Secondary battery

By integrating magnesium and other elements into the lithium cobalt oxide positive electrode active material, the battery addresses thermal stability and safety issues, achieving high capacity and safety through controlled current flow and reduced thermal runaway during charging and discharging.

WO2024201260A1PCT designated stage expired Publication Date: 2024-10-03SEMICON ENERGY LAB CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2024/052815
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-16
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium cobalt oxide-based secondary batteries face challenges in achieving both high capacity and safety due to thermal runaway issues during charging and discharging, particularly due to phase changes and low thermal stability, which can lead to safety concerns like thermal runaway and ignition during nail penetration tests.

Method used

Incorporating magnesium and other additive elements like fluorine and nickel into the lithium cobalt oxide positive electrode active material, with a higher magnesium concentration in the surface layer than in the interior, to create a stable crystal structure that slows down current flow and suppresses oxygen release, thereby enhancing thermal stability and safety.

Benefits of technology

The modified battery design achieves a safer and higher-capacity secondary battery with reduced temperature rise during nail penetration tests, maintaining stability and preventing thermal runaway, as evidenced by AC impedance values and temperature control within safe limits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2024052815_03102024_PF_FP_ABST
    Figure IB2024052815_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a secondary battery which has high safety. The secondary battery has a positive electrode and a negative electrode, wherein the positive electrode has a positive electrode active material, the positive electrode active material includes a magnesium-containing lithium cobalt oxide, the magnesium concentration in a surface layer portion of the positive electrode active material is higher than the magnesium concentration inside the positive electrode active material, the negative electrode has a negative electrode active material, the negative electrode active material includes a carbon material, and when AC impedance measurement is performed on the secondary battery charged to a voltage of 4.5 V, the AC impedance value at a frequency of 1 kHz is less than 90 milliohms.
Need to check novelty before this filing date? Find Prior Art

Description

secondary battery

[0001] One embodiment of the present invention relates to a secondary battery. The present invention is not limited to the above fields, but also relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, a vehicle, and a manufacturing method thereof. The above-described semiconductor device, display device, light-emitting device, power storage device, lighting device, electronic device, and vehicle can use the secondary battery of the present invention as a necessary power source. For example, the above-described electronic device includes an information terminal device equipped with a secondary battery. Furthermore, the above-described power storage device includes a stationary power storage device.

[0002] In recent years, the demand for high-power, high-capacity secondary batteries (also simply referred to as batteries) has rapidly increased, and they have become indispensable in modern society as a reusable energy source.

[0003] It is said that it is difficult to achieve both high capacity and safety in secondary batteries. For example, a positive electrode active material with a layered rock salt crystal structure used in lithium-ion secondary batteries is expected to achieve high capacity because the lithium ion diffusion paths exist two-dimensionally within the crystal structure. However, a positive electrode active material with a layered rock salt crystal structure is said to be prone to thermal runaway if too many lithium ions are desorbed during charging, resulting in a safety issue. Safety tests include nail penetration tests, and in order to suppress an increase in battery temperature during abnormal conditions such as nail penetration, Patent Document 1, for example, proposes a configuration in which a protective layer is provided between the positive electrode composite layer and the positive electrode current collector.

[0004] As a positive electrode active material with a layered rock salt crystal structure, lithium cobalt oxide (LiCoO 2 Lithium cobalt oxide has a layered rock salt crystal structure, and CoO 6Since lithium ions can move two-dimensionally between the octahedral layers, lithium cobalt oxide also has good cycle characteristics. However, lithium cobalt oxide has a problem of phase change during charging and discharging. For example, if a certain amount of lithium ions are desorbed during charging, lithium cobalt oxide undergoes a phase change from hexagonal to monoclinic. Therefore, in order to use lithium cobalt oxide with good cycle characteristics, the amount of lithium ions desorbed must be limited. To solve this problem, Patent Documents 2 to 4, for example, propose a configuration in which an additive element is added to lithium cobalt oxide.

