (measurement data) / (reference data), for example. The ratio γ is, for example, 0.9 ≤ γ ≤ 1.1. In addition, in addition to the above ratio γ, the acceptable range may be within (reference data) ± (an arbitrary reference range set from past measurement results, etc.).

[0081] FIG. 4 is a flowchart showing a second example of a method for acquiring reference data for a method for verifying a photosensitive composition of an embodiment of the present invention, and FIG. 5 is a flowchart showing a second example of a method for acquiring measurement data for a method for verifying a photosensitive composition of an embodiment of the present invention.

[0082] In addition, regarding the same process as in FIGS. 2 and FIGS. 3 in FIGS. 4 and FIGS. 5, a detailed description thereof is omitted.

[0083] The second example of the method for acquiring reference data and the second example of the method for acquiring measurement data differ from the first example of the method for acquiring reference data and the first example of the method for acquiring measurement data described above in that the resist film is pattern-exposed.

[0084] In the second example of the method for acquiring reference data, as shown in FIG. 4, after forming a resist film (step S20), pattern exposure is performed on the resist film (step S21). After step S21, the resist film is removed (step S22). Then, the number of defects on the substrate from which the resist film has been removed is measured using a defect inspection device (step S24), and reference data is acquired (step S10).

[0085] In the second example of the method for acquiring measurement data, as shown in FIG. 5, after forming a resist film (step S30), pattern exposure is performed on the resist film (step S31). After step S31, the resist film is removed (step S32). Then, the number of defects on the substrate from which the resist film has been removed is measured using a defect inspection device (step S34), and measurement data is acquired (step S12).

[0086] In this way, reference data and measurement data can be obtained by performing pattern exposure on the resist film.

[0087] In step S21 and step S31, it is preferable that the exposure pattern and the exposure conditions are the same. Also, the pattern exposure is performed by light of a wavelength corresponding to the photosensitive composition. For example, any one of KrF excimer laser light, ArF excimer laser light, electron beam, and extreme ultraviolet (EUV) light is used.

[0088] The pattern of the pattern exposure in steps S21 and S31 is not particularly limited and, for example, is an isolated resist pattern, a dot pattern, or a line and space.

[0089] When the photosensitive composition is of the positive type, a pattern is used as the pattern of pattern exposure in which exposed areas, such as holes and trenches, disappear upon development.

[0090] When the photosensitive composition is of the negative type, a pattern in which exposed locations, such as dots and lines, remain after development is used as the pattern of pattern exposure.

[0091] [2nd Example of Method for Testing Photosensitive Composition]

[0092] FIG. 6 is a flowchart showing a second example of a method for testing a photosensitive composition according to an embodiment of the present invention. In addition, regarding the second example of the method for testing a photosensitive composition shown in FIG. 6, a detailed description of the same process as the first example of the method for testing a photosensitive composition described above is omitted.

[0093] The second example of the method for testing a photosensitive composition is different from the first example of the method for testing a photosensitive composition described above in that, in step S14 (process 3), when the measurement data is compared with the reference data and the measurement data, if the measurement data falls outside the acceptable range, the component adjustment of the photosensitive composition for measurement (step S16) is performed.

[0094] Meanwhile, in Step S14 (Process 3), if the measurement data is within the acceptable range, component adjustment is not performed.

[0095] In addition, in step S14 (process 3), the adjustment of the components of the photosensitive composition for measurement (step S16) may be repeated until the measurement data is determined to be within an acceptable range.

[0096] The photosensitive composition for measurement includes components identical to those included in the reference photosensitive composition. In Step S16, when adjusting the components of the photosensitive composition for measurement, for example, the amount of at least one of the photogenerator and the acid-degradable resin is adjusted. When comparing the measurement data and the reference data, the component to be adjusted and the amount of adjustment may be pre-set according to the difference between the measurement data and the reference data, such as when the measurement data is greater or the measurement data is less, and the degree of difference between the measurement data and the reference data.

[0097] [Example of a method for manufacturing a photosensitive composition]

[0098] FIG. 7 is a flowchart illustrating an example of a method for manufacturing a photosensitive composition according to an embodiment of the present invention. The method for verifying the photosensitive composition described above can be used in the method for manufacturing a photosensitive composition.

[0099] In addition, regarding the method for manufacturing a photosensitive composition shown in FIG. 7, a detailed description of the process identical to the process of the first example of the method for verifying the photosensitive composition described above is omitted.

[0100] The method for manufacturing a photosensitive composition differs from the first example of a method for verifying a photosensitive composition in the following respects. In the method for manufacturing a photosensitive composition, in step S14 (Process 3), when the measurement data is compared with the reference data and the measurement data, if the measurement data is within an acceptable range, the photosensitive composition for measurement is classified as an acceptable product (step S40). Additionally, the acceptable product is classified as a product of the photosensitive composition.

[0101] Meanwhile, in step S14 (process 3), if the measurement data falls outside the acceptable range when comparing the reference data and the measurement data, there is a process (step S42) for rejecting the photosensitive composition for measurement. Additionally, the rejected product is not treated as a product.

[0102] In the method for manufacturing a photosensitive composition, for a photosensitive composition for measurement that has been rejected (step S42), the component adjustment of the photosensitive composition for measurement (step S44) may be performed.

[0103] The adjustment of the components of the photosensitive composition for measurement (Step S44) is the same process as the adjustment of the components of the photosensitive composition for measurement (Step S16) of the second example of the verification method for the photosensitive composition described above, so a detailed description thereof is omitted. In the method for manufacturing the photosensitive composition, the adjustment of the components of the photosensitive composition for measurement (Step S16) may be repeated until the measurement data is determined to be within an acceptable range.

[0104] In the above description, comparison and judgment are performed, for example, by inputting various numerical values ​​into a computer, comparing them with an allowable range, and making a judgment based on the allowable range. In this way, comparison and judgment are executed, for example, by a computer.

[0105] The present invention is basically configured as described above. Although the method for verifying a photosensitive composition and the method for manufacturing a photosensitive composition of the present invention have been described in detail above, the present invention is not limited to the embodiments described above, and it is understood that various improvements or modifications may be made within the scope of the present invention without departing from its basic principles.

[0106] Below, the materials used in the above-mentioned inspection method will be described in detail.

[0107] [Treatment Solution]

[0108] The treatment solution comprises aromatic hydrocarbons, an organic solvent other than aromatic hydrocarbons, and metal X, wherein the organic solvent comprises aliphatic hydrocarbons, and metal X is at least one metal selected from the group consisting of Al, Fe, and Ni, and the mass ratio of the content of aromatic hydrocarbons to the content of metal X is 5.0 × 10 4 ~2.0×10 10 am.

[0109] The components included in the treatment solution are described in detail below.

[0110] Aromatic hydrocarbons

[0111] The treatment solution contains aromatic hydrocarbons.

[0112] "Aromatic hydrocarbons" refer to hydrocarbons composed solely of hydrogen and carbon atoms and possessing an aromatic ring. Aromatic hydrocarbons are not included in organic solvents.

[0113] The content of aromatic hydrocarbons is preferably 1 mass% or less with respect to the total mass of the treatment solution, more preferably 1 to 10,000 mass ppm, more preferably 5 to 10,000 mass ppm, and particularly preferably 50 to 10,000 mass ppm. In addition, when the aromatic hydrocarbons include two or more types of aromatic hydrocarbons, it is preferable that the total content of the two or more types of aromatic hydrocarbons be within the above range.

[0114] The number of carbon atoms in the aromatic hydrocarbon is preferably 6 to 30, more preferably 6 to 20, and more preferably 10 to 12.

[0115] The aromatic ring of an aromatic hydrocarbon may be either a monocyclic or a polycyclic ring.

[0116] The number of reduced aromatic rings in aromatic hydrocarbons is preferably 6 to 12, more preferably 6 to 8, and more preferably 6.

[0117] The aromatic ring of the aromatic hydrocarbon may have additional substituents. Examples of such substituents include alkyl groups, alkenyl groups, and groups formed by combining them. The alkyl group and the alkenyl group may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group and the alkenyl group is preferably 1 to 10, and more preferably 1 to 5.

[0118] Examples of aromatic rings of aromatic hydrocarbons include benzene rings that may have substituents, naphthalene rings that may have substituents, and anthracene rings that may have substituents, and benzene rings that may have substituents are preferred.

[0119] In other words, as an aromatic hydrocarbon, benzene that may have substituents is preferred.

[0120] Aromatic hydrocarbons are, C 10 H 14 , C 11 H 16 and C 10 H12 It is desirable to include at least one type selected from the group consisting of

[0121] In addition, as an aromatic hydrocarbon, a compound represented by formula (c) is also preferred.

[0122] [Chemical Formula 1]

[0123]

[0124] In equation (c), R c represents a substituent. c represents an integer from 0 to 6.

[0125] R c represents a substituent.

[0126] R c As a substituent, an alkyl group or an alkeneyl group is preferred.

[0127] The above alkyl group and the above alkenyl group may be any of straight chain, branched chain, and cyclic.

[0128] The number of carbon atoms in the alkyl group and the alkeneyl group is preferably 1 to 10, and more preferably 1 to 5.

[0129] R c If there are multiple instances of , R c They may be identical or different, and R c They may combine with each other to form a ring.

[0130] Also, R c (R c If there are multiple instances of , multiple R c A condensed ring may be formed by condensing a benzene ring in formula (c) with part or all of the (and the benzene ring in formula (c).

[0131] c represents an integer from 0 to 6.

[0132] c is preferably an integer from 1 to 5, and more preferably an integer from 1 to 4.

[0133] The molecular weight of the aromatic hydrocarbon is preferably 50 or more, more preferably 100 or more, and more preferably 120 or more. The upper limit is preferably 1000 or less, more preferably 300 or less, and more preferably 150 or less.

[0134] As aromatic hydrocarbons, for example, C such as 1,2,4,5-tetramethyl-benzene, 1-ethyl-3,5-dimethyl-benzene, 1,2,3,5-tetramethyl-benzene and 1-ethyl-2,4-dimethyl-benzene 10 H 14 ; C, such as 1-methyl-4-(1-methylpropyl)-benzene and (1-methylbutyl)-benzene 11 H 16 ; C, such as 1-methyl-2-(2-propenyl)-benzene and 1,2,3,4-tetrahydro-naphthalene 10 H 12 ...can be cited.

[0135] As aromatic hydrocarbons, 1,2,4,5-tetramethyl-benzene, 1-ethyl-3,5-dimethyl-benzene, 1,2,3,5-tetramethyl-benzene, 1-methyl-4-(1-methylpropyl)-benzene and C 10 H 12 1-ethyl-3,5-dimethyl-benzene or 1,2,3,5-tetramethyl-benzene is preferred, and 1-ethyl-3,5-dimethyl-benzene or 1,2,3,5-tetramethyl-benzene is more preferred.

[0136] Aromatic hydrocarbons may be used as a single type or in two or more types.

[0137] The treatment liquid preferably contains two or more aromatic hydrocarbons, more preferably contains three or more aromatic hydrocarbons, more preferably contains three to eight aromatic hydrocarbons, and particularly preferably contains three to four aromatic hydrocarbons.

[0138] As a method for measuring the content of aromatic hydrocarbons, for example, the method for measuring the content of organic solvents described below can be cited.

[0139] Methods for adjusting the content of aromatic hydrocarbons include, for example, selecting raw materials with a low content of aromatic hydrocarbons as raw materials constituting various components, distilling under conditions that suppress contamination by lining the inside of the apparatus with Teflon (registered trademark), and adding aromatic hydrocarbons.

[0140] Organic solvents

[0141] The treatment solution comprises an organic solvent other than the aromatic hydrocarbons described above. That is, in this specification, aromatic hydrocarbons are not included in the organic solvent.

