Rubber mixture and tyre

The sulfur-crosslinkable rubber mixture for tire treads, combining diene rubber, biologically renewable terpene resin, and organosilicon-modified polybutadiene, addresses the balance of tire performance and sustainability, achieving low rolling resistance and enhanced durability.

WO2024199994A1PCT designated stage expired Publication Date: 2024-10-03CONTINENTAL REIFEN DEUTSCHLAND GMBH
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/056556
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-12
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current tire tread compositions face challenges in balancing properties like wet grip, braking, rolling resistance, winter performance, abrasion, and durability, while also needing to incorporate sustainable and environmentally friendly materials to reduce fossil raw material dependence and greenhouse gas emissions.

Method used

A sulfur-crosslinkable rubber mixture for tire treads comprising diene rubber, a terpene resin based on over 95% biologically renewable raw materials, organosilicon-modified liquid polybutadiene, and silica, which improves rolling resistance and structural durability.

Benefits of technology

The rubber mixture achieves low rolling resistance and high tensile strength and elongation, resulting in a sustainable tire with improved durability and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000017_0001
    Figure IMGF000017_0001
Patent Text Reader

Abstract

The invention relates to a sulfur-crosslinkable rubber mixture, in particular for the tread of pneumatic vehicle tyres, containing at least the following constituents: - at least one diene rubber; - 5 to 70 phr (parts by weight, based on 100 parts by weight of all of the rubber in the mixture) of at least one terpene resin, more than 95% of which is based on biologically renewable raw materials; - 1 to 40 phr of at least one liquid polybutadiene, which is modified with organosilicon and has an average molecular weight Mw according to GPC of 500 to 18000 g / mol; and - 40-350 phr of at least one filler.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description

[0002] Rubber compound and tires

[0003] The invention relates to a sulfur-crosslinkable rubber mixture, in particular for the tread of pneumatic vehicle tires.

[0004] The invention further relates to a pneumatic vehicle tire having at least one component consisting of such a sulfur-vulcanized rubber mixture.

[0005] Since the driving characteristics of a tire, especially a pneumatic tire, depend to a large extent on the rubber composition of the tread, particularly stringent requirements are placed on the composition of the tread compound. Conflicting objectives exist between most of the well-known tire properties, such as wet grip, braking, handling, rolling resistance, winter performance, abrasion, and tear resistance. Numerous attempts have already been made to positively influence tire properties by varying the polymer components, fillers, and other additives in the tread compound.

[0006] In addition to the aforementioned objectives regarding compound and vulcanizate properties, today's efforts are aimed at using the most sustainable and environmentally friendly materials possible in rubber compounds for vehicle tires, reducing dependence on fossil raw materials, and minimizing greenhouse gas emissions. One approach to sustainable products is through the recycling of old, no longer needed products, such as the recycling of old tires, with the recycled material being used in the production of new tires. Another way to improve the sustainability of products is to use substances from renewable raw materials as additives for rubber compounds. Examples of such additives from renewable raw materials include vegetable oils, resins based on renewable raw materials, and rice husk silica.The latter is silica, which is made from bio-based sodium silicate from rice husk ash.

[0007] EP 3 350 259 B1 and EP 3 350 260 B1 disclose rubber compounds for tire treads with a good property profile, which contain a terpene-styrene resin and a non-functionalized liquid polybutadiene.

[0008] US 10,654,995 B2 describes a rubber mixture for tire treads which contains a resin based on a-pinene and a liquid polybutadiene end-functionalized with hydroxyl groups.

[0009] The invention is based on the object of providing sustainable rubber compounds for the treads of pneumatic vehicle tires, which result in tires with good rolling resistance and, at the same time, good structural durability.

[0010] This object is achieved according to the invention by a sulfur-crosslinkable rubber mixture, in particular for the tread of pneumatic vehicle tires, which contains at least the following components:

[0011] - at least one diene rubber,

[0012] - 5 to 70 phr (parts by weight, based on 100 parts by weight of the total rubber in the mixture) of at least one terpene resin based on more than 95% bio-renewable raw materials,

[0013] - 1 to 40 phr of at least one liquid polybutadiene which is organosilicon-modified and has an average molecular weight Mw according to GPC of 500 to 18000 g / mol, and

[0014] - 40 - 350 phr of at least one filler.

