Copolymer, preparation method therefor, and application thereof

By copolymerizing pyrimidone and multiple hydrogen bonding monomers with pyrrolidone, a copolymer with excellent inhibitory properties is prepared, which solves the problem of insufficient performance of existing hydrate kinetic inhibitors and achieves effective inhibition and economicalization of hydrates. Production, suitable for oil and gas extraction and transportation.

WO2024199363A1PCT designated stage expired Publication Date: 2024-10-03CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/084445
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The inhibitory performance of existing hydrate kinetic inhibitors against hydrates needs to be improved, and it is difficult to apply them on a large scale. They also have problems such as high economic costs, environmental pollution, and low inhibitory activity.

Method used

An unsaturated monomer containing pyrimidinone and multiple hydrogen bonds is copolymerized with an unsaturated monomer of pyrrolidone to prepare a copolymer with a specific content. Through the combination of structural unit A and structural unit B, a copolymer with excellent inhibitory properties is formed. It can extend the hydrate induction time and slow down the formation rate at different supercooling degrees.

Benefits of technology

It achieves effective suppression of hydrates, has stable properties and a wide adaptable range of supercooling, is suitable for oil and gas production and transportation, reduces synthesis costs and expands application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024084445_03102024_PF_FP_ABST
    Figure CN2024084445_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of oil and gas extraction and conveying, and in particular to a copolymer, a preparation method therefor, and an application thereof. The copolymer comprises a structural unit A and a structural unit B, the structural unit A coming from an unsaturated monomer containing pyrimidone and multiple hydrogen bonds, and the structural unit B coming from an unsaturated monomer containing pyrrolidone; wherein, using the total weight of the copolymer as a benchmark, the content of the structural unit A is 0.5-10 wt%, and the content of the structural unit B is 90-99.5 wt%. The copolymer not only contains a specific content of structural unit A and a specific content of structural unit B, but structural unit A and structural unit B each comprise a specific structure, giving the copolymer excellent hydrate inhibition performance, and particularly being expressed as the copolymer being able to bear a greater degree of supercooling; furthermore, under different degrees of supercooling, the hydrate induction time can be effectively extended, slowing the rate of hydrate formation.
Need to check novelty before this filing date? Find Prior Art

Description

Copolymer and its preparation method and application

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Chinese patent application No. 202310340058.X filed on March 31, 2023, the contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to the technical field of oil and gas extraction and transportation, and in particular to a copolymer and a preparation method and application thereof. Background Art

[0004] Natural gas hydrates are cage-like substances formed by water molecules and small gases such as methane and ethane under high pressure and low temperature. Currently, there are three types of hydrate crystal structures: Type I, Type II, and Type H. Gas hydrates often appear during oil and gas field production and pipeline transportation. When hydrates begin to form in large quantities, they are very likely to cause blockage of equipment such as wellbores and pipelines, thereby affecting the normal operation of equipment and even causing pipeline ruptures, leading to flow safety accidents and unacceptable losses. Therefore, how to prevent and control the formation of hydrates has always been a difficult problem facing the oil and gas industry.

[0005] The addition of chemical inhibitors is the primary method for inhibiting hydrate formation, including thermodynamic inhibitors (THIs) and low-dose kinetic inhibitors (LDHs). Thermodynamic inhibitors prevent hydrate formation by altering the thermodynamic equilibrium conditions, reducing the equilibrium pressure or temperature of hydrate formation to below the actual pressure or temperature in the pipeline. Although thermodynamic inhibitors are widely used in oil and gas field production, they require large dosages (typically 10% to 60% of the aqueous phase), resulting in high economic costs and environmental pollution. Low-dose kinetic inhibitors, on the other hand, do not alter the thermodynamic conditions for hydrate formation in the system. Instead, they delay hydrate nucleation time, reduce the growth rate of hydrate crystals, and prevent hydrate crystal growth, thereby avoiding problems such as pipeline blockage. Compared with traditional thermodynamic inhibitors, the dosage required is much lower (typically less than 1%) and offers potential economic and environmental benefits.

