High-molecular-weight liquid hindered phenolic antioxidant and preparation method therefor
Through the method of transesterification reaction and catalyst removal, the problems of small molecular weight and complicated process of liquid hindered phenol antioxidant were solved, and a liquid hindered phenol antioxidant with high molecular weight and good compatibility was obtained, which simplified the process and reduced the cost. .
Patent Information
- Application Number
- PCT/CN2024/083569
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
The existing liquid hindered phenol antioxidant has a small molecular weight, which results in low compatibility with polyurethane materials, polyether polyols and polyester polyols, and is easy to precipitate during application. The production process is complex and the cost is high.
Through the transesterification reaction, 3,5-methyl ester and polypropylene glycol are used as raw materials, and the reaction conditions are controlled for transesterification to obtain a high molecular weight liquid hindered phenol antioxidant. The process is simplified by removing the catalyst and the production cost is reduced.
A liquid hindered phenol antioxidant with large molecular weight and good compatibility was obtained, which simplified the preparation process, reduced raw material and production costs, and improved the compatibility and stability with polyurethane materials, polyester polyols, and polyether polyols. Resistance to migration.
Smart Images

Figure CN2024083569_03102024_PF_FP_ABST
Abstract
Description
A high molecular weight liquid hindered phenol antioxidant and its preparation method Technical Field
[0001] The present invention relates to the technical field of antioxidants, in particular to a high molecular weight liquid hindered phenol antioxidant and a preparation method thereof. Background Art
[0002] Polyurethane materials and their raw materials, polyether polyols and polyester polyols, will cause odor, VOC, or affect the performance of raw materials or products due to aging and degradation during storage and use. Therefore, antioxidants are usually added to polyurethane materials, polyether polyols or polyester polyols to inhibit degradation and maintain their stability.
[0003] There are many types of antioxidants, among which hindered phenol antioxidants are a commonly used primary antioxidant. They are further divided into solid hindered phenol antioxidants and liquid hindered phenol antioxidants. Commonly used hindered phenol antioxidants on the market are mainly solid, such as antioxidants 1010, 1076, 3114, and 330, which are all solid. There are fewer types of liquid antioxidants, but solid hindered phenol antioxidants have problems with mixing and dissolving during use, and the mixing operation is difficult. Currently, the main liquid hindered phenol antioxidant used on the market is 1135 (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate). Although it has a high cost-effectiveness and wide application, its molecular weight is relatively low, and its compatibility with polyurethane materials, polyether polyols, and polyester polyols is low, making it prone to precipitation when used in these products. Existing research has also studied liquid hindered phenol antioxidants, but the resulting antioxidants also have relatively low molecular weights, with a maximum molecular weight not exceeding 700. They have low compatibility with polyurethane materials, polyether polyols, and polyester polyols and are also prone to precipitation. Moreover, existing liquid antioxidants need to undergo rigorous processes such as high temperature and high vacuum to remove excess raw materials after the production reaction is completed, or the reaction process needs to be strictly controlled in order to control the amount of raw materials used and prevent excess raw materials. The existing technology generally has problems such as complex processes, difficult reactions, and high production costs.
[0004] Summary of the Invention
[0005] The purpose of the present invention is to provide a high molecular weight liquid hindered phenol antioxidant and a preparation method thereof in view of the deficiencies in the prior art. The present invention can obtain a liquid hindered phenol antioxidant with a large molecular weight, good compatibility with polyurethane materials, polyester polyols, and polyether polyols, and greater migration resistance. The preparation process is simple and easy to operate, effectively reducing raw material and production costs.
[0006] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a high molecular weight liquid hindered phenol antioxidant, comprising the following steps:
[0007] (1) Transesterification reaction: Add a certain proportion of 3,5-methyl ester and polypropylene glycol to a reaction vessel, add a catalyst, stir, heat, and evacuate, and then carry out transesterification reaction at a certain temperature and vacuum degree. During the reaction, the methanol generated by the reaction is extracted. After the 3,5-methyl ester is completely reacted, the vacuum is broken and the temperature is lowered to obtain a crude product of a liquid hindered phenol antioxidant;
[0008] (2) Removing the catalyst: After removing the catalyst from the crude liquid hindered phenol antioxidant, the liquid hindered phenol antioxidant is obtained.
