Catalyst layer, membrane electrode assembly for solid polymer fuel cell, and solid polymer fuel cell

The catalyst layer in solid polymer fuel cells optimizes platinum usage by using carbon-supported platinum with controlled ionomer distribution, enhancing catalytic activity and output while reducing catalyst amounts.

KR103046625B1Active Publication Date: 2026-11-10AGC INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020227021536
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-24
Filing Date
2020-12-18
Publication Date
2026-11-10
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing solid polymer fuel cells face the challenge of achieving high output while minimizing the use of expensive platinum catalysts, as conventional methods to uniformly coat catalyst particles with ionomer often lead to reduced catalytic activity due to ionomer poisoning.

Method used

A catalyst layer is designed with platinum-containing catalyst supported on carbon, featuring mesopores with specific pore diameters and ionomer distribution, reducing direct contact between ionomer and platinum to maintain catalytic activity while optimizing ionomer content and catalyst usage.

Benefits of technology

The catalyst layer enables high fuel cell output with reduced platinum usage by forming a pseudo-three-phase interface, effectively utilizing platinum catalytic activity and minimizing ionomer penetration into mesopores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022065892413-PCT00008_ABST
    Figure 112022065892413-PCT00008_ABST
Patent Text Reader

Abstract

A catalyst layer comprising a catalyst-supported carbon in which a platinum-containing catalyst is supported on a carbon carrier, and an ionomer, wherein the catalyst-supported carbon has mesopores with a pore diameter of 2 nm or more and less than 10 nm in a pore distribution obtained by nitrogen adsorption, at least a portion of the ionomer exists within the mesopores with a pore diameter of 2 nm or more and less than 10 nm, the ionomer content per 100 parts by mass of the carbon carrier is 100 parts by mass or more, and the ionomer share of the total volume of the mesopores with a pore diameter of 2 nm or more and less than 10 nm is 50 volume% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a catalyst layer, a membrane electrode assembly for a solid polymer fuel cell, and a solid polymer fuel cell. Background Technology

[0002] A solid polymer fuel cell is, for example, formed by placing a membrane electrode assembly between two separators to form a cell, and stacking multiple cells.

[0003] In addition, the membrane electrode assembly comprises, for example, an anode having a catalyst layer and a gas diffusion layer, a cathode having a catalyst layer and a gas diffusion layer, and a polymer electrolyte membrane disposed between the anode and the cathode.

[0004] The catalyst layer used in the anode and cathode comprises, for example, a catalyst support formed by supporting a catalyst on a support, and an ionomer which is a polymer electrolyte.

[0005] Since platinum, which is mainly used as a catalyst, is expensive, it is desired to reduce the amount of catalyst used. Therefore, in order to utilize the catalyst efficiently, attempts are being made to increase the output of fuel cells while reducing the amount of catalyst used by coating as many catalyst particles as uniformly as possible with an ionomer (e.g., Patent Documents 1 to 3, etc.). Prior art literature

[0006] Japanese Published Patent Application No. 2010-167379, Japanese Published Patent Application No. 2010-186678, Japanese Published Patent Application No. 2011-081977 The problem to be solved

[0007] As mentioned above, conventionally, it has been thought that in order to achieve both a reduction in catalyst usage and high output of fuel cells, it is necessary to coat as many catalyst particles as uniformly as possible with ionomer in order to form a wide three-phase interface of the catalyst, ionomer, and water, which are the reaction sites in the catalyst layer.

[0008] However, when using a catalyst containing platinum, there is a need to increase the output of the fuel cell while reducing the amount of catalyst used.

[0009] The present disclosure is made in consideration of the above circumstances and aims to provide a catalyst layer that enables high output of a fuel cell while reducing the amount of catalyst used when used in a solid polymer fuel cell, a membrane electrode assembly for a solid polymer fuel cell using said catalyst layer, and a solid polymer fuel cell having said membrane electrode assembly for a solid polymer fuel cell. means of solving the problem

[0010] The specific means for achieving the above task are as follows.

[0011] <1> A catalyst-supported carbon in which a platinum-containing catalyst is supported on a carbon support, and a catalyst layer containing an ionomer, and

[0012] The above catalyst-supported carbon has mesopores with a pore diameter of 2 nm or more and less than 10 nm in the pore distribution obtained by nitrogen adsorption,

[0013] At least a portion of the above ionomer exists within the above mesopores with a pore diameter of 2 nm or more and less than 10 nm, and

[0014] The content of the ionomer per 100 parts by mass of the carbon carrier is 100 parts by mass or more, and

[0015] A catalyst layer in which the ionomer occupies 50 volume% or less of the total volume of mesopores with a pore diameter of 2 nm or more and less than 10 nm.

[0016] <2> The catalyst-supported carbon in the catalyst layer is a catalyst layer described in <1> having at least 0.03 cm³ / g of macropores with a pore diameter of 50 nm or more in a pore distribution obtained by nitrogen adsorption method, in a state where the ionomer is attached.

[0017] <3> A catalyst layer described in <1> or <2>, wherein the content of the catalyst per unit area of ​​the catalyst layer is 0.2 mg / cm² or less.

[0018] <4> The catalyst described above is a catalyst layer described in any one of <1> to <3>, comprising at least one type selected from the group consisting of platinum particles and platinum alloy particles.

[0019] <5> A catalyst layer described in <4>, wherein the number average particle size of the catalyst is 1 nm to 20 nm.

[0020] <6> A catalyst layer described in any one of <1> to <5>, wherein the content of the catalyst relative to the total catalyst-supported carbon is 10 mass% to 70 mass%.

[0021] <7> An anode having a first gas diffusion layer and a first catalyst layer formed on one side of the first gas diffusion layer, and

[0022] A cathode having a second gas diffusion layer and a second catalyst layer formed on one side of the second gas diffusion layer, and

[0023] A polymer electrolyte membrane disposed between the first catalyst layer and the second catalyst layer, and

[0024] A membrane electrode assembly for a solid polymer fuel cell, wherein at least one of the first catalyst layer and the second catalyst layer is a catalyst layer described in any one of <1> to <6>.

[0025] A solid polymer fuel cell having a membrane electrode assembly for a solid polymer fuel cell as described in <8> and <7>. Effects of the invention

[0026] According to the present disclosure, a catalyst layer that enables high output of a fuel cell while reducing the amount of catalyst used by using it in a solid polymer fuel cell, a membrane electrode assembly for a solid polymer fuel cell using said catalyst layer, and a solid polymer fuel cell having said membrane electrode assembly for a solid polymer fuel cell can be provided. Brief explanation of the drawing

[0027] FIG. 1 is a schematic cross-sectional view showing an example of a membrane electrode assembly for a solid polymer fuel cell. Specific details for implementing the invention

[0028] The following describes in detail the forms for carrying out the present disclosure. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not mandatory unless specifically stated otherwise. The same applies to numerical values ​​and their ranges, and this does not limit the present disclosure.

[0029] In this specification, the term "process" includes, in addition to processes independent from other processes, processes that cannot be clearly distinguished from other processes, provided that the purpose of such processes is achieved.

[0030] In the numerical range indicated using “∼” in this specification, the numerical values ​​listed before and after “∼” are included as the minimum value and the maximum value, respectively.

[0031] In this specification, each component may include multiple types of the corresponding substance. If multiple types of the substance corresponding to each component exist in the composition, the content or content of each component refers to the content or content of the total of the multiple types of substances present in the composition, unless specifically stated otherwise.

