Electrode material, electrode, preparation method therefor, and use thereof

By coating the surface of the electrode material lithium manganate with sulfonic acid group-modified Ti-MOF, the problems of slow lithium ion diffusion and impurity embedding in electrochemical salt lake lithium extraction are solved, achieving efficient lithium extraction and recovery of high-purity lithium ions.

WO2024197584A1PCT designated stage expired Publication Date: 2024-10-03GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/084471
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the process of electrochemical salt lake lithium extraction, the diffusion of lithium ions inside the electrode is slow under high voltage, causing impurity cations to be embedded in the electrode and reducing the purity of lithium ions.

Method used

Lithium manganate is used as the electrode material, and the surface is coated with a metal-organic framework Ti-MOF. A stable coating layer is formed through sulfonic acid group modification, which improves the conductivity and selectivity of lithium ions and reduces impurity embedding.

Benefits of technology

It reduces the cathodic polarization of the electrode under high voltage, increases the lithium extraction rate and purity of lithium ions, and enhances the cycle stability and structural stability of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023084471_03102024_PF_FP_ABST
    Figure CN2023084471_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are an electrode material, an electrode, a preparation method therefor, and use thereof, wherein the electrode material comprises lithium manganate and a metal-organic framework Ti-MOF coating the surface of the lithium manganate. The Ti-MOF forms a uniform coating layer on the surface of a lithium manganate electrode active material, capable of inhibiting the dissolution loss of Mn during the use of the lithium manganate electrode and improving the cycling stability of the electrode. The present invention modifies an electrode material of lithium extracted from salt-lake brine, and the electrode prepared using the electrode material can reduce the cathode polarization effect of the electrode under high voltage, reduce the intercalation of impurity cations into the electrode, and improve the purity of lithium while increasing the electrochemical lithium extraction rate.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode material, electrode, preparation method and application thereof Technical Field

[0001] The present invention belongs to the technical field of electrochemical lithium extraction from salt lakes, and particularly relates to an electrode material, an electrode, and a preparation method and application thereof. Background Art

[0002] During the electrochemical process of extracting lithium from salt lakes, the diffusion of the solution inside the electrode is slow, and the electrode reaction proceeds sequentially from the electrode surface to the interior of the electrode. During the production process, the cell voltage is usually increased to accelerate the reaction rate. However, when a higher voltage is applied, the electrochemical reaction rate is much faster than the diffusion rate of the solution inside the electrode, and the reaction is easily controlled by external diffusion. When the electrode is controlled by external diffusion, the reaction rate of lithium ions inside the electrode is accelerated, unreacted lithium ions are rapidly consumed, and lithium ions in the solution cannot be replenished to the interior of the electrode in a timely manner. At this time, the coexisting impurity cations in the solution are easily embedded in the internal electrode material and released into the solution, thereby reducing the purity of the lithium ions in the recovered solution. Therefore, there is an urgent need to develop an electrode material suitable for lithium extraction from salt lakes at higher voltages.

[0003] Summary of the Invention

[0004] The present invention aims to solve the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an electrode material, an electrode, a preparation method, and applications thereof. The electrode prepared using this electrode material can reduce the cathode polarization of the electrode under high voltage, reduce the insertion of impurity cations into the electrode, and improve the purity of lithium while increasing the electrochemical lithium extraction rate.

[0005] According to a first aspect of the present invention, an electrode material is provided, comprising lithium manganese oxide and a metal-organic framework Ti-MOF coated on the surface of the lithium manganese oxide.

[0006] In some embodiments of the present invention, the metal organic framework Ti-MOF is a sulfonic acid group-modified Ti-MOF.

[0007] According to a second aspect of the present invention, a method for preparing the electrode material is proposed, comprising the following steps:

[0008] (1) dissolving 2,5-dihydroxyterephthalic acid in N,N-dimethylformamide, adding lithium manganate and stirring to obtain a mixed solution A;

[0009] (2) dissolving titanium hydroxide in an aqueous solution of aminoethanol, adding polystyrene sulfonate, stirring, ultrasonicating, standing, and then performing solid-liquid separation to obtain polystyrene sulfonate-modified titanium hydroxide;

[0010] (3) Adding the polystyrene sulfonate-modified titanium hydroxide to the mixed solution A and heating the mixture to react, thereby obtaining the electrode material.

