Method for preparing sintered brick from lateritic nickel ore high-pressure acid leaching smelting tailings, and sintered brick
By mixing the high-pressure acid leaching smelting tailings of laterite nickel ore with additives in proportion and aging, drying and sintering, the sintered bricks are made, which solves the problem of tailings treatment, improves resource utilization and the strength of the bricks, and reduces the Reduce production costs and space usage.
Patent Information
- Application Number
- PCT/CN2023/117013
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-09-05
- Publication Date
- 2024-10-03
AI Technical Summary
Existing technology is difficult to effectively deal with the high-pressure acid leaching smelting tailings of laterite nickel ore, leading to problems such as low resource utilization, high construction investment, large land area, and risk of marine pollution.
The high-pressure acid leaching smelting tailings of laterite nickel ore after filtering are mixed with additives in a certain proportion, and then aged, dried and sintered to make sintered bricks, thereby realizing resource utilization of the tailings.
It improves the resource utilization rate of laterite nickel ore, reduces tailings storage costs and risks, reduces land resource occupation and production and operation costs, and produces sintered bricks with high strength and suitable for mass production.
Smart Images

Figure CN2023117013_03102024_PF_FP_ABST
Abstract
Description
Method for making sintered bricks using tailings from high-pressure acid leaching of laterite nickel ore and sintered bricks Technical Field
[0001] The present invention relates to the technical field of solid waste resource treatment, and in particular to a method for manufacturing sintered bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore, and the sintered bricks. Background Art
[0002] Laterite nickel ore is formed by the weathering, leaching, alteration, and enrichment of nickel-bearing rocks. It is primarily a loose, clay-like ore composed of hydrous oxides of iron, aluminum, and silicon. Low-grade laterite nickel ore is currently the primary source of nickel production worldwide. Nickel production from laterite nickel ore can be achieved through two processes: pyrometallurgical and hydrometallurgical. The primary hydrometallurgical process for processing laterite nickel ore is high-pressure acid leaching. High-pressure acid leaching is suitable for processing low-magnesium limonite laterite nickel ore, offering high metal recovery and high processing capacity, but it also produces significant amounts of tailings.
[0003] Currently, the common practices for tailings disposal include deep-sea landfill, wet stacking in tailings ponds, or dry stacking in tailings ponds. Deep-sea landfill carries the risk of marine pollution, while tailings pond storage has disadvantages such as high cost and large land occupation. Therefore, it is necessary to find an effective method for treating tailings from high-pressure acid leaching of laterite nickel ore to improve resource utilization and reduce project construction investment and production and operating costs.
[0004] Summary of the Invention
[0005] The purpose of the present invention is to provide a method for making sintered bricks using tailings from high-pressure acid leaching of laterite nickel ore. By mixing the tailings from high-pressure acid leaching of laterite nickel ore with additives in a certain proportion and then sintering them into bricks, the resource utilization of the tailings from high-pressure acid leaching of laterite nickel ore can be achieved.
[0006] The present invention provides a method for producing sintered bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore, comprising the following steps:
[0007] S10: mixing the filtered laterite nickel ore high-pressure acid leaching smelting tailings with an additive to obtain a mixture, adding a certain amount of water to the mixture, stirring evenly to obtain a mixed slurry, and then pressing the mixed slurry into a brick;
[0008] S20: aging the pressed brick for a period of time;
[0009] S30: drying the aged bricks;
[0010] S40: firing the dried green bricks into fired bricks.
[0011] In one achievable manner, in the above step S10, the moisture content of the tailings from the high-pressure acid leaching of laterite nickel ore after pressure filtration is 25%-40%.
[0012] In one achievable manner, in the above step S10, the additive includes one or more of ferronickel slag, blast furnace slag and clay.
[0013] In one achievable manner, in the above step S10, the weight percentage of the additive in the mixture is 5%-50%, and the rest is laterite nickel ore high-pressure acid leaching smelting tailings, and the sum of the weight percentages of the additive in the mixture and the laterite nickel ore high-pressure acid leaching smelting tailings is 100%.
