Lithium secondary battery and electric device
By using a combination of Li1+aM1bFe1-cAcP1-dEdO4 and graphite in lithium-ion batteries, the battery design parameters are optimized, the problem of insufficient life of lithium-ion batteries based on the same materials is solved, and longer cycle life and better performance are achieved. Energy Density and Cost.
Patent Information
- Application Number
- PCT/CN2023/085249
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-03
AI Technical Summary
It is difficult to further optimize the service life of existing lithium-ion batteries based on the same positive and negative electrodes, electrolytes, and separator materials.
A battery system composed of positive active material Li1+aM1bFe1-cAcP1-dEdO4 and graphite is used to meet specific battery design parameters by optimizing the area density of the positive active material layer, reversible lithium capacity, first lithium insertion capacity and conductivity of the electrolyte. formula relationship to improve battery cycle performance and service life.
It significantly improves the cycle life of lithium secondary batteries, brings the cell life to an optimal level, and takes into account both energy density and cost.
Smart Images

Figure CN2023085249_03102024_PF_FP_ABST
Abstract
Description
Lithium secondary batteries and electrical devices Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a positive electrode sheet, a lithium secondary battery, and an electrical device. Background Art
[0002] Lithium-ion batteries, known for their green, environmentally friendly, high-energy, and low-carbon nature, are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. With the development of society, the demand for lithium-ion batteries is increasing. Lifespan is a key performance indicator for lithium-ion batteries, and this demand is particularly prominent in the energy storage sector.
[0003] Public content
[0004] In view of the technical problems existing in the background technology, the present application provides a lithium secondary battery, aiming to improve the battery life based on the same positive and negative electrodes, electrolyte, and isolation membrane materials.
[0005] In order to achieve the above objectives, the first aspect of the present application provides a lithium secondary battery, comprising:
[0006] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on at least one side of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4, wherein -0.100≤a≤0.100, 0≤b≤1.1, 0≤c≤1, 0≤d≤0.100, M1 includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W, A includes one or more elements selected from Mn, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Ga, Sn, Sb, Nb, and Ge, E includes one or more elements selected from B, Si, N, S, F, Cl, and Br, and the Li 1+a M 1b Fe 1-c A c P 1-d E d The mass percentage of O4 in the positive electrode active material layer is not less than 85wt%;
[0007] A negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode active material layer provided on at least one side of the negative electrode current collector, the negative electrode active material layer comprising graphite, the mass proportion of the graphite in the negative electrode active material layer being not less than 85wt%,
[0008] Wherein: the surface density of the positive electrode active material layer located on one side of the positive electrode sheet is CWc, and the unit is g / 1540.25mm 2 , the reversible lithium capacity is Dc, the unit is mAh / 1540.25mm 2 The reversible lithium capacity of the negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet is Da, in units of mAh / 1540.25mm 2 The initial lithium insertion capacity of the negative electrode active material layer on the side of the negative electrode sheet facing away from the positive electrode sheet is Ca, in units of mAh / 1540.25mm 2 ; The lithium secondary battery meets:
[0009] Formula 1: 1.0337 + 0.37 × CWc – 7.79 × ρ ≤ K1 ≤ 1.07 + 0.93 × CWc – 2.9 × ρ; and / or,
[0010] Formula 2: 1.1485+0.43×CWc–9.2×ρ≤K2≤1.13+1.069×CWc–1.7×ρ;
[0011] in, ρ is the conductivity of the electrolyte of the lithium secondary battery at 25° C., and the unit is S / cm.
[0012] Compared with the prior art, the lithium secondary battery of the first aspect of the present application has at least the following beneficial effects: (1) the positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4 is beneficial to improve the cycle life of the battery; (2) Although the mechanism is not clear at present, for the Li 1+a M 1b Fe 1-c A c P 1-d E d The battery system composed of O4 and graphite, when satisfying at least one of the above formulas 1 and 2, can further improve the battery's cycle performance and extend the battery's service life on the basis of the same positive and negative electrodes, electrolyte, and isolation membrane materials, so that the battery cell life reaches a better level.
[0013] In some embodiments of the present application, the Li1+a M 1b Fe 1-c A c P 1-d E d O4 includes at least one of the positive electrode active materials corresponding to the following three conditions: (1) c=0; (2) c=1, A is a Mn element; (3) 0<c<1, and A is a Mn element.
[0014] In some embodiments of the present application, the Li 1+a M 1b Fe 1-c A c P 1-d E d O4 including LiFe 1-c Mn c PO4, 0≤c≤1.
[0015] In some embodiments of the present application, 0.25≤CWc≤0.6, optionally, 0.26≤CWc≤0.5. Controlling CWc to meet the given range is beneficial to significantly improve the cycle life of the lithium secondary battery.
[0016] In some embodiments of the present application, the value range of ρ is 0.008 to 0.020, and can be optionally 0.009 to 0.016. Controlling the conductivity of the electrolyte within the given range is beneficial to improving the dynamic performance of the lithium secondary battery and further increasing its service life.
[0017] In some embodiments of the present application, the viscosity of the electrolyte at 25°C is 1.5 mPa·s to 5 mPa·s, and may be 2 mPa·s to 4 mPa·s. Controlling the viscosity of the electrolyte within the given range is beneficial for achieving a higher ion migration rate and for allowing the positive and negative electrode sheets to be wetted by the electrolyte in a shorter period of time, thereby improving the overall performance of the lithium secondary battery.
[0018] In some embodiments of the present application, the surface density of the negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet is CWa, in units of g / 1540.25mm 2 ,in: Optionally, By controlling The ratio of is within the given range, which is conducive to obtaining an improved cycle life, and can further take into account the energy density and cost of the lithium secondary battery, and can further optimize the energy density and cost on the basis of improving the service life of the lithium secondary battery.
[0019] In some embodiments of the present application, the positive electrode active material in the positive electrode active material layer further includes one or more of nickel-cobalt-manganese ternary material, lithium cobaltate, Li2O2, lithium manganate, lithium nickelate, and lithium vanadate.
[0020] In some embodiments of the present application, the negative electrode active material in the negative electrode active material layer further includes one or more of hard carbon, soft carbon, mesocarbon microbeads, lithium titanate, carbon fiber, silicon-based materials, and tin-based materials.
[0021] In some embodiments of the present application, based on the total mass of the positive electrode active material in the positive electrode active material layer, the Li 1+a M 1b Fe 1-c A c P 1-d E d The content of O4 is not less than 94wt%.
[0022] In some embodiments of the present application, based on the total mass of the negative electrode active material in the negative electrode active material layer, the content of the graphite is not less than 85 wt %.
[0023] In some embodiments of the present application, the graphite satisfies at least one of the following conditions: the OI value of the graphite is 0.5 to 7, optionally 2 to 4.5; the BET specific surface area of the graphite is 0.8 m 2 / g~1.5m 2 / g; the graphite has a graphitization degree of 70% to 99%, optionally 75% to 98%; and the graphite has a Dv50 particle size of 1 μm to 20 μm, optionally 4 μm to 15 μm. Controlling the graphite to meet the given conditions is beneficial to further improving the overall performance of lithium secondary batteries and extending their service life.
[0024] In some embodiments of the present application, the graphite is artificial graphite.
