Glazing with low emissivity coating and enhanced bendability
The use of two separated TCO layers in the low-emissivity coating for automotive glazing addresses the brittleness and cracking issues of traditional coatings, enhancing bendability and thermal performance while maintaining low emissivity and visibility in complex shapes.
Patent Information
- Application Number
- PCT/EP2024/058387
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Traditional low-emissivity coatings in automotive glazing, particularly those using indium-tin-oxide (ITO), face challenges with brittleness and cracking when bent to complex shapes, which affects their performance and durability, especially in reducing heat transfer and maintaining visibility.
A low-emissivity coating comprising two transparent conductive oxide (TCO) layers separated by a separation layer, which reduces the risk of cracking and enhances bendability, while maintaining low emissivity and optical transparency, by distributing stress more evenly and reducing the thickness of individual TCO layers.
The solution effectively minimizes crack initiation strain by 30% and maintains low emissivity, improving the glazing's ability to control thermal radiation and visibility, even in complex curved shapes, thus addressing the brittleness issues of traditional coatings.
Smart Images

Figure EP2024058387_03102024_PF_FP_ABST
Abstract
Description
[0001] GLAZING WITH LOW EMISSIVITY COATING AND ENHANCED BENDABILITY
[0002] DESCRIPTION
[0003] FIELD OF THE INVENTION
[0004] The present invention falls in the field of glazing and more particularly, it relates to low- emissivity coatings disposed on automotive glazing, such as automotive roof, with low- emissivity capabilities. The invention also relates to a method for manufacturing such glazing with low-emissivity capabilities.
[0005] BACKGROUND
[0006] Low-emissivity coatings, abbreviated ‘low-E’, are commonly known in the state of the art. Historically, the term ‘low-E’ has been used interchangeably for two types of coatings.
[0007] First, in the architectural glass industry, this term is typically applied to solar-control (usually, silver-inclusive) coatings, while in the automotive glazing, ‘low-E’ typically implies a highly electrically conductive coating on the inner surface of a glass roof serving to prevent the absorption and consequent re-radiation of the heat energy from the sun on hot days into the passenger compartment. The more energy is transferred throughout the glass roof, the more fuel must be spent to keep the air conditioner working in order to provide passengers’ comfort. Besides, an automotive roof without a low-E coating may absorb sufficient solar radiation so that it gets very hot on touch.
[0008] In winter, the situation is the opposite: automotive roofs with a higher emissivity lose more heat energy to the cold environment from the inside of the vehicle towards the outside the vehicle, thus putting more load on the vehicle's heater to keep passengers warm.
[0009] There is a steadily growing segment for opaque glazing with strict requirements for thermal insulation. Examples include automotive roofs with zero- or next-to-zero visible transmission (such as roofs with laminated photovoltaic panels, colored non-transparent roofs, etc.), opaque decorative architectural facades, etc. Thermally insulating glazing employ two primary physical phenomena which can simultaneously be used in the same glazing:
[0010] 1) Reflectance of near-IR portion of solar light using so-called solar control coatings or infrared (IR) reflecting coatings, such as silver-based. These types of coatings are usually applied on an inner surface of a laminated glazing implemented as automotive windshields or roofs or on the inner surface of an architectural integrated glass unit.
[0011] 2) Reflectance of mid-IR portion of the solar spectrum in order to prevent it from being re-radiated by the glazing. This type of coating is called low-emissivity (Low-E) coating and is applied on the innermost surface of the glazing, thus preventing heat transfer by means of a combination of conduction and radiation, thus preventing heat energy absorption and subsequent re-radiation.
[0012] Traditional Low-E coatings used in automotive roofs use a layer of indium-tin-oxide (ITO), a transparent conductive oxide (TOO) with a sufficiently high sheet resistance to enable a low emissivity and, at the same time, be sufficiently transparent to provide daylight coming through the roof into the vehicle interior. The ITO layer is sandwiched between at least two dielectric layers that may also serve as a blocker against sodium diffusion from the glass and as top scratch protection layer.
[0013] Emissivity (E) is a measure of how much thermal radiation a body, such as an automotive glass roof, absorbs from one of its sides and re-emits to the other. This characteristic is unitless and ranges between 0 and 1. It is inversely proportionate to sheet resistance of a low-E coating. Thus, the higher the sheet resistance, the lower emissivity of the roof can be achieved.
[0014] In a typical manufacturing cycle, a low-E coating is deposited, by means of e.g. magnetron sputtering on a surface of a predominantly flat glass pane which becomes the surface oriented towards the inside of a vehicle where such a glass pane would be implemented. The ITO layer requires post-deposition activation for its crystallization to attain high levels of both electrical conductivity and optical transmission. The activation is usually achieved as a stand-alone thermal-assisted step or / and during high- temperature bending which is required to curve each of the two glass panes to a desired shape before laminating them together by means of a thermoplastic bonding layer, such as PVB.
[0015] Typical low-E coatings require a low sheet resistance material on the outer surface of the glazing oriented towards the inside of the vehicle.
[0016] Recently, one of the modern automotive trends is to use more ‘aggressive’ shapes of glazing with reduced curvature radii of glass. This is done for both a better aesthetics and to improve aerodynamic characteristics of the vehicle. Bending the constituents of a low-E coating, especially brittle polycrystalline layers such as ITO, to such ‘aggressive’ 3D shapes is a challenge.
[0017] In this regard, there is a need in the art for a glazing with a low-E coating with a suppressed brittleness and improved bendability, in particular, in the complex shaped glazing where ITO layers are known for cracking.
[0018] There is also a need in the art for a glazing having said low-E coating, wherein the glazing is suitable for being installed in a vehicle.
[0019] Finally, there is also a need in the art for a method for manufacturing such glazing having the low-E coating with the aforementioned needs.
[0020] DESCRIPTION OF THE INVENTION
[0021] The present invention provides a solution for the above-mentioned issues by providing a glazing with low-emissivity capacities according to independent claim 1 , a roof for a vehicle according to claim 11 , a vehicle comprising a glazing according to claim 12 and a method for manufacturing a glazing with low-emissivity capabilities according to claim 13. In dependent claims, preferred embodiments of the invention are defined.
[0022] The following terminology is used along the whole document to describe features of the invention.