[0009] Specifically, the transesterification reaction is carried out at a temperature of 130-160° C. and a vacuum degree of 4-5.5 kPa.
[0010] Specifically, removing the catalyst includes adding water to the crude liquid hindered phenol antioxidant to dissolve the catalyst, allowing the catalyst to stand and separate, and removing the water layer; then heating the material, removing the residual moisture in the material under a certain vacuum degree, breaking the vacuum with nitrogen, and cooling to obtain the liquid hindered phenol antioxidant.
[0011] Specifically, the molecular weight of the polypropylene glycol is 400-8000; preferably, the molecular weight of the polypropylene glycol is 400-2000.
[0012] Specifically, the molar ratio of the 3,5-methyl ester to the polypropylene glycol is 1:(0.5-1).
[0013] Specifically, the catalyst is one or more of aluminum chloride, magnesium chloride, ferric chloride, zinc chloride, boron fluoride, potassium fluoride, magnesium acetate, lithium acetate, lithium amide, sodium acetate, potassium acetate, zinc acetate, aluminum acetate, aluminum isopropoxide, and triethanolamine.
[0014] Specifically, the amount of the catalyst used is 0.1%-5% of the mass of the 3,5-methyl ester; preferably, the amount of the catalyst used is 0.5%-2% of the mass of the 3,5-methyl ester.
[0015] On the other hand, the present invention provides a high molecular weight liquid hindered phenol antioxidant, comprising a compound of formula I and a compound of formula II
[0016] Specifically, at 40°C, the kinematic viscosity of the liquid hindered phenol antioxidant is 100-400 mm 2 / s.
[0017] Specifically, the liquid hindered phenol antioxidant is used in polyether polyols, polyester polyols, and polyurethane foams.
[0018] The beneficial effects of the present invention are:
[0019] 1. The present invention uses 3,5-methyl ester and polypropylene glycol as raw materials, and can prepare a liquid hindered phenol antioxidant through an ester exchange reaction. The liquid hindered phenol antioxidant has a large molecular weight, better compatibility with polyurethane raw materials, polyester polyols, and polyether polyols, and is more resistant to migration;
[0020] 2. The present invention uses polypropylene glycol as a raw material, and controls the amount of 3,5-methyl ester and polypropylene glycol to allow the ester group of 3,5-methyl ester to react completely. After the transesterification reaction is completed, the next step is directly carried out to remove the catalyst in the crude liquid hindered phenol antioxidant to obtain the liquid hindered phenol antioxidant. Polypropylene glycol is a raw material for polyurethane, so whether the liquid hindered phenol antioxidant obtained by the present invention contains or contains residual polypropylene glycol has no effect on its application in polyurethane. Therefore, compared with the prior art, the present invention does not require rigorous high-temperature / high-vacuum processes. The reaction process and reaction conditions of the present invention are simple and easy to operate, which greatly simplifies the preparation process of the liquid hindered phenol antioxidant, reduces the reaction difficulty of the liquid antioxidant production, effectively reduces raw material and production costs, and improves product yield;
[0021] 3. Compared with other alcohols, the polypropylene glycol (PPG) used in the present invention not only has a large molecular weight, which is conducive to obtaining a high molecular weight liquid hindered phenol antioxidant, but also has moderate hydrophilicity, and will not affect the compatibility of the antioxidant product with polyurethane raw materials, polyether polyols, and polyester polyols due to excessive hydrophilicity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] FIG1 is an infrared spectrum of the liquid hindered phenol antioxidant obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0023] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, but the scope of implementation of the present invention is not limited thereto.
[0024] 3,5-methyl ester, Chinese chemical name: β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; CAS NO: 6386-38-5; molecular weight: 292.4; chemical structure:
[0025] Polypropylene glycol: PPG; chemical structure:
[0026] Example 1.
[0027] 58.4 g of 3,5-methyl ester and 150 g of PPG (1000 molecular weight) were added to a 500 ml three-necked flask in sequence, and 1 g of zinc chloride catalyst was added, and the stirring and heating reaction was started.
[0028] The temperature was raised to 130-140°C and the reaction was continued under a vacuum of 4 kPa for 3 hours to remove the by-product methanol until no significant distillate was produced. A total of 6.2 g of by-product methanol was collected by cold trapping.
