Resin composition, semiconductor device, and method of manufacturing a semiconductor device
A resin composition with modified polyphenylene ether and a butadiene elastomer ensures uniform film formation and prevents warping, addressing the challenges of non-uniformity and high-frequency requirements in semiconductor devices.
Patent Information
- Application Number
- KR1020247010951
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-04
- Filing Date
- 2022-09-15
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-09-15
AI Technical Summary
Existing resin compositions used in Wafer Level Chip technologies fail to address the formation of a uniform film on semiconductor devices, and the semiconductor substrate may warp during the curing process, leading to non-uniform thickness and high-frequency characteristics are not adequately met.
A resin composition comprising a modified polyphenylene ether resin with unsaturated double bonds and an elastomer with a butadiene backbone, along with a solvent, is applied using a spin coater, ensuring uniform film formation and minimizing substrate warping.
The resin composition achieves good high-frequency characteristics with minimal thickness variation and prevents substrate warping, suitable for semiconductor devices in high-frequency applications.
Smart Images

Figure 112024036093012-PCT00038_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a resin composition, a semiconductor device using the same, and a method for manufacturing a semiconductor device. Background Technology
[0002] As electronic devices become smaller, lighter, and more functional, there is a growing demand for semiconductor packages mounted on these devices to also be miniaturized, lightweight, and mount at high density on the mounting substrate. Under these circumstances, a semiconductor packaging technology called Wafer Level Chip Size Package (also known as "WL-CSP") has been proposed. A Wafer Level Chip Size Package is a semiconductor package that does not utilize internal wiring via bonding wires, leaving a portion of the semiconductor substrate (silicon wafer) exposed, and is approximately the same size as the semiconductor substrate.
[0003] For example, patent documents 1 and 2 disclose a WL-CSP. The WL-CSP has a multilayer structure such as an electrode, an insulating layer, a redistribution layer, and a sealing resin layer on a semiconductor substrate (silicon wafer), and external terminals such as a solder pump. Prior art literature
[0004] Japanese Patent Publication No. 2017-92152 Japanese Patent Publication No. 2010-192938 The problem to be solved
[0005] With the ultra-high speed of information transmission and the increase in the volume of information, high-frequency characteristics are required for electronic components, and high-frequency characteristics are also required for WL-CSPs mounted on electronic components. For example, excellent electrical characteristics (low dielectric constant (ε) and low dielectric loss tangent (tanδ)) are required in the high-frequency range, specifically in the frequency range from 1 GHz to 10 GHz.
[0006] In WL-CSP, a resin composition is applied onto a semiconductor substrate (silicon wafer) using a rotary spin coater to form an interlayer insulating film.
[0007] However, depending on the resin material, when a resin composition is applied to a semiconductor substrate using a spin coater, a uniform film cannot be formed on the semiconductor substrate, or warping may occur on the semiconductor substrate due to shrinkage during the curing of the resin composition after application.
[0008] Accordingly, the present invention aims to provide a resin composition for a wafer-level chip-size package type semiconductor device that has good high-frequency characteristics, a small variation in thickness even when applied to a semiconductor substrate using a spin coater, and a method for manufacturing a semiconductor device, a semiconductor device using the same, and a method for manufacturing a semiconductor device. means of solving the problem
[0009] The means for solving the above problem are as follows, and the present invention includes the following embodiments.
[0010] [1] (A) Modified polyphenylene ether resin having unsaturated double bonds at the ends, and
[0011] (B) A resin composition for a wafer-level chip-size package type semiconductor device comprising an elastomer having a butadiene backbone.
[0012] [2] The modified polyphenylene ether resin having an unsaturated double bond at the (A) end is the following formula (1):
[0013]
[0014] [In Equation (1), X represents an unsubstituted or substituted aromatic hydrocarbon group of p value,
[0015] Y is, as shown in Equation (2):
[0016]
[0017] [Equation (2), R 1 ~R 4Each represents independently a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, or an alkenylcarbonyl group.
[0018] Represents unsubstituted or substituted phenolic repeating units, and
[0019] Z represents a functional group containing a carbon-carbon double bond at the terminal, a vinyl group, a vinylene group, the following formula (3):
[0020]
[0021] [Equation (3), R 5 represents a hydrogen atom or an alkyl group.
[0022] (Meta)acryloyl group represented as, or the following formula (4):
[0023]
[0024] [Equation (4), R 6 ~R 8 Each represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, independently.
[0025] It represents a styrene group appearing as, and
[0026] m represents an integer from 1 to 100, and
[0027] n represents an integer of 0 or 1 to 6, and
[0028] p represents an integer from 1 to 4.
[0029] It is a resin composition described in [1] above, comprising a modified polyphenylene ether resin that appears as such.
[0030] [3] The above (B) elastomer having a butadiene backbone is a resin composition described in [1] or [2], comprising at least one selected from the group consisting of styrene / butadiene / styrene copolymer, styrene / butadiene / butylene / styrene copolymer, butadiene polymer, styrene / butadiene copolymer, and acrylonitrile / butadiene copolymer.
[0031] [4] The modified polyphenylene ether resin having an unsaturated double bond at the (A) end is the following formula (5):
[0032]
[0033] [Equation (5), R 5 represents a hydrogen atom or an alkyl group,
[0034] X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and
[0035] Y represents an unsubstituted or substituted phenolic repeating unit represented by the above formula (2), and
[0036] m represents an integer from 1 to 100, and
[0037] n represents an integer of 0 or 1 to 6, and
[0038] p represents an integer from 1 to 4.
[0039] Modified polyphenylene ether resin, represented by the following formula (6):
[0040]
[0041] [Equation (6), R 6 ~R 8 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, and
[0042] X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and
[0043] Y represents an unsubstituted or substituted phenolic repeating unit represented by the above formula (2), and
[0044] m represents an integer from 1 to 100, and
[0045] n represents an integer of 0 or 1 to 6, and
[0046] p represents an integer from 1 to 4.
[0047] It is a resin composition described in any one of [1] to [3], comprising at least one selected from the group consisting of modified polyphenylene ether resins.
[0048] [5] The above (B) elastomer having a butadiene backbone is formula (7):
[0049]
[0050] A styrene / butadiene / styrene block copolymer represented by [wherein in Equation (7), q and r represent integers from 0 to 1, at least one of which is not 0, s represents an integer from 1 to 1200, and t represents an integer from 1 to 1000], and the following Equation (8):
[0051]
[0052] [In Equation (8), u represents an integer from 1 to 1200, and v represents an integer from 1 to 1000.]
[0053] It is a resin composition described in any one of [1] to [4], comprising at least one selected from the group consisting of acrylonitrile / butadiene copolymers.
[0054] [6] The above (A) modified polyphenylene ether resin having an unsaturated double bond at the end is a modified polyphenylene ether resin represented by formula (6), and the above (B) elastomer having a butadiene backbone is a styrene / butadiene / styrene copolymer represented by formula (7), which is a resin composition described in any one of [1] to [5].
[0055] [7] (C) A resin composition described in any of [1] to [6] above, which further comprises a solvent.
[0056] [8] It is a resin composition described in [7] above, with a first viscosity of 300 mPa·s to 4000 mPa·s at 25°C and 10 rpm using a rotary viscometer.
[0057] [9] A second viscosity at 25°C and 1 rpm is within the range of 500 mPa·s to 4200 mPa·s, and the thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, is 0.8 to 1.2. This is the resin composition described in [8] above.
[0058]
[10] A resin composition described in any of [1] to [9], wherein the mass ratio of the above component (A) and the above component (B) is within the range of 10:90 to 80:20.
[0059]
[11] A resin composition described in any of [7] to
[10] , wherein the total amount of the above components (A) and (B) and the mass ratio with the above component (C) is within the range of 5:95 to 80:20.
[0060]
[12] A semiconductor device of wafer level chip size package type, comprising a semiconductor substrate, an electrode disposed on the semiconductor substrate, a wiring electrically connected to the electrode, an external terminal electrically connected to the electrode via the wiring, and an interlayer insulating film that seals the side of the semiconductor substrate where the electrode and the wiring are disposed, wherein the interlayer insulating film is disposed in contact with the wiring and is formed using a resin composition described in any one of [1] to
[11] .
[0061]
[13] The semiconductor device described in
[12] has at least two layers, including a first interlayer insulating film that seals the side of the semiconductor substrate of the wiring and a second interlayer insulating film that seals the opposite side of the semiconductor substrate of the wiring.
[0062]
[14] The semiconductor device described in
[12] or
[13] has a thickness of one of the interlayer insulating film, the first interlayer insulating film, or the second interlayer insulating film within the range of 3 μm or more and 20 μm or less.
[0063]
[15] The following components (A)~(C):
[0064] (A) Modified polyphenylene ether resin having unsaturated double bonds at the ends,
[0065] (B) an elastomer having a butadiene backbone, and
[0066] (C) preparing a liquid resin composition containing a solvent, and
[0067] Dropping the above resin composition onto a semiconductor substrate and rotating the semiconductor substrate around a vertical axis using a spin coater to apply the liquid resin composition to the semiconductor substrate, and
[0068] A method for manufacturing a wafer-level chip-size package type semiconductor device, comprising curing the above-mentioned liquid resin composition to form an interlayer insulating film.
[0069]
[16] The above spin coater has a rotation speed of 1000 rpm to 3000 rpm and a rotation time of 5 seconds to 30 seconds. This is a method for manufacturing a semiconductor device as described in
[15] .
[0070]
[17] The above liquid resin composition is a method for manufacturing a semiconductor device as described in
[15] or
[16] , wherein the first viscosity at 25°C and 10 rpm is 300 mPa·s to 4000 mPa·s using a rotary viscometer.
[0071]
[18] The above liquid composition is a method for manufacturing a semiconductor device as described in
[17] , wherein the second viscosity at 25°C and 1 rpm is 500 mPa·s to 4200 mPa·s using a rotary viscometer, and the thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, is 0.8 to 1.2.