[0023] The term “layer”, as used in this context, shall include the common definition of the word, i.e.: a sheet, quantity, or thickness, of material, typically of some homogeneous substance. The term “index of refraction”, “refractive index” (or “refraction index”), or its acronym IOR are synonyms and may be used interchangeably. It should be understood as a dimensionless number that gives the indication of the light bending ability of that medium (i.e. the material). The refractive index determines how much the path of light is bent, or refracted, when entering a material. The refractive index may vary with wavelength. This causes white light to split into constituent colors when refracted. This is called dispersion. Light propagation in absorbing materials can be described using a complex-valued refractive index. The imaginary part then handles the attenuation, while the real part accounts for refraction. For most materials the refractive index changes with wavelength by several percent across the visible spectrum. Refractive indices for materials are commonly reported using a single value, for example measured at 633 nm or at 550 nm. In the case of the present invention, the refractive index of the layer of the first phase-control layer is measured at a wavelength reference of 550 nm.
[0024] As it has already been mentioned, the term “emissivity” or its acronym “E” is a measure of how much thermal radiation a material's surface, such as an automotive glass roof, emits to its environment. Thermal radiation is electromagnetic radiation that may include both visible radiation (light) and radiation, which is not visible to human eyes. The thermal radiation from very hot objects is easily visible to the eye. Quantitatively, emissivity is the ratio of the thermal radiation from a surface to the radiation from an ideal black body at the same temperature as given by the Stefan Boltzmann law. This characteristic is unitless and ranges between 0 and 1. It is inversely proportionate to sheet resistance of a low-E coating. The higher the sheet resistance, the lower emissivity of the roof can be achieved. A low-E should be understood as below or equal to 0.3; and preferably below or equal to 0.2.
[0025] The term “optical thickness” means the geometric thickness of the material multiplied by the refractive index of the material at a reference wavelength of 550 nm. For example, a material having a geometric thickness (also called physical thickness) of 5 nm and a refractive index of 2.0 at a reference wavelength of 550 nm would have an optical thickness of 10 nm.
[0026] Thickness values, unless indicated to the contrary, are geometric thickness values. The term “glass substrate” or “glass pane” should be understood as a sheet, quantity, or thickness of material, typically of some homogeneous substance. The “glass substrate or pane” may comprise one or more layers. The glass substrate can be, for example, clear float glass or can be tinted or colored glass. The glass substrate can be of any desired dimensions, e.g., length, width, shape, or thickness.
[0027] The terms “glass pane” and “laminated glass pane” refer respectively to a glazing having one glass layer and to a laminated glazing having at least two glass layers respectively.
[0028] “Laminates”, in general, are products comprised of multiple sheets of thin, relative to their length and width, material, with each thin sheet having two oppositely disposed major faces and typically of a relatively uniform thickness, which are permanently bonded to each other across at least one major face of each sheet.
[0029] The term “stack” refers to the arrangement in a pile manner of a plurality of layers. When describing the coating stack, the convention of numbering the coating layers in the order of deposition upon the glass substrate should be used.
[0030] Also, throughout this document, when two layers of the coating are described, the one which is the closest to the substrate shall be referred to the bottom layer or the first layer and the subsequent layers shall be referred to second layer, and so on. Likewise, the top layer is the very last layer applied to the coating stack.
[0031] As for one individual layer of the coating, the top of an individual layer has to be understood as the side of the layer furthest from the substrate while the bottom has to be understood as the side of the layer which is either in contact with the substrate or oriented towards the substrate in case this layer is not the first layer of the coating stack.
[0032] With respect to a second layer located on a first layer in the coating, the term “on” should be understood as including both the option of the first and second layers being in direct contact (i.e. physical contact) and the option of having one or more additional layers located between the first layer and the second layer. The term “glass” can be applied to many organic and inorganic materials, including many that are not transparent. From a scientific standpoint, “glass” is defined as a state of matter comprising a non-crystalline amorphous solid that lacks the long-range ordered molecular structure of true solids. Glasses have the mechanical rigidity of crystals with the random structure of liquids.
[0033] The term “glazing” should be understood as a product comprised of at least one layer of a transparent material, preferably glass, which serves to provide for the transmission of light and / or to provide for viewing of the side opposite to the viewer and which is mounted in an opening in a building, vehicle, wall or roof or other framing member or enclosure.
[0034] Among the elements of a valuable appearance is the color of for example a vehicle roof laminate. Color can be described mathematically. Cl ELAB is one of the many color spaces and is normally used in automotive and architectural industries. The advantage of the Cl ELAB color system is that color shifts on the Cl ELAB diagram are perceived proportionally by the human eye. The Cl ELAB L*, a*, b* color space mathematically describes all perceivable colors in three dimensions: L* for perceptual lightness, a* for green-red, and b* for blue-yellow. See Hunter Lab, Applications Note, "Insight on Color," Vol. 8, No. 7 (2008). In the CIELAB color space, the L* axis runs from top to bottom. The maximum L* value is 100, which indicates a perfect reflecting diffuser (i.e., the lightest white). The minimum L* value is 0, which indicates a perfect absorber (i.e., the darkest black). Positive a* is red. Negative a* is green. Positive b* is yellow. Negative b* is blue. CIELAB a* or b* values equal to 0 indicate no red-green or blue-yellow color appearance, in which case the article would appear pure white. In contrast, a* or b* values that deviate far from 0 indicate that light is non-uniformly absorbed or reflected. As a* or b* values deviate from 0, the color may no longer appear as bright white. One of the most important attributes of the CIELAB model is device independence, which means that the colors are defined independent of their nature of creation or the device they are displayed on.
[0035] The L*, a*, and b* values of the CIELAB color scale can be obtained using any CIELAB color measurement instrument and are calculated from known formulas. See Hunter Lab, Applications Note, "Insight on Color," Vol. 8, No. 7 (2008).
[0036] Thus, the uniqueness of the Cl ELAB space is in its perceived uniformity. A change in the numerical difference between two color coordinates is proportionate difference in color perceived by the eye.
[0037] The terms “metal” and “metal alloy” include the traditionally recognized metals and metal alloys. Silicon and silica are non-metallic materials. By saying that the first electrically conductive layer is a metal or metal alloy it follows that the first electrically conducting layer cannot be an ITO. Due to the fact that an ITO is an N-type semiconductor with a large bandgap of around 4 eV, it is not strictly metallic.
[0038] When a range of values is provided in the application, it should be understood that the two limiting values of the range are also included. For example, if a range of 20 to 100 nm is provided, the values 20 and 100 nm are also included within the range.
[0039] In a first inventive aspect, the present invention provides a glazing with low-emissivity capabilities comprising: at least one glass layer having a first major surface and a second major surface, and a low-emissivity coating comprising: a first dielectric layer disposed on at least one portion of the first major surface or the second major surface of the at least one glass layer, a first transparent conductive oxide layer disposed on the first dielectric layer, a separation layer disposed on the first TCO layer, a second TCO layer disposed on the separation layer, wherein the visible reflectance (RVis) from the top layer of the coating, measured at an angle of 8 degrees, is lower than 15%, preferably in the range 1 to 10%, more preferably in the range 1.2 to 6%, even more preferably in the range 1.5 to 4%, and the sheet resistance of the coating is lower than 50 O / sq, preferably lower than 30 O / sq, more preferably lower than 25 O / sq.