[0032] When embodiments are described in this specification with reference to the drawings, the configuration of said embodiment is not limited to the configuration shown in the drawings. Furthermore, the sizes of the components in each drawing are conceptual, and the relative relationships of sizes between components are not limited thereto.

[0033] [Catalyst layer]

[0034] The catalyst layer in the present embodiment is a catalyst layer containing a catalyst-supported carbon in which a platinum-containing catalyst is supported on a carbon carrier, and an ionomer.

[0035] A mesopore generally refers to a pore with a diameter of 2 nm or more and less than 50 nm, but in the present embodiment, among them, an ionomer occupying a specific proportion of volume exists within a mesopore with a diameter of 2 nm or more and less than 10 nm. That is, the catalyst-supported carbon has mesopores with a diameter of 2 nm or more and less than 10 nm in the pore distribution obtained by nitrogen adsorption, at least a portion of the ionomer exists within the mesopores with a diameter of 2 nm or more and less than 10 nm, the content of the ionomer relative to 100 parts by mass of the carbon carrier is 100 parts by mass or more, and the share of the ionomer in the total volume of the mesopores with a diameter of 2 nm or more and less than 10 nm is 50 volume% or less.

[0036] Hereinafter, the pore distribution obtained by the nitrogen adsorption method is simply referred to as the "pore distribution," pores of 2 nm or more and less than 50 nm are referred to as "mesopores," mesopores with a pore diameter of 2 nm or more and less than 10 nm in the pore distribution are referred to as "specific mesopores," and the share of ionomer in the total volume of specific mesopores is referred to as the "ionomer share." In addition, the term "macropore" described below refers to a pore with a pore diameter of 50 nm or more and less than 300 nm.

[0037] The above "pore distribution" is obtained by performing analysis by the BJH method on the sample to be measured using an automatic specific surface area / pore distribution measuring device (e.g., manufactured by Shimadzu Corporation, model number: TriStar II 3020, measurement method: nitrogen adsorption method by fixed volume method). In addition, the specific surface area and pore capacity for the catalyst-supported carbon described below are calculated from the above pore distribution.

[0038] In addition, the "ionomer occupancy rate" is a value represented by the following equation (1), where P1 is the total volume of specific mesopores obtained by performing the above measurement and analysis on a sample of catalyst-supported carbon to which an ionomer is attached, and P0 is the total volume of specific mesopores obtained by performing the above measurement and analysis on a sample of catalyst-supported carbon to which an ionomer is not attached. In addition, the total volume of specific mesopores refers to the total pore area of ​​specific mesopores.

[0039] Ionomer share (volume %) = (P0 - P1) × 100 / P0‥‥ (1)

[0040] In addition, as a sample of the catalyst-supported carbon to which the above-mentioned ionomer is attached, for example, a coating solution for forming a catalyst layer is applied onto a substrate film such as a PET film, and a coating layer is formed by drying at 80°C to remove the solvent, and the obtained coating layer is scraped off to form a powder.

[0041] In addition, as a sample of catalyst-supported carbon that does not have the above-mentioned ionomer attached, for example, a mixture of catalyst-supported carbon and a solvent is applied onto a substrate film such as a PET film, dried to remove the solvent to form a coating layer, and the obtained coating layer is scraped off to form a powder. Here, "PET" refers to polyethylene terephthalate. Furthermore, it is preferable that the above-mentioned mixture undergoes the same mixing treatment as the mixing treatment (e.g., mixing treatment by a bead mill) performed during the process of preparing the coating solution for forming the catalyst layer.

[0042] By using the above catalyst layer in a solid polymer fuel cell, high output of the fuel cell is realized while reducing the amount of catalyst used. Although the reason is not certain, it is speculated as follows.

[0043] A specific mesopore has a large pore surface area relative to its pore capacity. Consequently, the surface area of ​​a carbon support having a specific mesopore becomes very large. For example, even in a carbon support where the ratio of the total pore capacity of the specific mesopore to the total pore capacity of the mesopores and macropores in the carbon support is about 30%, the ratio of the total pore surface area of ​​the specific mesopore to the total pore surface area of ​​the mesopores and macropores in the carbon support may exceed 85%. In short, in a catalyst-supported carbon in which a platinum-containing catalyst particle is supported on the surface of a carbon support, there is also catalyst supported on surfaces other than the pores of the carbon support or on the surface of the macropores, but it is thought that most of the catalyst is supported on the surface of the specific mesopore.

[0044] For this reason, conventionally, in order to bring the ionomer into contact with as many catalysts as possible, attempts have been made to bring the catalyst inside the pores into contact with the ionomer by allowing the ionomer to penetrate into the pores.

[0045] However, it was found that when an ionomer comes into contact with platinum catalyst particles, the ionomer is poisoned by the acidic functional groups of the ionomer, and the catalytic activity of the platinum is actually reduced.

[0046] Therefore, in the catalyst layer of the present embodiment, the content of the ionomer relative to 100 parts by mass of the carbon support is 100 parts by mass or more, and at least a portion of the ionomer exists in specific mesopores, so that the ionomer share is 50 volume% or less. In the catalyst layer of the present embodiment, the ionomer surrounding the catalyst-supported carbon is surrounded by a sufficient amount of ionomer, while the amount of ionomer penetrating into the specific mesopores is reduced. The ionomer surrounding the catalyst-supported carbon but not penetrating into the specific mesopores is in a state of close proximity without contact with the catalyst supported inside the specific mesopores. The ionomer in the state of close proximity without contact is thought to form a pseudo-three-phase interface through water in the reaction gas (e.g., hydrogen, oxygen, etc. used for battery operation) or water generated by the reaction. It is thought that, by doing so, the catalytic activity of platinum can be effectively utilized through the formation of a pseudo-three-phase interface while suppressing the decrease in platinum catalytic activity caused by the ionomer's direct contact with platinum.

[0047] For the reasons above, it is presumed that in the catalyst layer of the present embodiment, high output of the fuel cell is realized while reducing the amount of catalyst used.

[0048] Below, each component constituting the catalyst layer is described individually.

[0049] <Catalyst-supported carbon>

[0050] The catalyst-supported carbon comprises a carbon support having specific mesopores and a catalyst supported on the carbon support and containing platinum. The carbon support and the catalyst are described separately below.

[0051] The carbon carrier is not specifically limited to carbon having at least a certain mesopore.

[0052] Examples of carbon carriers include activated carbon and carbon black. Due to their high chemical durability, it is desirable to perform at least partial graphitization through heat treatment or the like. Additionally, regarding the carbon carrier, mesoporous carbon is preferred in that, from the perspective of keeping the ionomer share low, the ratio of the total pore capacity occupied by macropores is less than 40% relative to the total pore capacity of mesopores and macropores combined. The ratio of the total pore capacity occupied by macropores is preferably 5 to 35%, and more preferably 10 to 30%.

[0053] As for the catalyst, it is not particularly limited as long as it includes platinum and promotes the redox reaction in a solid polymer fuel cell. It is preferable that the catalyst be at least one selected from the group consisting of platinum and platinum alloys, and more preferable that it include at least one selected from the group consisting of platinum particles and platinum alloy particles.

[0054] As for the platinum alloy, an alloy of platinum with one or more metals selected from the group consisting of platinum group metals excluding platinum (ruthenium, rhodium, palladium, osmium, iridium), gold, silver, chromium, iron, titanium, manganese, cobalt, nickel, molybdenum, tungsten, aluminum, silicon, zinc, and tin is preferred. The platinum alloy may include an intermetallic compound of the metal alloyed with platinum and platinum.

