Bio-based epoxy monomer, medium-temperature curable epoxy resin system, and preparation method
By using protocatechuic aldehyde, erythritol and epoxychloropiane to synthesize tetraepoxy monomers, combined with an acid anhydride curing agent, and using a medium temperature curing procedure, the problem of low mechanical strength and glass transition temperature of bio-based epoxy resin was solved solve the problem and realize a multifunctional epoxy resin system with high performance and low energy consumption.
Patent Information
- Application Number
- PCT/CN2023/085503
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Existing bio-based epoxy resins have poor mechanical strength, low glass transition temperature, and high-temperature curing leads to high energy consumption. It is difficult to achieve a high-performance degradable multi-functional epoxy resin system with low and medium temperature curing.
Protocatechuic aldehyde, erythritol and epichlorohydrin are used to synthesize tetraepoxy monomers, combined with acid anhydride curing agents and catalysts, and medium-temperature curing procedures (≤120°C) are used to prepare high-performance degradable multi-functional epoxy resins system.
It achieves high-performance mechanical properties, good heat resistance and multifunctionality, such as self-healing, shape memory and mild degradation, with low energy consumption, short curing temperature and time, and is superior to existing biomass epoxy resins.
Smart Images

Figure CN2023085503_03102024_PF_FP_ABST
Abstract
Description
A bio-based epoxy monomer and medium-temperature curing epoxy resin system and preparation method Technical Field
[0001] The present invention relates to a novel bio-based epoxy monomer and preparation of a medium-temperature-cured high-performance degradable multifunctional epoxy resin system thereof, belonging to the technical field of polymer chemical synthesis and high-performance resin preparation. Background Art
[0002] Epoxy resin is a typical high-performance thermosetting resin, showing great application value in cutting-edge industrial fields such as electronic information, aerospace, electrical insulation, and rail transportation. At present, more than 90% of epoxy monomers are derived from bisphenol A, which is non-renewable and comes from petroleum resources. In view of environmental problems such as limited petroleum resources, climate change, and carbon dioxide emissions, biomass raw materials such as vegetable oils, lignin, isosorbide, starch, eugenol, vanillin, cardanol, etc. have been widely used to synthesize bio-based thermosetting epoxy resins, and show broad application prospects in coatings, adhesives, composite materials, electronic packaging and other fields. However, since the synthetic raw materials contain a large number of flexible chain segments, most bio-based epoxy monomer cured products have poor mechanical strength and low glass transition temperature (T g ) is low, which limits their practical application. Studies have shown that the introduction of rigid structures in epoxy monomers and the use of high-temperature curing agents can improve the mechanical and thermal properties of the epoxy matrix. In addition, like other thermosetting resins, the highly cross-linked network structure formed by bio-based epoxy resins is difficult to recycle and its waste will also cause serious environmental problems. Although some chemical and physical methods (such as mechanical grinding, pyrolysis, etc.) have been used to treat thermosetting resins, these methods usually require high energy consumption and harsh conditions. Therefore, effectively delaying the service life of materials and preparing easily degradable epoxy resin systems can avoid excessive consumption of materials and reduce energy consumption for the treatment of waste materials. Practice has shown that creating dynamic reversible bonds in polymer systems can achieve crack repair and extend the service life of materials. Unfortunately, the current epoxy resin systems with mild degradation behavior based on dynamic reversible bonds are generally T g Even if some epoxy resin systems have excellent mechanical and thermal properties, they usually use high-temperature curing agents, which result in high curing temperatures and high energy consumption. Therefore, actively developing high-performance bio-based epoxy resin systems with dynamic reversible bonds and mild degradation behavior that can be cured at low and medium temperatures has important economic value and social significance for promoting the application of bio-based epoxy resins. Technical issues
[0003] The present invention provides a novel bio-based epoxy monomer and its preparation for a high-performance, biodegradable, and multifunctional epoxy resin system that cures at a moderate temperature. The epoxy monomer is synthesized using biomass-derived protocatechuic aldehyde, erythritol, and epichlorohydrin as raw materials. A multifunctional, high-performance epoxy resin system with self-healing, shape memory, and biodegradability is prepared using a moderate-temperature curing process. Technical Solutions
[0004] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0005] A novel bio-based epoxy monomer and its medium-temperature curing high-performance degradable multifunctional epoxy resin system and preparation method are disclosed. The bio-based epoxy monomer is synthesized using protocatechuic aldehyde, erythritol, and epichlorohydrin as raw materials and is a tetraepoxy monomer called DGEVP. The bio-based epoxy monomer is used as the raw material, an anhydride curing agent and a catalyst are added, and a medium-temperature curing process (≤120°C) is adopted to obtain a high-performance degradable multifunctional epoxy resin system.