[0040] The glazing of the present invention has low-emissivity capabilities thanks to the layers of the low-emissivity coating which comprises a first dielectric layer, a first TCO layer, a separation layer, and a second TCO layer.
[0041] The visible reflectance from the top layer of the coating, measured at an angle of 8 degrees, is lower than 15%, and the sheet resistance of the coating is lower than 50 Q / sq.
[0042] Advantageously, the glazing of the invention comprises a coating which comprises two transparent conductive oxide (TCO) layers, both separated by a separation layer. By implementing two TCO layers instead of one unique TCO layer, which are the most fragile layer once under compression, the two TCO layers of the coating of the invention have less risk of cracking allowed by the fact of being divided into two separated layers.
[0043] The low-emissivity coating comprised in the glazing of the invention is substantially optically transparent.
[0044] Also, thanks to the coating disposed on the glazing of the invention, the two TCO layers separated by the separation layer help controlling the visible reflectance (RVjS) from the top layer of the glazing.
[0045] In glazing of the state of art having conventional coatings comprising one TCO layer, said layer is normally the thickest layer of the stack. At the same time, the thicker the layer, the more risk there is in cracking under stress. Therefore, the glazing of the present invention provides a solution to high complexity curvature glazing, since it comprises two separated TCO layers, each TCO layer being thinner than a glazing comprising one unique TCO layer of a coating of the state of the art and, thus, it results in less risk of cracking any of the two TCO layers when applying external stress, implying in eventual strain on the glazing.
[0046] Thus, the glazing of the present invention provides a solution regarding the reduction and minimization of stress on the coating layers, especially on the TCO layers.
[0047] By reducing TCO thickness, that is, by dividing a unique layer in two separated TCO layers as in the glazing of the invention, inventors surprisingly observed that the Crack Initiation Strain of the glazing is reduced by 30% compared to having one unique TCO layer in a coating as it is known in the art.
[0048] The TCO layers of the present invention are highly conductive and transparent which brings an enhanced visibility through the glazing of the invention, enhanced emissivity control, and independent control of transmission inside the glazing of the invention.
[0049] In some embodiments, the TCO layers are amorphous TCO.
[0050] The coating of the glazing of the invention also comprises a first dielectric layer. The first dielectric layer is located between at least one glass layer and the first TCO layer and intends to block sodium migration from the glass layer into the coating layers.
[0051] In some embodiments, the coating of the glazing of the invention comprises more than two TCO layers, each TCO layer being separated of the next TCO layer by a separation layer.
[0052] Preferably, the coating of the glazing of the invention has an emissivity less than 0.3, preferably less than 0.2, and more preferably less than 0.1.
[0053] The first and second major surfaces of the at least one glass layer are to be understood as the external surfaces of the at least one glass layer. That is, in case of a monolithic glass, both surfaces of the glass are major surfaces. In other cases, when the glazing comprises more than two glass layers, these glass layers are bonded one with the other and, thus, the surfaces that remain free of bonding material, i.e. , the external surfaces of the at least two glass layers, are the first and second major surfaces of the glazing formed by the at least two glass layers.
[0054] In a particular embodiment, the glazing of the invention further comprises a second dielectric layer disposed on the second TCO layer.
[0055] Advantageously, the second dielectric layer may be implemented in the glazing of the invention in order to prevent scratching of any of the layer of the coating. Thus, the TCO layers indirectly located in between a first and a second dielectric layer, respectively as bottom and top layer of the coating, mostly for protection purposes.
[0056] Furthermore, the provision of a metallic material in the first dielectric layer and / or in the second dielectric layer provides a lower resistivity to the coating, which is one of the objectives for, for example, low-E automotive roofs. In a particular embodiment, the separation layer is metal, an alloy, a semiconductor or a dielectric layer In a preferred embodiment, the separation layer is metal, an alloy or a semiconductor
[0057] In preferred embodiments, the separation layer is metal since said element enhances optical properties of the coating comprised in the glazing of the invention. In particular, introducing a separation layer which is metal, an alloy, a semiconductor or a dielectric layer, results in an improved emissivity and / or adds a darker coloration to the glazing.
[0058] In some embodiments, the separation layer comprises a plurality of sublayers combined in order to form the separation layer.
[0059] In a particular embodiment, the first and / or second TCO layers are Indium Tin Oxide (ITO), InZnOx, ZnAIOx, ZnSnOx or NiCrOx.
[0060] In a particular embodiment, the glazing further comprises a first additional layer located between the first dielectric layer and the first TCO layer, provided that such first additional layer is not a TCO layer
[0061] The first additional layer, which is not a TCO layer, located in between the first dielectric layer and the first TCO layer forms a specific sequence of layer, from the inside of the coating towards the glass layer, which is: separation layer - first TCO layer - first additional layer. This particular sequence of layers provides to the glazing an enhanced control of the exterior reflection color thanks to the combination of the emissivity management of both TCO layer and an additional layer, which is not a TCO layer, such as the first additional layer or the separation layer. This specific sequence of layer forms an optical interference cavity.
[0062] In a particular embodiment, the glazing further comprises a second additional layer located between the second TCO layer and the second dielectric layer, provided that such second additional layer is not a TCO layer
[0063] When the glazing comprises a second additional layer, the sequence of layers: separation layer - second TCO layer - second additional layer, provides to the glazing an enhanced control of the interior reflection color thanks to the combination of the emissivity management of both the TCO layer and an additional layer, which is not a TCO layer, such as the second additional layer or the separation layer. This specific sequence of layer forms an optical interference cavity.
[0064] In some embodiments, the glazing comprises a first additional layer and a second additional layer, both not TCO layers, which provides two sequences of separation layer - TCO layer - additional layer in the same coating. Therefore, the coating comprises two optical interference cavities in the same coating. By changing the reflectance of the first additional layer or the second additional layer, it provides two reflected waves which interfere with each other at different intensity levels. By tuning the thickness of the first and / or the second TCO layers, this enables tuning the phase between the reflected waves. Therefore, implementing a first and a second additional layers allow an optimal control of the intensity and color of reflected light penetrating the glazing of the invention. Additionally, the control of the intensity and color of the reflected light is independent for exterior and interior sides of the glazing as a result of the two sequences of separation layer - TCO layer - additional layer provided in the same coating.
[0065] Advantageously, the first additional layer, the second additional layer and the separation layer are more conductive than the TCO layers. Said combination provides to the glazing an optimal control of the transmittance, reflectance and absorptance of the light going through each layer of the coating.