[0055] When the catalyst comprises at least one type selected from the group consisting of platinum particles and platinum alloy particles, the number average particle size of the catalyst can be, for example, in the range of 1 nm to 20 nm, and from the perspective of power generation performance and catalyst durability, a range of 2 nm to 10 nm is preferred, and a range of 2 nm to 7 nm is more preferred.

[0056] In addition, the number average particle size of the above catalyst is a value obtained by number averaging the circle equivalent diameters obtained for 300 to 400 particles in an image observed at 300,000x magnification using a transmission electron microscope (TEM) HT7700 manufactured by Hitachi High Technologies Co., Ltd.

[0057] The method of supporting a catalyst on a carbon support is not particularly limited, and known methods such as sputtering, solution method, electrolytic deposition method, and electroless plating method are used.

[0058] The content of the catalyst relative to the total catalyst-supported carbon can range, for example, from 10 mass% to 70 mass%, and from the perspective of achieving both a reduction in catalyst usage and high output, a range of 20% to 60% is preferred, and a range of 30% to 60% is more preferred.

[0059] The catalyst content per unit area of ​​the catalyst layer is preferably 0.01 mg / cm² to 0.50 mg / cm² in terms of the optimal thickness of the catalyst layer for efficiently carrying out the electrode reaction, and more preferably 0.05 mg / cm² to 0.35 mg / cm² in terms of the balance between raw material cost and performance. In particular, since the catalyst layer of the present embodiment can achieve high output while reducing the amount of catalyst used, the catalyst content per unit area of ​​the catalyst layer may be 0.20 mg / cm² or less.

[0060] The specific surface area of ​​the entire catalyst-supported carbon is preferably in the range of 200 m² / g catalyst or more, and more preferably in the range of 250 m² / g catalyst or more, for example, from the perspective of achieving both a reduction in catalyst usage and high output. In addition, the specific surface area of ​​the entire catalyst-supported carbon refers to the total surface area of ​​the catalyst-supported carbon per unit mass in a state where no ionomer is attached.

[0061] In addition, the total specific surface area of ​​the catalyst-supported carbon may be 700 m² / g or less, 500 m² / g or less, or 350 m² / g or less.

[0062] The total specific surface area of ​​the catalyst-supported carbon is measured by nitrogen adsorption on the carbon surface using a BET specific surface area device.

[0063] The specific surface area of ​​mesopores in the catalyst-supported carbon is preferably in the range of 200 m² / g or more, and more preferably in the range of 250 m² / g or more, from the perspective of achieving both a reduction in catalyst usage and high output. In addition, the specific surface area of ​​mesopores in the catalyst-supported carbon refers to the total pore surface area of ​​mesopores in the catalyst-supported carbon per unit mass in a state where no ionomer is attached. Furthermore, the specific surface area of ​​the entire catalyst-supported carbon may be 700 m² / g or less, 500 m² / g or less, or 350 m² / g or less.

[0064] The specific surface area of ​​a specific mesopore in the catalyst-supported carbon is more preferably in a range of 200 m² / g catalyst or higher, for example, from the perspective of achieving both a reduction in catalyst usage and high output. In addition, the specific surface area of ​​a specific mesopore in the catalyst-supported carbon refers to the total pore surface area of ​​the specific mesopore in the catalyst-supported carbon per unit mass in a state where no ionomer is attached.

[0065] The total pore capacity of specific mesopores per unit mass of catalyst-supported carbon without attached ionomer can be, for example, in the range of 0.1 cm³ / g catalyst to 0.8 cm³ / g catalyst, and from the perspective of gas diffusivity and power generation performance, a range of 0.15 cm³ / g catalyst to 0.7 cm³ / g catalyst is preferred, and a range of 0.2 cm³ / g catalyst to 0.6 cm³ / g catalyst is more preferred.

[0066] The ratio of the total pore capacity of a specific mesopore to the total pore capacity of the mesopores and macropores in the catalyst-supported carbon without attached ionomer can be, for example, in the range of 20% to 90%, and in terms of the drainage and power generation performance of the generated water, a range of 25% to 80% is preferred, and a range of 30% to 70% is more preferred.

[0067] The total pore capacity of macropores per unit mass of catalyst-supported carbon without attached ionomer can be, for example, in the range of 0.05 cm³ / g catalyst or higher, and from the perspective of achieving both reduction in catalyst usage and high output, a range of 0.07 cm³ / g catalyst to 0.50 cm³ / g catalyst is preferred, and a range of 0.1 cm³ / g catalyst to 0.4 cm³ / g catalyst is more preferred.

[0068] <Ionomer>

[0069] The ionomer is not specifically limited to any polymer compound having an ion exchange group, but among them, a polymer compound having proton conductivity is preferred. Hereinafter, a polymer compound having an ion exchange group is also referred to as an "ion exchange resin." An "ion exchange group" refers to H + It refers to a group having , 1-valent metal cations, ammonium ions, etc.

[0070] Examples of ion exchangers include sulfonic acid groups, sulfonimide groups, sulfonamide groups, sulfonmethide groups, carboxyl groups, and phosphate groups, among which sulfonic acid groups with excellent proton conductivity are preferred. One type of ion exchanger is used alone or in combination of two or more types.

[0071] As for the ionomer, a fluorine-containing ion exchange resin is preferred in terms of durability, and a perfluorocarbon polymer having ion exchange groups is more preferred. In addition, the perfluorocarbon polymer may include etheric oxygen atoms.

[0072] Examples of the perfluorocarbon polymer include known polymers such as the polymer (H) described below, the polymer (Q) described below, and polymers having constituent units derived from perfluoro monomers having ion exchange groups and five-membered rings, as described in International Publication No. 2011 / 013577, etc. For ease of availability and ease of manufacturing, the ionomer preferably comprises at least one type selected from the group consisting of polymer (H) and polymer (Q).

[0073] Furthermore, "polymer" refers to a compound having a structure composed of multiple constituent units. Also, "constituent unit" refers to a unit derived from a monomer formed by the polymerization of the monomer. A constituent unit may be a unit directly formed by the polymerization reaction of the monomer, or a unit in which a portion of the unit is converted into a different structure by processing the polymer. "Monomer" refers to a compound having a polymerizable carbon-carbon double bond.

[0074] Polymer (H) :

[0075] Polymer (H) is a polymer having the following unit (U1) (excluding polymer (Q)).

[0076] [Chemical Formula 1]

[0077]

[0078] However, among the above units (U1), Q 3 It is a perfluoroalkylene group that may have a single bond or an etheric oxygen atom, and R f2 is a perfluoroalkyl group that may have an etheric oxygen atom, and X 2 is an oxygen atom, a nitrogen atom, or a carbon atom, and b is X 2 If is an oxygen atom, it is 0, and X 2 If is a nitrogen atom, it is 1, and X 2 If is a carbon atom, it is 2, and Y 2is a fluorine atom or a monovalent perfluoroorganic group, and t is 0 or 1. The single bond is CFY 2 It means that the carbon atom of SO2 is directly bonded to the sulfur atom of SO2. An organic group means a group containing one or more carbon atoms.

[0079] Q in the above unit (U1) 3 When the perfluoroalkylene group represented by has an etheric oxygen atom, the oxygen atom may be one or two or more. Also, the oxygen atom may be inserted between the carbon-carbon bonds of the perfluoroalkylene group or inserted at the ends of the carbon bonds.

[0080] The perfluoroalkylene group may be in a straight chain form or a branched form.

[0081] The number of carbon atoms in the perfluoroalkylene group is preferably 1 to 6, and more preferably 1 to 4.

[0082] R in the above unit (U1) f2 The perfluoroalkyl group represented by may be of the straight chain type or the branched type, and it is preferable that it be of the straight chain type.