[0072]
[19] The modified polyphenylene ether resin having an unsaturated double bond at the (A) end comprises the polyphenylene ether resin represented by the formula (1), and
[0073] The above (B) is a method for manufacturing a semiconductor device as described in any one of
[15] to
[18] , wherein the elastomer having a butadiene backbone comprises at least one selected from the group consisting of styrene / butadiene / styrene copolymer, styrene / butadiene / butylene / styrene copolymer, butadiene polymer, styrene / butadiene copolymer, and acrylonitrile / butadiene copolymer. Effects of the invention
[0074] According to the present invention, a resin composition for a wafer-level chip-size package type semiconductor device can be formed that has good high-frequency characteristics, has a small variation in thickness even when applied to a semiconductor substrate using a spin coater, and is unlikely to cause warping of the semiconductor substrate, a semiconductor device using the same, and a method for manufacturing a semiconductor device can be provided. Brief explanation of the drawing
[0075] FIG. 1 is a schematic cross-sectional view showing the schematic configuration of a part of a WL-CSP type semiconductor device. Specific details for implementing the invention
[0076] Hereinafter, the present disclosure describes a resin composition for a wafer-level chip-size package type semiconductor device, a semiconductor device using the same, and a method for manufacturing a semiconductor device based on embodiments related to the present disclosure. However, the embodiments described below are examples for embodying the technical concept of the present invention, and the present invention is not limited to the following resin composition, the semiconductor device using the same, and the method for manufacturing a semiconductor device.
[0077] The resin composition related to the first embodiment of the present invention comprises a specific modified polyphenylene ether (also referred to as "Component (A)") and (B) an elastomer having a butadiene backbone (also referred to as "Component (B)"). Since the resin composition comprises the modified polyphenylene ether of Component (A), it is preferable that the dielectric constant (ε) of the coating film formed by curing the resin composition constituting the interlayer insulating film be 3.0 or less, more preferable that it be 2.9 or less, more preferable that it be 2.8 or less, and particularly preferable that it be 2.7 or less. The dielectric constant (ε) of the coating film formed by curing the resin composition constituting the interlayer insulating film should be 1.0 or more, and is preferably 1.5 or more. In addition, it is preferable that the dielectric loss tangent (tanδ) of the coating film made of the resin composition constituting the interlayer insulating film is 0.015 or less, more preferable that it is 0.014 or less, and more preferable that it is 0.013 or less. It is preferable that the dielectric loss tangent (tanδ) of the coating film made of the resin composition constituting the interlayer insulating film is 0.001 or more. If the dielectric constant of the coating film made of the resin composition constituting the interlayer insulating film of a WL-CSP type light-emitting device is 3.0 or less and the dielectric loss tangent (tanδ) is 0.015 or less, it has a low dielectric constant and a low dielectric loss tangent, and the electrical characteristics are good when used in a high-frequency region. For example, a coating film with good electrical characteristics is obtained even when using a semiconductor device in a high-frequency region such as a 5th generation communication system "5G," where high capacity and high-speed communication are expected to progress.
[0078] Since the resin composition includes component (A) and component (B), it shrinks uniformly when the resin composition applied to the semiconductor substrate is cured, making it difficult for the semiconductor substrate to warp. For this reason, the resin composition including component (A) and component (B) is suitable for forming an interlayer insulating film of a WL-CSP type semiconductor device.
[0079] The resin composition preferably further comprises, as necessary, a solvent (C) (also referred to as “Component (C)”) together with Components (A) and (B). The resin composition comprising Components (C) together with Components (A) and (B) has good thixotropic properties. The resin composition comprising Components (C) together with Components (A) and (B) can form a film of approximately uniform thickness with minimal variation in thickness, even when applied to a semiconductor substrate, for example, using a spin coater.
[0080] A resin composition comprising component (A), component (B), and component (C) preferably has a first viscosity at 25°C and 10 rpm measured by a rotational viscometer within the range of 300 mPa·s to 4000 mPa·s. If the first viscosity of the resin composition is within the range of 300 mPa·s to 4000 mPa·s, the thickness variation is small, and a film of approximately uniform thickness can be formed even when applied to a semiconductor substrate, for example, using a spin coater, thereby suppressing warping of the semiconductor substrate during curing. It is more preferable that the resin composition has a first viscosity of 400 mPa·s to 4000 mPa·s, and even more preferable that it is 500 mPa·s to 2000 mPa·s. In this specification, the rotational viscometer can be measured using, for example, a TVE type viscometer (cone rotor: 1° 34'×R24, manufactured by Donggi Sangyo Co., Ltd.).
[0081] It is preferable that the resin composition comprising component (A), component (B), and component (C) has a second viscosity at 25°C and 1 rpm measured by a rotational viscometer within the range of 500 mPa·s to 4200 mPa·s. If the second viscosity of the resin composition is within the range of 500 mPa·s to 4200 mPa·s, even when applied to a semiconductor substrate using, for example, a spin coater, the variation in thickness is small, and a coating film of approximately uniform thickness can be formed, thereby suppressing warping of the semiconductor substrate during curing. It is more preferable that the resin composition has a second viscosity within the range of 550 mPa·s to 4000 mPa·s, and even more preferable that it is within the range of 550 mPa·s to 3500 mPa·s.
[0082] A resin composition comprising component (A), component (B), and component (C) preferably has a thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, within the range of 0.8 to 1.2 and possesses thixotropic properties similar to those of a Newtonian fluid. Here, a Newtonian fluid refers to a fluid having the property that shear stress is proportional to the shear rate. If the thixotropy index TI, which is the ratio of the second viscosity to the first viscosity of the resin composition, is within the range of 0.8 to 1.2, then, for example, when applied to a semiconductor substrate using a spin coater, the variation in thickness is small, and a coating film of approximately uniform thickness can be formed, thereby suppressing warping of the semiconductor substrate during curing. The resin composition may have a thixotropy index, which is the ratio of the second viscosity to the first viscosity, within the range of 0.90 to 1.10, and may also be within the range of 1.00 to 1.10.
[0083] In the resin composition, the mass ratio of component (A) and component (B) is preferably within the range of 10:90 to 80:20, more preferably within the range of 20:80 to 75:25, and even more preferably within the range of 30:70 to 70:30. When the mass ratio of component (A) and component (B) in the resin composition is within the range of 10:90 to 80:20, a cured product having low dielectric constant and low dielectric loss tangent and good electrical characteristics when used in a high-frequency region is obtained by using the resin composition. In addition, even when the resin composition is applied to a semiconductor substrate using, for example, a spin coater, the variation in thickness is small and a coating film of approximately uniform thickness can be formed, thereby obtaining a cured product that suppresses warping of the semiconductor substrate.
[0084] In the resin composition, the mass ratio of the total amount of component (A) and component (B) to component (C) is preferably within the range of 5:95 to 80:20, more preferably within the range of 10:90 to 70:30, more preferably within the range of 12:88 to 40:60, and particularly preferably within the range of 18:82 to 50:50. If the mass ratio of the total amount of component (A) and component (B) in the resin composition is within the range of 5:95 to 80:20, then, for example, when the resin composition is applied to a semiconductor substrate using a spin coater, the variation in thickness is small and a coating film of approximately uniform thickness can be formed, thereby obtaining a cured product that suppresses warping of the semiconductor substrate.
[0085] Ingredient (A) Modified polyphenylene ether
[0086] Component (A) is preferably a polyphenylene ether resin having a functional group containing a carbon-carbon double bond at its terminal. The modified polyphenylene ether (PPE) resin is also referred to as component (A) or the modified PPE resin of component (A). Examples of functional groups containing a carbon-carbon double bond include terminal vinyl groups, vinylene groups, vinylidene groups, acryloyl groups, or methacryloyl groups. As long as component (A) has a functional group containing a carbon-carbon double bond at its terminal and has polyphenylene ether in its backbone, there are no particular limitations. By including component (A), low dielectric properties can be imparted to the resin composition, and heat resistance and the coefficient of thermal expansion can also be improved. Component (A) is preferably a thermosetting resin. Furthermore, component (A) is particularly preferably a polyphenylene ether resin having a vinyl group at its terminal. Low dielectric properties are obtained by having a vinyl group at the terminal.
[0087] The modified PPE resin of component (A) preferably comprises a PPE resin represented by the following formula (1).
[0088]
[0089] [In Equation (1), X represents an unsubstituted or substituted aromatic hydrocarbon group of p,
[0090] Y is, as shown in Equation (2):
[0091]
[0092] [Equation (2), R 1 ~R 4 Each represents independently a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, or an alkenylcarbonyl group.
[0093] Represents unsubstituted or substituted phenolic repeating units, and
[0094] Z represents a functional group containing a carbon-carbon double bond at the terminal, a vinyl group, a vinylene group, the following formula (3):
[0095]
[0096] [Equation (3), R 5 represents a hydrogen atom or an alkyl group.
[0097] (Meta)acryloyl group, or, the following formula (4):
[0098]
[0099] [Equation (4), R 6 ~R 8 Each represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, independently.
[0100] It represents a styrene group appearing as, and
[0101] m represents an integer from 1 to 100, and
[0102] n represents an integer of 0 or 1 to 6, and
[0103] p represents an integer from 1 to 4.
[0104] The PPE resin of component (A) preferably comprises at least one selected from the group consisting of a modified PPE resin represented by the following formula (5) and a modified PPE resin represented by the following formula (6).
[0105]
[0106] [Equation (5), R 5 represents a hydrogen atom or an alkyl group,
[0107] X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and
[0108] Y represents an unsubstituted or substituted phenolic repeating unit represented by the above formula (2), and
[0109] m represents an integer from 1 to 100, and
[0110] n represents an integer of 0 or 1 to 6, and
[0111] p represents an integer from 1 to 4.