[0006] However, the inhibitory effect of low-dose kinetic inhibitors is significantly affected by the degree of supercooling, resulting in low inhibitory activity and limited application in highly supercooled systems. Furthermore, kinetic inhibitors such as N-vinylcaprolactam are limited to large-scale commercial application due to poor biodegradability, high synthesis costs, low inhibitory activity, and limited applicability.

[0007] At present, CN108219762A discloses a novel hydrate kinetic inhibitor, which is a phenylated poly N-vinyl pyrrolidone, which is polymerized from ethylbenzene and N-vinyl pyrrolidone monomers. CN113388379A provides a hydrate kinetic inhibitor and its preparation method and application, which is polymerized from vinyl pyrrolidone, cyclohexyl vinyl ether and acrylate monomers. CN105859963A discloses a hydrate inhibitor product obtained by free radical solution polymerization in a solvent using N-vinyl pyrrolidone (NVP), N-vinyl caprolactam (NVCL), acrylamide (AM) and acrylonitrile (AN) as synthetic monomers, ammonium persulfate and sodium bisulfite as initiators. CN104194756A discloses a novel hydrate kinetic inhibitor and its preparation method and application, the main component of which is a polyhydroxy polymer obtained by reacting chlorophenol with N-vinyl caprolactam or N-vinyl pyrrolidone. "Preparation and Performance of a New Natural Gas Hydrate Kinetic Inhibitor" (Zhou Shi-ming et al., Petrochemicals, 2017, 46(04): 467-470) discloses a solution polymerization method for synthesizing a kinetic inhibitor using N-vinyl pyrrolidone as a monomer and hydrogen peroxide as an initiator under the action of nitrogen. "Development and Performance Evaluation of a New Natural Gas Hydrate Kinetic Inhibitor" (Liu Shu-jie et al., China Offshore Oil and Gas, 2015, 27(06): 69-73) discloses a new hydrate kinetic inhibitor, KHI-S, which adsorbs onto the hydrate surface via a lactam ring to form a dense film, preventing the hydrate from further contacting with gas and water molecules, thereby delaying the continued growth of the hydrate. The hydrate kinetic inhibitors prepared in the above patent documents or non-patent documents need to be improved in their hydrate inhibition performance, making them difficult to apply on a large scale.

[0008] Summary of the Invention

[0009] The purpose of the present invention is to overcome the problem that the inhibitory performance of hydrate kinetic inhibitors on hydrates in the prior art needs to be improved, and to provide a copolymer and its preparation method and application. The copolymer has excellent inhibitory performance on hydrates, specifically, it can withstand a larger degree of supercooling. At the same time, under different degrees of supercooling, it can effectively prolong the hydrate induction time and slow down the hydrate formation rate.

[0010] In order to achieve the above object, the first aspect of the present invention provides a copolymer, characterized in that the copolymer comprises a structural unit A and a structural unit B, wherein the structural unit A is derived from an unsaturated monomer containing pyrimidone and multiple hydrogen bonds, and the structural unit B is derived from an unsaturated monomer containing pyrrolidone;

[0011] Wherein, based on the total weight of the copolymer, the content of the structural unit A is 0.5-10 wt%, and the content of the structural unit B is 90-99.5 wt%.

[0012] A second aspect of the present invention provides a method for preparing a copolymer, characterized in that the method comprises: contacting compound A and compound B in the presence of a first solvent and an initiator to perform a first reaction to obtain the copolymer;

[0013] Wherein, compound A is an unsaturated monomer containing pyrimidone and multiple hydrogen bonds; compound B is an unsaturated monomer containing pyrrolidone;

[0014] Based on the total weight of the compound A and the compound B, the amount of the compound A is 0.5-10 wt%, and the amount of the compound B is 90-99.5 wt%.

[0015] The third aspect of the present invention provides a copolymer prepared by the preparation method described in the second aspect of the present invention.

[0016] The fourth aspect of the present invention provides a use of the copolymer described in the first aspect or the third aspect of the present invention as a hydrate kinetic inhibitor.