[0011] In some embodiments of the present invention, in step (1), the mass ratio of the lithium manganate to the 2,5-dihydroxyterephthalic acid is 1: (0.01-0.1). In the actual production process of the positive electrode material, there will be a certain amount of volatilization during the high-temperature calcination of the lithium salt. The Li / M ratio will be slightly increased during the batching (i.e., the lithium salt is appropriately excessive) to make up for the loss caused by the sintering process. Excess Li exists in the form of Li2O at high temperatures. After the temperature is reduced to room temperature, Li2O will adsorb carbon dioxide and water in the air to form residual alkalis such as lithium hydroxide and lithium carbonate. The hydroxyl group can combine with the residual alkali on the surface of the lithium manganate to form a hydrogen bond, so that the 2,5-dihydroxyterephthalic acid is stably coated on the surface of the lithium manganate electrode active material.

[0012] In some embodiments of the present invention, in step (2), the titanium hydroxide is obtained by mixing a TiCl4 solution with aqueous ammonia and then separating the mixture into solid and liquid.

[0013] In some preferred embodiments of the present invention, the TiCl4 solution is obtained by diluting a 50% by mass TiCl4 solution with deionized water 60 times, and the ammonia water is obtained by diluting a 25% by mass ammonia water with deionized water 10 times, and the diluted TiCl4 solution and the diluted ammonia water are mixed in a volume ratio of 1:6 to react to obtain the titanium hydroxide.

[0014] In some more preferred embodiments of the present invention, the preparation of titanium hydroxide further comprises adjusting the pH of the solution after the reaction to 6-8, allowing the solution to stand, filtering, and washing the obtained titanium hydroxide solid with deionized water.

[0015] In some embodiments of the present invention, in step (2), the stirring time is 30-60 min, the ultrasonic time is 1-3 h, and the standing time is 10-16 h.

[0016] In some embodiments of the present invention, in step (2), the mass ratio of the titanium hydroxide, the aminoethanol and the polystyrene sulfonate is (90-110):(8-12):1.

[0017] In some embodiments of the present invention, in step (3), the mass ratio of the polystyrene sulfonate-modified titanium hydroxide to the lithium manganate is 1:(1.5-2.5).

[0018] In some preferred embodiments of the present invention, in step (3), the polystyrene sulfonate-modified titanium hydroxide is added to the mixed solution A, reacted at 80-100°C for 8-16 hours, cooled to room temperature, removed, filtered with anhydrous ethanol, and dried in a vacuum environment at 80°C for 8-16 hours to obtain the electrode material. A precursor is prepared by combining a polymer polystyrene sulfonate with titanium hydroxide, and then using 2,5-dihydroxyterephthalic acid as a ligand with titanium ions to form a three-dimensional porous MOF modified with sulfonic acid groups.

[0019] According to a third aspect of the present invention, an electrode is provided, which is prepared by the following method:

[0020] S1: Li4Ti5O 12 / Ag composite material is prepared into electrode slurry and coated on the surface of current collector;

[0021] S2: preparing the electrode material of the second aspect into an electrode slurry and coating it on the surface of the electrode slurry described in step S1.

[0022] In some embodiments of the present invention, in step S1, the Li4Ti5O 12 The Ag / Ag composite material is prepared by the following method: AgNO3, rutile TiO2 and LiCO3 are mixed, ethanol is added and ball-milled to obtain a ball-milled mixture, and the ball-milled mixture is calcined to obtain the Li4Ti5O 12 / Ag composite materials.

[0023] In some preferred embodiments of the present invention, in step S1, the AgNO3, the rutile TiO2 and the LiCO3 are mixed in a molar ratio of 1:(12-18):(15-21).

