Boom section forming method and boom section
The method of forming a boom section with high-strength aluminum alloy through sequential hot bending and closed-bending addresses the issue of structural weakness in existing methods, enhancing strength and rigidity while reducing weight and costs.
Patent Information
- Application Number
- US19/123066
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2023-09-21
- Filing Date
- 2023-10-18
- Publication Date
- 2026-11-12
AI Technical Summary
Existing boom section forming methods result in plate deformation and reduced structural strength due to weld joints, leading to compromised hoisting performance and increased weight.
A method involving cutting a high-strength aluminum alloy plate into specific portions, followed by sequential hot pre-bending and hot closed-bending using stationary and flexible reconfigurable molds, with laser tracking and air quenching to form a boom section with only one joint, improving strength and rigidity while reducing weight and energy consumption.
Enhances the strength and rigidity of the boom section, reduces machining costs, and improves production efficiency by forming a lightweight boom section with a single joint, thereby optimizing hoisting performance.
Smart Images

Figure US20260355809A1-D00000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The invention relates to a boom section forming method and a boom section, and belongs to the field of boom section formation.RELATED ART
[0002] Boom sections are core components of elevating platform trucks and also the most important load-bearing structural components in elevating and hoisting operation, and the strength of the boom sections basically determines the hoisting performance of hoisting equipment. The boom sections are machined and formed by plates, and the forming process of the boom sections is a crucial process in production of the boom sections and has a great impact on the mechanical properties of booms.
[0003] According to existing disclosed techniques (such as Patent Publication No. CN103287994A, Patent Publication No. CN205076723U, Patent Publication No. CN202785400U, Patent Publication No. CN110733992A and Patent Publication No. CN103015726B), boom sections are made by bending and welding plates and have at least two weld joints, deformation of the plates is inevitable in the welding process of the weld joints, and damage to the plates will be aggravated with the increase in welding, thereby inevitably reducing the structural strength of a whole boom.SUMMARY OF INVENTION
[0004] The invention provides a boom section forming method and a boom section to solve the problems disclosed in the description of related art.
[0005] To solve the abovementioned technical problems, the invention adopts the following technical solution:
[0006] A boom section forming method includes:
[0007] cutting a plate according to a size of a boom section to be formed to obtain a boom section base plate;
[0008] sequentially dividing, from one side to the other side of the boom section base plate, the boom section base plate into a first boom section top plate portion, a first boom section side plate portion, a boom section bottom plate portion, a second boom section side plate portion and a second boom section top plate portion;
[0009] performing hot pre-bending on the first boom section top plate portion and the second boom section top plate portion to bend the first boom section top plate portion and the second boom section top plate portion oppositely by a preset angle A;
[0010] performing hot pre-bending on the first boom section side plate portion and the second boom section side plate portion to bend the first boom section side plate portion and the second boom section side plate portion oppositely by a preset angle C; and
[0011] performing hot closed-bending on the boom section base plate subjected to hot pre-bending to obtain a formed boom section.
[0012] The cut plate is a high-strength aluminum alloy plate.
[0013] Stationary molds with a heating function are used to perform hot pre-bending on the first boom section top plate portion and the second boom section top plate portion.
[0014] Flexible reconfigurable molds with a heating function are used to perform hot pre-bending multiple times on the first boom section top plate portion and the second boom section top plate portion; in each time of hot pre-bending, the first boom section top plate portion and the second boom section top plate portion are bent oppositely by a preset angle B, and the sum of the angles B formed in all the times of hot pre-bending is equal to the preset angle A; and in each time of hot pre-bending, hot pre-bending is performed on a plate body segment-by-segment.
[0015] Flexible reconfigurable molds with a heating function are used to perform hot pre-bending multiple times on the first boom section side plate portion and the second boom section side plate; in each time of hot pre-bending, the first boom section side plate portion and the second boom section side plate portion are bent oppositely by a preset angle D, and the sum of the angles D formed in all the times of hot pre-bending is equal to the preset angle C; and in each time of hot pre-bending, hot pre-bending is performed on a plate body segment-by-segment.
[0016] Flexible reconfigurable molds with a heating function are used to perform hot closed-bending multiple times on the boom section base plate subjected to hot pre-bending; in each time of hot closed-bending, the first boom section top plate portion and the second boom section top plate portion are bent oppositely by a preset angle E, and the first boom section side plate portion and the second boom section side plate portion are bent oppositely by a preset angle F; and in each time of hot closed-bending, hot closed-bending is performed on a plate body segment-by-segment.
