Formula of heat absorption film, preparation method therefor and use thereof
By coating the surface of LOW-E coated glass with a heat-absorbing film, the problems of easy oxidation and difficult processing of the coating are solved, and anti-oxidation, wear-resistant and low-energy-consumption tempering is achieved, improving production efficiency and yield.
Patent Information
- Application Number
- PCT/CN2024/073178
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-03
AI Technical Summary
Existing LOW-E coated glass is prone to oxidation after coating, resulting in high packaging costs. Care must be taken during processing to avoid scratches. In addition, the tempering process requires high temperatures and a long time, resulting in low cost and efficiency.
A heat-absorbing film is coated on the surface of the coating layer, including acrylate, photoinitiator and hardener, and is cured by heating and ultraviolet irradiation to form an antioxidant and wear-resistant coating, which reduces the tempering temperature and time.
Simplify packaging, reduce costs, improve processing yield, reduce tempering energy consumption, and improve production efficiency.
Smart Images

Figure CN2024073178_03102024_PF_FP_ABST
Abstract
Description
A heat-absorbing film formulation, preparation method and application thereof Technical Field
[0001] The present invention belongs to the field of heat-absorbing film production, and in particular relates to a heat-absorbing film formula, a preparation method and application thereof. Background Art
[0002] The energy-saving Low-E coated glass currently used in the market, also known as low-emissivity glass, is a glass surface coated with multiple layers of metal or other compounds, also known as a functional film. However, due to the inherent silver coating, which easily oxidizes in air, Low-E products cannot be stored for long periods of time. After coating, Low-E glass must be promptly processed into finished products. The commonly used method in the domestic and international industry is to place a desiccant inside each package of glass and then tightly seal it with packaging materials such as PE cloth. The shortcomings / deficiencies of existing technologies are as follows:
[0003] 1. Since coated products are easily oxidized, they require very airtight packaging materials to protect them. Currently, the outer packaging materials used are PE film, aluminum film, edge sealing film, kraft paper and desiccant, which results in high packaging costs.
[0004] 2. Since the film layer of the coated product is relatively soft, especially for high-performance products, the later processing process requires extra care and the defective rate is relatively high.
[0005] 3. Since the functional film in the coated LOW-E product has a low surface emissivity, heat transfer is difficult to pass through the glass. Therefore, the coated product needs to be subjected to higher temperature and longer tempering time during tempering heat treatment. The tempering cost and production efficiency are far lower than ordinary glass.
[0006] In response to the above technical problems and defects, this solution proposes a method of coating a heat-absorbing film on the surface of the coating film layer to improve the glass's antioxidant properties and processing resistance, reduce the energy consumption of tempering processing, and solve a series of problems.
[0007] Summary of the Invention
[0008] Purpose of the invention: In order to overcome the shortcomings of the existing technology, the present invention provides a formula, preparation method and application of a heat-absorbing film, which can be coated on the surface of the coating film layer to improve the glass's antioxidant properties and processing resistance, reduce the energy consumption of tempering processing and other problems.
[0009] Technical solution: To achieve the above purpose, the technical solution of the present invention is as follows:
[0010] A heat-absorbing film formulation comprises a mixture of 85% to 98.5% by mass of component A, 1% to 10% by mass of component B, and 0.5% to 5% by mass of component C, wherein:
[0011] The component A comprises one or more of acrylic acid resins;
[0012] The component B comprises one or more photoinitiators, and the component B undergoes a cross-linking reaction during ultraviolet light irradiation, so that the component A is cured from a monomer to a polymer;
[0013] The component C comprises one or more of a hardener and a leveling agent.
[0014] Furthermore, the acrylic acid resins include butyl acrylate, isobornyl acrylate, methyl methacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and tripropylene glycol diacrylate.
[0015] Furthermore, the photoinitiator comprises 2-isopropylthioxanthone, ethyl 4-dimethylaminobenzoate, benzoin dimethyl ether, 2-hydroxy-2-methyl-1-phenyl-1-propanone, tetraethyl Michler's ketone, benzophenone, 1-hydroxycyclohexylphenyl ketone, and 2-methyl-1-(4-methylthiophenyl)-2-morpholine-propanone.
[0016] Furthermore, it contains 90.5% of methyl methacrylate, 3.5% of ethyl 4-dimethylaminobenzoate, 3.5% of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1.5% of benzophenone and 1% of polyethylene wax in proportion by mass.
