Method for performing laser cladding of silver layer on copper substrate, and use of method in repair of large-current copper busbar of hydroelectric generating set
Through the application of blue laser cladding technology and silver-copper alloy powder on copper substrates, the problem of thin and easy falling off of silver plating during infrared laser cladding is solved, and a high-quality silver coating on the copper busbar surface is achieved, ensuring that The compactness and bonding strength of the cladding layer are suitable for the repair of high-current copper busbars of hydroelectric units.
Patent Information
- Application Number
- PCT/CN2023/117770
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-09-08
- Publication Date
- 2024-10-03
AI Technical Summary
When the existing laser cladding technology plating silver on the surface of the copper busbar, due to the low absorption rate of copper and silver on infrared lasers, the thickness of the silver plating layer is insufficient and easy to fall off. Infrared laser processing is prone to splashing, pores and inclusion defects. It is difficult to achieve stable forming.
Using blue light laser cladding equipment, silver-copper alloy powder is used to laser cladding on the copper substrate through coaxial powder feeding, the laser power is controlled at 1100W-1350W, the scanning speed is 6mm/s-10mm/s, overlapping The ratio is between 45% and 65%, and the thickness and surface quality of the silver layer are ensured through pretreatment and subsequent grinding.
Improve the absorption rate of the material to laser, realize the metallurgical combination of highly reflective and thermally conductive silver alloy coatings, ensure the density and defects of the cladding layer are free, solve the problems of pores and inclusions, and improve the surface of the copper busbar. Silver layer combines strength and durability.
Smart Images

Figure CN2023117770_03102024_PF_FP_ABST
Abstract
Description
Laser cladding method of silver layer on copper substrate and its application in repairing high current copper busbar of hydropower unit Technical Field
[0001] The present invention belongs to the technical field of laser cladding, and in particular relates to a method for laser cladding a silver layer on a copper substrate and an application of the method in repairing a high-current copper busbar of a hydropower unit. Background Art
[0002] The copper busbars of hydropower units are crucial electrical connectors, carrying high currents. To improve conductivity, the copper busbar joints are typically plated with silver. However, due to the silver plating process and related standards, the silver layer on the copper busbar surface is relatively thin. Furthermore, after long-term operation, the silver coating on the copper busbar surface can become detached due to poor adhesion, leading to silver failure.
[0003] At present, laser cladding technology is a new laser additive manufacturing technology that has emerged with the development of high-power lasers. At the same time, laser cladding technology has outstanding technical advantages. The substrate and the surface cladding material are metallurgically bonded, the bonding strength is relatively high, the structure is dense and there are few pores, the dilution rate is therefore low, and the thickness of the cladding coating is controllable. These advantages also meet the needs of the silver layer on the surface of the copper busbar.
[0004] However, the laser light source commonly used at present is an infrared laser light source (wavelength of about 1000nm), which is not suitable for cladding silver layer on the surface of copper busbar. This is because copper and silver are highly reflective metals with very low absorption rate in the infrared laser band. The absorption rate of copper in the infrared band is only about 5%, and the absorption rate of silver to infrared laser is even lower. Due to the good thermal conductivity of copper, the laser cladding method using infrared laser light source will cause great spatter on the copper surface, and the cladding coating will have many pores and inclusions. The quality of the cladding coating is poor and even has difficulty in stable forming.
[0005] Summary of the Invention
[0006] The present invention provides a method for laser cladding a silver layer on a copper substrate and application thereof in repairing a high-current copper busbar of a hydropower unit. The method improves the absorption rate of the substrate and powder material to laser, and the cladding layer is free of pore inclusion defects.
[0007] The technical solution of the present invention is a method for laser cladding a silver layer on a copper substrate, which specifically comprises the following steps:
[0008] S1. Pretreatment before cladding: polish and remove impurities and oxide layer on the surface of copper substrate, clean and dry;
[0009] S2. Laser cladding: Using blue laser cladding equipment, silver-copper alloy powder is used as the powder material, and the copper substrate is laser clad with a silver layer through coaxial powder feeding. The laser power is 1100W-1350W, the laser cladding head scanning speed is 6mm / s-10mm / s, and the overlap rate is 45%-65%;
[0010] S3. Polish the surface of the copper substrate and coat the silver layer to make it meet the relevant requirements of the hydropower unit.