[0142] Aliphatic hydrocarbons

[0143] Organic solvents include aliphatic hydrocarbons.

[0144] "Aliphatic hydrocarbons" refer to hydrocarbons composed solely of hydrogen and carbon atoms and that do not possess aromatic rings.

[0145] Aliphatic hydrocarbons may be straight-chain, branched-chain, or cyclic (single or multiple), and straight-chain is preferred. Additionally, aliphatic hydrocarbons may be either saturated aliphatic hydrocarbons or unsaturated aliphatic hydrocarbons.

[0146] The number of carbon atoms in the aliphatic hydrocarbon is often 2 or more, preferably 5 or more, and more preferably 10 or more. The upper limit is preferably 30 or less, more preferably 20 or less, more preferably 15 or less, and particularly preferably 13 or less. Specifically, the number of carbon atoms in the aliphatic hydrocarbon is preferably 11.

[0147] Examples of aliphatic hydrocarbons include pentane, isopentane, hexane, isohexane, cyclohexane, ethylcyclohexane, methylcyclohexane, heptane, octane, isooctane, nonene, decaine, methyldecane, undecane, dodecane, tridecane, tetradecane, pentadecaine, hexadecane, heptadecaine, 2,2,4-trimethylpentane, and 2,2,3-trimethylhexane.

[0148] It is preferable that the aliphatic hydrocarbon comprises an aliphatic hydrocarbon having 5 or more carbon atoms (preferably 20 or fewer carbon atoms), more preferable that it comprises an aliphatic hydrocarbon having 10 or more carbon atoms (preferably 13 or fewer carbon atoms), more preferable that it comprises at least one selected from the group consisting of decane, undecane, dodecane, and methyldecane, and particularly preferable that it comprises undecane.

[0149] The content of aliphatic hydrocarbons is preferably 0.8 mass% or more and less than 100 mass% with respect to the total mass of the treatment solution, more preferably 1 to 50 mass%, more preferably 3 to 30 mass%, and particularly preferably 8 to 18 mass%.

[0150] The content of aliphatic hydrocarbons is preferably 0.8 mass% or more and 100 mass% or less with respect to the total mass of the organic solvent, more preferably 1 to 100 mass%, more preferably 2 to 100 mass%, more preferably 2 to 50 mass%, particularly preferably 3 to 30 mass%, and most preferably 8 to 18 mass%.

[0151] ≪Ester-based solvents≫

[0152] It is preferable that the organic solvent further include an ester-based solvent.

[0153] The ester solvent may be any of a straight chain, a branched chain, or a cyclic (single or multiple) chain, and a straight chain is preferred.

[0154] The number of carbon atoms in the ester-based solvent is often 2 or more, preferably 3 or more, more preferably 4 or more, and more preferably 6 or more. The upper limit is often 20 or less, preferably 10 or less, more preferably 8 or less, and particularly preferably 7 or less. Specifically, the number of carbon atoms in the ester-based solvent is preferably 6.

[0155] Examples of ester-based solvents include butyl acetate, isobutyl acetate, tert-butyl acetate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, hexyl acetate, methoxybutyl acetate, amyl acetate, isoamyl acetate, methyl formate, ethyl formate, butyl formate, propyl formate, amyl formate, isoamyl formate, methyl lactate, ethyl lactate, butyl lactate, propyl lactate, 2-methyl hydroxyisobutyrate, ethyl butyrate, ethyl isobutyrate, ethyl propionate, propyl propionate, isopropyl propionate, butyl propionate, and isobutyl propionate.

[0156] The ester solvent preferably comprises at least one selected from the group consisting of butyl acetate, isobutyl acetate, amyl formate, ethyl acetate, and hexyl acetate, more preferably comprises at least one selected from the group consisting of butyl acetate, isobutyl acetate, ethyl acetate, and hexyl acetate, and more preferably comprises butyl acetate.

[0157] The content of the ester-based solvent is preferably 10 mass% or more and less than 100 mass% with respect to the total mass of the treatment solution, more preferably 60 to 99 mass%, more preferably 60 to 95 mass%, and particularly preferably 80 to 90 mass%.

[0158] The content of the ester-based solvent is preferably 10 mass% or more and less than 100 mass% with respect to the total mass of the organic solvent, more preferably 60 to 99 mass%, more preferably 60 to 95 mass%, and particularly preferably 80 to 90 mass%.

[0159] It is preferable that the organic solvent comprises an aliphatic hydrocarbon and an ester-based solvent, and it is more preferable that it consists solely of an aliphatic hydrocarbon and an ester-based solvent. As the aliphatic hydrocarbon, it comprises at least one selected from the group consisting of undecae, dodecane, and decane, and as the ester-based solvent, it is more preferable that it comprises at least one selected from the group consisting of butyl acetate, isobutyl acetate, amyl formate, ethyl acetate, and hexyl acetate. Among these, it is particularly preferable that the organic solvent consists solely of undecae and butyl acetate.

[0160] When the organic solvent includes an aliphatic hydrocarbon and an ester-based solvent, the ratio of the content of the ester-based solvent to the content of the aliphatic hydrocarbon (content of the ester-based solvent / content of the aliphatic hydrocarbon) is preferably 65 / 35 to 99 / 1, more preferably 85 / 15 to 95 / 5, and more preferably 90 / 10.

[0161] The total content of aliphatic hydrocarbons and ester-based solvents is preferably 10 mass% or more and less than 100 mass% with respect to the total mass of the treatment solution, more preferably 80 mass% or more and less than 100 mass%, and more preferably 95 mass% or more and less than 100 mass%.

[0162] The total content of aliphatic hydrocarbons and ester-based solvents is preferably 10 to 100 mass% with respect to the total mass of the organic solvent, more preferably 80 to 100 mass%, more preferably 95 to 100 mass%, and particularly preferably 99 to 100 mass%.

[0163] Other Solvents

[0164] In addition to the above, the organic solvent may include other solvents.

[0165] Other solvents include, for example, ketone-based solvents, amide-based solvents, and ether-based solvents.

[0166] Organic solvents may be used as a single type or in two or more types.

[0167] The content of the organic solvent is preferably 90 mass% or more with respect to the total mass of the treatment solution, more preferably 95 mass% or more, and more preferably 98 mass% or more. The upper limit is often less than 100 mass% with respect to the total mass of the treatment solution.

[0168] Methods for measuring the content of organic solvents include, for example, using GC (gas chromatography) and GC-MS (gas chromatography-mass spectrometry).

[0169] Metal X

[0170] The treatment solution contains metal X.

[0171] Metal X is at least one metal selected from the group consisting of Al, Fe, and Ni. It is preferable that the treatment solution contains all metals of Al, Fe, and Ni.

[0172] The above metal X may exist in an ionic state in the treatment solution or may exist at zero valence. If it exists at zero valence, it may exist in a particulate state.

[0173] Metal X may be used as a single type or as two or more types.

[0174] The content of metal X is preferably 0.01 to 3000 mass ppt with respect to the total mass of the treatment solution, more preferably 0.1 to 2500 mass ppt, and more preferably 0.1 to 2000 mass ppt. In addition, if the treatment solution contains two or more metals, it is preferable that the total content of the two or more metals be within the above range.

[0175] In addition, the content of at least one of Al, Fe, and Ni in metal X is preferably 0.1 to 2000 mass ppt with respect to the total mass of the treatment solution.

[0176] The mass ratio of the content of aromatic hydrocarbons to the content of metal X (content of aromatic hydrocarbons / content of metal X) is 5.0 × 10 4 ~2.0×10 10 and 3.0×10 5 ~1.0×10 9 3.0×10 is desirable. 5 ~2.5×10 8 This is more desirable.

[0177] As a method for measuring the content of metal X, known measurement methods such as ICP-MS (ICP mass spectrometry) can be cited.

[0178] Methods for adjusting the content of the above metal X include, for example, filtering using the above filter, selecting a raw material with a low content of metal X as a raw material constituting various components, distilling under conditions that suppress contamination by lining the inside of the device with Teflon (registered trademark), and adding metal X or a compound containing metal X.

[0179] [Reference photosensitive composition, photosensitive composition for measurement]

[0180] The standard photosensitive composition comprises an acid-degradable resin having a group that decomposes by the action of acid to generate a polar group, and a photogenerator.

[0181] Furthermore, the photosensitive composition for measurement includes components of the same type as the reference photosensitive composition described above. Including components of the same type means including components of the same structure, and the content thereof may differ. Additionally, regarding the resin containing repeating units, the type constituting the repeating units must be the same, and the content of each repeating unit may differ.

[0182] More specifically, regarding the acid-degradable resin, the type of repeating unit in the acid-degradable resin included in the reference photosensitive composition and the type of repeating unit in the acid-degradable resin included in the measurement photosensitive composition must be the same, and the content of each repeating unit in the acid-degradable resin included in the reference photosensitive composition and the content of each repeating unit in the acid-degradable resin included in the measurement photosensitive composition may be different. In addition, the content of the acid-degradable resin included in the reference photosensitive composition and the content of the acid-degradable resin included in the measurement photosensitive composition may be different.

[0183] Furthermore, regarding the photogenerator, the photogenerator included in the reference photosensitive composition and the photogenerator included in the photosensitive composition for measurement must be compounds of the same structure, and the content of the photogenerator included in the reference photosensitive composition and the content of the photogenerator included in the photosensitive composition for measurement may be different. Accordingly, for example, if the reference photosensitive composition includes photogenerator X and an acid-degradable resin containing specific repeating unit A and specific repeating unit B, the photosensitive composition for measurement also includes photogenerator X and an acid-degradable resin containing specific repeating unit A and specific repeating unit B.

[0184] In addition, if the reference photosensitive composition contains components other than a photogenerator and an acid-degradable resin, the photosensitive composition for measurement also contains other components of the same type (e.g., an acid diffusion control agent). For example, if the reference photosensitive composition contains an acid diffusion control agent Z, the photosensitive composition for measurement also contains an acid diffusion control agent Z having the same structure as the acid diffusion control agent Z included in the reference photosensitive composition, and the content thereof may differ. Furthermore, if a resin containing repeating units is used as another component, just like the acid-degradable resin, the type of repeating unit of the resin included in the reference photosensitive composition and the type of repeating unit of the resin included in the photosensitive composition for measurement must be the same, and the content of the repeating unit and the content of the resin may differ.

[0185] In addition, the photosensitive composition for measurement is often a composition from a different lot with a different manufacturing time from the reference photosensitive composition.

[0186] Below, each component is explained in detail.

[0187] Acid-degradable resin having groups that decompose by the action of acid to generate polar groups

[0188] The standard photosensitive composition comprises an acid-degradable resin (hereinafter also simply referred to as "resin (A)") having a group that decomposes upon the action of an acid to generate a polar group (hereinafter also simply referred to as an "acid-degradable group").

[0189] The details of the acid-degradable resin will be explained in detail in the following paragraph, but as one of the suitable embodiments of the acid-degradable resin, the acid-degradable resin has repeating units derived from monomers having groups that decompose by the action of acid and generate polar groups, and all of the monomers have a solubility index (R) based on the Hansen solubility parameter for the treatment solution, represented by Equation (1) described later, of 2.0 to 5.0 (MPa). 1 / 2And, furthermore, at least one of the monomers has a difference (ΔR) in the solubility index (R) before and after oxy- 1 / 2 Examples of such modes can be cited.

[0190] Below, the above characteristics will be explained first.

[0191] As an example of specifying a resin having desired characteristics, Hansen solubility parameters can be used.

[0192] The Hansen solubility parameter represents the solubility of a substance in three dimensions by dividing it into three components (dispersion term δd, polarity term δp, and hydrogen bonding term δh). The dispersion term δd represents the effect of dispersion forces, the polarity term δp represents the effect of inter-dipole forces, and the hydrogen bonding term δh represents the effect of hydrogen bonding forces.