[0015] Surprisingly, it has been found that the specific combination of at least one terpene resin based on more than 95% biorenewable raw materials with a liquid polybutadiene, which is organosilicon-modified and has an average molecular weight Mw according to GPC of 500 to 18,000 g / mol, in the specified amounts in silicic acid-containing diene rubber mixtures leads to a low maximum loss factor tan δmax at 55 °C and a low tan δ (10%) by RPA, which correlates with low rolling resistance when used in tire treads. At the same time, the mixtures according to the invention exhibit good tensile properties, such as high tensile strength and high elongation at break, which is associated with improved structural durability.When the rubber mixture according to the invention is used in the treads of pneumatic vehicle tires, a vehicle tire is obtained which is characterized by good sustainability with good rolling resistance and good durability.

[0016] The term phr (parts per hundred parts of rubber by weight) used in this document is the standard quantity used in the rubber industry for compound formulations. The dosage of the parts by weight of the individual substances is always based on 100 parts by weight of the total mass of all solid rubbers present in the compound.

[0017] In the context of the present invention, the term “a terpene resin based on more than 95% biologically renewable raw materials” is to be understood as meaning a terpene resin which is materially produced from renewable raw materials as a source, with plant sources being particularly preferred.

[0018] According to the invention, the rubber mixture contains at least one diene rubber. Diene rubbers are rubbers produced by polymerization or copolymerization of dienes and / or cycloalkenes and thus contain C=C double bonds either in the main chain or in the side groups.

[0019] The diene rubber(s) is / are preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, styrene-butadiene rubber (SBR), in particular solution-polymerized styrene-butadiene rubber (SSBR) and emulsion-polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, liquid rubbers with a molecular weight Mw of greater than 20,000 g / mol, halobutyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, Acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile-butadiene rubber and hydrogenated styrene-butadiene rubber.

[0020] In particular, nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halobutyl rubber, or ethylene-propylene-diene rubber are used in the manufacture of technical rubber articles, such as belts, straps, and hoses, and / or shoe soles. The preferred blend compositions for these rubbers are those known to those skilled in the art—specific with regard to fillers, plasticizers, vulcanization systems, and additives.

[0021] According to a particularly preferred embodiment of the invention, the diene rubber(s) is / are selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene-

[0022] Rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), and emulsion-polymerized styrene-butadiene rubber (ESBR). This type of rubber compound is particularly suitable for the tread of vehicle tires. Natural polyisoprene is defined as rubber that can be obtained by harvesting sources such as rubber trees (Hevea brasiliensis) or non-rubber tree sources (such as guayule or dandelion (e.g., Taraxacum koksaghyz)). Natural polyisoprene (NR) is understood to be non-synthetic polyisoprene.

[0023] The rubber mixture according to the invention contains 5 to 70 phr, preferably 20 to 60 phr, particularly preferably 30 to 50 phr, of at least one terpene resin based on more than 95% biorenewable raw materials. Several different terpene resins can also be used in the mixture. Preferably, the terpene resin is based 100% on biorenewable raw materials. Terpene resins based on more than 95% biorenewable raw materials can be obtained, for example, from raw materials obtained from the production of fragrances from orange peels. However, the terpene resin is preferably based on by-products obtained from the pulp production of softwoods. Such by-products are commercially available in large quantities and can be refined on an industrial scale into terpene resins.

[0024] According to a preferred embodiment of the invention, the terpene resin is not based on limonene.

[0025] The terpene resin is preferably based on α- and β-pinene. Such terpene resins can be produced from byproducts resulting from the pulp production of softwoods.

[0026] The terpene resin, which is based on more than 95% biorenewable raw materials, preferably has an average molecular weight (Mw) according to GPC of 800 to 1500 g / mol. Such terpene resins are easy to process and exhibit good tensile properties.