[0066] In some embodiments, the first additional layer and / or the second additional layer is / are metal layer(s).
[0067] In some embodiments, the first additional layer and / or the second additional layer comprise Ni, Cr, NiCr, NiCr alloy, Al, AIOx, Ag, Ti, NbOx or a combination thereof. In some embodiments, the first additional layer and / or the second additional layer comprise Ni, Cr, NiCr, NiCr alloy, Al, AIOx, Ti, NbOx or a combination thereof. In preferred embodiments, the first additional layer and / or the second additional layer do not comprise Ag.
[0068] In a particular embodiment, the separation layer comprises Ni, Cr, NiCr, NiCr alloy, Al, AIOx, Ag, Ti, NbOx or a combination thereof. In an embodiment, the separation layer comprises Ni, Cr, NiCr, NiCr alloy, Al, AIOx, Ti, NbOx or a combination thereof. In preferred embodiments, the separation layer does not comprise Ag.
[0069] Advantageously, the metal and / or alloy materials above mentioned are selected from materials having a melting point above the temperature required for glass bending which depends on the type of glass implemented in the glazing.
[0070] Also advantageously, Al and Ti have a high affinity to oxygen and tend to quickly form a protective ultra-thin oxide layer when exposed to high processing temperatures or in an oxygen atmosphere. This oxide layer is very stable, self-healing, and protects the bulk of the metal layer from further oxidation.
[0071] In a particular embodiment, the dielectric layers comprise material selected from the following list: SiOx, SiOxNy, SiNx, TiOx, TiSiOx, ZrOx, ZrTiOx, AIOx, CrOxSi, AITiOx, and ZrSiOx.
[0072] The dielectric materials are, preferably, with a zero or very low extinction coefficient (fully oxidized and stoichiometric).
[0073] In a particular embodiment, the thickness of the first TCO layer and / or the thickness of the second TCO layer is / are comprised in the range of 20 to 100 nm, more preferably in the range of 40 to 60 nm.
[0074] In a particular embodiment, the thickness of the separation layer is comprised in the range 1 to 55 nm, more preferably in the range of 5 to 20 nm.
[0075] In a particular embodiment, the thickness of the first dielectric layer is comprised in the range of 10 to 120 nm, more preferably between 20 and 85 nm.
[0076] In a particular embodiment, the thickness of the second dielectric layer is comprised in the range of 10 to 120 nm, more preferably in the range of 20 to 85 nm.
[0077] In a particular embodiment, the thickness of the first additional layer is comprised in the range of 2 to 25 nm, more preferably in the range of 3 to 15 nm.
[0078] In a particular embodiment, the thickness of the second additional layer is comprised in the range of 2 to 25 nm, more preferably in the range of 3 to 15 nm.
[0079] In a particular embodiment, the at least one glass layer is a laminated glazing comprising two glass layers and at least one plastic bonding layer permanently bonding said two glass layers.
[0080] In a particular case of a laminated glazing having a first and a second glass layer, the first glass layer has an outer surface, also called surface 1 , and an inner surface, also called surface 2, wherein the inner surface of the first glass layer is facing the inner surface of the second glass layer. Furthermore, the inner surface of the second glass layer is called surface 3 and the outer surface of the second glass layer, also called surface 4, is facing towards the side where the first glass layer is not located. Therefore, in a laminated glazing having a first and a second glass layers, surface 1 and surface 4 are the major surfaces of said laminated glazing.
[0081] In automotive applications, surface 4 of a laminated glazing is the innermost surface of the glazing, i.e. the surface of the glass layer intended to face the interior of a vehicle when the glazing is in the operating position.
[0082] In the particular case of the present invention, the coating is preferably deposited on surface 4 of the laminated glazing. In some extents, the coating is the part of the glazing which defines which surface is called surface 4. Before the coating is deposited, either the first or the second major surface of the laminated glazing is to be considered surface 4 of the substrate.
[0083] In a particular embodiment, the low-emissivity coating, when measured from the top layer of the coating, at a viewing angle of 0°, has color values in the CIELAB color system wherein: a* is in the range of -15.0 to +1.0, more preferably in the range of -5.0 to 0, and b* is in the range of -10. O to +10.0, and more preferably in the range of -5.0 to +5.0.
[0084] Advantageously, the present invention helps controlling the optical properties of the low- emissivity coating. A neutral or slightly blue or greenish-blue reflection color of the side of the last layer of the coating is preferred for all the viewing angles. Purple or yellow transmitted and reflected colors are typically undesirable, including those at high viewing angles. In the CIELAB color system, neutral colors are defined by a* and b* color values of approximatively zero, while blue colors are characterized by negative b* color values, and red colors by positive a* color values.
[0085] In a particular embodiment, the glazing has a visible light transmittance of at most 90%, preferably in the range of 4 to 70%, more preferably in the range of 15 to 25%.
[0086] In a particular embodiment, the at least one glass layer is bent or partially bent.
[0087] In the context of the invention, to evaluate the complexity associated with the shape of a curved glass layer of the glazing, the inverse process of the bending process is considered. According to said inverse process, the glass layer is bent from target shape to flat. Thus, the inverse process is a flattening process. A finite element model can be implemented for the flattening process and solved by a structural non-linear solver such as Abaqus. The Maximal Compressive Strain (MCS) is defined herein as the maximal area strain that is generated on the mid-surface of the glass layer during the flattening process, that corresponds to the opposite (that is with a minus sign) of the minimal area strain for the bending process. For a point on the mid-surface, area strain corresponds to the sum of maximal and minimal in-plane principal components of the strain tensor for the same point. The finite element model is based on elastic properties of glass. Midsurface is formally defined as the imaginary surface that is equidistant from outer and inner surfaces of the glass layer.
[0088] In an embodiment, evaluation of the MCS value for an actual glass layer of the glazing can be made according to a method comprising the following steps:
[0089] (1) Scanning the glass layer surface to obtain a computer file including a cloud of points or a mesh that represents accurately the glass layer surface and size. Any surface of the glass layer may be scanned (i.e. any major surface of the glass layer), preferably a convex major surface of the glass layer, such as the surface intended to be an outer surface of the glazing when the glazing is in an operating position.
[0090] (2) Building a continuous surface that interpolates the cloud of points or mesh, for example using a CAD software.
[0091] (3) Building a finite element mesh from the obtained surface, the finite element mesh comprising nodes and shell elements, for example triangular and / or quadrilateral shell elements, such as S3 and / or S4 elements in Abaqus. Preferably, the finite element mesh is fine enough for the MCS value to be unchanged if the mesh is further refined.
[0092] (4) Associating to the shell elements the elastic properties of glass. In an embodiment, the following properties are used: E-modulus = 70 GPa and Poisson ratio = 0.22.