[0017] In the segment-by-segment hot bending process, a laser tracking and positioning method is used to align a current bend line with a previous bend line, a multi-point laser heating method is used to heat the current bend line, and then bending is performed.
[0018] In the hot closed-bending process, air quenching is performed on bends.
[0019] In the hot closed-bending process, molds for bending the first boom section top plate and the second boom section top plate are triangular male molds, and molds for bending the first boom section side plate portion, the boom section bottom plate portion and the second boom section side plate portion are arc-shaped female molds.
[0020] A boom section is formed by the boom section forming method.
[0021] The invention fulfills the following beneficial effects: the boom section base plate is obtained by cutting it according to the size of the boom section to be formed, and hot pre-bending and hot closed-bending are sequentially performed on the boom section base plate to obtain the boom section with only one joint, such that compared with boom sections with the same section formed by existing methods, the strength and rigidity of the boom section are effectively improved, the machining cost is reduced, the production efficiency is improved, and energy consumption is reduced; in addition, compared with boom sections with the same strength and rigidity formed by the existing methods, the sectional size of the boom section is effectively reduced, thus effectively reducing the weight of a boom.BRIEF DESCRIPTION OF DRAWINGS
[0022] FIG. 1 is a flow diagram of a boom section forming method.
[0023] FIG. 2 is a schematic structural diagram of a boom section base plate.
[0024] FIG. 3 is a schematic diagram of hot pre-bending performed by means of stationary molds according to a first boom section forming method.
[0025] FIG. 4 is a schematic diagram of hot pre-bending performed by means of flexible reconfigurable molds according to the first boom section forming method.
[0026] FIG. 5 is a schematic diagram of hot closed-bending performed by means of flexible reconfigurable molds according to the first boom section forming method.
[0027] FIG. 6 is a schematic diagram of hot pre-bending performed by means of stationary molds according to a second boom section forming method.
[0028] FIG. 7 is a schematic diagram of hot pre-bending performed by means of flexible reconfigurable molds according to the second boom section forming method.
[0029] FIG. 8 is a schematic diagram of hot closed-bending performed by means of flexible reconfigurable molds according to the second boom section forming method.
[0030] FIG. 9 is a schematic diagram of hot closed-bending in a case where rebounding of a plate body is taken into account.
[0031] FIG. 10 is a schematic diagram after the plate body rebounds.DESCRIPTION OF EMBODIMENTS
[0032] The invention is further described below in conjunction with accompanying drawings. The following embodiments are merely used for more clearly explaining the technical solution of the invention rather than limiting the protection scope of the invention.
[0033] As shown in FIG. 1, a boom section forming method includes the following steps:
[0034] Step 1, a plate is cut according to the size of a boom section to be formed to obtain a boom section base plate.
[0035] Step 2, the boom section base plate is sequentially divided into a first boom section top plate portion, a first boom section side plate portion, a boom section bottom plate portion, a second boom section side plate portion and a second boom section top plate portion from one side to the other side of the boom section base plate.
[0036] Step 3, hot pre-bending is performed on the first boom section top plate portion and the second boom section top plate portion to bend the first boom section top plate portion and the second boom section top plate portion oppositely by a preset angle A.
[0037] Step 4, hot pre-bending is performed on the first boom section side plate portion and the second boom section side plate portion to bend the first boom section side plate portion and the second boom section side plate portion oppositely by a preset angle C.
[0038] Step 5, hot closed-bending is performed on the boom section base plate subjected to hot pre-bending to obtain a formed boom section.
[0039] According to the boom section forming method, the boom section base plate is obtained by cutting it according to the size of the boom section to be formed, and hot pre-bending and hot closed-bending are sequentially performed on the boom section base plate to obtain the boom section with only one joint, such that compared with boom sections with the same section formed by existing methods, the strength and rigidity of the boom section are effectively improved, the machining cost is reduced, the production efficiency is improved, and energy consumption is reduced; in addition, compared with boom sections with the same strength and rigidity formed by the existing methods, the sectional size of the boom section is effectively reduced, thus effectively reducing the weight of a boom.