[0024] In some embodiments of the present invention, in step S2, the Li4Ti5O 12 The coating thickness of the electrode slurry prepared from the Ag / Ag composite material is the same as that of the electrode slurry prepared from the electrode material according to the second aspect.

[0025] The present invention also provides application of the electrode in extracting lithium from salt lakes.

[0026] According to a preferred embodiment of the present invention, there are at least the following beneficial effects:

[0027] 1. In the electrode material of this invention, the hydroxyl groups can form hydrogen bonds with residual bases on the surface of lithium manganate, allowing 2,5-dihydroxyterephthalic acid to be stably coated on the surface of the lithium manganate. Furthermore, the carboxyl groups on 2,5-dihydroxyterephthalic acid are highly reactive and can react with metal ions to form MOF. The Ti-MOF forms a uniform coating on the surface of the lithium manganate, inhibiting the dissolution of Mn during the use of the lithium manganate electrode and improving the electrode's cycling stability.

[0028] 2. The present invention intersperses polystyrene sulfonate into the Ti-MOF coated on the surface of lithium manganate to form a unique three-dimensional sulfonate network that anchors metal ions, thereby improving the conductivity of lithium ions. Combined with the porous structure of the Ti-MOF material, the Ti-MOF has a high conductivity for lithium ions and exhibits high selectivity.

[0029] 3. The outer side of the electrode of the present invention is a modified lithium manganate active material. The preparation of LiMn2O4 is relatively simple. It has a three-dimensional lithium intercalation and deintercalation tunnel, so lithium ions can be deintercalated under large currents. The lithium ion transmission rate is relatively fast, which is conducive to increasing the lithium extraction rate.

[0030] Since the lithium extraction process at the bottom of the electrode (near the current collector) is controlled by ion diffusion, cathode polarization is prone to occur, and lithium ions are consumed too quickly, resulting in impurity cations (such as sodium ions and magnesium ions) being embedded in the electrode. Therefore, lithium titanate composite materials are used at the bottom of the electrode near the current collector. The diffusion path for the embedding of lithium ions in spinel lithium titanate can be 8a→16c→8a or 8a→16c→48f→16d. The 3d orbital of Ti in spinel lithium titanate is completely empty, and the energy band energy is about 2eV. The diffusion distance of lithium ions is long, resulting in a decrease in its electrical conductivity. Its ionic conductivity is lower than that of lithium manganate. During the lithium extraction process, the deintercalation of lithium ions at the bottom of the electrode can be controlled by electrochemical reactions, thereby reducing cathode polarization, avoiding the embedding of impurity cations into the crystal lattice, and improving the purity of lithium ions in the lithium recovery solution from salt lakes.

[0031] Li4Ti5O 12 Insert lithium ions to form Li7Ti5O 12 The unit cell parameter a changes from 0.83595nm to 0.83538nm, and the volume change is only 0.2%. Using it as a lithium extraction electrode material can effectively prevent the structure from being destroyed due to repeated insertion and extraction of lithium ions, improve the structural stability of the electrode, and make the electrode have strong cycle stability. The capacity retention rate after multiple cycles of lithium extraction can still be at a high level. 12 / Ag two-phase composite material, Ag does not enter Li4Ti5O 12 lattice, but is dispersed in the Li4Ti5O 12It acts as a conductive bridge between the grains, does not change the electrochemical reaction mechanism of lithium ions, and improves the electronic conductivity of the electrode material itself.

[0032] 4. In the electrode of the present invention, Li4Ti5O 12 The / Ag composite material is at the bottom of the electrode, and its ion conductivity is low. The outer layer is modified lithium manganate, which has a higher conductivity. Therefore, lithium extraction under high current conditions can increase the lithium ion diffusion rate of the outer layer of the electrode, while reducing the cathode polarization effect at the bottom of the electrode, so that the bottom of the electrode is controlled by the electrochemical reaction, thereby reducing the impurity cations embedded in the electrode material. In addition, the use of lithium manganate active materials for lithium ion deintercalation under high current can easily lead to the destruction of the electrode structure. Li4Ti5O 12 / Ag has strong cycle stability as a lithium ion sieve, which can avoid the collapse of the internal structure of the electrode caused by large current lithium extraction. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:

[0034] FIG1 is a SEM image of the electrode material (sulfonic acid group-modified Ti-MOF coated lithium manganate) prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0036] Example 1

[0037] An electrode material comprises lithium manganate and a metal organic framework Ti-MOF coated on the surface of the lithium manganate.