[0193] The definition and calculation of Hansen solubility parameters are described in Charles M. Hansen's *Hansen Solubility Parameters: A Users Handbook* (CRC Press, 2007). Additionally, by using the computer software *Hansen Solubility Parameters in Practice* (HSPiP), Hansen solubility parameters can be easily estimated from the chemical structure, even for compounds for which literature values ​​are unknown. In the present invention, the dispersion term δd, polarity term δp, and hydrogen bonding term δh of the monomer are determined by using the estimated values ​​obtained using HSPiP version 4.1. For solvents and monomers registered in the database, their values ​​are used.

[0194] Generally, the Hansen solubility parameter of a monomer constituting a specific resin can be determined by a solubility test in which a sample of the monomer constituting the resin is dissolved in numerous different solvents for which the Hansen solubility parameter is determined, and the solubility is measured. Specifically, among the solvents used in the solubility test, a sphere (sodium sphere) is identified in which all three-dimensional points of the solvent in which the monomer constituting the resin is dissolved are contained within the sphere, and points of the solvent in which it is not dissolved are placed outside the sphere, and the center coordinates of that sphere are used as the Hansen solubility parameter of the monomer constituting the resin.

[0195] For example, if the Hansen solubility parameter of another solvent that was not used to measure the Hansen solubility parameter of the monomer constituting the resin is (δd, δp, δh), and the point represented by that coordinate is contained within the solubility sphere of the monomer constituting the resin, it is considered that the solvent dissolves the monomer constituting the resin. On the other hand, if the point represented by that coordinate is outside the solubility sphere of the monomer constituting the resin, it is considered that the solvent cannot dissolve the monomer constituting the resin.

[0196] In the present invention, a resin (A) composed of such structural units can be used, wherein, using the above Hansen solubility parameter, a structural unit (or monomer) located at a certain distance from the treatment solution—that is, based on the coordinates which are the Hansen solubility parameters of the treatment solution—is appropriately dissolved in the treatment solution.

[0197] That is, the dispersion term of the Hansen solubility parameter of the treatment solution is δd2(MPa) 1 / 2 , polar term δp2(MPa) 1 / 2 and hydrogen bonding term δh2(MPa) 1 / 2Thus, the solubility parameter distance R from the treatment solution, represented by Equation (1) based on the Hansen solubility parameter, is used as the solubility index for each monomer that induces the structural unit constituting the resin (hereinafter, it may be referred to as the solubility index (R).).

[0198] Equation (1) R=(4(δd1-δd2) 2 +(δp1-δp2) 2 +(δh1-δh2) 2 ) 1 / 2

[0199] δd1 represents the dispersion term in the Hansen solubility parameter of the above monomer.

[0200] δp1 represents the polar term in the Hansen solubility parameter of the above monomer.

[0201] δh1 represents the hydrogen bonding term in the Hansen solubility parameter of the above monomer.

[0202] δd2 represents the dispersion term in the Hansen solubility parameter of the above-mentioned treatment solution.

[0203] δp2 represents the polarity term in the Hansen solubility parameter of the above-mentioned treatment solution.

[0204] δh2 represents the hydrogen bonding term in the Hansen solubility parameter of the above-mentioned treatment solution.

[0205] In addition, δd2, δp2, or δh2 of the treatment solution is obtained by multiplying the δd2, δp2, or δh2 of the solvent component (e.g., aromatic hydrocarbon, organic solvent) included in the treatment solution by the content ratio of the solvent component and summing the results.

[0206] In resin (A), all monomers having groups that decompose by the action of acid to generate polar groups have a solubility index (R) of 2.0 to 5.0 (MPa) 1 / 2 It is desirable that it be 3.1~4.9 (MPa) 1 / 2 It is more desirable to have 3.2~4.9 (MPa)1 / 2 It is more desirable to be.

[0207] At least one of the structural units included in the resin (A) has a difference in solubility index (R) before and after oxy-nitrification (difference in solubility index (△R)) of 4.0 (MPa) 1 / 2 It is preferable that the structural unit be derived from a monomer having a group that generates a polar group by decomposing through the action of the above acid.

[0208] The upper limit of the above ΔR is not specifically restricted, but 10(MPa) 1 / 2 There are many cases where it is less than that.

[0209] The repeating units included in the acid-degradable resin are described in detail below.

[0210] ≪Repeating unit having an acid-degrading group (Aa)≫

[0211] It is preferable that the resin (A) has a repeating unit (Aa) having a group that decomposes by the action of an acid and generates a polar group (hereinafter also referred to as "repeating unit (Aa)").

[0212] The acid-degradable group is a group that decomposes upon the action of an acid to generate a polar group, and it is desirable for the polar group to have a structure in which the polar group is protected by a detaching group that is detached upon the action of an acid. A resin having a repeating unit (Aa) has increased polarity upon the action of an acid, which increases solubility in an alkaline developer and decreases solubility in an organic solvent.

[0213] As for the polar group, an alkali-soluble group is preferred, and examples include an acidic group such as a carboxyl group, a phenolic hydroxyl group, a fluorinated alcohol group, a sulfonic acid group, a sulfonamide group, a sulfonylimide group, a (alkylsulfonyl)(alkylcarbonyl)methylene group, a (alkylsulfonyl)(alkylcarbonyl)imide group, a bis(alkylcarbonyl)methylene group, a bis(alkylsulfonyl)imide group, a bis(alkylsulfonyl)methylene group, a bis(alkylsulfonyl)imide group, a tris(alkylcarbonyl)methylene group, and a tris(alkylsulfonyl)methylene group, and an alcoholic hydroxyl group.

[0214] Among these, as polar groups, a carboxyl group, a phenolic hydroxyl group, a fluorinated alcohol group (preferably a hexafluoroisopropanol group), or a sulfonic acid group is preferred.

[0215] Examples of groups that are removed by the action of acid include the groups represented by equations (Y1) to (Y4).

[0216] Equation (Y1): -C(Rx1)(Rx2)(Rx3)

[0217] Equation (Y2): -C(=O)OC(Rx1)(Rx2)(Rx3)

[0218] Equation (Y3): -C(R 36 )(R 37 )(OR 38 )

[0219] Equation (Y4): -C(Rn)(H)(Ar)

[0220] In formulas (Y1) and (Y2), Rx1 to Rx3 each independently represent an alkyl group (straight or branched), a cycloalkyl group (monocyclic or polycyclic), an alkeneyl group (straight or branched), or an aryl group (monocyclic or polycyclic). Additionally, when all of Rx1 to Rx3 are alkyl groups (straight or branched), it is preferable that at least two of Rx1 to Rx3 are methyl groups.

[0221] Among these, it is preferable that Rx1 to Rx3 each independently represent a straight-chain or branched-chain alkyl group, and it is more preferable that Rx1 to Rx3 each independently represent a straight-chain alkyl group.

[0222] Two of Rx1 to Rx3 may combine to form a monocyclic or polycyclic ring.

[0223] As for the alkyl groups of Rx1 to Rx3, alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and t-butyl groups, are preferred.

[0224] As for the cycloalkyl groups of Rx1 to Rx3, monocyclic cycloalkyl groups such as cyclopentyl and cyclohexyl groups, and polycyclic cycloalkyl groups such as norbornyl groups, tetracyclodecaneyl groups, tetracyclododecaneyl groups, and adamantyl groups are preferred.

[0225] As for the aryl groups of Rx1 to Rx3, aryl groups having 6 to 10 carbon atoms are preferred, and examples include phenyl groups, naphthyl groups, and anthryl groups.

[0226] As for the alkene groups of Rx1~Rx3, a vinyl group is preferred.

[0227] As for the ring formed by combining two of Rx1 to Rx3, a cycloalkyl group is preferred. As for the cycloalkyl group formed by combining two of Rx1 to Rx3, a monocyclic cycloalkyl group such as a cyclopentyl group or a cyclohexyl group, or a polycyclic cycloalkyl group such as a norbornyl group, a tetracyclodecaneyl group, a tetracyclododecaneyl group, or an adamantyl group is preferred, and a monocyclic cycloalkyl group having 5 to 6 carbon atoms is more preferred.

[0228] The cycloalkyl group formed by the combination of two of Rx1 to Rx3 may, for example, have one of the methylene groups constituting the ring substituted with a heteroatom such as an oxygen atom, a group having a heteroatom such as a carbonyl group, or a vinylidene group. In addition, one or more of the ethylene groups constituting the cycloalkane ring may be substituted with a vinylene group.

[0229] The group represented by formula (Y1) or formula (Y2) is preferably, for example, in which Rx1 is a methyl group or an ethyl group, and Rx2 and Rx3 are combined to form the cycloalkyl group described above.

[0230] In the case where the reference photosensitive composition and the photosensitive composition for measurement are, for example, a resist composition for EUV exposure, the alkyl group, cycloalkyl group, alkenyl group, aryl group represented by Rx1 to Rx3, and the ring formed by combining two of Rx1 to Rx3, may additionally have a fluorine atom or an iodine atom as a substituent.

[0231] In equation (Y3), R 36 ~R 38 Each independently represents a hydrogen atom or a monovalent organic group. R 37 and R 38 Silver may combine with each other to form rings. Examples of monovalent organic groups include alkyl groups, cycloalkyl groups, aryl groups, aralkyl groups, and alkenyl groups. R 36 It is also desirable that it be a hydrogen atom.

[0232] In addition, the above alkyl group, cycloalkyl group, aryl group, and aralkyl group may include a group having a heteroatom such as an oxygen atom and / or a heteroatom such as a carbonyl group. For example, the above alkyl group, cycloalkyl group, aryl group, and aralkyl group may be substituted with, for example, one or more methylene groups having a heteroatom such as an oxygen atom and / or a heteroatom such as a carbonyl group.

[0233] In addition, regarding the repeating unit having an acid-degradable group described later, R 38 It may combine with other substituents on the main chain of the repeating unit to form a ring. R 38 The group formed by the bonding of other substituents on the main chain of the repeating unit is preferably an alkylene group such as a methylene group.

[0234] In the case where the reference photosensitive composition and the photosensitive composition for measurement are, for example, a resist composition for EUV exposure, R 36 ~R 38 A monovalent organic group represented by, and, R 37 and R 38It is also desirable for the ring formed by these mutual bonding to additionally have a fluorine atom or an iodine atom as a substituent.

[0235] As for Equation (Y3), it is preferable to have a group represented by the following Equation (Y3-1).

[0236] [Chemical Formula 2]

[0237]

[0238] Here, L1 and L2 each independently represent a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, or a combination thereof (e.g., a combination of an alkyl group and an aryl group).

[0239] M represents a single bond or a divalent linker.

[0240] Q represents an alkyl group that may contain a heteroatom, a cycloalkyl group that may contain a heteroatom, an aryl group that may contain a heteroatom, an amino group, an ammonium group, a mercapto group, a cyano group, an aldehyde group, or a combination thereof (e.g., a combination of an alkyl group and a cycloalkyl group).

[0241] The alkyl group and the cycloalkyl group may be substituted, for example, with one of the methylene groups being a heteroatom such as an oxygen atom or a group having a heteroatom such as a carbonyl group.

[0242] In addition, it is preferable that one of L1 and L2 is a hydrogen atom, and the other is an alkyl group, a cycloalkyl group, an aryl group, or a group combining an alkylene group and an aryl group.

[0243] At least two of Q, M, and L1 may be combined to form a ring (preferably, a 5-membered or 6-membered ring).

[0244] In terms of pattern miniaturization, it is preferable that L2 be a secondary or tertiary alkyl group, and more preferable that it be a tertiary alkyl group. Examples of secondary alkyl groups include isopropyl groups, cyclohexyl groups, or norbornyl groups, and examples of tertiary alkyl groups include tert-butyl groups or adamantane groups.