[0083] The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 6, and more preferably 1 to 4. As for the perfluoroalkyl group, perfluoromethyl groups, perfluoroethyl groups, etc. are preferred.

[0084] Among the above units (U1), -(SO2X 2 (SO2R f2 ) b ) - H + The device is an ion exchanger.

[0085] -(SO2X in the above unit (U1) 2 (SO2R f2 ) b ) - H + The path is, sulfonic acid group (-SO3 - H +group), sulfonimide group (-SO2N(SO2R f2 ) - H + group), or sulfonated group (-SO2C(SO2R f2 )2) - H + Can be cited as (e.g.,

[0086] Y in the above unit (U1) 2 In this case, a fluorine atom or a trifluoromethyl group is preferred.

[0087] As for the unit (U1), the following unit (U1-1) is preferred, and the following units (U1-11), (U1-12), (U1-13), or (U1-14) are more preferred in that the polymer (H) is easy to manufacture and easy to industrially implement.

[0088] [Chemical Formula 2]

[0089]

[0090] However, among the above units (U1-1), Z is a fluorine atom or a trifluoromethyl group, t is 0 or 1, m is an integer from 0 to 3, n is an integer from 1 to 12, p is 0 or 1, and also m + p > 0.

[0091] The polymer (H) may additionally have a constituent unit derived from another monomer (hereinafter referred to as "other unit"). The ratio of the other unit may be appropriately adjusted so that the ion exchange capacity of the polymer (H) becomes within the preferred range described below.

[0092] As for other units, constituent units derived from perfluoro monomers are preferred in terms of mechanical strength and chemical durability, and constituent units derived from tetrafluoroethylene (hereinafter referred to as TFE) are more preferred.

[0093] Polymer (H) can be prepared by polymerizing the following compound (M1) and, if necessary, other monomers to obtain a precursor polymer, and then converting the -SO2F groups in the precursor polymer into sulfonic acid groups. The conversion of the -SO2F groups into sulfonic acid groups is carried out by hydrolysis and acidification treatment.

[0094] CF2=CF-(CF2) t OCF2-CFY 2 -Q 3 -SO2F … (M1).

[0095] In addition, t, Y in the above compound (M1) 2 , and Q 3 ☐, t and Y in the above unit (U1), respectively 2 , and Q 3 It has the same meaning as .

[0096] Polymer (Q) :

[0097] Polymer (Q) is a polymer having at least one of the following units (U2) and the following units (U3).

[0098] [Chemical Formula 3]

[0099]

[0100] However, among the above units (U2), Q 1 It is a perfluoroalkylene group that may have an etheric oxygen atom, and Q 2 is a perfluoroalkylene group that may have a single bond or an etheric oxygen atom, and R f1 It is a perfluoroalkyl group that may have an etheric oxygen atom, and X 1 silver is an oxygen atom, a nitrogen atom, or a carbon atom, and a is X 1 In the case of this oxygen atom, it is 0, and X 1 In the case where this is a nitrogen atom, it is 1, and X 1 In the case where this is a carbon atom, it is 2, and Y 1It is a fluorine atom or a monovalent perfluoroorganic group, and s is 0 or 1. The single bond is CY 1 It means that the carbon atom of SO2 is directly bonded to the sulfur atom of SO2. An organic group means a group containing one or more carbon atoms.

[0101] Among the above units (U2), Q 1 , Q 2 When the perfluoroalkylene group has an etheric oxygen atom, the oxygen atom may be one or two or more. Also, the oxygen atom may be inserted between the carbon-carbon bonds of the perfluoroalkylene group or inserted at the ends of the carbon bonds.

[0102] The perfluoroalkylene group may be of the straight chain type or the branched type, and it is preferable that it be of the straight chain type.

[0103] The number of carbon atoms in the perfluoroalkylene group is preferably 1 to 6, and more preferably 1 to 4. If the number of carbon atoms is 6 or less, the boiling point of the raw material, the fluorine-containing monomer, is lowered, making distillation purification easier.

[0104] Q in the above unit (U2) 2 It is preferable that it be a perfluoroalkylene group having 1 to 6 carbon atoms that may have an etheric oxygen atom. Q 2 If α is a carbon-1 to carbon-6 perfluoroalkylene group that may have an etheric oxygen atom, then Q 2 Compared to the case of a single bond, the stability of power generation performance is excellent when operating a solid polymer fuel cell over a long period.

[0105] Among the above units (U2), Q 1 , Q 2Preferably, at least one of them is a perfluoroalkylene group having 1 to 6 carbon atoms having an etheric oxygen atom. Since the fluorine-containing monomer having a perfluoroalkylene group having 1 to 6 carbon atoms having an etheric oxygen atom can be synthesized without undergoing a fluorination reaction with fluorine gas, it has a good yield and is easy to manufacture.

[0106] Among the above units (U2), R f1 The perfluoroalkyl group may be of the straight chain type or branched type, and it is preferable that it be of the straight chain type.

[0107] The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 6, and more preferably 1 to 4. As for the perfluoroalkyl group, perfluoromethyl groups, perfluoroethyl groups, etc. are preferred.

[0108] Unit (U2) is 2 or more R f1 In the case of having, R f1 Each has the same contribution and each has a different contribution.

[0109] Among the above units (U2), -(SO2X 1 (SO2R f1 ) a ) - H + The device is an ion exchanger.

[0110] -(SO2X in the above unit (U2) 1 (SO2R f1 ) a ) - H + The path is, sulfonic acid group (-SO3 - H + group), sulfonimide group (-SO2N(SO2R f1 ) - H + group), or sulfonated group (-SO2C(SO2R f1 )2) - H + Can be cited as (e.g.,

[0111] Y in the above unit (U2) 1It is preferable that the group be a straight-chain perfluoroalkyl group having 1 to 6 carbon atoms, which may have a fluorine atom or an etheric oxygen atom.

[0112] As for the unit (U2), the following unit (U2-1) is preferred, and the following unit (U2-11), unit (U2-12), or unit (U2-13) is more preferred in that the polymer (Q) is easy to manufacture and easy to industrially implement.

[0113] [Chemical Formula 4]

[0114]

[0115] However, among the above units (U2-1), R F11 It is a straight-chain perfluoroalkylene group having 1 to 6 carbon atoms that may have single bonds or etheric oxygen atoms, and R F12 is a straight-chain perfluoroalkylene group having 1 to 6 carbon atoms, and s is 0 or 1.

[0116] [Chemical Formula 5]

[0117]

[0118] However, among the above units (U3), R F1 and R F2 Each is independently a perfluoroalkylene group having 1 to 3 carbon atoms.

[0119] R F1 and R F2 Specific examples of this include -CF2-, -CF2CF2-, -CF(CF3)-, -CF2CF2CF2-, -CF(CF2CF3)-, -CF(CF3)CF2-, -CF2CF(CF3)-, and -C(CF3)(CF3)-.

[0120] In terms of the low cost of raw materials, ease of manufacturing, and the ability to increase the ion exchange capacity of the polymer (Q), R F1 and R F2Each independently, a perfluoroalkylene group having 1 or 2 carbon atoms is preferred. In the case of 2 carbon atoms, a straight chain is preferred. Specifically, -CF2-, -CF2CF2-, or -CF(CF3)- is preferred, -CF2- or -CF2CF2- is more preferred, and -CF2- is particularly preferred.

[0121] As for the unit (U3), the following unit (U3-1) is preferred.

