Double-air-pressure compounding method for tubular fabric
The molding process of textile composite materials is simplified through the double-air pressure compounding method, which solves the problems of high equipment cost and difficult operation in the existing technology, and achieves high roundness and good mechanical properties of the tubular fabric.
Patent Information
- Application Number
- PCT/CN2023/107131
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-07-13
- Publication Date
- 2024-10-03
AI Technical Summary
Existing molding methods for textile composite materials, such as resin transfer molding and vacuum-assisted molding equipment, are costly and difficult to operate, and are difficult to demould after composite molding, resulting in insufficient sample roundness.
The flexible tubular fabric is composited in one go using a double air pressure lamination method. Air pressure and resin are filled into the outer and inner membranes, combined with a heating device to melt the outer and inner membranes, wrap the flexible tubular fabric, and use vacuum to make the outer membrane and inner membrane melt. Resin immersion simplifies the process and reduces tube turning steps.
A tubular fabric composite material with simple operation, good sample roundness, good interface bonding performance and mechanical properties, and better safety performance is realized.
Smart Images

Figure CN2023107131_03102024_PF_FP_ABST
Abstract
Description
Double air pressure composite method for tubular fabric
[0001] Related applications
[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on March 29, 2023, with application number 202310321210.X and application name “A dual-air pressure composite method for tubular fabrics”, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present disclosure relates to the field of textile technology, and in particular to a dual-air pressure composite method for tubular fabrics. Background Art
[0004] Textile composites primarily refer to novel materials manufactured through a composite process using high-performance fibers as reinforcement and resin as a matrix. They exhibit advantages such as high specific strength, high specific modulus, and enhanced design flexibility. In recent years, tubular textile composites have become increasingly popular, finding widespread application in the production of various pipes, pipe shells, bushings, ultra-high-temperature insulated pipes, and various structural support applications. While my country's development of tubular textile composite production technology is relatively recent, some developed Western countries have already achieved relatively mature production processes. Composite molding methods include hand lay-up, compression molding, vacuum-assisted molding, winding, pultrusion, injection molding, and resin transfer molding.
[0005] Currently, the main molding methods used for textile composite materials are resin transfer molding and vacuum-assisted molding. However, vacuum-assisted resin transfer molding requires relatively complex equipment, which is costly and requires high investment from manufacturers. It also requires workers to master advanced operating techniques and experience, making it difficult to operate and requiring professional training and assessment. It also requires specific formulations and testing to determine the optimal ratio. Without experience, a certain amount of material will be wasted. Furthermore, these two methods are difficult to demold after composite molding, which is not conducive to forming a complete model and resulting in insufficient roundness of the sample. Some scholars have studied a two-step composite process, in which the inner membrane is first composited, and then the flexible composite tubular fabric is flipped over. At this point, the inside and outside are relatively swapped, and the same operation is then repeated to complete the composite process. The flexible tubular fabric is composited, but the process requires turning the tube over, which is relatively cumbersome.
[0006] Summary of the Invention
[0007] The purpose of the present invention is to address the shortcomings of the existing technology and propose a dual-air pressure composite method for tubular fabrics. Based on the dual-air pressure method, the flexible tubular fabric is composited in one go, which reduces the steps of turning the tube, saves time and cost, simplifies the process, and is easy to demold, has good sample roundness, and has better safety performance in use.
[0008] In order to achieve the above objectives, the present disclosure adopts the following technical solutions:
[0009] A dual-air pressure composite method for tubular fabrics, comprising the following steps:
[0010] S1: placing the outer membrane on a plane, and injecting a first air pressure into the outer membrane from the first opening, so that the outer membrane is propped up;
[0011] S2: inserting the inner membrane into the flexible tubular fabric first, and inserting the flexible tubular fabric into the outer membrane from the first opening;
[0012] S3: a second air pressure is injected into the inner membrane from the second opening, the inner membrane is propped up, and the outer membrane and the inner membrane are tightly wrapped around the surface of the flexible tubular fabric;
[0013] S4: Remove the first air pressure and continue to input the second air pressure;
[0014] S5: heating the entire model outside the outer membrane using a heating device until the inner layer of the outer membrane and the outer layer of the inner membrane are melted and the flexible tubular fabric is infiltrated;
[0015] S6: Filling resin from the first opening and simultaneously drawing vacuum from the third opening, so that the resin is impregnated into the interior of the flexible tubular fabric.