[0025] In some embodiments of the present application, the thickness of the positive electrode sheet is 130 μm to 350 μm, and the thickness of the negative electrode sheet is 100 μm to 300 μm.
[0026] In some embodiments of the present application, 1.036≤K1≤1.308. By controlling the value of K1 within a given range, the energy density and cost of the lithium secondary battery can be taken into consideration while improving the service life of the lithium secondary battery.
[0027] In some embodiments of the present application, 1.149≤K2≤1.427. By controlling the value of K2 within a given range, the energy density and cost of the lithium secondary battery can be taken into consideration while improving the service life of the lithium secondary battery.
[0028] The second aspect of the present application provides an electrical device, which includes: the lithium secondary battery described in the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0030] FIG1 is a schematic structural diagram of a positive electrode sheet of a lithium secondary battery according to one embodiment of the present application.
[0031] FIG2 is a schematic structural diagram of a negative electrode plate of a lithium secondary battery according to an embodiment of the present application.
[0032] FIG3 is a schematic diagram of a structure in which positive and negative electrode sheets of a lithium secondary battery are alternately distributed according to an embodiment of the present application.
[0033] FIG4 is a schematic structural diagram of an electric device according to an embodiment of the present application.
[0034] Figure numerals: 10 - positive electrode sheet; 11 - positive electrode current collector; 12 - positive electrode active material layer; 20 - negative electrode sheet; 21 - negative electrode current collector; 22 - negative electrode active material layer; 22a - negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet; 22b - negative electrode active material layer on the side of the negative electrode sheet facing away from the positive electrode sheet. DETAILED DESCRIPTION
[0035] The present application will be further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.
[0036] References to "embodiments" in this application mean that a particular feature, structure, or characteristic described in connection with the embodiment may be included in at least one embodiment of the application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described in this application may be combined with other embodiments.
[0037] The "range" disclosed in this application is defined in the form of a lower limit and / or an upper limit, and a given range is defined by selecting a lower limit and / or an upper limit, and the selected lower limit and / or the rear upper limit define the boundaries of a particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range that is not clearly stated, and any lower limit can be combined with other lower limits to form a range that is not clearly stated, and similarly any upper limit can be combined with any other upper limit to form a range that is not clearly stated. In addition, each separately disclosed point or single numerical value itself can be combined with any other point or single numerical value as a lower limit or upper limit or with other lower limits or upper limits to form a range that is not clearly stated. For example, if a range of not more than 150 is listed for a particular parameter, it is also contemplated that 10 to 140 and 20 to 120, etc., satisfy a range of not more than 150. Furthermore, if the minimum range values 2.1 and 3.5 are listed, and if the maximum range values 4.9 and 6.3 are listed, then the following ranges are all contemplated: 2.1-6.3, 2.1-4.9, 3.5-6.3, and 3.5-4.9. In this application, unless otherwise indicated, a numerical range such as "10-50" is an abbreviation for any combination of real numbers between 10 and 50, where 10 and 50 are real numbers. For example, a numerical range of "20-30" indicates that all real numbers between "20-30" are listed herein, and "20-30" is merely an abbreviation for these numerical combinations.
[0038] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0039] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0040] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps S1 and S2, which means that the method may include steps S1 and S2 performed sequentially, or may include steps S2 and S1 performed sequentially. For example, the method may further include step S3, which means that step S3 may be added to the method in any order, for example, the method may include steps S1, S2, and S3, or may include steps S1, S3, and S2, or may include steps S3, S1, and S2, etc.
[0041] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or comprised, or may mean that only the listed components are included or comprised. Furthermore, as used in this application, the terms "plurality" and "multiple" refer to two or more components.
[0042] Unless otherwise specified, the term "and / or" in this application simply describes an association between related objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. Furthermore, the character " / " in this document generally indicates that the related objects are in an "or" relationship.
[0043] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and any variations thereof are intended to cover non-exclusive inclusions. Unless otherwise specified, the terms used in this application have the well-known meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0044] Currently, there are many approaches to extending the life of lithium-ion batteries, but most focus on optimizing the positive and negative electrode materials, electrolyte, and separator materials. Once these materials are determined, further research is needed to further optimize the battery's service life.
[0045] In view of this, the first aspect of the present application provides a lithium secondary battery, which is understood with reference to Figures 1 to 3 and includes: a positive electrode sheet 10 and a negative electrode sheet 20. With reference to Figure 1, the positive electrode sheet 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12 provided on at least one side of the positive electrode current collector 11. The positive electrode active material layer 12 includes a positive electrode active material Li 1+a M 1b Fe 1- c A c P 1-d E dO4, wherein -0.100≤a≤0.100, 0≤b≤1.1, 0≤c≤1, 0≤d≤0.100, M1 includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W, A includes one or more elements selected from the group consisting of Mn, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Ga, Sn, Sb, Nb, and Ge, E includes one or more elements selected from the group consisting of B, Si, N, S, F, Cl, and Br, Li 1+a M 1b Fe 1-c A c P 1-d E d The mass proportion of O4 in the positive electrode active material layer 12 is not less than 85wt%. Referring to Figure 2, the negative electrode plate 20 includes a negative electrode current collector 21 and a negative electrode active material layer 22 provided on at least one side of the negative electrode current collector 21. The negative electrode active material layer 22 includes graphite, and the mass proportion of graphite in the negative electrode active material layer 22 is not less than 85wt%. The area density of the positive electrode active material layer 12 located on one side of the positive electrode plate 10 is CWc, and the unit is g / 1540.25mm 2 , the reversible lithium capacity is Dc, the unit is mAh / 1540.25mm 2 3, the reversible lithium capacity of the negative electrode active material layer 22a on the negative electrode sheet 20 facing the positive electrode sheet 10 is Da, in units of mAh / 1540.25mm 2 The first lithium insertion capacity of the negative electrode active material layer 22b on the side of the negative electrode sheet 20 away from the positive electrode sheet 10 is Ca, in units of mAh / 1540.25mm 2 The lithium secondary battery satisfies at least one of Formula 1 and Formula 2, which are as follows:
[0046] Formula 1: 1.0337+0.37×CWc–7.79×ρ≤K1≤1.07+0.93×CWc–2.9×ρ;
[0047] Formula 2: 1.1485+0.43×CWc–9.2×ρ≤K2≤1.13+1.069×CWc–1.7×ρ;
[0048] in, ρ is the conductivity of the electrolyte of the lithium secondary battery at 25°C, and its unit is S / cm.