[0038] A method for preparing the electrode material as described above comprises the following steps:

[0039] 1.25 g of 2,5-dihydroxyterephthalic acid was added to 300 mL of N,N-dimethylformamide and stirred. After the 2,5-dihydroxyterephthalic acid was completely dissolved, 25 g of lithium manganate was added and stirring was continued for 30 minutes to obtain a mixed solution A of 2,5-dihydroxyterephthalic acid-coated lithium-rich manganese-based positive electrode material.

[0040] A 50% mass fraction TiCl4 solution was diluted 60 times with deionized water, and a 25% mass fraction ammonia water was diluted 10 times with deionized water. The diluted TiCl4 and ammonia water were mixed and reacted in a volume ratio of 1:6. The pH of the solution was adjusted to 7 and then allowed to stand for 30 minutes. The obtained titanium hydroxide was repeatedly washed with deionized water. 25 g of the washed titanium hydroxide was dissolved in 500 mL of aminoethanol aqueous solution (containing 2.5 g of aminoethanol), 0.25 g of polystyrene sulfonate was added, stirred for 45 minutes, ultrasonicated for 2 hours, and filtered after standing for 12 hours to obtain polystyrene sulfonate-modified titanium hydroxide.

[0041] 12.5 g of polystyrene sulfonate-modified titanium hydroxide was added to mixed solution A, transferred to a reactor, reacted at 90°C for 12 hours, cooled to room temperature, removed, filtered with anhydrous ethanol, and vacuum-dried at 80°C for 12 hours to obtain an electrode material (sulfonic acid group-modified Ti-MOF coated lithium manganate). The SEM image of the electrode material is shown in Figure 1.

[0042] An electrode is prepared by the following method:

[0043] (1) Preparation of Li4Ti5O 12 / Ag composite materials:

[0044] A certain amount of rutile TiO2, LiCO3 and AgNO3 were weighed in a molar ratio of 1:15:18, mixed evenly, and then a certain amount of ethanol was added as a dispersant for wet ball milling for 4 hours. The mixture was then placed in a tube furnace, heated to 80°C, kept warm for 4 hours to remove the ethanol, and then heated to 850°C at a rate of 5°C / min and calcined for 12 hours. After cooling to room temperature, Li4Ti5O 12 / Ag composite materials.

[0045] (2) Li4Ti5O prepared in step (1) 12 The electrode slurry was prepared by coating the surface of the current collector titanium mesh with 20g of Li4Ti5O 12 / Ag loading is 6 mg / cm 2 After coating, the mixture was dried at 70°C for 10 min. Then, 20 g of the electrode material prepared above, 10 g of short carbon fiber, 3 g of acetylene black, 2.5 g of PVDF, 6.5 g of pore-forming agent NH4HCO3 and 80 g of N-methylpyrrolidone were prepared into an electrode slurry and coated on the surface of the first layer of electrode slurry. The loading amount of the electrode material was 6 mg / cm 2After coating, the electrode was dried at 70°C for 10 minutes and then dried at 100°C for 4 hours. The electrode was rolled and then immersed in water. The water was changed every 0.5 hours, and the water was changed 3 times in total to obtain the electrode.

[0046] Example 2

[0047] The difference between Example 2 and Example 1 is that in the preparation method of the electrode material, the amount of raw materials used and the reaction conditions are different.

[0048] An electrode material comprises lithium manganate and a metal organic framework Ti-MOF coated on the surface of the lithium manganate.

[0049] A method for preparing the electrode material as described above comprises the following steps:

[0050] 0.25 g of 2,5-dihydroxyterephthalic acid was added to 300 mL of N,N-dimethylformamide and stirred. After the 2,5-dihydroxyterephthalic acid was completely dissolved, 25 g of lithium manganate was added and stirring was continued for 30 minutes to obtain a mixed solution A of 2,5-dihydroxyterephthalic acid-coated lithium-rich manganese-based positive electrode material.