[0027] According to a preferred embodiment of the invention, the terpene resin has a softening point of 100 to 140 °C, preferably 110 to 130 °C.

[0028] For good braking performance of the tire whose tread consists of the rubber mixture according to the invention, the terpene resin has a glass transition temperature Tg according to DSC of 50 to 100 °C, preferably 50 to 80 °C.

[0029] Terpene resins that can be used according to the invention include, for example, those of the type Sylvatraxx® 8115 and Sylvatraxx® 8125 from Kraton Chemicals SAS. These are based 100% on biorenewable raw materials and not on limonene. The rubber mixture according to the invention contains 1 to 40 phr, preferably 2 to 17 phr, of at least one liquid polybutadiene that is organosilicon-modified and has an average molecular weight Mw according to GPC of 500 to 18,000 g / mol. The abbreviation Mw stands for the weight-average molecular weight of polymers. The weight-average Mw is determined by means of gel permeation chromatography (GPC with a polybutadiene standard). The Mw value range of 500 to 18,000 g / mol implies that the polybutadiene is liquid at room temperature. For the sake of simplicity, the short term “liquid polybutadiene” is therefore used in the context of the present invention.The Mw value refers to the polybutadiene including the organosilicon modification.

[0030] The liquid polybutadiene can be terminally and / or chain-organosilicon-modified.

[0031] Preferably, the liquid polybutadiene is modified with at least one radical according to formula I):

[0032] (R 1 R 2 R 3 )Si- I) where R 1 , R 2 , R 3in the structures may be identical or different and may be selected from linear or branched alkoxy, cycloalkoxy, alkyl, cycloalkyl, or aryl groups having 1 to 20 carbon atoms, and wherein the radical according to formula I) is bonded directly or via a bridge to the polymer chain of the polybutadiene, and wherein the bridge consists of a saturated or unsaturated carbon chain, which may also contain cyclic and / or aliphatic and / or aromatic elements as well as heteroatoms in or on the chain. Such a modification results in advantages in the rolling resistance of tires.

[0033] According to a preferred embodiment of the invention, the liquid polybutadiene is terminally modified with a triethoxysilane group. These polybutadienes are easy to produce and are commercially available on an industrial scale, for example, under the name Polyvest® EP ST-E 60 from Evonik. To improve winter properties and rolling resistance, the liquid polybutadiene, which is organosilicon-modified, has a glass transition temperature T g according to DSC from -85 to -30 °C. The determination of the glass transition temperature (T g ) of the polymers is carried out using dynamic scanning calorimetry (DSC according to DIN 53765: 1994-03 or ISO 11357-2: 1999-03, calibrated DSC with low temperature device, calibration according to device type and manufacturer's instructions, sample in an aluminum crucible with an aluminum lid, cooling to temperatures lower than -120 °C at 10 °C / min).

[0034] The liquid polybutadiene preferably has a vinyl content (content of 1,2-bonded butadiene, based on the monomers of the polybutadiene polymer chain) of 5 to 30%, particularly preferably 10 to 25%. The liquid polybutadiene preferably has a 1,4-trans content of 40 to 75% (based on the monomers of the polybutadiene polymer chain). The cis content of the liquid polybutadiene is preferably 5 to 30% (based on the monomers of the polybutadiene polymer chain).

[0035] The rubber mixture contains 40 to 350 phr of at least one filler. These can be fillers such as carbon black, silica, aluminosilicates, chalk, starch, magnesium oxide, titanium dioxide, or rubber gels in conventional amounts, whereby the fillers can be used in combination. Carbon nanotubes (CNTs) (including discrete CNTs, so-called hollow carbon fibers (HCFs), and modified CNTs containing one or more functional groups, such as hydroxyl, carboxyl, and carbonyl groups) are also conceivable. Graphite and graphene, as well as so-called "carbon-silica dual-phase fillers," can also be used as fillers.

[0036] Different fillers can be used in the mixture.

