Catalytic graphite material, preparation method, and use thereof
Patent Information
- Application Number
- MYPI2025004750
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-08
- Filing Date
- 2023-11-29
- Publication Date
- 2024-08-08
AI Technical Summary
Existing catalytic graphite materials have insufficient performance in lithium-ion batteries, low purity, presence of magnetic substances, high energy consumption during preparation, low production efficiency, and the graphite structure has not been optimized to meet the high-performance needs of lithium-ion battery anode materials.
Catalytic graphite materials including flake graphite and hollow spherical graphite particles are used to prepare catalytic graphite materials with 3R phase through pre-carbonization and heat treatment steps, combined with processes such as isostatic pressing and pickling, to improve its purity and graphitization. degree, and by uniformly loading the catalyst to reduce expansion and increase capacity.
The catalytic graphite material is realized in the lithium-ion battery anode material with high capacity, high first efficiency and low expansion characteristics, significantly improves the electrochemical performance of the lithium-ion battery, and achieves carbon recycling and carbon sequestration effects.
Smart Images

Figure PI2025004750_DRAWING_001 
Figure PI2025004750_DRAWING_002 
Figure PI2025004750_DRAWING_003
Abstract
Description
A catalytic graphite material and its preparation method and application Technical Field
[0001] The present application belongs to the field of battery technology and relates to a catalytic graphite material and a preparation method and application thereof. Background Art
[0002] Anode materials are the core materials of lithium-ion batteries, and graphite anode materials are currently the mainstream anode materials and the most produced and sold anode materials. Currently, higher requirements are being placed on the preparation technology of high-performance anode materials, as well as low-energy consumption and low-cost preparation processes. Biomass has the remarkable advantages of being a widely available raw material, being ecologically safe, and being pollution-free. Converting biomass into graphite anode materials is a carbon sink that not only achieves carbon sequestration but also reduces dependence on fossil fuels such as coal and oil. Using biomass to prepare graphite anode materials for energy storage has significant economic, ecological, and social benefits.
[0003] For example, patent application CN 107406259A discloses a method for producing graphite from biomass. This method involves subjecting biomass to a hydrothermal reaction with a transition metal salt catalyst in a high-temperature, high-pressure reactor, dispersing the catalyst, and thereby obtaining catalyst-loaded hydrothermal carbon. The carbon is then filtered and dried, and then graphitized using an electromagnetic radiation generator. Finally, the product is acid-washed, impurity-removed, washed with water, and dried. However, the high-temperature, high-pressure method for obtaining the hydrothermal carbon and the special graphitization apparatus limit the large-scale, low-cost production of this product.
[0004] Patent application CN 102502598A discloses a method for catalytic graphitization of wood powder. This method uses nano-metal or metal oxide as a catalyst. After the catalyst and wood powder are evenly mixed, the mixture is heat-treated at 900-1600°C to obtain a catalytic graphite material. The disclosed method does not pre-treat the wood powder, resulting in very limited space utilization of the heat treatment carbonization equipment, low production efficiency, and thus high overall energy consumption. In addition, because the synthesized catalytic graphite contains a large amount of catalyst that is not removed, the catalytic graphite material contains a large amount of magnetic material, which makes it unusable in lithium-ion batteries.
[0005] Patent application number CN 109301225A discloses a graphite negative electrode material with a dual-gradient structure of graphitization degree and pore size, and its preparation and application. The method requires first obtaining a porous carbon material with anthracite, biochar, petroleum coke, or pitch carbon as a carbon source, and the specific surface area of the carbon material is 100-2000m 2 / g, immersing the porous carbon material in a catalyst solution containing water-insoluble or water-soluble metal salts, nanometals, and water-soluble non-metallic salts, evacuating the container, and then drying to load the catalyst into the pores of the porous carbon material, followed by two-stage electric calcination. The main components added in this process are amorphous carbon sources of asphalt and resin, and finally forming a radial gradient structure; the disclosed method involves a process of activation and pore formation to obtain the porous carbon material, which will cause a large amount of carbon element loss, not only increasing the preparation cost, but also reducing the yield of the final finished graphite material.
[0006] It can be seen that the performance of the catalytic graphite materials disclosed in the prior art when applied to lithium-ion batteries needs to be improved, and the purity is not high. For example, the silicon impurities contained in biomass or coal-based raw materials often exist in the form of silicon dioxide and silicates. After the catalytic reaction, they are still retained. If they are not removed, their mass ratio will affect the overall gram capacity of the catalytic graphite, thereby reducing the capacity of the lithium-ion battery; and the main focus of the prior art is on the conversion rate and graphitization degree of the catalytic graphite, and the graphite structure required for the high performance of the negative electrode material of the lithium-ion battery is not focused on or ignored. Therefore, the application of the negative electrode material of the lithium-ion battery is not based on the The key processes of catalytic synthesis are optimized by taking into account the low expansion, high capacity and high first-effect graphite structural characteristics required; at the same time, in the preparation process of catalytic graphite, the carbon material needs to be activated to become a porous carbon material before the catalyst is loaded in order to impregnate the catalyst solution. The activation process will cause a large amount of carbon source loss, which not only has the cost of the activation process, but also reduces the yield of the final finished graphite material, resulting in high production costs; in addition, the existing technology for the treatment of biomass involves high-temperature and high-pressure hydrothermal reactions, and the catalytic conversion uses an electromagnetic radiation generator for heating, which limits the large-scale and low-cost production of the product.
[0007] Based on the above research, there is a need to provide a catalytic graphite material, which exhibits the advantages of high capacity, high initial efficiency and low expansion when applied to lithium-ion battery negative electrode materials.
[0008] Summary of the Invention
[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0010] The purpose of this application is to provide a catalytic graphite material and its preparation method and application. The catalytic graphite material has high purity, high degree of graphitization and 3R phase. When the catalytic graphite material is used as a negative electrode material for lithium-ion batteries, it exhibits the characteristics of high capacity, high initial efficiency and low expansion, thereby significantly improving the electrochemical properties such as capacity and initial efficiency of lithium-ion batteries.
[0011] To achieve this goal, this application adopts the following technical solutions:
[0012] In a first aspect, the present application provides a catalytic graphite material, wherein the catalytic graphite material comprises flake graphite and hollow spherical graphite particles, and the catalytic graphite material has a 3R phase.