[0006] The invention discloses a preparation method of the bio-based epoxy monomer. The method comprises the following steps: using protocatechuic aldehyde and erythritol as raw materials to prepare a tetrahydroxy monomer; and then using the tetrahydroxy monomer and epichlorohydrin as raw materials to prepare the bio-based epoxy monomer.
[0007] In the present invention, protocatechuic aldehyde and erythritol are used as raw materials, and a tetrahydroxy monomer is prepared by reaction in the presence of a catalyst in a solvent; preferably, the reaction is carried out at 70-100° C. for 12-24 hours; preferably, the catalyst is p-toluenesulfonic acid monohydrate (p-TSA.H2O) and the solvent is N,N-dimethylformamide; further preferably, the reaction is carried out in the presence of a water scavenger; the molar ratio of protocatechuic aldehyde, erythritol, and p-toluenesulfonic acid monohydrate is 200:(100-120):(4-6).
[0008] In the present invention, the bio-based epoxy monomer is prepared using tetrahydroxy monomer and epichlorohydrin as raw materials in the presence of an organic ammonium salt under an alkaline environment. Preferably, the tetrahydroxy monomer (VP) and epichlorohydrin (ECH) are reacted at 40-80° C. for 1-12 hours in the presence of an organic ammonium salt, and then reacted under an alkaline environment for 2-4 hours to prepare the bio-based epoxy monomer. Preferably, the organic ammonium salt is tetrabutylammonium bromide. Sodium hydroxide solution is added to form an alkaline environment. More preferably, sodium hydroxide solution is added at room temperature, and then reacted for 2-4 hours to prepare the bio-based epoxy monomer. The molar ratio of tetrahydroxy monomer, epichlorohydrin, and tetrabutylammonium bromide is 1:(40-250):(1-3).
[0009] The present invention discloses a medium-temperature curing epoxy resin system, which comprises the above-mentioned bio-based epoxy monomer, anhydride curing agent and a catalyst, and is a novel bio-based medium-temperature curing high-performance degradable multifunctional epoxy resin system; after medium-temperature curing, a high-performance degradable multifunctional epoxy resin is obtained.
[0010] The present invention discloses a method for preparing the aforementioned medium-temperature curing epoxy resin system. The method comprises melt-mixing the aforementioned bio-based epoxy monomer DGEVP with a catalyst, then adding an anhydride compound at 60-80°C and prepolymerizing for 20-40 minutes to obtain a medium-temperature curing epoxy resin system. The system is then cured using a medium-temperature curing process (curing temperature below 125°C) to obtain a high-performance, biodegradable, multifunctional epoxy resin. The molar ratio of the epoxy groups of the bio-based epoxy monomer to the anhydride groups of the anhydride compound is 1:(0.8-1.0), and the catalyst is present in an amount of 0.5-5% by mass of the DGEVP. Preferably, the temperature for melt-mixing the DGEVP and catalyst is 140-210°C.
[0011] In the present invention, the acid anhydride compound is a low melting point petroleum-based acid anhydride, a bio-based acid anhydride or a mixture thereof, mainly including glutaric anhydride, maleic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, dodecenylsuccinic anhydride, maleic anhydride, citraconic anhydride, succinic anhydride or a mixture thereof.
[0012] In the present invention, the catalyst is an organic metal complex, such as one or more of zinc acetylacetonate, zirconium acetylacetonate, aluminum acetylacetonate, iron acetylacetonate, and cadmium acetylacetonate.
[0013] In the present invention, the medium temperature curing process is a step-by-step temperature increase method, and the preferred medium temperature curing process is 80° C. / 2 h + 100° C. / 2 h + 120° C. / 0 to 4 h.