[0112]
[0113] [Equation (6), R 6 ~R 8 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, and
[0114] X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and
[0115] Y represents an unsubstituted or substituted phenolic repeating unit represented by the above formula (2), and
[0116] m represents an integer from 1 to 100, and
[0117] n represents an integer of 0 or 1 to 6, and
[0118] p represents an integer from 1 to 4.
[0119] Generally, a hydrocarbon group of x (where x represents an integer greater than or equal to 1) refers to a group of x that is formed by removing x hydrogen atoms from a carbon atom of a hydrocarbon. X is a p-valued unsubstituted or substituted aromatic hydrocarbon group, and X refers to a group of 1 to 4 that is formed by removing 1 to 4 hydrogen atoms from a carbon atom of an aromatic hydrocarbon, whether substituted or not.
[0120] The term "alkyl group" means a monovalent saturated hydrocarbon group. In the present invention, the alkyl group is preferably a C1-C 10 The alkyl group is, more preferably, a C1-C6 alkyl group, even more preferably a C1-C4 alkyl group, and particularly preferably a C1-C2 alkyl group. Examples of such alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, etc.
[0121] The term "alkenyl group" means a monovalent unsaturated hydrocarbon group having at least one carbon-carbon double bond. In the present invention, the alkenyl group is preferably C2-C 10 It is an alkenyl group, more preferably a C2-C6 alkenyl group, and more preferably a C2-C4 alkenyl group. Examples of such alkenyl groups include an ethenyl group (vinyl group), 1-propenyl group, 2-propenyl group, 1-butenyl group, 2-butenyl group, isobutenyl group, 1-pentenyl group, 1-hexenyl group, etc. The group -CR in the above formula (1). 1 =CR 2 R 3 It is also an alkenyl group.
[0122] The term "alkynyl group" means a monovalent unsaturated hydrocarbon group having at least one carbon-carbon triple bond. In the present invention, the alkynyl group is preferably a C2-C 10 It is an alkynyl group, more preferably a C2-C6 alkynyl group, and even more preferably a C2-C4 alkynyl group. Examples of such alkynyl groups include an ethinyl group, a 1-propynyl group, a 2-propynyl group, a butynyl group, an isobutynyl group, a fentinyl group, a hexinyl group, etc.
[0123] The term "alkenyl carbonyl group" refers to a carbonyl group substituted by the alkenyl group, and examples thereof include an acrylyl group, a methacryloyl group, etc.
[0124] In component (A), in formula (1), (5) or (6), -(Y) m The portion indicated by - corresponds to the main chain of the PPE resin. Preferably, R in the unsubstituted or substituted phenol repeating unit Y. 1 and R 3 This represents a hydrogen atom, and also R 2 and R 4 represents a methyl group. In formula (1), -(Y) mOne end of the part indicated by - is bonded to an aromatic hydrocarbon group X via an oxygen atom, and the other end is bonded to a terminal group (Z) via n methylene groups. In Equation (5), -(Y) m One end of the part indicated by - is bonded to an aromatic hydrocarbon group X via an oxygen atom, and the other end is bonded to a methacryloyl group via n methylene groups. In Equation (6), -(Y) m One end of the portion indicated by - is bonded to an aromatic hydrocarbon group X via an oxygen atom, and the other end is bonded to an alkenyl group -CR via n methylene groups. 6 =CR 7 R 8 The silver may be located at any of the ortho, meta, or para positions with respect to the methylene group. In one embodiment, n in Equation (1), (5), or (6) is 0 or an integer from 1 to 4. In one embodiment, n in Equation (1), (5), or (6) is 0, 1, or 2. In one embodiment, n in Equation (1) is 0 or 1. In another embodiment, R in Equation (6) 6 ~R 8 These are all hydrogen atoms.
[0125] In addition, the number of Y units of the repeating unit of formula (1), (5) or (6) is preferably 1 to 80, more preferably 1 to 30, and even more preferably 1 to 5.
[0126] In component (A), the aromatic hydrocarbon group X of formulas (1), (5), or (6) each has p -(Y) atoms interposed with an oxygen atom. m The part indicated by - is combined. Preferably, p is 2 or 3. More preferably, p is 2. Also, X is preferably of the following formula:
[0127]
[0128] [In the middle of the meal, R 11 ~R 18 [each independently representing a hydrogen atom or a C1-C6 alkyl group] has a structure represented by X. X is more preferably of the following formula:
[0129]
[0130] It has a structure that appears as.
[0131] The main chain end of the modified polyphenylene ether resin of component (A) may be a polyphenylene ether resin having an average of 1.5 to 5 functional groups represented by formulas (1), (5), or (6) per molecule. The terminal functional group is preferably a methacryloyl group and / or an acryloyl group in order to provide even better heat resistance when the resin composition is cured, and is more preferably a methacryloyl group in order to provide even better resin fluidity during heat molding.
[0132] For example, from the perspective of ease of applying the resin composition to a semiconductor substrate using a spin coater, electrical properties such as low dielectric properties and low dielectric loss tangent of the coating film made of the resin composition, and compatibility of other components included in the resin composition, it is also preferable that the number average molecular weight of component (A) be 500 or more and 5000 or less. More preferably, the number average molecular weight of component (A) is 750 or more and 3000 or less, and even more preferably 1000 or more and 2500 or less. If the number average molecular weight (Mn) of component (A) is excessively low, the toughness of the cured product obtained by curing the resin composition may decrease. On the other hand, if the number average molecular weight (Mn) of component (A) is excessively high, the compatibility of component (A) with the solvent of component (C) decreases, and it may become difficult to apply the resin composition to a semiconductor substrate using a spin coater, for example. The number average molecular weight (Mn) of component (A) or component (B) can be measured, for example, from a polystyrene equivalent value by gel permeation chromatography (GPC) measurement. In this specification, the number average molecular weight (Mn) can be measured, for example, by using high-speed liquid chromatography (e.g., LC-2OAD, manufactured by Shimadzu Corporation), a column (e.g., KF-802, manufactured by Showa Denko Co., Ltd.), and a tetrahydrofuran (THF) solution as the solvent.
[0133] The content of component (A) in the resin composition is preferably 5.0 to 40.0 mass% with respect to 100 mass% of the total amount of component (A), component (B), and component (C), more preferably 7.0 to 35.0 mass%, even more preferably 8.0 to 30.0 mass%, and particularly preferably 9.0 to 25.0 mass%. If the content of component (A) in 100 mass% of the total amount of component (A), component (B), and component (C) in the resin composition is 5.0 to 40.0 mass%, a cured product having a low dielectric constant and a low dielectric loss tangent is obtained, and a cured product with good electrical properties suitable for use in a high-frequency region is obtained.
[0134] For component (A), a commercially available product may be used. For the commercially available product of component (A), the modified PPE resin represented by formula (5) may be, for example, NORYL SA9000 (manufactured by SABIC Innovative Plastics), which is a modified PPE resin having 1.5 to 5 terminal methacryloyl groups per molecule represented by formula (3). For the commercially available product of component (A), the modified PPE resin represented by formula (6) may be, for example, OPE 2St 1200 or OPE 2St 2200 (manufactured by Mitsubishi Gas Chemical Co., Ltd.). Component (A) may be prepared by a known method. For example, X-(OH) p (In the formula, X and p have the same meaning as above.) A suitable p having a structure represented by phenol (2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol, etc.) and the following formula
[0135]
[0136] [In the middle of the meal, R 1 ~R 4 Each has the same meaning as above.]
[0137] Component (A) can be prepared by a method comprising oxidizing copolymerizing a suitable monovalent phenol (such as 2,6-dimethylphenol) having a structure as shown by a known method to prepare a polyphenylene ether resin having a hydroxyl group at the terminal end, and modifying the obtained resin by reacting it with a suitable modifying agent, such as chloromethylstyrene.
[0138] Component (B) Elastomer having a butadiene backbone
[0139] The elastomer having a butadiene backbone of component (B) may be a partially hydrogenated elastomer having a butadiene backbone in its molecule. Examples of elastomers having a butadiene backbone include block copolymers that include at least one terminal block of styrene or an analog thereof and at least one intermediate block of a conjugated diene elastomer. The elastomer having a butadiene backbone of component (B) preferably comprises at least one species selected from the group consisting of styrene / butadiene / styrene copolymer (SBS), styrene / butadiene / butylene / styrene copolymer (SBBS), butadiene copolymer (BR), styrene / butadiene copolymer (SBR), and acrylonitrile / butadiene copolymer (NBR). In addition, the elastomer having a butadiene backbone may have a portion modified, and, for example, may be a carboxylated nitrile-butadiene rubber (NBR) in which the terminals are modified to carboxylates.
[0140] A resin composition containing an elastomer having a butadiene backbone of component (B) together with component (A) can shrink more uniformly upon curing, thereby suppressing warping of the semiconductor substrate. In addition, when a solvent of component (C) is used in the resin composition, it is easily soluble in the solvent of component (C), resulting in better thixotropic properties. For example, when applied to a semiconductor substrate using a spin coater, the variation in thickness is smaller, and a film with a more uniform thickness can be formed. In particular, from the perspective of good electrical characteristics when used in a high-frequency region, a styrene-based elastomer having double bonds is preferred. Suitable examples include styrene-based elastomers including styrene / butadiene / styrene copolymer (SBS), styrene / butadiene / butylene / styrene copolymer (SBBS), and styrene / butadiene copolymer. In addition, component (B) may be a reactive elastomer to which functional groups such as amines are imparted. By using a reactive elastomer to which functional groups are imparted, the adhesive strength (peel strength) can be further improved. The weight-average molecular weight of component (B) is preferably 20,000 to 200,000, and more preferably 30,000 to 150,000. The weight-average molecular weight is determined by using a calibration curve based on standard polystyrene by gel permeation chromatography (GPC).
