Methods of forming semiconductor structure

TWI945845BActive Publication Date: 2026-11-11TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
TW114119754
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2025-03-31
Filing Date
2025-05-26
Publication Date
2026-11-11
Estimated Expiration
2045-05-25

AI Technical Summary

Technical Problem

As semiconductor devices continue to increase integration density by reducing minimum feature sizes, challenges arise in applying strain effectively to both p-type and n-type field-effect transistors (PFET and NFET) to enhance drive current.

Method used

A complementary field-effect transistor (CFET) is fabricated by bonding wafers with dielectric layers that apply opposite strains to PFET and NFET channels, using silicon nitride layers with controlled density and silicon-nitrogen atomic ratios to achieve compressive and tensile strains, respectively.

Benefits of technology

This approach increases the strain applied to PFET and NFET channels beyond what can be achieved with source/drain regions alone, thereby enhancing the drive current of both transistor types.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920597_001
    Figure TWG2TB001920597_001
  • Figure TWG2TB001920597_002
    Figure TWG2TB001920597_002
  • Figure TWG2TB001920597_003
    Figure TWG2TB001920597_003
Patent Text Reader

Abstract

This method includes forming a first wafer and a second wafer. Forming the first wafer includes forming a first semiconductor layer on a first substrate and depositing a first dielectric layer comprising a first top layer on the first semiconductor layer. The first dielectric layer comprises a first dielectric material. Forming the second wafer includes forming a second semiconductor layer on a second substrate and depositing a second dielectric layer comprising a second top layer on the second semiconductor layer. The second dielectric layer comprises a second dielectric material different from the first dielectric material. The second wafer is bonded to the first wafer to form a composite wafer, wherein the first dielectric layer is bonded and connected to the second dielectric layer. A complementary field-effect transistor is formed based on the composite wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] none Prior Technology

[0002] Semiconductor devices are used in a variety of electronic devices, such as personal computers, mobile phones, digital cameras, and other electronic devices. Semiconductor devices are typically manufactured by sequentially depositing an insulating or dielectric layer, a conductive layer, and a semiconductor layer on a semiconductor substrate, and then using lithography to pattern the individual material layers to form circuit components and elements on them.

[0003] The semiconductor industry continuously increases the integration density of various electronic components (such as transistors, diodes, resistors, capacitors, etc.) by constantly reducing the minimum feature size, thereby allowing more components to be integrated within a given area. However, as the minimum feature size decreases, some problems also arise that need to be addressed. Summary of the Invention

[0004] none Simple Explanation of the Diagram

[0005] The various features disclosed herein can be better understood through the following detailed description, in conjunction with the accompanying drawings. It should be noted that, according to industry standard practice, the features are not drawn to scale. In fact, for clarity of discussion, the dimensions of the features may be arbitrarily increased or decreased. Figures 1 through 7 show cross-sectional views of intermediate stages in the formation of a composite wafer with internal strain, according to some embodiments. Figures 8 through 10 show cross-sectional views of intermediate stages in wafer formation according to alternative embodiments. Figures 11 through 17 show cross-sectional views of intermediate stages in the formation of a complementary field-effect transistor (CFET) according to some embodiments. Figure 18 illustrates, according to some embodiments, the distribution of the density and Si / N atomic ratio of the strain-applied bonding layer in a CFET comprising a PFET and an NFET located above the PFET. Figure 19 illustrates, according to some embodiments, the distribution of the density and Si / N atomic ratio of the strain-applied bonding layer in a CFET comprising an NFET and a PFET located above the NFET. Figure 20 illustrates, according to some embodiments, the process of forming a composite wafer and a CFET. Implementation

[0006] The following disclosure provides numerous different embodiments or instances for implementing various features of the subject matter. Specific examples of components and configurations are described below to simplify this disclosure. Of course, these components and configurations are merely examples and are not intended to be limiting. For example, the formation of a first feature above or on a second feature in the following description may include embodiments where the first and second features are formed in direct contact, and may also include embodiments where additional features may be formed between the first and second features such that the first and second features are not in direct contact. Furthermore, reference numerals and / or letters may be repeated in various instances of this disclosure. This repetition is for simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed.

[0007] Additionally, spatial relative terms, such as "below," "under," "lower," "above," "upper," and similar terms, may be used herein for ease of description to describe the relationship between one element or feature as illustrated in the figures and another element or feature. Spatial relative terms are intended to cover different orientations of the device in use or operation than those depicted in the figures. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatial relative descriptive terms used herein may also be interpreted accordingly.

[0008] This disclosure provides a complementary field-effect transistor (CFET) including an upper FET (or transistor) and a lower FET, and a fabrication process thereof. According to some embodiments, this fabrication process includes: forming a lower wafer; and depositing a lower dielectric layer (lower bonding layer) on the lower wafer. The lower dielectric layer applies a first strain to the lower wafer. Additionally, an upper wafer is also formed, and an upper dielectric layer (upper bonding layer) is deposited on the upper wafer. The upper dielectric layer applies a second strain, opposite to the first strain, to the upper wafer.

[0009] The upper and lower wafers are bonded together by bonding the upper and lower dielectric layers to form a composite wafer. Next, a CFET is formed in the composite wafer, with the upper FET formed in the upper wafer and the lower FET formed in the lower wafer. A first strain is required for the lower FET, and a second strain is required for the upper FET. Therefore, the upper and lower dielectric layers function to apply the required strains to the upper and lower FETs respectively, and also function to improve the drive current of the upper and lower FETs.

[0010] Although the exemplary embodiments use gate-all-around (GAA) FETs as both the upper and lower FETs, these embodiments can also be applied to CFETs that include other FETs, such as FinFETs, planar transistors, or combinations of GAA FETs, FinFETs, and planar FETs. Throughout the description, the terms "FET" and "transistor" are used interchangeably. The embodiments discussed herein are intended to provide examples to enable the implementation or use of the subject matter of this disclosure, and those skilled in the art will readily understand that various modifications can be made without departing from the intended scope of the different embodiments. In the various views and illustrative embodiments, the same reference numerals are used to indicate the same elements. Although the method embodiments may be discussed as being performed in a particular order, other method embodiments can be performed in any logical order.