[0013] The catalytic graphite material described in the present application has a 3R phase (rhombohedral phase). Since the 3R structure of graphite is closely related to the high-capacity electrochemical properties of the graphite negative electrode material, the presence of the 3R phase provides more embedding sites for lithium ions. Therefore, the catalytic graphite material has better electrochemical properties than artificial graphite and natural graphite. At the same time, the present application also includes flake graphite and hollow spherical graphite, wherein the flake graphite has different orientations, bending and folding to form a pore structure, and combined with hollow graphite particles, it can provide space for the expansion of the graphite material, and the catalytic graphite material has a small specific surface area and low orientation, so that the performance of the product has a higher first coulomb and low expansion characteristics than the catalytic graphite of the prior art.
[0014] In one embodiment, the catalytic graphite material further comprises particle aggregates and random particles.
[0015] The catalytic graphite material described in the present application includes flake graphite, hollow spherical graphite, particle aggregates and irregular particles. The graphite materials with various morphologies reduce the degree of anisotropy of the catalytic graphite material, thereby showing the advantage of low expansion when used as negative electrode materials for lithium-ion batteries.
[0016] In one embodiment, the degree of graphitization of the catalytic graphite material is g, 95%≤g<100%, for example, it can be 95%, 96%, 97%, 98%, 99% or 99.9%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] In one embodiment, the sphericity of the hollow spherical graphite particles is greater than 0.7, for example, 0.75, 0.8, 0.85, or 0.9, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] The sphericity described in this application is the ratio of the shortest axis to the longest axis of the particle.
[0019] In one embodiment, the outer diameter of the hollow spherical graphite particles is D, wherein 5<D<50μm, for example, it can be 6μm, 10μm, 20μm, 30μm, 40μm or 49μm, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, and 10<D<30μm can be selected.
[0020] In one embodiment, the R value of the catalytic graphite material is in the range of 0.03-0.4, for example, it can be 0.03, 0.05, 0.1, 0.2, 0.3, 0.4 or 0.5, but is not limited to the listed values. Other values not listed in the numerical range are also applicable, where R value = I D / I G , I D is the peak intensity value of D peak, I G is the peak intensity value of the G peak, and the Raman shift of the D peak is 1350cm -1 The Raman shift of the G peak is around 1580 cm -1 nearby.
[0021] In one embodiment, the average value of the R value is less than 0.25, for example, it can be 0.24, 0.2, 0.18, 0.16, 0.14, or 0.12, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] In a second aspect, the present application provides a method for preparing the catalytic graphite material as described in the first aspect, the preparation method comprising the following steps:
[0023] (1) pre-carbonizing a carbon source to obtain carbon powder, mixing the carbon powder with a catalyst solution, and then performing solid-liquid separation to obtain catalyst-loaded composite particles;
[0024] (2) Heat treating the composite particles in step (1), and then performing post-treatment to obtain the catalytic graphite material.
[0025] In this application, the carbon source is first pre-carbonized so that the inherent pores of the carbon source or the gaps formed between the macromolecular structure are retained during the pre-carbonization process, and during the pre-carbonization process, small molecules will overflow to form tiny microchannels; then the carbon powder obtained by pre-carbonization is mixed with the catalyst solution, and the catalyst solution is filled into the gaps in the carbon powder, thereby obtaining composite particles with the catalyst uniformly loaded on the carbon surface and in the pore structure. Finally, after high-temperature heat treatment and post-processing to remove the catalyst, a catalytic graphite material with a purity of ≥99.9% is obtained. When the obtained catalytic graphite material is used as a negative electrode material for lithium-ion batteries, it exhibits the characteristics of high capacity, high initial efficiency and low expansion.
[0026] In one embodiment, the mixing of the carbon powder and the catalyst solution in step (1) comprises vacuum impregnating the carbon powder in the catalyst solution.
[0027] The carbon powder described in the present application can be optionally immersed in a catalyst solution under vacuum conditions, so that the catalyst solution can be fully filled in the gaps in the carbon powder, thereby facilitating the efficient and high-quality conversion of the carbon material into catalytic graphite.
[0028] In one embodiment, the vacuum impregnation time is 1-2.5 hours, for example, 1 hour, 1.5 hours, 2 hours or 2.5 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] In one embodiment, the mass ratio of the carbon powder and the catalyst solution in step (1) is 1:(4-7), for example, it can be 1:4, 1:5, 1:6 or 1:7, but is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0030] The amount of the catalyst described in this application can further improve the electrochemical performance of the catalytic graphite material within a reasonable range. If the amount of the catalyst is too much, the difficulty of acid washing and purification will increase, which will increase the production cost, and it will easily lead to an excessively large specific surface area of the catalytic graphite, so that the catalytic graphite material exhibits poor first coulombic efficiency. If the amount of the catalyst is too small, the catalytic conversion effect is poor, and the catalytic conversion rate is not high, so that the catalytic graphite material exhibits poor capacity and first coulombic efficiency.
[0031] In one embodiment, the mass of material A obtained after the solid-liquid separation in step (1) is 3-3.7 times the mass of the carbon powder, for example, it can be 3 times, 3.2 times, 3.4 times, 3.6 times or 3.7 times, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] In one embodiment, the catalyst solution in step (1) comprises a catalyst and water in a mass ratio of (1-2):1, for example, 1:1, 1.5:1 or 2:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] In one embodiment, the pre-carbonization temperature in step (1) is 500-1200°C, for example, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C or 1200°C, and the time is 1-6h, for example, 1h, 2h, 3h, 4h, 5h or 6h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] In one embodiment, the pre-carbonization in step (1) is performed under a protective gas, and the protective gas includes any one of nitrogen, argon, krypton or helium, or a combination of at least two of them.
[0035] In one embodiment, the particle size D50 of the carbon powder in step (1) is 5-45 μm, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm or 45 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] In one embodiment, the solid-liquid separation method in step (1) includes filter press.
[0037] In one embodiment, after the solid-liquid separation in step (1), drying is further performed, and the drying temperature is 150-300°C, for example, 150°C, 200°C, 250°C or 300°C, and the drying time is 2-4h, for example, 2h, 3h or 4h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] In one embodiment, the catalyst in step (1) comprises an inorganic salt and / or an organic salt, preferably an inorganic salt and / or an organic salt of any one or a combination of at least two of vanadium, chromium, manganese, iron, cobalt, nickel or copper, typical but non-limiting combinations include a combination of vanadium and chromium, and a combination of manganese and iron.
[0039] In one embodiment, the carbon source in step (1) includes a biomass carbon source and / or a biomass secondary processed material.
