Spherical catalyst for olefin polymerization
By using magnesium compounds to react with organic compounds with multi-polar functional groups and active hydrogen to form spherical catalysts in olefin polymerization, the problems of easily broken carriers and complex processes are solved, high mechanical strength and polymerization performance are improved, and high activity is obtained and low fines polymers.
Patent Information
- Application Number
- PCT/CN2024/083778
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
The existing olefin polymerization catalyst carrier is easily broken during the titanium loading process, the process is complicated, and the polymerization performance is poor, resulting in irregular morphology and low packing density of the polymer.
In the presence of polyvinylpyrrolidone and multipolar functional compounds, the magnesium compound reacts with an organic compound containing active hydrogen to form a complex, which is then reacted with an epoxy compound and washed with an inert alkane solvent to obtain a magnesium compound spherical carrier, which is then reacted with a titanium compound The reaction forms a spherical catalyst, which is dispersed and washed by a low-temperature inert alkane solvent to finally obtain a spherical catalyst with high mechanical strength.
The mechanical strength and polymerization performance of the catalyst are improved, the preparation process is simplified, and energy consumption is reduced. The obtained polymer has good morphology and low fine powder content, especially in olefin polymerization, with high activity and good hydrogen regulation sensitivity.
Smart Images

Figure CN2024083778_03102024_PF_FP_ABST
Abstract
Description
Spherical catalysts for olefin polymerization
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent application No. 202310325605.7 filed on March 27, 2023, the contents of which are incorporated herein by reference. Technical Field
[0003] The invention belongs to the field of olefin polymerization catalysts, and particularly relates to a spherical catalyst for olefin polymerization reactions. Background Art
[0004] To produce spherical polyethylene with a regular morphology, high bulk density, and low fine powder content, a spherical carrier is often prepared based on the "complex effect," and titanium tetrachloride is then loaded onto the carrier to produce a spherical catalyst. Currently, the mainstream spherical catalysts are mostly supported by magnesium chloride alcoholate or magnesium ethoxide.
[0005] CN101544710A discloses a method for preparing an alcoholate from a ternary component of magnesium halide, alcohol, and polyether. The ternary components are reacted at high temperature to form a molten mixture, which is then rapidly cooled and formed in a low-temperature inert medium. The resulting carrier exhibits good dispersibility, good particle morphology, and a small particle size. The supported catalyst exhibits high activity in olefin polymerization, particularly propylene polymerization, and the resulting polymer has a good morphology and low fine powder content. However, the above-mentioned preparation process is relatively complex and energy-intensive. Furthermore, to prevent the catalyst prepared from the alcoholate from fragmenting during polymerization, a dealcoholization step is required, further increasing energy consumption.
[0006] CN102040680A discloses a novel spherical alkoxymagnesium support and its preparation method, which is reacted with titanium tetrachloride in the presence of an internal electron donor to produce a catalyst. This method does not require quenching to precipitate the support, is relatively simple to operate, and exhibits high activity in propylene polymerization. While maintaining high polymerization activity and directional ability, it shows good hydrogen sensitivity, and the polymer has high stereoregularity at a high melt index. However, the support has poor mechanical strength and is prone to breakage during the highly exothermic titanium loading process. Moreover, the resulting polypropylene obtained from propylene polymerization has a low bulk density.
[0007] CN1563112A discloses a method for preparing a spherical MgCl2-alcohol-organic complexing agent supported polyolefin catalyst. The internal electron donor diisobutyl phthalate (DIBP) is introduced into the carrier synthesis in situ, so that the obtained carrier has high mechanical strength. Titanium tetrachloride is then added to this basis to obtain a spherical catalyst. However, the obtained catalyst particle size is large and the distribution is wide (D 50 : 70-200 μm), and the propylene polymerization activity is low.
[0008] In summary, existing olefin polymerization catalyst supports and their preparation methods have problems such as the support being easily broken during the titanium loading process, the process being complicated, and the polymerization performance being poor.