[0122] [Chemical Formula 6]

[0123]

[0124] The polymer (Q) may additionally have other units. The ratio of the other units can be appropriately adjusted so that the ion exchange capacity of the polymer (Q) becomes within the desirable range described below.

[0125] As for other units, constituent units derived from perfluoro monomers are preferred in terms of mechanical strength and chemical durability, and constituent units derived from TFE are more preferred.

[0126] Polymer (Q) can be manufactured by a method described, for example, in International Publication No. 2007 / 013533, International Publication No. 2020 / 116651, etc.

[0127] Regarding the ion exchange capacity of the ionomer, in terms of conductivity and gas permeability, 0.5 milliequivalents / g dry resin to 2.0 milliequivalents / g dry resin is preferred, and 0.8 milliequivalents / g dry resin to 1.5 milliequivalents / g dry resin is particularly preferred.

[0128] The content of the ionomer per 100 parts by mass of carbon carrier is 100 parts by mass or more, and from the perspective of achieving both a reduction in catalyst usage and high output, 100 parts by mass to 240 parts by mass is preferred, 110 parts by mass to 200 parts by mass is more preferred, and 120 parts by mass to 180 parts by mass is even more preferred.

[0129] <Characteristics of the Catalyst Layer>

[0130] The ionomer share is 50 volume% or less, and from the perspective of achieving both a reduction in catalyst usage and high output, 10 volume% to 50 volume% is preferred. Furthermore, from the perspective of achieving both a reduction in catalyst usage and high output in a low-humidity environment (e.g., an environment with 30% humidity), the ionomer share is more preferably 15 volume% to 40 volume%, and even more preferably 20 volume% to 35 volume%.

[0131] Methods for increasing the ionomer content while keeping the ionomer share low include adjusting the mixing treatment conditions during the process of preparing the coating solution for forming the catalyst layer, and adjusting the characteristics of the materials used in preparing the coating solution for forming the catalyst layer; these methods may also be used in combination.

[0132] Methods for adjusting mixing treatment conditions include methods to keep the shear stress applied during mixing low and methods to shorten the processing time of the mixing treatment.

[0133] Methods for adjusting the properties of the material include using a thickening ionomer (e.g., an ionomer with increased viscosity by adding a fluorine-based solvent), using an ionomer with a large molecular weight, and using a hydrophilic catalyst-supported carbon (e.g., a catalyst-supported carbon with increased hydrophilic functional groups on the surface by acid treatment).

[0134] It is preferable that the catalyst-supported carbon in the catalyst layer, when the ionomer is attached, has at least 0.03 cm³ / g of catalyst with macropores having a pore diameter of 50 nm or more in the pore distribution obtained by nitrogen adsorption.

[0135] The total pore capacity of macropores per unit mass of catalyst-supported carbon in a state where an ionomer is attached can be, for example, in the range of 0.03 cm³ / g catalyst to 0.3 cm³ / g catalyst, and from the perspective of achieving both reduction in catalyst usage and high output, a range of 0.05 cm³ / g catalyst to 0.25 cm³ / g catalyst is preferred, and a range of 0.07 cm³ / g catalyst to 0.20 cm³ / g catalyst is more preferred.

[0136] The thickness of the catalyst layer is not particularly limited, and for example, a range of 0.5 μm to 10 μm can be given, a range of 1 μm to 8 μm is preferred, and a range of 2 μm to 6 μm is more preferred.

[0137] The thickness of the catalyst layer is measured by observing the cross-section of the catalyst layer using a scanning electron microscope or the like.

[0138] <Method for manufacturing a catalyst layer>

[0139] A method for manufacturing a catalyst layer involves, for example, a preparation process for preparing a coating solution for forming a catalyst layer, and a catalyst layer formation process in which a coating solution for forming a catalyst layer is applied to the surface of a layer (gas diffusion layer, polymer electrolyte membrane, etc.) in contact with the catalyst layer in a membrane electrode assembly or to the surface of a substrate film, and then dried to form the catalyst layer.

[0140] In addition, when a coating solution for forming a catalyst layer is applied to the surface of a substrate film, an additional transfer process may be performed to transfer the formed catalyst layer to the surface of a layer in contact with the catalyst layer in a membrane electrode assembly.

[0141] In the preparation process, a coating solution for forming a catalyst layer is prepared by mixing, for example, catalyst-supported carbon, an ionomer, and a solvent as needed. The catalyst-supported carbon and the ionomer may each be pre-dispersed in a solvent. In short, a dispersion in which the catalyst-supported carbon is dispersed and a dispersion in which the ionomer is dispersed may be mixed.

[0142] Examples of solvents include water-based solvents such as water, alcohol, and mixtures thereof, and organic solvents; among these, water-based solvents are preferred from the perspective of safety during coating and drying.

[0143] The mixing method is not particularly limited and includes known mixing methods such as mixing by a bead mill, mixing by a ball mill, mixing by an ultrasonic disperser, and a jet mill. Among these, the mixing method by a bead mill is preferred in terms of keeping the ionomer content low.

[0144] The solid content concentration of the coating solution for forming the catalyst layer is not particularly limited, and, for example, can be in the range of 5 mass% to 30 mass%.

[0145] In addition to PET films, substrate films used in the catalyst layer formation process may include ETFE films, olefin-based resin films, etc. Furthermore, the above "ETFE" refers to tetrafluoroethylene-ethylene copolymer resin.

[0146] The method of applying the coating solution for forming the catalyst layer is not particularly limited, and known methods such as the die coating method may be cited, for example.

[0147] A known method is used for drying the layer of the coating solution for forming the applied catalyst layer. As for the drying temperature, for example, a range of 40°C to 130°C may be used, and a range of 45°C to 80°C is preferred. As for the drying time, for example, a range of 0.5 minutes to 10 minutes may be used, and a range of 1 minute to 7 minutes is preferred.

[0148] [Membrane electrode assembly for solid polymer fuel cells]

[0149] The membrane electrode assembly for a solid polymer fuel cell in the present embodiment (hereinafter also referred to as the "membrane electrode assembly") comprises an anode having a first gas diffusion layer and a first catalyst layer formed on one side of the first gas diffusion layer, a cathode having a second catalyst layer formed on one side of the second gas diffusion layer, and a polymer electrolyte membrane disposed between the first catalyst layer and the second catalyst layer, wherein at least one of the first catalyst layer and the second catalyst layer is the aforementioned catalyst layer.

[0150] Hereinafter, the membrane electrode assembly in the present embodiment will be described using the drawings.

[0151] FIG. 1 shows a schematic cross-sectional view of an example in which the aforementioned catalyst layer is used as the second catalyst layer, which is the catalyst layer of the cathode, in the membrane electrode assembly of the present embodiment.

[0152] The membrane electrode assembly (10) shown in FIG. 1 comprises an anode (13) having a catalyst layer (11) and a gas diffusion layer (12), a cathode (14) having a catalyst layer (21) and a gas diffusion layer (22), and a polymer electrolyte membrane (15) disposed in contact with the catalyst layer (11) and the catalyst layer (21) between the anode (13) and the cathode (14).

[0153] And, the catalyst layer (21) is the aforementioned catalyst layer.

[0154] The catalyst layer (21) and the catalyst layer (11) may be layers with the same components, composition, thickness, etc., or different layers.

[0155] The catalyst layer (11) may be, for example, a layer containing catalyst-supported carbon and an ionomer. The catalyst layer (11) may be a catalyst layer related to the above-described embodiment, or a catalyst layer other than the catalyst layer related to the above-described embodiment. In addition, the catalyst-supported carbon and ionomer in the catalyst layer (11) may be the same as the catalyst-supported carbon and ionomer in the catalyst layer related to the above-described embodiment.