[0017] Through the above technical solution, the copolymer provided by the present invention and its preparation method and application achieve the following beneficial effects:

[0018] (1) The copolymer provided by the present invention not only contains a specific content of structural unit A and a specific content of structural unit B, but also structural unit A and structural unit B each contain a specific structure, so that the copolymer has excellent hydrate inhibition performance, which is specifically manifested in that it can withstand a larger degree of supercooling. At the same time, under different degrees of supercooling, it can effectively prolong the hydrate induction time and slow down the hydrate formation rate.

[0019] (2) The preparation method of the present invention has the advantages of simple polymerization process and easy industrial production.

[0020] (3) The copolymer provided by the present invention can be used as a hydrate kinetic inhibitor for oil and gas production and transportation, and has the advantages of stable properties and a wide range of supercooling adaptability, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Fig. 1 is an infrared spectrogram of the copolymer S-1 obtained in Example 1;

[0022] FIG2 is a hydrogen NMR spectrum of the copolymer S-1 obtained in Example 1;

[0023] FIG3 is a schematic diagram of a hydrate inhibitor performance evaluation device.

[0024] Explanation of the accompanying symbols: 1-methane gas cylinder; 2-pressure regulating valve; 3-PID valve; 4-motor; 5-torque sensor; 6-stirrer; 7-reactor; 8-temperature sensor; 9-pressure sensor; 10-chassis and data acquisition and processing system. DETAILED DESCRIPTION

[0025] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0026] The first aspect of the present invention provides a copolymer, characterized in that the copolymer comprises a structural unit A and a structural unit B, wherein the copolymer comprises a structural unit A and a structural unit B, the structural unit A is derived from an unsaturated monomer containing pyrimidone and multiple hydrogen bonds, and the structural unit B is derived from an unsaturated monomer containing pyrrolidone;

[0027] Wherein, based on the total weight of the copolymer, the content of the structural unit A is 0.5-10 wt%, and the content of the structural unit B is 90-99.5 wt%.

[0028] In the present invention, the copolymer contains structural units A and B containing specific groups, and when the contents of structural units A and structural units B in the copolymer meet specific ranges, the copolymer has excellent hydrate inhibition performance, which is specifically manifested in that it can withstand a greater degree of supercooling. At the same time, under different degrees of supercooling, it can effectively prolong the hydrate induction time and slow down the hydrate formation rate.

[0029] Specifically, the pyrrolidone contained in structural unit B and the pyrimidone contained in structural unit A can be adsorbed on the hydrate growth site, causing lattice mismatch, destroying the crystal structure, and inhibiting the growth of the hydrate nucleus to a critical size; the multiple hydrogen bonds contained in structural unit A can enhance the ability of the copolymer to adsorb on the surface of the already formed hydrate nucleus, prevent the aggregation of hydrate crystal particles, and inhibit the growth of hydrate crystals.

[0030] In the present invention, the content of structural unit A and structural unit B in the copolymer is measured by nuclear magnetic resonance spectroscopy. About 5-10 mg of the purified copolymer is weighed and placed in a nuclear magnetic resonance tube, deuterated chloroform is added to dissolve it, and the experiment is carried out at room temperature using a nuclear magnetic resonance spectrometer. By comparing the nuclear magnetic resonance spectroscopy of the copolymer of structural units A and structural unit B with the structural unit B raw material, as shown in Figure 2, the relative content of structural unit A and structural unit B in the copolymer can be obtained by calculating the integrated area of ​​the characteristic signal peak.

[0031] Furthermore, based on the total weight of the copolymer, when the content of the structural unit A is preferably 1-3 wt % and the content of the structural unit B is preferably 97-99 wt %, it is beneficial to further improve the hydrate inhibition performance of the copolymer.

[0032] According to the present invention, the structural unit A has a structure shown in formula (1), and the structural unit B has a structure shown in formula (2);

[0033] Wherein, R1 is H or C1-C 10 R2 is H or a C1-C5 alkyl group;

[0034] n is an integer of 1-10; R3-R8 are each independently H or C1-C 10 of alkyl.

[0035] In the present invention, when the structural unit A and the structural unit B in the copolymer have the above-mentioned specific structure, the hydrate inhibition performance of the copolymer can be further improved.