[0009] Summary of the Invention
[0010] In order to improve the mechanical strength of the carrier, simplify the carrier preparation process, save energy, and achieve the purpose of increasing the commercial value of the olefin polymerization catalyst, the present invention provides a spherical catalyst for olefin polymerization reaction, which is prepared by the following steps:
[0011] (1) in the presence of polyvinyl pyrrolidone and a multipolar functional group compound, reacting a magnesium compound with an organic compound containing active hydrogen at 30-160° C. to form a complex solution;
[0012] (2) reacting the complex solution with an epoxy compound to precipitate a solid compound;
[0013] The epoxy compound is shown in the general formula (I):
[0014] In the general formula (I), R2 and R3 are each independently selected from hydrogen, a C1-C5 linear or branched alkyl group, wherein the hydrogen on the alkyl group may not be substituted, or may be substituted with a halogen atom X in an optional number;
[0015] (3) washing the solid compound obtained in step (2) with an inert alkane solvent to obtain a spherical magnesium compound carrier;
[0016] (4) dispersing the magnesium compound spherical carrier obtained in step (3) in a high-viscosity inert hydrocarbon solvent, and adding a titanium compound at low temperature to react to obtain an intermediate product;
[0017] The titanium compound is shown in the general formula (II):
[0018] R1', R2', R3', R4' in the general formula (II) are each independently selected from C1-C 10 Alkyl;
[0019] (5) dispersing the intermediate product in a high-viscosity inert hydrocarbon solvent, adding titanium tetrachloride to react with the intermediate product at low temperature, and washing the resulting solid product with an inert alkane solvent to obtain a spherical catalyst;
[0020] Wherein, the multipolar functional group compound described in step (1) is a compound having the general formula C n H 2n O n A compound with multipolar functional groups, wherein n is 4-8;
[0021] The organic compound containing active hydrogen in step (1) is a compound of the general formula R(OH) m A compound or a mixture of compounds shown in the formula, wherein R is C1-C 20 Hydrocarbon group, m ≥ 1;
[0022] The inert alkane solvent in step (3) is a solvent of the general formula C n H 2n+2 A mixture of one or more compounds shown, wherein n ≥ 5;
[0023] The high-viscosity inert hydrocarbon solvents described in step (4) and step (5) are independently alkyl-substituted cycloalkanes and alkyl-substituted aromatic hydrocarbons.
[0024] In the present invention, the polyvinyl pyrrolidone can be conventional polyvinyl pyrrolidone in the art, which can be prepared according to the method in the literature or directly purchased. The weight average molecular weight of the polyvinyl pyrrolidone can be 3000-1300000 g / mol.
[0025] As a preferred embodiment of the present invention, per mole of magnesium, the amount of the polyvinyl pyrrolidone is 0.001-0.1 mole, the amount of the multipolar functional group compound is 0.002-0.2 mole, the amount of the organic compound containing active hydrogen is 2-20 moles, the amount of the epoxy compound is 1-30 moles, the amount of the titanium compound is 0.05-1.5 moles, and the amount of the titanium tetrachloride is 0.5-15 moles.
[0026] In the present invention, the amount of the polyvinyl pyrrolidone per mole of magnesium (magnesium compound) can be 0.001 mole, 0.003 mole, 0.005 mole, 0.007 mole, 0.008 mole, 0.01 mole, 0.02 mole, 0.04 mole, 0.06 mole, 0.08 mole, 0.1 mole, and a range consisting of any two of the above. Preferably, the amount of the polyvinyl pyrrolidone per mole of magnesium is 0.001-0.06 mole.
[0027] In the present invention, the amount of the multipolar functional group compound used per mole of magnesium (magnesium compound) can be 0.002 mol, 0.003 mol, 0.005 mol, 0.007 mol, 0.008 mol, 0.01 mol, 0.02 mol, 0.04 mol, 0.06 mol, 0.08 mol, 0.1 mol, 0.2 mol, or ranges consisting of any two of the foregoing. Preferably, the amount of the multipolar functional group compound used per mole of magnesium is 0.002-0.08 mol.
[0028] In the present invention, the amount of the organic compound containing active hydrogen can be 2 mol, 4 mol, 6 mol, 8 mol, 10 mol, 12 mol, 14 mol, 16 mol, 18 mol, 20 mol, or any range consisting of any two of the above, per mol of magnesium (magnesium compound). Preferably, the amount of the organic compound containing active hydrogen is 4-16 mol per mol of magnesium.
[0029] In the present invention, the amount of the epoxy compound used per mole of magnesium (magnesium compound) can be 1 mole, 4 moles, 6 moles, 8 moles, 10 moles, 12 moles, 14 moles, 16 moles, 18 moles, 20 moles, 22 moles, 24 moles, 26 moles, 28 moles, 30 moles, or ranges consisting of any two of the foregoing. Preferably, the amount of the epoxy compound used per mole of magnesium is 1-18 moles.
[0030] In the present invention, the amount of the titanium compound used per mole of magnesium (spherical carrier) can be 0.05 mol, 0.08 mol, 0.1 mol, 0.2 mol, 0.3 mol, 0.4 mol, 0.5 mol, 0.6 mol, 0.8 mol, 1 mol, 1.2 mol, 1.4 mol, 1.5 mol, or a range consisting of any two of the above. Preferably, the amount of the titanium compound used per mole of magnesium is 0.08-0.8 mol.