[0245] In the case where the reference photosensitive composition and the photosensitive composition for measurement are, for example, a resist composition for EUV exposure, it is also preferable that the alkyl group, cycloalkyl group, aryl group, and a combination thereof represented by L1 and L2 further have a fluorine atom or an iodine atom as a substituent. In addition, it is also preferable that the alkyl group, cycloalkyl group, aryl group, and aralkyl group contain heteroatoms such as oxygen atoms in addition to fluorine atoms and iodine atoms (i.e., the alkyl group, cycloalkyl group, aryl group, and aralkyl group are, for example, one of the methylene groups is substituted with a heteroatom such as an oxygen atom or a heteroatom such as a carbonyl group).

[0246] In addition, when the reference photosensitive composition and the photosensitive composition for measurement are, for example, a resist composition for EUV exposure, among the alkyl group that may contain a heteroatom represented by Q, the cycloalkyl group that may contain a heteroatom, the aryl group that may contain a heteroatom, the amino group, the ammonium group, the mercapto group, the cyano group, the aldehyde group, and the groups combined therewith, the heteroatom is preferably a heteroatom selected from the group consisting of a fluorine atom, an iodine atom, and an oxygen atom.

[0247] In formula (Y4), Ar represents an aromatic group. Rn represents an alkyl group, a cycloalkyl group, or an aryl group. Rn and Ar may bond to each other to form a non-aromatic ring. More preferably, Ar is an aryl group.

[0248] In the case where the reference photosensitive composition and the photosensitive composition for measurement are, for example, a resist composition for EUV exposure, it is also preferable that the aromatic group represented by Ar, and the alkyl group, cycloalkyl group, and aryl group represented by Rn have fluorine atoms and iodine atoms as substituents.

[0249] In terms of further improving acid decompositionability, when a non-aromatic ring is directly bonded to a polar group (or its residue) in a degreasing agent protecting a polar group, it is also desirable that the reducing atom adjacent to the reducing atom directly bonded to the polar group (or its residue) among the non-aromatic rings does not have a halogen atom, such as a fluorine atom, as a substituent.

[0250] The detachable group that is removed by the action of acid may also be a 2-cyclopentenyl group having a substituent (alkyl group, etc.) such as a 3-methyl-2-cyclopentenyl group, and a cyclohexyl group having a substituent (alkyl group, etc.) such as a 1,1,4,4-tetramethylcyclohexyl group.

[0251] As for the repeating unit (Aa), the repeating unit represented by Equation (A) is also desirable.

[0252] [Chemical Formula 3]

[0253]

[0254] L1 represents a divalent linker that may have a fluorine atom or an iodine atom, R1 represents a hydrogen atom, a fluorine atom, an iodine atom, an alkyl group that may have a fluorine atom or an iodine atom, or an aryl group that may have a fluorine atom or an iodine atom, and R2 represents a detaching group that is detached by the action of an acid and may have a fluorine atom or an iodine atom.

[0255] In addition, as a suitable mode of the repeating unit represented by formula (A), at least one of L1, R1, and R2 may have a mode having a fluorine atom or an iodine atom.

[0256] L1 represents a divalent linker that may have a fluorine atom or an iodine atom. Examples of divalent linkers that may have a fluorine atom or an iodine atom include -CO-, -O-, -S-, -SO-, -SO2-, hydrocarbon groups that may have a fluorine atom or an iodine atom (e.g., alkylene groups, cycloalkylene groups, alkenylene groups, arylene groups, etc.), and linkers formed by connecting multiple such groups. Among these, as L1, -CO-, an arylene group, or -arylene group-alkylene group that may have a fluorine atom or an iodine atom is preferred, and -CO-, an arylene group, or -arylene group-alkylene group that may have a fluorine atom or an iodine atom is more preferred.

[0257] As for the arylene group, a phenylene group is preferred.

[0258] The alkylene group may be in a straight chain or a branched chain. The number of carbon atoms in the alkylene group is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 3.

[0259] When the alkylene group has a fluorine atom or an iodine atom, the total number of fluorine atoms and iodine atoms included in the alkylene group is not particularly limited, but 2 or more is preferred, 2 to 10 is more preferred, and 3 to 6 is more preferred.

[0260] R1 represents a hydrogen atom, a fluorine atom, an iodine atom, an alkyl group that may have a fluorine atom or an iodine atom, or an aryl group that may have a fluorine atom or an iodine atom.

[0261] The alkyl group may be in a straight chain or a branched chain. The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 3.

[0262] The total number of fluorine atoms and iodine atoms included in an alkyl group having a fluorine atom or an iodine atom is not particularly limited, but 1 or more is preferred, 1 to 5 is more preferred, and 1 to 3 is more preferred.

[0263] The above alkyl group may include heteroatoms such as oxygen atoms other than halogen atoms.

[0264] R2 represents a deluminater that is deluminated by the action of an acid and may have a fluorine atom or an iodine atom. Examples of deluminaters that may have a fluorine atom or an iodine atom include those represented by the above-described formulas (Y1) to (Y4) and those having a fluorine atom or an iodine atom, and the suitability mode is the same.

[0265] As for the repeating unit (Aa), the repeating unit represented by the general formula (AI) is also desirable.

[0266] [Chemical Formula 4]

[0267]

[0268] In the general formula (AI),

[0269] Xa1 represents a hydrogen atom, or an alkyl group that may have a substituent.

[0270] T represents a single bond, or a divalent linker.

[0271] Rx1 to Rx3 each independently represent an alkyl group (straight or branched), a cycloalkyl group (single or polycyclic), an aryl group, or an alkeneyl group. However, if all of Rx1 to Rx3 are alkyl groups (straight or branched), it is preferable that at least two of Rx1 to Rx3 are methyl groups.

[0272] Two of Rx1 to Rx3 may be combined to form a cycloalkyl group (monocyclic or polycyclic).

[0273] The alkyl group that may have a substituent, represented by Xa1, is, for example, a methyl group or -CH2-R 11 One example is the energy manifested as. R 11 It represents a halogen atom (such as a fluorine atom), a hydroxyl group, or a monovalent organic group, and examples include an alkyl group having 5 or fewer carbon atoms that may be substituted with a halogen atom, an acyl group having 5 or fewer carbon atoms that may be substituted with a halogen atom, and an alkoxy group having 5 or fewer carbon atoms that may be substituted with a halogen atom, wherein an alkyl group having 3 or fewer carbon atoms is preferred, and a methyl group is more preferred. As Xa1, a hydrogen atom, a methyl group, a trifluoromethyl group, or a hydroxymethyl group is preferred.

[0274] Examples of the divalent linking groups of T include alkylene groups, aromatic groups, -COO-Rt- groups, and -O-Rt- groups. In the formula, Rt represents an alkylene group or a cycloalkylene group.

[0275] T is preferably a single bond or a -COO-Rt- group. When T represents a -COO-Rt- group, Rt is preferably an alkylene group having 1 to 5 carbon atoms, and more preferably a -CH2- group, a -(CH2)2- group, or a -(CH2)3- group.

[0276] As for the alkyl groups of Rx1 to Rx3, alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and t-butyl groups, are preferred.

[0277] As for the cycloalkyl groups of Rx1 to Rx3, a monocyclic cycloalkyl group such as a cyclopentyl group and a cyclohexyl group, or a polycyclic cycloalkyl group such as a norbornyl group, a tetracyclodecaneyl group, a tetracyclododecaneyl group, and an adamantyl group is preferred.

[0278] As for the cycloalkyl group formed by the combination of two of Rx1 to Rx3, a monocyclic cycloalkyl group such as a cyclopentyl group and a cyclohexyl group is preferred, and additionally, a polycyclic cycloalkyl group such as a norvonyl group, a tetracyclodecaneyl group, a tetracyclododecaneyl group, and an adamantyl group is preferred. Among these, a monocyclic cycloalkyl group having 5 to 6 carbon atoms is preferred.

[0279] The cycloalkyl group formed by the combination of two of Rx1 to Rx3 may, for example, have one of the methylene groups constituting the ring substituted with a heteroatom such as an oxygen atom, or a group having a heteroatom such as a carbonyl group.

[0280] As for the alkene devices of Rx1~Rx3, vinyl devices can be cited.

[0281] Phenyl groups can be used as aryl groups of Rx1~Rx3.

[0282] The repeating unit represented by the general formula (AI) is preferably, for example, in which Rx1 is a methyl or ethyl group and Rx2 and Rx3 are combined to form the cycloalkyl group described above.

[0283] When each of the above groups has a substituent, examples of the substituents include alkyl groups (1 to 4 carbon atoms), halogen atoms, hydroxyl groups, alkoxy groups (1 to 4 carbon atoms), carboxyl groups, and alkoxycarbonyl groups (2 to 6 carbon atoms). The number of carbon atoms in the substituents is preferably 8 or less.

[0284] The repeating unit represented by the general formula (AI) is preferably an acid-degradable (meth)acrylic acid tertiary alkyl ester repeating unit (a repeating unit in which Xa1 represents a hydrogen atom or a methyl group and T represents a single bond).

[0285] The resin (A) may have only one type of repeating unit (Aa) or two or more types.

[0286] The content of repeating units (Aa) (total content in cases where two or more types of repeating units (Aa) exist) is preferably 15 to 80 mol% with respect to the total repeating units in the resin (A), and more preferably 20 to 70 mol%.

[0287] Preferably, resin (A) has at least one repeating unit selected from the group consisting of repeating units represented by the following general formulas (A-VIII) to (A-XII), as a repeating unit (Aa).

[0288] [Chemical Formula 5]

[0289]

[0290] In general formula (A-VIII), R5 represents a tert-butyl group, -CO-O-(tert-butyl) group.

[0291] In general formula (A-IX), R6 and R7 each independently represent a monovalent organic group. Examples of monovalent organic groups include alkyl groups, cycloalkyl groups, aryl groups, aralkyl groups, and alkenyl groups.

[0292] In the general formula (AX), p represents 1 or 2.

[0293] In general formulas (AX) to (A-XII), R8 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R9 represents an alkyl group having 1 to 3 carbon atoms.

[0294] Among the general formula (A-XII), R 10 It represents a carbon alkyl group having 1 to 3 carbon atoms or an adamantyl group.

[0295] ≪Repetitive unit with a variability (A-1)≫

[0296] The resin (A) may have a repeating unit (A-1) having an acid group.

[0297] As for the acid group, an acid group with a pKa of 13 or less is preferred. As for the acid dissociation constant of the acid group, 13 or less is preferred, 3 to 13 is more preferred, and 5 to 10 is more preferred.

[0298] When the resin (A) has acid groups with a pKa of 13 or less, the content of acid groups in the resin (A) is not particularly limited, but is often 0.2 to 6.0 mmol / g. Among these, 0.8 to 6.0 mmol / g is preferred, 1.2 to 5.0 mmol / g is more preferred, and 1.6 to 4.0 mmol / g is more preferred. If the content of acid groups is within the above range, the development proceeds well, the formed pattern shape is superior, and the resolution is also superior.

[0299] As for the acid group, for example, a carboxyl group, a hydroxyl group, a phenolic hydroxyl group, a fluorinated alcohol group (preferably a hexafluoroisopropanol group), a sulfonic acid group, a sulfonamide group, or an isopropanol group is preferred.

[0300] In addition, one or more (preferably one to two) fluorine atoms of the hexafluoroisopropanol group may be substituted with a group other than a fluorine atom (such as an alkoxycarbonyl group). The -C(CF3)(OH)-CF2- formed in this way is also preferred as an acid group. In addition, one or more fluorine atoms may be substituted with a group other than a fluorine atom to form a ring containing -C(CF3)(OH)-CF2-.