[0036] Furthermore, R1 is a C1-C5 alkyl group; R2 is a C1-C3 alkyl group; n is an integer of 2-5; and R3-R8 are each independently H or a C1-C5 alkyl group. When at least one of the above conditions is met, the copolymer's hydrate inhibition performance can be further improved.

[0037] In the present invention, the weight average molecular weight of the copolymer is 50,000-500,000, preferably 110,000-200,000.

[0038] A second aspect of the present invention provides a method for preparing a copolymer, characterized in that the method comprises: contacting compound A and compound B in the presence of a first solvent and an initiator to perform a first reaction to obtain the copolymer;

[0039] Wherein, compound A is an unsaturated monomer containing pyrimidone and multiple hydrogen bonds; compound B is an unsaturated monomer containing pyrrolidone;

[0040] Based on the total weight of the compound A and the compound B, the amount of the compound A is 0.5-10 wt%, and the amount of the compound B is 90-99.5 wt%.

[0041] In the present invention, an unsaturated monomer containing pyrimidone and multiple hydrogen bonds is polymerized with an unsaturated monomer containing pyrrolidone, so that the resulting copolymer simultaneously includes the five-membered ring structure of pyrrolidone, the six-membered ring structure of pyrimidone, and the multiple hydrogen bond structure. This allows the copolymer to not only adsorb on hydrate growth sites, causing lattice mismatch, destroying the crystal structure, and inhibiting the growth of hydrate nuclei to a critical size; it also enhances the copolymer's ability to adsorb on the surface of already formed hydrate nuclei, preventing the aggregation of hydrate crystal particles and inhibiting the growth of hydrate crystals. This results in the copolymer having excellent hydrate inhibition properties, specifically manifested in its ability to withstand greater degrees of supercooling. At the same time, under different degrees of supercooling, it can effectively prolong the hydrate induction time and slow the hydrate formation rate.

[0042] In particular, when the content of compound A and compound B is controlled to satisfy the above ranges, the obtained copolymer has excellent hydrate inhibition performance.

[0043] In addition, the method of the present invention has low synthesis cost and mild reaction conditions, thereby enabling large-scale commercial production.

[0044] Furthermore, based on the total weight of the compound A and the compound B, when the amount of the compound A is preferably 1-3 wt % and the amount of the compound B is preferably 97-99 wt %, it is beneficial to further improve the hydrate inhibition performance of the copolymer.

[0045] According to the present invention, compound A has a structure shown in formula (3); compound B has a structure shown in formula (4);

[0046] Wherein, R1' is H or C1-C 10 R2' is H or a C1-C5 alkyl group;

[0047] n' is an integer of 1-10; R3'-R8' are each independently H or C1-C 10 of alkyl.

[0048] Furthermore, R1' is a C1-C5 alkyl group; R2' is a C1-C3 alkyl group; n' is an integer of 2-5; and R3'-R8' are each independently a C1-C5 alkyl group. When one or more of the above conditions are met, the hydrate inhibition performance of the copolymer can be further improved.

[0049] According to the present invention, the conditions of the first reaction include: reaction temperature of 40-70° C., and reaction time of 6-10 h.

[0050] In the present invention, the conditions of the first reaction meet the above ranges, which has the advantages of simple polymerization process and easy industrial production.

[0051] Furthermore, the conditions of the first reaction include: the reaction temperature is preferably 50-60° C., and the reaction time is preferably 7-9 h.

[0052] According to the present invention, the first solvent is selected from at least one of deionized water, ethanol and methanol.

[0053] In one embodiment of the present invention, the first solvent is a mixture of deionized water and alcohol. When the above-mentioned type is met, it has the advantages of low cost and easy availability. The present invention does not particularly limit the ratio of deionized water to alcohol. For example, the volume ratio of deionized water to alcohol is 1:2.5-3.5.

[0054] In the present invention, the volume ratio of the compound B to the first solvent is 1:2.5-3.5; when the above range is met, the hydrate inhibition performance of the obtained copolymer is further improved.

[0055] According to the present invention, the initiator is selected from at least one of potassium persulfate, ammonium persulfate and sodium persulfate.

[0056] According to the present invention, based on the total weight of the compound A and the compound B, the amount of the initiator is 1-2 wt%, preferably 1.5-2 wt%.