[0040] At present, the lightweight design based on aluminum rather than steel has been widely applied to the fields such as the aerospace field and the rail traffic field. In the industry of construction machinery, considering the high strength requirement in the working condition, in one embodiment of the invention, high-strength aluminum alloy is used for preparing the boom section, that is, a high-strength aluminum alloy plate is cut according to the size of a boom section to be formed to obtain a boom section base plate, and specifically as shown in FIG. 2, the boom section base plate is sequentially divided into a first boom section top plate portion, a first boom section side plate portion, a boom section bottom plate portion, a second boom section side plate portion and a second boom section top plate portion from one side to the other side of the boom section base plate; wherein the first boom section top plate portion and the second boom section top plate portion are finally assembled into a boom section top plate, and the size of the first boom section top plate portion is generally consistent with the size of the second boom section top plate portion.
[0041] Although the high-strength aluminum alloy has high strength and can completely replace steel, the high-strength aluminum alloy is difficult to plastically bend and punch due to its poor formability. In view of this, in the invention, the boom section base plate is flexibly bent by multiple steps. Specifically:
[0042] 1. Hot pre-bending is performed on the first boom section top plate portion and the second boom section top plate portion to bend the first boom section top plate portion and the second boom section top plate portion oppositely by a preset angle A.
[0043] Generally, the pre-bend angle of the top plate portions is not large, and considering the cost and efficiency, stationary molds with a heating function may be used to perform pre-bending on the top plate portions. For example, stationary molds with a heating function (that is, resistive heaters are arranged in the molds to realize the heating function) are used to perform hot pre-bending on the first boom section top plate portion and the second boom section top plate portion of a square boom section as shown in FIG. 3 or a boom section with an arc-shaped top plate as shown in FIG. 6. The stationary molds realize bending formation at a time, that is, the stationary molds bend the top plate portions to the preset angle A at a time.
[0044] Of course, without considering the cost and efficiency, flexible reconfigurable molds with a heating function (similar to molds shown in FIGS. 4, 5, 7 and 8, laser heads are arranged on two sides of the molds) may be used to perform hot pre-bending multiple times on the first boom section top plate portion and the second boom section top plate portion; wherein, in each time of hot pre-bending, the first boom section top plate portion and the second boom section top plate are bent oppositely by a preset angle B, and the sum of the angles B formed in all the times of hot pre-bending is equal to the preset angle A; and in each time of hot pre-bending, hot pre-bending is performed on a plate body segment-by-segment, that is to say, the plate body may be moved by means of a moving device, and every time one segment of the plate body is bent, the plate body is moved by one segment to pre-bend a downstream segment of the plate body.
[0045] To guaranteed the alignment of bend lines between multiple pre-bent segments, in the invention, a laser tracking and positioning method is used in the segment-by-segment hot bending process to align a current bend line with a previous bend line; in addition, to facilitate bending, in the invention, a multi-point laser heating method is used to heat the current bend line.
[0046] 2. Hot pre-bending is performed on the first boom section side plate portion and the second boom section side plate portion to bend the first boom section side plate portion and the second boom section side plate portion oppositely by a preset angle C.
[0047] Flexible reconfigurable molds are used to perform hot pre-bending on the side plate portions. Referring to FIGS. 4 and 7, hot pre-bending is performed on the first boom section side plate portion and the second boom section side plate portion multiple times; in each time of hot pre-bending, the first boom section side plate portion and the second boom section side plate portion are bent oppositely by a preset angle D, and the sum of the angles D formed in all the times of hot pre-bending is equal to the preset angle C; and in each time of hot pre-bending, hot pre-bending is performed on the plate body segment-by-segment.
[0048] Similarly, to guarantee the alignment of bend lines between multiple pre-bent segments, the laser tracking and positioning method is used in the segment-by-segment hot bending process to align a current bend line with a previous bend line; in addition, to facilitate bending, the multi-point laser heating method is used to heat the current bend line.
[0049] 3. Hot closed-bending is performed on the boom section base plate subjected to hot pre-bending to obtain a formed boom section.
[0050] Similar to hot pre-bending of the side plate portions, as shown in FIGS. 5 and 8, flexible reconfigurable molds with a heating function are used to perform hot closed-bending multiple times on the boom section base plate subjected to hot pre-bending; in each time of hot closed-bending, the first boom section top plate portion and the second boom section top plate portion are bent oppositely by a preset angle E, and the first boom section side plate portion and the second boom section side plate portion are bent oppositely by a preset angle F; after multiple times of hot closed-bending, a desired boom section, such as the square boom section in FIG. 5 or the boom section with an arc-shaped top plate in FIG. 8, is formed; and in each time of hot closed-bending, hot closed-bending is performed on the plate body segment-by-segment.