[0093] (5) Rotating the finite element mesh in a way that it be essentially horizontal in the initial state of the analysis.
[0094] (6) Defining a static non-linear analysis.
[0095] (7) Creating boundary conditions forz-coordinates that will displace each individual node from its original z-coordinate to z=0, wherein z-direction is perpendicular to the horizontal plane. No boundary conditions on x- and y-coordinates are defined, so the shape can unfold in a natural manner during the flattening process, without generating artificial strains. It is allowed to fix x- and y-coordinates for one single node in the center of the finite element mesh to constrain rigid body motion and help convergence.
[0096] (8) Running the static non-linear analysis.
[0097] (9) Building a field output that is defined as the sum of maximal and minimal inplane principal strains. MCS value is the maximal value of this field output found in the mid-surface of the glass layer.
[0098] In an embodiment, at least one glass layer of the glazing has a Maximal Compressive Strain (MCS) greater than 7.
[0099] In an embodiment, every glass layer of the glazing has a Maximal Compressive Strain (MCS) greater than 7. In an embodiment, the glazing has two glass layers and both glass layers have a Maximal Compressive Strain greater than 7.
[0100] In some embodiments, the low-E coating is deposited on a flat glass layer and after that the resulting glazing is fully bent to achieve a fully bent configuration glazing.
[0101] In some other embodiments, the low-E coating is deposited on a partially bent glass layer and after that the resulting glazing is additionally bent to achieve a fully bent configuration glazing. In some other embodiments, the low-E coating is deposited on a fully bent glass layer without any other additional bent step.
[0102] In some other embodiments, the low-E coating is deposited on a fully bent and fully laminated glazing without any other additional bent step.
[0103] In a particular embodiment, the at least one glass layer is soda lime glass, aluminosilicate glass or borosilicate glass.
[0104] Preferably, the glazing according to any of the embodiments has a radius of curvature that infers to a complex shape or complex curvature.
[0105] In a second inventive aspect, the present invention provides a roof for a vehicle comprising a glazing according to any of the embodiments of the first inventive aspect of the invention.
[0106] In some embodiment, the glazing is a laminated glazing for a vehicle having a coating as corresponding to any of the embodiments previously mentioned, for example suitable for a roof, a windshield or a sidelite of a vehicle. In another embodiment, the glazing is an architectural glazing.
[0107] In a particular embodiment, the roof comprises a laminated glazing having two or more bonded glass layers and at least one bonding layer in between glass layers.
[0108] The term “vehicle” in the present invention includes, but is not limited to, road vehicles (e.g. cars, busses, trucks, agricultural and construction vehicles, cabin motorbikes), railway vehicles (e.g. locomotives, coaches), aircraft (e.g. airplanes, helicopters), boats, ships and the like. For instance, the vehicle may be a road vehicle and more particularly a car.
[0109] In a third inventive aspect, the present invention provides a vehicle comprising at least one glazing according to any of the embodiments of the first inventive aspect of the invention, or any combination thereof, or to any of the embodiments of the second inventive aspect of the present invention. The glazing of the invention, when implemented in a vehicle, is to be oriented such that the coating is located towards the inside of said vehicle and, thus, the remaining major surface of the glazing, the one free of coating, is oriented towards the outside of the vehicle.
[0110] In a fourth inventive aspect, the present invention provides a method for manufacturing a glazing according to any of the embodiments of the first inventive aspect of the invention, the method comprising the following steps: a) providing at least one glass layer having a first major surface and a second major surface, b) depositing the first dielectric surface of the low-emissivity coating on at least a portion of the first or the second major surface of the at least one glass layer, c) depositing the remaining layers of the low-emissivity coating according to any of the embodiments of the first inventive aspect.
[0111] In a particular embodiment of the method, in steps b) and c), the layers are deposited on the first or the second major surface of the at least one glass layer by means of sputter deposition, sol-gel deposition, spraying deposition.
[0112] In a particular embodiment of the method, before step b), the at least one glass layer is partially bent.
[0113] In a particular embodiment of the method, before step b), the at least one glass layer is partially bent and, after step c), the glazing is fully bent.
[0114] In a particular embodiment of the method, before step b), the at least one glass layer is fully bent.
[0115] In a particular embodiment of the method, the at least one glass layer comprises at least a first and a second glass layers, and wherein said first and second glass layers are further laminated, before step b) or after step c), with at least one plastic bonding layer.
[0116] In any embodiment, where the glazing of the invention is fully bent, said glazing is to be considered of high complexity curvature, that is that the glazing is bent and includes curvature in two directions, also called compound curvatures. The glazing of the invention is intended to provide high bendability performances and, thus, respond to high maximum compressive strain greater than 7.
[0117] All the features described in this specification (including the claims, description and drawings) can be combined in any combination, with the exception of combinations of mutually exclusive features and / or steps.
[0118] DESCRIPTION OF THE DRAWINGS
[0119] These and other features and advantages of the invention will be seen more clearly from the following detailed description of a preferred embodiment provided only by way of illustrative and non-limiting example in reference to the attached drawings.
[0120] Figures 1 to 4 These figures show a side view of a glazing (1) comprising a low emissivity coating (3) according to different embodiments of the present invention.
[0121] DETAILED DESCRIPTION OF THE INVENTION
[0122] As will be appreciated by one skilled in the art, aspects of the present invention may be embodied as a product, a system or a method.
[0123] The present invention provides a glazing (1) comprising at least one glass layer (2, 2.1 , 2.2) having a first major surface (2.1.1) and a second major surface (2.2.1)
[0124] The glazing (1) comprises a low-emissivity coating (3) comprising a first dielectric layer (4.1) disposed on at least one portion of the first major surface (2.2.1) or second major surface (2.1.1) of the at least one glass layer (2), a first transparent conductive oxide (TCO) layer (5.1) disposed on the first dielectric layer (4.1), a separation layer (6) disposed on the first TCO layer (5.1), and a second TCO layer (5.2) disposed on the separation layer (6).
[0125] The visible reflectance (RVjS) from the top layer of the low-emissivity coating (3), measured at an angle of 8 degrees, is lower than 15%. The sheet resistance of the coating (3) is lower than 50 Q / sq.
[0126] Embodiments of the glazing (1) of the invention are shown and detailed in the following Figures 1 to 4.
[0127] Figure 1 shows a glazing (1) having one glass layer (2), also called glass pane, where a low-emissivity coating (3) is deposited on one surface of said glass layer (2), either the first or the second major surface (2.1.1 , 2.2.1). The low-emissivity coating (3) of the present Figure includes the first dielectric layer (4.1) disposed in contact with one surface of the glass layer (2). Then, the first transparent conductive oxide layer (5.1) is disposed on the surface of the first dielectric layer (4.1) which is not deposited on the glass layer (2). The coating (3) includes a second TCO layer (5.2) which is separated from the first TCO layer (5.1) by a separation layer (6).
