Method for manufacturing a composite filter medium and a composite filter medium obtained by this method
By incorporating a degassing and reactivation plasma treatment, the composite filter medium ensures complete polymerization and adhesion of the coating, addressing the issue of pressure fluctuations, achieving superior water and oil repellency and air permeability for electroacoustic applications.
Patent Information
- Application Number
- KR1020227009535
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-19
- Filing Date
- 2020-10-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2040-10-21
AI Technical Summary
The pressure fluctuations in the vacuum chamber during plasma treatment of base fabrics and nanofibers due to moisture emission from the materials lead to incomplete polymerization of the coating, resulting in inferior water and oil repellency, and poor adhesion of the coating to the substrate, which affects the performance of composite filter media.
A degassing step is performed before plasma treatment to remove moisture from the materials, followed by a reactivation plasma treatment to create nanometer irregularities on the surface, ensuring complete polymerization and strong adhesion of the coating.
The composite filter medium achieves high water and oil repellency with strong adhesion, maintaining air permeability and preventing particle intrusion, suitable for electroacoustic components.
Smart Images

Figure 112022030815410-PCT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing a composite filter medium. The present invention also extends to a composite filter medium obtained by this method.
[0002] The field of the present invention relates to composite filter media, which are used particularly for protection against the intrusion of dust particles, and also for repelling liquids, such as water and oil, to ensure high permeability to air, i.e., low acoustic impedance, in order to deliver optimal sound, for example, in electroacoustic components of consumer electronic products, particularly mobile phones. Background Technology
[0003] The disclosed composite filter medium is formed by a combination of at least one nanofiber layer supported by a weft and warp base fabric, wherein the nanofiber layer is deposited on the base fabric by an electrospinning process in which a plasma coating is applied to the base fabric and the nanofibers. Through this method, a composite filter medium with a nanofiber layer attached to the base fabric is produced.
[0004] To ensure desired performance by plasma coating, it is essential that monomers injected into the plasma system chamber polymerize on the surfaces of base fabrics and nanofibers under optimal conditions. However, these polymerization conditions depend on process parameters set for the plasma treatment, such as power supply power, vacuum chamber sealing pressure, fiber exposure time to plasma treatment, and the distance from the electrode to the substrate.
[0005] During the aforementioned plasma treatment, the pressure inside the vacuum chamber may fluctuate relative to the set value; in particular, this can increase due to gases emitted by the material being processed inside the vacuum chamber. During the plasma process for forming a coating on the surface of base fabrics and nanofibers, the rise in pressure inside the chamber may be primarily attributed to the moisture content of the material placed in the vacuum chamber. In practice, during this process, water molecules leave the fibrous material to be coated, increasing the pressure and mixing with the coating plasma supply gas, thereby contaminating it. This is even more critical in industrial production processes involving operation with rolls made of materials having large diameters and heavy weights.
[0006] Such an increase in pressure inevitably alters the polymerization conditions of the materials forming the coating on the base fabric and nanofibers, causing incomplete polymerization of the coating. Consequently, it fails to lower the surface energy of the nanofibers, resulting in a failure to achieve the desired water and oil repellency in the final filter medium.
[0007] Contamination of the coating plasma supply gas by water molecules emitted from the fabric alters the polymerization reaction, thereby producing a coating with chemical and physical properties inferior to the desired water-repellent and oil-repellent coatings, which fails to ensure sufficient adhesion of the polymerized coating to the substrate.
[0008] The main objective of the present invention is to provide a composite filter medium and a process for manufacturing the same that ensures optimal polymerization of a coating deposited on the surface of a monofilament forming a base fabric and on the surface of nanofibers in relation to a known filter medium of this type.
[0009] In addition, the object of the present invention is to provide a process for manufacturing a filter medium having a coating that adheres strongly to the surface of monofilaments and nanofibers of a base fabric.
[0010] These and other objectives are achieved by the method and filter medium of claims 1 and 10, respectively. Preferred embodiments of the present invention will be apparent from the remaining claims.
