Method for mass simultaneous manufacturing of materials for fuel injection nozzles using hot isostatic pressing (HIP)

The innovative brazing process with a molten metal annular spring on the can pipe addresses high defect rates in bonding dissimilar materials, achieving zero defects and enhancing productivity in fuel injection nozzle manufacturing.

KR103046519B1Active Publication Date: 2026-11-10이명배
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020260110928
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2026-04-20
Filing Date
2026-06-17
Publication Date
2026-11-10
Estimated Expiration
2046-06-17

AI Technical Summary

Technical Problem

Existing methods for manufacturing fuel injection nozzles using the HIP method face high defect rates due to issues with bonding dissimilar materials like Inconel powder and SKD 61 tool steel, leading to inefficient small-batch production and increased costs due to structural problems with nozzle cans.

Method used

A brazing process involving a molten metal annular spring formed on the inner wall of the can pipe, separated from the can cap seating portion, to ensure uniform filling of gaps and precise application of filler material, reducing defects to zero.

Benefits of technology

The method achieves near-zero defect rates and significantly improves productivity by ensuring consistent sealing and efficient use of filler material, allowing for large-scale production of fuel injection nozzle materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026073927415-PAT00007_ABST
    Figure 112026073927415-PAT00007_ABST
Patent Text Reader

Abstract

A brazing process comprising: a first heating step of introducing a plurality of nozzle cans into a vacuum chamber capable of forming a vacuum of at least 1 Torr for simultaneously manufacturing a plurality of sealed nozzle cans, and then raising the temperature to a predetermined temperature between 350 and 550°C; a first constant temperature step of maintaining the predetermined temperature between 350 and 550°C for a predetermined time between 3 and 6 hours and performing a degassing process to form a vacuum state of at least 1 Torr; a second heating step of subsequently raising the temperature to a predetermined temperature between 950 and 1150°C; a second constant temperature step of maintaining the predetermined temperature between 950 and 1150°C for a predetermined time between 1 and 3 hours; and a subsequent cooling step of lowering the temperature; wherein the nozzle can comprises SKD 61 tool steel; a can pipe assembled with the SKD 61 tool steel inserted therein; and Inconel powder introduced in a certain amount through the open top of the can pipe in accordance with the specifications of the SKD 61 tool steel. It may include: a can cap formed with a convex shape at the bottom and fitted and fixed inside the upper side of the can pipe; a can cap seating portion formed by contact between the inner wall of the can pipe and the lower outer wall of the can cap; a filler material attachment portion located on the inner wall of the can pipe above the can cap seating portion; a portion where the lower end of the can pipe contacts the SKD 61 tool steel; and a molten metal annular spring formed above the can cap seating portion so that molten metal originating from the filler material of the filler material attachment portion between the can pipe and the can cap can flow down and accumulate in an annular shape during the brazing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a material for a fuel injection nozzle using the HIP method, and more specifically, to a method for simultaneously manufacturing a large quantity of a fuel injection nozzle material using the HIP method, wherein the material is used in large diesel engines such as marine engines, and vacuum brazing is used to facilitate the bonding of dissimilar materials by sintering Inconel powder and SKD 61 tool steel with different strengths using the HIP method, thereby enabling the sealing of the nozzle can. Background Technology

[0002] Generally, a fuel injection nozzle for a large diesel engine of the two-stroke type, such as a ship's engine, is used to have a nozzle body and a nozzle head, and the nozzle head is provided with a plurality of nozzle holes, through which fuel is injected into the combustion chamber, and a movable nozzle needle is configured to be mounted on the fuel injection nozzle to operate together with a valve seat to open and close a passage leading to the nozzle holes in the fuel injection nozzle to start or end the injection process.

[0003] The nozzle head described above is configured to protrude into the combustion chamber of the cylinder and is a product prone to natural wear because it is continuously subjected to high heat, mechanical and chemical loads during operation. The mechanical load is applied by high injection pressures of 1,000 bar or more, the thermal load is caused by heat generated due to the high temperature inside the combustion chamber and the enormous temperature difference between the combustion temperature and the temperature of the newly supplied scavenging air, and the chemical load is mainly due to high temperature, corrosion, or thermal corrosion.

[0004] There is a problem in that the lifespan of the nozzle head is shortened due to significant spontaneous wear caused by high heat, mechanical, and chemical loads applied to the nozzle head. Consequently, nozzle heads that have reached the end of their lifespan must be replaced, but this replacement work imposes a heavy burden of labor and cost, leading to reduced work efficiency and economic viability.

[0005] There have been many research and development efforts to solve this problem. Looking at Patent No. 2007-106453, "Method for manufacturing a material for a fuel injection nozzle using the HIP method," and Patent No. 2007-106454, "Method for manufacturing a material for a fuel injection nozzle using the HIP method," it is possible to provide a fuel injection nozzle material by sintering and bonding SKD 61 tool steel and Inconel powder to manufacture a fuel injection nozzle for a ship engine using composite materials. This enables the manufacture of a fuel injection nozzle material with excellent lifespan by sintering and bonding dissimilar materials using the HIP (Hot Isostatic Press) method on a nozzle can assembled through a canning operation.

[0006] Let us examine the details of the two inventions above. When looking at the process of assembling SKD 61 tool steel into a can into which Inconel powder has been introduced during the processing process and then sealing it, in the case of the above-mentioned Patent No. 2007-106453, "Method for manufacturing a material for a fuel injection nozzle using the HIP method," a certain amount of Inconel powder is introduced into the interior of a can formed with one side open, in accordance with the specifications of SKD 61 tool steel, and after assembling the SKD 61 tool steel so that it is inserted into the interior of the can into which the Inconel powder has been introduced, TIG (Tungsten Inert Gas) welding is performed on the part where the can and the SKD 61 tool steel come into contact to seal it.