[0057] In the present invention, the reaction is carried out under nitrogen or inert gas protection to prevent the reactants from being oxidized. In a specific embodiment of the present invention, the nitrogen or inert gas ventilation time is 20-30 minutes.

[0058] The present invention illustratively provides a method for preparing compound A, comprising: contacting compound C and compound D in the presence of a second solvent, performing a second reaction, and obtaining compound A;

[0059] Wherein, compound C has the structure shown in formula (5); compound D has the structure shown in formula (6);

[0060] Wherein, R1" is H or C1-C 10 R2" is H or a C1-C5 alkyl group; n" is an integer from 1 to 10.

[0061] Furthermore, R1" is a C1-C5 alkyl group; R2" is a C1-C3 alkyl group; and n" is an integer of 2-5.

[0062] In the present invention, the conditions of the second reaction include: reaction temperature of 20-30° C., and reaction time of 1.5-3 h.

[0063] In the present invention, the molar ratio of the compound C to the compound D is 1:0.8-1.2. In the present invention, there is no particular limitation on the type of the second solvent, and it can be any conventional solvent in the art, for example, dimethyl sulfoxide (DMSO).

[0064] In the present invention, there is no particular limitation on the amount of the second solvent. For example, the mass ratio of the compound C to the second solvent may be 1:90-110.

[0065] In the present invention, the method further comprises: after the reaction is completed, isolating, washing, and drying the obtained compound A. The present invention does not particularly limit the washing method, for example, washing with anhydrous ethanol; the present invention does not particularly limit the drying method, for example, drying at 30-50°C for 3-5 hours under vacuum conditions.

[0066] The present invention does not particularly limit the method for adding compound C, compound D, and the second solvent, as long as the second solvent can dissolve compound C and compound D. In one embodiment of the present invention, compound C is added to the second solvent and stirred until completely dissolved, and then compound D is added to carry out the second reaction; wherein the stirring temperature is 130-170°C and the stirring time is 0.1-0.5h.

[0067] The third aspect of the present invention provides a copolymer prepared by the preparation method described in the second aspect of the present invention.

[0068] The fourth aspect of the present invention provides a use of the copolymer described in the first aspect or the third aspect of the present invention as a hydrate kinetic inhibitor.

[0069] In the present invention, the specific method of using the copolymer as a hydrate kinetic inhibitor includes:

[0070] The copolymer is mixed with water to obtain an inhibitor solution, wherein the concentration of the copolymer in the inhibitor solution is 0.5-2 wt %. The inhibitor solution is added to an oil and gas production wellbore or a transportation pipeline through a ground injection device to inhibit the reaction.

[0071] The copolymer of the present invention is used as a hydrate kinetic inhibitor in oil and gas production and transportation, has the advantages of stable properties, a wide range of supercooling adaptability, and the like, and has broad application prospects.

[0072] The present invention will be described in detail below through examples.

[0073] In the following examples and comparative examples, the specific structures of the raw materials are as follows:

[0074] In compound C-1, R1″ is -CH3;

[0075] In compound C-2, R1″ is -C2H5;

[0076] In compound D-1, R2" is -CH3, and n" is 2;

[0077] In compound D-2, R2" is -C2H5, and n" is 3;

[0078] In compound B-1, R3'-R8' are all H;

[0079] In compound B-2, R5' is -CH3, and R3', R4' and R6'-R8' are all H;

[0080] Vinyl caprolactam, brand LUVICAP-EG, denoted as W-3, purchased from BASF, USA;

[0081] Polyvinylpyrrolidone, brand K90, denoted as W-4, was purchased from BASF, USA;

[0082] In the following examples and comparative examples, the raw materials used are all commercially available conventional products.

[0083] In the following examples, the content of each structural unit and the weight-average molecular weight of the copolymer were calculated using H NMR spectroscopy.

[0084] 1. Preparation of Compound A

[0085] Preparation Example 1

[0086] S1. Add 2 g of compound C-1 to 198 g of DMSO and stir at 150°C for 10 min. After complete dissolution, transfer to room temperature (20°C) and add 2.64 g of compound D-1. React for 2 h to generate a white solid. The molar ratio of compound C-1 to compound D-1 is 1:1.