[0051] A 50% mass fraction TiCl4 solution was diluted 60 times with deionized water, and a 25% mass fraction ammonia water was diluted 10 times with deionized water. The diluted TiCl4 and ammonia water were mixed and reacted in a volume ratio of 1:6. The pH of the solution was adjusted to 6 and then allowed to stand for 30 minutes. The obtained titanium hydroxide was repeatedly washed with deionized water. 25 g of the washed titanium hydroxide was dissolved in 500 mL of aminoethanol aqueous solution (containing 2.22 g of aminoethanol), 0.23 g of polystyrene sulfonate was added, stirred for 30 minutes, ultrasonicated for 1 hour, and filtered after standing for 8 hours to obtain polystyrene sulfonate-modified titanium hydroxide.

[0052] 10 g of titanium hydroxide modified with polystyrene sulfonate was added to solution A, transferred to a reactor, reacted at 80°C for 8 h, cooled to room temperature, taken out, filtered with anhydrous ethanol, and vacuum dried at 80°C for 8 h to obtain an electrode material (sulfonic acid group-modified Ti-MOF coated lithium manganate).

[0053] An electrode, the preparation method of which is the same as that of Example 1.

[0054] Example 3

[0055] The difference between Example 3 and Example 1 is that in the preparation method of the electrode material, the amount of raw materials used and the reaction conditions are different.

[0056] An electrode material comprises lithium manganate and a metal organic framework Ti-MOF coated on the surface of the lithium manganate.

[0057] A method for preparing the electrode material as described above comprises the following steps:

[0058] 2.5 g of 2,5-dihydroxyterephthalic acid was added to 300 mL of N,N-dimethylformamide and stirred. After the 2,5-dihydroxyterephthalic acid was completely dissolved, 25 g of lithium manganate was added and stirring was continued for 30 minutes to obtain a mixed solution A of 2,5-dihydroxyterephthalic acid-coated lithium-rich manganese-based positive electrode material.

[0059] A 50% mass fraction TiCl4 solution was diluted 60 times with deionized water, and a 25% mass fraction ammonia water was diluted 10 times with deionized water. The diluted TiCl4 and ammonia water were mixed and reacted in a volume ratio of 1:6. The pH of the solution was adjusted to 8 and then allowed to stand for 30 minutes. The obtained titanium hydroxide was repeatedly washed with deionized water. 25 g of the washed titanium hydroxide was dissolved in 500 mL of aminoethanol aqueous solution (containing 2.73 g of aminoethanol), 0.28 g of polystyrene sulfonate was added, stirred for 1 hour, ultrasonicated for 3 hours, and filtered after standing for 16 hours to obtain polystyrene sulfonate-modified titanium hydroxide.

[0060] 16.7 g of titanium hydroxide modified with polystyrene sulfonate was added to solution A, transferred to a reactor, reacted at 100°C for 16 hours, cooled to room temperature, taken out, filtered with anhydrous ethanol, and vacuum dried at 80°C for 16 hours to obtain an electrode material (sulfonic acid group-modified Ti-MOF coated lithium manganate).

[0061] An electrode, the preparation method of which is the same as that of Example 1.

[0062] Example 4

[0063] The difference between Example 4 and Example 1 is that the coating parameters of the electrode slurry in the electrode preparation method are different.

[0064] An electrode material comprises lithium manganate and a metal organic framework Ti-MOF coated on the surface of the lithium manganate.

[0065] A method for preparing the electrode material as described above is the same as that in Example 1.

[0066] An electrode is prepared by the following method:

[0067] (1) Preparation of Li4Ti5O 12 / Ag composite material: the same as in Example 1.