[0005] Research on the crystalline structure of positive electrode active materials has also been conducted (Non-Patent Documents 1 to 4). One of the methods used to analyze the crystalline structure of positive electrode active materials is XRD (X-ray diffraction). XRD can be analyzed using the Inorganic Crystal Structure Database (ICSD) introduced in Non-Patent Document 5. For example, the lattice constant of lithium cobalt oxide described in Non-Patent Document 6 can be referenced from the ICSD. Furthermore, for Rietveld analysis, for example, the analysis program RIETAN-FP (Non-Patent Document 7) can be used.

[0006] Also, image processing software such as ImageJ (Non-Patent Documents 8 to 10) is known. By using this software, for example, the shape of the positive electrode active material can be analyzed.

[0007] Microelectron diffraction is also effective for identifying the crystalline structure of the positive electrode active material, particularly the crystalline structure of the surface layer. For example, the analysis program ReciPro (Non-Patent Document 11) can be used to analyze the electron diffraction pattern.

[0008] Furthermore, fluorides such as fluorite (calcium fluoride) have long been used as fluxes in iron manufacturing and other processes, and their physical properties have been studied (Non-Patent Document 12).

[0009] It is known that when the temperature of a lithium ion secondary battery rises during charging, it goes through several states and eventually reaches thermal runaway (Non-Patent Document 13).

[0010] Various research and development efforts are also being conducted on the reliability and safety of lithium-ion secondary batteries. For example, Non-Patent Document 14 describes the thermal stability of positive electrode active materials and electrolyte solutions.

[0011] JP 2019-129009 A JP 2019-179758 A WO2020 / 026078 A JP 2020-140954 A

[0012] Toyoki Okumura et al.,”Correlation of lithium ion distribution and X−ray absorption near−edge structure in O3−and O2−lithium cobalt oxides from first−principle calculation”,Journal of Materials Chemistry,2012,22,p.17340−17348Motohashi,T.et al.,”Electronic phase diagram of the layered cobalt oxide system Li▲x▼CoO▲2▼(0.0≦x≦1.0)”,Physical Review B,80(16);165114Zhaohui Chen et al.,“Staging Phase Transitions in Li▲x▼CoO▲2▼”,Journal of The Electrochemical Society,2002,149(12)A1604−A1609G.G.Amatucci et.al.,“CoO▲2▼,The End Member of the Li▲x▼CoO▲2▼ Solid Solution”J.Electrochem.Soc.143(3)1114(1996).Belsky,A.et al.,“New developments in the Inorganic Crystal Structure Database(ICSD):accessibility in support of materials research and design”,Acta Cryst.,(2002)B58 364−369.Akimoto,J.;Gotoh,Y.;Oosawa,Y.“Synthesis and structure refinement of LiCoO▲2▼ single crystals”Journal of Solid State Chemistry(1998)141,p.298−302.F.Izumi and K.Momma,Solid State Phenom.,130,15−20(2007)Rasband,W.S.,ImageJ,U. S. National Institutes of Health, Bethesda, Maryland, USA, http: / / rsb. info. nih. gov / ij / , 1997-2012. Schneider, C. A. , Rasband, W. S. , Eliceiri, K. W. “NIH Image to ImageJ: 25 years of image analysis”, Nature Methods 9, 671-675, 2012. Abramoff, M. D. , Magelhaes, P. J. , Ram, S. J. , “Image Processing with ImageJ”, Biophotonics International, volume 11, issue 7, pp. 36-42, 2004. Seto, Y. & Ohtsuka, M. , “ReciPro: free and open-source multipurpose crystallographic software integrating a crystal model database and “viewer, diffraction and microscopy simulators, and diffraction data analysis tools” (2022) J. Appl. Cryst. ,55. W. E. Counts, R. Roy, and E. F. Osborn, "Fluoride Model Systems: II, The Binary Systems CaF2-BeF2, MgF2-BeF2, and LiF-MgF2", Journal of the American Ceramic Society, 36[1] 12-17 (1953). Nobuo Eda, 2-4 Heat Generation Mechanism: Learning from Data: Li-ion Battery Charging and Discharging Technology, CQ Publishing, April 4, 2020, pp. 68-72; Shinya Kitano et al., GSYuasa Technical Report, Vol. 2, No. 2, December 2015, pp. 18-24.