[0049] Compared with the related art which optimizes battery materials, such as positive and negative electrode active materials, electrolyte, and separator materials, the lithium secondary battery proposed in the first aspect of this application achieves the beneficial effect of improving battery life on the basis of the same positive and negative electrodes, electrolyte, and separator materials by optimizing battery design parameters. Although the mechanism is still unclear, the inventors found in the process of exploration that changes in battery design parameters such as the coating amount of the positive and negative electrode active material layer, reversible lithium capacity, first lithium insertion capacity, and conductivity of the electrolyte will affect the battery life to a certain extent. 1+a M 1b Fe 1-c A c P 1-d E d The battery system composed of O4 and graphite combined with graphite, when satisfying the above formula 1 and / or formula 2, can further improve the cycle performance of the battery on the basis of the same positive and negative electrodes, electrolyte, and isolation membrane materials, and extend the service life of the battery. Therefore, the lithium secondary battery of the first aspect of the present application has at least the following beneficial effects: (1) The positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4 is beneficial to improving the cycle life of the battery; (2) satisfying at least one of the above formulas 1 and 2 can further improve the cycle performance of the battery on the basis of the same positive and negative electrodes, electrolytes, and isolation membrane materials, extend the service life of the battery, and make the battery life reach a better level. It should be noted that the overall change trends of K1 and K2 are the same, and they generally increase or decrease at the same time. The main reason is that the denominators of K1 and K2 are the same, and the relative change trends of the two are mainly determined by the first lithium insertion ability and reversible lithium insertion ability of the negative electrode active material layer, and the first effect of the negative electrode active material layer = reversible lithium insertion ability / first lithium insertion ability, where , the negative electrode active material layers on both sides of the negative electrode sheet are the same. When the composition of the negative electrode active material layer is determined, the first effect of the negative electrode active material layer on both sides of the same negative electrode sheet is the same, so that the reversible lithium capacity Da of the negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet and the first lithium insertion capacity Ca of the negative electrode active material layer on the side away from the positive electrode sheet have the same change trend. When the battery design parameters are consistent, the absolute values of K1 and K2 will change, but the positive correlation between the two will not change. If one of Formula 1 and Formula 2 is satisfied, the cycle performance of the battery can be improved; (3) It provides new ideas and directions for the research of long-life batteries. It should be noted that "the side of the negative electrode sheet facing away from the positive electrode sheet" refers to the side of the negative electrode sheet that is not opposite to the positive electrode sheet.
[0050] In addition, it should be noted that in Formula 1 and Formula 2, only numerical values are entered in the calculation without units. For example, the surface density of the positive electrode active material layer on one side of the positive electrode sheet is 0.3g / 1540.25mm 2 Taking the conductivity of the electrolyte at 25°C as 0.014S / cm as an example, when using Formula 1 and Formula 2 to calculate the value ranges of K1 and K2, CWc=0.3, ρ=0.014, that is, the value ranges of K1 calculated by Formula 1 and the value ranges of K2 calculated by Formula 2 are: 1.0337+0.37×0.3–7.79×0.014≤K1≤1.07+0.93×0.3–2.9×0.014; 1.1485+0.43×0.3–9.2×0.014≤K2≤1.13+1.069×0.3–1.7×0.014.
[0051] According to the embodiments of the present application, the structure of the lithium secondary battery generally includes N (a positive integer) positive electrode sheets and N+1 negative electrode sheets (a separator is provided between the positive electrode sheet and the negative electrode sheet) alternately stacked. Each surface of the positive electrode sheet has a negative electrode sheet adjacent to it (oppositely arranged), which is conducive to making full use of the positive active material in the positive electrode sheet, thereby facilitating the improvement of the capacity and energy density of the lithium secondary battery. Among them, the content of each element in the positive and negative electrode sheets can be obtained by ICP testing. When the surface density or capacity of the positive / negative electrode sheet is tested, the following method can be used: after the lithium secondary battery is fully discharged at the nominal rate within the voltage range of use, it is disassembled in a nitrogen-filled glove box, and the disassembled electrode sheet is cleaned three times with DMC to obtain the positive electrode sheet and the negative electrode sheet; wherein:
[0052] When testing the surface density of the positive electrode active material layer located on one side of the positive electrode sheet, the positive electrode active material layer located on one side of the positive electrode sheet can be peeled off and weighed (with an accuracy of 0.0001g), and the surface density of the positive electrode active material layer can be obtained by combining the sample size.
[0053] When testing the capacity of the positive / negative electrode sheets, the positive and negative electrode sheets obtained by the disassembly method can be used with a lithium metal sheet to form a button half-cell for measurement. Taking the negative electrode sheet as an example, the negative electrode sheet capacity test method is as follows: the disassembled negative electrode sheet is cleaned three times with DMC (dimethyl carbonate) to obtain a negative electrode sheet (including the surface of the negative electrode sheet facing the positive electrode sheet and the surface of the negative electrode sheet facing away from the positive electrode sheet). The negative electrode sheet is then formed into a button half-cell with a lithium metal sheet. The half-cell is charged with a current of 0.1C and a voltage range of 0.005V-2.0V to test the reversible capacity of the negative electrode sheet and the first lithium insertion capacity of the negative electrode sheet that has not been previously inserted with lithium. The corresponding reversible capacity (the reversible capacity per unit area on the surface of the negative electrode sheet facing the positive electrode sheet, Da) and the first lithium insertion capacity (the first lithium insertion capacity per unit area on the surface of the negative electrode sheet facing away from the positive electrode sheet, Ca) of the negative electrode sheet are then converted proportionally by area. With reference to FIG3 , when testing the reversible capacity of the negative electrode, the surface 22a of the negative electrode 20 facing the positive electrode 10 is in contact with the separator. When testing the first lithium insertion capacity of a negative electrode that has not been previously inserted with lithium, the center of the negative electrode is sampled (because during the charge and discharge process, the side of the negative electrode facing away from the positive electrode usually does not participate in the reaction, i.e., does not insert lithium. However, lithium insertion may occur at the edge of the negative electrode facing away from the positive electrode, but the probability is very small, so avoid the edge area when sampling). The surface 22b of the negative electrode 20 facing away from the positive electrode 10 is in contact with the separator. It should be noted that the battery was assembled in a nitrogen-filled glove box.
[0054] Furthermore, after in-depth research, the inventors have discovered that, in addition to satisfying the aforementioned conditions, the lithium secondary battery of the present application can further improve its performance by controlling the composition and areal density of the positive electrode active material, the conductivity and viscosity of the electrolyte, the amounts of the positive and negative electrode active materials, and the characteristic parameters of the graphite. In other words, in addition to satisfying the aforementioned conditions, one or more of the following conditions may also be optionally satisfied.