[0040] The carbon source described in this application is a carbon-containing biomass raw material with pores, and a biomass secondary processed material that can form voids.
[0041] In one embodiment, the biomass carbon source includes any one of straw, fruit shell, wood or bamboo, or a combination of at least two of them. Typical but non-limiting combinations include a combination of straw and fruit shell, or a combination of wood and bamboo.
[0042] In one embodiment, the biomass secondary processing material includes any one or a combination of at least two of glucose, sucrose, starch, lignin, cellulose or hemicellulose. Typical but non-limiting combinations include a combination of glucose and sucrose, and a combination of starch and lignin.
[0043] In one embodiment, before the heat treatment in step (2), the composite particles are further subjected to isostatic pressing.
[0044] The present application performs isostatic pressing before heat treatment to further reduce residual voids and improve the contact between the catalyst and carbon, thereby facilitating the catalytic conversion of carbon to graphite material. At the same time, it is beneficial for part of the catalyst to be wrapped by carbon powder, which can form graphite hollow spheres after post-treatment removal.
[0045] In one embodiment, the pressure rise rate of the isostatic pressing treatment is 5-100 MPa / min, for example, it can be 5 MPa / min, 10 MPa / min, 20 MPa / min, 40 MPa / min, 60 MPa / min, 80 MPa / min or 100 MPa / min, and the pressure is 200-400 MPa, for example, it can be 200 MPa, 300 MPa or 400 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] In one embodiment, the holding time of the isostatic pressing treatment is 10-120 min, for example, it can be 10 min, 30 min, 50 min, 70 min, 90 min, 110 min or 120 min, the pressure reduction rate is 5-100 MPa / min, for example, it can be 5 MPa / min, 10 MPa / min, 20 MPa / min, 40 MPa / min, 60 MPa / min, 80 MPa / min or 100 MPa / min, and the pressure is 200-400 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0047] In one embodiment, the isostatic pressing treatment is performed no less than twice, for example, twice, three times, four times or five times, but is not limited to the listed values, and other unlisted integer values within the numerical range are also applicable.
[0048] The isostatic pressing treatment described in the present application is within a certain pressure range. The greater the isostatic pressing pressure peak, the more conducive it is to the catalytic conversion of carbon to graphite, and the pressure causes part of the catalyst to be tightly wrapped by the carbon powder, so that during the catalytic conversion process, this part of the carbon is converted into graphite on the catalyst surface, and hollow graphite spheres are obtained after removing the catalyst; however, when the pressure value is too large, exceeding the compressive resistance of the carbon powder or catalyst, the pressed material begins to crack, expand and pulverize, which is not conducive to the catalytic effect; in addition, within a suitable pressure range, slow pressure increase, extended pressure holding time, slow pressure release, and multiple isostatic pressing processes are all beneficial to the subsequent catalytic conversion of carbon to graphite.
[0049] In one embodiment, the temperature of the heat treatment in step (2) is 1300-1900°C, for example, 1300°C, 1500°C, 1700°C or 1900°C, and the time is 1-5h, for example, 1h, 2h, 3h, 4h or 5h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] In one embodiment, the post-treatment in step (2) includes pickling, water washing and drying performed in sequence.
[0051] In one embodiment, the pickling solution used in the pickling comprises hydrochloric acid and / or hydrofluoric acid.
[0052] In one embodiment, the concentration of the hydrochloric acid is 0.8-1.2 mol / L, for example, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L or 1.2 mol / L, and the concentration of the hydrofluoric acid is 0.3-0.7 mol / L, for example, 0.3 mol / L, 0.5 mol / L or 0.7 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] In one embodiment, the drying temperature is 150-300°C, for example, 150°C, 200°C, 250°C or 300°C, and the drying time is 0.5-3h, for example, 0.5h, 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] As an optional technical solution of the preparation method described in this application, the preparation method comprises the following steps:
[0055] (1) Pre-carbonizing the carbon source at a temperature of 500-1200° C. for 1-6 hours under protective gas to obtain carbon powder with a particle size D50 of 5-45 μm, then vacuum impregnating the carbon powder in a catalyst solution for 1-2.5 hours, and then performing filter pressing. The filter cake obtained by filter pressing is then dried at 150-300° C. for 2-4 hours to obtain catalyst-loaded composite particles;
[0056] The mass ratio of the carbon powder to the catalyst solution is 1:(4-7);
[0057] (2) The composite particles in step (1) are pressurized to 200-400 MPa at a pressure increase rate of 5-100 MPa / min and subjected to isostatic pressing for 10-120 min, and then the pressure is released at a pressure reduction rate of 5-100 MPa / min to obtain an isostatically pressed material. The isostatically pressed material is heat-treated at a temperature of 1300-1900° C. for 1-5 h, and then acid-washed, water-washed, and dried in sequence to obtain the catalytic graphite material.
[0058] In a third aspect, the present application provides a lithium-ion battery, wherein the lithium-ion battery comprises the catalytic graphite material as described in the first aspect.
[0059] Compared with the prior art, this application has the following beneficial effects:
[0060] The catalytic graphite material described in the present application has a 3R phase and includes flake graphite and hollow spherical graphite. Through the combination of flake graphite and hollow graphite, the catalytic graphite material has better electrochemical properties than artificial graphite, natural graphite and conventional catalytic graphite materials. Therefore, when the catalytic graphite material described in the present application is used as a negative electrode material for lithium-ion batteries, it exhibits the advantages of high capacity, high initial efficiency and low expansion; at the same time, the present application improves the preparation method to achieve a densification treatment between the catalyst and the carbon powder, thereby obtaining higher-quality biomass graphite, and realizing true carbon recycling and carbon fixation effects in the field of new energy.