[0051] Similarly, to guarantee the alignment of bend lines between multiple closed-bent segments, the laser tracking and positioning method is used in the segment-by-segment hot bending process to align a current bend line with a previous bend line; in addition, to facilitate bending, the multi-point laser heating method is used to heat the current bend line.
[0052] To improve the material performance of the bends, air quenching is performed on the bends in the hot closed-bending process. In the movable hot bending process, after one segment is bent, the bend needs to be further reinforced, so air quenching is instantly performed on the bend line at a high temperature (the strength can be improved by increasing the cooling rate at a high temperature) to recover the strength of the bend.
[0053] It should be noted that in the forming process, considering the influence of rebounding of the plate on a finally formed structural component and the possibility of breakage of a side plate and a bottom plate of the boom section under a high pressure, in the hot closed-bending process, molds are adjusted, and as shown in FIG. 9, molds for bending the first boom section top plate portion and the second boom section top plate portion are triangular male molds, and molds for bending the first boom section side plate portion, the boom section bottom plate portion and the second boom section side plate portion are arc-shaped female molds; as shown in FIG. 10, after closed-bending is completed, the flexible reconfigurable molds on two sides and at the top are separated from the plate; and after the bent metal plate rebounds (residual stress is eliminated naturally), the boom section deforms to be in a finally desired shape.
[0054] 4. The formed boom section has only one joint (a joint between the first boom section top plate portion and the second boom section top plate portion), the joint is welded to obtain a final boom section.
[0055] To further explain the boom section forming method, with a square boom section as an example, the forming process, as shown in FIGS. 3-5 and 9-10, includes:(S1)
[0056] According to drawings of the square boom section, the size of a whole high-strength aluminum alloy plate required for forming the boom section is obtained; then, the high-strength aluminum alloy plate is cut to form an integrated boom section base plate, including a first boom section top plate portion, a first boom section side plate portion, a boom section bottom plate portion, a second boom section side plate portion and a second boom section top plate portion which form the boom section finally, as shown in FIG. 2.(S2) Primary Hot Pre-Bending
[0057] Two pairs of stationary molds (wherein, a male mold on the left and a female mold on the left form one pair, and a male mold on the right and a female mold on the right form the other pair) are used, and resistive heaters are embedded in the molds.
[0058] The stationary molds are mounted on a press and heated to 180 °C, the press is started, and the male molds press the boom section base plate. The step of primary hot pre-bending allows for plastic deformation of the plate along pre-bends in the subsequent step of closed-bending. In this step, the two pairs of stationary molds may be used for forming all boom sections with a flat top plate and may be designed according to the shape of the top plate of the boom sections to be formed.(S3) Secondary Hot Pre-Bending
[0059] According to the sectional shape of the finally formed boom section, flexible reconfigurable molds are adjusted; after shape adjustment is completed, a plate body formed in (S2) is placed in the flexible reconfigurable molds to be subjected to secondary hot pre-bending.
[0060] Resistive heaters are embedded in the flexible reconfigurable molds, the flexible configurable molds are mounted on the press, and laser heads are also mounted on the press. Two ends of the 6061-T6 high-strength aluminum alloy plate subjected to primary pre-bending are fixed to clamping devices with traction gears and guide rails. The flexible reconfigurable molds are heated to 180 °C, the laser heads are started (the laser heads have a laser power of 5500 W, are pulse laser heads and provided with forming plates, and may be locally heated to 240 °C instantly), the traction gears are started synchronously to drive the forming plates to move (at a speed of 0.6 m / min), the press is started synchronously, and the molds reciprocate (at a speed of 0.2 m / min). In the secondary hot pre-bending process, the total press amount is 120 mm, and the number of reciprocating tractions is 3. Laser hot pre-bending is completed on boundaries of the top plate and the side plate, and as shown in FIG. 4, the step of secondary hot pre-bending allows for plastic deformation of the plate along the bends in the subsequent step of closed-bending.(S4) Hot Closed-Bending
[0061] First, the upper reconfigurable mold in (S3) is lifted, and then the upper, lower, left and right reconfigurable molds are adjusted; after adjustment is completed, the left, right and upper reconfigurable molds perform closed-bending on the plate synchronously, and the bending process is similar to the bending process in (S3), as shown in FIG. 5.