[0014] In one feasible manner, in the above-mentioned step S10, before the laterite nickel ore high-pressure acid leaching smelting tailings are mixed with the additive, the laterite nickel ore high-pressure acid leaching smelting tailings are first crushed to reduce the particle size of the laterite nickel ore high-pressure acid leaching smelting tailings to less than 5 mm.
[0015] In one achievable manner, in the above step S20, the specific step of aging the bricks is: placing the bricks naturally at room temperature and normal pressure for 12-48 hours.
[0016] In one achievable manner, in the above step S30, the drying temperature of the bricks is 30° C.-90° C., and the drying time is 12-48 hours.
[0017] In one achievable manner, in the above step S30, the moisture content of the dried bricks is controlled to be below 5%.
[0018] In one achievable manner, in the above step S40, the sintering temperature of the brick is 800° C.-1200° C., and the sintering time is 1-8 hours.
[0019] The present invention also provides a sintered brick, which is produced by the above-mentioned method of producing sintered bricks by utilizing the tailings of high-pressure acid leaching of laterite nickel ore.
[0020] The present invention provides a method for preparing sintered bricks using high-pressure acid leaching smelting tailings from laterite nickel ore. The method comprises mixing the high-pressure acid leaching smelting tailings from laterite nickel ore after pressure filtration with an additive in a certain proportion, adding a certain amount of water and stirring evenly, pressing and forming a brick blank, drying after aging for a period of time, and finally sintering the brick blank into a brick. This method realizes resource utilization of the high-pressure acid leaching smelting tailings from laterite nickel ore, improves the resource utilization rate of laterite nickel ore, reduces the cost and risk of tailings storage, reduces land resource occupation, and reduces project construction investment and production and operation costs. At the same time, the method is not only simple in manufacturing process, but also has cheap and readily available raw materials, which can save production costs, and the obtained sintered bricks have high strength and are suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] FIG1 is a schematic diagram of a process for producing sintered bricks from tailings of laterite nickel ore subjected to high-pressure acid leaching in an embodiment of the present invention. DETAILED DESCRIPTION
[0022] The following embodiments of the present invention are described in further detail with reference to the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0023] The terms "first," "second," "third," "fourth," and the like (if any) in the description and claims of the present invention are used to distinguish similar objects and are not necessarily used to describe a particular sequential order or sequence.
[0024] The directional terms "up," "down," "left," "right," "front," "back," "top," and "bottom" (if any) used in the specification and claims of the present invention are defined by the positions of the structures in the drawings and the positions of the structures relative to each other, and are intended only for clarity and convenience in expressing the technical solution. It should be understood that the use of directional terms should not limit the scope of protection claimed in the present invention.
[0025] FIG1 is a schematic diagram of a process for producing sintered bricks from tailings of laterite nickel ore subjected to high pressure acid leaching in accordance with an embodiment of the present invention. As shown in FIG1 , the method for producing sintered bricks from tailings of laterite nickel ore subjected to high pressure acid leaching in accordance with an embodiment of the present invention comprises the following steps:
[0026] S10: mixing the filtered laterite nickel ore high-pressure acid leaching smelting tailings with an additive to obtain a mixture, adding a certain amount of water to the mixture, stirring evenly to obtain a mixed slurry, and then pressing the mixed slurry into a brick; wherein the laterite nickel ore high-pressure acid leaching smelting tailings is the tailings obtained after nickel is produced from laterite nickel ore by a high-pressure acid leaching method;
[0027] S20: aging the pressed bricks for a period of time to allow the tailings in the bricks to fully react with the additives, thereby improving the strength of the fired bricks;
[0028] S30: drying the aged bricks;
[0029] S40: firing the dried green bricks into fired bricks.