[0301] A repeating unit (A-1) having an acid group is preferably a repeating unit having a structure in which a polar group is protected by a detaching group that is detached by the action of the acid described above, and a repeating unit (A-2) having a lactone group, a sulfonate group, or a carbonate group described later.

[0302] Repeating units having acid groups may have fluorine atoms or iodine atoms.

[0303] As for the repeating unit having an acid group, a repeating unit having a phenolic hydroxyl group is preferred, and a repeating unit represented by formula (Y) is more preferred.

[0304] [Chemical Formula 6]

[0305]

[0306] In formula (Y), A represents a hydrogen atom, an alkyl group, a cycloalkyl group, a halogen atom, or a cyano group.

[0307] L represents a single bond or a divalent linker having an oxygen atom. It is preferable that L be a single bond.

[0308] R represents a halogen atom, an alkyl group, a cycloalkyl group, an aryl group, an alkenyl group, an aralkyl group, an alkoxy group, an alkylcarbonyloxy group, an alkylsulfonyloxy group, an alkyloxycarbonyl group, or an aryloxycarbonyl group. If multiple Rs are present, they may be identical or different. If multiple Rs are present, they may be bonded to each other to form a ring. As R, a hydrogen atom is preferred.

[0309] a represents an integer from 1 to 3.

[0310] b represents an integer from 0 to (5-a).

[0311] Hereinafter, repeating units having a function are exemplified. In the formulas, a represents 1 or 2.

[0312] [Chemical Formula 7]

[0313]

[0314] [Chemical Formula 8]

[0315]

[0316] [Chemical Formula 9]

[0317]

[0318] As a repeating unit having an acid group, for example, a repeating unit having a phenolic hydroxyl group described in paragraphs 0089 to 0100 of Japanese Patent Publication No. 2018-189758 can also be suitably used.

[0319] When the resin (A) comprises repeating units (A-1) having acid groups, the reference photosensitive composition and the photosensitive composition for measurement comprising the resin (A) are preferred for KrF exposure, EB exposure, or EUV exposure. In such an embodiment, the content of repeating units having acid groups in the resin (A) is preferably 30 to 90 mol% with respect to the total repeating units in the resin (A), and more preferably 35 to 60 mol%.

[0320] ≪Repeating unit (A-2) having at least one selected from the group consisting of lactone structure, sulfone structure, carbonate structure, and hydroxyadamantane structure≫

[0321] The resin (A) may have a repeating unit (A-2) having at least one selected from the group consisting of a lactone structure, a carbonate structure, a sulfone structure, and a hydroxyadamantane structure.

[0322] The lactone structure or selton structure in the repeating unit having a lactone structure or a selton structure is not particularly limited, but a 5- to 7-membered ring lactone structure or a 5- to 7-membered ring selton structure is preferred, and it is more preferable that another ring structure is condensed in a form that forms a bicyclo structure or a spiro structure in the 5- to 7-membered ring lactone structure, or that another ring structure is condensed in a form that forms a bicyclo structure or a spiro structure in the 5- to 7-membered ring selton structure.

[0323] Examples of repeating units having a lactone structure or a sulfone structure include the repeating units described in paragraphs 0094 to 0107 of International Publication No. 2016 / 136354.

[0324] The resin (A) may have repeating units having a carbonate structure. The carbonate structure is preferably a cyclic carbonate ester structure.

[0325] Examples of repeating units having a carbonate structure include the repeating units described in paragraphs 0106 to 0108 of International Publication No. 2019 / 054311.

[0326] Resin (A) may have repeating units having a hydroxyadamantane structure. Examples of repeating units having a hydroxyadamantane structure include repeating units represented by the following general formula (AIIa).

[0327] [Chemical Formula 10]

[0328]

[0329] In general formula (AIIa), R1c represents a hydrogen atom, a methyl group, a trifluoromethyl group, or a hydroxymethyl group. R2c to R4c each independently represent a hydrogen atom or a hydroxyl group. However, at least one of R2c to R4c represents a hydroxyl group. It is preferable that one or two of R2c to R4c are hydroxyl groups and the remainder are hydrogen atoms.

[0330] ≪Repeating unit having a fluorine atom or an iodine atom≫

[0331] Resin (A) may have repeating units having fluorine atoms or iodine atoms.

[0332] Examples of repeating units having a fluorine atom or an iodine atom include the repeating units described in paragraphs 0080 to 0081 of Japanese Patent Publication No. 2019-045864.

[0333] ≪Repeating unit having a mine generator≫

[0334] Resin (A) may have a repeating unit other than the above that has a group that generates acid upon irradiation with radiation.

[0335] Examples of repeating units having a light generator include the repeating units described in paragraphs 0092 to 0096 of Japanese Patent Publication No. 2019-045864.

[0336] ≪Repeating unit having alkali-soluble groups≫

[0337] The resin (A) may have repeating units having alkali-soluble groups.

[0338] Examples of alkali-soluble groups include carboxyl groups, sulfonamide groups, sulfonylimide groups, bissulfonylimide groups, and aliphatic alcohols in which the α-position is substituted with an electron-repellent group (e.g., hexafluoroisopropanol groups), and carboxyl groups are preferred. As the resin (A) has repeating units having alkali-soluble groups, the resolution for contact hole applications is increased.

[0339] Examples of repeating units having alkali-soluble groups include repeating units in which the alkali-soluble group is directly bonded to the main chain of the resin, such as repeating units made of acrylic acid and methacrylic acid, or repeating units in which the alkali-soluble group is bonded to the main chain of the resin through a linker. Additionally, the linker may have a monocyclic or polycyclic cyclic hydrocarbon structure.

[0340] As a repeating unit having an alkali-soluble group, a repeating unit made of acrylic acid or methacrylic acid is preferred.

[0341] ≪Repeating unit having neither an acid-degrading group nor a polar group≫

[0342] The resin (A) may also have repeating units that do not have either acid-degradable groups or polar groups. The repeating units that do not have either acid-degradable groups or polar groups preferably have a cycloaliphatic hydrocarbon structure.

[0343] Examples of repeating units that do not have either an acid-degrading group or a polar group include, for instance, the repeating unit described in paragraphs 0236–0237 of U.S. Patent Application Publication No. 2016 / 0026083, and the repeating unit described in paragraph 0433 of U.S. Patent Application Publication No. 2016 / 0070167.

[0344] In addition to the repeating structure unit described above, the resin (A) may have various repeating structure units for the purpose of controlling dry etching resistance, standard developer suitability, substrate adhesion, resist profile, resolution, heat resistance, and sensitivity.

[0345] ≪Characteristics of Suji (A)≫

[0346] As for the resin (A), all of the repeating units may be composed of repeating units derived from (meth)acrylate-based monomers. In this case, any resin may be used in which all of the repeating units are derived from methacrylate-based monomers, all of the repeating units are derived from acrylate-based monomers, or all of the repeating units are derived from methacrylate-based monomers and acrylate-based monomers. It is preferable that the repeating units derived from acrylate-based monomers are 50 mol% or less of the total repeating units in the resin (A).

[0347] When the reference photosensitive composition and the photosensitive composition for measurement are for argon fluoride (ArF) exposure, it is preferable that the resin (A) substantially does not have aromatic groups in terms of the transmittance of ArF light. More specifically, it is preferable that the repeating unit having an aromatic group is 5 mol% or less with respect to the total repeating unit of the resin (A), more preferable that it is 3 mol% or less, and ideally 0 mol%, that is, it is more preferable that it has no repeating unit having an aromatic group.

[0348] In addition, when the reference photosensitive composition and the photosensitive composition for measurement are for ArF exposure, it is preferable that the resin (A) has a monocyclic or polycyclic alicyclic hydrocarbon structure, and also preferable that it does not contain both fluorine atoms and silicon atoms.

[0349] When the reference photosensitive composition and the photosensitive composition for measurement are for krypton fluoride (KrF) exposure, EB exposure, or EUV exposure, it is preferable that the resin (A) has repeating units having aromatic hydrocarbon groups, and more preferable that it has repeating units having phenolic hydroxyl groups.

[0350] Examples of repeating units having a phenolic hydroxyl group include the repeating unit (A-1) exemplified above having an acid group, and repeating units derived from hydroxystyrene (meth)acrylate.

[0351] In addition, when the reference photosensitive composition and the photosensitive composition for measurement are for KrF exposure, EB exposure, or EUV exposure, it is also preferable that the resin (A) has repeating units having a structure protected by a group (detacher) in which a hydrogen atom of a phenolic hydroxyl group is decomposed and detached by the action of an acid.

[0352] When the reference photosensitive composition and the photosensitive composition for measurement are for KrF exposure, EB exposure, or EUV exposure, the content of repeating units having aromatic hydrocarbon groups included in the resin (A) is preferably 30 to 100 mol% with respect to the total repeating units in the resin (A), and more preferably 35 to 100 mol%.

[0353] Resin (A) can be synthesized by a conventional method (e.g., radical polymerization).

[0354] The weight average molecular weight (Mw) of the resin (A) is preferably 1,000 to 200,000, more preferably 3,000 to 20,000, and more preferably 5,000 to 15,000. By setting the weight average molecular weight (Mw) of the resin (A) to 1,000 to 200,000, deterioration of heat resistance and dry etching resistance can be prevented, and also deterioration of developability and deterioration of film-forming ability due to increased viscosity can be prevented. In addition, the weight average molecular weight (Mw) of the resin (A) is a polystyrene equivalent value measured by the GPC method described above.

[0355] The degree of dispersion (molecular weight distribution) of the resin (A) is typically 1 to 5, 1 to 3 is preferred, and 1.1 to 2.0 is more preferred. The smaller the degree of dispersion, the better the resolution and resist shape, and the smoother the sidewalls of the pattern, the better the roughness.

[0356] In the reference photosensitive composition and the photosensitive composition for measurement, the content of resin (A) is preferably 50 to 99.9 mass% with respect to the total solid content of the reference photosensitive composition and the photosensitive composition for measurement, and more preferably 60 to 99.0 mass%.

[0357] Also, resin (A) may be used as a single type or in combination with two or more types.

[0358] Mineral Generator

[0359] The reference photosensitive composition and the photosensitive composition for measurement include a photogenerator (B). The photogenerator (B) is not particularly limited as long as it is a compound that generates acid upon irradiation with radiation.

[0360] The photogenerator (B) may be in the form of a low-molecular-weight compound or introduced into a part of the polymer. In addition, the form of a low-molecular-weight compound and the form introduced into a part of the polymer may be used in combination.

[0361] When the photogenerator (B) is in the form of a low molecular weight compound, it is preferable that the weight average molecular weight (Mw) is 3000 or less, more preferable that it is 2000 or less, and more preferable that it is 1000 or less.

[0362] When the photogenerator (B) is in a form introduced into a part of the polymer, it may be introduced into a part of the resin (A), or it may be introduced into a resin different from the resin (A).

[0363] The photogenerator (B) is preferably in the form of a low-molecular-weight compound.

[0364] As for the photogenerator (B), it is not particularly limited as long as it is a known one, but a compound that generates an organic acid upon irradiation with radiation is preferred, and a photogenerator having a fluorine atom or an iodine atom in its molecule is more preferred.

[0365] Examples of the above organic acids include sulfonic acid (aliphatic sulfonic acid, aromatic sulfonic acid, and camphorsulfonic acid, etc.), carboxylic acid (aliphatic carboxylic acid, aromatic carboxylic acid, and aralkylcarboxylic acid, etc.), carbonylsulfonylimide, bis(alkylsulfonyl)imide, and tris(alkylsulfonyl)methide.