[0031] In the present invention, the amount of the titanium tetrachloride can be 0.5 mole, 1 mole, 4 moles, 6 moles, 8 moles, 10 moles, 12 moles, 14 moles, 15 moles, and the range consisting of any two of the above points per mole of magnesium. The amount of the titanium tetrachloride is a conventional amount in this area, and those skilled in the art can make conventional selections as needed. For example, the amount of the titanium tetrachloride can be 0.5-40 moles per mole of magnesium (intermediate product). Those skilled in the art can select a less amount of titanium tetrachloride or a more amount of titanium tetrachloride according to conventional operations in this area.
[0032] As a preferred embodiment of the present invention, in step (4), the amount of the high-viscosity inert hydrocarbon solvent used is 1000-6000 mL (for example, 1000 mL, 2000 mL, 3000 mL, 4000 mL, 5000 mL, 6000 mL, and a range consisting of any two of the above points) per mole of magnesium (spherical carrier).
[0033] As a preferred embodiment of the present invention, in step (5), the amount of the high-viscosity inert hydrocarbon solvent used is 3000-12000 mL (for example, 3000 mL, 4000 mL, 5000 mL, 6000 mL, 7000 mL, 8000 mL, 9000 mL, 10000 mL, 11000 mL, 12000 mL, and a range consisting of any two of the above points) per mole of magnesium (intermediate product).
[0034] As a preferred embodiment of the present invention, the multipolar functional group compound in step (1) is one of glucose, fructose, sorbose, galactose, cyclohexanehexol, ribose or a mixture of multiple thereof.
[0035] As a preferred embodiment of the present invention, the magnesium compound in step (1) is a mixture of one or more of magnesium halide, phenoxymagnesium chloride, isopropoxymagnesium chloride, and butoxymagnesium chloride. The magnesium halide may be magnesium dichloride, magnesium dibromide, or the like.
[0036] As a preferred embodiment of the present invention, the R(OH) m A mixture of two or three selected from methanol, ethanol, propanol, n-butanol, isobutanol, amyl alcohol, isopentanol, n-hexanol, 2-ethylhexanol, isooctyl alcohol, ethylene glycol, propylene glycol, and glycerol.
[0037] As a preferred embodiment of the present invention, the R(OH) m is selected from ethanol, n-butanol and isooctyl alcohol; more preferably, the molar ratio of ethanol, n-butanol and isooctyl alcohol is 0.1-8:0.1-12:1.
[0038] As a preferred embodiment of the present invention, the epoxy compound in step (2) is ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epichlorohydrin, epibromohydrin or epibromobutylene oxide.
[0039] As a preferred embodiment of the present invention, the inert alkane solvent in step (3) is selected from a mixture of one or more of n-hexane, cyclohexane, n-heptane, n-octane and n-nonane.
[0040] As a preferred embodiment of the present invention, the high-viscosity inert hydrocarbon solvents in step (4) and step (5) are independently a mixture of one or more of paraffin oil, white oil, methyl silicone oil, and vaseline oil.
[0041] The methyl silicone oil can be a methyl silicone oil that is commonly available in the art, for example, a methyl silicone oil that can be purchased, such as a commercially available methyl silicone oil (with a kinematic viscosity of 50±5 mm2 / s at 25°C). Similarly, the white oil can be a white oil that is commonly available in the art, for example, No. 32 white oil (with a kinematic viscosity of 28.8-35.2 mm2 / s at 40°C). 2 / s), No. 68 white oil, No. 100 white oil.
[0042] As a preferred embodiment of the present invention, the low temperature in step (4) and step (5) is independently -40 to 0°C, preferably -20 to -10°C.
[0043] As a preferred embodiment of the present invention, the preparation processes of the carrier and the catalyst are both carried out under a nitrogen atmosphere.
[0044] The present invention also provides an application of a polymerization catalyst system comprising the aforementioned spherical catalyst component in α-olefin polymerization reaction.
[0045] The general formula of an α-olefin is CH2=CHR1. Preferably, R1 is hydrogen or an alkyl group of 1 to 12 carbon atoms. The α-olefin polymerization reaction may be an oligomerization reaction of an α-olefin or a copolymerization reaction using an α-olefin as one of the polymerization monomers. For example, the α-olefin may be at least one of ethylene, propylene, butene, pentene, and hexene.
[0046] According to the present invention, the conditions for the α-olefin polymerization reaction can be conventional polymerization conditions in the art. For example, the conditions for the α-olefin polymerization reaction can be: polymerization temperature of 50-150° C., polymerization time of 0.08-10 h, and polymerization pressure of 0.3-50 bar.
[0047] In the present invention, 1 bar = 0.1 MPa, and pressure refers to gauge pressure.
[0048] According to the present invention, the cocatalyst used in the α-olefin polymerization reaction can be a cocatalyst commonly used in the art, for example, the cocatalyst is AlR' p X 3-p , wherein p can be an integer of 1-3, R' can be a C1-C10 alkyl group, and X can be a halogen atom; specifically, the co-catalyst can be at least one of trimethylaluminum, triethylaluminum, diethylaluminum chloride, triethylbutylaluminum and trioctylaluminum.