[0007] In the case of Patent No. 2007-106454, "Method for manufacturing a material for a fuel injection nozzle using the HIP method," a nozzle can formed by assembling SKD 61 tool steel into a can into which Inconel powder is introduced in the same manner as the patent invention is loaded into a vacuum chamber, and after performing a degassing process to remove impurities such as moisture and gas from the Inconel powder filled inside the nozzle can by the vacuum in the vacuum chamber, electron beam welding is performed using an electron beam device on the assembled part of the nozzle can, that is, the part where the can and the SKD 61 tool steel come into contact, to seal it.

[0008] However, these inventions have a problem in that, in order to sinter and bond dissimilar materials, such as Inconel powder and SKD 61 tool steel, using the HIP method, the sealing work on the nozzle can, which is assembled and formed so that SKD 61 tool steel is inserted into the inside of the can into which Inconel powder is inserted, must be processed individually, which delays the work time, and the work efficiency is reduced because, due to the sealing work on the individual nozzle cans, small-batch production that must be produced individually is unavoidable.

[0009] The invention developed to solve this problem is Patent No. 10-0899780. This invention adopts a joining process in which brazing, a type of soldering, uses a filler metal having a lower melting point than the base metal at 450°C or higher, melts only the filler metal without melting the base metal, fills the narrow gap between the two base metals using the spreadability, wettability, and capillary action of the molten metal, and then joins the two base metals through phenomena such as diffusion, alloying, and adhesion between the filler metal and the base metal.

[0010] The invention of Patent No. 10-0899780 is vacuum brazing, which is a brazing process performed in a vacuum atmosphere. When brazing is performed in a vacuum, not only is oxidation not prevented due to the clean atmosphere, but the oxide film on the metal surface is also easily removed by decomposition or diffusion, thereby improving the fluidity and wettability of the molten metal. Consequently, there is no need to use flux to remove the oxide film, so post-treatment to remove flux is not required after brazing is finished. Additionally, by applying uniform heating, it has the advantage of effectively joining complex assemblies with large thickness variations.

[0011] However, in actual application, due to structural issues with the nozzle can and the difficulty of fine-tuning the application of filler material, there was a serious problem where the defect rate of the product after the brazing process exceeded 30%, and even reached up to 80%. Of course, compared to previous technology, there were many advantages in terms of being able to produce dozens of products simultaneously, but the defect rate exceeding 30% was a major problem that significantly undermined those advantages. Therefore, although we have consistently pursued a solution to the problem through various research and developments, we had no choice but to continue production for a long time while bearing this issue due to the advantage of being able to mass-produce simultaneously.

[0012] The present invention was completed after many trials and errors, based on various attempts and research over more than 10 years to solve the above problems of the invention of Patent No. 10-0899780. The problem to be solved

[0013] The invention of Patent No. 10-0899780 has the advantage of being able to manufacture multiple nozzle cans simultaneously using vacuum brazing. However, in actual application, due to structural problems with the nozzle cans, there was a serious issue where the product defect rate after the brazing process exceeded 30%, and even 80%. Although many experiments and various analyses were conducted over a considerable period, it was difficult to find a solution by understanding the cause and detailed mechanism, as the defects resulted from the complex interaction of minute factors in a high-temperature enclosed room.

[0014] However, through a long and systematic research and experimental process, as well as feedback from the actual production process, the causes of defects could be summarized as follows.

[0015] The first problem is poor bonding at the point where the lower end of the can pipe contacts the tool steel. In this regard, the invention of Patent No. 10-0899780 describes bonding using a filler material, but through repeated failures, it was found that bonding using a filler material is fundamentally difficult when considering the flow of molten metal.

[0016] The second cause of defect is that the metal powder originating from the filler material tends to be partially scattered and lost during the degassing process.

[0017] In the invention of Patent No. 10-0899780, the filler material is positioned at the top of the can cup seating area, that is, at the top of the part where the inner wall of the can pipe and the outer wall of the can cup meet, i.e., the part to be welded. Furthermore, since the filler material consists of metal powder and an organic binder, while maintaining it at a constant temperature of approximately 400°C in a vacuum chamber for about 5 hours, the organic binder completely volatilizes and disappears, leaving only the metal powder, which has not yet reached its melting point, in a solid state. At this time, the shape of the metal powder from which the organic solvent has been removed is not uniform, and there are also some differences in the shape and spacing of the gaps where degassing typically occurs. Therefore, it is judged that the metal powder originating from the filler material tends to be partially scattered and lost in various forms during the degassing process, as it is located in the path where gas leaks out during the degassing process.

[0018] The third cause of the defect is as follows.

[0019] Although there is a very small gap in the area where the inner wall of the can pipe and the outer wall of the can cap meet to form the can cap seating area, it is almost impossible to make that gap uniform. Therefore, as the contact area and the area with a somewhat wider gap exist in an unpredictable state, the scattering of solidified metal powder, which was pointed out as the second problem above, tends to be partially intensified by the uneven degassing airflow caused by the uneven spacing of the gap, and in particular, these factors become a significant cause of the molten metal powder failing to uniformly and sufficiently fill all the gaps.

[0020] In particular, it was discovered after significant experiments and research that the larger the gap, the more metal particles are scattered and lost during the degassing process, and that these two factors tend to interact synergistically to exacerbate defects.

[0021] At the time of the invention of Patent No. 10-0899780, it was determined that molten metal would seep into the gaps where degassing would naturally occur in the liquid state. When viewed in detail, given that these gaps have various shapes and spacings, it is naturally reasonable to expect that a large portion would be filled by the molten metal. However, it is important to note that if they are not filled 100% perfectly, they will inevitably result in defects. Although work has been carried out for a long time by fine-tuning various conditions such as the amount of filler material used and the application method, there were limitations in lowering the defect rate, and it was particularly problematic that it was not easy to maintain a consistent defect rate.