[0087] S2. Separate the white solid by suction filtration, wash with anhydrous ethanol, and dry in vacuo at 40° C. for 4 h to obtain compound A-1; wherein R1′ is —CH3; R2′ is —CH3, and n′ is 2.

[0088] Preparation Example 2

[0089] Compound A-2 was prepared according to the method of Preparation Example 1, except that Compound C-1 was replaced by Compound C-2, and Compound D-1 was replaced by Compound D-2. In Compound A-2, R1' was -C2H5, R2' was -C2H5, and n' was 2.

[0090] 2. Preparation of Copolymer

[0091] Example 1

[0092] 16 mL of compound B-1, 12 mL of deionized water, and 36 mL of ethanol were mixed, 0.32 g of compound A-1 was added, and after ultrasonic dissolution, 0.241 g of potassium persulfate was added to the reaction system. After dissolution, nitrogen was passed through for 20 minutes, and the mixture was reacted at 55°C for 8 hours. The reaction product was separated by filtration to obtain copolymer S-1. The specific characteristics are shown in Table 2.

[0093] Wherein, based on the total weight of compound A-1 and compound B-1, the amount of compound A-1 is 2wt%, and the amount of compound B-1 is 98wt%; the first solvent is a mixture of deionized water and ethanol, and the volume ratio of deionized water to ethanol is 1:3; the volume ratio of compound B-1 to the first solvent is 1:3; based on the total weight of compound A-1 and compound B-1, the amount of potassium persulfate is 1.5wt%;

[0094] The structure of copolymer S-1 was determined by infrared spectroscopy, as shown in Figure 1, where 3434 cm -1 The characteristic peak of amide group is at 2924 cm -1 The characteristic peak of methylene is at 1724 cm -1 The characteristic peak of the carbonyl group in the ester group is 1633 cm -1 The characteristic peak of carbonyl in amide group is 1535cm -1 The peak at the center is a characteristic peak of a six-membered ring, indicating that compounds A-1 and B-1 were successfully polymerized. The H NMR spectrum of copolymer S-1 is shown in Figure 2, where Figure 2 (left) is the entire spectrum obtained from the test, and Figure 2 (right) is an enlarged spectrum of the dotted line portion, which is the H NMR spectrum of copolymer S-1. The contents of structural unit A and structural unit B in copolymer S-1 can be calculated from Figure 2 (right), and the results are shown in Table 2.

[0095] Examples 2-7

[0096] Copolymers S-2 to S-7 were prepared according to the method of Example 1, except that the reaction conditions were different from those of Example 1, as shown in Table 1. The characteristics of copolymers S-2 to S-7 are shown in Table 2.

[0097] Example 8

[0098] Copolymer S-8 was prepared according to the method of Example 1, except that compound A-1 was replaced by compound A-2, and compound B-1 was replaced by compound B-2 to obtain copolymer S-8. See Table 1 for details. The characteristics of copolymer S-8 are shown in Table 2.

[0099] Comparative Example 1

[0100] The copolymer S-1 was replaced by LUVICAP-EG and designated as W-1.

[0101] Comparative Example 2

[0102] The copolymer S-1 was replaced with polyvinylpyrrolidone K90 (PVPk90), and was designated as W-2.

[0103] Comparative Example 3

[0104] When the copolymer S-1 was replaced with the compound B-1 and the compound B-1 was allowed to self-polymerize with the compound B-1, it was found that the reaction did not proceed.

[0105] Comparative Example 4

[0106] Copolymer D-1 was prepared according to the method of Example 1, except that the reaction conditions were different from those of Example 1, as shown in Table 1. The characteristics of copolymer D-1 are shown in Table 2.

[0107] Comparative Example 5

[0108] Copolymer D-2 was prepared according to the method of Example 1, except that an equal mass fraction of N-(3-aminopropyl)acrylamide was used to replace compound A-1 to obtain copolymer D-2.