[0011] Furthermore, the copper substrate is T2 copper, the copper content (wt%) is ≥99.9, and other impurities (wt%) are ≤0.1.
[0012] Furthermore, the silver-copper alloy powder in S2 comprises, by mass fraction, 20-30% Cu, 8-15% Ni, 0.5-2% Si, and the remainder being silver and unavoidable impurities.
[0013] Furthermore, the silver-copper alloy powder has a particle size of 75 μm-150 μm and is dried before use.
[0014] Furthermore, the blue laser wavelength of the blue laser cladding equipment in S2 is 450nm-480nm.
[0015] Furthermore, during laser cladding in S2, the light spot is a circular spot with a diameter of 1.5 mm to 1.8 mm.
[0016] Furthermore, the coaxial powder feeding method in S2 adopts an annular powder feeding nozzle, and the powder feeding nozzle is coaxial with the circular light spot.
[0017] Furthermore, during laser cladding in S2, the powder feeding gas flow rate is 10-15 L / min; the powder feeding amount is 4 g / min-8 g / min; the shielding gas flow rate is 10-15 L / min; and both the powder feeding gas and the shielding gas are inert gases, including but not limited to nitrogen, argon or helium.
[0018] Furthermore, the thickness of the silver layer on the surface of the copper substrate in S3 after polishing is required to be greater than 0.1 mm, and the surface roughness is required to be less than Ra0.8.
[0019] Furthermore, the surface of the copper busbar can be clad with a multi-layer silver coating, and the thickness of a single-layer cladding silver layer is 0.1mm-0.4mm.
[0020] The present invention has the following beneficial effects:
[0021] 1. The present invention uses a blue laser light source, which can greatly improve the material's absorption rate of laser light compared to a red laser light source. In addition, the laser cladding substrate and powder material in the present invention are both highly reflective materials. In particular, the absorption rate of the silver powder material to infrared laser light (less than 3%) is lower than that of the copper substrate (less than 5% absorption rate to infrared laser light). As a result, the process window for cladding the silver powder material on the copper substrate is narrow, and it is difficult to find the balance point where the copper substrate and silver powder material absorb the laser energy and fully melt and combine. However, the use of a short-wavelength blue laser to clad the copper substrate and silver powder can effectively improve the absorption rate of laser light.
[0022] 2. When silver powder material is clad on a copper substrate by blue laser, although the absorption rate of laser energy by the copper substrate and silver powder is improved, there is still a large difference in the absorption rate of laser energy by the copper substrate and silver powder materials. The difference in laser energy absorption rate of different materials will lead to different minimum energy thresholds for each material to absorb laser energy to open the molten pool and the maximum energy thresholds for the molten pool to boil and overburn. If the copper substrate only absorbs the laser energy to reach the minimum threshold for opening the molten pool but the silver powder material fails to reach the melting threshold, the prepared cladding layer will have defects such as agglomeration and unfusion; if the threshold for complete melting of the silver powder material is fully reached, the copper substrate absorbs more laser energy, which leads to overburning of the copper substrate and boiling of the molten pool. Copper has good fluidity in liquid state and will flow quickly when the molten pool boils and close quickly when solidified, resulting in gases and impurities that have not fully escaped from the molten pool being trapped to form pores and inclusion defects. The inventor creatively discovered that a power of 1100-1350W can better match the molten pool state of the copper substrate and the silver-copper alloy powder. At the same time, by controlling the low scanning speed and high overlap rate, the cladding layer can be made dense and free of pore inclusion defects.