[0014] The novel bio-based epoxy monomer of the present invention adopts a high-performance degradable multifunctional epoxy resin cured at medium temperature, which has excellent mechanical properties, bending strength: 105-156MPa, impact strength: 13.5-32kJ / cm 2 , tensile strength: 45 ~ 81MPa; good heat resistance, T g : 113~158℃; and has multifunctional properties such as self-repair, shape memory and mild degradability. Beneficial effects
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The present invention uses natural raw materials to synthesize tetraepoxy monomers. Due to the high content of epoxy groups, the reaction activity is high. The process for preparing tetraepoxy monomers in the present invention is also applicable to the reaction of protocatechuic aldehyde with other polyol compounds and epichlorohydrin to prepare epoxy monomers with multiple epoxy functional groups.
[0017] (2) The present invention uses anhydride as a curing agent and adopts a medium-temperature curing procedure (80℃ / 2h+100℃ / 2h+120℃ / 0-4h) to obtain a high-performance resin system with multifunctional properties such as self-repairing, shape memory and mild acid degradation. Compared with existing biomass epoxy monomers and even traditional commercial bisphenol A epoxy resins, the resin system of the present invention has the advantages of low curing temperature and short curing time, which can effectively save energy consumption. In addition, the comprehensive mechanical and thermal properties of the cured system are significantly better than the currently reported biomass epoxy system with mild degradation characteristics containing dynamic reversible bonds, and are comparable to the mechanical and thermal properties of traditional commercial bisphenol A epoxy resin systems cured with the same curing agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a schematic diagram of the synthesis of VP and DGEVP.
[0019] Figure 2 shows the FTIR images of PCA, erythritol, VP and DGEVP (a); VP 1 H NMR spectra (b); VP 13 C NMR spectra (c); DGEVP 1 H NMR spectra (d); DGEVP 13 C NMR spectra (e); LC-MS spectra of VP (f) and DGEVP (g).
[0020] FIG3 is a diagram showing the healing process of scratches on the surface of the cured sample of Example 1 at 200° C. A scalpel was used to scratch the surface of the cured sample to form a scratch with a depth of about 22 μm, and then the sample was placed in an oven.
[0021] FIG4 is a diagram showing the shape deformation and recovery of the cured sample of Example 1 at 130° C. The cured sample was first bent at 130° C. and shaped at room temperature. The bent sample was then placed in an oven and allowed to recover in a short time.
[0022] FIG5 is a DSC curve of the resin system in Example 1 and Comparative Example 1, 10° C. / min.
[0023] Figure 6 shows the degradation profile of the cured product of Example 2 in a 1 M hydrochloric acid solution (acetone / water = 9:1, v:v) at 50°C (a); and the real-time 1H NMR spectra of the main degradation products of the cured product of Example 2 in a 0.1 M HCl solution (acetone / water = 9:1, v:v) at 50°C (b).
[0024] FIG7 is a diagram showing the healing process of scratches on the surface of the cured sample of Example 2 at 200° C.
[0025] FIG8 is a graph showing the shape deformation and recovery of the cured sample of Example 2 at 130° C. and a graph showing three shape memory cycle curves.
[0026] FIG9 is a diagram showing the healing process of scratches on the surface of the cured sample of Example 3 at 210°C.
[0027] FIG10 is a diagram showing the shape deformation and recovery of the cured sample of Example 3 at 176°C.
[0028] FIG11 is a diagram showing the healing process of scratches on the surface of the cured sample of Example 3 at 200°C.