[0061] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0063] FIG1 is a SEM image of the carbon powder described in Example 1 of the present application;
[0064] FIG2 is a SEM image of the composite particles described in Example 1 of the present application;
[0065] FIG3 is a SEM image of a cross section of the composite particles described in Example 1 of the present application;
[0066] FIG4 is a mapping diagram of C in the composite particles described in Example 1 of the present application;
[0067] FIG5 is a mapping diagram of Ni in the composite particles described in Example 1 of the present application;
[0068] FIG6 is an XRD pattern of the catalytic graphite material described in Example 1 of the present application in the range of 2θ of 20-80°;
[0069] FIG7 is an XRD pattern of the catalytic graphite material described in Example 1 of the present application in the range of 2θ of 40-48°;
[0070] FIG8 is an XRD pattern of the catalytic graphite material described in Example 1 of the present application in the range of 2θ of 52-80°;
[0071] FIG9 is a Raman 2D image and corresponding optical image obtained by laser Raman spectroscopy scanning of the catalytic graphite material described in Example 1 of the present application;
[0072] FIG10 is a SEM image of flake graphite in the catalytic graphite material described in Example 1 of the present application;
[0073] FIG11 is a SEM image of hollow spherical graphite particles in the catalytic graphite material described in Example 1 of the present application;
[0074] FIG12 is a SEM image of particle aggregates in the catalytic graphite material described in Example 1 of the present application;
[0075] FIG13 is a SEM image of irregular particles in the catalytic graphite material described in Example 1 of the present application;
[0076] FIG14 is a SEM image of hollow spherical graphite particles after rupture in the catalytic graphite material described in Example 1 of the present application;
[0077] FIG15 is a cross-sectional morphology diagram of the catalytic graphite material described in Example 1 of the present application;
[0078] FIG16 is a charge and discharge curve diagram of a battery made of the catalytic graphite material described in Example 1 of the present application;
[0079] FIG17 is a charge and discharge curve diagram of a battery made of the catalytic graphite material described in Example 5 of the present application;
[0080] FIG18 is a charge and discharge curve diagram of a battery made of the catalytic graphite material described in Example 7 of the present application;
[0081] FIG19 is a cross-sectional SEM image of the artificial graphite material described in Comparative Example 2 of the present application;
[0082] FIG20 is an XRD pattern of the artificial graphite material described in Comparative Example 2 of the present application in the range of 2θ of 20-80°;
[0083] FIG21 is an XRD pattern of the artificial graphite material described in Comparative Example 2 of the present application in the range of 2θ of 40-48°;
[0084] FIG22 is an XRD pattern of the artificial graphite material described in Comparative Example 2 of the present application in the range of 2θ of 52-80°;
[0085] FIG23 is a SEM image of the flake graphite material described in Comparative Example 3 of the present application at a scale of 500 μm;
[0086] FIG24 is a SEM image of the flake graphite material described in Comparative Example 3 of the present application at a scale of 20 μm;
[0087] FIG25 is an XRD pattern of the flake graphite material described in Comparative Example 3 of the present application when 2θ is in the range of 20-80°;
[0088] FIG26 is an XRD pattern of the flake graphite material described in Comparative Example 3 of the present application when 2θ is in the range of 40-48°;
[0089] FIG27 is an XRD pattern of the flake graphite material described in Comparative Example 3 of the present application when 2θ is in the range of 52-80°;
[0090] FIG28 is an XRD pattern of the catalytic graphite material described in Example 1 of the present application and the flake graphite material described in Comparative Example 3 in the range of 2θ of 12-32°;
[0091] FIG29 is a SEM image of the spheroidized natural graphite material described in Comparative Example 4 of the present application;
[0092] Figure 30 is a cross-sectional SEM image of the spheroidized natural graphite material described in Comparative Example 4 of the present application;
[0093] FIG31 is a Raman 2D image and corresponding optical image obtained by laser Raman spectrum scanning of the spheroidized natural graphite material described in Comparative Example 4 of the present application. DETAILED DESCRIPTION
[0094] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0095] Example 1
[0096] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0097] The preparation method of the catalytic graphite material comprises the following steps:
[0098] (1) The corn stalks were pre-carbonized at 900°C for 1 h under nitrogen protection and crushed to obtain carbon powder with a particle size D50 of 45 μm. The carbon powder was then vacuum impregnated in a catalyst solution. After vacuum impregnation for 1 h, the mixture was filtered to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3.7 times that of the carbon powder, that is, the mass ratio of carbon powder to catalyst solution was 1:2.7. The mixture was then dried at 300°C for 2 h to obtain catalyst-loaded composite particles.
[0099] The mass ratio of the carbon powder to the catalyst solution is 1:5; the catalyst solution comprises nickel chloride and water in a mass ratio of 1.8:1;
[0100] (2) The composite particles in step (1) are pressurized to 350 MPa at a pressure increasing rate of 5 MPa / min and subjected to isostatic pressing for 120 min, and then the pressure is released at a pressure decreasing rate of 5 MPa / min to obtain an isostatically pressed material, the isostatically pressed material is heat-treated at a temperature of 1900° C. for 1 h, and then pickled with a mixture of 1 mol / L hydrochloric acid and 0.5 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 200° C. for 2 h to obtain the catalytic graphite material;
[0101] The SEM image of the carbon powder of this embodiment is shown in FIG1 , the SEM image of the composite particles is shown in FIG2 , the SEM image of the cross section of the composite particles is shown in FIG3 , the mapping diagram of C in the composite particles is shown in FIG4 , and the mapping diagram of Ni is shown in FIG5 ;
[0102] The XRD pattern of the catalytic graphite material in the range of 20-80° at 2θ is shown in FIG6 , the XRD pattern in the range of 40-48° at 2θ is shown in FIG7 , the XRD pattern in the range of 52-80° at 2θ is shown in FIG8 , the Raman 2D imaging and the corresponding optical image obtained by laser Raman spectroscopy are shown in FIG9 , the SEM image of the flake graphite in the catalytic graphite material is shown in FIG10 , the SEM image of the hollow spherical graphite particles is shown in FIG11 , the SEM image of the particle aggregates is shown in FIG12 , the SEM image of the irregular particles is shown in FIG13 , and the SEM image of the hollow spherical graphite particles after rupture is shown in FIG14 ; the cross-sectional morphology of the catalytic graphite material is shown in FIG15 , and the charge and discharge curve of the battery made of the catalytic graphite material is shown in FIG16 .
[0103] The XRD pattern in the 2θ range of 12-32° is shown in FIG28 .
[0104] Example 2
[0105] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0106] The preparation method of the catalytic graphite material comprises the following steps:
[0107] (1) Soybean straw was pre-carbonized at 1200°C for 2 h under nitrogen protection and crushed.
[0108] A carbon powder having a particle size D50 of 37 μm was obtained, and then the carbon powder was vacuum impregnated in a catalyst solution. After vacuum impregnation for 1.5 hours, filter pressing was performed to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3.3 times the mass of the carbon powder, that is, the mass ratio of carbon powder to catalyst solution was 1:2.3. The material was then dried at 250°C for 2.5 hours to obtain catalyst-loaded composite particles.