[0017] Furthermore, it contains 50% of isobornyl acrylate, 44.5% of trimethylolpropane triacrylate, 1% of benzoin dimethyl ether, 3% of tetraethyl Michler's ketone, 1% of polyethylene wax and 0.5% of a leveling agent distributed in proportion by mass.
[0018] Furthermore, it contains 30% of isobornyl acrylate, 30% of tripropylene glycol diacrylate, 32.5% of trimethylolpropane triacrylate, 2.5% of 2-isopropylthioxanthone, 2.5% of ethyl 4-dimethylaminobenzoate, 1.5% of benzophenone and 1% of polyethylene wax distributed in proportion by mass.
[0019] Furthermore, it contains 20% methyl methacrylate, 20% tripropylene glycol diacrylate, 20% 1,6-hexanediol diacrylate, 32.5% trimethylolpropane triacrylate, 1.5% 2-isopropylthioxanthone, 3.5% ethyl 4-dimethylaminobenzoate, 1% benzoin dimethyl ether, 0.5% benzophenone and 1% polyethylene wax distributed in proportion by mass.
[0020] A method for preparing a heat-absorbing film from a heat-absorbing film formula comprises:
[0021] Heat the formula mixture until it becomes fluid;
[0022] coating the heated mixture on the surface of the substrate to form a coating layer;
[0023] The coating layer is dried and cured by ultraviolet irradiation to obtain a heat-absorbing film attached to the surface of the substrate.
[0024] The invention discloses an application of a heat-absorbing film in the manufacture of coated glass.
[0025] A coated glass has a functional film coated on the outside of a glass substrate and a heat absorbing film coated on the outer surface of the functional film layer.
[0026] Beneficial effects: The heat-absorbing film of the present invention has the characteristics of anti-oxidation, wear resistance and heat absorption, and its specific advantages are as follows:
[0027] 1. The coated products with heat-absorbing film on roller can simplify the outer packaging, and no packaging is required during the processing, which saves the use cost.
[0028] 2. For products coated with heat-absorbing film on rollers, there is no need to worry about the functional film being scratched in the subsequent processes, which greatly improves the processing yield.
[0029] 3. The heat-absorbing film can be used in the manufacture of coated glass. Since the heat-absorbing film of the present invention can well absorb the tempering temperature, the temperature required for tempering is reduced, the tempering time is shortened, the tempering energy consumption is reduced, and the cost is saved. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a formula of the heat-absorbing film of the present invention;
[0031] FIG2 shows the formula and performance parameters of the heat-absorbing film according to the first embodiment of the present invention;
[0032] FIG3 shows the formula and performance parameters of the heat-absorbing film according to the second embodiment of the present invention;
[0033] FIG4 shows the formula and performance parameters of the heat-absorbing film according to the third embodiment of the present invention;
[0034] FIG5 shows the formula and performance parameters of the heat-absorbing film according to the fourth embodiment of the present invention. DETAILED DESCRIPTION
[0035] The present invention will be further described below with reference to the accompanying drawings.
[0036] As shown in FIG1 , a heat-absorbing film formulation comprises a mixture of 85%-98.5% by mass of component A, 1%-10% by mass of component B, and 0.5%-5% by mass of component C, wherein:
[0037] The component A contains one or more acrylates; acrylate is a general term for esters of acrylic acid and its homologues. Acrylates can self-polymerize or copolymerize with other monomers to form mixtures with different degrees of adhesion and bonding strength, which are used to form the film body of the heat-absorbing film. Component A mainly plays the role of preventing glass coating oxidation, preventing scratches, and absorbing heat during the tempering process.
[0038] The component B comprises one or more photoinitiators, and the component B undergoes a cross-linking reaction during ultraviolet light irradiation, so that the component A is cured from a monomer to a polymer;
[0039] The component C comprises one or more of a hardener and a leveling agent.
[0040] Hardeners include but are not limited to polyethylene wax (such as AF-29, AF-30), and leveling agents (such as BYK-361, BYK-307) are used as lubricants to improve the lubrication properties of the mixture and ensure that the mixture fluid has a certain fluidity for surface coating. The leveling agent makes the product bond better with the glass, and at the same time makes the surface of the heat-absorbing film smoother and has better adhesion during the reaction process.
[0041] The acrylic acid esters include but are not limited to butyl acrylate, isobornyl acrylate, methyl methacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and tripropylene glycol diacrylate.