[0022] Fourth, it is difficult to determine the appropriate amount of filler material. It is also difficult to gauge the unevenness of the gap between the metal powder that scatters and falls off and the can cap's seating area. In particular, molten metal powder often flows down the outer wall of the can pipe and the inner wall of the can cap. To address this, there has been a tendency to apply as much filler material as possible for a long period of time to reduce defects.

[0023] Fifth, it is difficult to reduce the defect rate even if one attempts to reduce it by applying a large amount of filler material. Although increasing the amount of filler material applied did lower the defect rate to some extent, the effect was limited because the amount and shape of the dripping during actual production varied for each product. Furthermore, increasing the amount of filler material used was also limited due to the narrow application space.

[0024] Due to the combined effects of the aforementioned problems, it was unavoidable to work while enduring a defect rate of over 30% for a long period, but the present invention innovatively improves these problems to enable the defect rate to be eliminated to almost zero. means of solving the problem

[0025] A brazing process comprising: a first heating step of introducing a plurality of nozzle cans into a vacuum chamber capable of forming a vacuum of at least 1 Torr for simultaneously manufacturing a plurality of sealed nozzle cans, and then raising the temperature to a predetermined temperature between 350 and 550°C; a first constant temperature step of maintaining the predetermined temperature between 350 and 550°C for a predetermined time between 3 and 6 hours and performing a degassing process to form a vacuum state of at least 1 Torr; a second heating step of subsequently raising the temperature to a predetermined temperature between 950 and 1150°C; a second constant temperature step of maintaining the predetermined temperature between 950 and 1150°C for a predetermined time between 1 and 3 hours; and a subsequent cooling step of lowering the temperature; wherein the nozzle can comprises SKD 61 tool steel; a can pipe assembled with the SKD 61 tool steel inserted therein; and Inconel powder introduced in a certain amount through the open top of the can pipe in accordance with the specifications of the SKD 61 tool steel. It may include: a can cap formed with a convex shape at the bottom and fitted and fixed inside the upper side of the can pipe; a can cap seating portion formed by contact between the inner wall of the can pipe and the lower outer wall of the can cap; a filler material attachment portion located on the inner wall of the can pipe above the can cap seating portion; a portion where the lower end of the can pipe contacts the SKD 61 tool steel; and a molten metal annular spring formed above the can cap seating portion so that molten metal originating from the filler material of the filler material attachment portion between the can pipe and the can cap can flow down and accumulate in an annular shape during the brazing process.

[0026] The upper part of the can cap seating portion is welded by filler material, and the portion where the lower end of the can pipe and the SKD 61 tool steel come into contact can be welded by argon welding.

[0027] The above-mentioned filler material attachment portion may be positioned spaced upward within a range of 1 to 5 mm from the top of the can cap seating portion.

[0028] The top of the can pipe may be higher than the top of the can cap, and the filler material attachment part may be located on the inner wall of the can pipe which is higher than the top of the can cap.

[0029] The part of the above-mentioned filler material attachment section where the filler material is applied may have a shape that is engraved in a semicircle or triangle inside the inner wall of the can pipe.

[0030] The above molten metal annular spring can be formed on the upper part of the can cap seating portion such that the gap between the inner wall of the can pipe and the outer wall of the can cap allows molten metal originating from the filler material to flow down during the brazing process and accumulate in an annular shape.

[0031] The amount of molten metal collected in the above molten metal annular spring may be greater than the amount of molten metal that seeps into the can cap seating portion, and preferably, the amount of molten metal collected in the above molten metal annular spring may be 70 to 90 weight percent of the total molten metal.

[0032] The above can cap seating portion can be formed into a cylindrical shape in surface contact.

[0033] The height of the top of the can cap is higher than the height of the top of the can pipe, and the filler material attachment part may be located on the upper part of the outer wall of the can cap, which is higher than the top of the can pipe. Effects of the invention

[0034] First, even if the shape of the gap in the can cap seating area varies and the spacing is different, if less than 30% of the molten metal of the filler material fills the gap in the can cap seating area and more than 70% of the molten metal forms a molten metal ring that is connected in an annular shape, the can cap seating area can always be 100% sealed regardless of the shape of the can cap seating area or the spacing of the gap.

[0035] Secondly, it is possible to precisely adjust the amount of filler material used. This is because if a molten metal ring well is formed to sufficiently accommodate the amount of molten metal, the phenomenon of molten metal flowing out along the outer wall can be almost completely eliminated.

[0036] Third, it is possible to improve productivity by alleviating the burden of having to very sensitively machine the shape and spacing of the gap in the can cap seating area.

[0037] Fourth, it eliminates the possibility of metal powder scattering during degassing, and second, it allows the molten metal powder to naturally flow into the molten metal ring during melting.

[0038] To this end, an important component adopted by the present invention is that the portion where the filler material is applied is located on the inner wall of the can pipe, separated from the top of the can cap seating portion by a certain distance. However, if the can cap is extended upward to form a molten metal ring, this does not exclude the possibility that the filler material can be applied to the upper part of the can cap's outer wall at a certain distance from the top of the can cap seating portion. Therefore, the essential significance of this component is, first, that the portion where the filler material is applied is separated from the top of the can cap seating portion by a certain distance to eliminate the potential for metal dust to scatter during degassing, and second, that the molten metal powder must naturally flow into the molten metal ring during melting; satisfying these two conditions constitutes a substantially identical outcome.

[0039] Fifth, a component optionally adopted by the present invention is that the shape of the area where the filler material is applied can be varied indefinitely, allowing the operator to easily apply the filler material.