[0141] The elastomer having a butadiene backbone of component (B) preferably comprises at least one selected from the group consisting of a styrene / butadiene / styrene block copolymer represented by the following formula (7) and an acrylonitrile / butadiene copolymer represented by the following formula (8).
[0142]
[0143] [In Equation (7), q and r represent integers from 0 to 1, where at least one of them is not 0, s represents an integer from 1 to 1200, and t represents an integer from 1 to 1000.]
[0144]
[0145] [In Equation (8), u represents an integer from 1 to 1200, and v represents an integer from 1 to 1000.]
[0146] The styrene / butadiene / styrene block copolymer (SBS) represented by formula (7) of component (B) is an unhydrogenated block copolymer. By including the styrene / butadiene / styrene block copolymer in component (B), the resin composition has improved flexibility and solubility in solvents, allowing the resin composition to be coated well onto a semiconductor substrate using a spin coater. In addition, the resin composition can be coated well onto a semiconductor substrate in the same way even if it includes the styrene / butadiene / butylene / styrene copolymer (SBBS), which is a partially hydrogenated elastomer. Meanwhile, it is preferable that the resin composition or component (B) does not include an elastomer that does not have double bonds. Examples of elastomers that do not have double bonds include styrene / ethylene / butylene / styrene block copolymer (SEBS) obtained by fully hydrogenating a styrene / butadiene / styrene block copolymer. In SEBS, the compatibility of component (C) with the solvent is reduced, so the resin composition does not achieve the desired viscosity, and it may become difficult to apply the resin composition to a semiconductor substrate, for example, using a spin coater. Although the details of the mechanism are not clear, it is presumed that styrene / butadiene / styrene block copolymer (SBS) and styrene / butadiene / butylene / styrene copolymer (SBBS) have improved solubility in solvents compared to styrene / ethylene / butylene / styrene block copolymer (SEBS) because the butadiene double bond remains. However, the present invention is not limited to this reasoning.
[0147] In Equation (7), s may represent an integer from 1 to 1200 or an integer from 150 to 900. In Equation (7), t may represent an integer from 1 to 1000 or an integer from 50 to 700.
[0148] In addition, when component (B) includes an acrylonitrile / butadiene copolymer (NBR) represented by formula (8), if the solvent of component (C) is used in the resin composition, the NBR is easily soluble in the solvent of component (C), and the thixotropic properties are improved, and even when applied to a semiconductor substrate using, for example, a spin coater, the variation in thickness is small, and a coating film with a more uniform thickness can be formed.
[0149] The styrene content included in component (B) of the resin composition is preferably within the range of 10 mass% or more and 70 mass% or less with respect to 100 mass% of the resin composition, more preferably within the range of 15 mass% or more and 60 mass% or less, and more preferably within the range of 20 mass% or more and 55 mass% or less. If the styrene content included in component (B) of the resin composition is within the range of 10 mass% or more and 70 mass% or less with respect to 100 mass% of the resin composition, the elasticity of the resin composition during curing is good, and, for example, when applied to a semiconductor substrate, the bending of the semiconductor substrate during curing can be suppressed.
[0150] The styrene content in component (B) of the resin composition can be measured using nuclear magnetic resonance (NMR). Specifically, tetrachloroethane is used as the solvent, and the integral value of the peak in the range of 5.5 ppm to 6.5 ppm corresponding to styrene and the integral value of the peak in the range other than that are obtained, and the styrene content can be calculated from the obtained value.
[0151] The styrene / butadiene ratio (%, mass ratio) of component (B) may be 15 / 85 or higher, 20 / 80 or higher, preferably 70 / 30 or lower, 60 / 40 or lower, or 55 / 45 or lower.
[0152] For example, when the resin composition is applied to a semiconductor substrate using a spin coater, the uniformity of the film thickness of the coating, the suppression of warping of the semiconductor substrate during curing of the resin composition, and the compatibility of the solvent of component (C) are taken into account, the number average molecular weight (Mn) of component (B) is preferably 40,000 or more and 600,000 or less, more preferably 50,000 or more and 150,000 or less, and more preferably 60,000 or more and 120,000 or less. The number average molecular weight (Mn) of component (B) can be measured from the polystyrene equivalent value by gel permeation chromatography (GPC) measurement, for example, in the same way as described above.
[0153] Preferably, the resin composition comprises a modified polyphenylene ether resin represented by Formula (6) in component (A) and a styrene / butadiene / styrene copolymer (SBS) in component (B). Since the resin composition comprises a modified PPE resin represented by Formula (6) in component (A) and SBS in component (B), it shrinks uniformly when the resin composition applied to the semiconductor substrate is cured, making it difficult for the semiconductor substrate to warp. For this reason, the resin composition is suitable for forming an interlayer insulating film of a WL-CSP type semiconductor device.
[0154] The content of component (B) in the resin composition is preferably 5.0 to 40.0 mass% with respect to 100 mass% of the total amount of component (A), component (B), and component (C), more preferably 7.0 to 35.0 mass%, even more preferably 8.0 to 30.0 mass%, and particularly preferably 9.0 to 25.0 mass%. If the content of component (B) in 100 mass% of the total amount of component (A), component (B), and component (C) in the resin composition is 5.0 to 40.0 mass%, a cured product having a low dielectric constant and a low dielectric loss tangent is obtained, and a cured product with good electrical properties suitable for use in a high-frequency region is obtained. In addition, if the content of component (B) in the total amount of component (A), component (B), and component (C) in the resin composition is 5.0 to 40.0 mass%, then when the resin composition is applied to a semiconductor substrate using, for example, a spin coater, the variation in thickness is small and a coating film of approximately uniform thickness can be formed, thereby obtaining a cured product that suppresses warping of the semiconductor substrate.
[0155] For ingredient (B), commercially available products may be used. Examples of commercially available products of ingredient (B) include “TR2827,” “TR2000,” “TR2003,” and “TR2250” manufactured by JSR Corporation; “P1083,” “P1500,” “P5051,” and “MP10” manufactured by Asahi Chemical Co., Ltd.; and “Nipol (trademark) 1072” manufactured by Nippon Zeon Corporation.
[0156] Ingredient (C) Solvent
[0157] It is preferable that the resin composition includes a solvent of component (C). It is preferable that the solvent of component (C) be an organic solvent. It is preferable that the organic solvent allows components (A) and (B) to dissolve or disperse easily, and when the resin composition is applied to a semiconductor substrate, for example using a spin coater, a coating film of approximately uniform thickness with minimal thickness variation can be formed, making it difficult to remain in the coating film, thereby suppressing the degradation of dielectric properties. It is preferable that the organic solvent include at least one selected from the group consisting of aromatic solvents and ketone solvents. It is preferable that the solvent of component (C) be at least one selected from the group consisting of toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, cyclohexanone, cyclohexane, dimethyl carbonate, methylcyclohexanone, and γ-butyrolactone. The solvent of component (C) may be used alone or in combination of two or more types. Toluene and cyclohexanone may be used as the solvent of component (C), and among these, it is preferable to use cyclohexanone from the perspective of toxicity. The resin composition may be used as a varnish by dissolving or dispersing component (A) and component (B) in the solvent of component (C). The varnish formed from the resin composition containing component (A), component (B), and component (C) preferably has the aforementioned first viscosity and second viscosity. In addition, the varnish formed from the resin composition containing component (A), component (B), and component (C) preferably has the aforementioned thixotropy index TI.
[0158] The content of component (C) in the resin composition is preferably within the range of 20 to 90 mass% with respect to 100 mass% of the total amount of component (A), component (B), and component (C), and may be within the range of 30 to 86 mass%, within the range of 40 to 84 mass%, or within the range of 50 to 82 mass%. If the content of component (C) with respect to 100 mass% of the total amount of component (A), component (B), and component (C) is within the range of 20 to 90 mass%, it is easy to dissolve or disperse component (A) and component (B) in component (C), and when the resin composition is applied to a semiconductor substrate using, for example, a spin coater, a coating film of approximately uniform thickness can be formed with a small variation in thickness, making it difficult for it to remain in the coating film, thereby suppressing the degradation of dielectric properties.
[0159] For component (C), a commercially available product may be used. For example, commercially available products of component (C) may include toluene (toluene concentration 100 mass%, manufactured by Daisin Chemical Co., Ltd.), anon (cyclohexanone) (cyclohexanone concentration 90-100 mass%, manufactured by Daisin Chemical Co., Ltd.), etc.
[0160] The resin composition may include component (A) and component (B), may include component (C), may include components other than component (A), component (B), and component (C), or may not include components other than component (A), component (B), and component (C). The resin composition may consist only of component (A), component (B), and component (C).
[0161] The resin composition may include a coupling agent to increase adhesion to the semiconductor substrate. Additionally, the resin composition may include an organic peroxide to increase reactivity. The resin composition may include at least one additive selected from the group consisting of organic peroxides, coupling agents, ion trapping agents, leveling agents, antioxidants, viscosity modifiers, and flame retardants. The coupling agent is a compound having two or more different functional groups in one molecule, one of which is a functional group that chemically bonds with an inorganic material, and the other is a functional group that chemically bonds with an organic material. Examples of coupling agents include at least one selected from the group consisting of silane coupling agents, aluminum coupling agents, and titanium coupling agents, and may be a silane coupling agent. One type of coupling agent may be used, or two or more types may be used in combination. Examples of functional groups possessed by silane coupling agents include alkoxy groups, vinyl groups, epoxy groups, styryl groups, methacrylic groups, acrylic groups, amino groups, isocyanurate groups, ureido groups, mercapto groups, sulfide groups, isocyanate groups, etc.
[0162] The resin composition may include an organic peroxide that initiates a radical polymerization reaction, taking into account the reactivity of component (A) and component (B). Peroxycarbonates, etc., may be used as the organic peroxide. Perbutyl Z (trademark) manufactured by Nichiyu Co., Ltd. may be used as the peroxycarbonate.