[0366] The volume of acid generated from the photogenerative agent (B) is not particularly limited, but in terms of suppressing the diffusion of acid generated by exposure to the non-exposed area and improving resolution, 240 Å 3 The above is desirable, and 305Å 3 The above is more preferable, and 350Å 3 The above is more desirable, and 400Å 3 The above is particularly desirable. In addition, in terms of sensitivity or solubility as a coating solvent, the volume of acid generated from the photogenerator (B) is 1500 Å. 3 The following is preferable, and 1000 Å 3 The following is more preferable, and 700Å 3 The following is more desirable.

[0367] The above volume values ​​are obtained using "WinMOPAC" manufactured by Fujitsu Corporation. In calculating the above volume values, first, the chemical structure of the acid for each example is input, and next, the most stable stereochemical position of each acid is determined by calculating the molecular force field using the MM (Molecular Mechanics) 3 method with this structure as the initial structure, and then, the "accessible volume" of each acid can be calculated by performing molecular orbital calculations using the PM (Parameterized Model Number) 3 method for these most stable stereochemical positions.

[0368] The structure of the acid generated from the photogenerator (B) is not particularly limited, but it is desirable that the interaction between the acid generated from the photogenerator (B) and the resin (A) be strong in order to suppress the diffusion of the acid and improve the resolution. In this regard, when the acid generated from the photogenerator (B) is an organic acid, for example, it is desirable to have additional polar groups in addition to organic acid groups such as sulfonic acid groups, carboxylic acid groups, carbonylsulfonylimide acid groups, bissulfonylimide acid groups, and trissulfonylmedide acid groups.

[0369] Examples of polar groups include, for instance, ether groups, ester groups, amide groups, acyl groups, sulfo groups, sulfonyloxy groups, sulfonamide groups, thioether groups, thioester groups, urea groups, carbonate groups, carbamate groups, hydroxyl groups, and mercapto groups.

[0370] The number of polar groups of the acid generated is not particularly limited, but it is preferable to have one or more, and more preferable to have two or more. However, from the perspective of suppressing excessive phenomena, it is preferable that the number of polar groups be less than 6, and more preferable to have less than 4.

[0371] Among them, it is preferable that the photogenerator (B) be a photogenerator composed of an anionic part and a cation part.

[0372] As for the photocatalytic agent (B), the photocatalytic agent described in paragraphs 0144 to 0173 of Japanese Patent Publication No. 2019-045864 can be cited.

[0373] The content of the photogenerator (B) is not particularly limited, but with respect to the total solid content of the reference photosensitive composition and the photosensitive composition for measurement, 5 to 50 mass% is preferred, 5 to 40 mass% is more preferred, and 5 to 35 mass% is more preferred.

[0374] The photocatalytic agent (B) may be used as a single type or in combination of two or more types. When two or more types of photocatalytic agents (B) are used in combination, it is preferable that the total amount be within the above range.

[0375] <Acid Diffusion Control Agent (C)>

[0376] The reference photosensitive composition and the photosensitive composition for measurement may include an acid diffusion control agent (C).

[0377] The acid diffusion control agent (C) acts as a quencher that traps the acid generated from the photogenerative agent (B) during exposure and suppresses the reaction of the acid-degradable resin in the unexposed area caused by the excess generated acid. As for the acid diffusion control agent (C), examples may be used, such as a basic compound (CA), a basic compound whose basicity is reduced or lost upon irradiation with radiation (CB), an onium salt (CC) that becomes a relatively weak acid with respect to the photogenerative agent (B), a low-molecular-weight compound (CD) having a nitrogen atom and a group that is detached by the action of the acid, and an onium salt compound (CE) having a nitrogen atom in the cation portion.

[0378] In the reference photosensitive composition and the photosensitive composition for measurement, known acid diffusion control agents may be appropriately used. For example, known compounds disclosed in paragraphs

[0627] –

[0664] of U.S. Patent Application Publication No. 2016 / 0070167, paragraphs

[0095] –

[0187] of U.S. Patent Application Publication No. 2015 / 0004544, paragraphs

[0403] –

[0423] of U.S. Patent Application Publication No. 2016 / 0237190, and paragraphs

[0259] –

[0328] of U.S. Patent Application Publication No. 2016 / 0274458 may be suitably used as acid diffusion control agents (C).

[0379] As basic compounds (CA), the repeating units described in paragraphs 0188 to 0208 of Japanese Patent Publication No. 2019-045864 can be cited.

[0380] In the reference photosensitive composition and the photosensitive composition for measurement, an onium salt (CC) that is relatively weak acid to the photogenerative agent (B) can be used as an acid diffusion control agent (C).

[0381] When a photogenerative agent (B) and an onium salt that generates an acid that is relatively weak compared to the acid generated from the photogenerative agent (B) are mixed and used, if the acid generated from the photogenerative agent (B) collides with the onium salt having unreacted weak acid anions due to irradiation with active photogenicity or radiation, the weak acid is released through salt exchange to generate an onium salt having strong acid anions. In this process, since the strong acid is exchanged for a weak acid with lower catalytic activity, the acid is seemingly deactivated and acid diffusion can be controlled.

[0382] Examples of onium salts that are relatively weak acids to the photogenerative agent (B) include the onium salts described in paragraphs 0226 to 0233 of Japanese Patent Publication No. 2019-070676.

[0383] When an acid diffusion control agent (C) is included in the reference photosensitive composition and the photosensitive composition for measurement, the content of the acid diffusion control agent (C) (the total if multiple types exist) is preferably 0.1 to 10.0 mass% with respect to the total solid content of the reference photosensitive composition and the photosensitive composition for measurement, and more preferably 0.1 to 5.0 mass%.

[0384] Acid diffusion control agent (C) may be used alone or in combination of two or more types. When two or more acid diffusion control agents (C) are used in combination, it is preferable that the total amount be within the above range.

[0385] <Hypohydrophobic resin (E)>

[0386] The reference photosensitive composition and the photosensitive composition for measurement may include a hydrophobic resin (E) that is different from the resin (A) as the hydrophobic resin.

[0387] The hydrophobic resin (E) is preferably designed to be localized on the surface of the resist film, but unlike surfactants, it does not necessarily need to have hydrophilic groups within its molecule and does not need to contribute to the uniform mixing of polar and non-polar substances.

[0388] Effects of adding a hydrophobic resin (E) include control of the static and dynamic contact angles of the resist film surface with respect to water, and suppression of out-gas.

[0389] The hydrophobic resin (E) preferably has one or more of “fluorine atoms,” “silicon atoms,” and “CH3 substructures included in the side chain portion of the resin” in terms of localization to the film surface layer, and it is more preferable to have two or more. In addition, the hydrophobic resin (E) preferably has hydrocarbon groups having five or more carbon atoms. These groups may be present in the main chain of the resin or substituted in the side chain.

[0390] When the hydrophobic resin (E) contains fluorine atoms and / or silicon atoms, the fluorine atoms and / or silicon atoms in the hydrophobic resin may be included in the main chain of the resin or in the side chain.

[0391] When the hydrophobic resin (E) has fluorine atoms, the partial structure having fluorine atoms is preferably an alkyl group having fluorine atoms, a cycloalkyl group having fluorine atoms, or an aryl group having fluorine atoms.

[0392] The alkyl group having a fluorine atom (preferably 1 to 10 carbon atoms, more preferably 1 to 4 carbon atoms) is a straight-chain or branched-chain alkyl group in which at least one hydrogen atom is substituted with a fluorine atom, and may additionally have substituents other than fluorine atoms.

[0393] The cycloalkyl group having a fluorine atom is a monocyclic or polycyclic cycloalkyl group in which at least one hydrogen atom is substituted with a fluorine atom, and may additionally have substituents other than the fluorine atom.

[0394] Examples of aryl groups having a fluorine atom include phenyl groups and naphthyl groups in which at least one hydrogen atom is substituted with a fluorine atom, and may also have substituents other than fluorine atoms.

[0395] Examples of repeating units having fluorine atoms or silicon atoms include those exemplified in paragraph 0519 of U.S. Patent Application Publication No. 2012 / 0251948.

[0396] In addition, as described above, it is also desirable that the hydrophobic resin (E) has a CH3 part structure in the side chain portion.

[0397] Here, the CH3 part structure having a side chain portion in the hydrophobic resin includes a CH3 part structure having an ethyl group and a propyl group, etc.

[0398] Meanwhile, methyl groups directly bonded to the main chain of the hydrophobic resin (E) (e.g., α-methyl groups of repeating units having a methacrylic acid structure) are not included in the CH3 substructure of the present invention because they contribute little to the surface localization of the hydrophobic resin (E) due to the influence of the main chain.

[0399] Regarding hydrophobic resin (E), reference may be made to paragraphs

[0348] to

[0415] of Japanese Patent Publication No. 2014-010245, and the contents thereof are incorporated herein by reference.

[0400] As for the hydrophobic resin (E), the resins described in Japanese Patent Publication No. 2011-248019, Japanese Patent Publication No. 2010-175859, and Japanese Patent Publication No. 2012-032544 may also be preferably used.

[0401] When the reference photosensitive composition and the photosensitive composition for measurement include a hydrophobic resin (E), the content of the hydrophobic resin (E) is preferably 0.01 to 20 mass% with respect to the total solid content of the reference photosensitive composition and the photosensitive composition for measurement, and more preferably 0.1 to 15 mass%.

[0402] <Solvent (F)>

[0403] The reference photosensitive composition and the photosensitive composition for measurement may include a solvent (F).

[0404] When the reference photosensitive composition and the photosensitive composition for measurement are radioactive resin compositions for EUV exposure, the solvent (F) preferably comprises at least one selected from the group consisting of (F1) propylene glycol monoalkyl ether carboxylate and (F2) propylene glycol monoalkyl ether, lactic acid ester, acetic acid ester, alkoxypropionic acid ester, chain ketone, cyclic ketone, lactone, and alkylene carbonate. In this case, the solvent may further comprise components other than components (F1) and (F2).

[0405] A solvent containing at least one of components (F1) and (F2) is preferred because, when used in combination with the resin (A) described above, the applicability of the reference photosensitive composition and the photosensitive composition for measurement is improved, and a pattern with a small number of development defects can be formed.

[0406] In addition, when the reference photosensitive composition and the photosensitive composition for measurement are radioactive resin compositions for ArF, the solvent (F) may be an organic solvent such as, for example, alkylene glycol monoalkyl ether carboxylate, alkylene glycol monoalkyl ether, alkyl lactate ester, alkyl alkoxypropionate, cyclic lactone (preferably 4 to 10 carbon atoms), monoketone compound that may contain a ring (preferably 4 to 10 carbon atoms), alkylene carbonate, alkyl alkoxyacetate, and alkyl pyruvate.

[0407] It is preferable to set the content of solvent (F) in the standard photosensitive composition and the photosensitive composition for measurement so that the solid content concentration is 0.5 to 40 mass%.

[0408] As one embodiment of the reference photosensitive composition and the photosensitive composition for measurement, it is also preferable that the solid content concentration be 10 mass% or more.

[0409] <Surfactant (H)>

[0410] The reference photosensitive composition and the photosensitive composition for measurement may include a surfactant (H). By including the surfactant (H), a pattern with better adhesion and fewer development defects can be formed.

[0411] As for the surfactant (H), fluorine-based and / or silicone-based surfactants are preferred.

[0412] As for fluorine-based and / or silicone-based surfactants, examples include the surfactant described in paragraph

[0276] of U.S. Patent Application Publication No. 2008 / 0248425.

[0413] In addition, the surfactant (H) may be synthesized using a fluoroaliphatic compound prepared by the telomerization method (also called the telomer method) or the oligomerization method (also called the oligomer method), in addition to the known surfactant as described above. Specifically, a polymer having fluoroaliphatic groups derived from this fluoroaliphatic compound may be used as the surfactant (H). This fluoroaliphatic compound may be synthesized, for example, by the method described in Japanese Patent Publication No. 2002-90991.

[0414] These surfactants (H) may be used as a single type, or two or more types may be used in combination.