[0011] Figures 1 through 17 illustrate cross-sectional views of the various intermediate stages of forming the composite wafer and CFET according to some embodiments. The corresponding processes are also schematically illustrated in manufacturing process 200 shown in Figure 20.

[0012] Referring to Figure 1, a wafer 2L comprising a substrate 20L is provided. According to some embodiments, the substrate 20L is a bulk substrate formed of a homogeneous semiconductor material (e.g., silicon). According to an alternative embodiment, the substrate 20L may be a composite substrate having a composite structure. This composite structure may include a first semiconductor layer and a second semiconductor layer (which may be silicon layers), and a stop layer located between the first and second semiconductor layers. The stop layer may be formed of or contain a semiconductor material (e.g., silicon germanium). Alternatively, the stop layer may include a dielectric material (e.g., silicon nitride, silicon oxide, etc.).

[0013] Referring to Figure 2, a (lower) multilayer stack 22L is formed above the substrate 20L. As shown in Figure 20, this corresponds to process 202 in manufacturing process 200. The multilayer stack 22L includes alternating dummy semiconductor layers 24L and a lower semiconductor layer 26L. The lower semiconductor layer 26L is used to form a lower field-effect transistor (FET). In the following discussion, it is assumed that the lower FET formed in a subsequent process is a p-type FET, and the upper FET formed in a subsequent process is an n-type FET. According to an alternative embodiment, the lower FET may be an n-type field-effect transistor FET, and the upper FET may be a p-type FET.

[0014] Suitable wells (not shown separately) can be formed in the lower semiconductor layer 26L. For example, the lower semiconductor layer 26L can be in-situ doped (during epitaxial growth) and / or implanted to achieve the desired conductivity type. For example, when the lower FET is a p-type FET, the well can be doped with an n-type dopant, such as phosphorus or arsenic.

[0015] In the example shown, the multilayer stack 22L includes three dummy semiconductor layers 24L and two underlying semiconductor layers 26L. It should be understood that the multilayer stack 22L may include any number of dummy semiconductor layers 24L and underlying semiconductor layers 26L. Each layer of the multilayer stack 22L can be grown using processes such as vapor phase epitaxy (VPE) or molecular beam epitaxy (MBE), or deposited using processes such as chemical vapor deposition (CVD) or atomic layer deposition (ALD).

[0016] A dummy semiconductor layer 24L is formed of a first semiconductor material, and a lower semiconductor layer 26L is formed of a second semiconductor material different from the first semiconductor material. The first and second semiconductor materials can be selected from candidate semiconductor materials of the substrate 20L. The first and second semiconductor materials have high etch selectivity towards each other. Therefore, in subsequent processes, the dummy semiconductor layer 24L can be removed at a faster rate than the lower semiconductor layer 26L.

[0017] In some embodiments, the dummy semiconductor layer 24L is formed of or contains silicon germanium, while the lower semiconductor layer 26L is formed of silicon. The thicknesses of the lower semiconductor layers 26L may be the same or different from each other. The thicknesses of the dummy semiconductor layers 24L may be the same or different from each other.

[0018] According to some embodiments, as shown in Figure 2, the multilayer stack 22L further includes a semiconductor layer 26M deposited above the top layer of the dummy semiconductor layer 24L. The semiconductor layer 26M may be formed of the same material as the underlying semiconductor layer 26L. For example, the semiconductor layer 26M may be formed of or contain silicon. Alternatively, the semiconductor layer 26M may be formed of or contain silicon germanium, wherein the atomic percentage of germanium is lower than the atomic percentage of germanium in the dummy semiconductor layer 24L.

[0019] According to an alternative embodiment, the semiconductor layer 26M may not be formed, and the subsequently formed dielectric layer 28L (Figure 3) is formed above and in contact with the topmost dummy semiconductor layer 24L in the multilayer stack 22L. According to some embodiments, the thickness of the semiconductor layer 26M may be less than the thickness of the dummy semiconductor layer 24L and the thickness of the lower semiconductor layer 26L.

[0020] Referring to Figure 3, the (lower) dielectric layer 28L is deposited on the lower multilayer stack 22L. The dielectric layer 28L can also be referred to as a bonding layer or strain-applying bond layer. As shown in Figure 20, this corresponds to process 204 in manufacturing process 200. The dielectric layer 28L may contact the semiconductor layer 26M, or, if the semiconductor layer 26M is not formed, contact the topmost dummy semiconductor layer 24L. The dielectric layer 28L may contain a dielectric material and may have an amorphous or crystalline structure.

[0021] According to some embodiments, the dielectric layer 28L can be formed through a conformal deposition process, such as plasma-enhanced atomic layer deposition (PEALD) or thermal atomic layer deposition (ALD). In embodiments using PEALD, the wafer temperature can be below about 100°C and can be in the range of about 100°C to about 200°C. In embodiments using thermal ALD, the wafer temperature can be above about 100°C and can be in the range of about 200°C to about 700°C.

[0022] According to some embodiments, dielectric layer 28L comprises silicon nitride (SiN). According to alternative embodiments, dielectric layer 28L comprises other suitable materials, such as silicon oxynitride (SiON), silicon carbonitride (SiCN), etc., or combinations thereof. The choice of materials is consistent with the formation process to generate the required strain in dielectric layer 28L, which is applied to the underlying multilayer stack 22L and the channel region of the subsequently formed lower FET.

[0023] According to certain embodiments in which the dielectric layer 28L comprises silicon nitride, the corresponding precursors may include silicon-containing precursors, such as silane (SiH4), disilane (Si2H6), dichlorosilane (SiCl2H2, DCS), etc., or combinations thereof. Precursors also include nitrogen-containing precursors, such as ammonia (NH3), nitrogen (N2), etc. Formation may include multiple cycles, each cycle including a pulse process and a purge process for the silicon-containing precursor, and a pulse process and a purge process for the nitrogen-containing precursor.