[0040] Due to the effects mentioned above, innovative results were achieved in which the defect rate practically approached zero. Brief explanation of the drawing

[0041] FIG. 1 is a flowchart illustrating the manufacturing process of a material for a fuel injection nozzle using the HIP method applied to the present invention. FIG. 2 is an example of tool steel used in the manufacture of a material for a fuel injection nozzle using the HIP method applied to the present invention. FIGS. 3a and 3b are cross-sectional views of a can pipe and a can cap of an embodiment of the prior art (Registered Patent 10-0899780) used in the manufacture of a material for a fuel injection nozzle using the HIP method. FIG. 4 is a cross-sectional view illustrating the process of assembling a tool steel and a can into which Inconel powder has been introduced during the manufacture of a nozzle can, as an embodiment of the prior art (Registered Patent 10-0899780). FIG. 5 is a cross-sectional view illustrating a state in which a filler material is applied to an assembled part of a nozzle can applied as an embodiment of the prior art (Registered Patent 10-0899780). FIGS. 6 to 10 are cross-sectional views illustrating embodiments of the present invention, wherein the portion where the lower end of the can pipe contacts the tool steel is argon welded, the can cap is seated on the can pipe, and a filler material is applied. FIGS. 11 and 12 are cross-sectional views of another embodiment of the present invention in which the diameter of the can pipe is further expanded to accommodate all the tool steel, and the lower end of the pipe is argon welded. FIG. 13 is a cross-sectional view of one embodiment of a fuel injection nozzle that has been finally processed. FIG. 14 is a state in which a nozzle can is loaded into a vacuum chamber. FIG. 15 is a bubble test device for identifying the leak status of a defective nozzle can. Fig. 16 is a photograph showing a defective nozzle can generating bubbles inside a bubble test device. Specific details for implementing the invention

[0042] Specific structural or functional descriptions regarding embodiments according to the concept of the present invention disclosed in this specification are merely illustrative for the purpose of explaining embodiments according to the concept of the present invention. Since embodiments according to the concept of the present invention may be subject to various modifications and may take various forms, they include all modifications, equivalents, or substitutions that fall within the spirit and technical scope of the present invention. Furthermore, terms and words used in the specification and claims are not limited to their ordinary or dictionary meanings, and should be interpreted in a meaning and concept consistent with the technical spirit of the present invention, based on the understanding that the inventor may appropriately define the concept of the terms to best describe his invention. Accordingly, the embodiments described in the specification and the configurations illustrated in the drawings are merely one preferred embodiment of the present invention and do not represent all aspects of the technical spirit of the present invention; therefore, it should be understood that various equivalents and modifications capable of replacing them may be possible or exist at the time of filing the present invention.

[0043] Furthermore, unless otherwise defined in the specification of the present invention, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this specification.

[0045] The present invention relates to a method for manufacturing a fuel injection nozzle material using the HIP method, wherein the material is produced by sintering and joining Inconel powder and SKD 61 tool steel of different strengths using the HIP method, and a "sealed nozzle can" is manufactured by sealing the nozzle can to facilitate the joining of the dissimilar materials using vacuum brazing, and then the material is subjected to a HIP process.

[0046] In particular, the present invention relates to a method for innovatively improving the structure of a conventional nozzle can in the pre-vacuum brazing stage, which is the core of the high defect rate and low productivity of the production of the sealing nozzle can, so as to enable the simultaneous production of a large quantity of materials for fuel injection nozzles, thereby reducing the defect rate of the sealing nozzle can, which has long been over 30%, to 0% and dramatically improving productivity.

[0047] In the present invention, "nozzle can" refers to a product prior to the vacuum brazing process, which is introduced into the vacuum brazing process to create a "sealed nozzle can." The "sealed nozzle can" subsequently undergoes a HIP process to become a "material for fuel injection nozzles."

[0048] Conventional nozzle cans generally have a shape consisting of a can pipe having an inner diameter such that the processed SKD 61 tool steel is inserted and assembled into the center of the SKD 61 tool steel processed according to the shape of the fuel injection nozzle, and a can cap having a convex shape at the bottom that is fitted and fixed inside the upper side of the can pipe.

[0049] The first problem with the prior art was that filler material was used at the point where the lower end of the can pipe and the tool steel meet, but when applied as is, a large number of welding defects occurred. Without solving this problem, the defect rate of the product reached over 80%. Therefore, in the present invention, the problem was fundamentally prevented by joining the relevant part with argon welding (3510, 3520).

[0050] However, even after the above problem was resolved in the early stages, the defect rate exceeded an average of 30%, and although continuous efforts were made to resolve it for a long time, it could not be resolved. Nevertheless, production continued despite the high defect rate due to the advantage of being able to produce large quantities simultaneously.

[0051] To summarize, the structure of conventional nozzle cans had many potential defects, such as problems caused by scattering of filler metal powder during the degassing process, molten metal flowing down, problems caused by the excessive use of filler, and the fact that although there is a very small gap when viewed as a whole in the can cap seating area where the inner wall of the can pipe and the outer wall of the can cap are in contact, when viewed microscopically, the shape varies and the spacing differs.

[0052] Therefore, attempts have long been made to solve the problem by fine-tuning these various aspects. However, although there were some improvements, there were issues such as the fundamental difficulty in consistently maintaining 100% sealing of the molten metal due to the nature of the product, where a gap of less than 0.1% inevitably results in a defect. Consequently, all of these problems combined to result in a defect rate of over 30%. In other words, since a fundamental solution was difficult to achieve through conventional fine-tuning or efforts alone, the problem remained unresolved for a long time.

[0053] The present invention has innovatively improved the structure of the nozzle can to fundamentally solve the above problems in a completely different way.

[0054] The most critical component that enables the fundamental solution to the above problem in the nozzle can of the present invention is the formation of molten metal annular springs (3311, 3312, 3313, 3314, 3315, 3316, 3317).