[0013] Lithium cobalt oxide (LiCoO 2Lithium cobalt oxide (LCO) is said to have low thermal stability. Furthermore, if an internal short circuit occurs in a secondary battery during a nail penetration test, which is one of the safety tests for lithium-ion secondary batteries, Joule heat is generated, which can lead to thermal runaway. Therefore, when using lithium cobalt oxide as described above, safety measures are essential for the secondary battery. Patent Document 1 discloses a configuration in which a protective layer is provided between the positive electrode current collector and the positive electrode composite layer to suppress an increase in battery temperature during nail penetration.

[0014] In view of the above, an object of one embodiment of the present invention is to provide a battery with high safety. Another object of one embodiment of the present invention is to provide a battery with high capacity and high safety.

[0015] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description in the specification, drawings, and claims.

[0016] One embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode. The positive electrode has a positive electrode active material, and the positive electrode active material includes lithium cobalt oxide containing magnesium. A magnesium concentration in a surface layer portion of the positive electrode active material is higher than a magnesium concentration in an interior of the positive electrode active material. The negative electrode has a negative electrode active material, and the negative electrode active material includes a carbon material. When AC impedance measurement is performed on the secondary battery in a state where the secondary battery is charged to a voltage of 4.5 V, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ.

[0017] Another embodiment of the present invention is a secondary battery including a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode includes a positive electrode active material, and the positive electrode active material includes lithium cobalt oxide containing magnesium. A magnesium concentration in a surface layer portion of the positive electrode active material is higher than a magnesium concentration in an interior of the positive electrode active material. The negative electrode includes a negative electrode active material, and the negative electrode active material includes a carbon material. A solvent for the electrolyte includes ethylene carbonate and diethyl carbonate. The separator includes polypropylene. When AC impedance measurement is performed on the secondary battery in a state where the secondary battery is charged to a voltage of 4.5 V, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ.

[0018] Another embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, wherein the positive electrode has a positive electrode active material, and the positive electrode active material has lithium cobalt oxide containing magnesium, and a magnesium concentration in a surface layer portion of the positive electrode active material is higher than a magnesium concentration in an interior of the positive electrode active material, and the negative electrode has a negative electrode active material, and the negative electrode active material has a carbon material, and when the secondary battery is charged to a voltage of 4.5 V and AC impedance measurement is performed in a state where the capacity is 2000 mAh or more, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ.

[0019] Another embodiment of the present invention is a secondary battery including a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode includes a positive electrode active material, and the positive electrode active material includes lithium cobalt oxide containing magnesium. A magnesium concentration in a surface layer portion of the positive electrode active material is higher than a magnesium concentration in an interior of the positive electrode active material. The negative electrode includes a negative electrode active material, and the negative electrode active material includes a carbon material. A solvent for the electrolyte includes ethylene carbonate and diethyl carbonate. The separator includes polypropylene. When the secondary battery is charged to a voltage of 4.5 V and AC impedance measurement is performed in a state where the capacity is 2000 mAh or more, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ.

[0020] In the present invention described above, when a nail penetration test is carried out on the secondary battery using a nail with a diameter of 3 mm at a nail penetration speed of 5 mm / sec, it is preferable that the temperature rise ΔT is 50° C. or less.

[0021] In the present invention described above, it is preferable that the lithium cobalt oxide further contains aluminum.

[0022] In the present invention described above, it is preferable that the lithium cobalt oxide further contains nickel.

[0023] In the present invention described above, it is preferable that the lithium cobalt oxide further contains fluorine.

[0024] According to one embodiment of the present invention, a highly safe secondary battery can be provided.Furthermore, according to one embodiment of the present invention, a high-capacity and highly safe secondary battery can be provided.

[0025] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.