[0037] If the rubber mixture contains carbon black, all types of carbon black known to those skilled in the art can be used. However, preference is given to using a carbon black that has an iodine adsorption number according to ASTM D 1510 of 30 to 180 g / kg, preferably 30 to 130 kg / g, and a DBP number according to ASTM D 2414 of 80 to 200 m 1 / 100 g, preferably 100 to 200 m 1 / 100 g, particularly preferably 100 to 180 ml / 100 g. This achieves particularly good rolling resistance indicators (rebound resilience at 70 °C) for use in vehicle tires, along with good other tire properties.

[0038] To reduce rolling resistance, it has proven advantageous for the rubber compound to contain 20 to 200 phr of silica as a filler. Additional fillers, such as carbon black, are also included in the compound, resulting in a total filler content of 40 to 350 phr.

[0039] A wide variety of silicas, such as low surface area or highly dispersible silica, can be used, even in mixtures. It is particularly preferred to use a finely dispersed, precipitated silica with a CTAB surface area (according to ASTM D 3765) of 30 to 350 m². 2 / g, preferably from 110 to 250 m 2 / g. Both conventional silicas such as type VN3 (trade name) from Evonik and highly dispersible silicas, so-called HD silicas (e.g., Ultrasil 7000 from Evonik), can be used as silicas. Silicas produced from rice husk ash are also suitable.

[0040] To improve processability and to bond the silica to the diene rubber in silica-containing mixtures, at least one silane coupling agent is preferably used in the rubber mixture in amounts of 1-15 parts by weight (parts by weight, based on 100 parts by weight of silica). The silane coupling agents can also be used in the mixture.

[0041] The term phf (parts per hundred parts of filler by weight) used in this document is the quantity commonly used in the rubber industry for coupling agents for polar fillers. In the context of the present application, phf refers to the silica present, meaning that other fillers that may be present, such as carbon black, are not included in the calculation of the amount of silane coupling agent. The silane coupling agents react with the surface silanol groups of the silica or other polar groups during mixing of the rubber or rubber mixture (in situ) or even before the filler is added to the rubber in the sense of pretreatment (premodification). Silane coupling agents that can be used are all silane coupling agents known to the person skilled in the art for use in rubber mixtures.Such coupling agents known from the prior art are bifunctional organosilanes which have at least one alkoxy, cycloalkoxy or phenoxy group as a leaving group on the silicon atom and which have as another functionality a group which, optionally after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group can, for example, be the following chemical groups: -SCN, -SH, -NH2 or -Sx- (where x = 2-8). Thus, silane coupling agents which can be used include, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl)polysulfides having 2 to 8 sulfur atoms, such as e.g. B. 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide or mixtures of the sulfides with 1 to 8 sulfur atoms with different contents of the various sulfides can be used.TESPT can also be added, for example, as a mixture with carbon black (trade name X50S from Degussa). Blocked mercaptosilanes, such as those known from WO 99 / 09036, can also be used as silane coupling agents. Silanes such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1, and WO 2008 / 083244 A1 can also be used. Examples of suitable silanes include those marketed under the name NXT® in various versions by Momentive, USA, or those marketed under the name VP Si 363 by Evonik Industries. So-called “silated core polysulfides” (SCP, polysulfides with a silylated core) can also be used, which are described, for example, in US 20080161477 A1 and EP 2 114 961 B1.

[0042] Preferably, at least one silane coupling agent in the rubber mixture is 3,3'-bis(triethoxysilylpropyl) disulfide (TESPD). The rubber mixture according to the invention may further contain various plasticizers. These are preferably present in the mixture in amounts of 5 to 50 phr, particularly preferably 5 to 30 phr. These plasticizers do not include the organosilicon-modified, liquid polybutadienes.

[0043] The plasticizer(s) are preferably selected from the group consisting of plasticizers from renewable raw materials such as rapeseed oil or sunflower oil, mineral oils, phosphoric acid esters such as tri-(2-ethylhexyl) phosphate, and liquid polymers having a weight average molecular weight distribution Mw according to GPC of 60,000 g / mol or less.