[0011] In relation to the disclosed filter media, the filter media of the present invention provides the advantage of maintaining a desired level of water and oil repellency due to the formation of a fully polymerized coating that adheres strongly to the surface of the base fabric and nanofibers.
[0012] The composite filter medium of the present invention, in which individual nanofibers and individual threads of a fabric are covered with a thin, highly hydrophobic and oleophobic coating, also possesses the ability to prevent dust, and in particular, the ability to prevent liquids such as water (high surface tension, 72 mN / m) as well as liquids such as oil (low surface tension, 30-40 mN / m). These characteristics of the filter medium of the present invention are particularly useful for applications as a protective screen for electroacoustic components of mobile phones. In practice, the filter medium of the present invention consists of nanofibers that provide very high permeability to air (and very low acoustic impedance), ensuring effective protection against the intrusion of particles. Additionally, due to a specific coating, the composite filter medium of the present invention prevents the penetration of water, oil, and other types of liquids. In practice, the filter medium of the present invention not only prevents the penetration of these liquids but is also easier to clean due to its water-repellent properties. Brief explanation of the drawing
[0013] These and other purposes, advantages, and features will be apparent from the following description of preferred embodiments of the method and filter medium according to the present invention, which are illustrated as non-limiting examples in the accompanying drawings. - FIG. 1 is a cross-sectional view and schematic diagram of an example of a composite filter medium of the present invention. - Figure 2 shows a detailed view of nanofibers deposited by electrospinning on corresponding threads of a base fabric, where both the nanofibers and the threads of the base fabric are coated with a nanometer layer of water-repellent and oil-repellent polymer applied by plasma treatment. - Figure 3 illustrates an electrospinning method for manufacturing a nanofiber layer in a filter medium of the present invention. - Figure 4 schematically illustrates the plasma treatment of the filter medium of the present invention obtained by depositing a nanofiber layer produced by an electrospinning process onto a base fabric. - Figure 5 illustrates the relationship between flow rate and pressure measured across the filter medium for dry and wet samples. - Figure 6 illustrates the relationship between the emptying pressure and the corresponding pressure drop for a declogging test performed on two different samples. Specific details for implementing the invention
[0014] The composite filter medium of the present invention (indicated collectively by number 1 in FIG. 1) comprises a support formed by a base fabric (2) of the warp and weft type, preferably a monofilament fabric, on which nanofibers (4) are deposited by electrospinning. Suitable for the present invention are monofilaments (3) manufactured starting from monofilaments of polyester, polyamide, polypropylene, polyether sulfone, polyimide, polyamide imide, polyphenylene sulfide, polyether ether ketone, polyvinylidene fluoride, polytetrafluoroethylene, and aramid, and the mesh opening of the base fabric (2) is in the range of 2500 microns to 5 microns.
[0015] The base fabric used in the manufacture of the composite filter medium of the present invention is selected from a wide range of synthetic monofilament fabrics, wherein the chemical properties of the monofilaments used for weaving differ, such as polyester, polyamide, polypropylene, polyether sulfone, polyimide, polyamide imide, polyphenylene sulfide, polyether ether ketone, polyvinylidene fluoride, polytetrafluoroethylene, and aramid. Textile structure of 4 to 300 threads / cm, thread diameter of 10 to 500 microns, and 15 to 300 g / m² 2 Base fabrics having a weight weave and a thickness of 18 to 1000 microns are also suitable for the present invention. For finishing and additional surface treatment, in addition to metallization, washed and heat-cured "white" fabrics, colored fabrics, plasma-treated fabrics, hydrophobic, hydrophilic, antibacterial, antistatic fabrics, etc. may be used. Preferred for the present invention is a polyester monofilament fabric having 48 threads / cm, a diameter of 55 μm, and a mesh opening of 153 μm in the base fabric.
[0016] Suitable for the present invention are nanofibers (4) of polyester, polyurethane, polyamide, polyimide, polypropylene, polysulfone, polyethersulfone, polyamideimide, polyphenylene sulfide, polyetheretherketone, polyvinylidene fluoride, polytetrafluoroethylene, alginate, polycarbonate, PVA (polyvinyl alcohol), PLA (polylactic acid), PAN (polyacrylonitrile), PEVA (polyethylene vinyl acetate), PMMA (polymethyl methacrylate), PEO (polyethylene oxide), PE (polyethylene), PVC, PEI, PUR, and polystyrene. These nanofibers may have a diameter of 50 nm to 700 nm. Polyvinylidene fluoride (PVDF) nanofibers with a diameter in the range of 75 to 200 nm are preferred.