[0049] According to the present invention, the amount of the co-catalyst may be a conventional amount in the art. For example, the molar ratio of the spherical catalyst calculated as Ti to the co-catalyst calculated as Al may be 0.0005-1, or 0.001-0.05.
[0050] According to the present invention, the solvent used in the polymerization process may be a conventional solvent in the art, such as an alkane (eg, n-heptane), an aromatic hydrocarbon, or the like.
[0051] The catalyst provided by the present invention has a simple and feasible preparation process, and the resulting spherical catalyst has a good morphology and controlled size. When used in olefin polymerization, especially ethylene polymerization, the catalyst exhibits high activity, good hydrogen modulation sensitivity, and a high 1-hexene insertion rate. Furthermore, the polymer particles obtained from the catalyst have a low fines content. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] FIG1 is a spherical morphology diagram of the catalyst of Example 1;
[0053] FIG2 is a diagram showing the catalyst particle size distribution of Example 1;
[0054] FIG3 is a spherical morphology of polymer particles of Example 1;
[0055] FIG4 is a particle size distribution diagram of the polymer particles of Example 1;
[0056] FIG5 is a sphericity distribution diagram of the polymer particles of Example 1;
[0057] FIG6 is a diagram showing the catalyst particle size distribution of Example 4. DETAILED DESCRIPTION
[0058] The present invention will be further described and illustrated below in conjunction with specific embodiments. The embodiments are merely illustrative of the present disclosure and do not limit its scope. The technical features of the various embodiments of the present invention may be combined accordingly, provided that there is no conflict between them.
[0059] Test method:
[0060] 1. Determine the Ti and Mg contents of the catalyst or support using an inductively coupled plasma atomic emission spectrometer (ICP-AES). The specific testing steps include: weighing approximately 10-20 mg of catalyst or support into a clean glass vial equipped with a small magnet, adding 10 ml of dilute sulfuric acid solution (1.0 mol / L), and stirring the mixture on a stirring device for at least 8 hours. Filter the mixed solution through a filter needle into a glass vial, and remove an equal amount of the catalyst solution or support solution to measure the Ti and Mg contents of the catalyst or support in the test instrument.
[0061] 2. The catalyst morphology was observed using a scanning electron microscope (SU8010, USA) and the particle size and particle size distribution of the catalyst were measured using Image J software. The specific test steps included: applying double-sided conductive adhesive to the electron microscope stage, transferring the sample to a glove box, sprinkling carrier particles, blowing off unattached particles on the surface with an ear bulb, and then transferring the sample to the scanning electron microscope sample chamber for imaging; opening the SEM image with Image J software, and performing the Find edge—Threshold (8-bit)—Fill holes—Watershed operations in sequence, with the sphericity limit set to 0.5-1.0 and the area statistical range limited to 4-10000μm. 2 ; Ten SEM images were taken for each sample, and the particle size data were summarized and imported into Origin software to calculate D10, D50, D90 and Span values.
[0062] 3. The weight average molecular weight (M) of the polymer was determined by high temperature gel permeation chromatography (HT-GPC, PL-GPC-220, UK). w ) and molecular weight distribution (MWD). The specific testing steps included: the mobile phase was 1,2,4-trichlorobenzene (HPLC grade, Honeywell, USA) at a flow rate of 1.0 mL / min and a temperature of 150°C; and the molecular weight standard curve was calibrated using extremely narrow-distribution polystyrene (PS) as the standard sample.
[0063] 4. Determine the comonomer content of the polymer using a nuclear magnetic resonance spectrometer (Bruker AC-80, 400MHz). The specific test steps include: before testing, dissolve the polymer in deuterated o-dichlorobenzene at a test temperature of 120°C, and analyze the comonomer content of the polymer sample according to the nuclear magnetic resonance C spectrum ( 13 C NMR) to calculate the comonomer content (i.e., the comonomer insertion rate) of the polymer.
[0064] 5. The micromorphology of the polymer particles was observed using a scanning electron microscope (SU3500 / SU8010, USA). The specific testing steps included applying double-sided conductive tape to the microscope stage, sprinkling the polymer particles, and then blowing away any unattached particles with an ear bulb. The samples were then transferred to the SEM chamber for imaging. Prior to SEM testing, the sample was treated with Pt spray for 60 seconds to improve conductivity.
[0065] 6. The apparent density of the polymer particles is measured according to ASTM-D1895.
[0066] 7. The sphericity and particle size distribution of the polymer were determined using the BT-2900LD Dynamic Image Particle Size and Shape Analysis System (dry method). The specific testing steps include: approximately 20g of sample is placed in a storage funnel. The particles are dispersed using an electromagnetic vibrating feeder and a distribution chute, and then allowed to freely fall at the end of the distribution chute. A high-speed camera captures images of the particles as they fall, and these images are analyzed by a computer to determine the average particle size and shape data.