[0156] The gas diffusion layer (12) and the gas diffusion layer (22) each have the function of uniformly diffusing gas into the catalyst layer (11) and the catalyst layer (21), and also function as a current collector. The gas diffusion layer (12) and the gas diffusion layer (22) are, for example, made of a gas-diffusing substrate. Examples of the gas diffusion layer (12) and the gas diffusion layer (22) include carbon paper, carbon cloth, carbon felt, etc. It is preferable that the gas diffusion layer (12) and the gas diffusion layer (22) be treated to be water-repellent with polytetrafluoroethylene, etc. Additionally, the gas diffusion layer (12) and the gas diffusion layer (22) may be layers with the same components, composition, thickness, etc., or different layers.

[0157] The anode (13) may have a carbon layer (not shown) as an intermediate layer between the catalyst layer (11) and the gas diffusion layer (12). Likewise, the cathode (14) may also have a carbon layer (not shown) as an intermediate layer between the catalyst layer (21) and the gas diffusion layer (22). By having a carbon layer, the gas diffusion properties of the surface of the catalyst layer are improved, and the power generation performance of the solid polymer fuel cell is greatly improved.

[0158] Examples of carbon layers include a layer comprising carbon and a nonionic fluorine-containing polymer. Examples of carbon used in the carbon layer include carbon nanofibers with a fiber diameter of 1 nm to 1000 nm and a fiber length of 1000 μm or less. Examples of nonionic fluorine-containing polymers include polytetrafluoroethylene.

[0159] The polymer electrolyte membrane (15) is a membrane containing an ion exchange resin. As for the ion exchange resin, a fluorine-containing ion exchange resin is preferred in terms of durability, a perfluorocarbon polymer having ion exchange groups is more preferred, the polymer (H) or polymer (Q) described above is even more preferred, and polymer (H) is particularly preferred. In addition, the perfluorocarbon polymer may contain etheric oxygen atoms.

[0160] The ion exchange capacity of the fluorine-containing ion exchange resin is preferably 0.5 milliequivalents / g dry resin to 2.0 milliequivalents / g dry resin, and particularly preferably 0.8 milliequivalents / g dry resin to 1.5 milliequivalents / g dry resin.

[0161] In addition, the ion exchange capacity of a fluorine-containing ion exchange resin can be measured in the same way as the ion exchange capacity of an ionomer.

[0162] The polymer electrolyte membrane (15) may be reinforced with a reinforcing material. Examples of reinforcing materials include porous materials, fibers, woven fabrics, nonwoven fabrics, etc. Examples of reinforcing materials include polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, polyethylene, polypropylene, polyphenylene sulfide, etc.

[0163] The polymer electrolyte membrane (15) may contain one or more atoms selected from the group consisting of cerium and manganese to further improve durability. Cerium and manganese decompose hydrogen peroxide, which is a substance that causes deterioration of the polymer electrolyte membrane (15). It is preferable that cerium and manganese exist as ions in the polymer electrolyte membrane (15).

[0164] The polymer electrolyte membrane (15) may contain silica, heteropoly acid (zirconium phosphate, phosphomolybdic acid, phosphotungstic acid, etc.) as a water retention agent to prevent drying.

[0165] The thickness of the polymer electrolyte membrane is preferably 10 μm to 30 μm, and more preferably 15 μm to 25 μm. If the thickness of the polymer electrolyte membrane is lower than or equal to the upper limit of the above range, the degradation of the power generation performance of the solid polymer fuel cell under low humidity conditions is suppressed. In addition, by making the thickness of the polymer electrolyte membrane higher than or equal to the lower limit of the above range, gas leakage or electrical short circuits can be suppressed.

[0166] The thickness of the polymer electrolyte membrane is measured by observing a cross- section of the polymer electrolyte membrane using a scanning electron microscope or the like.

[0167] <Method for manufacturing a membrane electrode assembly>

[0168] The membrane electrode assembly (10) is manufactured, for example, by the following method.

[0169] (α) A method of forming a catalyst layer (11) and a catalyst layer (21) on a polymer electrolyte membrane (15) to form a membrane catalyst layer assembly, and forming the membrane catalyst layer assembly into a gas diffusion layer (12) and a gas diffusion layer (22).

[0170] (β) A method of forming a catalyst layer (11) on a gas diffusion layer (12) to form an anode (13), forming a catalyst layer (21) on a gas diffusion layer (22) to form a cathode (14), and forming a polymer electrolyte membrane (15) on the anode (13) and cathode (14).

[0171] When the membrane electrode assembly (10) has a carbon layer, the membrane electrode assembly (10) is manufactured, for example, by the following method.

[0172] (γ) A method of applying a dispersion containing carbon and a nonionic fluorine-containing polymer onto a substrate film, drying to form a carbon layer, forming a catalyst layer (11) on the carbon layer, separately manufacturing a laminate formed in the order of a carbon layer and a catalyst layer (21) on a substrate film in the same way, bonding the catalyst layer (11) and the polymer electrolyte membrane (15), and the catalyst layer (21) and the polymer electrolyte membrane (15) respectively, peeling off each substrate film to form a membrane catalyst layer assembly having a carbon layer, and bonding the membrane catalyst layer assembly into a gas diffusion layer (12) and a gas diffusion layer (22).

[0173] (δ) A method of forming a carbon layer by applying a dispersion containing carbon and a nonionic fluorine-containing polymer onto a gas diffusion layer (12) and a gas diffusion layer (22), respectively, and drying to form a carbon layer, and forming a catalyst layer (11) and a catalyst layer (21) on a polymer electrolyte membrane (15), and then forming a membrane catalyst layer composite with a carbon layer on a gas diffusion layer (12) and a carbon layer on a gas diffusion layer (22).

[0174] A polymer electrolyte membrane (15) can be formed by, for example, by applying a liquid composition containing an ion exchange resin onto a substrate film or a catalyst layer (catalyst layer (11) or catalyst layer (21)) and drying it (casting method).

[0175] When forming the polymer electrolyte membrane (15), for example, a liquid composition containing a liquid medium, a fluorinated polymer having sulfonic acid groups, and trivalent or tetravalent cerium ions may be used.

[0176] When using the above liquid composition, it is preferable to perform heat treatment to stabilize the polymer electrolyte membrane (15). The temperature of the heat treatment varies depending on the type of ion exchange resin, but is preferably 130°C to 200°C. If the temperature of the heat treatment is 130°C or higher, the ion exchange resin does not become excessively water-soluble. If the temperature of the heat treatment is 200°C or lower, the thermal decomposition of the sulfonic acid group is suppressed, and the decrease in proton conductivity of the polymer electrolyte membrane (15) is suppressed. The polymer electrolyte membrane (15) may be treated with hydrogen peroxide as needed.

[0177] [Solid Polymer Fuel Cell]

[0178] The solid polymer fuel cell in this embodiment comprises the aforementioned membrane electrode assembly.

[0179] A solid polymer fuel cell is manufactured, for example, by forming a cell by placing a membrane electrode assembly between two separators and stacking a plurality of cells.

[0180] Examples of separators include conductive carbon plates having grooves formed therein that serve as passages for fuel gas or oxidizer gas containing oxygen (air, oxygen, etc.).

[0181] Examples of solid polymer fuel cells include hydrogen / oxygen fuel cells and direct methanol fuel cells (DMFC). The methanol or aqueous methanol solution used as fuel for DMFCs may be a liquid feed or a gas feed.