[0016] Optionally, the outer film is a double-layer composite flexible film, the outer film includes an outer film inner layer and an outer film outer layer, and the melting point of the outer film inner layer is lower than the melting point of the outer film outer layer.
[0017] Optionally, the inner film is a double-layer composite flexible film, the inner film comprising an inner film inner layer and an inner film outer layer, and the melting point of the inner film outer layer is lower than the melting point of the inner film inner layer.
[0018] Optionally, the inner layer of the outer film is a thermoplastic material, the inner layer of the outer film is polyethylene, polypropylene or polyester, and the outer layer of the outer film is a thermoplastic material or a thermosetting material.
[0019] Optionally, the outer layer of the inner film is a thermoplastic material, the outer layer of the inner film is polyethylene, polypropylene or polyester, and the inner layer of the inner film is a thermoplastic material or a thermosetting material.
[0020] Optionally, the thickness of the inner layer of the adventitia and the outer layer of the intima are both 1-5 mm, and the thickness of the outer layer of the adventitia and the inner layer of the intima are both 1-2 mm.
[0021] Optionally, in step S1, the first air pressure is greater than a standard atmospheric pressure, and the first air pressure is 0.1-1 MPa; in step S3, the second air pressure is greater than the first air pressure, and the pressure difference between the second air pressure and the first air pressure is 0.1-0.5 MPa.
[0022] Optionally, in steps S1, S3, and S6, the first opening, the second opening, and the third opening can be opened or closed, and are in a sealed state after closing. The size of the opening can be 1 / 3 or 1 / 4 of the inner membrane diameter.
[0023] Optionally, in step S5, the heating temperature of the heating device is 130-150° C., the heating device is located outside the outer membrane, and the heating device moves at a uniform speed along the outer membrane so that the entire model is heated evenly.
[0024] Optionally, the heating temperature of the heating device is higher than the melting point of the inner layer of the outer membrane and the outer layer of the inner membrane, and the heating temperature of the heating device is lower than the melting point of the outer layer of the outer membrane and the inner layer of the inner membrane.
[0025] Among them, in step S6, the resin has good fluidity at room temperature and can be cured at room temperature or cured in the air; choosing room temperature curing can improve the overall mechanical properties, and choosing air-curing resin can make it have self-healing properties. Both types of resins will provide better safety performance in use.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention adopts a dual-air pressure compounding method to prepare a flexible tubular fabric composite material, which is simple to operate, and the surface of the tubular fabric will not be uneven. After compounding, the tubular fabric composite material has better roundness, and is endowed with good interface bonding performance and mechanical properties, while having better safety performance in use.
[0028] 2. The present invention is based on a double air pressure method, which completes the one-time compounding of flexible tubular fabrics, reduces the steps of turning the tube, saves time and cost, simplifies the process, and is easy to demould and has good sample roundness. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] FIG1 is a schematic structural diagram of a flexible tubular fabric composite material in the present disclosure;
[0030] FIG2 is a schematic diagram of the structure of the outer membrane in the present disclosure;
[0031] FIG3 is a schematic diagram of the structure of the inner membrane in the present disclosure;
[0032] FIG4 is a perspective schematic diagram of a flexible tubular fabric composite material according to the present disclosure. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present disclosure will be described clearly and completely below in conjunction with the accompanying drawings so that those skilled in the art can better understand the advantages and features of the present disclosure and thus more clearly define the scope of protection of the present disclosure. The embodiments described in the present disclosure are only a part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by those of ordinary skill in the art without making any creative work are within the scope of protection of the present disclosure.
[0034] Example 1:
[0035] 1-4 , a dual-air pressure composite method for a tubular fabric is shown, and the specific steps are as follows:
[0036] S1: Take an outer film 6 and an inner film 4 made of a double-layer composite film material, wherein the outer film inner layer 9 is polyethylene, the outer film outer layer 8 is polyester, the inner film outer layer 10 is polyethylene, and the inner film inner layer 11 is polyester. The thickness of the outer film inner layer 9 and the inner film outer layer 10 are both 3 mm, and the thickness of the outer film outer layer 8 and the inner film inner layer 11 are both 1 mm;
[0037] S2: Cut the outer membrane 6 and the inner membrane 4 into closed hollow tubes of appropriate size;
[0038] S3: placing the outer membrane 6 on a flat surface and filling the outer membrane 6 with the first air pressure 2;
[0039] S4: first insert the inner membrane 4 into the flexible tubular fabric 5, and then insert the flexible tubular fabric 5 into the outer membrane 6 from the first opening 1;
[0040] S5: Inflate the inner membrane 4 with the second air pressure 3, so that the inner membrane 4 is propped up. At this time, the outer membrane 6 and the inner membrane 4 are tightly wrapped around the surface of the flexible tubular fabric 5;
[0041] S6: Turn off the first air pressure 2 and continue to input the second air pressure 3;
[0042] S7: Start the heating device 7 so that the heating device 7 moves at a constant speed outside the outer membrane 6. The heating temperature of the heating device 7 is 130-150°C.