[0055] In some embodiments of the present application, the positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E dIn O4, M1 can be a lithium-site doping element, such as one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W; A can be an iron-site doping element, such as one or more elements selected from Mn, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Ga, Sn, Sb, Nb, and Ge, and another example can be one or more elements selected from Mn, Ti, V, and Mg; E can be a phosphorus-site doping element, such as one or more elements selected from B, Si, N, S, F, Cl, and Br, and another example can be one or more elements selected from B, Si, N, and S. Doping at least one of the lithium, iron, and phosphorus sites is beneficial to assisting in improving the performance of the positive electrode active material, such as improving the interface performance, reducing the interface side reaction with the electrolyte, reducing the concentration of antisite defects, improving the material kinetics and gram capacity, etc. At the same time, by regulating the iron-site doping element, it is also beneficial to improve the particle morphology and increase the compaction density. If the value of a is too small, the lithium content of the entire core system will be reduced, affecting the specific capacity of the material; the c value will limit the total amount of all doping elements, affecting the iron content in the system, and may also affect the voltage platform of the positive electrode active material; the E element is doped in the position of phosphorus, and since the PO tetrahedron is relatively stable, a large d value may affect the stability of the material; when a, c and d meet the given range of -0.100≤a≤0.100 (such as -0.1, -0.08, -0.05, -0.02, 0, 0.02 , 0.05, 0.08, 0.1, etc., or a range consisting of any of the above values), 0≤c≤1 (such as 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, etc., or a range consisting of any of the above values), 0≤d≤0.100 (such as 0, 0.02, 0.05, 0.08, 0.1, etc., or a range consisting of any of the above values), the positive electrode active material can have better performance. In addition, the selection of the above doping elements and the values of a, b, c, and d can also make Li 1+a M 1b Fe 1-c A c P 1-d E dO4 maintains electrical neutrality, and maintaining electrical neutrality can ensure that the defects and impurities in the positive active material are as few as possible. In the embodiments of the present application, the relative molar amount of each element (such as A element and Fe element) in the positive active material layer can be calculated after respectively measuring the mass of the positive active material layer and the mass of each element in the positive active material layer, wherein the mass of the positive active material layer can be obtained by the disassembly and weighing (accurate to 0.0001g) described in the aforementioned part, and the mass of the A element and the Fe element in the positive active material layer can be obtained in combination with ICP testing. In addition, it can be understood that in the "iron position" doping described in this application, the iron position only represents the positive active material Li 1+a M 1b Fe 1-c A c P 1-d E d The position of the iron element or the A element in the O4 lattice does not mean that there must be an iron element in the iron position. The iron element on the iron position can be partially or completely replaced by the A element. For example, when the c value is 1, the second positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4 does not contain iron. For example, the iron position may include manganese or include manganese and other doping elements.
[0056] In this application, for the above-mentioned positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4, unless otherwise specified, when a doping site has two or more elements, the numerical range of the stoichiometric number of the elements of the corresponding doping site in the chemical formula is limited not only to the stoichiometric number of each element as the site, but also to the sum of the stoichiometric numbers of the elements as the site. For example, when A is two or more elements A1, A2...A n When A1, A2...A n The respective stoichiometric numbers c1, c2, ... c n Each of them must fall within the numerical range of c specified in this application, and c1, c2...c n Similarly, for the case where M1 or E is two or more elements, the numerical ranges of the stoichiometric numbers of M1 and E defined in this application also have the above meanings.
[0057] In some embodiments of the present application, the positive electrode active material Li 1+a M 1b Fe1-c A c P 1-d E d O4 can include lithium iron phosphate system, lithium manganese phosphate system, lithium manganese phosphate iron system, etc. 1+a M 1b Fe 1-c A c P 1-d E d One or more of the positive electrode active materials of O4, for example, the positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4 may include at least one of the following three positive electrode active materials: (1) c = 0, in which case the corresponding positive electrode active material has the general formula Li 1+a M 1b FeP 1-d E d O4, such as but not limited to LiFePO4; (2) c = 1, A is Mn element, then the corresponding positive electrode active material general formula is Li 1+a M 1b MnP 1-d E d O4, such as but not limited to LiMnPO4; (3) 0<c<1, A is Mn element, and the corresponding general formula of the positive electrode active material is Li 1+a M 1b Fe 1-c Mn c P 1-d E d O4, such as but not limited to LiMn 0.5 Fe 0.5 PO4、LiMn 0.3 Fe 0.7 PO4、LiMn 0.5 Fe 0.5 PO4, etc. It should be noted that the positive electrode active material Li 1+a M 1b FeP 1-d E d O4、Li 1+a M 1b MnP 1-d E d O4 and Li 1+a M 1b Fe 1- c Mn c P 1-d Ed In O4, the stoichiometric numbers of elements at the same site can be the same or different, but they all satisfy the chemical formula Li 1+a M 1b Fe 1-c A c P 1-d E d The numerical range defined for the stoichiometric number of each element in O4.
[0058] In some embodiments of the present application, the positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4 can include LiFe 1- c Mn c PO4, 0≤c≤1, among which LiFe 1-c Mn c PO4 can also include LiFePO4, LiMnPO4 and LiFePO4 doped with manganese in the iron position (i.e. LiFe 1-c Mn c One or more of the cases where 0<c<1 in PO4).
[0059] In some embodiments of the present application, 0.25≤CWc≤0.6 (i.e., the surface density of the positive electrode active material layer 12 on one side of the positive electrode sheet can be 0.25g / 1540.25mm 2 ~0.6g / 1540.25mm 2 ), for example, the value of CWc can be 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or 0.6, etc., or can be a range consisting of any of the above values. When the value of CWc is too small, it is not conducive to improving the effect of improving the cycle lithium consumption of the lithium secondary battery that meets the design rules of the embodiment of the present application and the energy density of the lithium secondary battery, and it is easy to increase the cost of the lithium secondary battery; increasing the surface density of the positive electrode active material layer is conducive to improving this problem, but when the value of CWc is too large, on the one hand, it is easy to increase the polarization of the battery, resulting in a deterioration in the cycle life, and on the other hand, it will increase the cost of raw materials and fail to achieve the cost benefit of life improvement. On the basis of satisfying the above formula 1 and / or formula 2, controlling the surface density CWc of the positive electrode active material layer on one side of the positive electrode sheet to meet the given range is conducive to significantly improving the cycle lithium consumption and energy density of the lithium secondary battery, and taking into account the battery cost while improving the battery life. Optionally, 0.26≤CWc≤0.5, and controlling CWc to meet the given range can further improve the life of the lithium secondary battery while taking the battery cost into consideration.
[0060] In some embodiments of the present application, the conductivity ρ of the electrolyte of the lithium secondary battery at 25°C is in the range of 0.008S / cm to 0.020S / cm, for example, it can be 0.008S / cm, 0.01S / cm, 0.012S / cm, 0.014S / cm, 0.016S / cm, 0.018S / cm or 0.02S / cm, or it can be a range composed of any of the above values. The conductivity test of the electrolyte is carried out under a constant temperature of 25°C. For details, please refer to: HG / T4067-2015 Determination of the conductivity of 5.8 lithium hexafluorophosphate electrolyte. An electrolyte with high conductivity can improve the battery kinetics level and improve the overall performance of the lithium secondary battery. On the basis of satisfying Formula 1 and / or Formula 2, by controlling the conductivity of the electrolyte within the given range, it is beneficial to improve the kinetics of the lithium secondary battery and obtain a further improved service life. Optionally, the conductivity ρ of the electrolyte at 25° C. may be set in the range of 0.009 S / cm to 0.016 S / cm, thereby further improving the service life of the lithium secondary battery.
[0061] In some embodiments of the present application, the viscosity of the electrolyte of the lithium secondary battery at 25°C can be 1.5mPa·s to 5mPa·s, for example, 1.5mPa·s, 2mPa·s, 2.5mPa·s, 3mPa·s, 3.5mPa·s, 4mPa·s, 4.5mPa·s or 5mPa·s, or a range consisting of any of the above values. The viscosity test of the electrolyte is carried out at 25°C, and specific reference can be made to: GB / T10247-2008 "Viscosity Measurement Method" Rotation Method. Controlling the viscosity of the electrolyte within the given range is beneficial for obtaining a higher ion migration rate and for allowing the positive electrode and negative electrode to be wetted by the electrolyte in a shorter time, thereby improving the overall performance of the lithium secondary battery. Optionally, the viscosity of the electrolyte can be 2mPa·s to 4mPa·s.