[0068] (2) Li4Ti5O prepared in step (1) 12 The electrode slurry of the Ag / Ag composite material was prepared as described in Example 1 at a concentration of 3 mg / cm 2The loading amount was coated on the titanium mesh surface, and after coating, it was dried at 70°C for 10 minutes. The electrode material prepared above was prepared into an electrode slurry with a density of 3 mg / cm 2 The loading amount is coated on the surface of the first layer of electrode slurry. After coating, it is dried at 70°C for 10 minutes and then dried at 100°C for 4 hours. The electrode is rolled and then immersed in water. The water is changed every 0.5 hours, and the water is changed 3 times in total to obtain the electrode.

[0069] Example 5

[0070] The difference between Example 5 and Example 1 is that the coating parameters of the electrode slurry in step (3) are different.

[0071] An electrode material comprises lithium manganate and a metal organic framework Ti-MOF coated on the surface of the lithium manganate.

[0072] A method for preparing the electrode material as described above is the same as that in Example 1.

[0073] An electrode is prepared by the following method:

[0074] (1) Preparation of Li4Ti5O 12 / Ag composite material: the same as in Example 1.

[0075] (2) Li4Ti5O prepared in step (1) 12 The electrode slurry of the Ag / Ag composite material was prepared as described in Example 1 at a concentration of 9 mg / cm 2 The loading amount was coated on the titanium mesh surface, and after coating, it was dried at 70°C for 10 minutes. The electrode material prepared above was prepared into an electrode slurry with a density of 9 mg / cm 2 The loading amount is coated on the surface of the first layer of electrode slurry. After coating, it is dried at 70°C for 10 minutes and then dried at 100°C for 4 hours. The electrode is rolled and then immersed in water. The water is changed every 0.5 hours, and the water is changed 3 times in total to obtain the electrode.

[0076] Comparative Example 1

[0077] The unmodified Li4Ti5O 12 The active material 20g and short carbon fiber 1g, acetylene black 3g, PVDF 2.5g, pore-forming agent NH4HCO3 6.5g and N-methylpyrrolidone 80g were prepared into an electrode slurry and coated on the surface of the current collector titanium mesh. 12 The loading capacity is 6 mg / cm 2The coating thickness is the same as that of the electrode prepared in Example 1. After coating, it is dried at 70°C for 10 minutes and then dried at 100°C for 4 hours. The electrode is rolled and then immersed in water. The water is changed every 0.5 hours, and the water is changed 3 times in total to obtain an electrode for electrochemical lithium extraction.

[0078] Comparative Example 2

[0079] The unmodified lithium manganese oxide active material 20g and short carbon fiber 1g, acetylene black 3g, PVDF 2.5g, pore-forming agent NH4HCO3 6.5g and N-methylpyrrolidone 80g were prepared into an electrode slurry and coated on the surface of the current collector titanium mesh. The loading amount of lithium manganese oxide was 6mg / cm 2 The coating thickness is the same as that of the electrode prepared in Example 1. After coating, it is dried at 70°C for 10 minutes and then dried at 100°C for 4 hours. The electrode is rolled and then immersed in water. The water is changed every 0.5 hours, and the water is changed 3 times in total to obtain an electrode for electrochemical lithium extraction.

[0080] Test example

[0081] 1. The prepared electrode was prepared into a delithiated electrode as the positive electrode and activated carbon as the negative electrode. After applying a voltage of 1.3 V in simulated brine (Table 1), electrolysis was carried out at a temperature of 25°C for 5 hours. The solution ion concentration before and after electrolysis was tested using an inductively coupled plasma spectrometer (ICP), and the lithium recovery rate was calculated as shown in Table 2.

[0082] Table 1 Brine composition

[0083] Table 2 Lithium recovery rate

[0084] It can be seen from Table 2 that the lithium recovery rates of the electrodes prepared by modifying the electrode materials according to the present invention are all higher than 93.8%, especially in Example 1, which is as high as 96.7%. Compared with the electrodes prepared by the unmodified materials, the lithium extraction efficiency is significantly improved.