[0109] The mass ratio of the carbon powder to the catalyst solution is 1:5; the catalyst solution comprises cobalt chloride and water in a mass ratio of 1:1;
[0110] (2) The composite particles in step (1) are pressurized to 400 MPa at a pressure increasing rate of 50 MPa / min and subjected to isostatic pressing for 120 min, and then the pressure is released at a pressure decreasing rate of 50 MPa / min to obtain an isostatically pressed material. The isostatically pressed material is heat-treated at a temperature of 1700°C for 3 h, and then pickled with a mixture of 0.8 mol / L hydrochloric acid and 0.7 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 250°C for 1 h to obtain the catalytic graphite material.
[0111] Example 3
[0112] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0113] The preparation method of the catalytic graphite material comprises the following steps:
[0114] (1) Coconut shells were pre-carbonized at 800°C for 2 h under nitrogen protection and crushed to obtain carbon powder with a particle size D50 of 25 μm. The carbon powder was then vacuum impregnated in a catalyst solution. After vacuum impregnation for 2 h, the mixture was filtered to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3 times that of the carbon powder, i.e., the mass ratio of carbon powder to catalyst solution was 1:2.0. The mixture was then dried at 150°C for 4 h to obtain catalyst-loaded composite particles.
[0115] The mass ratio of the carbon powder to the catalyst solution is 1:6; the catalyst solution comprises ferric chloride and water in a mass ratio of 1:1;
[0116] (2) The composite particles in step (1) are pressurized to 200 MPa at a pressure increasing rate of 10 MPa / min and subjected to isostatic pressing for 60 min, and then the pressure is released at a pressure decreasing rate of 5 MPa / min to obtain an isostatically pressed material. The isostatically pressed material is heat-treated at a temperature of 1300°C for 4 h, and then pickled with a mixture of 1 mol / L hydrochloric acid and 0.5 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 300°C for 0.5 h to obtain the catalytic graphite material.
[0117] Example 4
[0118] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0119] The preparation method of the catalytic graphite material comprises the following steps:
[0120] (1) Beech wood was pre-carbonized at 600°C for 3 h under argon protection and crushed to obtain carbon powder with a particle size D50 of 20 μm. The carbon powder was then vacuum impregnated in a catalyst solution. After vacuum impregnation for 2 h, the mixture was filtered to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3.2 times that of the carbon powder, i.e., the mass ratio of carbon powder to catalyst solution was 1:2.2. The carbon powder was then dried at 150°C for 4 h to obtain catalyst-loaded composite particles.
[0121] The mass ratio of the carbon powder to the catalyst solution is 1:4; the catalyst solution comprises ferric nitrate and water in a mass ratio of 1.5:1;
[0122] (2) The composite particles in step (1) are pressurized to 250 MPa at a pressure increasing rate of 50 MPa / min and subjected to isostatic pressing for 10 min, and then the pressure is released at a pressure decreasing rate of 50 MPa / min to obtain an isostatically pressed material. The isostatically pressed material is heat-treated at a temperature of 1500°C for 3 h, and then pickled with a mixture of 1.2 mol / L hydrochloric acid and 0.3 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 150°C for 3 h to obtain the catalytic graphite material.
[0123] Example 5
[0124] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0125] The preparation method of the catalytic graphite material comprises the following steps:
[0126] (1) Poplar wood was pre-carbonized at 700°C for 3 h under nitrogen protection and crushed to obtain carbon powder with a particle size D50 of 9 μm. The carbon powder was then vacuum impregnated in a catalyst solution. After vacuum impregnation for 2.5 h, it was filtered to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3.4 times the mass of the carbon powder, that is, the mass ratio of carbon powder to catalyst solution was 1:2.4. The carbon powder was then dried at 150°C for 4 h to obtain catalyst-loaded composite particles.
[0127] The mass ratio of the carbon powder to the catalyst solution is 1:7; the catalyst solution comprises cobalt sulfate and water in a mass ratio of 1:1;
[0128] (2) The composite particles in step (1) are pressurized to 250 MPa at a pressure increasing rate of 20 MPa / min and subjected to isostatic pressing for 30 min, and then the pressure is released at a pressure decreasing rate of 20 MPa / min to obtain an isostatically pressed material, which is heat-treated at a temperature of 1300° C. for 4 h, and then pickled with a mixture of 1 mol / L hydrochloric acid and 0.5 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 150° C. for 3 h to obtain the catalytic graphite material;
[0129] The charge and discharge curve of the battery made of the catalytic graphite material described in this embodiment is shown in FIG17 .
[0130] Example 6
[0131] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0132] The preparation method of the catalytic graphite material comprises the following steps:
[0133] (1) Bamboo was pre-carbonized at 700°C for 4 h under nitrogen protection and crushed to obtain carbon powder with a particle size D50 of 43 μm. The carbon powder was then vacuum impregnated in a catalyst solution. After vacuum impregnation for 1 h, it was filtered to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3.1 times the mass of the carbon powder, that is, the mass ratio of carbon powder to catalyst solution was 1:2.1. The carbon powder was then dried at 200°C for 3 h to obtain catalyst-loaded composite particles.
[0134] The mass ratio of the carbon powder to the catalyst solution is 1:5; the catalyst solution comprises cobalt chloride, nickel chloride and water in a mass ratio of 1:1:1;
[0135] (2) The composite particles in step (1) are pressurized to 400 MPa at a pressure increasing rate of 100 MPa / min and subjected to isostatic pressing for 60 min, and then the pressure is released at a pressure decreasing rate of 100 MPa / min to obtain an isostatically pressed material. The isostatically pressed material is heat-treated at a temperature of 1700°C for 5 h, and then pickled with a mixture of 1 mol / L hydrochloric acid and 0.5 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 150°C for 3 h to obtain the catalytic graphite material.
[0136] Example 7
[0137] This embodiment provides a catalytic graphite material having a 3R phase, including flake graphite, hollow spherical graphite particles, particle aggregates, and random particles;
[0138] The preparation method of the catalytic graphite material comprises the following steps:
[0139] (1) Lignin was pre-carbonized at 500°C for 6 h under argon protection and crushed to obtain carbon powder with a particle size D50 of 5 μm. The carbon powder was then vacuum impregnated in a catalyst solution. After vacuum impregnation for 2 h, it was filtered to obtain material A containing the catalyst solution. The mass of material A was weighed to be 3.4 times the mass of the carbon powder, that is, the mass ratio of carbon powder to catalyst solution was 1:2.4. The material was then dried at 200°C for 4 h to obtain catalyst-loaded composite particles.