[0128] In the present invention, the first dielectric layer (5.1) is part of the coating (3) in order to avoid migration of sodium from the glass layer (2) to the other layers of the coating (3).
[0129] In an embodiment, the sheet resistance of the coating (3) is preferably lower than 30 Q / sq, more preferably lower than 25 Q / sq.
[0130] In an embodiment, the separation layer (6) is metal, an alloy, a semiconductor or a dielectric layer. In a preferred embodiment, the separation layer (6) is metal, an alloy or a semiconductor.
[0131] In an embodiment, the first (5.1) and / or second TCO layers (5.2) are Indium Tin Oxide (ITO), InZnOx, ZnAIOx, ZnSnOx or NiCrOx.
[0132] In an embodiment, the visible reflectance RVjSis comprised in the range 1 to 10%, preferably in the range 1 .2 to 6%, more preferably in the range 1 .5 to 4%.
[0133] In an embodiment, the thickness of the first TCO layer (5.1) and / or the thickness of the second TCO layer (5.2) is / are comprised in the range of 20 to 100 nm, more preferably in the range of 40 to 60 nm. In an embodiment, the thickness of the separation layer (6) is comprised in the range 1 to 55 nm, more preferably in the range of 5 to 20 nm.
[0134] In an embodiment, the thickness of the first dielectric layer (4.1) is comprised in the range of 10 to 120 nm, more preferably between 20 and 85 nm.
[0135] In some embodiments, the glazing (1) has a visible light transmittance of at most 90%, preferably in the range of 4 to 70%, more preferably in the range of 15 to 25%.
[0136] Figure 2 illustrates an embodiment of the glazing (1) of the invention which comprises all the layers described in Figure and further includes a second dielectric layer (4.2) disposed on the free surface of the second TCO layer (5.2).
[0137] In an embodiment, the dielectric layers (4.1 , 4.2) comprise material selected from the following list: SiOx, SiOxNy, SiNx, TiOx, TiSiOx, ZrOx, ZrTiOx, AIOx, CrOxSi, AITiOx, and ZrSiOx.
[0138] The second dielectric layer (4.2) helps protecting the other layers of the low-emissivity coating (3) from external conditions.
[0139] In an embodiment, the thickness of the second dielectric layer (4.1) is comprised in the range of 10 to 120 nm, more preferably in the range of 20 to 85 nm.
[0140] Figure 3 shows a particular embodiment of the glazing (1) of the invention. This embodiment depicts a laminated glazing comprising two glass layers (2.1 , 2.2) wherein each glass layer has a major surface (2.1.1 , 2.2.1), which are the external surface of the laminated glazing, The two glass layers (2.1 , 2.2) are bonded together by one plastic bonding layer (2.3).
[0141] In this particular embodiment, the low-emissivity coating (3) is disposed on the second major surface (2.2.1). In other embodiments, the coating (3) is disposed, in the same sequence of layers, on the first major surface (2.1.1).
[0142] Back to the embodiment of Figure 3, the first dielectric layer (4.1) is disposed on the second major surface (2.2.1). Then, a first additional layer (AL1), which is not a TCO layer, is disposed on the first dielectric layer (4.1). The first TCO layer (5.1) is disposed on the first additional layer (AL1) and is separated, by the separation layer (6), from the second TCO layer (5.2). A second dielectric layer (4.2) is disposed on the second TCO layer (5.2).
[0143] The low-emissivity coating (3) of Figure 3 provides enhanced control to the glazing (1) of the exterior reflection color due to the combination of the emissivity management of both first and second TCO layers (5.1 , 5.2) together with a non TCO layer such as the additional layer (AL1) or such as the separation layer (6).
[0144] In an embodiment, the thickness of the first additional layer (AL1) is comprised in the range of 2 to 25 nm, more preferably in the range of 3 to 15 nm.
[0145] Figure 4 shows another embodiment of the glazing (1) wherein the coating (3) is located on a major surface of one glass layer (2) such as the one of Figures 1 and 2.
[0146] In the embodiment of Figure 4, the coating (3) comprises all the layers of the coating (3) described in Figure 3 and further includes a second additional layer (AL2) located in between the second TCO layer (5.2) and the second dielectric layer (4.2).
[0147] In this embodiment, where the coating (3) includes both the first and the second additional layers (AL1 , AL2), these layers provide to the glazing (1) two optical interference cavities in the same coating (3). By changing the reflectance of the first additional layer (AL1) or the second additional layer (AL2), it provides two reflected waves which interfere with each other at different intensity levels. By tuning the thickness of the first and / or the second TCO layers (5.1 , 5.2), this enables tuning the phase between the reflected waves. Therefore, implementing a first and a second additional layer (AL1 , AL2), which are not TCO layers, allows an optimal control of the intensity and color of reflected light penetrating the glazing (1). Additionally, the control of the intensity and color of the reflected light is independent for exterior and interior sides of the glazing (1) due to the two sequences of layers such as separation layer - TCO layer - additional non-TCO layer provided in the same coating (3) as shown in Figure 4.
[0148] In some embodiments, the coating (3) only includes one additional layer (AL1 , AL2) which is either the first additional layer (AL1) disposed as described in Figure 3 without the second additional layer (AL2) or the second additional layer (AL2) disposed as described in Figure 4, that is in between the second TCO layer (5.2) and the second dielectric layer (4.2), without the first additional layer (AL1).
[0149] When the coating (3) only includes the second additional layer (AL2) and does not include the first additional layer (AL1), the second additional layer (AL2) provides to the glazing (1) an enhanced control of the interior reflection color thanks to the combination of the emissivity management of both the TCO layer (5.1 , 5.2) together with a non TCO layer such as the second additional layer (AL2) or the separation layer (6).
[0150] In an embodiment, the thickness of the second additional layer (AL2) is comprised in the range of 2 to 25 nm, more preferably in the range of 3 to 15 nm.
[0151] In some embodiments, the first additional layer (AL1) and / or the second additional layer (AL2) and / or the separation layer (6) comprise Ni, Cr, NiCr, Inconel, Al, Ag, Ti, NbOx or any combination thereof. In preferred embodiments, the first additional layer (AL1) and / or the second additional layer (AL2) and / or the separation layer (6) comprises Ni, Cr, NiCr, NiCr alloy, Al, AIOx, Ti, NbOx or a combination thereof. In preferred embodiments, the first additional layer (AL1) and / or the second additional layer (AL2) and / or the separation layer (6) do not comprise Ag.