[0029] FIG12 is a diagram showing the shape deformation and recovery of the cured sample of Example 4 at 160°C. Modes for Carrying Out the Invention
[0030] This invention synthesizes a tetraepoxy monomer (DGEVP) using protocatechuic aldehyde, erythritol, and epichlorohydrin as the main raw materials. This epoxy monomer is then used as the raw material, along with an anhydride curing agent and a catalyst, to produce a high-performance, biodegradable, multifunctional epoxy resin system using a medium-temperature curing process (≤120°C). The invention uses protocatechuic aldehyde and erythritol as raw materials to prepare the tetrahydroxy monomer; then, the tetrahydroxy monomer and epichlorohydrin are used as raw materials to prepare the bio-based epoxy monomer. The specific reaction example is as follows:
[0031] (1) Protocatechuic aldehyde, erythritol, catalyst p-toluenesulfonic acid monohydrate (p-TSA.H2O), solvent N,N-dimethylformamide and dehydrating agent petroleum ether were placed in a reactor equipped with a water separator and a spherical condenser; under nitrogen protection, the mixture was reacted at 70-100°C for 12-24 hours, the product was cooled, and then poured into deionized water to precipitate, which was filtered and washed with water, and finally dried in a vacuum oven to obtain a tetrahydroxy monomer product (VP).
[0032] (2) The obtained tetrahydroxy monomer VP, epichlorohydrin (ECH) and tetrabutylammonium bromide are added to a reactor and reacted at 40-80°C for 1-12 hours. Then, sodium hydroxide solution is added dropwise at room temperature. After the addition is completed, the reaction is continued for 2-4 hours. The crude product is then filtered to obtain a crude product. Dichloromethane and water are added to collect the organic layer. The obtained organic layer is dried over anhydrous magnesium sulfate, and the solvent and possible ECH are removed by rotary evaporation. Finally, the target epoxy monomer (DGEVP) is obtained by drying.
[0033] In the above technical solution, the molar ratio of protocatechuic aldehyde, erythritol, p-toluenesulfonic acid monohydrate, N,N-dimethylformamide and petroleum ether is 200: (100-120): (4-6): 300-500: 2000-4000; the molar ratio of tetrahydroxy monomer VP, epichlorohydrin (ECH) and tetrabutylammonium bromide is 1: (40-250): (1-3).
[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be further clearly and completely described below through specific embodiments and accompanying drawings. Obviously, the described embodiments are part of embodiments of the present invention, rather than all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. In addition, unless otherwise indicated, all scientific and technical terms used in the present invention have the same meanings as those commonly understood by those in the technical field to which the present invention belongs. The experimental methods for which specific conditions are not specified in the following examples are generally based on conventional conditions or the conditions recommended by the manufacturer. The raw materials of the present invention and the specific preparation operations and performance tests are conventional techniques.
[0035] Synthesis Example Preparation of Tetraepoxy Monomer
[0036] (1) Protocatechuic aldehyde (PCA, 0.2 mol), erythritol (0.1 mol), catalyst p-toluenesulfonic acid monohydrate (p-TSA·H2O, 0.0042 mmol), solvent N,N-dimethylformamide (0.39 mol) and dehydrating agent petroleum ether (3.3 mol) were placed in a reactor equipped with a water separator and a spherical condenser. Under nitrogen protection, the mixture was reacted at 90°C for 24 hours. The product was cooled and then poured into deionized water to precipitate. The precipitate was filtered and washed with deionized water five times, and finally dried in a vacuum oven for 6 hours to obtain the tetrahydroxy monomer product (VP). Figure 1 (a) shows the schematic diagram of the synthesis of VP.
[0037] (2) The obtained tetrahydroxy monomer VP (10 g, 0.0026 mol), epichlorohydrin (ECH) (51 g, 0.551 mol), and tetrabutylammonium bromide (1 g, 0.0031 mol) were added to the reactor in sequence. After reacting at 80°C for 3 hours, a sodium hydroxide aqueous solution (40 wt%, 11 g) was added dropwise at room temperature over 5 minutes. The reaction was continued for 3 hours. The crude product was filtered to obtain a crude product. Dichloromethane and water were added, and the organic layer was collected. The organic layer was dried over anhydrous magnesium sulfate, and the solvent was removed by rotary evaporation. Finally, the target epoxy monomer (DGEVP) was dried in vacuo at 90°C for 5 hours. Figure 1 (b) shows a schematic diagram of the synthesis of DGEVP.