[0024] According to some embodiments, the thickness of the dielectric layer 28L is controlled so that it is neither too thick nor too thin. For example, the thickness of the dielectric layer 28L can be in the range of about 5 nm to about 20 nm. When the dielectric layer 28L is too thin (e.g., less than about 5 nm), the strain applied to it may not be high enough. When the dielectric layer 28L is too thick (e.g., greater than about 20 nm), the aspect ratio of the source / drain trench 46 (Figure 12) may be too high during the subsequent formation of the CFET, and it may be difficult to form the feature of filling the trench 46.

[0025] According to some embodiments, the lower FET is a PFET, whose channel region is prone to compressive strain. Therefore, the dielectric layer 28L has compressive strain (and is referred to as the compressive dielectric layer), and compressive strain is applied to the multilayer stack 22L. According to some embodiments, the compressive strain can be achieved by adjusting the material, formation process, and / or characteristics of the dielectric layer 28L.

[0026] According to certain embodiments in which the dielectric layer 28L comprises silicon nitride, its density and silicon-nitrogen atomic ratio can be increased to modulate the strain to make it more compressible. For example, increasing the density of the dielectric layer 28L and decreasing its silicon-nitrogen atomic ratio can result in an increase in the magnitude of compressive strain, a change in tensile strain to compressive strain, or a decrease in the magnitude of tensile strain.

[0027] Therefore, the dielectric layer 28L with compressive strain (for PFE) has a relatively high density and a relatively low silicon-nitrogen atomic ratio. For example, the density of the dielectric layer 28L with compressive strain can be greater than about 2.5 g / cm³, and can be in the range of about 2.5 g / cm³ to about 3.5 g / cm³. When the density of the dielectric layer 28L exceeds this range, the strain may not be compressive. The silicon-nitrogen atomic ratio can be in the range of 0.1 to about 0.8. When the silicon-nitrogen atomic ratio exceeds this range, the strain may not be compressive. The corresponding compressive strain in the dielectric layer 28L (and applied to the multilayer stack 22L) may be greater than 0 GPa and less than about 1 GPa.

[0028] After depositing the dielectric layer 28L, the wafer temperature is lowered to, for example, room temperature. To make the strain more compressible, the cooling rate after depositing the dielectric layer 28L can be controlled; a larger cooling rate can generate larger compressive stress. For example, the cooling rate after the formation of the dielectric layer 28L can be greater than about 200˚C / min, and can be in the range of about 100˚C / min to about 1,000˚C / min.

[0029] According to some embodiments, dielectric layer 28L includes a top that overlaps with multilayer stack 22L, and a sidewall portion located on the sidewall of multilayer stack 22L. Dielectric layer 28L may or may not extend to the sidewall of substrate 20L.

[0030] According to some embodiments, due to the formation of a dielectric layer 28L with compressive strain, wafer 2L may warp, with the central portion of wafer 2L being higher than the edge portions. Depending on the size of wafer 2L and the strain applied by the dielectric layer 28L, the height difference DH1 can range from about 1 µm to about 20 µm.

[0031] Referring to Figure 4, a wafer 2U comprising a substrate 20U is provided. According to some embodiments, the substrate 20U is a bulk substrate formed of a homogeneous semiconductor material (e.g., silicon). According to an alternative embodiment, the substrate 20U may be a composite substrate having a composite structure. This composite structure may include a first semiconductor layer and a second semiconductor layer (which may be silicon layers), and a stop layer located between the first and second semiconductor layers. The stop layer may be formed of or contain a semiconductor material (e.g., silicon germanium). Alternatively, the stop layer may include a dielectric material (e.g., silicon nitride, silicon oxide, etc.).

[0032] Referring to Figure 5, a (top) multilayer stack 22U is formed above the substrate 20U. As shown in Figure 20, this corresponds to process 206 in manufacturing process 200. The multilayer stack 22U includes alternating dummy semiconductor layers 24U and a top semiconductor layer 26U. The top semiconductor layer 26U is used to form the top FET. In the following discussion, it is assumed that the top FET is an NFET.

[0033] Suitable wells (not shown separately) can be formed in the upper semiconductor layer 26U. For example, the upper semiconductor layer 26U can be in-situ doped (during epitaxial growth) and / or implanted to achieve the desired conductivity type. For example, when the upper FET is an n-type FET, the wells can be doped with p-type dopants, such as phosphorus, arsenic, etc.

[0034] In the example shown, the multilayer stack 22U includes two dummy semiconductor layers 24U and one top semiconductor layer 26U. It should be understood that the multilayer stack 22U may include any number of dummy semiconductor layers 24U and top semiconductor layers 26U. Each layer of the multilayer stack 22U can be grown using processes such as VPE, MBE, CVD, ALD, etc.

[0035] To achieve sufficient etch selectivity, the material of the dummy semiconductor layer 24U is different from that of the upper semiconductor layer 26U. In some embodiments, the dummy semiconductor layer 24U is formed of or contains silicon germanium, while the upper semiconductor layer 26U is formed of or contains silicon.

[0036] According to some embodiments, as shown in Figure 5, the multilayer stack 22U further includes a semiconductor layer 26M, which is deposited above the topmost dummy semiconductor layer 24U. The semiconductor layer 26M may be formed of the same material as the upper semiconductor layer 26U. For example, the semiconductor layer 26M may be formed of or contain silicon. According to an alternative embodiment, the semiconductor layer 26M may not be formed, and a subsequently formed dielectric layer 28U (Figure 6) is formed above and in contact with the topmost semiconductor layer 24U of the multilayer stack 22U. According to some embodiments, the thickness of the semiconductor layer 26M may be less than the thickness of the dummy semiconductor layer 24U and the thickness of the upper semiconductor layer 26U.