[0055] In principle, the molten metal ring-shaped spring refers to the small space artificially created between the inner wall of the can pipe and the outer wall of the can cap at the top of the can cap seating portion in this invention. Ultimately, when the metal powder of the filler material melts, it collects in the molten metal ring-shaped spring. If the size of the molten metal ring-shaped spring is made somewhat generous, the molten metal can be prevented from overflowing at the source. Even if it overflows, it is not a problem because it fills the molten metal ring-shaped spring before overflowing. Of course, some of the molten metal seeps into the gap in the can cap seating portion, and it is desirable to control the amount so that it is typically 10 to 30% and 70 to 90% in the molten metal ring-shaped spring.

[0056] The process by which molten metal melts within a molten metal annular spring to form a continuous annular spring cannot be observed externally. However, its role and effects can be specifically distinguished.

[0057] First, even if the shape of the gap in the can cap seating area varies and the spacing is different, if 30% or less of the molten metal fills the gap and 70% or more of the molten metal forms a molten metal ring that is connected without interruption, 100% sealing can be achieved regardless of the shape of the can cap seating area or the spacing of the gap.

[0058] Second, it is possible to precisely adjust the amount of filler material used. This is because the phenomenon of molten metal flowing down the outer wall can be almost completely eliminated.

[0059] Third, it is possible to improve productivity by alleviating the burden of having to very sensitively machine the shape and spacing of the gap in the can cap seating area.

[0060] The molten metal ring spring shown in the drawing is as follows.

[0061] Looking at the molten metal piping formed in Figs. 6, 7, 8, 11, and 12, it can be seen that although the shapes vary, in all cases, the can cap wall is extended further from the upper end of the can cap seating portion, and the inner wall of the can pipe is also formed with a gap from the outer wall of the can cap at the upper end of the can cap seating portion, thereby forming a molten metal piping that allows molten metal to accumulate.

[0062] Therefore, anyone skilled in the art can expect the molten metal annular spring to have any variety of shapes, such as V or U.

[0063] In FIGS. 9 and 10, although the can cap wall is not extended further from the upper end of the can cap mounting section in a slightly modified form, it is also possible to form a molten metal phantom by cutting the can cap at an angle such that the upper end of the can cap is higher from the upper end of the outer wall of the can cap in contact with the upper end of the can cap mounting section to the upper end of the inner wall of the can cap. However, while this case can produce a similar effect, it is likely not frequently applied due to some disadvantages in terms of effectiveness and production costs. Ultimately, the technical concept of the molten metal phantom formed in FIGS. 6, 7, 8, 11, and 12 can be considered substantially equivalent.

[0064] Next, an important component adopted by the present invention is that the portion where the filler material is applied is located on the inner wall of the can pipe, separated from the top of the can cap seating portion by a certain distance. If the can cap is extended upward to form a molten metal ring, the filler material can naturally be applied to the upper part of the outer wall of the can cap, separated from the top of the can cap seating portion by a certain distance. Therefore, the essential significance of this component is, first, that the portion where the filler material is applied is separated from the top of the can cap seating portion by a certain distance to eliminate the potential for metal dust to scatter during degassing, and second, that the molten metal powder must naturally flow into the molten metal ring during melting; satisfying these two conditions results in a substantially identical outcome.

[0065] In other words, it is desirable to have a gap (hereinafter referred to as the "filler gap") (3411, 3412, 3413, 3414, 3415, 3416, 3417) between the top of the can cap seating area and the filler material application area. The focus mentioned here is to emphasize that it is undesirable for the filler material to be applied in a way that fills the top of the can cap seating area. A person skilled in the art can find an appropriate range for the gap mentioned above through implementation, provided they possess the new concept mentioned above.

[0066] In addition, it is desirable that the contact portion of the can cap seating part be formed as a surface in a cylindrical shape. In other words, if it is made in the shape of an annular line as in the embodiment shown in Drawing 8, it is significantly better than the prior art as shown in Example 6, but it also causes some defects.

[0067] Next, a component that the present invention selectively adopts is that the shape of the area where the filler material is applied can be varied in any way, allowing the worker to easily apply the filler material (Figs. 6 to 12).

[0068] Through this, all the problems examined in the “task to be solved” can be resolved.

[0069] The second problem mentioned, 'since the filler material consists of metal powder and an organic binder, the organic binder completely volatilizes and disappears while maintaining the first stage at approximately 400°C for about 5 hours in a vacuum chamber, leaving only the metal powder that has not yet reached its melting point in a solid state. At this time, the shape of the metal powder from which the organic solvent has been removed is not uniform, and the shape and spacing of the degassing gaps differ. In the case of conventional cases where the filler material was applied to the top of the can cap seating area, the metal powder tends to be scattered and lost in various forms during the degassing process because it is located in the path where gas leaks out during the degassing process,' and the fifth problem, 'it is difficult to reduce the defect rate even if one tries to apply a somewhat large amount of filler material,' are also resolved by "the part where the filler material is applied exists on the inner wall of the can pipe, separated from the top of the can cap seating area by a certain distance."

[0070] In addition, 'although there is a very small gap when viewed as a whole between the inner wall of the can pipe forming the can cap seating area and the outer wall of the can cap where they come into contact, it is almost impossible to make that gap uniform. Therefore, although the difference is small, the contact area and the area with a somewhat wider gap exist in an unpredictable state, which leads to a tendency for the scattering of solidified metal powder, pointed out as the second problem above, to be partially intensified by the skewed degassing airflow caused by the uneven spacing of the gap, and in particular, these factors become a significant cause for the molten metal powder not being able to uniformly and sufficiently fill all the gaps,' and

[0071] Fourth, problems such as “the difficulty in determining the appropriate amount of filler material. It is also difficult to gauge the unevenness of the gap between the metal powder that is scattered and falls off and the can cap’s seating area. In particular, there are many cases where molten metal powder flows down the outer wall of the can pipe and the inner wall of the can cap, and there is a tendency to solve the problem by applying as much filler material as possible for a long time to reduce defects in preparation for such cases” are all resolved by “forming a molten metal annular spring.”

[0072] Thanks to the aforementioned solution, innovative results were achieved where the defect rate practically approached zero.