[0038] Figure 2 is the infrared spectra (FTIR) of PCA, erythritol, VP and DGEVP; the nuclear magnetic resonance spectrum of VP ( 1 H NMR) and carbon NMR spectroscopy ( 13 C NMR) diagram of DGEVP 1 H NMR and 13 C NMR spectrum; liquid chromatography-mass spectrometry (LC-MS) spectrum of VP and DGEVP. VE is obtained by condensation of PCA and erythritol, and DGEVP is obtained by reaction of the hydroxyl groups on VE with ECH. As shown in Figure 1(a), the FTIR spectrum of PCA shows that the hydroxyl groups (approximately 3190-3300 cm -1 ), CH in the benzene ring (3047 cm -1 ), CH in aldehyde group (-CHO) (2890-2725 cm -1 ), -CHO (1750 cm -1 ), and aromatic rings (1650, 1600, and 1530 cm -1 ) characteristic absorption peak. The FTIR spectrum of erythritol shows -OH (3100-3500 cm -1 ), CH (2965 and 2908 cm -1 , 1406 cm -1 ), primary and secondary alcohols (1080 and 1050 cm -1 )CO(972 cm -1 ) characteristic absorption peak. Compared with the spectra of PCA and erythritol, the FTIR spectrum of VP shows new changes. -1 、1280 cm -1 、1160 cm -1 and 1107cm -1 There are new strong characteristic peaks at 910 cm, which are due to the formation of -COC-, -CO-, and COC. In addition, there is no characteristic peak of -CHO in the FTIR spectrum of VP. When VP reacts with ECH, the peak at 910 cm -1 There is a characteristic peak at 3100-3500 cm -1 No obvious -OH peak appeared, which means that the bio-based tetrafunctional epoxy monomer DGEVP was successfully synthesized.
[0039] To further determine the chemical structures of VP and DGEVP, 1 H NMR and 13 C NMR characterization of the product structure, in VP 1In the H NMR spectrum, δ=8.97 ppm corresponds to the hydrogen protons in the OH group linked to the benzene ring; δ=6.83, 6.76, and 6.58 ppm correspond to the hydrogen protons in the benzene ring; δ=5.58 ppm corresponds to the hydrogen protons in -O-CH-O-; δ=4.18 ppm and 3.90-3.67 ppm correspond to the hydrogen protons in -CH-O and -C-CH2-. 13 The chemical shifts and peak numbers in C NMR also correspond to the carbon atoms in VP. In addition, the LC-MS spectrum shows that the molar mass of VP is 385.0911 g / mol, which is consistent with the theoretical value of 385.0900 g / mol. This means that VP was successfully synthesized. In the 1H NMR spectrum of DGEVP, the hydrogen protons in the epoxy group are at δ=3.42-3.31ppm, 2.89ppm and 2.76ppm, the hydrogen protons in -O-CH-CH2- are at δ=3.76-3.64ppm, the hydrogen protons in -CH2-O-CH2-C- are at δ=3.88-3.79ppm, the hydrogen protons in the aldehyde structure are at δ=5.58ppm, and the hydrogen protons in the benzene ring are at δ=7.10, 7.00 and 6.94ppm. 1 Compared with the H NMR spectrum of DGEVP 1 The H NMR spectrum does not show the proton peak of the phenolic hydroxyl group at 8.97 ppm. 13 The chemical shifts and peak numbers in C NMR also corresponded closely to the carbon atoms in VP, while the LC-MS spectrum showed that the molar mass of DGEVP was 609.1948 g / mol, consistent with the theoretical value. This indicates that DGEVP was successfully synthesized.
[0040] Example 1: Medium-temperature curing epoxy resin system and high-performance degradable multifunctional epoxy resin
[0041] A mixture of 100g DGEVP and 1.25g zinc acetylacetonate (ZAA) was heated and stirred at 140°C until it became a transparent liquid. Then, 33g glutaric anhydride (GA) was added at 80°C and stirred for 20 minutes to produce a uniform prepolymer-cured epoxy resin system. The prepolymer was then poured into a preheated mold and placed in a vacuum oven at 80°C to remove air bubbles. The product was then cured using a temperature program of 80°C / 2h followed by 100°C / 2h to obtain the final product.
[0042] Comparative Example 1
[0043] A mixture of 100g of bisphenol A epoxy resin (E51) and 1.25g of zinc acetylacetonate (ZAA) was heated and stirred at 140°C until a transparent liquid formed. 30g of glutaric anhydride (GA) was then added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold and placed in a vacuum oven at 80°C to remove air bubbles. The product was then cured using a temperature program of 80°C / 2h followed by 100°C / 2h to obtain the resulting product.