[0037] Referring to Figure 6, a dielectric layer 28U is deposited (on top) on the multilayer stack 22U. Dielectric layer 28U is also called a bonding layer or strain-applied bonding layer. As shown in Figure 20, this corresponds to process 208 in fabrication process 200. Dielectric layer 28U may contact semiconductor layer 26M, or, if semiconductor layer 26M is not formed, contact the topmost dummy semiconductor layer 24U. Dielectric layer 28U may contain a dielectric material and may have an amorphous or crystalline structure.

[0038] According to some embodiments, the dielectric layer 28U can be formed through a conformal deposition process (e.g., PEALD process, thermal ALD process, etc.). In embodiments using PEALD, the wafer temperature can be below about 100°C, and can be in the range of about 100°C to about 200°C. In embodiments using thermal ALD, the wafer temperature can be above about 100°C, and can be in the range of about 200°C to about 700°C.

[0039] According to some embodiments, dielectric layer 28U also comprises silicon nitride (SiN), but other suitable materials such as SiON, SiCN, or combinations thereof can also be used. The choice of materials is consistent with the formation process to generate the required strain in dielectric layer 28U, which is applied to the underlying multilayer stack 22U and the corresponding upper FET channel regions.

[0040] According to certain embodiments where the dielectric layer 28U comprises silicon nitride, the corresponding precursor may include silicon-containing precursors, such as silane (SiH4), disilane (Si2H6), dichlorosilane (SiCl2H2, DCS), etc., or combinations thereof. Precursors may also include nitrogen-containing precursors, such as ammonia (NH3), nitrogen (N2), etc. Formation may include multiple cycles, each cycle including a pulse process and a purge process for the silicon-containing precursor, and a pulse process and a purge process for the nitrogen-containing precursor.

[0041] According to some embodiments, the thickness of the dielectric layer 28U is controlled so that it is neither too thick nor too thin. For example, the thickness of the dielectric layer 28U can be in the range of about 5 nm to about 20 nm. When the dielectric layer 28U is too thin (e.g., less than about 5 nm), the strain it generates may not be high enough. When the dielectric layer 28U is too thick (e.g., greater than about 20 nm), the aspect ratio of the source / drain trench 46 (Figure 12) may be too high during the subsequent formation of the CFET, and it may be difficult to form the feature of filling the trench 46.

[0042] According to some embodiments, the upper FET is an NFET, whose channel region is prone to tensile strain. Therefore, the dielectric layer 28U has tensile strain (and is a stretched dielectric layer), and tensile strain is applied to the multilayer stack 22U. According to some embodiments, the tensile strain can be achieved by adjusting the material, formation process, and / or characteristics of the dielectric layer 28U.

[0043] According to some embodiments, the dielectric layer 28U comprises silicon nitride, and its density and silicon-nitrogen atom ratio can be adjusted to make the strain more tensile. The dielectric layer 28U with tensile strain (for NFETs) can have a relatively low density and a relatively high silicon-nitrogen atom ratio. For example, the density of the dielectric layer 28U with tensile strain can be less than about 2.7 g / cm³, and can be in the range of about 2.0 g / cm³ to about 2.7 g / cm³. When the density of the dielectric layer 28U exceeds this range, the strain may not be tensile.

[0044] The silicon-to-nitrogen (SiN) ratio of dielectric layer 28U can range from 0.5 to approximately 1.0. When the SiN ratio of dielectric layer 28U exceeds this range, the strain may not be tensile. The corresponding tensile strain applied to the underlying multilayer stack 22U in dielectric layer 28U may be greater than -1 GPa and less than approximately 0 GPa.

[0045] After depositing dielectric layer 28U, the wafer temperature is lowered to, for example, room temperature. To make the strain in dielectric layer 28U more tensile, the cooling rate after dielectric layer 28U deposition can be controlled; a lower cooling rate generates greater tensile stress. Therefore, the cooling rate of dielectric layer 28U can be lower than the cooling rate of dielectric layer 28L. For example, the cooling rate of wafer 2U can be below about 600°C / min, and can be in the range of about 10°C / min to about 300°C / min.

[0046] Compared to dielectric layer 28L, dielectric layer 28L may have a higher density, for example, a density difference greater than about 0.3 g / cm³, possibly between about 0.5 g / cm³ and about 1.5 g / cm³. The silicon-to-nitrogen (SiN) ratio of dielectric layer 28L may also be lower than that of dielectric layer 28U, for example, a SiN ratio greater than about 0.2, possibly between about 0.4 and about 0.9. After the formation of wafer 2L and wafer 2U, the wafer temperature drop rate (post-deposition) of wafer 2L (and dielectric layer 28L) may also be greater than that of wafer 2U (and dielectric layer 28U), for example, a difference greater than about 200°C / min, possibly between about 200°C / min and about 500°C / min.

[0047] According to some embodiments, dielectric layer 28U includes a top that overlaps with multilayer stack 22U, and a sidewall portion located on the sidewall of multilayer stack 22U. Dielectric layer 28U may or may not extend to the sidewall of substrate 20L.

[0048] According to some embodiments, due to the formation of a dielectric layer 28U with tensile strain, wafer 2U may warp, with the central portion of wafer 2U being lower than the edge portion. Depending on the size of wafer 2U and the strain applied by the dielectric layer 28U, the height difference DH2 can range from about 1 µm to about 20 µm.

[0049] In Figure 7, wafer 2U and wafer 2L are bonded by fusion bonding, wherein Si-O-Si bonds are formed to connect dielectric layer 28U and dielectric layer 28L. This corresponds to process 210 in manufacturing process 200, as shown in Figure 20. The bonding process may include a pre-bonding process and an annealing process following the pre-bonding process. According to some embodiments, during the pre-bonding process, the center of wafer 2U contacts the center of wafer 2L, and this contact extends to the edges of wafers 2U and 2L.

[0050] After pre-bonding, an annealing process is performed, for example, to form Si-O-Si bonds between dielectric layer 28U and dielectric layer 28L, thereby bonding dielectric layer 28U and dielectric layer 28L together with high bonding strength. Therefore, dielectric layer 28U and dielectric layer 28L are also referred to as bonding layers. This forms composite wafer 2, as shown in Figure 7. In this paper, dielectric layer 28U and dielectric layer 28L can be collectively referred to as dielectric layer (bonding layer) 28. Multilayer stack 22U and multilayer stack 22L can be collectively referred to as multilayer stack 22.