[0029] The temperature was lowered to room temperature, and the reaction of 3,5-methyl ester was confirmed to be complete by gas chromatography.
[0030] 20 g of deionized water was added, and the mixture was allowed to stand for separation, and the water layer was removed.
[0031] The material was heated to 120°C and placed under a vacuum of 1 kPa for 1 hour to remove the remaining water. The vacuum was broken with nitrogen and the temperature was lowered to obtain 199.5 g of a colorless, transparent liquid. Its kinematic viscosity (40°C) was 250 mm 2 / s.
[0032] Example 2.
[0033] 48.7 g of 3,5-methyl ester and 150 g of PPG (1000 molecular weight) were added to a 500 ml three-necked flask in sequence, and 0.9 g of zinc chloride catalyst was added, and the stirring and heating reaction was started.
[0034] The temperature was raised to 140-150°C and the reaction was continued under a vacuum of 5 kPa for 3 hours to remove the by-product methanol until no significant distillate was produced. A total of 5.2 g of by-product methanol was collected by cold trapping.
[0035] The temperature was lowered to room temperature, and the reaction of 3,5-methyl ester was confirmed to be complete by gas chromatography.
[0036] 20 g of deionized water was added, and the mixture was allowed to stand for separation, and the water layer was removed.
[0037] The material was heated to 120°C and placed under a vacuum of 1 kPa for 1 hour to remove the remaining water. The vacuum was broken with nitrogen and the temperature was lowered to obtain 190.7 g of a colorless, transparent liquid. Its kinematic viscosity (40°C) was 200 mm 2 / s.
[0038] Example 3.
[0039] 116.8 g of 3,5-methyl ester and 120 g of PPG (400 molecular weight) were added to a 500 ml three-necked flask in sequence, and 2 g of aluminum isopropoxide catalyst was added, and the reaction was started by stirring and heating.
[0040] The temperature was raised to 150-160°C and the reaction was continued under a vacuum of 5.5 kPa for 3 hours to remove the by-product methanol until no significant distillate was produced. A total of 12.5 g of by-product methanol was collected by cold trapping.
[0041] The temperature was lowered to room temperature, and the reaction of 3,5-methyl ester was confirmed to be complete by gas chromatography.
[0042] 20 g of deionized water was added, and the mixture was allowed to stand for separation, and the water layer was removed.
[0043] The material was heated to 120°C and placed under a vacuum of 1 kPa for 1 hour to remove the remaining water. The vacuum was broken with nitrogen and the temperature was lowered to obtain 221.6 g of a colorless, transparent liquid. Its kinematic viscosity (40°C) was 350 mm 2 / s.
[0044] The liquid hindered phenol antioxidants obtained in Examples 1, 2, and 3 were used to stabilize a common polyether polyol (molecular weight 3000). This antioxidant exhibited excellent compatibility with the polyether polyol, and its oxidation induction temperature (OIT) was measured by DSC. For comparison, common antioxidants 1076 and 1135 were mixed uniformly with a common polyether polyol (molecular weight 3000), and their OIT was measured by DSC. The test results are shown in Table 1 below:
[0045] Table 1:
[0046] FIG1 is an infrared spectrum of Example 3 of the present invention. It can be seen from the spectrum that at 1732 cm -1 An absorption peak appears at , indicating that an ester exchange reaction occurs between 3,5-methyl ester and polypropylene glycol in the present invention.
[0047] In the present invention, when the molecular weight of the polypropylene glycol (PPG) used is 400, the molecular weight of the obtained liquid hindered phenol antioxidant is within the range of 674-949; when the molecular weight of the polypropylene glycol (PPG) used is 1000, the molecular weight of the obtained liquid hindered phenol antioxidant is within the range of 1274-1549; when the molecular weight of the polypropylene glycol (PPG) used is 2000, the molecular weight of the obtained liquid hindered phenol antioxidant is within the range of 2274-2549; and so on, when the molecular weight of the polypropylene glycol used is higher, the molecular weight of the obtained liquid hindered phenol antioxidant will also be higher. It can be seen from this that the present invention can obtain a liquid hindered phenol antioxidant with a higher molecular weight. The liquid hindered phenol antioxidant of the present invention can have better compatibility with polyurethane raw materials, polyester polyols, and polyether polyols, is more resistant to migration, and the liquid antioxidant is easier to mix and dissolve.