[0026] FIGS. 1A and 1B are diagrams illustrating a nail penetration test. FIGS. 2A and 2B are diagrams illustrating the nail penetration operation. FIG. 3 is a graph showing changes when the internal temperature of a secondary battery in which an internal short circuit has occurred increases. FIG. 4 is a graph showing changes when the internal temperature of a secondary battery increases. FIGS. 5A to 5C are examples of cross-sectional structures of positive electrode active materials. FIG. 6 is an example of a TEM image in which the crystal orientations are roughly consistent. FIG. 7A is an example of an STEM image in which the crystal orientations are roughly consistent. FIG. 7B is an FFT pattern of a region of rock salt crystal RS, and FIG. 7C is an FFT pattern of a region of layered rock salt crystal LRS. FIG. 8 is a diagram illustrating the crystalline structure of a positive electrode active material. FIG. 9 is a diagram illustrating the crystalline structure of a conventional positive electrode active material. FIG. 10 is a diagram illustrating the depth of charge and c-axis length of a positive electrode active material. FIG. 11 is a diagram illustrating an XRD pattern calculated from the crystalline structure. FIG. 12 is a diagram illustrating an XRD pattern calculated from the crystalline structure. FIGS. 13A and 13B are diagrams showing XRD patterns calculated from the crystal structure. FIGS. 14A to 14C are diagrams showing lattice constants calculated from XRD. FIGS. 15A and 15B are cross-sectional views of a positive electrode active material. FIGS. 16A and 16B are diagrams illustrating a laminate-type secondary battery. FIG. 17 is a phase diagram showing the relationship between the composition of lithium fluoride and magnesium fluoride and temperature. FIG. 18 is a diagram illustrating the results of DSC measurement. FIGS. 19A to 19C are diagrams illustrating a method for preparing a positive electrode active material. FIGS. 20A to 20C are diagrams illustrating a method for preparing a positive electrode active material. FIG. 21 is a diagram illustrating a method for preparing a positive electrode active material. FIGS. 22A to 22C are diagrams illustrating a method for preparing a positive electrode active material. FIG. 23 is a diagram illustrating a heating furnace and heating conditions. FIGS. 24A and 24B are diagrams illustrating a positive electrode. FIGS. 25A to 25C are diagrams illustrating a coin-type secondary battery. Fig. 26A to Fig. 26D are diagrams illustrating a cylindrical secondary battery. Fig. 27A and Fig. 27B are diagrams illustrating a wound type secondary battery. Fig. 28 is a diagram illustrating a wound type secondary battery. Fig. 29A to Fig. 29D are diagrams illustrating an electronic device. Fig. 30A to Fig. 30C are diagrams illustrating an electronic device. Fig. 31A to Fig. 31C are diagrams illustrating a vehicle.Figures 32A to 32C are graphs showing charge / discharge curves. Figure 33A is a graph showing the results of an impedance test, and Figure 33B is a diagram showing the equivalent circuit used for the analysis. Figures 34A to 34C are photographs explaining the results of a nail penetration test. Figures 35A to 35C are graphs explaining the results of the nail penetration test. Figures 36A to 36C are graphs explaining the results of the nail penetration test. Figures 37A to 37C are graphs explaining the results of the nail penetration test. Figures 38A to 38C are graphs explaining the results of the nail penetration test.

[0027] Hereinafter, examples of embodiments of the present invention will be described with reference to the drawings, etc. However, the present invention should not be construed as being limited to the following examples. The embodiments of the present invention can be modified within the scope of the spirit of the present invention.

[0028] In this specification, space groups are expressed using short notation in international notation (or Hermann-Mauguin notation). Crystal planes and crystal directions are expressed using Miller indices. In crystallography, space groups, crystal planes, and crystal directions are expressed by adding a superscript bar to the numbers. However, due to formatting constraints, in this specification, instead of adding a bar above the numbers, a minus sign (-) may be added before the numbers. Individual orientations indicating directions within a crystal are expressed using [ ], collective orientations indicating all equivalent directions are expressed using < >, individual planes indicating crystal planes are expressed using ( ), and collective planes with equivalent symmetry are expressed using {}. For ease of understanding the structure, trigonal crystals represented by the space group R-3m are generally expressed as a hexagonal composite hexagonal lattice. Unless otherwise specified, the space group R-3m will also be expressed as a composite hexagonal lattice in this specification. Miller indices may also be expressed as (hkil) rather than (hkl). Here, i is −(h+k).