[0042] Among them, the photoinitiator includes but is not limited to one or more of 2-isopropylthioxanthone, ethyl 4-dimethylaminobenzoate, benzoin dimethyl ether, 2-hydroxy-2-methyl-1-phenyl-1-propanone, tetraethyl Michler's ketone, benzophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-(4-methylthiophenyl)-2-morpholine-propanone; it is a photoinitiator, which undergoes a cross-linking reaction during irradiation with ultraviolet light or a mercury lamp, so that component A is cured from a monomer to a polymer.
[0043] Example 1, as shown in Figure 2:
[0044] The invention comprises 90.5% of methyl methacrylate, 3.5% of ethyl 4-dimethylaminobenzoate, 3.5% of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1.5% of benzophenone and 1% of polyethylene wax, which are distributed in proportion by mass.
[0045] The coating thickness is 18μm and can be edge-grinded. The indicators after glass tempering are: bow 0.08% (factory standard ≤0.1%), wave 0.03% (factory standard ≤0.05%), particle size 42 particles / 25cm 2 (factory standard ≥40 grains / 25cm 2), stress 96MPa (factory standard ≥90MPa), film adhesion is level 1, pencil hardness is 4H. All the above performances are within the factory standard parameter range.
[0046] In this embodiment, only one type of component A is used with a content of 90.5%, a higher content of component B is 8.5% and there are three types, a lower content of component C is 1%, and only a hardener is used without a leveling agent.
[0047] The advantage is better adhesion.
[0048] The disadvantages are that the paint has a strong odor and the coating hardness is not very good.
[0049] Example 2, as shown in Figure 3:
[0050] The invention comprises 50% of isobornyl acrylate, 44.5% of trimethylolpropane triacrylate, 1% of benzoin dimethyl ether, 3% of tetraethyl Michler's ketone, 1% of polyethylene wax and 0.5% of a leveling agent, which are distributed in proportion by mass.
[0051] The coating thickness is 20μm and can be edge-grinded. The indicators after glass tempering are: bow 0.06% (factory standard ≤0.1%), wave 0.05% (factory standard ≤0.05%), particle size 44 particles / 25cm 2 (factory standard ≥40 grains / 25cm 2 ), stress 102MPa (factory standard ≥90MPa), film adhesion is level 1, pencil hardness is 4H. All the above performances are within the factory standard parameter range.
[0052] The advantage is better adhesion.
[0053] The disadvantage is that the coating hardness is not very good.
[0054] Compared with Example 1, Example 2 increases the content and number of component A, which is 94.5%, the content of component B is 4%, and the content of component C is 1.5%. Among them, the content of the hardener remains unchanged, the leveling agent is added, and the content of component B is reduced. As a result, there is no significant change in adhesion and hardness.
[0055] Example 3, as shown in Figure 4:
[0056] The invention comprises 30% of isobornyl acrylate, 30% of tripropylene glycol diacrylate, 32.5% of trimethylolpropane triacrylate, 2.5% of 2-isopropylthioxanthone, 2.5% of ethyl 4-dimethylaminobenzoate, 1.5% of benzophenone and 1% of polyethylene wax, which are distributed in proportion by mass.
[0057] The coating thickness is 20μm and can be edged. The indicators after glass tempering are: bow 0.06% (factory standard ≤0.1%), wave 0.03% (factory standard ≤0.05%), particle size 45 particles / 25cm 2 (factory standard ≥40 grains / 25cm 2 ), stress 98MPa (factory standard ≥90MPa), film adhesion is level 2, pencil hardness is 5H. All the above performances are within the factory standard parameter range.
[0058] The advantage is that the coating has better hardness.
[0059] The disadvantage is that the coating adhesion is slightly reduced compared to Example 2.
[0060] Compared with Example 2, Example 3 increases the number of component A types to three, with a content of 92.5%, a content of component B of 6.5%, and a content of component C of 1%. Component C uses only 1% of a hardener, and no leveling agent is used. It can be seen that the bow degree remains unchanged, the waviness is reduced, the particle size is basically inconvenient, and the stress is slightly reduced, but the adhesion and hardness of the film are significantly improved.
[0061] Compared with Example 1, the contents of component A, component B, and component C in Example 3 are similar, and the main variable factors are the type and quantity of component A;
[0062] By comparing Example 3 with Example 1 and Example 2, the increase in the number of types of component A can make component A have better copolymerization performance and can make the heat-absorbing film have better hardness.