[0030] Specifically, the present embodiment provides a method for making sintered bricks from high-pressure acid leaching smelting tailings of laterite nickel ore, wherein the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration are mixed with additives in a certain proportion, a certain amount of water is added and stirred evenly, and then pressed to form a brick blank, dried after aging for a period of time, and finally sintered into bricks, thereby realizing the resource utilization of high-pressure acid leaching smelting tailings of laterite nickel ore, improving the resource utilization rate of laterite nickel ore, while reducing the cost and risk of tailings storage, reducing the amount of land resources occupied, and reducing project construction investment and production and operation costs. At the same time, the method is not only simple in manufacturing process, but also has cheap and easily available raw materials, is simpler to operate than processes such as autoclaving, and can significantly save production costs, and the obtained sintered bricks have high strength and are suitable for mass production.
[0031] As an embodiment, in the above step S10, the moisture content of the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration is 25%-40%.
[0032] Specifically, since the laterite nickel ore high-pressure acid leaching smelting tailings are tailings obtained after nickel is produced from laterite nickel ore through a high-pressure acid leaching method, the water content of the laterite nickel ore high-pressure acid leaching smelting tailings is relatively high (the water content generally reaches 50%-60%), and dehydration treatment is required during brick making. By performing filter press treatment on the laterite nickel ore high-pressure acid leaching smelting tailings, the water content of the tailings is reduced to 25%-40%, which can not only produce a good cross-linking effect between the tailings and the additives during the mixing process, but also avoid the bricks being unable to be formed due to excessive water content when pressed into bricks, and avoid affecting the quality ratio of the tailings and the additives due to excessive water content in the tailings; at the same time, since the bricks need to be dried and sintered later, the filter press treatment of the tailings in advance can facilitate the subsequent drying and sintering work.
[0033] As an embodiment, in the above-mentioned step S10, before the high-pressure acid leaching tailings of laterite nickel ore are mixed with the additive, the tailings of laterite nickel ore high-pressure acid leaching can be crushed to reduce the particle size of the tailings to less than 5 mm. The crushing process not only makes the subsequent mixing of the tailings and the additive more uniform, but also facilitates the pressing and forming of the brick blanks. At the same time, it prevents the tailings particles from protruding from the brick surface due to being too large and affecting the flatness of the fired brick, thereby improving the quality of the fired brick.
[0034] As an embodiment, in the above-mentioned step S10, the additive includes one or more of nickel iron slag, blast furnace slag, and clay. The additive is not only cheap and easy to obtain, but also can achieve a higher structural strength after mixing with the tailings, thereby making the sintered brick have a higher strength. Among them, nickel iron slag and blast furnace slag are both solid wastes. Using nickel iron slag and blast furnace slag as additives can further achieve solid waste recycling, reduce production costs, and alleviate the pressure of solid waste treatment. Of course, in other embodiments, other materials can also be used as additives.
[0035] As an embodiment, in step S10 above, the weight percentage of the additive in the mixture is 5%-50%, and the remainder is laterite nickel ore high pressure acid leaching smelting tailings (excluding the weight of water in the laterite nickel ore high pressure acid leaching smelting tailings, that is, the laterite nickel ore high pressure acid leaching smelting tailings is the dry weight). The sum of the weight percentages of the additive in the mixture and the laterite nickel ore high pressure acid leaching smelting tailings is 100%. For example, if the weight percentage of the additive is 20%, the weight percentage (dry weight) of the laterite nickel ore high pressure acid leaching smelting tailings is 80%.
[0036] As an embodiment, in the above step S10, the specific step of pressing the mixed slurry into a brick comprises: filling the mixed slurry into a mold, and then punching the mixed slurry in the mold to obtain a brick of a certain shape.
[0037] As an embodiment, in the above-mentioned step S20, the specific steps of aging the brick green are: placing the brick green naturally at room temperature and normal pressure for 12-48 hours. During the aging process, the tailings in the brick green can fully react with the additives, which is beneficial to improving the strength of the sintered brick.