[0029] In this specification and the like, the space group of the positive electrode active material and the like is identified by X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, etc. Therefore, in this specification and the like, "belonging to a certain space group," "belonging to a certain space group," or "being a certain space group" can be rephrased as "identified with a certain space group."

[0030] Furthermore, if the anions have a structure in which three layers are stacked with a mutual shift, such as ABCABC, it is called a cubic close-packed structure. Therefore, the anions do not need to be strictly cubic lattices. At the same time, since real crystals always have defects, the analysis results do not necessarily have to be theoretical. For example, in an FFT (fast Fourier transform) pattern such as an electron diffraction pattern or a TEM (transmission electron microscope) image, spots may appear at positions slightly different from the theoretical positions. For example, if the deviation in orientation from the theoretical positions is 5 degrees or less, or 2.5 degrees or less, it can be said to have a cubic close-packed structure.

[0031] In this specification and the like, the term "particle" is not limited to referring only to spherical particles (having a circular cross-sectional shape), and examples of the cross-sectional shape of individual particles include ellipsoids, rectangles, trapezoids, triangles, squares with rounded corners, and asymmetric shapes, and further, individual particles may have an irregular shape.

[0032] In this specification, the theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated. For example, LiCoO 2 The theoretical capacity of LiNiO is 274 mAh / g per weight of the positive electrode active material. 2 The theoretical capacity of LiMn is 275 mAh / g per weight of the positive electrode active material. 2 O 4 The theoretical capacity of the positive electrode active material is 148 mAh / g.

[0033] In this specification, the amount of lithium remaining in the positive electrode active material that can be inserted or removed is determined by x in the composition formula, for example, Li x MO 2 In the above formula, M represents a transition metal, and unless otherwise specified in this specification, M is cobalt and / or nickel. In the case of a positive electrode active material in a lithium ion secondary battery, x can be expressed as (theoretical capacity - charging capacity) / theoretical capacity (both are capacity per weight of the positive electrode active material). For example, LiMO 2 When a lithium ion secondary battery using as a positive electrode active material is charged up to 219.2 mAh / g per weight of the positive electrode active material, Li 0.2 MO 2Or we can say x = 0.2. x MO 2 The small value of x in the formula means, for example, 0.1<x≦0.24. When the lithium cobalt oxide satisfies the stoichiometric ratio, LiCoO 2 When lithium cobalt oxide is used in the positive electrode, the lithium cobalt oxide in the lithium ion secondary battery after discharge is also LiCoO 2 It can be said that x = 1. The completion of discharge here refers to a state in which the current per weight of the positive electrode active material is 100 mA / g or less and the voltage is 3.0 V or 2.5 V or less.

[0034] Li x MO 2 The charge capacity and / or discharge capacity used to calculate x in the above should preferably be calculated under conditions where there is no influence of short circuit and / or decomposition of the electrolyte in the lithium ion secondary battery, or where such influence is minimal. For example, data on a lithium ion secondary battery that has experienced a sudden change in capacity that is considered to be due to a short circuit should not be used to calculate x.

[0035] In this specification and the like, segregation of a certain element refers to a state in which a certain element (for example, A) is distributed non-uniformly in a solid composed of a plurality of elements (for example, A, B, C).

[0036] In this specification, the distribution of a certain element refers to the continuous presence of that element when the element is detected within a range that is not noise using any analytical method. The continuous change in the concentration of the element is sometimes called a concentration gradient. The maximum value in the distribution is sometimes called a peak. When identifying a peak, it is possible to target a distribution limited to a certain region. The above-mentioned distribution is not limited to a normal distribution. When it corresponds to a normal distribution, the half-width of the distribution can also be determined.