[0163] The content of the additive included in the resin composition may be 10.0 mass% or less, 8.0 mass% or less, or 5.0 mass% or less with respect to 100 mass% of the resin composition. The content of the additive included in the resin composition may be 0.10 mass% or more, 0.20 mass% or more, 0.30 mass% or more, or 0.50 mass% or more. The additive may be a commercially available product, and if the additive is a silane coupling agent, for example, 3-methacryloxypropyltrimethoxysilane KBM 503, vinyltrimethoxysilane KBM 1003 (manufactured by Shin-Etsu Silicon Co., Ltd.), or Coatsil MP200 Silane (manufactured by Momentive Performance Materials Japan) may be used.
[0164] In addition, the present resin composition is a non-photosensitive resin composition for a wafer-level chip-size package type semiconductor device. Furthermore, it is preferable that the present resin composition does not contain inorganic fillers such as silica. When forming an interlayer insulating film using a thermosetting insulating resin, a perforation process is performed on the interlayer insulating film by laser irradiation in a subsequent process to form via holes for wiring. At this time, if the interlayer insulating film contains inorganic fillers such as silica, the silica portion cannot be effectively reduced during laser processing, and it may become difficult to effectively copper-plat the via holes thereafter; therefore, it is preferable that the present resin composition does not contain inorganic fillers such as silica. Here, "not containing inorganic fillers such as silica" means intentionally not adding inorganic fillers to the resin composition, and the inorganic material may be included in a range of 0.0001 mass% or more and 0.01 mass% or less with respect to 100 mass% of the resin composition, or the inorganic material may be 0 mass% or not included.
[0165] Method for manufacturing a resin composition
[0166] A resin composition can be prepared by mixing component (A) and component (B), and optionally component (C). A resin composition may also be prepared by mixing component (A) and component (B), and optionally component (C), together with an additive as needed. However, it is not desirable to include fillers such as silicon dioxide or aluminum oxide, as this may result in poor coating properties. It is preferable that the resin composition does not contain powder of silicon dioxide or aluminum oxide. The method of preparing the resin composition is not particularly limited. A resin composition may be prepared by mixing the raw materials that constitute each component using a mixer such as a Leica machine, a pot mill, a three-roll mill, a hybrid mixer, a rotary mixer, or a twin-screw mixer. Each of these components may be mixed simultaneously, or a portion may be mixed first and the remainder later. Additionally, a resin composition may be prepared by using a suitable combination of the above devices.
[0167] The cured product obtained by curing the resin composition preferably has a dielectric constant (ε) of 3.0 or less, more preferably 2.8 or less, and more preferably 2.7 or less. The dielectric loss tangent (tanδ) preferably has a dielectric constant of 0.015 or less, more preferably 0.014 or less, and more preferably 0.013 or less. Since the cured product having a low dielectric constant and a low dielectric loss tangent has good electrical characteristics when used in a high-frequency region, it can be used for electronic components, semiconductor devices, etc., used in a high-frequency region. In addition, when the resin composition is applied to a semiconductor substrate, for example using a spin coater, it is sufficiently cured, and a cured product in the form of a thin film having a roughly uniform film thickness is obtained, which has good electrical characteristics even when used in a high-frequency region such as a 5th generation communication system "5G," where high capacity and high-speed communication are expected to progress. Accordingly, the resin composition can be suitably used as a material for forming an interlayer insulating film that seals the side on which the electrode and wiring are disposed on the semiconductor substrate in a semiconductor device comprising a semiconductor substrate, an electrode disposed on the semiconductor substrate, wiring connected to the electrode, an external terminal electrically connected via the wiring, and an interlayer insulating film. This interlayer insulating film is disposed in contact with the wiring. In this specification, the "re-wiring layer" includes the wiring and the interlayer insulating film. In the literature, "wiring" may be described as a "re-wiring layer," and "interlayer insulating film" may be described as a "sealing resin layer." Furthermore, the resin composition can be suitably used as a material for forming an interlayer insulating film that seals the side of the wiring on the semiconductor substrate and the side of the wiring opposite to the semiconductor substrate in the semiconductor device. Furthermore, the film thickness of the re-wiring layer may be approximately 5 to 30 μm. Additionally, the film thickness of the re-wiring layer may be 5 μm or more, or 10 μm or more. In addition, the film thickness of the redistribution layer may be 30㎛ or less, or 20㎛ or less.
[0168] The resin composition can be suitably used as a sealing resin for WL-CSP type semiconductor devices.
[0169] Next, a WL-CSP type semiconductor device using a resin composition is described. The WL-CSP type semiconductor device comprises a semiconductor substrate, an electrode disposed on the semiconductor substrate, a wiring connected to the electrode, an external terminal electrically connected via the wiring, and an interlayer insulating film that seals the side of the semiconductor substrate where the electrode and wiring are disposed. The interlayer insulating film is formed using a resin composition comprising the aforementioned components (A), (B), and (C). The interlayer insulating film has an interlayer insulating film disposed in contact with the wiring. The WL-CSP type semiconductor device preferably comprises at least two layers: a first interlayer insulating film (also called a "conductor film") that seals the semiconductor substrate side of the wiring, and a second interlayer insulating film that seals the opposite side of the semiconductor substrate of the wiring. Both layers of the first interlayer insulating film (dielectric film) and the second interlayer insulating film are disposed in contact with the wiring and function as interlayer insulating films for the wiring.
[0170] semiconductor device
[0171] A WL-CSP type semiconductor device is described with reference to the drawings. FIG. 1 is a schematic cross-sectional view showing the schematic configuration of a WL-CSP type semiconductor device. The WL-CSP type semiconductor device is not limited to the example shown in FIG. 1.
[0172] A WL-CSP type semiconductor device (10) is provided with an electrode (2), a wiring (4) connected to the electrode (2), and an external connection terminal (8), such as a conductive ball, electrically connected to the wiring (4), on a semiconductor substrate (1). A protective layer (3), made of an oxide film or the like, may be formed between the wiring (4) and the semiconductor substrate (1). The WL-CSP type semiconductor device (10) is provided with interlayer insulating films (5, 6) that seal the side of the semiconductor substrate (1) where the electrode (2) and the wiring (4) are arranged. The interlayer insulating films (5, 6) are arranged to be in contact with the wiring (4). The film sealing the side of the wiring (4) toward the semiconductor substrate (1) is a first interlayer insulating film (dielectric film) (5). The film sealing the side of the wiring (4) opposite to the side of the semiconductor substrate (1) is a second interlayer insulating film (6). The interlayer insulating film (5, 6) may have at least two layers. The first interlayer insulating film (dielectric film) (5) and the second interlayer insulating film (6) are arranged so that both layers are in contact with the wiring (4). By using the same resin composition in the first interlayer insulating film (5) and the second interlayer insulating film (6), lower dielectric properties can be achieved, and electrical properties when used in a high-frequency range can be improved. The wiring (4), the first interlayer insulating film (dielectric film) (5), and the second interlayer insulating film (6) constitute a redistribution layer (7).
[0173] Method for manufacturing a semiconductor device
[0174] Next, a method for manufacturing a WL-CSP type semiconductor device will be described. Unless otherwise specifically stated, the semiconductor device refers to a WL-CSP type semiconductor device.
[0175] A semiconductor substrate made of materials such as silicon, SiGe, or SOI can be used. For electrodes, electrode material can be deposited on approximately the entire surface of the semiconductor substrate, for example by vacuum deposition or sputtering, and then patterned by, for example by photolithography, to form a plurality of electrodes at predetermined positions on the semiconductor substrate.
[0176] After forming an electrode on the surface of a semiconductor substrate, silicon nitride (SiN) can be deposited on the entire surface of the semiconductor substrate by, for example, a deposition method, and an oxide film (passivation film) can be formed on the surface of the silicon nitride to form a protective layer. The thicknesses of the semiconductor substrate, the electrode, and the protective layer are not particularly limited.
[0177] Next, a resin composition is dropped onto a semiconductor substrate, and the semiconductor substrate is rotated around a vertical axis using a spin coater to apply the liquid resin composition onto the semiconductor substrate, and the liquid resin composition is cured to form an interlayer insulating film. Specifically, the resin composition is dropped onto an electrode and a protective layer on a semiconductor substrate, and the semiconductor substrate is rotated around a vertical axis using a spin coater to apply the liquid resin composition onto the electrode and the protective layer on the semiconductor substrate, and the liquid resin composition is cured to form a first interlayer insulating film (dielectric film).
[0178] When applying a resin composition to form an interlayer insulating film, it is preferable that the rotation speed of the spin coater be 1000 rpm to 3000 rpm and the rotation time be 5 seconds to 30 seconds. If the rotation speed and rotation time of the spin coater are within the above ranges, the resin composition can be applied to the semiconductor substrate with a roughly uniform thickness, and an interlayer insulating film having a desired roughly uniform thickness can be formed after curing, thereby suppressing warping of the semiconductor substrate during curing.
[0179] The interlayer insulating film can be formed using a resin composition comprising the aforementioned components (A) and (B), and optionally including component (C). By using the aforementioned resin composition, even when the resin composition is applied to a semiconductor substrate using a spin coater, a coating film of approximately uniform thickness with minimal variation in thickness can be formed, thereby enabling the formation of a first interlayer insulating film (dielectric film) that suppresses warping of the semiconductor substrate during curing.
[0180] A resin composition comprising the aforementioned components (A) and (B), and optionally comprising component (C), can be used to form a correlated insulating film, and the interlayer insulating film may be a first interlayer insulating film (dielectric film) or a second interlayer insulating film. The aforementioned component (A) preferably comprises a modified PPE resin represented by Formula (1), and the component (A) preferably comprises at least one selected from the group consisting of a modified PPE resin represented by Formula (5) and a modified PPE resin represented by Formula (6). The aforementioned component (B) preferably comprises at least one selected from the group consisting of SBS represented by Formula (7) and NBR represented by Formula (8).