[0062] In some embodiments of the present application, referring to FIG3 , the surface density of the negative active material layer 22 a on the side of the negative electrode sheet 20 facing the positive electrode sheet 10 is CWa, in units of g / 1540.25 mm 2 , wherein the ratio of the area density CWc of the positive electrode active material layer on one side of the positive electrode sheet 10 to the area density CWa of the negative electrode active material layer 22a on the side facing the positive electrode sheet 10 can satisfy the following relationship: For example, The ratio can be 1.6, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6, or can be a range consisting of any of the above values. The surface density test of the negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet can be carried out with reference to the method for testing the surface density of the single layer of the positive electrode active material layer in the aforementioned section. CWa and CWc reflect to a certain extent the reversible lithium insertion amount per unit weight of the negative electrode sheet and the positive electrode sheet active material layer. A decrease in CWc or an increase in CWa will result in The ratio of becomes smaller, and The smaller the ratio of will cause the energy density of lithium secondary batteries to decrease. The ratio of is within the given range, which is conducive to better matching the reversible lithium content of the positive and negative electrodes, thereby improving the cycle life, and further taking into account the energy density and cost of the lithium secondary battery, thereby further optimizing the energy density and cost on the basis of improving the service life of the lithium secondary battery. The ratio can further satisfy Meeting this condition is conducive to further balancing the long service life, high energy density and low cost of lithium secondary batteries.
[0063] In some embodiments of the present application, the positive electrode sheet can be made of the positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4 to form the positive electrode active material layer, or Li 1+a M 1b Fe 1-c A c P 1-d E d O4 is mixed with other positive electrode active materials to form a positive electrode active material layer. 1+a M 1b Fe 1-c A c P 1-d E d In addition to O4, the positive electrode active material used in the positive electrode active material layer can also include one or more of nickel-cobalt-manganese ternary materials, lithium cobalt oxide, Li2O2, lithium manganate (such as lithium-rich lithium nickel oxide), lithium nickel oxide, and lithium vanadate. 1+a M 1b Fe 1-c A c P 1-d E d Mixing O4 with other positive active materials is beneficial to further improve the performance of lithium secondary batteries. As a specific example, nickel-cobalt-manganese ternary materials can be mixed with Li 1+aM 1b Fe 1-c A c P 1-d E d O4 mixing can further take into account the specific capacity of the positive electrode active material layer and the stability during the charge and discharge process, thereby improving the energy density and service life of the lithium secondary battery.
[0064] In some embodiments of the present application, based on the total mass of the positive electrode active material in the positive electrode active material layer, Li 1+a M 1b Fe 1-c A c P 1-d E d The content of O4 may be not less than 94wt%, for example, 94wt%, 95wt%, 96wt%, 97wt%, 98wt%, 99wt% or 100wt%, or any range thereof. 1+a M 1b Fe 1-c A c P 1-d E d The mass proportion of O4 in the positive electrode active material layer satisfies the given range, which can further improve the cycle life of the lithium secondary battery and extend its service life.
[0065] In some embodiments of the present application, in the negative electrode sheet, the negative electrode active material graphite can be used alone to form the negative electrode active material layer, or graphite can be mixed with other negative electrode active materials to form the negative electrode active material layer. For example, in addition to graphite, the negative electrode active material in the negative electrode active material layer can also include one or more of hard carbon, soft carbon, mesophase carbon microbeads, lithium titanate, carbon fiber, silicon-based materials, and tin-based materials. Mixing graphite with other negative electrode active materials is beneficial to achieving the purpose of improving the lithium insertion capacity, rate performance, raw material cost, etc. of the negative electrode sheet according to actual needs. As a specific example, graphite can be mixed with silicon-based materials to form a negative electrode active material layer. This method can further improve the lithium insertion capacity of the negative electrode active material layer and improve the energy density of the lithium secondary battery.
[0066] In some embodiments of the present application, the graphite content may be no less than 85wt% based on the total mass of the negative electrode active material in the negative electrode active material layer, for example, 85wt%, 88wt%, 90wt%, 92wt%, 95wt%, 98wt%, or 100wt%, or a range consisting of any of the above values. Graphite has a relatively stable structure and relatively small volume change during lithium ion insertion and extraction. By controlling the mass percentage of graphite in the negative electrode active material layer to meet the given range, it is beneficial to further improve the stability of the negative electrode sheet and improve the cycle life of the lithium secondary battery.
[0067] In some embodiments of the present application, the graphite in the negative electrode active material layer may be artificial graphite. Compared with natural graphite, artificial graphite has better cycle stability and less side reactions with the electrolyte, which is more conducive to improving the cycle life of lithium secondary batteries.
[0068] In some embodiments of the present application, the OI value of graphite can be 0.5 to 7 (Orientation Index), for example, 0.5, 1, 2, 3, 4, 5, 6 or 7, or a range consisting of any of the above values. The OI value of graphite can refer to JIS / K0131-1996 General Rules for X-ray Diffraction Analysis, and the C004 and C110 peak positions are scanned at a low speed respectively, and the OI value is calculated by the formula OI=I(C004) / I(C110), where I(C004) refers to the peak intensity of the C004 peak, and I(C110) refers to the peak intensity of C110. Controlling the OI value of graphite within the given range can enable the negative electrode active material to have better electrolyte wetting performance, better conductivity and good stability, thereby helping to improve the overall performance of the lithium secondary battery. Optionally, the OI value of graphite may be 2 to 4.5. Controlling the OI value of graphite within the given range may further improve the overall performance of the lithium secondary battery.
[0069] In some embodiments of the present application, the BET specific surface area of graphite can be 0.8 m 2 / g~1.5m 2 / g, for example, it can be 0.8m 2 / g, 1.0m 2 / g, 1.2m 2 / g, 1.5m 2 / g, etc., or can be a range consisting of any of the above values. The specific surface area of graphite can be measured by conventional methods in the art, such as nitrogen physical adsorption. Increasing the specific surface area helps to increase the active sites of graphite and improve power performance, but these increased active sites also increase the side reactions of graphite during the charge and discharge cycle, thereby causing the cycle performance to deteriorate. By controlling the specific surface area of graphite within the given range, the capacity and cycle performance of lithium secondary batteries can be further improved, and the service life can be extended.
[0070] In some embodiments of the present application, the degree of graphitization of the graphite may be 70% to 99%, for example, 70%, 74%, 80%, 85%, 90%, 96%, 99%, or the like, or a range consisting of any of the above values. The degree of graphitization of the graphite may be determined by X-ray diffraction or laser Raman spectroscopy. For example, the degree of graphitization of the graphite may be determined according to JIS / K0131-1996, General Rules for X-ray Diffraction Analysis Methods, by calculating the crystal cell parameters using X-ray polycrystalline diffraction, obtaining the C004 and Si311 peak positions of two parallel samples using the center of gravity method, and substituting the peak positions into the interplanar spacing formula to calculate the value of the graphite interlayer spacing d002; substituting the obtained d002 into the Mering-Maire formula (also known as the Franklin formula): g = [(3.440-d002) / (3.440-3.354)] × 100% to obtain the value of the degree of graphitization g. Controlling the graphitization degree of the graphite within a given range can further improve the conductivity of the negative electrode active material layer, facilitate the diffusion of lithium ions, and improve the overall performance of the lithium secondary battery. Optionally, the graphitization degree of the graphite can be 75% to 98%. Controlling the graphitization degree of the graphite within the given range can further improve the overall performance of the lithium secondary battery.