[0038] As an embodiment, in the above step S30, the bricks are dried at a temperature of 30°C to 90°C for 12 to 48 hours. The moisture content of the dried bricks is controlled below 5%, thereby facilitating the subsequent sintering process.
[0039] As an embodiment, in the above step S40, the sintering temperature of the brick is 800°C-1200°C, and the sintering time is 1-8 hours. By sintering the brick at high temperature, the brick is hardened and has good structural strength.
[0040] The embodiment of the present invention further provides a sintered brick, which is produced by the above-mentioned method of producing sintered bricks using high-pressure acid leaching smelting tailings of laterite nickel ore.
[0041] The method for making sintered bricks using high-pressure acid leaching smelting tailings of laterite nickel ore provided in an embodiment of the present invention comprises mixing the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration with an additive in a certain proportion, adding a certain amount of water and stirring evenly, pressing and forming a brick blank, drying after aging for a period of time, and finally sintering into bricks, thereby realizing resource utilization of the high-pressure acid leaching smelting tailings of laterite nickel ore, improving the resource utilization rate of laterite nickel ore, and reducing the cost and risk of tailings storage, reducing the amount of land resources occupied, and reducing project construction investment and production and operation costs. At the same time, the method is not only simple in manufacturing process, but also has cheap and easily available raw materials, which can save production costs, and the obtained sintered bricks are high in strength and suitable for mass production.
[0042] Example 1
[0043] The filtered laterite nickel ore high-pressure acid leaching tailings have a moisture content of 30%. The tailings are then mixed with the additive nickel-iron slag in a dry weight ratio of 75:25. The mixture is then placed into a 90mm*40mm*40mm mold and pressed into bricks. The pressed bricks are then aged for 15 hours and demolded. The bricks are then dried at 30-90°C for 24 hours, calcined at 1100°C for 2 hours, and cooled to room temperature to produce sintered bricks. Tests conducted in accordance with the relevant provisions of the national standard GB5101-2017, "Sintered Ordinary Bricks," show that the strength of the sintered bricks exceeds 10 MPa.
[0044] Example 2
[0045] The water content of the filtered laterite nickel ore high-pressure acid leaching smelting tailings is 35%. The tailings are then mixed with blast furnace slag (additive) at a dry weight ratio of 85:15. The mixture is then placed into a 90mm*40mm*40mm mold and pressed into bricks. The pressed bricks are then aged for 15 hours and demolded. The bricks are then dried at 30-90°C for 24 hours, calcined at 1000°C for 3 hours, and cooled to room temperature to produce sintered bricks. Tests conducted in accordance with the relevant provisions of the national standard GB5101-2017, "Sintered Ordinary Bricks," show that the strength of the sintered bricks exceeds 10 MPa.
[0046] Example 3
[0047] The water content of the filtered laterite nickel ore high-pressure acid leaching tailings is 33%. The tailings are then mixed with a clay additive at a dry weight ratio of 90:10. The mixture is then placed into a 90mm*40mm*40mm mold and pressed into bricks. The pressed bricks are then aged for 15 hours and demolded. The bricks are then dried at 30-90°C for 24 hours, calcined at 1050°C for 2.5 hours, and cooled to room temperature to produce sintered bricks. Tests conducted in accordance with the national standard GB5101-2017, "Sintered Ordinary Bricks," show that the strength of the sintered bricks exceeds 10 MPa.
[0048] Example 4
[0049] The filtered laterite nickel ore high-pressure acid leaching tailings have a moisture content of 30%. The tailings are then mixed with the additive nickel-iron slag in a 50:50 dry weight ratio. The mixture is then placed into a 90mm*40mm*40mm mold and pressed into bricks. The pressed bricks are then aged for 15 hours and demolded. The bricks are then dried at 30-90°C for 24 hours, calcined at 1100°C for 2 hours, and cooled to room temperature to produce sintered bricks. Tests conducted in accordance with the relevant provisions of the national standard GB5101-2017, "Sintered Ordinary Bricks," show that the strength of the sintered bricks exceeds 10 MPa.