[0181] It is preferable that the rotational speed of the spin coater be 1000 rpm to 3000 rpm, and the rotation time be 5 seconds to 30 seconds.
[0182] When applying to a semiconductor substrate using a spin coater, the resin composition described above preferably has a first viscosity of 300 mPa·s to 4000 mPa·s at 25°C and 10 rpm using a rotational viscometer, is more preferably 400 mPa·s to 4000 mPa·s, and even more preferably 500 mPa·s to 2000 mPa·s. If the first viscosity of the resin composition described above when applying to a semiconductor substrate using a spin coater is within the above range, the variation in thickness is small, and a coating film of approximately uniform thickness can be formed, thereby suppressing warping of the semiconductor substrate during curing.
[0183] When applying to a semiconductor substrate using a spin coater, the resin composition described above preferably has a second viscosity at 25°C and 1 rpm measured by a rotational viscometer within the range of 600 mPa·s to 4200 mPa·s, more preferably within the range of 500 mPa·s to 4200 mPa·s, more preferably within the range of 550 mPa·s to 4000 mPa·s, and even more preferably within the range of 550 mPa·s to 3500 mPa·s. If the second viscosity of the resin composition described above is within the above range when applying to a semiconductor substrate using a spin coater, the variation in thickness is small, and a coating film of approximately uniform thickness can be formed, thereby suppressing warping of the semiconductor substrate during curing.
[0184] When applying to a semiconductor substrate using a spin coater, the resin composition described above preferably has a thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, within the range of 0.8 to 1.2, and may be within the range of 0.9 to 1.1 or within the range of 1.0 to 1.1. When applying to a semiconductor substrate using a spin coater, if the second viscosity relative to the first viscosity of the resin composition described above is within the above range, the variation in thickness is small and a coating film of approximately uniform thickness can be formed, thereby suppressing warping of the semiconductor substrate during curing.
[0185] It is preferable that the thickness of one film of the interlayer insulating film, the first interlayer insulating film (dielectric film), or the second interlayer insulating film be within the range of 3㎛ or more and 20㎛ or less, and may be within the range of 4㎛ or more and 18㎛ or less, or within the range of 5㎛ or more and 17㎛ or less. If the thickness of one film of the interlayer insulating film, the first interlayer insulating film (dielectric film), or the second interlayer insulating film is within the range of 3㎛ or more and 20㎛ or less, the requirements for miniaturization and thinning of the semiconductor device can be satisfied even when multiple films are stacked.
[0186] In a method for manufacturing a semiconductor device, after applying a resin composition, drying and curing it, a first interlayer insulating film (dielectric film) can be formed by laser direct patterning, for example, using a laser direct patterning device (manufactured by Mitsubishi Electric Corporation), to open the surface portion of the electrode.
[0187] Next, a seed layer for forming wiring is formed on approximately the entire surface of a semiconductor substrate having an electrode, a protective layer, and a first interlayer insulating film (dielectric film) formed thereon by deposition, sputtering, chemical vapor deposition (CVD), electroless plating, etc. The seed layer may include copper, copper oxide, an alloy of copper and chromium, copper, tantalum, cobalt, titanium, and their alloys, and the seed layer may have a stacked structure in which multiple layers are stacked. A resist is formed in a predetermined pattern on this seed layer, for example by photolithography, and wiring of a predetermined pattern is formed by electroplating or electroless plating using this resist film as a mask. After forming the wiring, the resist film is peeled off, and the seed layer remaining in the non-forming area of the wiring is removed by etching, etc. The thickness of the wiring is not specifically limited, but the thickness of the wiring may be 0.1㎛ or more, 15㎛ or less, 12㎛ or less, or 10㎛ or less.
[0188] Next, a resin composition is applied to the wiring using a spin coater so that the surface height becomes approximately uniform, thereby forming a second interlayer insulating film. Similar to the first interlayer insulating film, the second interlayer insulating film may utilize a resin composition comprising the aforementioned components (A), (B), and (C), and may be applied to a semiconductor substrate using a spin coater with the same rotation speed and rotation time as the first interlayer insulating film, specifically applied to the wiring. Furthermore, after applying the resin composition, it may be dried and cured, and then, for example, a laser direct patterning device (manufactured by Mitsubishi Electric Corporation) may be used to form a second interlayer insulating film by laser direct patterning, thereby opening the surface portion of the wiring where the external terminal described later is placed. The second interlayer insulating film may also be formed by opening the surface portion of the electrode through exposure and development.
[0189] There are also cases where the formation of the first interlayer insulating film (dielectric film), the formation of wiring, and the formation of the second interlayer insulating film are combined to form a redistribution layer.
[0190] Afterwards, external terminals such as solder balls can be formed in the opening portion of the redistribution layer by means of a solder ball mounting method, a solder plating method, a solder paste method, a solder paste defense method, a solder deposition method, etc., thereby forming a WL-CSP type semiconductor device. Since the first interlayer insulating film and the second interlayer insulating film formed in this way are formed using a resin composition containing the aforementioned components (A), (B), and (C), the WL-CSP type semiconductor device has a low dielectric constant and a low dielectric loss tangent, and the electrical characteristics are good even when the semiconductor device is used in a high-frequency region such as a 5th generation communication system "5G," where high capacity and high-speed communication are expected to progress.
[0191] The resin composition of an embodiment of the present invention and the semiconductor device using the same can be used in electronic components of electronic devices such as mobile phones, smartphones, laptops, tablet terminals, and camera modules.
[0192] Examples
[0193] The present invention will be described in more detail below in the examples. The present invention is not limited to these examples. In the following examples and comparative examples, the numbers indicating the mixing ratio of each component included in the resin composition represent the ratio (mass (%)) of the total amount of the resin composition as 100 mass%, unless otherwise specifically stated. In cases where only component (A), component (B), and component (C) are included in the resin composition and no additives are included, the total amount of the resin composition represents the sum of component (A), component (B), and component (C).
[0194] Component (A): Modified polyphenylene ether (PPE) resin
[0195] A-1: OPE 2St 1200 (a modified polyphenylene ether resin represented by Formula (6) having vinyl groups at both ends (reaction product of 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol·2,6-dimethylphenol condensate and chloromethylstyrene), number average molecular weight (Mn) 1200) (manufactured by Mitsubishi Gas Chemical Co., Ltd.)
[0196] A-2: OPE 2St 2200 (a modified polyphenylene ether resin represented by Formula (6) having vinyl groups at both ends (reaction product of 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol·2,6-dimethylphenol condensate and chloromethylstyrene), number average molecular weight (Mn) 2200) (manufactured by Mitsubishi Gas Chemical Co., Ltd.)
[0197] A-3: NORYL SA9000 (a modified polyphenylene ether resin represented by Formula (5) having a group represented by Formula (3) at the terminals and methacryloyl groups at both terminals, number average molecular weight (Mn) 1850~1950.) (Made by SABIC) (SABIC Innovative Plastics)
[0198] Component (B): Unhydrogenated styrene / butadiene / styrene block copolymer (SBS)
[0199] B-1: Styrene / butadiene / styrene block copolymer (SBS) TR2827, styrene / butadiene ratio 24 / 76 (%), number average molecular weight (Mn) 130,000 (manufactured by JSR Corporation).
[0200] B-2: Styrene / butadiene / styrene block copolymer (SBS) TR2003, styrene / butadiene ratio 43 / 57 (%), number average molecular weight (Mn) 100,000 (manufactured by JSR Corporation).
[0201] B-3: Styrene / butadiene / styrene block copolymer (SBS) TR2250, styrene / butadiene ratio 52 / 48 (%), number average molecular weight (Mn) 100,000 (manufactured by JSR Corporation).
[0202] B-4: Partially Hydrogenated Styrene / Butadiene / Butylene / Styrene Block Copolymer (SBBS) P5051, Styrene / Butadiene Ratio 47 / 53 (%), Number Average Molecular Weight (Mn) 53,000 (Manufactured by Asahi Chemical Co., Ltd.)
[0203] B-5: Carboxylated nitrile-butadiene rubber (NBR) with carboxyl-terminated ends (NBR) Nipol (trademark) 1072, number average molecular weight (Mn) 500,000 (manufactured by Nippon Zeon Co., Ltd.)
[0204] Component (B'): Tetrafluoroethylene resin
[0205] B'-6: Tetrafluorinated ethylene resin Lubron (registered trademark) L-5F (manufactured by Daikin Industries, Ltd.).
[0206] Ingredient (C): Solvent
[0207] C-1: Toluene (manufactured by Daisin Chemical Co., Ltd.) Boiling point: 110.6℃.
[0208] C-2: Anone (cyclohexanone, manufactured by Daisin Chemical Co., Ltd.), boiling point 155.65℃.
[0209] Additive: Organic peroxide
[0210] Perbutyl (registered trademark) Z (manufactured by Nichiyu Co., Ltd.)
[0211] Examples 1–12, Comparative Example 1
[0212] Component (A), Component (B) or Component (B'), and Component (C) were mixed and dissolved using a stirrer (SSR-112, manufactured by AGC Technoglass Co., Ltd.) in a constant temperature water bath (SB-35, Tokyo Iwa Machinery Co., Ltd.) at a constant temperature of 70°C to prepare each resin composition of the Examples and Comparative Examples. In Table 1, the symbol “-” indicates that the corresponding component is not included in the resin composition. Also, in Table 1, “Mn” represents the number average molecular weight.
[0213]
[0214] Evaluation of resin composition
[0215] The solubility and viscosity of each resin composition of the examples and comparative examples were measured, and the results are listed in Table 3. In Table 3, for Comparative Example 1, where component (B') does not dissolve in the solvent of component (C), since a coating film cannot be formed, no evaluation can be performed, and it is listed as NA (Not Available).