[0062] It should be noted that in the forming process, considering the influence of rebounding of the plate on a finally formed structural component and the possibility of breakage of the side plate and the bottom plate of the boom section under a high pressure, when the shape of the reconfigurable molds is adjusted in the step of closed-bending, as shown in FIG. 9, the reconfigurable molds on the two sides and at the bottom are adjusted to be arched, and the mold at the top is adjusted to be conical, such that the press amount decreases gradually from the middle to the two sides. In this way, after the step of closed-bending is completed, the reconfigurable molds on the two sides and at the top may be separated from the plate to form the bottom section; and after the bent metal plate rebounds (residual stress is eliminated naturally), the boom section deforms to be in a finally desired shape, as shown in FIG. 10.
[0063] The boom section forming method provided by the invention is a novel flexible forming method and can make high-strength aluminum alloy plates into boom sections of different shapes or lengths by means of bending molds that can be reconfigured quickly, without changing a forming device.
[0064] Based on the same technical solution, the invention further discloses a boom section, which is formed by the boom section forming method mentioned above. Compared with boom sections with the same section formed by existing methods, the strength and rigidity of the boom section are effectively improved, the machining cost is reduced, the production efficiency is improved, and energy consumption is reduced; in addition, compared with boom sections with the same strength and rigidity formed by the existing methods, the sectional size of the boom section is effectively reduced, thus effectively reducing the weight of a boom.
[0065] Preferred embodiments of the invention are described above. It should be noted that those ordinarily skilled in the art can make some improvements and transformations without departing from the technical principle of the invention, and all these improvements and transformations should also fall within the protection scope of the invention.
Claims
1. A boom section forming method, wherein comprising:cutting a plate according to a size of a boom section to be formed to obtain a boom section base plate;sequentially dividing, from one side to the other side of the boom section base plate, the boom section base plate into a first boom section top plate portion, a first boom section side plate portion, a bottom section bottom plate portion, a second boom section side plate portion and a second boom section top plate portion;performing hot pre-bending on the first boom section top plate portion and the second boom section top plate portion to bend the first boom section top plate portion and the second boom section top plate portion oppositely by a preset angle A;performing hot pre-bending on the first boom section side plate portion and the second boom section side plate portion to bend the first boom section side plate portion and the second boom section side plate portion oppositely by a preset angle C; andperforming hot closed-bending on the boom section base plate subjected to hot pre-bending to obtain a formed boom section.
2. The boom section forming method according to claim 1, wherein the cut plate is a high-strength aluminum alloy plate.
3. The boom section forming method according to claim 1, wherein stationary molds with a heating function are used to perform hot pre-bending on the first boom section top plate portion and the second boom section top plate portion.
4. The boom section forming method according to claim 1, wherein flexible reconfigurable molds with a heating function are used to perform hot pre-bending multiple times on the first boom section top plate portion and the second boom section top plate portion; in each time of hot pre-bending, the first boom section top plate portion and the second boom section top plate portion are bent oppositely by a preset angle B, and the sum of the angles B formed in all the times of hot pre-bending is equal to the preset angle A; and in each time of hot pre-bending, hot pre-bending is performed on a plate body segment-by-segment.
5. The boom section forming method according to claim 1, wherein flexible reconfigurable molds with a heating function are used to perform hot pre-bending multiple times on the first boom section side plate portion and the second boom section side plate portion; in each time of hot pre-bending, the first boom section side plate portion and the second boom section side plate portion are bent oppositely by a preset angle D, and the sum of the angles D formed in all the times of hot pre-bending is equal to the preset angle C; and in each time of hot pre-bending, hot pre-bending is performed on a plate body segment-by-segment.
6. The boom section forming method according to claim 1, wherein flexible reconfigurable molds with a heating function are used to perform hot closed-bending multiple times on the boom section base plate subjected to hot pre-bending; in each time of hot closed-bending, the first boom section top plate portion and the second boom section top plate portion are bent oppositely by a preset angle E, and the first boom section side plate portion and the second boom section side plate portion are bent oppositely by a preset angle F; and in each time of hot closed-bending, hot closed-bending is performed on a plate body segment-by-segment.
7. The boom section forming method according to claim 4, wherein in the segment-by-segment hot bending process, a laser tracking and positioning method is used to align a current bend line with a previous bend line, a multi-point laser heating method is used to heat the current bend line, and then bending is performed.
8. The boom section forming method according to claim 1, wherein in the hot closed-bending process, air quenching is performed on bends.
9. The boom section forming method according to claim 1, wherein in the hot closed-bending process, molds for bending the first boom section top plate and the second boom section top plate are triangular male molds, and molds for bending the first boom section side plate portion, the boom section bottom plate portion and the second boom section side plate portion are arc-shaped female molds.
10. A boom section, being formed by the boom section forming method according to claim 1.