[0051] Figures 8 through 10 illustrate the formation and bonding of wafers 2U and 2L according to alternative embodiments, thereby forming a composite wafer 2. These embodiments are similar to those shown in Figures 1 through 7, except that dielectric layers 28L and 28U also include bottoms located beneath the corresponding wafers 2L and 2U, respectively. The structures, materials, and formation processes according to these embodiments are substantially the same as those discussed with reference to Figures 1 through 7, and therefore will not be described again herein.

[0052] Referring to Figure 8, a wafer 2L, a multilayer stack 22L, and a dielectric layer 28L are formed. The dielectric layer 28L may include a top portion above the multilayer stack 22L, sidewall portions on the sidewalls of the multilayer stack 22L and the substrate 20L, and a bottom portion below the substrate 20L. According to some embodiments, the thickness T1 of the top portion is greater than the thickness T2 of the bottom portion. According to an alternative embodiment, the thickness T1 is equal to the thickness T2. The formation of the bottom portion can reduce warpage of the wafer 2L. Making the thickness T1 equal to the thickness T2 can eliminate or reduce warpage of the wafer 2L.

[0053] Referring to Figure 9, a wafer 2U, a multilayer stack 22U, and a dielectric layer 28U are formed. The dielectric layer 28U may include a top portion above the multilayer stack 22U, sidewall portions on the sidewalls of the multilayer stack 22U and the substrate 20U, and a bottom portion below the substrate 20U. According to some embodiments, the thickness T3 of the top portion is greater than the thickness T4 of the bottom portion. According to an alternative embodiment, the thickness T3 is equal to the thickness T4. The formation of the bottom portion can reduce warpage of the wafer 2U. Making the thickness T3 equal to the thickness T4 can eliminate or reduce warpage of the wafer 2U.

[0054] Figure 10 illustrates the bonding process between wafer 2U and wafer 2L to form composite wafer 2. The bonding process is essentially the same as that discussed in Figure 7, and will not be repeated here.

[0055] Figures 11 through 17 illustrate, according to some embodiments, the process of forming a CFET based on a composite wafer 2. Figure 11 illustrates, according to some embodiments, a portion of wafer 2 as shown in Figure 7 or Figure 10.

[0056] According to some embodiments, the substrate 20U is thinned, and the remaining portion of the substrate 20U forms a top semiconductor layer 26U, which covers the topmost dummy semiconductor layer 24U.

[0057] Referring to Figure 12, in subsequent processes, the multilayer stacks 22U and 22L, along with the substrate 20, are patterned to form semiconductor strips 32. As shown in Figure 20, this corresponds to process 212 in manufacturing process 200. Each semiconductor strip 32 includes a semiconductor strip 20' (a portion of the original substrate 20) and a multilayer stack 22', which includes the patterned remainder of the multilayer stacks 22U and 22L. The remainder 22' of the multilayer stack 22 is referred to hereinafter as a nanostructure, indicated by the corresponding reference numeral followed by an apostrophe. Therefore, the multilayer stack 22' includes a dummy nanostructure 24', a lower semiconductor nanostructure 26'L, an intermediate semiconductor nanostructure 26'M, and a upper semiconductor nanostructure 26'U. Patterning can be anisotropic. The lower semiconductor nanostructure 26'L and the upper semiconductor nanostructure 26'U can be collectively referred to as semiconductor nanostructure 26'.

[0058] The lower semiconductor nanostructure 26'L will serve as the channel region for the lower nanostructure FET of the CFET. The upper semiconductor nanostructure 26'U will serve as the channel region for the upper nanostructure FET of the CFET. The intermediate semiconductor nanostructure 26'M is a semiconductor nanostructure 26' located directly above / below (e.g., in contact with) the dielectric layer 28. The intermediate semiconductor nanostructure 26'M can be used for isolation and may or may not serve as the channel region for the CFET. The isolation structure and the intermediate semiconductor nanostructure 26'M can be used to define the boundary between the lower nanostructure FET and the upper nanostructure FET.

[0059] An isolation region (Shallow Trench Isolation (STI) region, not shown in the figure) is formed above the substrate 20 and between adjacent semiconductor strips 32. The isolation region is not shown in the illustrated cross-section and therefore is not shown in the figure. The isolation region may include a dielectric pad and a dielectric material above the dielectric pad. The isolation region is then recessed. Some upper portions of the semiconductor strips 32 (including the multilayer stack 22') protrude above the remaining isolation region, thereby forming protruding fins.

[0060] Referring further to Figure 12, dummy gate stacks 42 are formed on the top surface and sidewalls of the protruding fins. As shown in Figure 20, this corresponds to process 214 in manufacturing process 200. Each dummy gate stack 42 may include a dummy dielectric layer 36, a dummy gate layer 38, and a masking layer 40. The dummy dielectric layer 36 may be formed of or contain materials such as silicon oxide, silicon nitride, or combinations thereof. The material of the dummy gate layer 38 may be conductive or non-conductive and may be selected from the group including amorphous silicon, polycrystalline silicon, polycrystalline silicon-germanium, and poly-SiGe. The masking layer 40 is formed over the planarized dummy gate layer 38 and may include materials such as silicon nitride and silicon oxynitride.

[0061] The mask layer 40 can be patterned using lithography and etching processes to form a photomask. Then, the dummy gate layer 38 and possibly the dummy dielectric layer 36 are etched and patterned using the mask. The remaining portions of the mask layer 40, the dummy gate layer 38, and the dummy dielectric layer 36 form the dummy gate stack 42.

[0062] Gate spacers 44 are formed above the multilayer stack 22' and on the exposed sidewalls of the dummy gate stack 42. As shown in Figure 20, this corresponds to process 216 in manufacturing process 200. Suitable dielectric materials may include silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, etc., and can be formed through deposition processes such as CVD, ALD, etc.