[0109] Table 1

[0110] Table 2

[0111] Test Example 1: Determination of Maximum Subcooling

[0112] (1) Experimental setup

[0113] FIG3 shows an apparatus for evaluating the hydrate inhibition performance of a copolymer. The apparatus comprises: a methane cylinder 1; a pressure regulating valve 2; a PID valve 3 for adjusting the inlet and outlet pressures between 0 and 16 MPa; a motor 4; a torque sensor 5; and an agitator 6 for stirring at a speed between 0 and 1000 r / min; a reactor 7 with a capacity of 500 mL, a pressure resistance of 20 MPa, and an operating temperature between -20°C and 50°C; a temperature sensor 8 with a range exceeding 600°C and an accuracy of 0.1°C; a pressure sensor 9 with a range of 25 MPa and an accuracy of 0.25%; and a chassis and data acquisition and processing system 10.

[0114] (2) Test method

[0115] The test method includes the following steps:

[0116] S1. Dissolve the compound prepared in each example and comparative example in deionized water to prepare an inhibitor-containing solution;

[0117] S2. Add 170 mL of inhibitor solution to reactor 7, fill it with 8 MPa of methane, start the magnetic stirrer, adjust the speed to 300 r / min, control the initial temperature of reactor 7 to 10 ° C, and cool it down at a rate of 1 ° C / d. Monitor the changes in temperature, pressure and torque over time during the cooling process. When the torque suddenly increases, record the temperature and pressure at this time, and record them as the generation pressure P1 and generation temperature T0 respectively. According to the methane hydrate phase equilibrium curve, calculate the phase equilibrium temperature T1 corresponding to the generation pressure P1 and the maximum supercooling T e =T1-T0; see Table 3 for specific data.

[0118] In the above process, when the torque suddenly increases, it indicates that a phase transition occurs in the inhibitor-containing solution, and solid methane hydrate particles are generated.

[0119] Table 3

[0120] It can be seen from the results in Table 3 that the copolymer of the present invention can withstand a greater degree of supercooling when used as an inhibitor.

[0121] Test Example 2: Determination of induction time

[0122] The induction time was measured by the temperature-pressure torque change method using the apparatus shown in FIG3 , which specifically includes the following steps:

[0123] S1. Dissolve the compounds prepared in each example and comparative example in deionized water to prepare a 1 wt% inhibitor solution;

[0124] S2. Add 170 mL of the inhibitor solution to reactor 7 and cool to the specified experimental temperature (experimental temperature T = phase equilibrium temperature T corresponding to initial pressure P0 minus subcooling). When the temperature stabilizes, introduce methane gas into reactor 7. Once the desired experimental pressure (i.e., initial pressure P0) is reached, stir at 300 rpm. This is marked as time zero. While maintaining a constant temperature, record the change in torque over time. When the torque suddenly increases, record the time at this point, which is the torque-temperature jump time (induction time T). Record the system pressure after 1000 minutes, which is the end-of-experiment pressure P1. Calculate gas consumption n using PV = nRT. Detailed data is shown in Table 4.

[0125] In the above process, when methane hydrate is formed, a phase change occurs in the original inhibitor solution, from liquid to solid-liquid, which will cause a sudden increase in torque. By measuring the time point of the torque mutation, the induction time of methane hydrate nucleation can be obtained.

[0126] The amount of hydrate generated is proportional to the gas consumption. The smaller the gas consumption, the less hydrate is generated and the better the inhibitory performance.

[0127] Table 4

[0128] The results in Table 4 show that, at different degrees of supercooling, the pressure drop amplitude (P1-P0) within 1000 min for each inhibitor system is lower than that of the pure water system, indicating that the addition of the inhibitor inhibits the growth of hydrates. Among them, the copolymer of the present invention has better hydrate growth inhibition performance as an inhibitor. At the same time, the torque-temperature mutation time (induction time) of each inhibitor system is longer than that of the pure water system, and all exhibit a certain ability to inhibit nucleation. Among them, when the copolymer of the present invention is used as an inhibitor, the system has the longest induction time and better nucleation inhibition performance.