[0050] Example 5
[0051] The water content of the filtered laterite nickel ore high-pressure acid leaching smelting tailings is 30%. The tailings are then mixed with the additive nickel-iron slag at a dry weight ratio of 97:3. The mixture is then placed into a 90mm*40mm*40mm mold and pressed into a brick. The pressed bricks are then aged for 15 hours and demolded. The bricks are then dried at 30°C-90°C for 24 hours, calcined at 1100°C for 2 hours, and cooled to room temperature to produce sintered bricks. Testing according to the relevant provisions of the national standard GB5101-2017 "Sintered Ordinary Bricks" shows that the strength of the sintered bricks is less than 10 MPa.
[0052] Example 6
[0053] The filtered laterite nickel ore high-pressure acid leaching smelting tailings have a moisture content of 30%. The tailings are then mixed with the additive nickel-iron slag in a dry weight ratio of 40:60. The mixture is then placed into a 90mm*40mm*40mm mold and pressed into bricks. The pressed bricks are then aged for 15 hours and demolded. The bricks are then dried at 30-90°C for 24 hours, calcined at 1100°C for 2 hours, and cooled to room temperature to produce sintered bricks. Testing according to the relevant provisions of the national standard GB5101-2017 "Sintered Ordinary Bricks" shows that the strength of the sintered bricks is less than 10 MPa.
[0054] The above are merely specific embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.
Claims
1. A method for making sintered bricks using high pressure acid leaching smelting tailings from laterite nickel ore, characterized in that: The following steps are involved: S10: mixing the filtered laterite nickel ore high pressure acid leaching smelting tailings with an additive to obtain a mixture, adding a certain amount of water to the mixture, stirring evenly to obtain a mixed slurry, and then pressing the mixed slurry into a brick; S20: aging the pressed brick for a period of time; S30: drying the aged bricks; S40: firing the dried green bricks into fired bricks.
2. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S10, the moisture content of the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration is 25%-40%.
3. The method for preparing sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S10, the additive includes one or more of nickel-ferro slag, blast furnace slag and clay.
4. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S10, the weight percentage of the additive in the mixture is 5%-50%, and the rest is laterite nickel ore high pressure acid leaching smelting tailings. The sum of the weight percentages of the additive in the mixture and the laterite nickel ore high pressure acid leaching smelting tailings is 100%.
5. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S10, before the laterite-nickel ore high-pressure acid leaching smelting tailings are mixed with the additive, the laterite-nickel ore high-pressure acid leaching smelting tailings are first crushed to reduce the particle size of the laterite-nickel ore high-pressure acid leaching smelting tailings to less than 5 mm.
6. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S20, the specific step of aging the brick blank is: placing the brick blank naturally at room temperature and pressure for 12-48 hours.
7. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S30, the drying temperature of the bricks is 30°C-90°C, and the drying time is 12-48 hours.
8. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S30, the moisture content of the dried bricks is controlled below 5%.
9. The method for making sintered bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S40, the sintering temperature of the brick is 800°C-1200°C, and the sintering time is 1-8 hours.
10. A fired brick, characterized in that: The brick is made by the method for making sintered bricks by using high-pressure acid leaching smelting tailings of laterite nickel ore as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Acid-leaching-method laterite-nickel-slag-based autoclaved product and preparation method thereof
CN104829181A
Fired brick and preparation method thereof
CN105948711A
Method for preparing light brick by using metallurgical waste slag
CN106747320A
Cobalt smelting waste-based sintered brick and preparation method thereof
CN106747321A
Method for producing building ceramsite from laterite-nickel ore acid leaching waste residues
CN106938895A
Cited By
All-component comprehensive utilization method for leaching residues of laterite-nickel ore high-pressure acid leaching process
CN119876587A