[0048] From the test results in Table 1 above, it can be seen that the liquid hindered phenol antioxidant obtained by the present invention can increase the oxidation resistance temperature of the raw material, making the raw material have better stability; compared with Examples 1, 2, and 3 of the present invention and Comparative Examples 1 and 2 (commonly used solid antioxidant 1076 and liquid antioxidant 1135), it can be seen that the oxidation induction temperature (OIT) of the present invention is slightly better than that of the commonly used antioxidants 1076 and 1135. In addition, the hindered phenol antioxidant of the present invention is a liquid, and its kinematic viscosity at 40°C is 100-400mm 2 / s, which is not only convenient for pumping and use of the product, but also has good compatibility with polyurethane raw materials, polyester polyols, and polyether polyols compared to existing antioxidants, and is easier to mix and dissolve with the raw materials.
[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a high molecular weight liquid hindered phenol antioxidant, characterized in that: The following steps are involved: (1) Transesterification reaction: a certain proportion of 3,5-methyl ester and polypropylene glycol are added to a reaction vessel, and a catalyst is added. After stirring, heating and vacuuming, a transesterification reaction is carried out at a certain temperature and vacuum degree. During the reaction, the methanol generated by the reaction is extracted. After the 3,5-methyl ester is completely reacted, the vacuum is broken and the temperature is lowered to obtain a crude product of a liquid hindered phenol antioxidant. (2) Removing the catalyst: After removing the catalyst from the crude liquid hindered phenol antioxidant, the liquid hindered phenol antioxidant is obtained.
2. The method for preparing a high molecular weight liquid hindered phenol antioxidant according to claim 1, characterized in that: The transesterification reaction is carried out at a temperature of 130-160°C and a vacuum degree of 4-5.5 kPa.
3. The method for preparing a high molecular weight liquid hindered phenol antioxidant according to claim 1, characterized in that: The catalyst removal process includes adding water to the crude liquid hindered phenol antioxidant to dissolve the catalyst, allowing the catalyst to stand for stratification, and removing the water layer; then heating the material, removing the residual water in the material under a certain vacuum degree, breaking the vacuum with nitrogen, and cooling the material to obtain the liquid hindered phenol antioxidant.
4. The method for preparing a high molecular weight liquid hindered phenol antioxidant according to claim 1, characterized in that: The molecular weight of the polypropylene glycol is 400-8000.
5. The method for preparing a high molecular weight liquid hindered phenol antioxidant according to claim 1, characterized in that: The molar ratio of the 3,5-methyl ester to the polypropylene glycol is 1:(0.5-1).
6. The method for preparing a high molecular weight liquid hindered phenol antioxidant according to claim 1, characterized in that: The catalyst is one or more of aluminum chloride, magnesium chloride, ferric chloride, zinc chloride, boron fluoride, potassium fluoride, magnesium acetate, lithium acetate, lithium amide, sodium acetate, potassium acetate, zinc acetate, aluminum acetate, aluminum isopropoxide, and triethanolamine.
7. The method for preparing a high molecular weight liquid hindered phenol antioxidant according to claim 1, characterized in that: The amount of the catalyst used is 0.1%-5% of the mass of the 3,5-methyl ester.
8. A high molecular weight liquid hindered phenol antioxidant obtained by the preparation method according to claims 1 to 7, characterized in that: Including compounds of structural formula I and compounds of structural formula II, 9. A high molecular weight liquid hindered phenol antioxidant according to claim 8, characterized in that: The liquid hindered phenol antioxidant is used in polyether polyols, polyester polyols and polyurethane foams.
10. A high molecular weight liquid hindered phenol antioxidant according to claim 8, characterized in that: At 40°C, the kinematic viscosity of the liquid hindered phenol antioxidant is 100-400 mm 2 / s.
Citation Information
Patent Citations
Hindered phenolic antioxidant having stellate molecular structure, and synthesis method and application thereof
CN110272343A
High-molecular-weight liquid hindered phenol antioxidant and preparation method thereof
CN116284742A
Mixtures containing isocyanate stabilisers of the hindered phenol type with a high molecular weight
CN1806002A
Mixtures containing polytetrahydrofuran and a stabiliser
CN1906241A
Novel liquid phenolic antioxidants
TW406127B
Cited By