[0415] The content of surfactant (H) is preferably 0.0001 to 2 mass% with respect to the total solid content of the reference photosensitive composition and the photosensitive composition for measurement, and more preferably 0.0005 to 1 mass%.

[0416] Other Additives

[0417] The reference photosensitive composition and the photosensitive composition for measurement may further include a crosslinking agent, an alkali-soluble resin, a dissolution-inhibiting compound, a dye, a plasticizer, a photosensitizer, a light absorber, and / or a compound that promotes solubility in a developer.

[0418] Examples

[0419] The features of the present invention will be explained more specifically below with reference to examples. The materials, reagents, amounts of substances and their ratios, and operations, etc., shown in the following examples may be appropriately modified without departing from the spirit of the present invention. Accordingly, the scope of the present invention is not limited to the following examples.

[0420] [Preparation of composition]

[0421] Each composition was prepared by mixing the ingredients listed in Table 1 below.

[0422] The "Content (mass%)" column in Table 1 indicates the content of each component relative to the total solid content in the composition. The solid content concentration of the composition was 1.5 mass%.

[0423] R in Table 1 represents the solubility index (R) of the monomer having an acid-degradable group constituting the repeating unit included in the acid-degradable resin, and the difference in solubility index (△R) before and after acid removal. In addition, R B and ΔR B and represent the solubility index (R) of the monomer and the difference in solubility index (△R) before and after oxy- C and ΔR CEach represents the solubility index (R) of the monomer and the difference in solubility index (△R) before and after oxy-

[0424] [Table 1]

[0425]

[0426] Acid-degradable resins A-1 and A-2 are resins obtained by radical polymerization of monomers represented by the following formulas, and are resins having repeating units derived from each monomer. The content, molecular weight, and degree of dispersion of each repeating unit are shown in Table 2.

[0427] [Chemical Formula 11]

[0428]

[0429] [Table 2]

[0430]

[0431] B-1: The photocatalysts shown below

[0432] [Chemical Formula 12]

[0433]

[0434] C-1: Acid diffusion control agent shown below

[0435] [Chemical Formula 13]

[0436]

[0437] F-1: Propylene glycol monomethyl ether acetate (PGMEA)

[0438] F-2: Propylene glycol monomethyl ether (PGME)

[0439] F-3: γ-beautyllactone

[0440] F-4: 2-heptanone

[0441] [Preparation of Treatment Solution]

[0442] The treatment solutions of the examples and comparative examples were prepared by mixing the components and contents as shown in the table below.

[0443] The content of metal X was adjusted by passing the treatment solution prepared in the filter through the solution or by adding metal X until a predetermined content was reached. In addition, the water content in each treatment solution was adjusted to be 20 to 1000 mass ppm relative to the total mass of each treatment solution. The content of various components was calculated from the input amount or measured using the above-described method for measuring the content of various components.

[0444] In addition, for each treatment solution, the content of the organic solvent corresponds to the remainder other than the components listed in the table below and water.

[0445] [Aliphatic hydrocarbons]

[0446] · Undecain

[0447] [Ester-based solvents]

[0448] · Butyl acetate

[0449] [Aromatic Hydrocarbons]

[0450] ·C1: 1-ethyl-3,5-dimethyl-benzene (C 10 H 14 )

[0451] ·C2: 1,2,3,5-tetramethyl-benzene (C 10 H 14 )

[0452] ·C3: (1-methylbutyl)-benzene(C 11 H 16 )

[0453] ·C4: 1,2,3,4-tetrahydro-naphthalene (C 10 H 12 )

[0454] In Table 3 below, each entry indicates the following.

[0455] The column “content (a)” of “organic solvent” indicates the mass of aliphatic hydrocarbons when the total mass of the organic solvent is set to 100.

[0456] The column “content (b)” of “organic solvent” indicates the mass of the ester-based solvent when the total mass of the organic solvent is set to 100.

[0457] Therefore, for example, treatment solution 1 has a mass ratio of aliphatic hydrocarbon to ester solvent of 10:90.

[0458] The "total" column for "aromatic hydrocarbons" indicates the total content of aromatic hydrocarbons C1 to C4 relative to the total mass of the treatment solution.

[0459] The "C1" to "C4" columns of "aromatic hydrocarbons" indicate the respective content (mass ppm) of aromatic hydrocarbons C1 to C4 relative to the total mass of the treatment solution.

[0460] The "total" column of "Metal X" indicates the total content (mass ppt) of Fe, Ni, and Al relative to the total mass of the treatment solution.

[0461] The columns "Fe", "Ni", and "Al" in "Metal X" represent the respective contents (mass ppt) of Fe, Ni, and Al relative to the total mass of the treatment solution.

[0462] The column "(c) / (e)" represents the mass ratio of the content of aromatic hydrocarbons (total content of C1~C4 aromatic hydrocarbons) to the content of metal X (total content of Fe, Ni, and Al) (content of aromatic hydrocarbons / content of metal X (total content of Fe, Ni, and Al)). Also, "E+n" is "×10 n Represents ", and "En" is "×10 -n It represents ". n represents an integer greater than or equal to 0. Specifically, "1.2E+06" is "1.2×10 6 It represents ". Also, regarding the above "E+n" and the above "En", the same meaning applies to other columns as well.

[0463] [Table 3]

[0464]

[0465] [Example 1]

[0466] Test 1

[0467] (Test 1-1)

[0468] A composition AL-412 (manufactured by Brewer Science) for forming a sublayer was applied to a 12-inch silicon wafer and baked at 205°C for 60 seconds to form a sublayer with a thickness of 20 nm. On top of this, the composition 1 prepared above was applied and baked (PB) at 90°C for 60 seconds to form a resist film with a thickness of 35 nm. Thus, a silicon wafer having a resist film was fabricated. In addition, the above operation was repeated twice to fabricate two silicon wafers having a resist film.

[0469] The resist film on a silicon wafer having one obtained resist film was brought into contact with processing solution 1 to remove the resist film, and the number of defects on the silicon wafer from which the resist film was removed was measured using UVision 5 (manufactured by AMAT). The number of defects was 100 per wafer.

[0470] For another silicon wafer having a resist film, pattern irradiation was performed using an EUV exposure device (ASML NXE-3400, NA0.33, Quadrupole, outer sigma 0.68, inner sigma 0.36). Additionally, as a reticle, a photomask with a line size of 20 nm and a line-to-space ratio of 1:1 was used. Subsequently, after baking (PEB) at 100°C for 60 seconds, the wafer was developed by paddle-feeding with processing solution 1 for 30 seconds, and the wafer was rotated at a speed of 4000 rpm for 30 seconds to obtain a line-and-space pattern with a pitch of 40 nm.

[0471] The LWR was measured from the obtained pattern and was 3.0 nm.

[0472] (Test 1-2)

[0473] Next, the same operation as above was repeated once more using resist composition 1. Specifically, composition AL-412 (manufactured by Brewer Science) for forming a sublayer was applied onto a 12-inch silicon wafer and baked at 205°C for 60 seconds to form a sublayer with a thickness of 20 nm. On top of this, composition 1 prepared above was applied and baked (PB) at 90°C for 60 seconds to form a resist film with a thickness of 35 nm. Thus, a silicon wafer having a resist film was produced. In addition, the above operation was repeated twice to produce two silicon wafers having a resist film.

[0474] The resist film on a silicon wafer having one obtained resist film was brought into contact with processing solution 1 to remove the resist film, and the number of defects on the silicon wafer from which the resist film was removed was measured using UVision 5 (manufactured by AMAT). The number of defects was 105 per wafer.

[0475] For another silicon wafer having a resist film, pattern irradiation was performed using an EUV exposure device (ASML EUV scanner NXE3300 (NA0.33), Quadrupole, outer sigma 0.68, inner sigma 0.36). Additionally, as a reticle, a photomask with a line size of 20 nm and a line:space ratio of 1:1 was used. Afterward, the wafer was baked (PEB) at 100°C for 60 seconds, then developed by paddle-drying with processing solution 1 for 30 seconds, and the wafer was rotated at a speed of 4000 rpm for 30 seconds to obtain a line and space pattern with a pitch of 40 nm.

[0476] The LWR was measured from the obtained pattern and was 3.1 nm.

[0477] In the above results, the number of defects was measured twice after the operation of removing the resist film formed using composition 1 with processing solution 1, but the number of defects in the first attempt was 100 / wafer and the number of defects in the second attempt was 105 / wafer, and the results of both were almost identical, and the ratio of the number of defects (number of defects in the second attempt / number of defects in the first attempt) was 1.05. Also, the result of LWR when the first pattern formation was performed was 3.0 nm, and the result of LWR when the second pattern formation was performed was 3.1 nm, and the results of both were almost identical, and the difference in LWR was 0.1 nm.

[0478] Test 2

[0479] The evaluation was performed in the same procedure as in <Test 1>, except that composition 2 was used instead of composition 1 used in (Test 1-2) of the above <Test 1>.

[0480] The number of defects after removing the resist film formed using composition 1 with processing solution 1 was 100 / wafer, and the number of defects after removing the resist film formed using composition 2 with processing solution 1 was 120 / wafer, and the ratio of the number of defects (number of defects in the second attempt / number of defects in the first attempt) was 1.20, which was larger compared to the case of <Test 1> above.

[0481] Also, when the first pattern was formed using composition 1, the result of the LWR was 3.0 nm, and when the second pattern was formed using composition 2, the result of the LWR was 3.6 nm, and the difference in LWR was 0.6 nm, which was large compared to the case of <Test 1> above.

[0482] From the results of the above <Test 1> and <Test 2>, it was confirmed that when the ratio of the number of defects is small, the difference in LWR is small, and when the ratio of the number of defects is large, the difference in LWR is large. From these results, it was demonstrated that the number of defects is closely related to the evaluation result of LWR.

[0483] Based on the above results, for example, the ratio of the number of defects is set to an acceptable range of 0.9 to 1.1, and if a test of another photosensitive composition is performed instead of the composition 1 used in <Test 1> (Test 1-2) above, and the ratio of the number of defects is within the above acceptable range, it can be determined that the LWR result also shows an LWR result of the same degree as that of resist composition 1.

[0484] [Example 2]

[0485] The experiment was conducted in the same procedure as in Example 1, except that treatment solution 2 was used instead of treatment solution 1. The results are shown in Table 4, and it was demonstrated that, as in Example 1, the number of defects is closely related to the evaluation results of LWR.

[0486] [Example 3]

[0487] The experiment was conducted in the same procedure as in Example 1, except that treatment solution 5 was used instead of treatment solution 1. The results are shown in Table 4, and it was demonstrated that, as in Example 1, the number of defects is closely related to the evaluation results of LWR.

[0488] [Example 4]

[0489] The experiment was conducted in the same procedure as in Example 1, except that treatment solution 6 was used instead of treatment solution 1. The results are shown in Table 4, and it was demonstrated that, as in Example 1, the number of defects is closely related to the evaluation results of LWR.

[0490] [Comparative Example 1]

[0491] As a result of conducting an experiment in the same procedure as <Test 2> of [Example 1] using treatment solution 3 instead of treatment solution 1, as shown in Table 4, the number of defects after removing the resist film formed using composition 2 with treatment solution 3 was 105 / wafer, and the result of the LWR when the second pattern formation using composition 2 was performed was 4.0 nm.

[0492] As shown in Table 4, in this Comparative Example 1, even though the ratio of the number of defects (number of defects in the second attempt / number of defects in the first attempt) is close to 1.05, the difference between the LWR when the first pattern formation was performed using Composition 1 and the LWR when the second pattern formation was performed using Composition 2 is large at 1.0 nm, and there is no correlation between the number of defects and the difference in LWR.