[0017] As illustrated in FIG. 3, the electrospinning process for the formation of nanofibers (4) and subsequent deposition on the base fabric (2) consists of injecting a material for forming nanofibers (4), which is dissolved in a suitable solvent, through a nozzle (5) to spread onto an electrode (6). Due to the potential difference between the nozzle (5) and the electrode (6), nanofibers (4) are formed through the evaporation of the solvent, which is caused by the electric field and stretching of the polymer deposited on the electrode by the nozzle. The nanofibers thus formed are subsequently stretched and subsequently deposited on the base fabric (2).
[0018] The composite filter medium obtained in this way is then surface-treated by plasma deposition of a nanometer-thick polymer layer (7) on the exposed surface of the fabric (2) and the nanofiber layer (4), thereby completely covering the outer surfaces of the base fabric (2) and the monofilaments (3) of the aforementioned nanofibers (4) (Fig. 2).
[0019] As shown in FIG. 4, the composite filter medium (8) obtained from the electrospinning process of FIG. 3 above is placed inside a plasma treatment chamber (9) in the presence of a gas that forms a coating (7) to cover the composite filter medium (1) of the present invention.
[0020] Gases based on fluorocarbon acrylates, particularly heptadecafluorodecyl acrylates, perfluorooctyl acrylates, etc. Gases advantageous to the present invention are those that form a deposition of fluorocarbon acrylates by plasma treatment, which is attributed to water-repellent and oil-repellent properties.
[0021] In the aforementioned plasma treatment, a carrier gas of the type described in WO2011089009A1 is also used, for example.
[0022] The aforementioned plasma treatment includes generating a vacuum of 10 to 50 mTorr, an electrode power of 150 to 350 W, and an exposure time of 0.5 to 6 minutes.
[0023] Coatings deposited through plasma technology can have a thickness of up to 500 nm, can have a continuous film structure due to the specific technology used, and can also coat 3D surfaces such as fabrics. Depending on the compound used, the aforementioned coating can have various intrinsic properties such as hydrophobicity, oleophobicity, hydrophilicity, and antistatic properties.
[0024] Coatings obtained starting from the following compounds in starting gases are preferred in the present invention:
[0025] 1 H ,1 H ,2 H ,2 H -HEPTADECAFLUORODECYL ACRYLATE (CAS #27905-45-9, H2C=CHCO2CH2CH2(CF2)7CF3)
[0026] 1 H ,1 H ,2H ,2 H -PERFLUOROOCTYL ACRYLATE (CAS #17527-29-6, H2C=CHCO2CH2CH2(CF2)5CF3)
[0027] The thickness of the coating (7) is 15 to 60 nm, which is suitable for preventing the composite filter medium (1) from excessively narrowing the pores formed in both the fabric (2) and the nanofibers (4) to prevent free sound passage.
[0028] A test was performed on a composite filter medium (8) obtained from the electrospinning process of Fig. 3, compared with a similar composite filter medium (1) that underwent subsequent plasma treatment of Fig. 4.
[0029] In particular, the aforementioned filter medium (8) is formed by a weft and warp fabric made of synthetic monofilament (3) (e.g., polyester), and on it, nanofibers (4) made of synthetic material (e.g., polyester) are deposited to obtain an acoustic impedance of 25 MKS Rayls, and the acoustic impedance / air permeability is measured by a Textest instrument or a similar instrument.
[0030] After plasma treatment of the filter medium (8), it can be observed that the acoustic impedance of the composite filter medium (1) of the present invention remains unchanged at a value of 25 MKS Rayls. 5,200 l / m at a pressure of 200 Pa. 2 The air permeability value and filtration efficiency of s are also maintained without change.