[0044] When using mineral oil, it is preferably selected from the group consisting of DAE (Distilled Aromatic Extracts), RAE (Residual Aromatic Extract), TDAE (Treated Distilled Aromatic Extracts), MES (Mild Extracted Solvents), white oils and naphthenic oils, with RAE being particularly preferred.

[0045] According to an advantageous development of the invention, a vegetable oil is used as the plasticizer. This is advantageous from an ecological and economic perspective and offers advantageous properties in tires. It is particularly preferred if the vegetable oil is rapeseed oil.

[0046] Furthermore, the rubber mixture can contain customary additives in customary parts by weight, which are preferably added in at least one basic mixing stage during its production. These additives include a) ageing inhibitors, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) activators, such as zinc oxide and fatty acids (e.g. stearic acid) or zinc complexes such as zinc ethylhexanoate, c) waxes, d) mastication aids, such as B. 2,2'-dibenzamidodiphenyl disulfide (DBD), and e) processing aids, such as fatty acid salts, such as zinc soaps, and fatty acid esters and their derivatives.

[0047] The proportion of the total amount of other additives is 3 to 150 phr, preferably 3 to 100 phr and particularly preferably 5 to 80 phr.

[0048] The vulcanization of the rubber compound is carried out in the presence of sulfur and / or sulfur donors using vulcanization accelerators, whereby some vulcanization accelerators can also act as sulfur donors. The accelerator is selected from the group consisting of thiazole accelerators and / or mercapto accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or thiuram accelerators and / or thiophosphate accelerators and / or thiourea accelerators and / or xanthate accelerators and / or guanidine accelerators.

[0049] Preference is given to using a sulfenamide accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazolesufenamide (CBS) and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or benzothiazyl-2-sulfenemorpholide (MBS) and / or N-tert-butyl-2-benzothiazylsulfenamide (TBBS).

[0050] The rubber compound may also contain vulcanization retarders.

[0051] Any sulfur-donating substance known to the person skilled in the art can be used as the sulfur-donating substance. If the rubber mixture contains a sulfur-donating substance, it is preferably selected from the group consisting of, for example, thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD), tetramethylthiuram disulfide (TMTD) or tetraethylthiuram disulfide (TETD), thiuram tetrasulfides, such as, for example,

[0052] Dipentamethylenethiuram tetrasulfide (DPTT), dithiophosphates such as DipDis (bis-(diisopropyl)thiophosphoryl disulfide), bis(O,O-2-ethylhexylthiophosphoryl)polysulfide (e.g. Rhenocure SDT 50®, Rheinchemie GmbH), zinc dichloryldithiophosphate (e.g. Rhenocure ZDT / S®, Rheinchemie GmbH) or zinc alkyldithiophosphate, and 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and diarylpolysulfides and dialkylpolysulfides.

[0053] Other network-forming systems, such as those available under the trade names Vulkuren®, Duralink®, or Perkalink®, or network-forming systems as described in WO 2010 / 049216 A2, can also be used in the rubber compound. The latter system contains a vulcanizing agent that crosslinks with a functionality greater than four and at least one vulcanization accelerator.

[0054] During the final mixing stage, at least one vulcanizing agent selected from the group consisting of sulfur, sulfur donor, vulcanization accelerator, and vulcanizing agents that crosslink with a functionality greater than four is preferably added to the rubber mixture during its production. This allows the mixed final mixture to be vulcanized to produce a sulfur-crosslinked rubber mixture for use in rubber products, particularly pneumatic vehicle tires.

[0055] The terms “vulcanized” and “crosslinked” are used synonymously in the context of the present invention.

[0056] The rubber compound is manufactured according to the process customary in the rubber industry, in which a base compound containing all components except the vulcanization system (sulfur and vulcanization-influencing substances) is first produced in one or more mixing stages. The finished compound is created by adding the vulcanization system in a final mixing stage. The finished compound is further processed, for example, by an extrusion process, and formed into the appropriate shape. Further processing then takes place by vulcanization, whereby sulfur crosslinking occurs due to the vulcanization system added within the scope of the present invention. The rubber compound can be used for a wide variety of rubber products. It can be used in various components of pneumatic vehicle tires.It is preferably used for the manufacture of pneumatic vehicle tires, such as car, van, truck or two-wheeler tires, wherein the rubber mixture forms at least the part of the tread that comes into contact with the road surface.