[0073] Let's examine the examples.

[0074] [Prerequisites for Implementation of the Example]

[0075] ○ Brazing process conditions

[0076] Brazing is carried out in a vacuum furnace, and the vacuum level is maintained at 0.1 Torr after degassing from the first constant temperature stage.

[0077] 1. Temperature increase stage 1. Constant temperature stage 2. Temperature increase stage 2. Constant temperature stage Cold temperature stage temperature Room temperature → 400℃ 400℃ 400℃→1050℃ 1050℃ 1050℃→Room temperature hour 8.5 hours 5 hours 2.5 hours 2 hours 7 hours

[0078] ○ Types of nozzle cans to be inserted

[0079] For each run, nozzle cans of the following two types were introduced, with an equal number of 200 of each, for a total of 400 cans being introduced into the vacuum chamber.

[0080] Large nozzle can small nozzle can Outer diameter of the nozzle cap 23.2 ㎜ 19 ㎜ Product height 80 ㎜ 71 ㎜

[0081] The filler material used has an average volume ratio of 65% metal powder (Stainless Steel (STS / SUS) powder) and 35% organic binder.

[0082] ○ Defective product screening and inspection

[0083] Defect inspections of the nozzle cans were primarily conducted via visual inspection. Nozzle cans that passed the visual inspection proceeded to the HIP process normally, but some nozzle cans were found to be uncompressed despite having undergone the HIP process. This is because the sealing by the filler material was not properly performed, allowing air to re-enter after the brazing stage; this is a typical defect, and most defects are identified at this stage.

[0084] To specifically identify the cause of the defect, the aforementioned defective products undergo a test using the bubble test device shown in FIGS. 15 and 16 to determine the location and size of the welding defect. If the defect gap is large, a large number of bubbles are generated, and if the defect gap is small, small bubbles rise slowly.

[0085] Furthermore, through the above experiments and observations using a magnifying glass, efforts were made to identify the causes of defects in the defective products. While some causes of defects were easily identifiable, there were cases where they could not be easily identified even with the use of bubble tests and magnifying glasses. However, through consultations held at several expert meetings, the causes were eventually narrowed down to four categories and classified within those categories. Since this classification process served as an important foundation for creating the concept of the present invention, it can be concluded that this is a significant embodiment of the present invention.

[0086] The causes of welding defects were summarized as follows, and for all defects, the cause was determined from the following options and classified into the closest category.

[0087] Cause of Defect 1 (hereinafter referred to as "Cause of Defect 1"): Dispersion of metal powder from the filler material during degassing

[0088] Below, other causes of defects are also referred to as non-causes 2 to non-causes 5.

[0089] Non-perforation 2: A phenomenon in which a significant portion of the molten metal powder melts and overflows over the outer wall.

[0090] Problem 3: The phenomenon where the filler material seeps in unevenly due to the uneven gap in the can cap seating area.

[0091] Bulwon 4: Partial imbalance in the supply of filler material, resulting in shortages in certain areas

[0092] Unexpected 5: The above cases interact in combination

[0094] Examples 1 to 3 apply prior art or prior art with some improvements.

[0095] [Example 1]

[0096] A can cap is seated on a can pipe and a can case, and a filler material is applied to the upper part where the can cap and the can pipe come into contact (5011), and the lower part where the can pipe and the SKD 61 tool steel come into contact (5012) is also applied with a filler material so that the 5011 part and the 5012 part are welded by the filler material as shown in Drawing 5.

[0097] The nozzle cans loaded into the vacuum chamber consisted of 200 large nozzle cans and 200 small nozzle cans, and the above-described operating conditions were operated.

[0098] In this embodiment, an overwhelming 70% defect occurred in the part where the bottom of the can pipe and the SKD 61 tool steel come into contact (5012) and where the filler material is welded. Also, 37% defects occurred in the part where the can cap and the can pipe come into contact (5011) and where the filler material is welded.

[0099] This can be represented in a table as follows.

[0100] Large nozzle can small nozzle can total Number % Number % Number % Normal product 32 16 36 18 68 17 defective 168 84 164 82 332 83 Defect in part 5011 75 38 73 37 148 37 Defect in part 5012 142 71 138 69 280 70 (5011, 5012 defective) (49) (24) (47) (23) (96) (24)

[0101] In this embodiment, the classification by cause of defect involved analyzing only the defects in the 5011 section. This is because the analysis of the cause of defect itself is difficult, and in particular, the defects in the 5012 section are inevitably mass-produced due to difficulties in inserting filler material. Therefore, during the post-implementation analysis, it was determined that the 5012 section would subsequently be argon-welded. Accordingly, the following analysis of the cause of defect was conducted on 148 defective 2011 items among the defective products of this embodiment.

[0103] Large nozzle can small nozzle can total Number % Number % Number % Defect in part 5011 75 100 73 100 148 100 Soon 1 46 61 44 60 90 61 Soon 2 34 45 32 44 66 45 Soon 3 14 19 11 15 25 17 Soon 4 25 33 22 30 47 32 (2 or more combinations) (36) (48) (47) (23) (96) (24)

[0105] [Example 2]

[0106] The can cap is seated on the can pipe, and the upper portion (5011) where the can cap and the can pipe meet is coated with a filler material as shown in Drawing 5, so that it is ultimately sealed by the filler material.

[0107] However, unlike Example 1, the part (5012) where the bottom of the can pipe and the SKD 61 tool steel come into contact was argon welded in advance before entering the vacuum chamber. In all subsequent examples, this part or the corresponding part was also argon welded in advance before entering the vacuum chamber.

[0108] The amount of filler material used was 0.5g for the 5011 portion of the large nozzle can and 0.35g for the 5011 portion of the small nozzle can.

[0109] The amount of product that went into the vacuum chamber was 200 large nozzle cans and 200 small nozzle cans.