[0067] Taking magnesium halide MgX2 as an example, the preparation route of the spherical catalyst of the present invention is as follows:
[0068] 1. Preparation of Spherical Carriers
[0069] (a) Under nitrogen protection, polyvinyl pyrrolidone and multipolar functional group compound C n H 2n O n Under the presence of , magnesium halide MgX2 and an alcohol mixture are reacted at 30-160 ° C to form a complex solution;
[0070] (b) reacting the above complex solution with an alkylene oxide compound represented by formula (I) at 30-160° C. to produce a solid adduct, and washing the solid adduct obtained in (2) with an inert alkane solvent to obtain a magnesium halide spherical carrier.
[0071] In the general formula (I), R2 and R3 are the same or different and are hydrogen or a C1-C5 linear or branched alkyl group, wherein the hydrogen on the alkyl group is optionally substituted by a halogen atom X;
[0072] The general formula is C n H 2n O n The multipolar functional group compound is one of glucose, fructose, sorbose, galactose, cyclohexanehexol, ribose or a mixture of multiple thereof.
[0073] The epoxy compound described in general formula (I) is a mixture of one or more of ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epichlorobutane, epibromohydrin or epibromobutane.
[0074] 2. Preparation of spherical catalysts
[0075] The spherical carrier is dispersed in a high-viscosity inert hydrocarbon solvent, and a titanium compound is added at low temperature to react to obtain an intermediate product; the intermediate product is dispersed in a high-viscosity inert hydrocarbon solvent, and titanium tetrachloride is added at low temperature to react with it, and the solid product obtained is washed with an inert alkane solvent to obtain a spherical catalyst.
[0076] The titanium compound is shown in the general formula (II):
[0077] In the general formula (II), R1', R2', R3', and R4' are the same or different and are C1-C 10 of alkyl.
[0078] The high-viscosity inert hydrocarbon solvent is a mixture of one or more of decane, paraffin oil, white oil, methyl silicone oil, and vaseline oil.
[0079] Calculated per mole of magnesium, the amount of the polyvinyl pyrrolidone is 0.001-0.1 mole, the amount of the multipolar functional group compound is 0.002-0.2 mole, the amount of the mixed alcohol is 2-20 moles, the amount of the epoxy compound is 1-30 moles, the amount of the titanium compound is 0.05-1.5 moles, and the amount of the titanium tetrachloride is 0.5-15 moles.
[0080] The present invention will be further described below by way of examples.
[0081] The weight average molecular weight of polyvinylpyrrolidone (PVP) is 100,000-150,000 g / mol;
[0082] The kinematic viscosity of methyl silicone oil at 25°C is 50±5mm 2 / s;
[0083] The white oil is No. 32 white oil, and the kinematic viscosity of No. 32 white oil at 40°C is 28.8-35.2mm 2 / s.
[0084] Example 1
[0085] (1) Vector preparation
[0086] Under N2 protection, 10g MgCl2, 160mg galactose, 1.6g PVP (0.0002mol), and a certain amount of mixed alcohol (MgCl2: ethanol: n-butanol: isooctyl alcohol (molar ratio) = 1:3:7:2) were added to a 250ml three-necked flask in sequence. The stirring speed was 600rpm, and the temperature was raised to 70°C. After the solid was completely dissolved, the reaction was continued for 1h. 30ml epichlorohydrin (0.384mol) was slowly added dropwise via a microsyringe pump. A white to light yellow solid gradually precipitated during the addition. After 1h of addition, the reaction was allowed to continue for another 1h, and the reaction was stopped. After standing, the supernatant was removed, washed with n-hexane three times, and vacuum dried at room temperature for 4h to obtain the carrier (white powder).
[0087] (2) Catalyst preparation
[0088] 3g of the obtained support (Mg content in the support was 0.0221mol) was dispersed in a 100ml three-necked flask containing 50ml of methyl silicone oil. Under nitrogen, the flask was placed in a constant temperature bath at -20°C and mechanically stirred (120rpm) to ensure uniform dispersion of the support. After stirring for 30 minutes and the system cooled to a relatively low temperature, 0.75ml of tetrabutyl titanate (0.0022mol) was added dropwise using a microsyringe pump over 1 hour. After the addition was complete, the system was heated to 60°C at a heating rate of 0.5°C / min while stirring and the reaction was continued for 2 hours. After the reaction was completed, the solution was allowed to stand and the supernatant was removed. The solution was washed three times with n-hexane and then dried under vacuum at room temperature for 4 hours to obtain the pretreated support (i.e., the intermediate product).