[0031] On the other hand, a significant increase is observed in both the contact angle with water (50° to 130°) and the contact angle with oil (50° to 120° for corn oil containing a surface tension of 32 mN / m), where the contact angle is measured in droplets of water or oil on nanofibers (4) using a sessile method with a Kruss instrument (contact angle measurement via droplet deposition and high-resolution camera).
[0032] Declogging test
[0033] To provide evidence for the observations described above, a test method was developed to numerically quantify the energy required to remove oil deposited on the surface of the composite filter medium of the present invention.
[0034] This test was performed using a phorometer (PMI 1200, manufactured by PMI), an instrument utilizing capillary flow porometry, to determine the bubble point, minimum pore size, and pore size distribution of the tested samples. Capillary flow porometry (or simply porometry) is based on a very simple principle of measuring the pressure of a gas required to force a wetting liquid through the pores of a material. The pressure required to empty a pore is inversely proportional to the size of the pore itself. Large pores require low pressure, while small pores require high pressure.
[0035] The test consists of cutting the sample to be analyzed and placing it inside the test chamber. The sample is then secured in place using an O-ring to ensure there is no lateral air leakage. When the chamber is closed, the air permeability of the filter medium is measured, yielding a curve representing the airflow through the sample in relation to the pressure drop measured across the filter medium (the dry curve in the graph of Fig. 5). Once the dry curve is obtained, the test chamber is opened, the sample is placed in place, and the surface is covered with a test liquid having low surface tension (typically < 20 mN / m). Then, the test chamber is closed, and the air permeability of the material is measured again. As the material is blocked by the test liquid, the pressure increases, but no airflow is measured downstream until the pressure becomes high enough to allow the liquid to pass through the pores. From this moment on, the pores, which decrease in size as the pressure value increases, are emptied until the sample (in the previous wet state) is completely dry and the two curves in Fig. 5 overlap. Without going into analytical details, at a qualitative level, the bubble point value (largest pore), the size of the smallest pore, and the distribution of pore sizes can be determined from the difference between the two curves.
[0036] In a specific case, to determine oil repellency / removal ability, a test was performed using corn oil (surface tension 32 mN / m) instead of the test liquid.
[0037] The graph in FIG. 6 shows the emptying pressure and the corresponding pressure drop (energy required for emptying). The samples considered in the graph in FIG. 6 are the filter medium (8) (curve (10)) from electrospinning treatment and the filter medium (1) of the present invention (curve (11)). It can be seen that when using the filter medium (1) of the present invention, oil can be removed at a significantly lower pressure, or at the same pressure, a decisively larger amount of oil can be removed than with the composite filter medium (8) that has not undergone plasma treatment.
[0038] According to the present invention, it has now been surprisingly discovered that by adding a subsequent plasma treatment performed prior to the method described above, which includes a preliminary step of degassing the material forming the monofilament (3) and nanofibers (4) of the composite filter medium (8) to be processed in a vacuum chamber and a step of forming the coating (7), complete polymerization and strong adhesion of the coating subsequently deposited on the monofilaments and nanofibers forming the base fabric are achieved.
[0039] In particular, according to the present invention, prior to the plasma coating (7) formation step, a degassing step of the filter medium (8) obtained from the preceding electrospinning process is performed in the chamber (9) so that the pressure in the chamber (9) becomes a value of 5-250 mTorr. For this purpose, a degassing step is provided with a material exposure time typically ranging from 5 seconds to 5 minutes, depending on the size, weight, and hygroscopicity of the material to be processed. Of course, once an appropriate exposure time is defined that allows for the complete drying of the medium—that is, a time that ensures a stable vacuum in the subsequent coating step—the exact speed of the degassing step must be set according to the exposed area within the chamber. This area is defined by the distance between the unwinding cylinder and the winding cylinder and the electrode size. In particular, if the material is packaged in rolls, the material is continuously unwinded and rewinded inside the chamber (9) at a speed of 0.1 to 50 m / min depending on the moisture content of the material. An opening appropriately controlled by a valve system is provided in the chamber (9) so that gases to be removed can be discharged.