[0110] In this embodiment, 38% of defects were found in the filler welding portion at the part (5011) where the can cap and the can pipe meet. There were no defects in other parts.

[0111] This can be represented in a table as follows.

[0112] Large nozzle can small nozzle can total Number % Number % Number % Normal product 122 61 128 18 250 62.5 defective 78 39 72 36 150 37.5

[0114] The cause of the defect in the above 5011 section was analyzed, and the details are as follows.

[0115] Large nozzle can small nozzle can total Number % Number % Number % Defect in part 5011 78 100 72 100 150 100 Soon 1 47 60 45 63 92 61 Soon 2 22 28 31 43 65 43 Soon 3 19 24 13 18 32 21 Soon 4 24 31 20 28 44 29 (2 or more combinations) (32) (41) (44) (61) (76) (51)

[0117] [Example 3]

[0118] The procedure was carried out under the same conditions as Example 2, but the amount of filler material used was increased. For large nozzle cans, the amount was increased from 0.5g to 0.7g, and for small nozzle cans, the amount was increased from 0.35g to 0.5g.

[0119] The amount of product that went into the vacuum chamber was 200 large nozzle cans and 200 small nozzle cans.

[0120] In this embodiment, 29.5% of defects were found in the filler welding portion at the part (5011) where the can cap and the can pipe meet. There were no defects in other parts.

[0121] This can be represented in a table as follows.

[0122] Large nozzle can small nozzle can total Number % Number % Number % Normal product 138 69 144 72 282 70.5 defective 62 31 56 28 118 29.5

[0123] The cause of the defect in the above 5011 section was analyzed, and the details are as follows.

[0124] Large nozzle can small nozzle can total Number % Number % Number % Defect in part 5011 62 100 56 100 118 100 Soon 1 39 63 35 62 74 63 Soon 2 35 56 31 55 66 56 Soon 3 13 21 11 18 24 20 Soon 4 5 8 4 7 9 8 (2 or more combinations) (31) (50) (27) (48) (58) (49)

[0126] The following Examples 4 to 6 apply the concept of the present invention.

[0128] [Example 4]

[0129] It was manufactured and implemented using the structure of the nozzle can disclosed in Drawing 7. The specific features of the configuration of Drawing 7 are described as follows. It has a molten metal annular spring (3312). In particular, the molten metal annular spring (3312) is structurally formed on the upper part connected to the can cap seating portion (3113). The inner wall of the can pipe is formed long upwards, and the outer wall of the can cap is formed very close to the inner wall of the can pipe, thereby forming a can cap seating portion where air passes through but the passage of liquid is significantly suppressed. On the upper part of the can cap seating portion, the molten metal annular spring (3312) is formed in a V-shape. Next, an important point is that a portion (5022) for applying filler material is formed at a certain distance from the upper part of the can cap seating portion and the molten metal annular spring (3312). Drawings 6, 11, and 12 can be considered substantially identical.

[0130] The number of nozzle cans to be applied was 200 large nozzle cans and 200 small nozzle cans, and the amount of filler material applied was 0.6g to the large nozzle cans and 0.4g to the small nozzle cans.

[0131] The result of the experiment was that no defective products were produced.

[0132] Large nozzle can small nozzle can total Number % Number % Number % Normal product 200 100 200 100 400 100 defective 0 0 0 0 0 0

[0134] [Example 5]

[0135] The procedure was carried out as in Example 4, but with the concept described in Drawing 6 applied to the nozzle can.

[0136] The number of nozzle cans to be applied was 200 large nozzle cans and 200 small nozzle cans, and the amount of filler material applied was 0.6g to the large nozzle cans and 0.4g to the small nozzle cans.

[0137] The result of the experiment was that no defective products were produced.

[0138] Large nozzle can small nozzle can total Number % Number % Number % Normal product 200 100 200 100 400 100 defective 0 0 0 0 0 0

[0140] [Example 6]

[0141] A nozzle can was manufactured and implemented by applying the concept described in Figure 8. The difference between Figure 6 or Figure 7 and Figure 8 is that in Figure 6 or Figure 7, the can cap seating portion has a circular surface contact with a certain width, whereas in Figure 8, it takes the form of an almost circular line contact.

[0142] The number of nozzle cans to be applied was 200 large nozzle cans and 200 small nozzle cans, and the amount of filler material applied was 0.6g to the large nozzle cans and 0.4g to the small nozzle cans.

[0143] A significant number of defects occurred.

[0144] Large nozzle can small nozzle can total Number % Number % Number % Normal product 188 94 192 96 380 95 defective 12 6 8 4 20 5

[0146] The causes of the above defects were analyzed, and the details are as follows.

[0147] Large nozzle can small nozzle can total Number % Number % Number % error 12 100 8 100 20 100 Soon 1 0 0 0 0 0 0 Soon 2 0 0 0 0 0 0 Soon 3 12 100 8 100 20 100 Soon 4 12 100 8 100 20 100 (2 or more combinations) (12) (100) (8) (100) (20) (100)

[0149] [Example 7]

[0150] A nozzle can was manufactured and implemented by applying the concept described in Drawing 10. The difference between Drawing 6 or Drawing 7 and Drawing 10 is as follows.

[0151] It is identical in that a molten metal annular spring (3315) is formed. Structurally, it is formed on the upper part connected to the can cap seating portion (3116). While Figure 6 or Figure 7 has a V or U-shaped groove to form a space to receive and contain molten metal flowing down between the inner wall of the can pipe and the outer wall of the can cap, Figure 10 has no groove shape using the outer wall of the can cap; instead, the molten metal annular spring (3315) is formed by cutting diagonally upward from the outer wall of the can cap to the inner wall of the can cap to create a concave shape.

[0152] The number of nozzle cans to be applied was 200 large nozzle cans and 200 small nozzle cans, and the amount of filler material applied was 0.6g to the large nozzle cans and 0.4g to the small nozzle cans.