[0089] Take 1g of the obtained pretreated support (the Mg content in the pretreated support is 0.0089mol) and disperse it in a 100ml three-necked flask filled with 50ml of methyl silicone oil; under nitrogen protection, place the flask in a constant temperature bath at -15℃ and stir mechanically (60rpm); after stirring for 30min until the system cools down to a lower temperature, add 12.5ml of TiCl4 (0.1138 mol) was added for 3 hours; after the addition was completed, the mixture was heated to 90°C with stirring at a heating rate of 0.5°C / min and the reaction was continued for 2 hours; the methyl silicone oil and unreacted TiCl4 were filtered out, and the mixture was washed three times with 300 ml of n-hexane; the mixture was placed in a constant temperature bath at -15°C for 30 minutes, and the above steps of TiCl4 addition, heating, reaction, and washing were repeated; after the washing was completed, the catalyst was vacuum dried at room temperature for 4 hours to obtain a spherical catalyst with a titanium content of 9.1 wt%. The catalyst had a spherical morphology as shown in Figure 1, an average particle size (D50) of 42.74 μm, and a uniform particle size distribution as shown in Figure 2.
[0090] (3) Ethylene polymerization
[0091] The spherical catalyst prepared above was used to carry out ethylene polymerization experiments in a 1L reactor; the solvent was n-heptane, the reaction temperature was 70°C, the spherical catalyst and the co-catalyst triethylaluminum (TEA) were added according to an Al / Ti molar ratio of 100, the polymerization time was 1 h, and the polymerization pressure was 4 bar.
[0092] The polymerization activity is 10134gPE / gCat, and the weight average molecular weight of the polymerization product (M w ) is 100×10 4 g / mol, the molecular weight distribution (MWD) is 4.0, and the apparent density of the polymer particles is 0.31 g / cm 3 The polymer particles have a relatively regular spherical morphology as shown in Figure 3, an average particle size of 1040 μm, and a uniform particle size distribution as shown in Figure 4. The sphericity results are shown in Figure 5, with an average sphericity of 0.911.
[0093] Example 2
[0094] The preparation of the support and catalyst was the same as in Example 1. The ethylene polymerization was carried out in the same manner as in Example 1 except that 10 mL of 1-hexene was added. The polymerization activity was 16214 g PE / g Cat, which was 60% higher than that in Example 1. The 1-hexene insertion rate in the polymer product was 11.4 mol‰, and the M w 82.9×10 4 g / mol, MWD was 5.7, and the other characterization results of the polymer products were similar to those in Example 1. The apparent density of the polymer particles was 0.30 g / cm 3 The average particle size is 996 μm and the average sphericity is 0.909.
[0095] Example 3
[0096] The preparation of the support and catalyst was the same as in Example 1. During the ethylene polymerization, hydrogen was introduced at a pressure of 3 bar and an ethylene pressure of 4 bar, resulting in a total polymerization pressure of 7 bar. The remaining ethylene polymerization conditions were the same as in Example 1. The polymerization activity decreased by 80% compared to that in Example 1, and the weight-average molecular weight of the polymer product was reduced to 17% (16.76×10 4 g / mol), the hydrogen adjustment effect was significant, and the characterization results of the other polymer products were close to those in Example 1. The MWD of the polymer product was 4.6, and the apparent density of the polymer particles was 0.38 g / cm 3 The average particle size is 897 μm and the average sphericity is 0.913.
[0097] Comparative Example 1
[0098] The preparation of the carrier was the same as in Example 1 except that galactose was not added. The preparation of the catalyst and the ethylene polymerization were the same as in Example 1. The catalyst particle size distribution was uneven, with a tail in the direction of small particle size (about 1 μm). The results are shown in Figure 6. The polymerization activity was 5000 gPE / gCat. The product contained a lot of fine powder and had a low sphericity. The M of the polymer product was w 96×10 4 g / mol, MWD is 8.6, and the apparent density of the polymer particles is 0.27 g / cm 3 The average particle size is 765 μm and the average sphericity is 0.798.
[0099] Example 4
[0100] The preparation of the carrier was the same as in Example 1 except that galactose was replaced by fructose. The preparation of the catalyst and the ethylene polymerization were the same as in Example 1. The characterization results of the catalyst and the polymer product were similar to those in Example 1. The polymerization activity was 13764 gPE / gCat, and the M w 118×104 g / mol, MWD is 3.7, and the apparent density of the polymer particles is 0.33 g / cm 3 The average particle size is 1124 μm and the average sphericity is 0.912.
[0101] Example 5
[0102] The preparation of the catalyst was the same as in Example 1 except that the methyl silicone oil was replaced with white oil. The preparation of the carrier and the ethylene polymerization were the same as in Example 1. The characterization results of the catalyst and the polymer product were similar to those in Example 1. The polymerization activity was 12891 gPE / gCat, and the M w 106×10 4 g / mol, MWD is 4.1, and the apparent density of the polymer particles is 0.32 g / cm 3 The average particle size is 1071 μm and the average sphericity is 0.908.