[0063] By comparing Example 3 with Example 1, under the effect of using the same content of hardener, the number of component A types increases, which can make the heat absorption film body have better hardening.
[0064] Example 4, as shown in Figure 5:
[0065] The invention comprises 20% of methyl methacrylate, 20% of tripropylene glycol diacrylate, 20% of 1,6-hexanediol diacrylate, 32.5% of trimethylolpropane triacrylate, 1.5% of 2-isopropylthioxanthone, 3.5% of ethyl 4-dimethylaminobenzoate, 1% of benzoin dimethyl ether, 0.5% of benzophenone and 1% of polyethylene wax in proportion by mass.
[0066] The coating thickness is 22μm and can be edge-grinded. The indicators after glass tempering are: bow 0.06% (factory standard ≤0.1%), wave 0.04% (factory standard ≤0.05%), particle size 41 particles / 25cm 2 (factory standard ≥40 grains / 25cm 2), stress 92MPa (factory standard ≥90MPa), film adhesion is level 2, pencil hardness is 6H. All the above performances are within the factory standard parameter range.
[0067] The advantages are good coating hardness and no odor.
[0068] The disadvantage is that the coating adhesion is slightly lower than that of Example 2, and the hardness of Example 4 is basically the same as that of Example 3.
[0069] The component ratios of the embodiment are: 92.5% of component A, 6.5% of component B and 1% of polyethylene wax.
[0070] The contents of component A, component B and component C in Example 4 are the same as those in Example 3. The types of component A and component B in Example 4 are increased and the types of components are selected differently, but the hardness and adhesion are not affected.
[0071] Compared with Examples 1 and 2, Examples 3 and 4 both show that, when the hardener is the same, the multi-component component A can achieve improved hardness compared with the single-component component A.
[0072] By comparing Implementation 4 with Implementation 3 and Implementation 2, it can be shown that: when the content ratio of component A is the same or similar, as the types of components of component A increase, the copolymerization effect is better and the hardness of the film can be increased, but the degree of film adhesion is slightly reduced due to the increase in the thickness of the attached film.
[0073] In the above embodiments, component C contains at least 1% of a hardener. It is also shown that the use of a leveling agent can achieve better film adhesion performance, but when the leveling agent is not used, the effect on the adhesion performance is not obvious, so the use of the leveling agent can be omitted. Therefore, component C contains at least a hardener, or may contain a leveling agent.
[0074] In summary, the best comprehensive performance is achieved when the ratio by mass is 92.5% of component A, 6.5% of component B and 1% of polyethylene wax.
[0075] A method for preparing a heat-absorbing film from a heat-absorbing film formula comprises:
[0076] Heat the formula mixture until it becomes fluid;
[0077] coating the heated mixture on the surface of the substrate to form a coating layer;
[0078] The coating layer is dried and hardened by ultraviolet radiation to obtain a heat-absorbing film attached to the surface of the substrate.
[0079] Specifically:
[0080] S1: Pour the coating into the feed barrel of the roller coater according to the formula ratio in advance, turn on the heating switch and heat it to 30-50 degrees Celsius to reduce the viscosity of the coating;
[0081] S2: Start the roller coater and set the roller speed to 10-60 m / min. Adjust the squeeze roller speed to about 50-300 to ensure uniform coating thickness. Adjust the roller coating according to the thickness of the glass.
[0082] S3: Start the LED UV curing lamp, adjust the energy density to 50-100%, and check whether the LED curing lamp is working properly;
[0083] S4: Start the pump lamp, adjust the energy density to 50-100%, and check whether the mercury lamp is working properly;
[0084] S5: Test a piece of glass to be roller coated to check whether the coating thickness, uniformity and curing effect meet the standards. If they meet the standards, formal production can begin.
[0085] Technical indicators: pencil hardness greater than or equal to 4H, adhesion level less than or equal to level 3.
[0086] The glass is sent for FE edge grinding, and the glass is brushed with a hard brush on the edge grinding and washing machine to test the processing resistance of the coating in the production of heat-absorbing film.
[0087] The glass is tempered with parameters close to those for clear glass. If there are dark cracks or coating residue after tempering, the tempering temperature can be slightly increased.