[0071] In some embodiments of the present application, the Dv50 particle size of graphite can be 1 μm to 20 μm, for example, it can be 1 μm, 3 μm, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 12 μm, 15 μm, 18 μm or 20 μm, etc., or it can be a range composed of any of the above numerical values. The Dv50 particle size of graphite refers to the particle size corresponding to when the cumulative volume distribution percentage of graphite reaches 50%, which can be measured by laser diffraction particle size analysis, for example, it can be measured using a laser particle size analyzer (such as Malvern Master Size 3000) with reference to standard GB / T 19077-2016. Smaller graphite particle size is beneficial to improving the rate performance and cycle performance of the negative electrode, but the first efficiency is poor. By controlling the particle size of graphite within the given range, it is beneficial to make the lithium secondary battery have both good rate performance and cycle performance, as well as higher initial discharge capacity and first effect. Optionally, the Dv50 particle size of the graphite may be 4 μm to 15 μm. Controlling the particle size of the graphite within the given range is beneficial to further improving the overall performance of the lithium secondary battery.
[0072] In some embodiments of the present application, the thickness of the positive electrode sheet 10 can be 130 μm to 350 μm, for example, 130 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 320 μm, 350 μm, etc., or can be a range consisting of any of the above values. The thickness of the negative electrode sheet 20 can be 100 μm to 300 μm, for example, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, etc., or can be a range consisting of any of the above values. The thickness of the positive electrode sheet and the negative electrode sheet can be measured separately by a micrometer, specifically by measuring the thickness of the electrode sheet at multiple points and obtaining the average value of the thickness of the electrode sheet by statistics. In the present application, by controlling the thickness of the positive electrode sheet and the negative electrode sheet within a given range, it is beneficial to obtain a higher energy density while taking into account better rate performance.
[0073] In some embodiments of the present application, referring to FIG1 , the reversible lithium capacity of the positive active material layer 12 located on one side of the positive electrode sheet 10 is Dc, in units of mAh / 1540.25 mm 2 3, the reversible lithium capacity of the negative electrode active material layer 22a on the negative electrode sheet 20 facing the positive electrode sheet 10 is Da, in units of mAh / 1540.25mm 2 ;in, The value range of K1 can satisfy: 1.036≤K1≤1.308, for example, the value of K1 can be 1.05, 1.08, 1.1, 1.12, 1.15, 1.18, 1.2, 1.22, 1.25, 1.28, 1.3, etc., or can be a range composed of any of the above values. For the lithium secondary battery of the embodiment of the present application, it is necessary to consider the mutual matching of the reversible lithium amount of the positive and negative electrode plates, improve the utilization rate of the positive electrode active material, and also take into account the cycle life, energy density and cost of the lithium secondary battery. Increasing the value of K1 is conducive to improving the cycle life of the battery and extending the service life. However, when the value of K1 is too large, although it will also increase the life of the lithium secondary battery, the increase in its life is small, but the cost will increase significantly. By controlling the value of K1 within the given range, the energy density and cost of the lithium secondary battery can be further taken into account on the basis of improving the service life of the lithium secondary battery.
[0074] In some embodiments of the present application, referring to FIG1 , the reversible lithium capacity of the positive active material layer 12 located on one side of the positive electrode sheet 10 is Dc, in units of mAh / 1540.25 mm 2 3, the first lithium insertion capacity of the negative electrode active material layer 22b on the side of the negative electrode sheet 20 away from the positive electrode sheet 10 is Ca, in units of mAh / 1540.25mm 2 ;in, The value range of K2 can satisfy: 1.149≤K2≤1.427, for example, the value of K2 can be 1.15, 1.18, 1.2, 1.22, 1.25, 1.28, 1.3, 1.32, 1.35, 1.38, 1.4 or 1.42, etc., or can be a range composed of any of the above values. During the charge and discharge process, the surface of the negative electrode plate facing away from the positive electrode plate does not participate in the reaction, and the surface of the negative electrode plate facing away from the positive electrode plate does not embed lithium. By making the value of K2 satisfy the given range, the matching relationship between the reversible lithium capacity of the negative electrode active material layer on the side of the negative electrode plate facing the positive electrode plate and the reversible lithium capacity of the positive electrode active material layer on the single side of the positive electrode plate can be further improved, and energy density and cost can be further taken into account on the basis of improving the service life of the lithium secondary battery.
[0075] In some embodiments of the present application, the lithium secondary battery can be either a laminated battery or a wound battery, and the wound battery can be either a square battery or a cylindrical battery. Depending on the battery type, the positive electrode sheet, the negative electrode sheet, and the separator can be stacked to form a laminate unit, or can be stacked and then wound to form a wound body.
[0076] In some embodiments of the present application, the battery may be a single cell or a battery module assembled from cells. A battery module may include multiple cells, the specific number of which may be adjusted based on the application and capacity of the battery module. Furthermore, the battery module may also include a packaging assembly having a storage space, which may include a bottom plate, side plates, and a cover plate.
[0077] In some embodiments of the present application, the above-mentioned battery modules may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0078] In addition, the present application also provides an electrical device, which includes: the lithium secondary battery of the first aspect of the present application.
[0079] The lithium secondary battery, such as a battery cell, a battery module or a battery pack, can be used as both a power source and an energy storage unit of the electrical device. The electrical device may include, but is not limited to, a mobile device (e.g., a mobile phone, a laptop computer), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, and an energy storage system. As a specific example, as shown in FIG4 , the electrical device may be a vehicle.
[0080] The electrical device can select the specific type of battery according to its usage requirements, such as battery cells, battery modules or battery packs.
[0081] As an example, the electric device may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the electric device's requirements for high power and high energy density of the battery, a battery pack or battery module may be used.
[0082] As another example, the electrical device may be a mobile phone, a tablet computer, or a laptop computer. The electrical device is generally required to be lightweight and thin, and may use a battery cell as a power source.
[0083] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0084] Preparation and testing methods of lithium secondary batteries:
[0085] (1) Preparation of positive electrode sheet
[0086] The positive electrode active material LiFePO4 (gram capacity of 160 mAh / g), the conductive agent acetylene black, and the binder PVDF (polyvinylidene fluoride) were mixed in a weight ratio of 94:4:2, and the solvent N-methylpyrrolidone was added and stirred thoroughly to obtain a positive electrode slurry, which was then coated on both surfaces of the positive electrode current collector aluminum foil. The coating weight of the positive electrode slurry on one side of the aluminum foil was 0.256 g / 1540.25 mm 2 (based on weight excluding solvent), and then dried and cold pressed to obtain a positive electrode sheet.