[0153] A significant number of defects occurred.

[0154] Large nozzle can small nozzle can total Number % Number % Number % Normal product 195 97.5 196 98 391 97.7 defective 5 2.5 4 2 9 2.3

[0155] The causes of the above defects were analyzed, and the details are as follows.

[0156] Large nozzle can small nozzle can total Number % Number % Number % error 5 100 4 100 9 100 Soon 1 0 0 0 0 0 0 Soon 2 5 100 4 100 9 100 Soon 3 2 40 2 50 4 44 Soon 4 1 20 2 50 3 33 (2 or more combinations) (3) (60) (3) (60) (6) (66) Explanation of the symbols

[0158] 10. SKD 61 Tool Steel 20. Inconel Powder 30. Can 31. Can pipe 3111, 3112, 3113, 3114, 3115, 3116, 3117, 3118 Can cap seating area 3120 Can pipe exterior wall 3130 Can pipe inner wall 32. Can cap 3210 Can Cap Inner Wall 3220 Can Cap Outer Wall 3221 Upper part of can cap outer wall 3222 Lower part of can cap outer wall 3223 Corner part of can cap outer wall 3230 Can cap opening edge 3311, 3312, 3313, 3314, 3315, 3316, 3317 Molten metal annular source 3411, 3412, 3413, 3414, 3415, 3416, 3417 Filler material spacing (distance between the molten metal annular spring and the filler material attachment point) 3510, 3520 Argon Welded Area 40 nozzle cans 50 Dragon Lobster 5011 Filler material located above the point where the top of the outer wall of the can cap and the top of the inner wall of the can pipe meet in the prior art 5012 Filler material located at the contact point between the bottom of the thinned surface of the can pipe and the SKD 61 tool steel of the prior art 5021, 5022, 5023, 5024, 5025, 2026, 2027 Filler material attachment part and filler material of embodiments of the present invention 60 vacuum chambers 61 Base 62 Heating element 63 Vacuum pump 70 Fuel injection nozzle 80 bubble test device 8010 Bubble test container 8011 Vent valve 8012 Pressure Gauge 8013 Vacuum Pump 8020 Glycerin 9010 Normal processing nozzle can 9020 Defective processing nozzle can 9021 Bubbles generated from a leak

Claims

Claim 1 A plurality of sealed nozzle cans manufactured simultaneously by a brazing process comprising: a first heating step of raising the temperature to a predetermined temperature between 350 and 550°C after introducing a plurality of nozzle cans into a vacuum chamber capable of forming a vacuum of at least 1 Torr; a first constant temperature step of performing a degassing process to form a vacuum of at least 1 Torr while maintaining the predetermined temperature between 350 and 550°C for a predetermined time between 3 and 6 hours; a second heating step of subsequently raising the temperature to a predetermined temperature between 950 and 1150°C; a second constant temperature step of maintaining the predetermined temperature between 950 and 1150°C for a predetermined time between 1 and 3 hours; and a subsequent cooling step of lowering the temperature; wherein the nozzle can comprises SKD 61 tool steel; a can pipe assembled with the SKD 61 tool steel inserted therein; and Inconel powder introduced in a predetermined amount through the open top of the can pipe in accordance with the specifications of the SKD 61 tool steel. A nozzle can introduced into a brazing process for simultaneously manufacturing multiple sealed nozzle cans, comprising: a can cap formed with a convex shape at its lower end and fitted and fixed inside the upper side of the can pipe; a can cap seating portion formed by contact between the inner wall of the can pipe and the lower part of the outer wall of the can cap; a filler material attachment portion located on the inner wall of the can pipe, such that the height of the upper end of the can pipe is higher than the height of the upper end of the can cap, and the portion for applying filler material is positioned on the inner wall of the can pipe, separated by a range of 1 to 5 mm above the upper end of the can cap seating portion; a portion where the lower end of the can pipe contacts the SKD 61 tool steel; and a molten metal annular spring formed by creating a space between the inner wall of the can pipe and the outer wall of the can cap on the upper part of the can cap seating portion, so that molten metal originating from the filler material in the filler material attachment portion can flow down and accumulate in an annular shape during the brazing process. Claim 2 A nozzle can introduced into a brazing process for simultaneously manufacturing a plurality of sealed nozzle cans, wherein, in claim 1, the upper part of the can cap seating portion is welded by filler material and the portion where the lower end of the can pipe contacts the SKD 61 tool steel is welded by argon welding. Claim 3 delete Claim 4 delete Claim 5 A nozzle can introduced into a brazing process for simultaneously manufacturing a plurality of sealed nozzle cans, wherein the part of the filler material attachment portion is engraved with a semicircle or triangle shape into the inner wall of the can pipe, in the first paragraph. Claim 6 delete Claim 7 A nozzle can introduced into a brazing process for simultaneously manufacturing a plurality of sealed nozzle cans, wherein, in claim 1, the amount of molten metal accumulating in the molten metal annular spring is greater than the amount of molten metal seeping into the can cap seating portion. Claim 8 In claim 7, a nozzle can introduced into a brazing process for simultaneously manufacturing a plurality of sealed nozzle cans, wherein the amount of molten metal accumulating in the molten metal annular spring is 70 to 90 weight percent of the total molten metal. Claim 9 A nozzle can introduced into a brazing process for simultaneously manufacturing a plurality of sealed nozzle cans formed in a cylindrical shape with the can cap seating portion in surface contact, in accordance with claim 1. Claim 10 A nozzle can introduced into a brazing process for simultaneously manufacturing a plurality of sealed nozzle cans, wherein, in claim 1, the height of the top of the can cap is higher than the height of the top of the can pipe and the filler material attachment part is located on the upper part of the outer wall of the can cap, which is higher than the top of the can pipe.

Citation Information

Patent Citations

  • Manufacturing method of material for fuel injection nozzle using hip processing

    KR100899780B1