[0088] Application of a heat-absorbing film in the manufacture of coated glass:
[0089] A coated glass comprises a functional coating (typically deposited by vacuum sputtering) on the outer surface of a glass substrate. A heat-absorbing film formulated in this embodiment is applied to the outer surface of the functional coating. The heat-absorbing film is then roll-coated on the surface of the functional coating. The heat-absorbing film can be cured by UV irradiation (i.e., hardened by ultraviolet radiation). The UV curing lamp operates within a wavelength range of 245 to 395 nm, with an optimal range of 280 to 350 nm. After the glass is tempered, the heat-absorbing film can be removed by thermal decomposition or combustion.
[0090] The present invention provides a heat-absorbing film capable of reducing the cost of heat treatment of glass. The film has good heat absorption properties, can reduce the cost of heat treatment of glass, and improve production efficiency. Since the heat-absorbing film is resistant to corrosion, oxidation, and scratches, it has the function of protecting the coating layer on the coated glass from damage caused by external influences.
[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A formula of a heat-absorbing film, characterized in that: A mixture comprising 85% to 98.5% by mass of component A, 1% to 10% by mass of component B and 0.5% to 5% by mass of component C, wherein: The component A comprises one or more of acrylic acid resins; The component B comprises one or more photoinitiators, and the component B undergoes a cross-linking reaction during ultraviolet light irradiation, so that the component A is cured from a monomer to a polymer; The component C comprises one or more of a hardener and a leveling agent.
2. The heat absorbing film formulation according to claim 1, characterized in that: The acrylic acid esters include butyl acrylate, isobornyl acrylate, methyl methacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and tripropylene glycol diacrylate.
3. The heat absorbing film formulation according to claim 2, characterized in that: The photoinitiator comprises 2-isopropylthioxanthone, ethyl 4-dimethylaminobenzoate, dimethyl benzoate, 2-hydroxy-2-methyl-1-phenyl-1-propanone, tetraethyl Michler's ketone, benzophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-(4-methylthiophenyl)-2-morpholine-propanone.
4. The heat absorbing film formulation according to claim 3, characterized in that: The invention comprises 90.5% of methyl methacrylate, 3.5% of ethyl 4-dimethylaminobenzoate, 3.5% of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1.5% of benzophenone and 1% of polyethylene wax in proportion by mass.
5. The heat absorbing film formulation according to claim 3, characterized in that: The invention comprises 50% of isobornyl acrylate, 44.5% of trimethylolpropane triacrylate, 1% of benzoin dimethyl ether, 3% of tetraethyl Michler's ketone, 1% of polyethylene wax and 0.5% of a leveling agent in proportion by mass.
6. The heat absorbing film formulation according to claim 3, characterized in that: The invention comprises 30% of isobornyl acrylate, 30% of tripropylene glycol diacrylate, 32.5% of trimethylolpropane triacrylate, 2.5% of 2-isopropylthioxanthone, 2.5% of ethyl 4-dimethylaminobenzoate, 1.5% of benzophenone and 1% of polyethylene wax in proportion by mass.
7. The heat absorbing film formulation according to claim 3, characterized in that: The invention comprises 20% of methyl methacrylate, 20% of tripropylene glycol diacrylate, 20% of 1,6-hexanediol diacrylate, 32.5% of trimethylolpropane triacrylate, 1.5% of 2-isopropylthioxanthone, 3.5% of ethyl 4-dimethylaminobenzoate, 1% of benzoin dimethyl ether, 0.5% of benzophenone and 1% of polyethylene wax in proportion by mass.
8. The method for preparing a heat-absorbing film according to the formula of a heat-absorbing film according to claim 1, characterized in that: include: heating the formula mixture to a fluid state; coating the heated mixture on the surface of the substrate to form a coating layer; The coating layer is dried and cured by ultraviolet irradiation to obtain a heat-absorbing film attached to the surface of the substrate.
9. Use of the heat-absorbing film according to claim 8 in the manufacture of coated glass.
10. The coated glass according to claim 9, wherein a functional film is coated on the outer side of the glass substrate, characterized in that: A heat absorbing film is coated on the outer surface of the functional mold film layer.
Citation Information
Patent Citations
Hardened optical thin film and preparation method thereof
CN102565885A
Transparent thermal insulation coating material system for glass substrate
CN102942841A
Heat-absorbing coating for toughening coated glass and film forming method of heat-absorbing coating
CN116395980A
Formula, preparation method and application of heat absorption film
CN116496002A
Coated glass protective film and preparation method thereof
CN116925585A