[0182] Examples

[0183] The present disclosure is described in detail below by presenting examples and reference examples. However, the present disclosure is not limited by the following examples.

[0184] [Catalyst-supported carbon]

[0185] As catalyst-supported carbons, the following catalyst-supported carbons (1), catalyst-supported carbons (2), and catalyst-supported carbons (3) were prepared.

[0186] Catalyst-supported carbon (1): Catalyst: Platinum particles, Catalyst content relative to the total catalyst-supported carbon: 60 mass%, Average particle size of the number of platinum particles: 4.8 nm

[0187] Catalyst-supported carbon (2): Catalyst: Platinum particles, Catalyst content relative to the total catalyst-supported carbon: 50 mass%, Average particle size of the number of platinum particles: 3.3 nm

[0188] Catalyst-supported carbon (3): Catalyst: platinum particles, catalyst content relative to the total catalyst-supported carbon: 20 mass%, average particle size of the number of platinum particles: 2.5 nm

[0189] In addition, as the catalyst-supported carbon (3), a general platinum-supported carbon catalyst with a platinum support rate of 20% was used.

[0190] The characteristics of the catalyst-supported carbon (1) are as follows.

[0191] Total specific surface area: 283 m² / g catalyst

[0192] Total pore capacity of specific mesopores: 0.15 cm³ / g catalyst

[0193] Ratio of the total crafting capacity of a specific Meso Gong to the total Meso Gong and Macro Gong: 28%

[0194] Total macropore capacity: 0.25 cm³ / g catalyst

[0195] The characteristics of the catalyst-supported carbon (2) are as follows.

[0196] Total specific surface area: 410 m² / g catalyst

[0197] Total pore capacity of specific mesopores: 0.15 cm³ / g catalyst

[0198] Ratio of the total crafting capacity of a specific Meso Gong to the total Meso Gong and Macro Gong: 50%

[0199] Total macropore capacity: 0.25 cm³ / g catalyst

[0200] [Ionomer dispersion]

[0201] As an ionomer, a polymer (H1) having a constituent unit derived from TFE and the unit (U1-11) was prepared (ion exchange capacity: 1.1 milliequivalent / g dry resin).

[0202] A polymer (H1) was dispersed in a dispersion medium of ethanol / water = 6 / 4 (mass ratio) to prepare a polymer (H1) dispersion (A) with a solid content concentration of 25.0 mass%.

[0203] [Preparation of coating solution for forming a catalyst layer]

[0204] <Potential liquid (a1)>

[0205] 50.0 g of catalyst-supported carbon (1) was added to 363 g of distilled water and stirred well. Additionally, 177 g of ethanol and 65 g of 2-propanol were added and stirred well. 56.0 g of polymer (H1) dispersion (A) was added to this, and 1 mm of zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 6 m / s and a residence time of 1.1 min, and this was prepared as a coating solution (a1).

[0206] <Potation liquid (a2)>

[0207] 50.0 g of catalyst-supported carbon (1) was added to 389 g of distilled water and stirred well. Additionally, 188 g of ethanol and 71 g of 2-propanol were added and stirred well. 80.0 g of polymer (H1) dispersion (A) was added to this, and 1 mm of zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 6 m / s and a residence time of 1.1 min, and this was prepared as a coating solution (a2).

[0208] <Potation liquid (a3)>

[0209] 50.0 g of catalyst-supported carbon (1) was added to 431 g of distilled water and stirred well. Additionally, 207 g of ethanol and 81 g of 2-propanol were added and stirred well. 120 g of polymer (H1) dispersion (A) was added to this, and 1 mm of zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 6 m / s and a residence time of 1.1 min, and this was prepared as a coating solution (a3).

[0210] <Potation Liquid (a4)>

[0211] 50.0 g of catalyst-supported carbon (1) was added to 363 g of distilled water and stirred well. Additionally, 177 g of ethanol and 65 g of 2-propanol were added and stirred well. 56.0 g of polymer (H1) dispersion (A) was added to this, and 0.5 mm zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 8 m / s and a residence time of 5.5 minutes, and this was prepared as a coating solution (a4).

[0212] <Potential Liquid (a5)>

[0213] 50.0 g of catalyst-supported carbon (1) was added to 389 g of distilled water and stirred well. Additionally, 188 g of ethanol and 71 g of 2-propanol were added and stirred well. 80.0 g of polymer (H1) dispersion (A) was added to this, and 0.5 mm zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 8 m / s and a residence time of 5.5 minutes, and this was prepared as a coating solution (a5).

[0214] <Potwork liquid (a6)>

[0215] 50.0 g of catalyst-supported carbon (1) was added to 431 g of distilled water and stirred well. Additionally, 207 g of ethanol and 81 g of 2-propanol were added and stirred well. 120 g of polymer (H1) dispersion (A) was added to this, and 0.5 mm zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 8 m / s and a residence time of 5.5 minutes, and this was prepared as a coating solution (a6).

[0216] <Potwork liquid (a7)>

[0217] 50.0 g of catalyst-supported carbon (3) was added to 357 g of distilled water and stirred well. Additionally, 376 g of ethanol was added and stirred well. 128 g of polymer (H1) dispersion (A) was added to this, and 1.0 mm zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 6 m / s and a residence time of 4.3 minutes, and this was prepared as a coating solution (a7).

[0218] <Potter Liquid (a8)>

[0219] 50.0 g of catalyst-supported carbon (2) was added to 375 g of distilled water and stirred well. Additionally, 397 g of ethanol was added and stirred well. 150 g of polymer (H1) dispersion (A) was added to this, and 1.0 mm zirconia beads were used in a bead mill (LZ015 manufactured by Ashizawa Fine Tech) to disperse the mixture at a peripheral speed of 6 m / s and a residence time of 1.1 min, and this was prepared as a coating solution (a8).

[0220] [Preparation of coating solution for forming an intermediate layer (carbon layer)]

[0221] <Potter Liquid (c1)>

[0222] 21.0 g of ethanol and 24.0 g of distilled water were added to 10.0 g of vapor-grown carbon fiber (manufactured by Showa Denko, product name: VGCF-H, average fiber diameter: about 150 nm, fiber length: 10 to 20 μm) and stirred well. 20.0 g of polymer (H1) dispersion (A) was added to this and stirred well, and further mixed and ground using a homogenizer to make the coating solution (c1).

[0223] [Formation of the catalyst layer]

[0224] <Example C1>

[0225] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then a coating solution (a1) was additionally applied to the substrate using a die coater to obtain a platinum content of 0.20 mg / cm² and dried to obtain a cathode (gc1). In addition, the "platinum content" refers to the amount of catalyst per unit area of ​​the catalyst layer.

[0226] A coating solution (a7) was applied to a gas diffusion layer substrate (manufactured by SGL Carbon Co., 25BC) with a coating layer formed thereon using a die coater to obtain a platinum content of 0.05 mg / cm², and dried to obtain an anode (ga1).

[0227] As a polymer electrolyte membrane, an ion exchange membrane with a thickness of 20 μm made of a perfluorocarbon polymer having sulfonic acid groups (manufactured by Asahi Glass Co., Ltd., trade name: Flemion, ion exchange capacity: 1.1 milliequivalent / g dry resin) was prepared.

[0228] A membrane electrode assembly (electrode area: 25 cm²) was obtained by forming a polymer electrolyte membrane into an anode (ga1) and a cathode (gc1) and pressing the catalyst layers of the anode (ga1) and cathode (gc1) onto the polymer electrolyte membrane by a hot press method.

[0229] <Example 1>

[0230] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then an additional coating solution (a2) was applied to the substrate using a die coater to obtain a platinum content of 0.20 mg / cm² and dried to obtain a cathode (gc2).