[0040] According to the present invention, moisture contained in the material to be processed in the chamber (9) can be completely removed through a preliminary check of the aforementioned pressure value, thereby enabling the desired polymerization pressure of the coating (7) on the surface of the base fabric and nanofibers to be reached in the subsequent step of the coating formation.
[0041] Additionally, according to the present invention, after the aforementioned degassing treatment and before the step of forming the coating (7), the surface of the monofilament (3) and nanofibers (4) forming the base fabric (2) is reactivated in the chamber (9) by plasma treatment performed in the chamber (9) maintained at a pressure of 10 to 400 mTorr, with an electrode power in the range of 100 to 2000 W, an exposure time in the range of 5 seconds to 5 minutes, and a carrier gas preferably selected from nitrogen, helium, argon, and oxygen. Depending on the gas, exposure time, and power used, a somewhat noticeable etching effect is obtained, and nanometer / micrometer irregularities are formed on the surface to be treated.
[0042] At this stage, since no polymeric monomers are present, no coating is formed on the treated surface. Conversely, ions from a carrier gas appropriately activated by plasma strike the substrate surface with some energy, creating nanogrooves and consequently generating nanometer irregularities that aid in the grip and adhesion of the polymer coating (7) to the surface of the monofilament (3) and nanofibers (4), and significantly contribute to the repulsion of the filter medium against water and oily liquids.
[0043] The results provided by the filter medium produced by the process of the present invention are shown in the table below, the values of which were measured in a filter medium having a layer (7) of polymer material and subsequently obtained by performing plasma treatment for the formation of the latter:
[0044] - A degassing step performed by maintaining the material to be processed inside the chamber (9) for a period of 30 seconds suitable for ensuring a stable pressure of 25 mTorr in subsequent processing;
[0045] - and subsequent plasma treatment step of the material to be coated, performed in the presence of helium as a carrier gas, at a vacuum of 150 mTorr, an electrode power of 600 W, and an exposure time of 1 minute:
[0046]
[0047] From these results, it can be seen how the polymer coating (7) formed in the vacuum chamber (9) after the degassing step and preliminary plasma treatment ensures that the filter medium of the present invention has a very high contact angle (>110°) with oil and a level of adhesion to the substrate much higher than the required minimum.
[0048] In the present invention as described above and illustrated in the attached drawings, modifications may nevertheless be made to produce variations that fall within the scope of the appended claims.
[0049] In particular, when the filter medium starts with slightly hygroscopic materials and undergoes a plasma deposition process, it is possible to perform the plasma treatment and reactivation step using a carrier gas selected from nitrogen, helium, argon, and oxygen alone. In practice, for this type of slightly hygroscopic material, the aforementioned preliminary degassing step may be omitted.
Claims
Claim 1 A method for manufacturing a composite filter medium (1), comprising the steps of forming a composite filter medium (1) by depositing nanofibers (4) on a base fabric (2) through an electrospinning process, and covering the composite filter medium (1) by plasma depositing a coating (7) on the composite filter medium (1) in a vacuum chamber (9), wherein the method comprises the step of degassing the base fabric (2) and the nanofibers (4) forming the composite filter medium (1) in the vacuum chamber (9) after the electrospinning process and before plasma depositing the coating (7). Claim 2 A method according to claim 1, characterized in that during the degassing step, the vacuum chamber (9) has an internal pressure value of 5 to 250 mTorr. Claim 3 A method according to claim 1, characterized in that during the degassing step, the material is exposed to the vacuum chamber (9) for 5 seconds to 5 minutes. Claim 4 A method according to claim 1, wherein, after the degassing step and before plasma deposition of the coating (7), the method further provides a step of forming irregularities on the surface of the base fabric (2) and the nanofibers (4) through plasma treatment of the composite filter medium (1) obtained in the previous degassing step, which is performed in the vacuum