[0044] Comparative Example 1-1
[0045] A mixture of 100g of bisphenol A epoxy resin (E51) and 1.25g of zinc acetylacetonate (ZAA) was heated and stirred at 140°C until it became a transparent liquid. Then, 30g of glutaric anhydride (GA) was added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold and placed in a vacuum oven at 80°C to remove air bubbles. The product was then cured according to a temperature program of 80°C / 2h, 100°C / 2h, 140°C / 2h, and 180°C / 2h to obtain the cured product.
[0046] Table 1 shows the mechanical properties data of the cured samples of Example 1, Comparative Example 1-1 and Comparative Example 1-2, the activation energy of the resin system reaction (Ea), the conversion rate of epoxy groups in the cured resin system (α) and the glass transition temperature (T g As can be seen from Table 1, the mechanical properties and thermal properties of the resin system prepared by the biomass epoxy resin synthesized by the present invention at medium temperature are superior to those of the traditional commercial bisphenol A epoxy resin cured at medium and high temperatures. The activation energy E of the resin system reaction is a The resin system has a high epoxy conversion rate even after medium temperature curing. Moreover, the present invention has a significantly higher T g , overcomes the existing biomass epoxy resin T g In particular, DGEVP cured products not only have mild acid degradation behavior, but also have good crack self-healing ability at 200°C (Figure 3). g At +20°C, it exhibits excellent shape deformation and recovery capabilities (Figure 4). Conventional bisphenol A epoxy resins cured with anhydride exhibit no acidic degradation behavior, while DGEVP cured products are highly susceptible to degradation under acidic conditions.
[0047]
[0048] a,b,c : The flexural strength, impact strength and tensile strength tests were conducted in accordance with the resin casting performance test standard GB / T 2567-2008.
[0049] d :The apparent activation energy was calculated using the Kissinger extreme value method.
[0050] e : The conversion rate of epoxy groups was calculated based on the infrared spectrum of the samples using the internal standard method.
[0051] f : Use DMA to obtain T g .
[0052] g : Soak 50 mg of sample in 10 ml of hydrochloric acid solution and observe the degradation time.
[0053] Existing technology synthesizes a semi-biobased PH-ODA using protocatechuic aldehyde and 4,4-diaminodiphenyl ether (ODA) as raw materials. A two-step process synthesizes a semi-biobased flame-retardant epoxy prepolymer using PH-ODA, epichlorohydrin, and NaOH as raw materials. The epoxy prepolymer PH-ODA-EP is cured with the curing agent DDM to produce the epoxy cured product PH-ODA-EP / DDM. Compared to DGEBA / DDM, the PH-ODA-EP / DDM curing system exhibits a higher Ea value. However, the reactivity of the PH-ODA-EP / DDM curing system is lower than that of the DGEBA / DDM curing system, requiring a curing temperature of 190°C. Furthermore, the system contains a portion of petroleum-based ODA, which does not fully utilize bio-based raw materials. Compared to previously reported curing systems containing diepoxy monomers with helical acetal, monocyclic acetal, and bicyclic acetal structures, the epoxy resin / anhydride curing system of the present invention exhibits excellent self-healing behavior, a low curing temperature, and reduced production energy consumption.
[0054] The curing temperature of the resin system of the present invention is low. The curing temperature of the existing acetal epoxy / anhydride system is relatively high. FIG5 shows the DSC curves of the resin systems in Example 1 and Example 2. Obviously, the reaction temperature of DGEVP / GA / ZAA is lower than that of E51 / GA / ZAA.
[0055] Example 2
[0056] A mixture of 100g of DGEVP and 2.5g of zinc acetylacetonate (ZAA) was heated and stirred at 140°C until it became a transparent liquid. Then, 33g of glutaric anhydride (GA) was added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold, de-bubbled in a vacuum oven, and cured according to a temperature program of 80°C / 2h followed by 100°C / 2h to obtain the cured product.