[0231] A membrane electrode assembly was obtained in the same manner as Example C1, except that a cathode (gc2) was used instead of a cathode (gc1).

[0232] <Example 2>

[0233] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then an additional coating solution (a3) ​​was applied to the substrate using a die coater to obtain a platinum content of 0.20 mg / cm² and dried to obtain a cathode (gc3).

[0234] A membrane electrode assembly was obtained in the same manner as Example C1, except that cathode (gc3) was used instead of cathode (gc1).

[0235] <Example C2>

[0236] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then an additional coating solution (a4) was applied to the substrate using a die coater to obtain a platinum content of 0.20 mg / cm² and dried to obtain a cathode (gc4).

[0237] A membrane electrode assembly was obtained in the same manner as Example C1, except that a cathode (gc4) was used instead of a cathode (gc1).

[0238] <Example 3>

[0239] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then an additional coating solution (a5) was applied to the substrate using a die coater to obtain a platinum content of 0.20 mg / cm² and dried to obtain a cathode (gc5).

[0240] A membrane electrode assembly was obtained in the same manner as Example C1, except that cathode (gc5) was used instead of cathode (gc1).

[0241] <Example C3>

[0242] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then an additional coating solution (a6) was applied to the substrate using a die coater to obtain a platinum content of 0.20 mg / cm² and dried to obtain a cathode (gc6).

[0243] A membrane electrode assembly was obtained in the same manner as Example C1, except that a cathode (gc6) was used instead of a cathode (gc1).

[0244] <Example 4>

[0245] A coating solution (c1) was applied to a gas diffusion layer substrate (manufactured by NOK, H2315 T10X6) without a coating layer using a die coater to obtain a solid content of 3.0 mg / cm² and dried, and then an additional coating solution (a8) was applied to the substrate using a die coater to obtain a platinum content of 0.10 mg / cm² and dried to obtain a cathode (gc7).

[0246] A membrane electrode assembly was obtained in the same manner as Example C1, except that cathode (gc7) was used instead of cathode (gc1).

[0247] [Measurement and Evaluation]

[0248] <Content of ionomer per 100 parts by mass of carbon carrier>

[0249] The content of ionomer (parts by mass) per 100 parts by mass of carbon carrier in the cathode of the above example is shown in Table 1 ("Ionomer content" in Table 1).

[0250] <Ionomer Market Share>

[0251] The coating solution used for forming the cathode in the above example was applied onto a PET film, dried, and the powder obtained by scraping off the coating layer was used as a "sample of catalyst-supported carbon with attached ionomer." In addition, a coating solution not containing ionomer (in other words, a mixture of catalyst-supported carbon and a solvent) was applied onto a PET film, dried, and the powder obtained by scraping off the coating layer was used as a "sample of catalyst-supported carbon without attached ionomer." Using these samples, the pore distribution was determined for each by the method described above, and the ionomer share (%) for each example was calculated. The results are shown in Table 1.

[0252] <Macropore pore capacity after ionomer attachment>

[0253] From the pore distribution of the "catalyst-supported carbon sample with attached ionomer" in each example, the total pore capacity of macropores per unit mass of the catalyst-supported carbon with attached ionomer (cm³ / g catalyst) was calculated. The results are shown in Table 1 ("macropore pore capacity" in Table 1).

[0254] <Power Generation Performance (1)>

[0255] The membrane electrode assembly obtained in the above example was mounted in a power generation cell, and hydrogen (utilization rate 70%) / air (utilization rate 50%) was supplied at atmospheric pressure, and the cell voltage (V) at the beginning of operation was measured at a cell temperature of 80°C and a current density of 1.0 A / cm². In addition, hydrogen with a dew point of 80°C was supplied to the anode side, and air with a dew point of 80°C was supplied to the cathode side, respectively, into the cell (relative humidity inside the cell: 100%RH). The results are shown in Table 1 ("100%RH cell voltage" in Table 1).

[0256] <Power Generation Performance (2)>

[0257] The membrane electrode assembly obtained in the above example was mounted in a power generation cell, and hydrogen (utilization rate 70%) / air (utilization rate 50%) was supplied at atmospheric pressure, and the cell voltage (V) at the beginning of operation was measured at a cell temperature of 80°C and a current density of 1.0 A / cm². In addition, hydrogen with a dew point of 53°C was supplied to the anode side, and air with a dew point of 53°C was supplied to the cathode side, respectively, into the cell (relative humidity inside the cell: 30%RH). The results are shown in Table 1 ("30%RH cell voltage" in Table 1).

[0258]

[0259] As can be seen from the results shown in Table 1, in Examples 1 to 4, compared to Examples C1 to C3, it can be seen that high output of the fuel cell is realized while reducing the amount of catalyst used.

[0260] The disclosure of Japanese Patent Application No. 2019-232523, filed on December 24, 2019, is incorporated herein by reference in its entirety.

[0261] All documents, patent applications, and technical specifications described in this specification are incorporated herein to the same extent that individual documents, patent applications, and technical specifications are incorporated by reference as they are specifically and individually described. Explanation of the symbols

[0262] 10: Membrane electrode assembly 11: Catalyst layer 12: Gas diffusion layer 13 : Anode 14 : Cathode 21: Catalyst layer 22: Gas diffusion layer

Claims

Claim 1 A catalyst supporting carbon in which a platinum-containing catalyst is supported on a carbon support, and a catalyst layer containing an ionomer, wherein the catalyst supporting carbon has mesopores with a pore diameter of 2 nm or more and less than 10 nm in a pore distribution obtained by nitrogen adsorption, at least a portion of the ionomer exists within the mesopores with a pore diameter of 2 nm or more and less than 10 nm, the content of the ionomer relative to 100 parts by mass of the carbon support is 100 parts by mass or more, and the share of the ionomer in the total volume of the mesopores with a pore diameter of 2 nm or more and less than 10 nm is 50 volume% or less, and the catalyst layer used as a catalyst layer of a cathode in a membrane electrode assembly for a solid polymer fuel cell. Claim 2 In claim 1, the catalyst-supported carbon in the catalyst layer is a catalyst layer having at least 0.03 cm³ / g of macropores with a pore diameter of 50 nm or more in a pore distribution obtained by nitrogen adsorption method in a state where the ionomer is attached. Claim 3 In claim 1, the catalyst layer having a catalyst content per unit area of ​​the catalyst layer of 0.2 mg / cm² or less. Claim 4 In claim 1, the catalyst comprises a catalyst layer including at least one selected from the group consisting of platinum particles and platinum alloy particles. Claim 5 In claim 4, the number average particle size of the catalyst is 1 nm to 20 nm, in the catalyst layer. Claim 6 A catalyst layer according to claim 1, wherein the content of the catalyst relative to the total catalyst-supported carbon is 10 mass% to 70 mass%. Claim 7 A membrane electrode assembly for a solid polymer fuel cell, comprising: an anode having a first gas diffusion layer and a first catalyst layer formed on one side of the first gas diffusion layer; a cathode having a second gas diffusion layer and a second catalyst layer formed on one side of the second gas diffusion layer; and a polymer electrolyte membrane disposed between the first catalyst layer and the second catalyst layer, wherein at least the second catalyst layer is a catalyst layer described in any one of claims 1 to 6. Claim 8 A solid polymer fuel cell having a membrane electrode assembly for a solid polymer fuel cell as described in claim 7.

Citation Information

Patent Citations

  • Catalyst layer for fuel cell and production method therefor

    KR1020190129746A