[0103] Comparative Example 2
[0104] The preparation of the catalyst was the same as in Example 1 except that the methyl silicone oil was replaced with n-heptane. The preparation of the carrier and the ethylene polymerization were the same as in Example 1. The catalyst was not successfully prepared into a spherical morphology. The polymer product contained a lot of fine powder and the apparent density of the polymer product was low. The polymerization activity was 11281 gPE / gCat. The M w 87×10 4 g / mol, MWD is 6.8, and the apparent density of the polymer particles is 0.22 g / cm 3 The average particle size is 689 μm and the average sphericity is 0.29.
[0105] Comparative Example 3
[0106] The catalyst was prepared and ethylene polymerization was conducted according to the method of Example 1, except that the catalyst preparation process did not include the step of preparing a pretreated support. Instead, the support was directly reacted with TiCl4 to prepare the catalyst. The catalyst partially collapsed, and the polymer product contained a large amount of fine powder, resulting in a low apparent density.
[0107] The polymerization activity is 12487gPE / gCat, and the M w 94×10 4 g / mol, MWD is 5.6, and the apparent density of the polymer particles is 0.28 g / cm 3 The average particle size is 788 μm and the average sphericity is 0.764.
[0108] Example 6
[0109] (1) Vector preparation
[0110] Under N2 protection, 10g MgCl2, 80mg galactose, 1.2g PVP (0.0001mol) and a certain amount of mixed alcohol (MgCl2: ethanol: n-butanol: isooctyl alcohol (molar ratio) = 1:4:5:1) were added to a 250ml three-necked flask in sequence. The stirring speed was 600rpm, and the temperature was raised to 80°C. After the solid was completely dissolved, the reaction was continued for 2h. 20ml epichlorohydrin (0.2557mol) was slowly added dropwise via a microsyringe pump. During the addition, a white to light yellow solid gradually precipitated. The addition was completed in 1.5h. After another 1.5h of reaction, the reaction was stopped. After standing, the supernatant was removed, washed with n-hexane three times, and vacuum dried at room temperature for 4h to obtain the carrier (white powder).
[0111] (2) Catalyst preparation
[0112] 3g of the obtained support (Mg content in the support was 0.0236mol) was dispersed in a 100ml three-necked flask containing 60ml of methyl silicone oil. Under nitrogen, the flask was placed in a constant temperature bath at -30°C and mechanically stirred (120rpm) to ensure uniform dispersion of the support. After stirring for 30 minutes and the system cooled to a relatively low temperature, 0.9ml of tetrabutyl titanate (0.0026mol) was added dropwise using a microsyringe pump over 1.5 hours. After the addition was complete, the system was heated to 50°C at a heating rate of 0.5°C / min while stirring and the reaction was continued for 2 hours. After the reaction was completed, the solution was allowed to stand and the supernatant was removed. The solution was then washed three times with n-hexane and dried under vacuum at room temperature for 4 hours to obtain the pretreated support.
[0113] Take 1g of the obtained pretreated support (the Mg content in the pretreated support is 0.0089mol) and disperse it in a 100ml three-necked flask containing 60ml of methyl silicone oil; under nitrogen protection, place the flask in a constant temperature bath at -40°C, during which mechanical stirring (60rpm); after stirring for 30min and the system drops to a lower temperature, add 10ml TiCl4 (0.0911mol) dropwise, and complete it in 2.5h; after the addition is completed, heat to 80°C while stirring at a heating rate of 0.5°C / min and continue the reaction for 3h; filter out the methyl silicone oil and unreacted TiCl4, and wash with 300ml of n-hexane three times; place it back in a constant temperature bath at -40°C for 30min, and repeat the above TiCl4 addition, heating, reaction, and washing steps; after washing, dry the catalyst in vacuum at room temperature for 4h to obtain a spherical catalyst with a titanium content of 8.7wt%.
[0114] (3) The conditions for ethylene polymerization were the same as those in Example 1.
[0115] The catalyst has a spherical morphology, an average particle size of 38.74 μm, and a uniform particle size distribution. The polymerization activity is 14532 gPE / gCat, and the M w 121×10 4 g / mol, MWD is 4.2, and the apparent density of the polymer particles is 0.33 g / cm 3 The average particle size is 896 μm and the average sphericity is 0.912.
[0116] The above-described embodiments merely illustrate several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. Persons skilled in the art will readily appreciate that variations and modifications may be made without departing from the scope of the present invention, all of which fall within the scope of protection of the present invention.