[0057] Comparative Example 2
[0058] A mixture of 100g of E51 and 2.5g of zinc acetylacetonate (ZAA) was heated and stirred at 140°C until it became a transparent liquid. 30g of glutaric anhydride (GA) was then added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold, debubbled in a vacuum oven, and cured according to a temperature program of 80°C / 2h, 100°C / 2h, 140°C / 2h, and 180°C / 2h to obtain the cured product.
[0059] Table 2 is the mechanical properties data of the cured samples of Example 2 and Comparative Example 2, the E a , epoxy conversion rate α and T g As can be seen from Table 2, the mechanical properties and thermal properties of the resin system prepared by the biomass epoxy resin synthesized in the present invention at medium temperature are superior to those of the traditional commercial bisphenol A epoxy resin cured at medium and high temperatures. The activation energy of the resin system reaction E a The resin system has a high epoxy conversion rate even after medium-temperature curing. DGEVP cured products are easily degraded under acidic conditions (Figure 6(a)). The degradation products of the cured product sample in 0.1M HCl solution (acetone / water = 9:1, v:v) at 50°C were monitored using real-time nuclear magnetic resonance (NMR), see Figure 6(b). In addition, DGEVP cured products have good crack self-healing ability at 200°C (Figure 7). g Above the temperature, it has good shape deformation and recovery capabilities (Figure 8).
[0060]
[0061] Example 3
[0062] A mixture of 100g DGEVP and 5.0g zirconium acetylacetonate (AAZ) was heated and stirred at 200°C until it became a transparent liquid. Then, 55g of methylhexahydrophthalic anhydride (MeHHPA) was added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold, de-bubbled in a vacuum oven, and cured according to a temperature program of 80°C / 2h, 100°C / 2h, and 120°C / 4h.
[0063] Comparative Example 3
[0064] A mixture of 100g of E51 and 5.0g of zirconium acetylacetonate (AAZ) was heated and stirred at 200°C until it became a transparent liquid. Then, 45g of methylhexahydrophthalic anhydride (MeHHPA) was added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold, debubbled in a vacuum oven, and cured according to a temperature program of 80°C / 2h, 100°C / 2h, 140°C / 2h, and 180°C / 2h.
[0065] Table 3 shows the mechanical properties data of the cured samples of Example 3 and Comparative Example 3, Ea of the resin system, conversion rate α of the epoxy group of the cured resin system, and glass transition temperature T g As can be seen from Table 3, the mechanical properties and thermal properties of the resin system prepared by the biomass epoxy resin synthesized in the present invention at medium temperature are superior to those of the traditional commercial bisphenol A epoxy resin cured at medium and high temperatures. The resin system reaction activation energy Ea is low. Even after medium temperature curing treatment, the resin system has a high epoxy group conversion rate, and its cured product is easily degraded under acidic conditions. In addition, the DGEVP cured product has good crack self-repairing ability at 200°C (Figure 9). The DGEVP cured product at T g Above the temperature, it has good shape deformation and recovery capabilities (Figure 10).
[0066]
[0067] Example 4
[0068] A mixture of 60g of DGEVP and 0.5g of zinc acetylacetonate (ZAA) was heated and stirred at 140°C until it became a transparent liquid. Then, 22g of citraconic anhydride was added at 80°C and stirred for 20 minutes to obtain a uniform prepolymer. The prepolymer was then poured into a preheated mold, de-bubbled in a vacuum oven, and cured according to a temperature program of 80°C / 2h, 100°C / 2h, and 120°C / 2h to obtain the product.
[0069] Comparative Example 4
[0070] A mixture of 60g of E51 and 0.5g of zinc acetylacetonate (ZAA) was heated and stirred at 140°C until it became a transparent liquid. Then, 18g of citraconic anhydride was added at 80°C and stirred for 20 minutes to obtain a homogeneous prepolymer. The prepolymer was then poured into a preheated mold, debubbled in a vacuum oven, and cured according to a temperature program of 80°C / 2h, 100°C / 2h, 140°C / 2h, and 180°C / 2h to obtain the cured product.