[0129] At the same time, the experiment found that the pressure drop amplitude of each inhibitor system at low supercooling of 5.5℃ and 6.5℃ was significantly higher than that at 7.5℃. This is because hydrates grow in a funnel shape at low supercooling, and the hydrate film formed at the gas-liquid interface is easy to rupture, resulting in a weakening of the effect of hindering mass transfer between gas and liquid; at high supercooling, the hydrate film formed at the gas-liquid interface is relatively strong, and the resistance of gas entering the liquid becomes greater, resulting in a lower pressure drop amplitude.

[0130] Combining the contents of Table 3 and Table 4, it can be seen that the copolymer provided by the present invention can significantly inhibit the growth of hydrates while withstanding a maximum supercooling of not less than 3°C, and the gas consumption does not exceed 0.22 mol.

[0131] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A copolymer, characterized in that The copolymer comprises a structural unit A and a structural unit B, wherein the structural unit A is derived from an unsaturated monomer containing pyrimidone and multiple hydrogen bonds, and the structural unit B is derived from an unsaturated monomer containing pyrrolidone; Wherein, based on the total weight of the copolymer, the content of the structural unit A is 0.5-10wt%, and the content of the structural unit B is 90-99.5wt%.

2. The copolymer according to claim 1, wherein Based on the total weight of the copolymer, the content of the structural unit A is 1-3wt%, and the content of the structural unit B is 97-99wt%.

3. The copolymer according to claim 1 or 2, wherein The structural unit A has a structure shown in formula (1), and the structural unit B has a structure shown in formula (2); Where R1 is H or C1-C 10 R2 is H or a C1-C5 alkyl group; n is an integer of 1-10; R3-R8 are each independently H or C1-C 10 of alkyl.

4. The copolymer according to claim 3, characterized in that R1 is a C1-C5 alkyl group; Preferably, R2 is a C1-C3 alkyl group; Preferably, n is an integer from 2 to 5; Preferably, R3-R8 are each independently H or a C1-C5 alkyl group.

5. A method for preparing a copolymer, characterized in that: The method comprises: contacting compound A and compound B in the presence of a first solvent and an initiator to perform a first reaction to obtain the copolymer; Wherein, compound A is an unsaturated monomer containing pyrimidone and multiple hydrogen bonds; compound B is an unsaturated monomer containing pyrrolidone; Based on the total weight of the compound A and the compound B, the amount of the compound A is 0.5-10 wt %, and the amount of the compound B is 90-99.5 wt %.

6. The preparation method according to claim 5, wherein: Based on the total weight of the compound A and the compound B, the amount of the compound A is 1-3 wt %, and the amount of the compound B is 97-99 wt %.

7. The preparation method according to claim 5 or 6, wherein: Compound A has a structure shown in formula (3); Compound B has a structure shown in formula (4); Wherein, R1' is H or C1-C 10 R2' is H or a C1-C5 alkyl group; n' is an integer of 1-10; R3'-R8' are each independently H or C1-C 10 of alkyl.

8. The preparation method according to any one of claims 5 to 7, characterized in that: The conditions of the first reaction include: reaction temperature of 40-70°C, preferably 50-60°C; reaction time of 6-10h, preferably 7-9h.

9. The preparation method according to any one of claims 5 to 8, characterized in that: The first solvent is selected from at least one of deionized water, ethanol and methanol; Preferably, the initiator is selected from at least one of potassium persulfate, ammonium persulfate and sodium persulfate.

10. The preparation method according to any one of claims 5 to 9, characterized in that: Based on the total weight of the compound A and the compound B, the amount of the initiator is 1-2 wt %.

11. A copolymer prepared by the preparation method according to any one of claims 5 to 10.

12. Use of the copolymer according to any one of claims 1 to 4 and 11 as a hydrate kinetic inhibitor.

Citation Information

Patent Citations

  • Composite hydrate inhibitor and application thereof

    CN102181275A

  • Composite hydrate kinetic inhibitor based on cyclic vinyl copolymer and application thereof

    CN115353584A

  • Inhibitor as well as preparation method and application thereof

    CN115433314A

  • Acrylamide-based copolymers, terpolymers, and use as hydrate inhibitors

    US20170321050A1

  • Composition that can be used to delay the formation of gas hydrates

    US20210403795A1