[0043] S8: Fill the fabric with resin from the first opening 1 and simultaneously draw vacuum from the third opening 13. The resin is preferably a modified low-viscosity epoxy resin that can be cured at room temperature to improve the overall mechanical properties of the composite pipe, thereby having better safety performance in use.
[0044] Example 2:
[0045] 1-4 , a dual-air pressure composite method for a tubular fabric is shown, and the specific steps are as follows:
[0046] S1: Take an outer film 6 and an inner film 4 made of a double-layer composite film material, wherein the outer film inner layer 9 is polyethylene, the outer film outer layer 8 is polyester, the inner film outer layer 10 is polyethylene, and the inner film inner layer 11 is polypropylene. The thickness of the outer film inner layer 9 and the inner film outer layer 10 are both 3 mm, and the thickness of the outer film outer layer 8 and the inner film inner layer 11 are both 1 mm;
[0047] S2: Cut the outer membrane 6 and the inner membrane 4 into closed hollow tubes of appropriate size;
[0048] S3: placing the outer membrane 6 on a flat surface and filling the outer membrane 6 with the first air pressure 2;
[0049] S4: first insert the inner membrane 4 into the flexible tubular fabric 5, and then insert the flexible tubular fabric 5 into the outer membrane 6 from the first opening 1;
[0050] S5: Inflate the inner membrane 4 with the second air pressure 3, so that the inner membrane 4 is propped up. At this time, the outer membrane 6 and the inner membrane 4 are tightly wrapped around the surface of the flexible tubular fabric 5;
[0051] S6: Turn off the first air pressure 2 and continue to input the second air pressure 3;
[0052] S7: Start the heating device 7 so that the heating device 7 moves at a constant speed outside the outer film 6, and the heating temperature of the heating device 7 is set to 130-150° C.;
[0053] S8: Fill the fabric with resin from the first opening 1 and simultaneously draw vacuum from the third opening 13. The resin is preferably α-ethyl cyanoacrylate, which can be cured when exposed to air, so that the composite tube has self-healing properties, thereby having better safety performance.
[0054] Example 3:
[0055] 1-4 , a dual-air pressure composite method for a tubular fabric is shown, and the specific steps are as follows:
[0056] S1: Take an outer film 6 and an inner film 4 made of a double-layer composite film material, wherein the outer film inner layer 9 is polyethylene, the outer film outer layer 8 is polypropylene, the inner film outer layer 10 is polyethylene, and the inner film inner layer 11 is polypropylene. The thickness of the outer film inner layer 9 and the inner film outer layer 10 are both 3 mm, and the thickness of the outer film outer layer 8 and the inner film inner layer 11 are both 1 mm;
[0057] S2: Cut the outer membrane 6 and the inner membrane 4 into closed hollow tubes of appropriate size;
[0058] S3: placing the outer membrane 6 on a flat surface and filling the outer membrane 6 with the first air pressure 2;
[0059] S4: first insert the inner membrane 4 into the flexible tubular fabric 5, and then insert the flexible tubular fabric 5 into the outer membrane 6 from the first opening 1;
[0060] S5: Inflate the inner membrane 4 with the second air pressure 3, so that the inner membrane 4 is propped up. At this time, the outer membrane 6 and the inner membrane 4 are tightly wrapped around the surface of the flexible tubular fabric 5;
[0061] S6: Turn off the first air pressure 2 and continue to input the second air pressure 3;
[0062] S7: Start the heating device 7 so that the heating device 7 moves at a constant speed outside the outer film 6, and the heating temperature of the heating device 7 is set to 130-150° C.;
[0063] S8: Fill the fabric with resin from the first opening 1 and simultaneously draw vacuum from the third opening 13. Modified alkyd resin is preferably used as the resin, which can be cured when exposed to air, so that the composite pipe has self-healing properties, thereby having better safety performance.
[0064] In summary, the present invention adopts a dual-air pressure compounding method to prepare a flexible tubular fabric composite material, which is simple to operate, and there will be no unevenness on the surface of the tubular fabric. After compounding, the tubular fabric composite material has better roundness, and is endowed with good interface bonding performance and mechanical properties, while having better safety performance in use.