chamber (9) in the presence of a carrier gas without a polymer-containing gas. Claim 5 A method according to claim 4, wherein the carrier gas is selected from nitrogen, helium, argon, or oxygen. Claim 6 A method according to claim 5, wherein the plasma treatment is performed in the vacuum chamber (9) at a pressure of 10-400 mTorr, an electrode power of 100-2000 W, and an exposure time of 5 seconds to 5 minutes. Claim 7 A method according to claim 1, wherein the electrospinning process comprises extruding a polymer dissolved in a solvent by means of a nozzle (5), subsequently stretching fibers between the nozzle (5) itself and the electrode, thereby obtaining a deposition of nanometer fibers on the base fabric interposed between the nozzle (5) and the electrode, and the composite filter medium (1) thus obtained subsequently being applied to surface treatment through plasma deposition of a nanometer-thick coating (7) on the exposed surfaces of the base fabric (2) and the nanofibers (4), and obtaining the composite filter medium (1) in which the outer surface of the monofilaments (3) of the base fabric (2) and the nanofibers (4) is coated with the coating (7). Claim 8 A method according to claim 7, wherein the plasma deposition treatment comprises generating a vacuum of 10-50 mTorr, an electrode power of 150-350 W, and an exposure time of 0.5-6 minutes. Claim 9 A method for manufacturing a composite filter medium (1), comprising the steps of forming a composite filter medium (1) by depositing nanofibers (4) on a base fabric (2) through an electrospinning process, and covering the composite filter medium (1) by plasma depositing a coating (7) on the composite filter medium (1) in a vacuum chamber (9), wherein the method comprises the step of forming irregularities on the surface of the base fabric (2) and the nanofibers (4) through plasma treatment of the composite filter medium (1), which is performed in the vacuum chamber (9) in the presence of a carrier gas without a polymer-containing gas after the electrospinning process and before plasma depositing the coating (7). Claim 10 A composite filter medium comprising a base fabric (2) in which nanofibers (4) are deposited, wherein the base fabric (2) and the nanofibers (4) are covered with a nanometer coating (7) applied by a plasma process, and the base fabric (2) and the nanofibers (4) have nanogrooves obtained through plasma treatment in the presence of a carrier gas without a polymer-containing gas. Claim 11 A composite filter medium according to claim 10, wherein the coating (7) is formed by a film having a maximum thickness of 500 nm, including a thickness of 15-60 nm. Claim 12 A composite filter medium according to claim 10, wherein the coating (7) is a coating based on fluorocarbon acrylate having water-repellent and oil-repellent properties. Claim 13 A method according to claim 7, wherein the monofilaments (3) are manufactured starting from monofilaments of polyester, polyamide, polypropylene, polyether sulfone, polyimide, polyamide imide, polyphenylene sulfide, polyether ether ketone, polyvinylidene fluoride, polytetrafluoroethylene, and aramid. Claim 14 A composite filter medium according to claim 10, wherein the base fabric (2) has a mesh opening of 2500-5 microns. Claim 15 In claim 10, the base fabric (2) has a textile structure of 4-300 threads / cm, a thread diameter of 10-500 microns, and 15-300 g / m 2 A composite filter medium characterized by having a weave of weight and a thickness of 18 to 1,000 microns. Claim 16 A composite filter medium according to claim 10, wherein the nanofibers (4) are nanofibers of polyester, polyurethane, polyamide, polyimide, polypropylene, polysulfone, polyethersulfone, polyamideimide, polyphenylene sulfide, polyetheretherketone, polyvinylidene fluoride, polytetrafluoroethylene, alginate, polycarbonate, PVA (polyvinyl alcohol), PLA (polylactic acid), PAN (polyacrylonitrile), PEVA (polyethylene vinyl acetate), PMMA (polymethyl methacrylate), PEO (polyethylene oxide), PE (polyethylene), PVC, PI, or polystyrene. Claim 17 A composite filter medium according to claim 10, wherein the nanofibers (4) have a diameter of 50 nm to 700 nm, and the nanofibers (4) are PVDF (polyvinylidene fluoride) nanofibers with a diameter in the range of 75 to 200 nm. Claim 18 delete
Citation Information
Patent Citations
Composite multilayer filtering construction for use as a subcomponent in acoustic and electronic products in general
KR1020180111827A
Protective air-permeable material and method for producing the same
JP2018134634A
Plasma Fluorination Treatment of Porous Materials
KR100903233B1