[0057] In a pneumatic vehicle tire, the tread can consist of a single compound designed according to the invention. However, pneumatic vehicle tires today often have a tread with a so-called cap / base construction. The term "cap" refers to the part of the tread that comes into contact with the road surface and is arranged radially on the outside (upper tread section or tread cap). The term "base" refers to the part of the tread that is arranged radially on the inside and thus does not come into contact with the road surface during driving or only at the end of the tire's life (lower tread section or tread base). In a pneumatic vehicle tire with such a cap / base construction, at least the rubber compound for the cap is designed according to claim 1.

[0058] The pneumatic vehicle tire according to the invention can also have a tread consisting of different tread compounds arranged side by side and / or one below the other (multi-component tread).

[0059] During the production of the pneumatic vehicle tire, the mixture is formed as a ready-mixed compound into the shape of a tread, preferably at least into the shape of a tread cap, prior to vulcanization and is applied during the production of the green vehicle tire as known in the art. The tread, preferably at least the tread cap, can also be wound onto a green tire in the form of a narrow strip of rubber compound.

[0060] The invention encompasses all advantageous embodiments, which are reflected, inter alia, in the patent claims. In particular, the invention also encompasses embodiments that result from the combination of different features, for example, components of the rubber mixture, with varying degrees of preference for these features, so that a combination of a first feature designated as "preferred" or described within the context of an advantageous embodiment with another feature designated, for example, as "particularly preferred" is also encompassed by the invention.

[0061] The invention will now be explained in more detail using comparative and exemplary embodiments, which are summarized in Table 1.

[0062] The comparison mixtures are marked with V, the mixture according to the invention is marked with E.

[0063] The compound was manufactured according to standard rubber industry procedures under standard conditions in three stages in a laboratory mixer. In the first mixing stage (basic mixing stage), all components except the vulcanization system (sulfur and vulcanization-influencing substances) were mixed. In the second mixing stage, the base mixture was thoroughly mixed again. The final mixture was created by adding the vulcanization system in the third stage (final mixing stage), which was mixed at 90 to 120 °C.

[0064] Subsequently, the loss factor tan δ (10%) of the compound was determined using RPA (rubber process analyzer) in accordance with ASTM D6601 from the second elongation run at 1 Hz, 70°C and 10% elongation in the vulcanized, conditioned state, whereby the test specimens were produced in the apparatus by vulcanization under pressure at 170 °C for 10 minutes.

[0065] Furthermore, test specimens were produced from all mixtures by vulcanization under pressure at 160 °C for 20 minutes and material properties typical for the rubber industry were determined using these test specimens using the test methods specified below:

[0066] - Shore A hardness at room temperature according to ISO 868 - Rebound resilience at room temperature and 70 °C according to ISO 4662

[0067] - Tensile strength at room temperature according to ISO 37

[0068] - Elongation at break at room temperature according to ISO 37

[0069] - Maximum loss factor tan ömax at 55 °C as maximum value over the strain sweep from dynamic mechanical measurement at a frequency of 10 Hz according to ISO 4664-1

[0070] The maximum loss factor tan δmax at 55 °C (Eplexor) and the loss factor tan δ (10%) measured using RPA can be correlated with rolling resistance. A low loss factor tan δmax at 55 °C and a low loss factor tan δ (10%) measured using RPA indicate low rolling resistance. Tensile and elongation properties, such as tensile strength and elongation at break, can be correlated with structural durability.