[0023] 3. The method provided by the present invention can be used to clad a highly reflective and highly thermally conductive silver alloy coating on the surface of the copper busbar, and the copper busbar and the surface cladding silver layer can be metallurgically bonded with each other, with high bonding strength. The present invention can achieve a single-layer cladding silver layer with a thickness of 0.1 mm to 0.4 mm, and can also perform multi-layer cladding as needed.
[0024] 4. The silver-copper alloy powder used in the present invention can improve its oxidation resistance and strengthen its mechanical properties by adding a certain amount of Cu. When the amount of Cu added is large, Cu and Ag form a eutectic to strengthen its mechanical properties. However, the addition of a large amount of Cu easily causes crystallization. In the present invention, by adding a certain amount of Ni, the grains can be refined and the segregation of the internal structure of the silver-based alloy can be reduced. Furthermore, a certain amount of Si is added to the alloy material, which synergizes with Cu to significantly improve the high-temperature oxidation resistance of the alloy material. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 shows a picture of the high-current copper busbar of a hydropower unit after silver cladding. DETAILED DESCRIPTION
[0026] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.
[0027] The silver-copper alloy powder used in the following examples contains, by mass percentage, 28% Cu, 10% Ni, 1% Si, and the remainder Ag and unavoidable impurities, and has a particle size of 75 μm to 150 μm.
[0028] Example 1:
[0029] The method of laser cladding silver layer on copper substrate uses copper plate as copper substrate and performs single-layer cladding. The thickness of the silver layer after cladding and polishing is required to be above 0.1mm and the roughness is less than Ra0.8.
[0030] The specific steps are:
[0031] 1. Place the silver-copper alloy powder in a drying equipment at 140°C and dry it for 30 minutes.
[0032] 2. Turn on the protective gas (high-purity nitrogen) and keep the gas flow constant until the power of the equipment is turned off.
[0033] 3. The laser cladding head should always maintain a distance of 12 to 14 mm from the copper plate surface.
[0034] 4. Use 800-grit sandpaper to polish the copper plate. Use a dust-free cloth and industrial alcohol to wipe off metal dust, dust, oil, etc. on the surface of the copper plate to ensure that the surface of the copper plate is clean and dry.
[0035] 5. The selected process parameters are as follows: laser spot diameter 1.6 mm, laser power 1300 W, laser cladding head scanning speed 6 mm / s, cladding scanning overlap rate 50%, silver-copper alloy powder feeding rate 4.5 g / min, powder feeding gas flow rate 11 L / min, laser cladding shielding gas flow rate 11 L / min.
[0036] 6. After laser cladding, polish the silver cladding layer using 100-grit and then 400-grit sandpaper. Inspect the surface roughness and thickness of the silver cladding layer before and after polishing. After polishing, the copper busbar requirements for hydropower units should be met: a roughness less than Ra0.8, a silver layer thickness greater than 0.1 mm, and no pores or inclusions. See Table 1 for details.
[0037] Example 2-1
[0038] Based on Example 1, the only difference is that the laser power is 1100 W. A molten pool can be formed when the laser energy density reaches the minimum energy threshold for opening a molten pool, thereby achieving laser cladding.
[0039] Example 2-2
[0040] Based on Example 1, the only difference is that the laser power is 1000 W. The molten pool cannot be opened and cladding cannot be achieved.
[0041] Example 2-3
[0042] Based on Example 1, the only difference is the laser power of 1400 W. Excessively high laser energy density can cause overburning of the copper substrate and boiling of the molten pool, which in turn increases molten pool fluidity and rapidly closes during solidification, ultimately leading to defects such as pores and inclusions in the cladding layer. Furthermore, Cu and Ag form a eutectic, which can also cause structural segregation in an unstable molten pool.
[0043] Example 3-1
[0044] Based on Example 1, the only difference is that the scanning speed of the laser cladding head is 10 mm / s.
[0045] Example 3-2
[0046] Based on Example 1, the only difference is that the laser cladding head scanning speed is 20 mm / s. This shortens the laser heat input time per unit cladding area and reduces heat accumulation per unit cladding area, resulting in an unstable and insufficient melting of the molten pool and a large number of unfused defects in the cladding layer.