[0065] The descriptions and practices disclosed in this disclosure are easy to understand and comprehend for those skilled in the art, and modifications and refinements can be made without departing from the principles of this disclosure. Therefore, modifications or improvements made without departing from the spirit of this disclosure should also be considered within the scope of protection of this disclosure.
Claims
1. A dual-air pressure composite method for a tubular fabric, the specific steps are as follows: S1: placing the outer film (6) on a plane, and injecting the first air pressure (2) into the outer film (6) from the first opening (1), so that the outer film (6) is propped up; S2: insert the inner membrane (4) into the flexible tubular fabric (5) first, and insert the flexible tubular fabric (5) into the outer membrane (6) from the first opening (1); S3: the second air pressure (3) is charged into the inner membrane (4) from the second opening (12), and the inner membrane (4) is propped up. At this time, the outer membrane (6) and the inner membrane (4) are tightly wrapped around the surface of the flexible tubular fabric (5); S4: the first air pressure (2) is removed, and the second air pressure (3) is continuously input; S5: using a heating device (7) to heat the entire mold outside the outer film (6) until the inner layer of the outer film (9) and the outer layer of the inner film (10) melt and infiltrate the flexible tubular fabric (5); S6: Resin is filled in from the first opening (1) and vacuum is simultaneously drawn from the third opening (13) so that the resin is infiltrated into the flexible tubular fabric.
2. A double air pressure composite method for a tubular fabric according to claim 1, wherein: The outer film (6) is a double-layer composite flexible film, comprising an outer film inner layer (9) and an outer film outer layer (8), and the melting point of the outer film inner layer (9) is lower than the melting point of the outer film outer layer (8).
3. A double air pressure composite method for a tubular fabric according to claim 2, wherein: The inner film (4) is a double-layer composite flexible film, comprising an inner film inner layer (11) and an inner film outer layer (10), and the melting point of the inner film outer layer (10) is lower than the melting point of the inner film inner layer (11).
4. A double air pressure composite method for a tubular fabric according to claim 3, wherein: The outer film inner layer (9) is a thermoplastic material, the outer film inner layer (9) is polyethylene, polypropylene or polyester, and the outer film outer layer (8) is a thermoplastic material or a thermosetting material.
5. A double air pressure composite method for a tubular fabric according to claim 4, wherein: The inner film outer layer (10) is a thermoplastic material, the inner film outer layer (10) is polyethylene, polypropylene or polyester, and the inner film inner layer (11) is a thermoplastic material or a thermosetting material.
6. A double air pressure composite method for a tubular fabric according to claim 4, wherein: The thickness of the outer membrane inner layer (9) and the inner membrane outer layer (10) are both 1-5 mm, and the thickness of the outer membrane outer layer (8) and the inner membrane inner layer (11) are both 1-2 mm.
7. A double air pressure composite method for a tubular fabric according to claim 1, wherein: In step S1, the first air pressure (2) is greater than a standard atmospheric pressure, and the first air pressure (2) is 0.1-1 MPa; in step S3, the second air pressure (3) is greater than the first air pressure (2), and the pressure difference between the second air pressure (3) and the first air pressure (2) is 0.1-0.5 MPa.
8. A double air pressure composite method for a tubular fabric according to claim 1, wherein: In the steps S1, S3 and S6, the first opening (1), the second opening (12) and the third opening (13) can be opened or closed, and are in a sealed state after being closed.
9. A double air pressure composite method for a tubular fabric according to claim 1, wherein: In step S5, the heating temperature of the heating device (7) is 130-150°C, the heating device (7) is located outside the outer film (6), and the heating device (7) moves at a uniform speed along the outer film (6) so that the entire model is heated evenly.
10. A double air pressure composite method for a tubular fabric according to claim 9, wherein: The heating temperature of the heating device (7) is higher than the melting points of the outer film inner layer (9) and the inner film outer layer (10), and the heating temperature of the heating device (7) is lower than the melting points of the outer film outer layer (8) and the inner film inner layer (11).
Citation Information
Patent Citations
Forming device and forming method for tubular three-dimensional braided composite product
CN106313584A
Double-layer composite once-formed safety air bag and manufacturing method thereof
CN113650379A
Double-layer internally-bonded flexible freight bag processing technology
CN114083818A
Pressure-maintaining safety airbag compound fabric forming method and compound fabric
CN114905771A
Light flexible rubber tube
CN86205867U