[0085] 2. In order to test the cycling stability and lithium purity of the prepared electrode, the prepared delithiation electrode was used as the working electrode, the activated carbon AC electrode was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The reaction was carried out at a constant current (current density of 50 mA / cm 2 ) was discharged to 0.3 V (vs. Ag / AgCl) for lithium extraction, and then the fluid was switched to the recovery liquid for lithium removal. The working electrode and the counter electrode were interchanged, and constant current charging was performed to 1.1 V (vs. Ag / AgCl). After 15 cycles, the purity of lithium ions in the recovery liquid was obtained as shown in Table 3, and the adsorption capacity was shown in Table 4.

[0086] Table 3 Lithium extraction purity

[0087] Table 4 Adsorption capacity of electrodes for lithium

[0088] It can be seen from Tables 3 and 4 that after 15 cycles, the purity retention rate of lithium ions in Example 1 is as high as 95%, and the adsorption capacity of the electrode is 30.1 mg / mL, which achieves efficient separation of lithium resources, reduces the lithium loss rate of lithium extraction from salt lake brine, and has good cycle stability of lithium extraction from the electrode.

[0089] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.

Claims

1. An electrode material, It is characterized in that It comprises lithium manganate and a metal organic framework Ti-MOF coated on the surface of the lithium manganate.

2. The electrode material according to claim 1, It is characterized in that The metal organic framework Ti-MOF is a sulfonic acid group-modified Ti-MOF.

3. A method for preparing an electrode material according to any one of claims 1 to 2, Features: The following steps are involved: (1) dissolving 2,5-dihydroxyterephthalic acid in N,N-dimethylformamide, adding lithium manganate and stirring to obtain a mixed solution A; (2) dissolving titanium hydroxide in an aqueous solution of aminoethanol, adding polystyrene sulfonate, stirring, ultrasonicating, standing, and then performing solid-liquid separation to obtain polystyrene sulfonate-modified titanium hydroxide; (3) Adding the polystyrene sulfonate-modified titanium hydroxide into the mixed solution A and heating the mixture to react, thereby obtaining the electrode material.

4. The method for preparing the electrode material according to claim 3, It is characterized in that In step (1), the mass ratio of the lithium manganate to the 2,5-dihydroxyterephthalic acid is 1:(0.01-0.1).

5. The method for preparing the electrode material according to claim 3, It is characterized in that In step (2), the titanium hydroxide is TiCl 4 The solution is mixed with ammonia water for reaction and then solid-liquid separation is performed to obtain the product.

6. The method for preparing the electrode material according to claim 3, It is characterized in that In step (2), the mass ratio of the titanium hydroxide, the aminoethanol and the polystyrene sulfonate is (90-110):(8-12):

1.

7. The method for preparing the electrode material according to claim 3, It is characterized in that In step (3), the mass ratio of the polystyrene sulfonate-modified titanium hydroxide to the lithium manganate in the mixed solution A is 1:(1.5-2.5).

8. An electrode, It is characterized in that Prepared by the following method: S1: Li 4 Ti 5 O 12 / Ag composite material is prepared into electrode slurry and coated on the surface of current collector; S2: Prepare the electrode material according to any one of claims 1 to 2 into an electrode slurry and apply it on the surface of the electrode slurry described in step S1.

9. The electrode according to claim 8, It is characterized in that In step S1, the Li 4 Ti 5 O 12 The Ag / Ag composite material was prepared by the following method: 3 , rutile TiO 2 and LiCO 3 Mix, add ethanol and perform ball milling to obtain a ball milled mixture, and calcine the ball milled mixture to obtain the Li 4 Ti 5 O 12 / Ag composite materials.

10. Use of the electrode according to any one of claims 8 to 9 in extracting lithium from salt lakes.

Citation Information

Patent Citations

  • Nanostructured quasi-solid electrolyte applied to lithium ion batteries or lithium sulfur batteries and preparation method and application thereof

    CN105070946A

  • Composite solid electrolyte material and preparation method and application thereof

    CN110085909A

  • Electrolyte modulator, fabrication methods and applications of same

    CN110915055A

  • Composite electrolyte membrane, fabrication methods and applications of same

    CN111052477A

  • Electrodes having electrode additive for high performance batteries and applications of same

    CN113330608A