[0047] Example 4:
[0048] After a single layer of silver coating is applied to the surface of the copper plate, multiple layers of silver coating are further applied to the surface of the copper plate.
[0049] The operation process is the same as that of Example 1.
[0050] After the second layer of blue light laser cladding silver layer was completed, the thickness and surface roughness of the cladding silver layer before and after polishing were tested, as shown in Table 1.
[0051] After polishing, the silver layer on the copper plate surface meets the basic requirements of roughness less than Ra0.8, the silver layer thickness is greater than 0.3mm and there are no pore inclusion defects.
[0052] The surface roughness and thickness test results of the silver cladding layer obtained in the above examples before and after polishing are shown in Table 1.
[0053] Table 1
[0054] The method of the present invention is used for laser silver cladding repair of high-current copper busbars in hydropower units. Both the copper busbar and the cladding silver layer have high absorption rates of the blue laser light source, and a silver coating with a certain thickness and no pores or inclusions can be formed on the copper busbar, as shown in Figure 1, achieving metallurgical bonding.
Claims
1. A method for laser cladding a silver layer on a copper substrate, characterized in that: The specific steps are: S1. Pretreatment before cladding: polish and remove impurities and oxide layer on the surface of copper substrate, clean and dry; S2. Laser cladding: Blue light laser cladding equipment is used, silver-copper alloy powder is used as powder material, and the copper substrate is laser clad with a silver layer by coaxial powder feeding. The laser power is 1100W-1350W, the scanning speed of the laser cladding head is 6mm / s-10mm / s, and the overlap rate is 45%-65%; S3. Polish the surface of the copper substrate and melt the silver layer to make it meet the relevant requirements.
2. The method according to claim 1, characterized in that: The copper substrate is T2 red copper, the copper content (wt%) is ≥99.9, and other impurities (wt%) are ≤0.
1.
3. The method according to claim 1, characterized in that: The silver-copper alloy powder in S2 is composed of 20-30% Cu, 8-15% Ni, 0.5-2% Si, and the rest is silver and unavoidable impurities.
4. The method according to claim 1, characterized in that: The particle size of the silver-copper alloy powder is 75 μm-150 μm and is dried before use.
5. The method according to claim 1, characterized in that: The blue laser wavelength of the blue laser cladding equipment in S2 is 450nm-480nm.
6. The method according to claim 1, characterized in that: In S2, the laser cladding light spot is a circular light spot with a diameter of 1.5mm-1.8mm; the coaxial powder feeding method adopts an annular powder feeding nozzle, which is coaxial with the circular light spot.
7. The method according to claim 1, characterized in that: In S2, during laser cladding, the powder feeding gas flow rate is 10-15 L / min; the powder feeding amount is 4 g / min-8 g / min; the shielding gas flow rate is 10-15 L / min; both the powder feeding gas and the shielding gas are inert gases, including but not limited to nitrogen, argon or helium.
8. The method according to any one of claims 1 to 8, characterized in that: In S3, the thickness of the silver layer on the copper substrate after polishing is required to be greater than 0.1mm, and the surface roughness is less than Ra0.
8.
9. The method according to claim 1, characterized in that: The surface of the copper busbar can be clad with multiple layers of silver coating, and the thickness of a single-layer cladding silver layer is 0.1mm-0.4mm.
10. Application of the method according to any one of claims 1 to 9 in the repair of high-current copper busbars of hydropower units.
Citation Information
Patent Citations
Copper base material and manufacturing method for silver-coated layer on surface of copper base material
CN114574858A
Silver-based multi-component alloy powder material and preparation method and application thereof
CN114974645A
Method for manufacturing functionally graded material through copper-silver dissimilar metal blue laser additive
CN115026304A
Process for laser cladding of silver layer on copper bus
CN115216767A
Device and process for preparing silver layer on copper base material through blue laser cladding processing
CN116397226A
Cited By
Heavy-duty bearing with silver-copper bimetal composite structure and preparation method of heavy-duty bearing
CN121649571A