[0063] As further shown in Figure 12, source / drain recesses 46 are formed in the semiconductor strip 32. This corresponds to process 218 in manufacturing process 200, as shown in Figure 20. The source / drain recesses 46 are formed by etching and can extend through the multilayer stack 22'. The bottom surface of the source / drain recesses 46 can be located above, below, or flush with the top surface of the isolation region, which is not shown in the cross-sectional view. During the etching process, the gate spacers 44 and the dummy gate stack 42 will cover some portions of the semiconductor strip 32.

[0064] The virtual nanostructures 24'U and 24'L are also laterally recessed, and dielectric material is filled in the corresponding recesses to form an internal spacer layer 54, which is a dielectric isolation layer.

[0065] Referring to Figure 13, a lower epitaxial source / drain region 62L is formed in the lower part of the source / drain groove 46. As shown in Figure 20, this corresponds to process 220 in manufacturing process 200. The lower epitaxial source / drain region 62L is in contact with the lower semiconductor nanostructure 26'L, but not with the upper semiconductor nanostructure 26'U. An internal spacer layer 54 electrically insulates the lower epitaxial source / drain region 62L from the dummy nanostructure 24'L, which will be replaced by a replacement gate in a subsequent process.

[0066] The lower epitaxial source / drain region 62L is epitaxially grown, and its conductivity type is adapted to the device type (p-type or n-type) of the lower nanostructure FET. When the lower epitaxial source / drain region 62L is a p-type source / drain region, the corresponding material may include silicon or silicon-germanium, and be doped with p-type dopants, such as boron or indium. The corresponding dielectric layer 28L has compressive strain.

[0067] When the lower epitaxial source / drain region 62L is an n-type source / drain region, the corresponding material may include silicon or carbon-doped silicon doped with n-type dopants (such as phosphorus, arsenic, etc.). The corresponding dielectric layer 28L has tensile strain.

[0068] Referring to Figure 14, a first contact etch stop layer (CESL) 66 and a first interlayer dielectric (ILD) 68 are formed. As shown in Figure 20, this corresponds to process 222 in manufacturing process 200. The first CESL 66 can be formed from a dielectric material with high etch selectivity relative to the first ILD 68, such as silicon nitride, silicon oxide, silicon oxynitride, etc. These materials can be formed through any suitable deposition process, such as CVD, ALD, etc. The first ILD 68 can be formed from a dielectric material. Suitable dielectric materials for the first ILD 68 may include phospho-silicate glass (PSG), boro-silicate glass (BSG), boron-doped phospho-silicate glass (BPSG), undoped silicate glass (USG), silicon oxide, etc.

[0069] Next, as shown in Figure 15, an upper epitaxial source / drain region 62U is formed on the upper part of the source / drain groove 46. As shown in Figure 20, this corresponds to process 224 in manufacturing process 200. The material of the upper epitaxial source / drain region 62U can be selected according to the required conductivity type.

[0070] The conductivity type of the upper epitaxial source / drain region 62U can be opposite to that of the lower epitaxial source / drain region 62L. In other words, the doping type of the upper epitaxial source / drain region 62U can be opposite to that of the lower epitaxial source / drain region 62L. When the upper epitaxial source / drain region 62U is an n-type region, the corresponding dielectric layer 28U exhibits tensile strain. Conversely, when the upper epitaxial source / drain region 62U is a p-type region, the corresponding dielectric layer 28U exhibits compressive strain.

[0071] Referring to Figure 16, a second CESL70 and a second ILD72 are formed. As shown in Figure 20, this corresponds to process 226 in manufacturing process 200. The materials and formation methods are similar to those of the first CESL66 and the first ILD68, respectively, and will not be described further here. The formation process may include depositing the layers of the second CESL70 and the second ILD72, and performing a planarization process to remove excess portions of the corresponding layers. After the planarization process, the top surfaces of the second ILD72, the gate spacer 44, and the dummy gate stack 42 are coplanar (within the range of process variations). The planarization process may remove the mask 40, or retain and not remove the hard mask 40.

[0072] Then, the dummy gate stack 42 is removed through one or more etching processes, and replacement gate stacks 90 (including gate stack 90L and gate stack 90U) are formed in corresponding recesses, as shown in Figure 17. As shown in Figure 20, this corresponds to process 228 in manufacturing process 200. Gate stack 90L includes gate dielectric 78 and gate electrode 80L. Gate stack 90U includes gate dielectric 78 and gate electrode 80U. Each gate dielectric 78 may include an interface layer (e.g., a silicon oxide layer) and a high-k dielectric layer above the interface layer. This forms a lower FET 10L and an upper FET 10U, which together constitute CFET 10.

[0073] Figure 18 illustrates the properties of dielectric layers 28L and 28U according to certain embodiments. The X-axis represents the position indicated by arrow 94 in Figure 17, where dielectric layers 28L and 28U are shown. The left Y-axis represents the density of dielectric layers 28L and 28U, and the right Y-axis represents the silicon-nitrogen (S / N) atomic ratio of dielectric layers 28L and 28U. The left Y-axis corresponds to line 96. As shown by line 96, the density decreases from dielectric layer 28L to dielectric layer 28U. The right Y-axis corresponds to line 98. As shown by line 98, the Si / N atomic ratio of dielectric layer 28 increases from dielectric layer 28L to dielectric layer 28U.

[0074] It is worth noting that the values ​​shown in Figure 18 correspond to a CFET with a PFET as the lower FET and an NFET as the upper FET. In an alternative embodiment with an NFET as the lower FET and a PFET as the upper FET, the density is shown in Figure 19. As shown by line 96' in Figure 19, the density gradually increases from dielectric layer 28L to dielectric layer 28U. As shown by line 98', the Si / N atom ratio of dielectric layer 28 gradually decreases from dielectric layer 28L to dielectric layer 28U.

[0075] The embodiments disclosed herein have several advantages. By applying compressive strain to the channel of the PFET and tensile strain to the channel of the NFET using a bonding layer, the strain can be increased to a higher degree than by applying strain using only the source / drain regions. The drive current of both the NFET and PFET can be increased.