[0140] The mass ratio of the carbon powder to the catalyst solution is 1:5; the catalyst solution comprises cobalt chloride, nickel chloride, ferric chloride and water in a mass ratio of 0.6:0.6:0.6:1;
[0141] (2) The composite particles in step (1) are pressurized to 350 MPa at a pressurization rate of 5 MPa / min and subjected to isostatic pressing for 120 min, then depressurized at a depressurization rate of 5 MPa / min, and the isostatic pressing is repeated once to obtain a static pressing material, which is heat-treated at a temperature of 1900° C. for 2 h, and then pickled with a mixture of 1 mol / L hydrochloric acid and 0.5 mol / L hydrofluoric acid. After pickling, the material is filtered and washed with water, and finally dried at 150° C. for 3 h to obtain the catalytic graphite material;
[0142] The charge and discharge curve of the battery made of the catalytic graphite material described in this embodiment is shown in FIG18 .
[0143] Example 8
[0144] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that of Example 1 except that in the preparation method, the vacuum impregnation in step (1) is replaced by mechanical stirring to change the adaptability of the obtained catalytic graphite material.
[0145] Specifically, the mechanical stirring includes the following steps: stirring the carbon powder and the catalyst solution at a stirring rate of 60 rpm for 1 hour and then filtering to obtain material A containing the catalyst solution. The mass of material A is 2.6 times the mass of the carbon powder, that is, the mass ratio of carbon powder to catalyst solution is 1:1.6.
[0146] Example 9
[0147] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that the temperature of the heat treatment in step (2) in the preparation method is 1100° C. to adapt the obtained catalytic graphite material.
[0148] Example 10
[0149] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that the temperature of the heat treatment in step (2) in the preparation method is 2100° C. to adapt the obtained catalytic graphite material.
[0150] Example 11
[0151] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that in the preparation method, step (2) is not acid-washed to change the adaptability of the obtained catalytic graphite material.
[0152] Example 12
[0153] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that in the preparation method, step (2) is not subjected to isostatic pressing, which changes the adaptability of the obtained catalytic graphite material.
[0154] Example 13
[0155] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that in the preparation method, the pressure is increased to 100 MPa in step (2) to adapt the obtained catalytic graphite material.
[0156] Example 14
[0157] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that in the preparation method, the pressure is increased to 500 MPa in step (2) to change the adaptability of the obtained catalytic graphite material.
[0158] Example 15
[0159] This embodiment provides a catalytic graphite material. The catalytic graphite material is the same as that in Example 1 except that in the preparation method, step (1) is not pre-carbonized to change the adaptability of the obtained catalytic graphite material.
[0160] Comparative Example 1
[0161] This comparative example provides a carbon material, which is the same as Example 1 except that nickel chloride is not added in the preparation method to change the adaptability of the obtained carbon material.
[0162] Comparative Example 2
[0163] This comparative example provides an artificial graphite material, and the preparation method of the artificial graphite material comprises the following steps:
[0164] (1) Grinding the coal-based needle-shaped green coke into coke powder with a particle size D50 of 10 μm;
[0165] (2) graphitizing the coke powder described in step (1) in a graphitization furnace at a graphitization temperature of 3000° C. for 10 h, and then cooling the material to room temperature to obtain an artificial graphite material;
[0166] The cross-sectional SEM image of the artificial graphite material described in this comparative example is shown in Figure 19, the XRD pattern in the range of 2θ of 20-80° is shown in Figure 20, the XRD pattern in the range of 2θ of 40-48° is shown in Figure 21, and the XRD pattern in the range of 2θ of 52-80° is shown in Figure 22.
[0167] Comparative Example 3
[0168] This comparative example provides a flaky natural graphite material, and the preparation method of the natural graphite material comprises the following steps:
[0169] (1) Purifying -195 flake natural graphite with mixed acid, wherein the mixed acid solution is prepared by mixing aqua regia and 5 mol / L hydrofluoric acid solution in a mass ratio of 2:1;
[0170] (2) washing and drying the acid-washed flaky natural graphite at a temperature of 300° C. for 0.5 h to obtain the flaky natural graphite material;
[0171] The SEM image of the flaky graphite material at a scale of 500 μm is shown in FIG23 , the SEM image at a scale of 20 μm is shown in FIG24 , the XRD pattern in the range of 20-80° is shown in FIG25 , the XRD pattern in the range of 40-48° is shown in FIG26 , the XRD pattern in the range of 52-80° is shown in FIG27 , and the XRD pattern in the range of 2θ of 12-32° is shown in FIG28 .
[0172] Comparative Example 4
[0173] This comparative example provides a spheroidized natural graphite material, and the preparation method of the spheroidized natural graphite material comprises the following steps:
[0174] (1) crushing the flotation-separated -195 flaky natural graphite to a Dv50 of 16 μm, and then spheroidizing the flaked natural graphite in a spheroidizer to obtain spheroidized natural graphite;
[0175] (2) purifying the spheroidized natural graphite with mixed acid, wherein the mixed acid solution is prepared by mixing aqua regia and 5 mol / L hydrofluoric acid solution in a mass ratio of 2:1;
[0176] (3) washing and drying the spheroidized natural graphite after acid washing and purification at a drying temperature of 300° C. for 0.5 h, thereby obtaining the spheroidized natural graphite material;
[0177] The SEM image of the spheroidized natural graphite material is shown in FIG29 , the cross-sectional SEM image is shown in FIG30 , and the Raman 2D imaging and corresponding optical image obtained by laser Raman spectroscopy are shown in FIG31 .