[0037] In this specification, uneven distribution refers to the concentration of an element in a certain region being different from that in other regions. It is synonymous with uneven distribution or the coexistence of areas with high and low concentrations. Uneven distribution through solid solution is called segregation.

[0038] In this specification, the surface layer portion of the positive electrode active material refers to a region within 20 nm or within 50 nm from the surface toward the interior in a direction perpendicular or approximately perpendicular to the surface. The surface layer portion is synonymous with the near-surface and near-surface region. Specifically, perpendicular or approximately perpendicular refers to an angle with the surface of 80° or more and 100° or less. The region deeper than the surface layer portion of the positive electrode active material is referred to as the interior. The interior is synonymous with the bulk or core.

[0039] In this specification and the like, the positive electrode active material may be expressed as a composite oxide, a positive electrode material, a positive electrode material for a secondary battery, a positive electrode material for a lithium-ion secondary battery, or the like. Also in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a compound. Also in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composition. Also in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composite.

[0040] Although the present specification and the like may describe characteristics of a positive electrode active material, it is not necessary that all of the positive electrode active materials in the positive electrode have the characteristics. For example, if three or more of five or more randomly selected particles of a positive electrode active material have the characteristics, it can be said that the effect of sufficiently improving the characteristics of the positive electrode active material and a secondary battery including the same is achieved.

[0041] In this specification, an internal short circuit of a secondary battery refers to contact between the positive electrode and the negative electrode inside the battery. An external short circuit of a secondary battery refers to contact between the positive electrode and the negative electrode outside the battery, which is assumed to occur due to misuse. An internal short circuit of a secondary battery can be intentionally induced by a nail penetration test.

[0042] In this specification, ignition in a nail penetration test refers to the observation of a flame outside the exterior packaging within one minute of the nail being inserted, or the occurrence of thermal runaway in the secondary battery. For example, thermal runaway is said to have occurred if thermal decomposition products of the positive electrode and / or negative electrode are observed in an area at least 2 cm away from the nail penetration point after the nail penetration test. Examples of thermal decomposition products of the positive electrode and / or negative electrode include aluminum oxide, which is the oxidized form of aluminum when aluminum foil is used as the positive electrode current collector, and copper oxide, which is the oxidized form of copper when copper foil is used as the negative electrode current collector. Even if flames, sparks, and / or smoke are observed in the nail penetration test, if they remain at the puncture site, i.e., do not spread, and do not result in thermal runaway in the secondary battery, this is not considered ignition. For example, if no ignition occurs during a nail penetration test, the secondary battery can be said to be non-ignition-resistant.

[0043] Unless otherwise specified, in this specification and the like, the materials (positive electrode active material, negative electrode active material, electrolyte, separator, etc.) contained in a secondary battery are described in their pre-degradation state. Note that a decrease in charge capacity and / or discharge capacity due to aging and burn-in treatments during the secondary battery manufacturing stage is not considered degradation. For example, a secondary battery consisting of a single cell or a battery pack can be said to be in its pre-degradation state when it has a discharge capacity of 97% or more of its rated capacity. For secondary batteries for portable devices, the rated capacity conforms to JIS C 8711:2019. For other secondary batteries, the rated capacity conforms not only to the above JIS standard but also to various JIS and IEC standards for electric vehicle propulsion, industrial use, etc.

[0044] In this specification and the like, a lithium ion secondary battery refers to a battery that uses lithium ions as carrier ions, but in the present invention, the carrier ions are not limited to lithium ions. For example, alkali metal ions or alkaline earth metal ions can be used as carrier ions, and specifically, sodium ions can be used. In this case, the present invention can be understood by reading lithium ions as sodium ions. Furthermore, when there is no limitation on the carrier ions, the battery may be referred to as a secondary battery.

[0045] In this specification, the (001) plane and the (003) plane may be collectively referred to as the (001) plane. The (001) plane may also be referred to as the C-plane, the basal plane, or the like. In addition, in lithium cobalt oxide, lithium ions have two-dimensional diffusion paths. In other words, it can be said that the diffusion paths of lithium ions exist along the plane. In this specification, a plane on which the diffusion paths of lithium ions are exposed, that is, a plane other than the plane where lithium is inserted and extracted (specifically, the (001) plane), may be referred to as an edge plane.