[0076] According to some embodiments of the present disclosure, a method includes: forming a first wafer, including forming a first semiconductor layer over a first substrate; and depositing a first dielectric layer including a first top over the first semiconductor layer, wherein the first dielectric layer includes a first dielectric material; forming a second wafer, including forming a second semiconductor layer over a second substrate; and depositing a second dielectric layer including a second top over the second semiconductor layer, wherein the second dielectric layer includes a second dielectric material different from the first dielectric material; bonding the second wafer to the first wafer to form a composite wafer, wherein the first dielectric layer is bonded and connected to the second dielectric layer; and forming a complementary field-effect transistor based on the composite wafer.

[0077] In one embodiment, the deposition of the first dielectric layer and the deposition of the second dielectric layer contain the same elements but are performed using different process conditions. In another embodiment, the first and second dielectric layers comprise silicon nitride, and the first dielectric layer is deposited using a first silicon-containing precursor and a first nitrogen-containing precursor, and the second dielectric layer is deposited using a second silicon-containing precursor and a second nitrogen-containing precursor, wherein a first flow rate ratio of the first silicon-containing precursor to the first nitrogen-containing precursor is less than a second flow rate ratio of the second silicon-containing precursor to the second nitrogen-containing precursor.

[0078] In one embodiment, depositing the first dielectric layer includes a first wafer cooling process with a first wafer cooling rate, and depositing the second dielectric layer includes a second wafer cooling process with a second wafer cooling rate, wherein the second wafer cooling rate is lower than the first wafer cooling rate. In one embodiment, the first dielectric layer has a first density, and the second dielectric layer has a second density that is lower than the first density.

[0079] In one embodiment, a first portion of the first semiconductor layer is formed as a first channel of a p-type transistor in a complementary field-effect transistor (CFD), wherein a first dielectric layer applies compressive strain to the first semiconductor layer; and a second portion of the second semiconductor layer is formed as a second channel of an n-type transistor in the CFD, wherein a second dielectric layer applies tensile strain to the second semiconductor layer. In one embodiment, after the CFD is formed, the first dielectric layer and the second dielectric layer are located between the p-type transistor and the n-type transistor.

[0080] In one embodiment, when depositing the first dielectric layer, the first dielectric layer includes a first sidewall portion located on a sidewall of the first semiconductor layer. In one embodiment, the first dielectric layer includes a first bottom portion located beneath the first substrate. In one embodiment, when depositing the second dielectric layer, the second dielectric layer includes a second sidewall portion located on a second sidewall of the second semiconductor layer. In one embodiment, the second dielectric layer further includes a second bottom portion located beneath the second substrate.

[0081] According to some embodiments of the present disclosure, a method includes: forming a first wafer, including depositing a first plurality of semiconductor layers on a first substrate; and depositing a first dielectric layer as part of the first wafer, wherein the first dielectric layer is configured to apply compressive strain to the first plurality of semiconductor layers; forming a second wafer, including forming a second plurality of semiconductor layers on a second substrate; and depositing a second dielectric layer as part of the second wafer, wherein the second dielectric layer is configured to apply tensile strain to the second plurality of semiconductor layers; bonding the second wafer to the first wafer to form a composite wafer, wherein the first dielectric layer is bonded and connected to the second dielectric layer; and forming a complementary field-effect transistor, including a p-type transistor comprising a first portion of the first plurality of semiconductor layers as a first channel; and an n-type transistor comprising a second portion of the second plurality of semiconductor layers as a second channel.

[0082] In one embodiment, the first dielectric layer has a first density, and the second dielectric layer has a second density less than the first density. In one embodiment, both the first and second dielectric layers comprise silicon nitride. In one embodiment, the first dielectric layer has a first silicon-to-nitrogen atomic ratio, and the second dielectric layer has a second silicon-to-nitrogen atomic ratio greater than the first silicon-to-nitrogen atomic ratio. In one embodiment, depositing the first dielectric layer includes a first wafer cooling process with a first wafer cooling rate, and depositing the second dielectric layer includes a second wafer cooling process with a second wafer cooling rate less than the first wafer cooling rate.

[0083] According to some embodiments of the present disclosure, a method includes forming a complementary field-effect transistor structure, comprising: forming a p-type transistor including a first channel region; and a first source / drain region located on one side of the first channel region; forming a first dielectric layer, wherein the first dielectric layer overlaps with the first channel region, and wherein the first dielectric layer comprises a first dielectric material; forming a second dielectric layer, wherein the second dielectric layer is located above and bonded to the first dielectric layer, and wherein the second dielectric layer comprises a second dielectric material different from the first dielectric material; and forming an n-type transistor above the second dielectric layer, the n-type transistor including a second channel region; and a second source / drain region located on one side of the second channel region.

[0084] In one embodiment, the first dielectric layer has a higher density than the second dielectric layer. In one embodiment, both the first and second dielectric layers comprise silicon nitride, wherein the first dielectric layer has a first silicon-to-nitrogen atomic ratio, and the second dielectric layer has a second silicon-to-nitrogen atomic ratio greater than the first silicon-to-nitrogen atomic ratio. In one embodiment, the thickness of both the first and second dielectric layers is in the range of about 5 nm to about 20 nm.

[0085] The foregoing outlines some features of the embodiments to enable those skilled in the art to better understand the various aspects of this disclosure. Those skilled in the art should understand that they can readily design or modify other processes and structures based on this disclosure to achieve the same purposes and / or the same advantages as the embodiments described herein. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of this disclosure, and that they can make various changes, substitutions, and alterations to this disclosure without departing from its spirit and scope.