[0152] In any combination with the above mentioned embodiments, the low-emissivity coating (3) of the glazing (1), when measured from the coating side of the glazing (1) at a viewing angle of 0°, has color values in the Cl ELAB color system wherein: a* is in the range of -15.0 to +1.0, more preferably in the range of -5.0 to 0, and b* is in the range of -10.0 to +10.0, and more preferably in the range of -5.0 to +5.0.
[0153] In some embodiments where the glazing (1) comprises one glass layer (2) or more than one glass layer (2.1 , 2.2), said at least on glass layer (2, 2.1 , 2.2) is / are bent or partially bent. Also in these embodiments, the at least one glass layer (2.1 , 2.2) is soda lime glass, aluminosilicate glass or borosilicate glass.
[0154] The present invention also embodies a roof comprising any of the above described embodiments, or combination thereof, of the glazing (1) of the invention.
[0155] The present invention also embodies a vehicle comprising at least one of any of the embodiments, or combination thereof, of the glazing (1) or any embodiment of the roof above mentioned.
[0156] In an embodiment of the method for manufacturing the glazing (1) of the present invention, the layers of the low-emissivity coating (3) are deposited on one major surface of the at least one glass layer (2.1 , 2.2) by means of sputter deposition, sol-gel deposition, spraying deposition.
[0157] Also in some embodiments of the method, the at least one glass layer (2, 2.1 , 2.2) is partially bent before depositing the first layer of the coating (3) and then fully bent after all the layers of the coating (3) are deposited on the at least one glass layer (2, 2.1 , 2.2).
[0158] In some other embodiments of the method, the at least one glass layer (2, 2.1 , 2.2) is fully bent before depositing the first layer of the coating (3).
[0159] EXAMPLES
[0160] Example 1
[0161] In one preferred embodiment of the glazing of the invention, the first and second TCO layers are two ITO layers separated by a 9.2 nm NiCr alloy layer. Two thinner NiCr layers, the first and the second additional layers, are deposited on the distal (from the center NiCr) sides of each ITO layers. The thicknesses of both ITO and NiCr layers are tuned, in between ranges as mentioned in some embodiments of the invention, in order to achieve a low interior and low exterior reflectance of penetrating light as well as to optimize the reflected and transmitted colors inside the glazing, more particularly, inside the coating.
[0162] The low-E coating of the present example 1 is either to be deposited on one of the major surfaces of a single glass pane or either on one major surface of a two glass layers laminated glass with a plastic bonding layer, in the particular case of a laminated glass, said coating is deposited on the major surface which will be referred as surface 4 (the major surface of the second glass layer) based on the following design:
[0163] Clear soda lime (2.1 mm) I SiNx(70.5nm) I NiCr(9.1nm) I ITO(29.5nm) I NiCr(9.2nm) I NbOx(13.2nm) I ITO(38.7nm) I NiCr(3.9nm) I NbOx(15.8nm) I SiOx(80.3nm)
[0164] In this particular example, the separation layer is a combination of two sublayers, one sublayer of NiCr (9.2nm), deposited over the first TCO layer (ITO (29.5nm)) and one sublayer of NbOx (13.2nm), deposited over the previous NiCr layer.
[0165] Also in this particular example, the second additional layer is a combination of two sublayers, one sublayer of NiCr (3.9nm) deposited over the second TCO layer (ITO (38.7nm)) and one sublayer of NbOx (15.8nm), deposited over the previous NiCr layer.
[0166] Thanks to the tuning of thicknesses of the layers of the first example and the sequence of said layers in the coating of the present embodiment, the achieved optical characteristics are as follows:
[0167] T(0°) = 7.4% and corresponding Cl ELAB color coordinates are: a*( T(0°) ) = 0.5 b*( T(0°) ) = -5.2
[0168] Rf(8°) = 1.6% and corresponding Cl ELAB color coordinates are: a*( Rf(8°) ) = -0.2 b*( Rf(8°) ) = 0.4
[0169] Rf(60°) = 4.4%; and corresponding CIELAB color coordinates are: a*( Rf(60°) ) = -1.6 b*( Rf(60°) ) = -1.8
[0170] Rg(8°) = 14.7%; and corresponding CIELAB color coordinates are: -1.0 -8.6
[0171] T(X) being the visible transmittance measured at a particular value of X degrees and following the measurement norm according to ISO 9050. Rf(X) being the visible reflectance measured from the coating side of the glazing, which is the interior side of a vehicle comprising the glazing, at a particular value of X degrees. Rg(X) being the visible reflectance measured from the glass side of the glazing, which is the exterior side of the vehicle comprising the glazing, at a particular value of X degrees.
[0172] In this particular example, the sheet resistance is 21 Q / sq.
[0173] Example 2
[0174] In a second preferred embodiment, example 2, the glazing is similar to the one of example 1 but the low-emissivity coating has the following design:
[0175] Clear soda lime (2.1 mm) / SiNx(74.8nm) / NiCr(9.1nm) / ITO(29.5nm) / NiCr(9.2nm) / NbOx(4 1.4nm) / ITO(51.7nm) / NiCr(4.4nm) / NbOx(17.1 nm) / SiOx(72.8nm)
[0176] In this particular example, the separation layer is a combination of two sublayers, one sublayer of NiCr (9.2nm), deposited over the first TCO layer (ITO (29.5nm)) and one sublayer of NbOx (41 ,4nm), deposited over the previous NiCr layer.
[0177] Also in this particular example, the second additional layer is a combination of two sublayers, one sublayer of NiCr (4.4nm) deposited over the second TCO layer (ITO (51.7nm)) and one sublayer of NbOx (17.1 nm), deposited over the previous NiCr layer.
[0178] Thanks to the tuning of thicknesses of the layers of the second example and the sequence of said layers in the coating of the present embodiment, the achieved optical characteristics are as follows:
[0179] T(0) = 9.4% and corresponding Cl ELAB color coordinates are: -3.7 -0.3
[0180] Rf(8) = 13.8% and corresponding Cl ELAB color coordinates are: a*( Rf(8) ) = -3.3 b*( Rf(8) ) = 0.0 Rf(60) = 20.6% and corresponding Cl ELAB color coordinates are: a*( Rf(60) ) = -12.7 b*( Rf(60) ) = 9.5
[0181] Rg(8) = 19.3% and corresponding Cl ELAB color coordinates are: -6.5 -9.0
[0182] In this particular example, the sheet resistance is 18 Q / sq.
[0183] Example 3
[0184] In a third preferred embodiment, example 3, the glazing is similar to the one of the previous examples but the low-e coating has the following design:
[0185] Clear soda lime (2.1 mm) / SiNx(72.6nm) / ITO(34.0nm) / AI(1.18nm) / AIOx(native;4nm) NbOx(22.0nm) / ITO(75.0nm) / AI(1.3nm) / AIOx(native;4nm) / NbOx(10.1 nm) / SiOx(72.6nm)
[0186] In this particular example, the design does not comprise any first additional layer.