[0493] From these results, it was confirmed that the photosensitive composition cannot be tested if a specific treatment solution is not used.

[0494] [Comparative Example 2]

[0495] As a result of conducting an experiment in the same procedure as <Test 2> of [Example 1] using treatment solution 4 instead of treatment solution 1, as shown in Table 4, the number of defects after removing the resist film formed using composition 2 with treatment solution 3 was 97 / wafer, and the result of the LWR when the second pattern formation using composition 2 was performed was 4.2 nm.

[0496] As shown in Table 4, in this Comparative Example 2, although the ratio of the number of defects (number of defects in the second attempt / number of defects in the first attempt) is close to 0.97, the difference between the LWR when the first pattern formation was performed using Composition 1 and the LWR when the second pattern formation was performed using Composition 2 is large at 1.2 nm, and there is no correlation between the number of defects and the difference in LWR.

[0497] From these results, it was confirmed that the photosensitive composition cannot be tested if a specific treatment solution is not used.

[0498] In Table 4, the "Correlation" column is marked as "Yes" if there is a correlation between the number of defects and the difference in LWR (cases with correlation), and "No" if there is no correlation.

[0499] [Table 4]

[0500]

[0501] As shown in Table 4 above, it was confirmed that the desired effect is obtained in the testing method of the present invention.

[0502] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used, except that the mass ratio of undecane and butyl acetate was 5:95, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0503] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used, except that the mass ratio of undecane and butyl acetate was 15:85, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0504] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used, except that the mass ratio of undecane and butyl acetate was 40:60, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0505] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used, except that the mass ratio of undecane and butyl acetate was 60:40, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0506] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used except that undecane was replaced with decane, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0507] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used except that undecane was replaced with dodecane, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0508] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used, except that butyl acetate was replaced with isoamyl acetate, it was confirmed that the number of defects was closely related to the LWR evaluation results, just as in Example 1.

[0509] In addition, in Example 1, even when a treatment solution with the same composition as Treatment Solution 1 was used, except that butyl acetate was replaced with isoamyl formate, it was confirmed that the number of defects was closely related to the LWR evaluation results, just as in Example 1.

[0510] In addition, in Example 2, even when a treatment solution with the same composition as Treatment Solution 2 was used except that undecane was replaced with decane, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 2.

[0511] In addition, in Comparative Example 1, even when a treatment solution with the same composition as Treatment Solution 3 was used except that Undecane was replaced with Decane, it was confirmed that the number of defects was not related to the evaluation results of LWR, just as in Comparative Example 1.

[0512] In addition, in Comparative Example 2, even when a treatment solution with the same composition as Treatment Solution 4 was used except that Undecane was replaced with Decane, it was confirmed that the number of defects was not related to the LWR evaluation results, just as in Comparative Example 2.

[0513] In addition, in Example 2, even when a treatment solution with the same composition as Treatment Solution 2 was used except that undecane was replaced with dodecane, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 2.

[0514] In addition, in Comparative Example 1, even when a treatment solution with the same composition as Treatment Solution 3 was used except that undecane was replaced with dodecane, it was confirmed that the number of defects was not related to the evaluation results of LWR, just as in Comparative Example 1.

[0515] In addition, in Comparative Example 2, even when a treatment solution with the same composition as Treatment Solution 4 was used except that undecane was replaced with dodecane, it was confirmed that the number of defects was not related to the evaluation results of LWR, just as in Comparative Example 2.

[0516] In addition, in Example 2, even when a treatment solution with the same composition as Treatment Solution 2 was used, except that butyl acetate was replaced with amyl acetate, it was confirmed that the number of defects was closely related to the LWR evaluation results, just as in Example 2.

[0517] In addition, in Comparative Example 1, even when a treatment solution with the same composition as Treatment Solution 3 was used except that butyl acetate was replaced with amyl acetate, it was confirmed that the number of defects was not related to the LWR evaluation results, just as in Comparative Example 1.

[0518] In addition, in Comparative Example 2, even when a treatment solution with the same composition as Treatment Solution 4 was used except that butyl acetate was replaced with amyl acetate, it was confirmed that the number of defects was not related to the LWR evaluation results, just as in Comparative Example 2.

[0519] In addition, in Example 2, even when a treatment solution with the same composition as Treatment Solution 2 was used, except that butyl acetate was replaced with isoamyl formate, it was confirmed that the number of defects was closely related to the LWR evaluation results, just as in Example 2.

[0520] In addition, in Comparative Example 1, even when a treatment solution with the same composition as Treatment Solution 3 was used, except that butyl acetate was replaced with isoamyl formate, it was confirmed that the number of defects was not related to the LWR evaluation results, just as in Comparative Example 1.

[0521] In addition, in Comparative Example 2, even when a treatment solution with the same composition as Treatment Solution 4 was used except that butyl acetate was replaced with isoamyl formate, it was confirmed that the number of defects was not related to the LWR evaluation results, just as in Comparative Example 2.

[0522] Also, in Example 1, the mass ratio of the aromatic hydrocarbon content to the metal X content is 5.0 × 10 7 It was confirmed that even when a treatment solution with the same composition as treatment solution 1 was used, except for the fact that the number of defects was closely related to the evaluation result of LWR, just as in Example 1.

[0523] In Example 1, even when a composition with the same composition as Composition 1 was used, except that acid-degradable resin A-3 (see below) was used instead of acid-degradable resin A-1, it was confirmed that the number of defects was closely related to the LWR evaluation results, just as in Example 1.

[0524] Table 5 below shows the content, molecular weight, and dispersion of each repeating unit of acid-degradable resin A-3, and the solubility index (R) and solubility index difference (ΔR) of the monomer having acid-degradable groups, respectively.

[0525] [Chemical Formula 14]

[0526]

[0527] [Table 5]

[0528]

[0529] In Example 1, even when a composition with the same composition as Composition 1 was used, except that acid-degradable resin A-1 and acid-degradable resin A-3 were used in a mass ratio of 7:3 instead of acid-degradable resin A-1, it was confirmed that the number of defects was closely related to the LWR evaluation results, just as in Example 1.

[0530] In Example 1, even when a composition with the same composition as Composition 1 was used, except that photogenerative agent B-2 (see below) was used instead of photogenerative agent B-1, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1.

[0531] [Chemical Formula 15]

[0532]

[0533] In Example 1, even when a composition with the same composition as Composition 1 was used, except that photogenerator B-1 and photogenerator B-2 were used in a mass ratio of 1:1 instead of photogenerator B-1, it was confirmed that the number of defects was closely related to the evaluation results of LWR, just as in Example 1. Explanation of the symbols

[0534] S10, S12, S14, S16, S20, S21, S22, S24 steps S30, S31, S32, S34, S40, S22, S24 steps S40, S42, S44 steps

Claims

Claim 1 The method comprises: a process 1 for acquiring reference data by using a reference photosensitive composition comprising an acid-degradable resin having a group that decomposes by the action of an acid to generate a polar group, and a photogenerator, wherein a resist film is formed on a substrate 1 using a reference photosensitive composition comprising a photodegradable resin having a group that decomposes by the action of an acid and a photogenerator, wherein the resist film on the substrate 1 is removed using a treatment solution, and the number of defects on the substrate 1 after the resist film on the substrate 1 has been removed is measured; a process 2 for acquiring measurement data by using a measurement photosensitive composition comprising a component of the same type as the component included in the reference photosensitive composition, wherein the resist film on the substrate 2 is removed using a treatment solution, and the number of defects on the substrate 2 after the resist film on the substrate 2 has been removed is measured; and a process 3 for determining whether the reference data and the measurement data are within an acceptable range, wherein the treatment solution comprises an aromatic hydrocarbon, an organic solvent, and a metal X, wherein the organic solvent does not include the aromatic hydrocarbon and also includes an aliphatic hydrocarbon Including, wherein the metal X is at least one metal selected from the group consisting of Al, Fe, and Ni, and the mass ratio of the content of the aromatic hydrocarbon to the content of the metal X is 5.0 × 10 4 ~2.0×10 10 Phosphorus, method for testing a photosensitive composition. Claim 2 A method for verifying a photosensitive composition according to claim 1, wherein in process 3, if the measurement data falls outside the allowable range, the component adjustment of the photosensitive composition for measurement is performed. Claim 3 A method for verifying a photosensitive composition according to claim 1 or claim 2, wherein in process 1 and process 2, the resist film on substrate 1 and the resist film on substrate 2 are each formed by performing pattern exposure on the resist film after forming the resist film, and the exposed resist film is a photosensitive composition. Claim 4 A method for verifying a photosensitive composition according to claim 3, wherein the pattern exposure in process 1 and process 2 utilizes any one of KrF excimer laser light, ArF excimer laser light, electron beam, and extreme ultraviolet light. Claim 5 A method for verifying a photosensitive composition according to claim 1 or claim 2, wherein the number of defects on substrate 1 from which the resist film on substrate 1 has been removed and the number of defects on substrate 2 from which the resist film on substrate 2 has been removed are each measured using a defect inspection device. Claim 6 A method for testing a photosensitive composition according to claim 1 or claim 2, wherein the acid-degradable resin comprises repeating units having phenolic hydroxyl groups. Claim 7 A method for testing a photosensitive composition according to claim 1 or claim 2, wherein the aliphatic hydrocarbon is undecayne and the organic solvent further comprises butyl acetate. Claim 8 A method for testing a photosensitive composition according to claim 7, wherein the ratio of the content of butyl acetate to the content of undecane is 65 / 35 to 99 / 1. Claim 9 A method for testing a photosensitive composition according to claim 8, wherein the ratio of the content of butyl acetate to the content of undecane is 90 / 10. Claim 10 In claim 1 or claim 2, the acid-degradable resin has repeating units derived from monomers having groups that decompose by the action of acid to generate polar groups, and all monomers have a solubility index (R) based on the Hansen solubility parameter for the treatment solution represented by formula (1) of 2.0 to 5.0 (MPa). 1 / 2 And, furthermore, at least one of the above monomers has a solubility index difference (△R) before and after oxy- 1 / 2 Method for verifying a photosensitive composition, as described above. Formula (1) R=(4(δd1-δd2) 2 +(δp1-δp2) 2 +(δh1-δh2) 2 ) 1 / 2 δd1 represents the dispersion term in the Hansen solubility parameter of the monomer. δp1 represents the polarity term in the Hansen solubility parameter of the monomer. δh1 represents the hydrogen bonding term in the Hansen solubility parameter of the monomer. δd2 represents the dispersion term in the Hansen solubility parameter of the treatment solution. δp2 represents the polarity term in the Hansen solubility parameter of the treatment solution. δh2 represents the hydrogen bonding term in the Hansen solubility parameter of the treatment solution. Claim 11 In claim 1 or claim 2, in the reference data, the number of defects on the description 1 is 0.0001 to 10 defects / cm 2 Phosphorus, method for testing a photosensitive composition. Claim 12 A method for testing a photosensitive composition according to claim 1 or claim 2, wherein the content of the aromatic hydrocarbon is 1 mass% or less with respect to the total mass of the treatment solution. Claim 13 A method for manufacturing a photosensitive composition comprising a method for testing the photosensitive composition described in claim 1 or claim 2. Claim 14 A method for testing a photosensitive composition according to claim 1 or claim 2, wherein the description 1 and the description 2 are each semiconductor substrates. Claim 15 A method for testing a photosensitive composition according to claim 1 or claim 2, wherein the substrate 1 and the substrate 2 are each silicon substrates.

Citation Information

Patent Citations

  • A photomask of testing for procesing margine and testing method

    KR100172801B1

  • Method of lithography

    KR1020010104236A

  • Resist quality control method and method for obtaining resist quality prediction model

    KR1020190049517A

  • Photoresist stripping composition and method

    KR1020190133115A

  • Treatment liquid and pattern forming method

    US20180101100A1