[0086] 2: Composite wafers, wafers 2L: Wafer 2U: Wafer 10: CFET 10L: Lower FET 10U: Upper FET 20:Substrate 20L:Substrate 20U:Substrate 20': Semiconductor strip 22: Multi-layer stacking 22L: Multi-layer stacking 22U: Multi-layer stacking 22': Multi-layer stacking, remaining portion 24L: Dummy Semiconductor Layer 24U: Virtual semiconductor layer, semiconductor layer 24': Virtual nanostructure 24'L: Virtual nanostructure 24'U: Virtual Nanostructure 26L: Lower semiconductor layer 26M: Semiconductor layer 26U: Upper semiconductor layer, top semiconductor layer 26': Semiconductor nanostructure 26'L: Lower semiconductor nanostructure 26'M: Intermediate semiconductor nanostructure 26'U: Upper semiconductor nanostructure 28: Dielectric layer 28L: Dielectric layer 28U: Dielectric layer 32: Semiconductor strip 36: Dummy dielectric layer 38: Virtual gate layer 40: Mask, Hard Mask, Mask Layer 42: Dummy gate stack 44: Gate spacer 46: Source / Drain groove, groove 54: Internal spacer layer 62L: Lower epitaxial source / drain region 62U: Upper epitaxial source / drain region 66: First CESL 68: First ILD 70: Second CESL 72: Second ILD 78: Gate Dielectric 80L: Gate electrode 80U: Gate electrode 90: Replace gate stack 90L: Gate Stack 90U: Gate Stack 94: Arrow 96: Line 96':line 98: Line 98':line 200: Manufacturing Process 202,204,206,208,210: Manufacturing Process 212, 214, 216, 218, 220: Manufacturing Process 222,224,226,228: Manufacturing Process DH1: Height difference DH2: Height difference T1: Thickness T2: Thickness T3: Thickness T4: Thickness X: axis Y: axis

[0087] Domestic storage information (please note in order of storage institution, date, and number) none Overseas storage information (please note in the order of storage country, institution, date, and number) none

Claims

1. A method for forming a semiconductor structure, comprising: Forming a first wafer includes: forming a first semiconductor layer on a first substrate; and depositing a first dielectric layer including a first top layer on the first semiconductor layer, wherein the first dielectric layer includes a first dielectric material, the first dielectric layer being configured to apply compressive strain to the first semiconductor layer; forming a second wafer includes: forming a second semiconductor layer on a second substrate; and depositing a second dielectric layer including a second top layer on the second semiconductor layer, wherein the second dielectric layer includes a second dielectric material different from the first dielectric material, the second dielectric layer being configured to apply tensile strain to the second semiconductor layer; bonding the second wafer to the first wafer to form a composite wafer, wherein the first dielectric layer is bonded and connected to the second dielectric layer; and forming a complementary field-effect transistor based on the composite wafer.

2. The method as described in claim 1, wherein, The deposition of the first dielectric layer and the deposition of the second dielectric layer contain the same elements, but are performed using different process conditions.

3. The method as described in claim 2, wherein the first dielectric layer and the second dielectric layer comprise silicon nitride, and wherein: The first dielectric layer is deposited using a first silicon-containing precursor and a first nitrogen-containing precursor; and the second dielectric layer is deposited using a second silicon-containing precursor and a second nitrogen-containing precursor, wherein a first flow rate ratio of the first silicon-containing precursor to the first nitrogen-containing precursor is less than a second flow rate ratio of the second silicon-containing precursor to the second nitrogen-containing precursor.

4. The method as described in claim 2, wherein, The deposition of the first dielectric layer includes a first wafer cooling process having a first wafer cooling rate, and the deposition of the second dielectric layer includes a second wafer cooling process having a second wafer cooling rate, wherein the second wafer cooling rate is lower than the first wafer cooling rate.

5. A method for forming a semiconductor structure, comprising: Forming a first wafer includes: forming a plurality of first semiconductor layers on a first substrate; and depositing a first dielectric layer as a part of the first wafer, wherein the first dielectric layer is configured to apply compressive strain to the first semiconductor layers; forming a second wafer includes: forming a plurality of second semiconductor layers on a second substrate; and depositing a second dielectric layer as a part of the second wafer, wherein the second dielectric layer is configured to apply tensile strain to the second semiconductor layers; bonding the second wafer to the first wafer to form a composite wafer, wherein the first dielectric layer is bonded and connected to the second dielectric layer; and forming a complementary field-effect transistor includes: a p-type transistor including a first portion of the first semiconductor layers as a first channel; and an n-type transistor including a second portion of the second semiconductor layers as a second channel.

6. The method as described in claim 5, wherein the first dielectric layer has a first density and the second dielectric layer has a second density less than the first density.

7. The method as described in claim 5, wherein both the first dielectric layer and the second dielectric layer comprise silicon nitride.

8. A method for forming a semiconductor structure, comprising: Forming a complementary field-effect transistor structure includes: forming a p-type transistor, including: a first channel region; and a first source / drain region located on one side of the first channel region; forming a first dielectric layer, wherein the first dielectric layer overlaps with the first channel region, and wherein the first dielectric layer includes a first dielectric material, the first dielectric layer being configured to apply compressive strain to the first semiconductor layer; forming a second dielectric layer, wherein the second dielectric layer is located above and bonded to the first dielectric layer, and wherein the second dielectric layer includes a second dielectric material different from the first dielectric material, the second dielectric layer being configured to apply tensile strain to the second semiconductor layer; and forming an n-type transistor above the second dielectric layer, the n-type transistor including: a second channel region; and a second source / drain region located on one side of the second channel region.

9. The method as described in claim 8, wherein, The first dielectric layer has a higher density than the second dielectric layer.

10. The method as described in claim 8, wherein, Both the first dielectric layer and the second dielectric layer contain silicon nitride, and the first dielectric layer has a first silicon-nitrogen atom ratio, while the second dielectric layer has a second silicon-nitrogen atom ratio greater than the first silicon-nitrogen atom ratio.

Citation Information

Patent Citations

  • Semiconductor devices and methods for forming the same

    TW202324511A

  • Semiconductor structure and method of forming the same

    TW202435368A

  • Integrated circuit structure and forming method thereof

    TW202447868A

  • Bonding and Isolation Techniques for Stacked Transistor Structures

    US20240282815A1