[0087] (2) Preparation of negative electrode sheet
[0088] The negative electrode active material artificial graphite (initial lithium insertion capacity of 370 mAh / g, reversible lithium insertion capacity of 333 mAh / g), conductive agent acetylene black, binder SBR (styrene-butadiene rubber) + CMC (sodium carboxymethyl cellulose) were mixed in a weight ratio of 95:1.5:3.1:0.4, and deionized water was added as a solvent. The mixture was stirred and mixed to obtain a negative electrode slurry, which was then coated on both surfaces of the negative electrode current collector copper foil. The coating weight of the negative electrode slurry on one side of the copper foil was 0.1370 g / 1540.25 mm 2 (based on weight excluding solvent), and after drying and cold pressing, a negative electrode sheet is obtained.
[0089] (3) Preparation of electrolyte
[0090] In an argon atmosphere glove box with a water content of <10ppm, EC (ethylene carbonate), PC (propylene carbonate), and DMC (dimethyl carbonate) are mixed in a specific proportion, and then the fully dried lithium salt LiPF6 is dissolved in the above mixed organic solvent. After stirring evenly, an electrolyte with a conductivity of 0.014S / cm is obtained, in which the concentration of LiPF6 is 1mol / L.
[0091] (4) Preparation of isolation membrane
[0092] A polyethylene porous membrane was used as the separator.
[0093] (5) Preparation of lithium secondary batteries
[0094] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to provide isolation, and then wound to form a bare cell. The bare cell is placed in an outer packaging, injected with the prepared electrolyte, and packaged to obtain a lithium-ion secondary battery.
[0095] Under this design:
[0096] The surface density CWc of the positive active material layer on one side of the positive electrode sheet is 0.256g / 1540.25mm 2 ;
[0097] The reversible lithium capacity Dc (mAh / 1540.25mm) of the positive active material layer on one side of the positive electrode 2 ) = the surface density of the positive electrode active material layer located on one side of the positive electrode sheet × the mass ratio of the positive electrode active material in the positive electrode active material layer × the gram capacity of the positive electrode active material, that is, Dc = 0.256g / 1540.25mm 2 ×0.94×160mAh / g;
[0098] The surface density CWa of the negative active material layer on the side of the negative electrode sheet facing away from the positive electrode sheet is 0.1370 g / 1540.25 mm 2 ;
[0099] The initial lithium insertion capacity of the negative electrode active material layer on the side of the negative electrode sheet facing away from the positive electrode sheet is Ca(mAh / 1540.25mm 2 ) = CWa × 0.95 × 370 mAh / g;
[0100] The reversible lithium capacity of the negative active material layer on the side of the negative electrode sheet facing the positive electrode sheet is Da (mAh / 1540.25mm 2 ) = CWa × 0.95 × 333 mAh / g;
[0101] The conductivity ρ of the electrolyte at 25°C is 0.014 S / cm;
[0102] Formula 1 is: 1.0337+0.37×CWc–7.79×ρ≤K1≤1.07+0.93×CWc–2.9×ρ.
[0103] Formula 2 is: 1.1485+0.43×CWc–9.2×ρ≤K2≤1.13+1.069×CWc–1.7×ρ.
[0104] (3) Room temperature cycle performance test of lithium secondary batteries
[0105] At 25°C, the lithium secondary battery was first charged at a constant current of 1C (the current value that completely discharges the theoretical capacity within 1 hour) to a voltage of 3.65V. Then, it was charged at a constant voltage of 3.65V to a current of 0.05C. After standing for 5 minutes, the lithium secondary battery was discharged at a constant current of 1C to a voltage of 2.5V. This constitutes one charge-discharge cycle, and the discharge capacity at this time is the discharge capacity of the first cycle. The lithium secondary battery was subjected to multiple charge-discharge cycles according to the above method until the discharge capacity of the lithium secondary battery decayed to 80%. The number of cycles of the lithium secondary battery was recorded.
[0106] Examples 2 to 10 and Comparative Examples 1 to 7
[0107] The difference between Comparative Examples 1 and 2 and Example 1 is that the surface density CWc (unit: g / 1540.25 mm2) of the positive electrode active material layer on one side of the positive electrode sheet is 2 ) are different, see Table 1 for details.
[0108] The difference between Example 2 and Example 1 is that the surface density CWc (unit: g / 1540.25mm) of the positive electrode active material layer on one side of the positive electrode sheet is 2 ) are different, see Table 1 for details.
[0109] The difference between Example 3 and Example 1 is that the surface density CWc (unit: g / 1540.25mm) of the positive electrode active material layer on one side of the positive electrode sheet is 2 ) is different, the surface density CWa (unit: g / 1540.25mm) of the negative electrode active material layer on the side of the negative electrode sheet away from the positive electrode sheet 2 ) are different, see Table 1 for details.
[0110] The difference between Example 4 and Example 1 is that the conductivity ρ (unit: S / cm) of the electrolyte at 25° C. is different, see Table 1 for details.
[0111] The difference between Comparative Example 3 and Example 1 is that the surface density CWa (unit: g / 1540.25 mm2) of the negative electrode active material layer on the side of the negative electrode sheet facing away from the positive electrode sheet is 2 ) are different, see Table 1 for details.
[0112] The difference between Example 5 and Example 1 is that the surface density CWc (unit: g / 1540.25mm) of the positive electrode active material layer on one side of the positive electrode sheet is 2 ) is different, the surface density CWa (unit: g / 1540.25mm) of the negative electrode active material layer on the side of the negative electrode sheet away from the positive electrode sheet 2 ) are different, see Table 1 for details.
[0113] The difference between Example 6 and Example 1 is that the surface density CWc (unit: g / 1540.25mm) of the positive electrode active material layer on one side of the positive electrode sheet is 2 ) are different, see Table 1 for details.
[0114] The difference between Examples 7 and 8 and Example 1 is that the surface density CWa (unit: g / 1540.25 mm2) of the negative electrode active material layer on the side of the negative electrode sheet facing away from the positive electrode sheet is 2 ) different, reversible lithium insertion capacity of artificial graphite (unit: mAh / g), see Table 1 for details.
[0115] The difference between Comparative Example 4 and Example 1 is that the surface density CWc (unit: g / 1540.25mm) of the positive electrode active material layer on one side of the positive electrode sheet is2 ) is different, the surface density CWa (unit: g / 1540.25mm) of the negative electrode active material layer on the side of the negative electrode sheet away from the positive electrode sheet 2 ) are different, see Table 1 for details.
[0116] The difference between Comparative Example 5 and Example 1 is that the surface density CWc (unit: g / 1540.25mm) of the positive electrode active material layer on one side of the positive electrode sheet is 2 ) are different, and the conductivity ρ (unit: S / cm) of the electrolyte at 25°C is different, see Table 1 for details.
[0117] The difference between Example 9 and Example 1 is that the positive active material in the positive electrode sheet is LiFe 0.4 Mn 0.6 PO4 (gram capacity is 156 mAh / g), the surface density CWc of the positive electrode active material layer on one side of the positive electrode sheet (unit: g / 1540.25 mm 2 )different.
[0118] The difference between Example 10 and Example 1 is that the positive active material in the positive electrode sheet is LiFe 0.8 Mn 0.2 PO4 (gram capacity is 158 mAh / g), the surface density CWc of the positive electrode active material layer on one side of the positive electrode sheet (unit: g / 1540.25 mm 2 )different.
[0119] The difference between Comparative Example 6 and Example 1 is that the positive active material in the positive electrode sheet is LiFe 0.4 Mn 0.6 PO4, the surface density CWc of the positive electrode active material layer on one side of the positive electrode sheet (unit: g / 1540.25mm 2 )different.