[0071] Table 1 a Sprintan® SLR-3402, Trinseo, functionalized, solution-polymerized styrene

[0072] Butadiene copolymer with functionalization for the polymer / silica and polymer / carbon black interaction, T g = -62 °C b LBR-302, Kuraray, liquid polybutadiene, T g = -85 °C c Polyvest® EP ST-E 60, Evonik, liquid polybutadiene terminally modified with triethoxysilane, Tg = -80 °C, average molar mass Mw approx. 13600 g / mol (GPC, polybutadiene standard) dZEOSIL® 1165 MP, Solvay SA, BET surface area = 155 m 2 / g (measured with nitrogen), CTAB surface area = 156-157 m 2 / G; e Sylvatraxx® 4401 , Kraton Chemicals SAS, Alpha-Methyl-Styrene resin, softening point = 85 °C (according to ASTM E 28), T g = 45 °C f Sylvatraxx® 8115, Kraton Chemicals SAS, non-limonene-based terpene resin, softening point = 115 °C (according to ASTM E 28), T g = 66 °C s 3, 3'-bis(triethoxysilylpropyl) disulfide (TESPD)

[0073] The data in Table 1 demonstrate that the combined presence of the terpene resin, which is based on more than 95% biorenewable raw materials, with a liquid organosilicon-modified polybutadiene with an average molecular weight Mw according to GPC of 13600 g / mol, in mixture 4(E) improves, i.e., increases, the tensile properties of tensile strength and elongation at break, surprisingly far exceeding the expected effect of the individual measures (sole addition of the modified polybutadiene 2(V) and sole replacement of the alpha-methyl-styrene resin with terpene resin 3(V)). Therefore, mixture 4(E) exhibits high structural durability. The maximum loss factor tan ömax at 55 °C and the tan ö (10%) by means of RPA are also significantly improved, ie reduced, in compound 4(E), which leads to a reduced rolling resistance in the treads of pneumatic vehicle tires.

Claims

Patent claims 1 . Sulphur-curable rubber mixture, in particular for the tread of pneumatic vehicle tires, containing at least the following components: - at least one diene rubber, - 5 to 70 phr (parts by weight, based on 100 parts by weight of the total rubber in the mixture) of at least one terpene resin based on more than 95% bio-renewable raw materials, - 1 to 40 phr of at least one liquid polybutadiene which is organosilicon-modified and has an average molecular weight Mw according to GPC of 500 to 18000 g / mol, and - 40 - 350 phr of at least one filler.

2. Sulphur-crosslinkable rubber mixture according to claim 1, characterized in that it contains 20 to 60 phr, preferably 30 to 50 phr, of at least one terpene resin based to more than 95% on biologically renewable raw materials.

3. Sulphur-crosslinkable rubber mixture according to claim 1 or 2, characterized in that the terpene resin is based 100% on biologically renewable raw materials.

4. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin is not based on limonene.

5. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin is based on α- and β-pinene.

6. Sulfur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin has an average molecular weight Mw according to GPC of 800 to 1500 g / mol.

7. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin has a softening point of 100 to 140 °C, preferably 110 to 130 °C.

8. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin has a glass transition temperature Tg of 50 to 100 °C, preferably of 50 to 80 °C.

9. Sulfur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that it contains 2 to 17 phr of the liquid polybutadiene which is organosilicon-modified.

10. Sulfur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the liquid polybutadiene is terminally and / or organosilicon-modified along the chain.

11. Sulfur-crosslinkable rubber mixture according to claim 10, characterized in that the liquid polybutadiene, which is organosilicon-modified, is terminally modified with a triethoxysilane group.

12. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the liquid polybutadiene, which is organosilicon-modified, has a glass transition temperature T g according to DSC from -85 to -30 °C.

13. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that it contains 20 to 200 phr of silica as filler.

14. A pneumatic vehicle tire having at least one component consisting of a sulfur-vulcanized rubber mixture according to one of claims 1 to 13.

15. Pneumatic vehicle tire according to claim 14 having a tread whose part at least coming into contact with the road surface consists of a sulfur-vulcanized rubber mixture according to one of claims 1 to 13.

Citation Information

Patent Citations

  • Silated core polysulfides, their preparation and use in filled elastomer compositions

    EP2114961B1

  • Elastomeric compositions for tyre components and tyres thereof

    EP3350259B1

  • Winter tyres

    EP3350260B1

  • Pneumatic tire

    US10654995B2

  • Silated core polysulfides, their preparation and use in filled elastomer compositions

    US20080161477A1