[0216] Solubility
[0217] For each resin composition, the solubility of component (A) and component (B) or component (B') was evaluated by setting the solvent of component (C) to 70°C. A resin composition in which component (A) and component (B) or component (B') were visually identifiable as dissolved in the solvent of component (C) was rated as G (good), and a resin composition in which they were visually identifiable as not dissolving was rated as N (not-good).
[0218] viscosity
[0219] For each resin composition, a first viscosity at 25°C and 10 rpm and a second viscosity at 25°C and 1 rpm were measured using a TVE type viscometer (cone rotor: 1° 34'×R24, manufactured by Donggi Sangyo Co., Ltd.), and the thixotropy index TI (viscosity at 1 rpm / viscosity at 10 rpm) of the second viscosity relative to the first viscosity was measured.
[0220] Formation of interlayer insulating film
[0221] A coating film serving as an interlayer insulating film was formed using each resin composition of the examples and comparative examples, and the following evaluation was performed on the cured product in which the coating film made of the resin composition was cured by heat treatment under the following conditions. The results are listed in Table 3.
[0222] Thickness of interlayer insulating film by spin coating
[0223] As a semiconductor substrate, each resin composition of the example and comparative example was spin-coated on a silicon wafer with a diameter of 150 mm and a thickness of 0.525 mm using a spin coater (MS-A200, manufactured by MIKASA Co., Ltd.). Spin coating was performed by operating the spin coater at 1000 rpm for 5 seconds, followed by at 2000 rpm for 30 seconds, to spin-coat the resin composition onto the surface of the silicon wafer and form a film.
[0224] In addition, as a semiconductor substrate, each resin composition of the example and comparative example was spin-coated on a silicon wafer with a diameter of 150 mm and a thickness of 0.525 mm using a spin coater (MS-A200, manufactured by MIKASA Co., Ltd.). Spin coating was performed by operating the spin coater at 1000 rpm for 5 seconds, followed by at 3000 rpm for 30 seconds, to spin-coat the resin composition onto the surface of the silicon wafer and form a film.
[0225] Next, a silicon wafer having a thin film of the resin composition was subjected to pre-heat treatment (drying) at 130°C for 10 minutes under a nitrogen atmosphere and heated to obtain a sample in which the film of the resin composition was dried. Subsequently, a sample in which the film of the resin composition was cured was obtained by subjecting it to heat treatment (curing) at 200°C for 60 minutes under a nitrogen atmosphere. The film thickness of the resin composition was measured using a stylus-type profiling system (Surfcom 300B, manufactured by Tokyo Precision Co., Ltd.). Additionally, the film thickness of the interlayer insulating film can be approximately 5 µm to 30 µm. Additionally, the film thickness of the interlayer insulating film may be 5 µm or more, or 10 µm or more. Additionally, the film thickness of the interlayer insulating film may be 30 µm or less, or 20 µm or less.
[0226] Bending of semiconductor substrates
[0227] As a semiconductor substrate, the warping of the silicon wafer itself (before coating) with a diameter of 150 mm and a thickness of 0.525 mm was measured using a 3D heated surface shape measuring device (Thermoray AXP 2.0, manufactured by Akrometrix) (hereinafter referred to as "initial warping amount"). 3 g of a resin composition was dropped onto the center of this silicon wafer, and each resin composition of the example and comparative example was spin-coated using a spin coater (MS-A200, manufactured by MIKASA Corporation). Spin coating was performed by operating the spin coater to spin-coat the resin composition onto the surface of the silicon wafer, thereby forming a coating film.
[0228] Next, a silicon wafer having a thin film of a resin composition was subjected to heat treatment (drying) at 130°C for 10 minutes under a nitrogen atmosphere and heated to obtain a sample in which the film of the resin composition was dried. After that, a sample in which the film of the resin composition was cured was obtained by subjecting it to heat treatment (curing) at 200°C for 60 minutes under a nitrogen atmosphere.
[0229] Next, the warping of the silicon wafer was measured using a 3D heated surface shape measuring device (Thermoray AXP 2.0, manufactured by Akrometrix) (hereinafter referred to as "warping amount after curing"). Warping amount refers to the value (height) obtained by subtracting the initial warping amount from the "warping amount after curing." Hereinafter, the silicon wafer will also be simply referred to as a "wafer."
[0230] Bending amount = (Bending amount after hardening) - (Initial bending amount)
[0231] The amount of warping is preferably within the range of -5 mm to 5 mm, more preferably within the range of -3 mm to 3 mm, and even more preferably within the range of -2 mm to 2 mm. If the amount of warping is within the range of -5 mm to 5 mm, the wafer can be adsorbed and held using a wafer holding device (e.g., vacuum tweezers) having a vacuum suction mechanism, and the wafer can be transported to a desired position by moving the wafer holding device. However, if the wafer has a large amount of warping, the entire surface of the wafer cannot be adsorbed, and, for example, only the central part of the wafer is partially adsorbed. In this case, sufficient holding force cannot be obtained, and there is a risk that the wafer may move away from the vacuum tweezers and fall off due to a slight impact during wafer transport. If the holding force becomes extremely small, there are cases where the wafer cannot be adsorbed.
[0232] Strength (Adhesion) Measurement (Cross-cut Peel Test)
[0233] Strength (adhesion) was measured in accordance with ASTM D3359-97.
[0234] Specifically, as a semiconductor substrate, each resin composition of the example and comparative example was spin-coated using a silicon wafer spin coater (MS-A200, manufactured by Mikasa Corporation) with a diameter of 150 mm and a thickness of 0.525 mm. Spin coating was performed by operating the spin coater to spin-coat the resin composition onto the surface of the silicon wafer, thereby forming a film.
[0235] Next, a silicon wafer having a thin film of the resin composition was subjected to heat treatment (drying) at 130°C for 10 minutes under a nitrogen atmosphere and heated to obtain a sample in which the film of the resin composition was dried. After that, a sample in which the film of the resin composition was cured was obtained by subjecting it to heat treatment (curing) at 200°C for 60 minutes under a nitrogen atmosphere. In this way, a sample for a cross-cut peel test was prepared.
[0236] Using a cross-cut guide (manufactured by Kotech Co., Ltd.), slits are made in a grid shape that intersect in a cross pattern on the surface of a sample having a coating that functions as an interlayer insulating film. Then, cellophane tape (manufactured by Nichiban Co., Ltd.) is attached to the intersecting slits, and the attached cellophane tape is quickly peeled off. Accordingly, the area of the peeled coating is measured and judged as 6 levels from 0B to 5B as shown in Table 2 below.
[0237]
[0238] Relative permittivity (ε), genetic tangent (tanδ)
[0239] The measurement sample was prepared as follows.
[0240] Each resin composition of the examples and comparative examples was applied to a polyethylene terephthalate (PET) support, and a heat treatment (drying) was performed at 130°C for 10 minutes under a nitrogen atmosphere, and the resin composition was dried by heating, and a heat treatment (curing) was performed at 200°C for 60 minutes under a nitrogen atmosphere to obtain a coating film made of a resin composition with a film thickness of 10 μm.
[0241] The relative permittivity (ε) and dielectric loss tangent (tanδ) of the measurement sample were measured at a dielectric resonance frequency of 5 GHz by the cavity resonator perturbation method. The relative permittivity (ε) is preferably 1.5 to 3.0, and the dielectric loss tangent (tanδ) is preferably 0.001 to 0.010.
[0242]
[0243] As shown in Tables 1 and 3, the resin compositions of Examples 1 to 12 had good solubility for component (C) of component (A) and component (B), and when applied to a semiconductor substrate using a spin coater, a film with approximately uniform thickness could be formed. In addition, the film obtained from the resin compositions of Examples 1 to 12 had a relative permittivity (ε) of 2.7 or less and a dielectric loss tangent (tanδ) of 0.015 or less, and had good electrical characteristics even when using semiconductor devices in high-frequency regions such as the 5th generation communication system "5G," where high capacity and high-speed communication are expected to progress.
[0244] In addition, as shown in Tables 1 and 3, the resin compositions of Examples 1 to 12 had a first viscosity at 25°C and 10 rpm measured by a rotational viscometer in the range of 300 mPa·s to 4000 mPa·s, a second viscosity at 25°C and 1 rpm measured in the range of 500 mPa·s to 4200 mPa·s, and a thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, in the range of 0.8 to 1.2. The resin compositions of Examples 1 to 9 had a small variation in thickness even when applied to a semiconductor substrate using a spin coater, and could form a film of approximately uniform thickness, thereby suppressing warping of the semiconductor substrate during curing. Furthermore, the resin compositions of Examples 1 to 12 received a 5B rating in the cross-cut peel test, with a removed area of 0%, and the adhesion was also good.
[0245] The resin composition containing the tetrafluoride ethylene resin of Comparative Example 1 could not form a film because SEBS or the tetrafluoride ethylene resin did not dissolve in the solvent of component (C), so the resin composition could not be applied to a semiconductor substrate. Industrial applicability
[0246] The resin composition related to the present invention can be used in WL-CSP type semiconductor devices. The resin composition of an embodiment of the present invention and the semiconductor device using it can be used in electronic components of electronic devices such as mobile phones, smartphones, laptops, tablet terminals, and camera modules. Explanation of the symbols
[0247] 1: Semiconductor substrate, 2: Electrode, 3: Protective layer, 4: Wiring, 5: First interlayer insulating film (dielectric film), 6: Second interlayer insulating film, 7: Redistribution layer, 8: External terminal, 10: Semiconductor device.