[0071] Table 4 shows the mechanical properties data, resin system reaction activation energy Ea, conversion rate α of epoxy groups in the cured resin system, and glass transition temperature Tg of the cured samples of Example 4 and Comparative Example 4. As can be seen from Table 4, the mechanical and thermal properties of the resin system prepared at medium temperature using the biomass epoxy resin synthesized in the present invention are superior to those of the traditional commercial bisphenol A epoxy resin cured at medium and high temperatures. The resin system reaction activation energy Ea is low, and even after medium temperature curing, the resin system has a high epoxy group conversion rate. Its cured product is very easy to degrade under acidic conditions. In addition, the DGEVP cured product has good crack self-repairing ability at 200°C (Figure 11). The DGEVP cured product has good crack self-repairing ability at T g Above the temperature, it has good shape deformation and recovery capabilities (Figure 12).
[0072]
Claims
1. A bio-based epoxy monomer, characterized in that The chemical formula of the bio-based epoxy monomer is as follows: 。 2. The method for preparing the bio-based epoxy monomer according to claim 1, characterized in that: The bio-based epoxy monomer is synthesized using protocatechuic aldehyde, erythritol and epichlorohydrin as raw materials.
3. The method for preparing the bio-based epoxy monomer according to claim 2, characterized in that: Protocatechuic aldehyde and erythritol are used as raw materials to prepare a tetrahydroxy monomer; and then the tetrahydroxy monomer and epichlorohydrin are used as raw materials to prepare the bio-based epoxy monomer.
4. The method for preparing a bio-based epoxy monomer according to claim 3, characterized in that: Protocatechuic aldehyde and erythritol are used as raw materials, and a tetrahydroxy monomer is prepared by reaction in the presence of a catalyst and in a solvent; and the bio-based epoxy monomer is prepared by reaction in the presence of an organic ammonium salt and in an alkaline environment using a tetrahydroxy monomer and epichlorohydrin as raw materials.
5. The method for preparing a bio-based epoxy monomer according to claim 4, characterized in that: The catalyst is p-toluenesulfonic acid monohydrate; the molar ratio of protocatechuic aldehyde, erythritol and p-toluenesulfonic acid monohydrate is 200: (100-120): (4-6); the organic ammonium salt is tetrabutylammonium bromide; sodium hydroxide solution is added to form an alkaline environment; the molar ratio of tetrahydroxy monomer, epichlorohydrin and tetrabutylammonium bromide is 1: (40-250): (1-3).
6. A medium temperature curing epoxy resin system, characterized in that: It comprises the bio-based epoxy monomer, anhydride curing agent and a catalyst as described in claim 1.
7. The method for preparing the medium temperature curing epoxy resin system according to claim 6, characterized in that: The bio-based epoxy monomer described in claim 1 and the catalyst are melted and mixed uniformly, and then an anhydride compound is added at 60-80° C. to perform prepolymerization to obtain a medium-temperature curing epoxy resin system.
8. The method for preparing the medium temperature curing epoxy resin system according to claim 7, characterized in that: The acid anhydride compound is a low melting point petroleum-based acid anhydride, a bio-based acid anhydride or a mixture thereof; and the catalyst is an organic metal complex.
9. A high-performance biodegradable multifunctional epoxy resin obtained by medium-temperature curing the medium-temperature curing epoxy resin system according to claim 6.
10. Use of the bio-based epoxy monomer according to claim 1, the medium-temperature curing epoxy resin system according to claim 6, or the high-performance degradable multifunctional epoxy resin according to claim 9 in the preparation of high-performance degradable multifunctional epoxy materials.
Citation Information
Patent Citations
Epoxy monomer and preparation method thereof and epoxy resin
CN109320521A
Epoxy resin, epoxy resin composition including same, and cured product using said epoxy resin composition
CN110945049A
Rigid bio-based diol monomer with cyclic acetal structure and preparation method and application thereof
CN113620968A
Aldehyde group-containing epoxy resin prepolymer as well as preparation method and application thereof
CN115466372A
Cited By
Epoxy resin daub and preparation method thereof
CN119351022A
Three-functionality bio-based epoxy resin monomer, bio-based epoxy resin, preparation method and remolding method
CN120081804A
A trifunctional bio-based epoxy resin monomer, bio-based epoxy resin, and methods of preparation and rework
CN120081804B
Epoxy resin composite material with adjustable degradation performance and preparation method thereof