[0120] The difference between Comparative Example 7 and Example 1 is that the positive active material in the positive electrode sheet is LiFe 0.8 Mn 0.2 PO4, the surface density CWc of the positive electrode active material layer on one side of the positive electrode sheet (unit: g / 1540.25mm 2 )different.
[0121] The lithium secondary batteries assembled in Examples 1 to 10 and Comparative Examples 1 to 7 were tested. The test results are shown in Table 1.
[0122] Table 1 Differences between Examples 1 to 8 and Comparative Examples 1 to 5 and related test results
[0123] Table 2 Analysis of cycle test results of Examples 1 to 10 and Comparative Examples 1 to 7
[0124] Results and Conclusions:
[0125] From Examples 1 to 10 and Comparative Examples 1 to 7, as well as Tables 1 and 2, it can be seen that, on the basis of the consistency of the positive electrode sheet material, negative electrode sheet material, electrolyte, and separator of the lithium secondary battery, when Formula 1 and / or Formula 2 are satisfied, the cycle life of the lithium secondary battery can be significantly improved. In addition, appropriately increasing K1 and / or K2 is beneficial to improving the cycle life of the battery, but too high will sacrifice performance in terms of cost and energy density. Further, when preparing a lithium secondary battery, selecting an electrolyte with relatively high conductivity is also beneficial to improving the cycle performance of the battery. On this basis, further satisfying Formulas 1 and 2 is beneficial to further optimize the cycle life. In addition, when preparing a lithium secondary battery, by further optimizing the selection of the positive active material, the density and / or reversible lithium capacity of the positive active material layer, the first lithium insertion capacity and / or reversible lithium capacity of the negative active material layer, the matching relationship between the density of the positive active material layer and the density of the negative active material layer, etc., the cycle life of the lithium secondary battery can also be further improved. On this basis, further satisfying Formulas 1 and 2 is also beneficial to further optimize the cycle life.
[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A lithium secondary battery, characterized in that: include: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material Li 1+a M 1b Fe 1-c A c P 1-d E d O4, wherein -0.100≤a≤0.100, 0≤b≤1.1, 0≤c≤1, 0≤d≤0.100, M1 includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W, A includes one or more elements selected from Mn, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Ga, Sn, Sb, Nb and Ge, E includes one or more elements selected from B, Si, N, S, F, Cl and Br, and the Li 1+a M 1b Fe 1-c A c P 1-d E d The mass percentage of O4 in the positive electrode active material layer is not less than 85wt%; A negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, the negative electrode active material layer comprising graphite, the mass proportion of the graphite in the negative electrode active material layer being not less than 85wt%, Wherein: the surface density of the positive electrode active material layer located on one side of the positive electrode sheet is CWc, in units of g / 1540.25mm 2 , the reversible lithium capacity is Dc, the unit is mAh / 1540.25mm 2 The reversible lithium capacity of the negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet is Da, in units of mAh / 1540.25mm 2 The first lithium insertion capacity of the negative electrode active material layer on the side of the negative electrode sheet away from the positive electrode sheet is Ca, in units of mAh / 1540.25mm 2 ; The lithium secondary battery meets: Formula 1: 1.0337 + 0.37 × CWc – 7.79 × ρ ≤ K1 ≤ 1.07 + 0.93 × CWc – 2.9 × ρ; and / or, Formula 2: 1.1485+0.43×CWc–9.2×ρ≤K2≤1.13+1.069×CWc–1.7×ρ; in, ρ is the conductivity of the electrolyte of the lithium secondary battery at 25° C., and the unit is S / cm.
2. The lithium secondary battery according to claim 1, characterized in that: The Li 1+a M 1b Fe 1-c A c P 1-d E d O4 includes at least one of the following three positive electrode active materials: (1)c=0; (2) c = 1, A is Mn element; (3) 0<c<1, and A is a Mn element.
3. The lithium secondary battery according to claim 1, characterized in that: The Li 1+a M 1b Fe 1-c A c P 1-d E d O4 includes LiFe 1-c Mn c PO4, 0≤c≤1.
4. The lithium secondary battery according to any one of claims 1 to 3, characterized in that 0.25≤CWc≤0.6, optionally, 0.26≤CWc≤0.
5.
5. The lithium secondary battery according to any one of claims 1 to 4, characterized in that: The value range of ρ is 0.008~0.020, and can be selected as 0.009~0.
016.
6. The lithium secondary battery according to any one of claims 1 to 5, characterized in that The viscosity of the electrolyte at 25° C. is 1.5 mPa·s to 5 mPa·s, and can be optionally 2 mPa·s to 4 mPa·s.
7. The lithium secondary battery according to any one of claims 1 to 6, characterized in that The surface density of the negative electrode active material layer on the side of the negative electrode sheet facing the positive electrode sheet is CWa, in g / 1540.25 mm 2 ,in: Optionally, 8. The lithium secondary battery according to any one of claims 1 to 7, characterized in that The positive electrode active material in the positive electrode active material layer further includes one or more of nickel-cobalt-manganese ternary material, lithium cobalt oxide, Li2O2, lithium manganate, lithium nickel oxide, and lithium vanadate; and / or, The negative electrode active material in the negative electrode active material layer further comprises one or more of hard carbon, soft carbon, mesophase carbon microbeads, lithium titanate, carbon fiber, silicon-based material, and tin-based material.
9. The lithium secondary battery according to any one of claims 1 to 8, characterized in that Based on the total mass of the positive electrode active material in the positive electrode active material layer, the Li 1+a M 1b Fe 1-c A c P 1-d E d The content of O4 is not less than 94wt%; and / or, Based on the total mass of the negative electrode active material in the negative electrode active material layer, the content of the graphite is not less than 85wt%.
10. The lithium secondary battery according to any one of claims 1 to 9, characterized in that The graphite satisfies at least one of the following conditions: The OI value of the graphite is 0.5 to 7, and can be optionally 2 to 4.5; The BET specific surface area of the graphite is 0.8 m 2 / g~1.5m 2 / g; The graphitization degree of the graphite is 70% to 99%, and can be optionally 75% to 98%; The Dv50 particle size of the graphite is 1 μm to 20 μm, and can be optionally 4 μm to 15 μm.
11. The lithium secondary battery according to any one of claims 1 to 10, characterized in that: The graphite is artificial graphite.
12. The lithium secondary battery according to any one of claims 1 to 11, characterized in that: The thickness of the positive electrode sheet is 130 μm to 350 μm, and the thickness of the negative electrode sheet is 100 μm to 300 μm.
13. The lithium secondary battery according to any one of claims 1 to 12, characterized in that: 1.036≤K1≤1.308; and / or, 1.149≤K2≤1.
427.
14. An electrical device, wherein: A lithium secondary battery comprising the lithium secondary battery according to any one of claims 1 to 13.
Citation Information
Patent Citations
Lithium ion secondary battery and preparation method thereof
CN110212193A
Lithium ion battery
CN110896143A
Electrochemical device and electronic device
CN114938689A
Lithium ion battery and battery pack
CN115275319A
Negative pole piece and preparation method thereof, secondary battery, battery module, battery pack and power utilization device
CN115842094A