[0178] The materials obtained from the above examples and comparative examples were tested, and the tests included:
[0179] (1) The sample was scanned by XRD spectrum. The X-ray diffractometer used a copper target with a wavelength of 0.154056 nm and a scanning speed of about 4° / min. The spectrum information was obtained by analysis software such as HighScore Plus and Jade. The orientation of graphite is determined by the ratio of the peak intensity of the (004) peak near 54.5° to the peak intensity of the (110) peak near 77.7°. 004 / I 110 ;
[0180] (2) Observe the morphology of the sample using a scanning electron microscope;
[0181] (3) The basic principle of Raman detection is not to damage or ablate the sample. The sample is detected by a laser Raman spectrometer with a laser wavelength of 532nm. Raman 2D imaging, i.e., Raman's surface scanning function, is used to scan the sample selection area. The area is actually composed of 400 single-point Raman spectra. The instrument's built-in function calculates the R values of the above 400 single-point laser Raman spectra and obtains a color cloud map of the distribution of the R values of the measured area. On the right side of the cloud map, colored columns are used to represent the R values represented by different colors in the cloud map, and the average value and standard deviation are calculated. The R=I D / I G , I D is the peak intensity value of D peak, I G is the peak intensity value of the G peak, and the Raman shift of the D peak is 1350cm -1 The Raman shift of the G peak is around 1580 cm -1 nearby;
[0182] (4) The sample was cut and polished by argon ion beam, and the cross-sectional structure of the sample was observed by scanning electron microscopy;
[0183] (5) The graphitization degree of the sample was determined according to the method described in GB / T 24533-2019;
[0184] (6) The first coulombic efficiency and the first lithium de- / intercalation capacity of the sample are tested according to the following method: the negative electrode sheet is obtained by coating, drying and rolling after slurrying according to the mass ratio of graphite negative electrode material: CMC: SP: SBR = 93.5:1.5:2:3, and then a CR2430 button half-cell is prepared, and the electrode is a metal lithium sheet; the first lithium insertion capacity and lithium de-capacity and the first coulombic efficiency of the graphite negative electrode material are tested, and the button half-cell is discharged to 0.005V at 0.1C, and allowed to stand for 10 minutes, and then discharged to 0.005V at 0.01C, and allowed to stand for 10 minutes, and then charged to 2V at 0.1C, and then ended, thereby obtaining the first lithium insertion capacity and lithium de-capacity, respectively. The ratio of the first lithium de-capacity to the lithium insertion capacity is the first coulombic efficiency;
[0185] (7) The specific surface area of the sample shall be determined in accordance with the provisions of GB / T 19587;
[0186] (8) The true density of the sample is measured according to the method described in GB / T 24533-2019;
[0187] (9) The ash content of the sample was determined according to the method described in YS / T 63.19-2012.
[0188] The I obtained by the test 004 / I 110 , graphitization degree, R value, first delithiation capacity, first coulombic efficiency, BET, true density and ash content are shown in the following table.
[0189] Table 1
[0190] From Table 1 and the accompanying drawings, we can see that:
[0191] (1) Figure 1 shows the characteristic structure of biochar and its natural pores. Figure 2 shows that the catalyst is evenly dispersed on the surface and pores of biochar. Figure 5 shows that the catalyst is evenly dispersed in the internal voids of biochar. Figures 6-8 show that there is an obvious 3R phase near 43.3° and 46.1°. The orientation result is 1.77 based on the ratio of the (004) and (110) peak intensities. The reason for the low orientation is that there are graphite balls, clusters of small particles and irregular graphite particles in the catalytic graphite, which leads to the low orientation of the graphite sheets during the sample test. Figure 9 shows that the R value distribution is relatively small, the graphite conversion rate is high, and the structure is relatively uniform. Figures 10-13 show that some particles have a flake morphology similar to that of flake natural graphite. There are also spherical graphite particles. In addition, there are clusters formed by the aggregation of small particles and other irregularly shaped particles. Figure 14 proves that the hollow Spherical graphite particles are non-solid structures. Figure 15 shows that graphite spheres are hollow structures. In addition, the interior of catalytic graphite also has a porous structure formed by the different orientations, bending and dislocations of graphite sheets. Figure 19 shows that the interior of artificial graphite particles is dense. Figures 20-22 show that there is no 3R phase near 43.3° and 46.1° in artificial graphite. The orientation result obtained based on the ratio of the (004) to (110) peak intensities is 9. 48; As can be seen from Figures 25-27, there is a 3R phase in the flake graphite material near 43.3° and 46.1°, and the orientation result is 139.5 based on the ratio of the (004) to (110) peak intensities; As can be seen from Figure 28, at the (002) peak near 26.4°, the peak intensity of flake graphite is significantly higher than that of catalytic graphite material; As can be seen from Figure 31, the R value distribution in this figure is generally larger, which is significantly larger than the results measured for catalytic graphite material.
[0192] (2) The catalytic graphite material described in the present application has a 3R phase. The presence of the 3R phase provides more embedding sites for lithium ions. It can be seen from Examples 1-7 that the increase in the proportion of the catalyst and the increase in the heat treatment temperature are beneficial to the improvement of the capacity, first efficiency and graphitization degree of the catalytic graphite material. It can be seen from the SEM morphology of the carbon powder in Example 1 that the biochar has obvious natural channels and pore structures, which also provides favorable conditions for the uniform dispersion of the catalyst. In addition, the orientation degree of the catalytic graphite material of the present application is low, so the expansion caused during the charge and discharge process tends to be isotropic, thereby showing low expansion characteristics; it can be seen from Examples 1 and 8 that the vacuum impregnation process is beneficial to the impregnation of the catalyst solution in the pores of the carbon material, thereby facilitating the efficient and high-quality conversion of the carbon material into catalytic graphite.
[0193] (3) It can be seen from Examples 1 and 9-10 that if the heat treatment temperature is too low, the catalyst cannot convert the carbon material into catalytic graphite well, which leads to a lower true density, higher specific surface area, lower capacity and first efficiency of the catalytic graphite negative electrode material. If the heat treatment temperature is too high, the performance of the material will also be affected. It can be seen from Examples 1 and 11 that if acid washing is not performed, the presence of impurities will result in high ash content, high true density and low capacity. It can be seen from Examples 1 and 12-14 that isostatic pressing and the pressure of isostatic pressing will affect the performance of the material. Isostatic pressing within the appropriate pressure range can make part of the catalyst tightly wrapped by carbon powder, so that this part of the carbon is converted into graphite on the surface of the catalyst during the catalytic conversion process, and graphite hollow spheres can be obtained after the catalyst is removed by acid washing; it can be seen from Example 1 and Example 15 that if pre-carbonization is not carried out, the carbon material will shrink more during the catalytic heat treatment process and have more volatile matter, resulting in poor catalytic effect, which is specifically manifested in an increase in surface area, a decrease in capacity and a lower first efficiency. In addition, the space utilization rate of the heat treatment equipment is very limited, resulting in reduced production efficiency, thereby leading to high overall energy consumption.