Claims
Claim 1 A resin composition for forming a redistribution layer of a wafer-level chip-size package type semiconductor device, comprising (A) a modified polyphenylene ether resin having an unsaturated double bond at the terminal end, and (B) an elastomer having a butadiene backbone, wherein the first viscosity at 25°C and 10 rpm, measured by a rotational viscometer, is within the range of 300 mPa·s to 4000 mPa·s. Claim 2 A resin composition for forming a redistribution layer of a wafer-level chip-size package type semiconductor device, comprising (A) a modified polyphenylene ether resin having an unsaturated double bond at the terminal end, and (B) an elastomer having a butadiene backbone, wherein (B) the elastomer having a butadiene backbone comprises at least one selected from the group consisting of a styrene / butadiene / styrene copolymer having a styrene / butadiene ratio of 15 / 85 or more, a styrene / butadiene / butylene / styrene copolymer having a styrene / butadiene ratio of 47 / 53 or more, a butadiene polymer, a styrene / butadiene copolymer having a styrene / butadiene ratio of 15 / 85 or more, and an acrylonitrile / butadiene copolymer. Claim 3 In claim 1 or 2, the modified polyphenylene ether resin having an unsaturated double bond at the (A) end is of the following formula (1): [In Equation (1), X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and Y is the following Equation (2): [Equation (2), R 1 ~R 4 [represents an unsubstituted or substituted phenol repeating unit represented by, each independently representing a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, or an alkenylcarbonyl group, and Z represents a functional group containing a terminal carbon-carbon double bond, a vinyl group, a vinylene group, the following formula (3): [Equation (3), R 5 [represents a hydrogen atom or an alkyl group], a (meth)acryloyl group represented by the following formula (4): [Equation (4), R 6 ~R 8 A resin composition comprising a modified polyphenylene ether resin represented by [each independently representing a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group], m representing an integer from 1 to 100, n representing an integer from 0 or 1 to 6, and p representing an integer from 1 to 4. Claim 4 A resin composition according to claim 1, wherein the elastomer having (B) a butadiene backbone comprises at least one selected from the group consisting of styrene / butadiene / styrene copolymer, styrene / butadiene / butylene / styrene copolymer, butadiene polymer, styrene / butadiene copolymer, and acrylonitrile / butadiene copolymer. Claim 5 In claim 1 or 2, the modified polyphenylene ether resin having an unsaturated double bond at the (A) end is of the following formula (5): [Equation (5), R 5 represents a hydrogen atom or an alkyl group, X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and Y is the following formula (2): [Equation (2), R 1 ~R 4 [represents an unsubstituted or substituted phenol repeating unit, each independently representing a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, or an alkenyl carbonyl group, and m represents an integer from 1 to 100, n represents an integer from 0 or 1 to 6, and p represents an integer from 1 to 4], a modified polyphenylene ether resin, and the following formula (6): [Equation (6), R 6 ~R 8 A resin composition comprising at least one selected from the group consisting of modified polyphenylene ether resins represented by [each independently representing a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, X representing an unsubstituted or substituted aromatic hydrocarbon group of p value, Y representing an unsubstituted or substituted phenol repeating unit represented by the above formula (2), m representing an integer from 1 to 100, n representing an integer from 0 or 1 to 6, and p representing an integer from 1 to 4.] Claim 6 In claim 1 or 2, the elastomer having the (B) butadiene backbone is of the following formula (7): A styrene / butadiene / styrene block copolymer represented by [wherein in Equation (7), q and r represent integers from 0 to 1, at least one of which is not 0, s represents an integer from 1 to 1200, and t represents an integer from 1 to 1000], and the following Equation (8): A resin composition comprising at least one selected from the group consisting of acrylonitrile / butadiene copolymers represented by [wherein u represents an integer from 1 to 1200 and v represents an integer from 1 to 1000]. Claim 7 In claim 1 or 2, the modified polyphenylene ether resin having an unsaturated double bond at the (A) end is of the following formula (6): [Equation (6), R 6 ~R 8 Each represents independently a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, X represents a p-valent unsubstituted or substituted aromatic hydrocarbon group, and Y is represented by the following formula (2): [Equation (2), R 1 ~R 4 A resin composition comprising a modified polyphenylene ether resin represented by [where each represents an unsubstituted or substituted phenol repeating unit, which is represented by [each independently representing a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, or an alkenyl carbonyl group,] where m is an integer from 1 to 100, n is an integer from 0 or 1 to 6, and p is an integer from 1 to 4, wherein the elastomer having the butadiene backbone (B) comprises a styrene / butadiene / styrene copolymer. Claim 8 A resin composition according to claim 1 or 2, further comprising (C) a solvent. Claim 9 A resin composition according to claim 2, wherein the first viscosity at 25°C and 10 rpm, measured by a rotational viscometer, is within the range of 300 mPa·s to 4000 mPa·s. Claim 10 A resin composition according to claim 1 or 9, wherein, using a rotational viscometer, the second viscosity at 25°C and 1 rpm is within the range of 500 mPa·s to 4200 mPa·s, and the thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, is 0.8 to 1.
2. Claim 11 A resin composition according to claim 1 or 2, wherein the mass ratio of (A) and (B) is within the range of 10:90 to 80:
20. Claim 12 A resin composition according to claim 8, wherein the mass ratio of the total amount of (A) and (B) to (C) is within the range of 5:95 to 80:
20. Claim 13 A wafer-level chip-size package type semiconductor device comprising: a semiconductor substrate; an electrode disposed on the semiconductor substrate; a wiring electrically connected to the electrode; an external terminal electrically connected to the electrode via the wiring; and an interlayer insulating film that seals the side of the semiconductor substrate where the electrode and the wiring are disposed, wherein the interlayer insulating film is disposed in contact with the wiring and is formed using a resin composition described in claim 1 or 2. Claim 14 A semiconductor device according to claim 13, comprising at least two layers: a first interlayer insulating film sealing the semiconductor substrate side of the wiring, and a second interlayer insulating film sealing the opposite side of the semiconductor substrate of the wiring. Claim 15 A semiconductor device according to claim 14, wherein the thickness of one of the interlayer insulating film, the first interlayer insulating film, and the second interlayer insulating film is within the range of 3㎛ or more and 20㎛ or less. Claim 16 A method for manufacturing a wafer-level chip-size package type semiconductor device, comprising the following components (A) to (C): (A) a modified polyphenylene ether resin having an unsaturated double bond at the terminal end, (B) an elastomer having a butadiene backbone, and (C) a solvent; dropping the resin composition onto a semiconductor substrate and rotating the semiconductor substrate around a vertical axis using a spin coater to apply the resin composition to the semiconductor substrate; and curing the resin composition to form an interlayer insulating film, wherein the resin composition is a resin composition for forming a redistribution layer, wherein the first viscosity at 25°C and 10 rpm, measured by a rotational viscometer, is within the range of 300 mPa·s to 4000 mPa·s. Claim 17 The following components (A) to (C): (A) a modified polyphenylene ether resin having an unsaturated double bond at the terminal end, (B) an elastomer having a butadiene backbone, and (C) a solvent; preparing a liquid resin composition comprising the above components; dropping the resin composition onto a semiconductor substrate and rotating the semiconductor substrate around a vertical axis using a spin coater to apply the liquid resin composition to the semiconductor substrate; and curing the liquid resin composition to form an interlayer insulating film, wherein the (B) elastomer having a butadiene backbone is a styrene / butadiene / styrene copolymer having a styrene / butadiene ratio of 15 / 85 or more, a styrene / butadiene / butylene / styrene copolymer having a styrene / butadiene ratio of 47 / 53 or more, a butadiene polymer, a styrene / butadiene copolymer having a styrene / butadiene ratio of 15 / 85 or more, A method for manufacturing a wafer-level chip-size package type semiconductor device comprising at least one selected from the group consisting of acrylonitrile / butadiene copolymers, wherein the liquid resin composition is a resin composition for forming a redistribution layer. Claim 18 A method for manufacturing a semiconductor device according to claim 16 or 17, wherein the rotational speed of the spin coater is 1000 rpm to 3000 rpm and the rotational time is 5 seconds to 30 seconds. Claim 19 A method for manufacturing a semiconductor device according to claim 17, wherein the liquid resin composition has a first viscosity of 300 mPa·s to 4000 mPa·s at 25°C and 10 rpm using a rotational viscometer. Claim 20 A method for manufacturing a semiconductor device according to claim 16 or 19, wherein the liquid composition has a second viscosity of 500 mPa·s to 4200 mPa·s at 25°C and 1 rpm using a rotational viscometer, and a thixotropy index TI, which is the ratio of the second viscosity to the first viscosity, is 0.8 to 1.
2. Claim 21 In claim 16, the modified polyphenylene ether resin having an unsaturated double bond at the (A) end is of the following formula (1): [In Equation (1), X represents an unsubstituted or substituted aromatic hydrocarbon group of p, and Y is the following Equation (2): [Equation (2), R 1 ~R 4 [represents an unsubstituted or substituted phenol repeating unit represented by, each independently representing a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, or an alkenylcarbonyl group, and Z represents a functional group containing a terminal carbon-carbon double bond, a vinyl group, a vinylene group, the following formula (3): [Equation (3), R 5 [represents a hydrogen atom or an alkyl group], a (meth)acryloyl group represented by the following formula (4): [Equation (4), R 6 ~R 8 A method for manufacturing a semiconductor device comprising a modified polyphenylene ether resin, wherein [a styrene group is represented as shown in [each independently representing a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group], m is represented as an integer from 1 to 100, n is represented as an integer from 0 or 1 to 6, and p is represented as an integer from 1 to 4], and wherein the elastomer having a butadiene backbone (B) comprises at least one selected from the group consisting of styrene / butadiene / styrene copolymer, styrene / butadiene / butylene / styrene copolymer, butadiene polymer, styrene / butadiene copolymer, and acrylonitrile / butadiene copolymer.
Citation Information
Patent Citations
Thermally curable resin composition, insulating film, inter-layer insulating film, multilayer wiring board, and semiconductor device
WO2019103086A1
Resin composition, prepreg, metal foil-clad laminated plate, resin sheet, and printed-wiring board
WO2020017412A1
Resin composition, insulation film and semiconductor device using the same
JP2016079354A
Resin composition, copper foil with resin, printed circuit board, and treatment method of copper foil with resin
JP2019172803A