Claims
1. A spherical carrier for olefin polymerization, It is characterized in that The vector is prepared by the following steps: (1) reacting a magnesium compound with an organic compound containing active hydrogen at 30-160° C. in the presence of polyvinyl pyrrolidone and a multipolar functional group compound to form a complex solution; (2) reacting the complex solution with an epoxy compound to precipitate a solid compound; The epoxy compound is shown in the general formula (I): In the general formula (I), R 2 and R 3 are each independently selected from hydrogen, C 1 -C 5 A straight or branched alkyl group, wherein the hydrogen on the alkyl group is optionally substituted by a halogen atom X; (3) washing the solid compound obtained in step (2) with an inert alkane solvent to obtain a spherical carrier of magnesium compound; Wherein, the multipolar functional group compound described in step (1) is a compound having a general formula of C n H 2n O n A compound with multipolar functional groups, wherein n is 4-8; The organic compound containing active hydrogen in step (1) is a compound of the general formula R(OH): m A compound or a mixture of compounds as shown, wherein R is C 1 -C 20 Hydrocarbyl, m≥1; The inert alkane solvent described in step (3) is a solvent of the general formula C n H 2n+2 A mixture of one or more compounds shown, wherein n≥5.
2. The spherical carrier according to claim 1, It is characterized in that Calculated per mole of magnesium, the amount of polyvinyl pyrrolidone used is 0.001-0.1 mole, the amount of the multipolar functional group compound used is 0.002-0.2 mole, the amount of the organic compound containing active hydrogen is 2-20 moles, and the amount of the epoxy compound used is 1-30 moles.
3. The spherical carrier according to claim 1, It is characterized in that The multipolar functional group compound described in step (1) is a mixture of one or more of glucose, fructose, sorbitol, galactose and cyclohexanehexol.
4. The spherical carrier according to claim 1, It is characterized in that The magnesium compound described in step (1) is a mixture of one or more of magnesium halide, phenoxymagnesium chloride, isopropoxymagnesium chloride and butoxymagnesium chloride.
5. The spherical carrier according to claim 1, It is characterized in that R(OH) in step (1) m A mixture of two or three selected from methanol, ethanol, propanol, n-butanol, isobutanol, amyl alcohol, isopentanol, n-hexanol, 2-ethylhexanol, isooctyl alcohol, ethylene glycol, propylene glycol and glycerol.
6. The spherical carrier according to claim 1, It is characterized in that The epoxy compound described in step (2) is ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epichlorohydrin, epibromohydrin or epibromobutylene.
7. The spherical carrier according to claim 1, It is characterized in that The inert alkane solvent described in step (3) is selected from a mixture of one or more of n-hexane, cyclohexane, n-heptane, n-octane and n-nonane.
8. A spherical catalyst for olefin polymerization, It is characterized in that The catalyst is prepared by the following steps: (A) dispersing the spherical carrier according to any one of claims 1 to 7 in a high-viscosity inert hydrocarbon solvent, and adding a titanium compound at low temperature to react to obtain an intermediate product; The titanium compound is shown in the general formula (II): R in the general formula (II) 1 '、R 2 '、R 3 '、R 4 'Each independently selected from C 1 -C 10 The alkyl group; (B) dispersing the intermediate product in a high-viscosity inert hydrocarbon solvent, adding titanium tetrachloride at low temperature for reaction, and washing the obtained solid product with an inert alkane solvent to obtain a spherical catalyst; The high-viscosity inert hydrocarbon solvents in step (A) and step (B) are independently alkyl-substituted cycloalkanes and alkyl-substituted aromatic hydrocarbons.
9. The spherical catalyst according to claim 8, It is characterized in that The amount of the titanium compound used is 0.05-1.5 moles per mole of magnesium, and the amount of the titanium tetrachloride used is 0.5-15 moles.
10. The spherical catalyst according to claim 8, It is characterized in that The high-viscosity inert hydrocarbon solvents in step (A) and step (B) are independently a mixture of one or more of paraffin oil, white oil, methyl silicone oil and vaseline oil.
11. The spherical catalyst according to claim 8, It is characterized in that The low temperature in step (A) and step (B) is independently -40 to 0°C.
12. The spherical catalyst according to claim 8, It is characterized in that The low temperature in step (A) and step (B) is independently -20 to -10°C.
13. Use of a polymerization catalyst system comprising the spherical catalyst component according to any one of claims 8 to 12 in alpha-olefin polymerization.
14. Use of the carrier according to any one of claims 1 to 7 in α-olefin polymerization.
Citation Information
Patent Citations
Spherical carrier for olefin polymerization catalyst and preparation method thereof
CN102453127A
Ball shape ethylene polymerization solid titanium catalytic agent and preparation and application thereof
CN103130931A
Catalyst component for ethylene polymerization, preparation method thereof and catalyst for ethylene polymerization
CN108341902A
Spherical catalyst for olefin polymerization reaction
CN116554371A
Solid catalytic component for producing ultra-high-molecular weight polyethylene
JP1994016718A