[0194] (4) It can be seen from Example 1 and Comparative Example 1 that without adding a catalyst, graphite conversion cannot be achieved under high-temperature carbonization conditions, and the capacity and initial efficiency of the composite negative electrode material are low, which shows that the addition of a catalyst is a necessary condition for converting carbon materials into graphite materials; It can be seen from Example 1 and Comparative Example 2 that the catalytic graphite has a 3R phase (rhombohedral phase), while the artificial graphite has no 3R phase (rhombohedral phase), and the cross-sectional structure of the catalytic graphite material has a pore structure and hollow graphite balls formed by different orientations, bends and dislocations of graphite sheets, while the cross-sectional structure of the artificial graphite is a dense structure, and the graphitization degree of the catalytic graphite is higher than that of the artificial graphite; It can be seen from Example 1 and Comparative Example 3 that due to the high crystallinity of natural graphite, the layered structure is more obvious and the interlayer spacing is small, and it is around 26.4° on the XRD spectrum. The peak intensity of the (002) peak is significantly higher than the peak intensity of the (002) peak near 26.4° in the XRD spectrum of catalytic graphite; and the flaky natural graphite in Comparative Example 3 is mainly composed of flaky graphite particles. In addition to some particles having a flaky morphology similar to that of natural graphite, the particle morphology of the catalytic graphite also contains hollow spherical graphite particles, clusters of small particles, and irregular graphite particles. For this reason, the orientation of the catalytic graphite material is significantly smaller than that of the flaky natural graphite material; it can be seen from Example 1 and Comparative Example 4 that the cross-section of the spherical natural graphite has a pore structure, but no hollow graphite spheres, while the catalytic graphite material has hollow spherical graphite particles, and the average R value obtained by the Raman surface scan of the catalytic graphite is smaller than the average R value obtained by the Raman surface scan of the spherical natural graphite.
[0195] In summary, the present application provides a catalytic graphite material, a preparation method and an application thereof. The catalytic graphite material has high purity, a high degree of graphitization and a 3R phase. When the catalytic graphite material is used as a negative electrode material for lithium-ion batteries, it exhibits the characteristics of high capacity, high initial efficiency and low expansion, thereby significantly improving the electrochemical properties of lithium-ion batteries such as capacity and initial efficiency.
[0196] The above description is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Those skilled in the art should understand that any changes or replacements that can be easily thought of by those skilled in the art within the technical scope disclosed in the present application fall within the protection scope and disclosure scope of the present application.
Claims
1. A catalytic graphite material, comprising flake graphite and hollow spherical graphite particles, wherein the catalytic graphite material has a 3R phase.
2. The catalytic graphite material according to claim 1, wherein The catalytic graphite material also includes particle aggregates and random particles; The graphitization degree of the catalytic graphite material is g, 95%≤g<100%; The R value of the catalytic graphite material is in the range of 0.03-0.4, wherein R value = I D / I G ; The outer diameter of the hollow spherical graphite particles is D, wherein 5<D<50μm.
3. A method for preparing the catalytic graphite material as claimed in claim 1 or 2, comprising the following steps: (1) pre-carbonizing a carbon source to obtain carbon powder, mixing the carbon powder and a catalyst solution, and then performing solid-liquid separation to obtain composite particles loaded with the catalyst; (2) The composite particles of step (1) are heat treated and then post-treated to obtain the catalytic graphite material.
4. The preparation method according to claim 3, wherein The step (1) of mixing the carbon powder and the catalyst solution comprises vacuum impregnating the carbon powder in the catalyst solution; The vacuum impregnation time is 1-2.5h; The mass ratio of the carbon powder to the catalyst solution in step (1) is 1:(4-7); The mass of material A obtained after the solid-liquid separation in step (1) is 3-3.7 times the mass of the carbon powder.
5. The preparation method according to claim 3 or 4, wherein The pre-carbonization temperature in step (1) is 500-1200° C. and the time is 1-6 hours; The pre-carbonization in step (1) is carried out under a protective gas, wherein the protective gas comprises any one of nitrogen, argon, krypton or helium, or a combination of at least two thereof; The particle size D50 of the carbon powder in step (1) is 5-45 μm; The solid-liquid separation method in step (1) includes filter press; After the solid-liquid separation in step (1), drying is also performed, and the drying temperature is 150-300° C. and the drying time is 2-4 hours.
6. The preparation method according to any one of claims 3 to 5, wherein: The catalyst in step (1) comprises an inorganic salt and / or an organic salt, which is an inorganic salt and / or an organic salt of any one or a combination of at least two of vanadium, chromium, manganese, iron, cobalt, nickel or copper; The carbon source in step (1) includes a biomass carbon source and / or a biomass secondary processed material; The biomass carbon source includes any one of straw, fruit shell, wood or bamboo, or a combination of at least two of them; The biomass secondary processing material includes any one of glucose, sucrose, starch, lignin, cellulose or hemicellulose, or a combination of at least two of them.
7. The preparation method according to any one of claims 3 to 6, wherein: Prior to the heat treatment in step (2), the composite particles are also subjected to isostatic pressing; The pressure increase rate of the isostatic pressing treatment is 5-100 MPa / min, and the pressure is 200-400 MPa; The holding time of the isostatic pressing treatment is 10-120 min, and the pressure reduction rate is 5-100 MPa / min; The number of isostatic pressing treatments is not less than two times; The heat treatment temperature in step (2) is 1300-1900° C. and the time is 1-5 hours.
8. The preparation method according to any one of claims 3 to 7, wherein: The post-treatment in step (2) includes pickling, water washing and drying in sequence; The pickling solution used in the pickling includes hydrochloric acid and / or hydrofluoric acid; The drying temperature is 150-300° C. and the drying time is 0.5-3 h.
9. The preparation method according to any one of claims 3 to 8, wherein: The preparation method comprises the following steps: (1) pre-carbonizing the carbon source at a temperature of 500-1200° C. for 1-6 h under protective gas to obtain carbon powder with a particle size D50 of 5-45 μm, and then vacuum impregnating the carbon powder in a catalyst solution for 1-2.5 h, and then performing filter pressing, and drying the filter cake obtained by the filter pressing at 150-300° C. for 2-4 h to obtain composite particles loaded with the catalyst; The mass ratio of the carbon powder to the catalyst solution is 1:(4-7); (2) The composite particles in step (1) are pressurized to 200-400 MPa at a pressure increase rate of 5-100 MPa / min and subjected to isostatic pressing for 10-120 min, and then the pressure is released at a pressure reduction rate of 5-100 MPa / min to obtain an isostatically pressed material. The isostatically pressed material is heat treated at a temperature of 1300-1900°C for 1-5 h, and then acid-washed, water-washed and dried in sequence to obtain the catalytic graphite material.
10. A lithium ion battery comprising the catalytic graphite material according to claim 1 or 2.