[0187] Also, in this particular example, the separation layer is a combination of three sublayers, one sublayer of Al (1.18nm), deposited over the first TCO layer (ITO (34nm)), one sublayer of AIOx (4nm) deposited on the Al layer and one sublayer of NbOx (22nm) deposited over the previous layer.
[0188] Additionally, in this particular example, the second additional layer is a combination of three sublayers, one sublayer of Al (1 ,3nm), deposited over the second TCO layer (ITO (75nm)), one sublayer of AIOx (4nm) deposited over the previous Al layer and one sublayer of NbOx (10.1nm) deposited over the previous layer.
[0189] The present example includes an AIOx layer adjacent to each Al. During heat treatment or when exposed to an oxygen atmosphere, Al is known to form a protective layer of AIOx, 4 nm thick.
[0190] Thanks to the tuning of thicknesses of the layers of the third example and the sequence of said layers in the coating of the present embodiment, the achieved optical characteristics are as follows:
[0191] T(0) = 70.9% and corresponding Cl ELAB color coordinates are: -2.8 1.9
[0192] Rf(8) = 6.0% and corresponding Cl ELAB color coordinates are: a* ( Rf(8) ) = -0.1 b* ( Rf(8) ) = 0.3;
[0193] Rf(60) = 12.7% and corresponding CIELAB color coordinates are: -9.1 19.0;
[0194] Rg(8) = 5.3% and corresponding CIELAB color coordinates are: -1.0 -7.7.
[0195] In this particular example, the sheet resistance is 19 Q / sq.
Claims
CLAIMS1.- A laminated glazing (1) with low-emissivity capabilities suitable for automotive application comprising two glass layers (2.1 , 2.2) and at least one plastic bonding layer (2.3) permanently bonding said two glass layers (2.1 , 2.2), wherein at least one glass layer (2.2) having a first major surface (2.1.1) and a second major surface (2.2.1), and the laminated glazing (1) comprises: a low-emissivity coating (3) comprising: a first dielectric layer (4.1) disposed on at least one portion of the second major surface (2.2.1) of the at least one glass layer (2.2), a first transparent conductive oxide (TCO) layer (5.1) disposed on the first dielectric layer (4.1), a separation layer (6) disposed on the first TCO layer (5.1) wherein the separation layer (6) is a metal, an alloy, or a semiconductor, and wherein the separation layer (6) comprises Ni, Cr, NiCr, NiCr alloy, Al, AIOx, Ti, NbOx, or a combination thereof, a second TCO layer (5.2) disposed on the separation layer (6), wherein the visible reflectance (RVjS) from the top layer of the low-emissivity coating (3), measured at an angle of 8 degrees, is lower than 15%, preferably in the range 1 to 10%, more preferably in the range 1.2 to 6%, even more preferably in the range 1.5 to 4%, and the sheet resistance of the coating (3) is lower than 50 Q / sq, preferably lower than 30 Q / sq, more preferably lower than 25 Q / sq.2.- The glazing (1) according to the previous claim, further comprising a second dielectric layer (4.2) disposed on the second TCO layer (5.2).
3. The glazing (1) according to any of the previous claims, wherein at least one glass layer of the glazing has a maximal compressive strain greater than 7.4.- The glazing (1) according to any of the previous claims, further comprising a first additional layer (AL1) located between the first dielectric layer (4.1) and the first TCO layer (5.1), provided that such first additional layer (AL1) is not a TCO layer.5.- The glazing (1) according to any of claims 2 to 4, further comprising a second additional layer (AL2) located between the second TCO layer (5.2) and the second dielectric layer (4.2), provided that such second additional layer (AL2) is not a TCO layer.6.- The glazing (1) according to any of the previous claims, wherein the thickness of the first TCO layer (5.1) and / or the thickness of the second TCO layer (5.2) is / are comprised in the range of 20 to 100 nm, more preferably in the range of 40 to 60 nm.7.- The glazing (1) according to any of the previous claims, wherein the thickness of the separation layer (6) is comprised in the range 1 to 55 nm, more preferably in the range of 5 to 20 nm.8.- The glazing (1) according to any of the previous claims, wherein the thickness of the first dielectric layer (4.1) is comprised in the range of 10 to 120 nm, more preferably between 20 and 85 nm and / or the thickness of the second dielectric layer (4.2) is comprised in the range of 10 to 120 nm, more preferably in the range of 20 to 85 nm and / or the thickness of the first additional layer (AL1) is comprised in the range of 2 to 25 nm, more preferably in the range of 3 to 15 nm and / or the thickness of the second additional layer (AL2) is comprised in the range of 2 to 25 nm, more preferably in the range of 3 to 15 nm9.- The glazing (1) according to any of the previous claims, has a visible light transmittance of at most 90%, preferably in the range of 4 to 70%, more preferably in the range of 15 to 25%.
10. The glazing (1) according to any of the previous claims, wherein the separation layer metal and / or alloy materials are selected from materials having a melting point above the temperature required for glass bending.11 .- A roof for a vehicle comprising a glazing (1 ) according to any of the preceding claims.12.- A vehicle comprising at least one glazing (1) according to any of the claims 1 to 10 or a roof according to claim 11 .13.- A method for manufacturing a glazing (1) according to any of claims 1 to 10,comprising the following steps: a) providing at least one glass layer (2.2) having a first major surface (2.1.1) and a second major surface (2.2.1), b) depositing the first dielectric layer (4.1) of the low-emissivity coating (3) on at least a portion of the second major surface (2.2.1) of the at least one glass layer(2.2), c) depositing the remaining layers of the low-emissivity coating (3) according to any of claims 1 to 9, wherein the at least one glass layer (2, 2.1 , 2.2) comprises at least a first (2.1) and a second (2.2) glass layers, and wherein said first and second glass layers (2.1, 2.2) are further laminated, before step b) or after step c), with at least one plastic bonding layer (2.3).
14. The method according to the preceding claim, wherein before step b), the at least one glass layer (2.2) is partially bent, or before step b), the at least one glass layer (2.2) is partially bent and, after step c), the glazing (1) is fully bent, before step b), the at least one glass layer (2.2) is fully bent.
Citation Information
Patent Citations
Optical device including stack of optical layers with functional treatment
EP3540478A2
Coated glass sheet
US20040137235A1
Optical coatings for ultraviolet and infrared reflection
US20060154089A1
Method for producing a substrate coated with a stack including a conductive transparent oxide film
US20160229741A1
Substrate coated with a low-E multilayer
US9950951B2