[0046] In this specification, the term "supported amount" refers to the weight of the active material per unit surface area of ​​the current collector. The supported amount of the negative electrode active material can be adjusted according to the capacity of the positive electrode. In the case of double-sided coating, in which a slurry containing the active material is applied to both sides of the current collector, the supported amount is considered per side.

[0047] In this specification, etc., secondary particles refer to particles formed by aggregation of primary particles. Also, in this specification, etc., single particles refer to particles that do not have grain boundaries on their appearance. Also, in this specification, etc., single crystal particles refer to crystalline particles in which there are no grain boundaries inside the particles, and polycrystalline particles refer to crystalline particles in which there are grain boundaries inside the particles. Polycrystalline particles may be said to be an aggregate of multiple crystallites, and grain boundaries may be said to be the interface that exists between two or more crystallites.

[0048] In this specification etc., the term "A and / or B" may be used, but this is an example of the description including only A, only B, and both A and B.

[0049] (Embodiment 1) The nail penetration test is a test in which a secondary battery is fully charged and a nail having a predetermined diameter selected from 2 mm to 20 mm is inserted into the secondary battery at a predetermined speed. Full charge refers to a state in which the charge rate, expressed as State of Charge (hereinafter referred to as SOC), is 100%. In this embodiment, a nail penetration test device will first be described.

[0050] <Nail Penetration Test Apparatus> FIG. 1A shows a cross-sectional view of a nail penetration test apparatus 1000. The nail penetration test apparatus 1000 includes a stage 1001, a drive unit 1002, a nail 1003, a voltage measuring device 1015, a temperature measuring device 1016, and a control unit 1018. The drive unit 1002 includes a drive mechanism 1012 that moves the nail 1003 in the direction of the arrow in the figure. The drive mechanism 1012 operates to cause the nail 1003 to penetrate a secondary battery 1004 placed on the stage 1001. At this time, the secondary battery 1004 is in a fully charged state, and this operation is called a nail penetration operation. Note that the dashed line in FIG. 1A indicates a recess in the stage 1001 that is provided to accommodate the nail 1003 that has penetrated the secondary battery 1004 during the nail penetration operation.

[0051] The voltage measuring device 1015 transmits information about the voltage of the secondary battery during the nail penetration operation to the control unit 1018. Specifically, the amount of voltage change and the like are transmitted to the control unit 1018. Furthermore, the temperature measuring device 1016 transmits information about the temperature during the nail penetration operation to the control unit 1018. When controlling the operating conditions of the nail 1003, the control unit 1018 can transmit a control signal to the drive unit 1002.

[0052] FIG. 1B is a perspective view illustrating the vicinity of the upper portion of the stage 1001 of the nail penetration test device 1000. The secondary battery 1004 placed on the stage 1001 is electrically connected to wires 1005a and 1005b. The wires 1005a and 1005b belong to a voltage measuring device 1015, and the wires 1005a and 1005b are electrically connected to the positive and negative electrode tabs of the secondary battery 1004, respectively, to measure the voltage of the secondary battery 1004. The voltage of the secondary battery 1004 is simply referred to as voltage, voltage value between the positive and negative electrodes, battery voltage, cell voltage, or open-circuit voltage. When a temperature sensor is used as the temperature measuring device 1016, the temperature sensor is disposed so as to contact the surface of the exterior body of the secondary battery 1004.

[0053] 1B shows an example in which a first temperature sensor 1006a and a second temperature sensor 1006b are arranged on the secondary battery 1004, and a third temperature sensor 1006c is further provided on the nail 1003 shown in FIG. 1A, but one or three or more temperature sensors may be arranged on the secondary battery 1004. In the secondary battery 1004, the first temperature sensor 1006a is arranged on the side where the wiring 1005a and the wiring 1005b are not arranged, and the second temperature sensor 1006b is arranged on the side where the wiring 1005a and the wiring 1005b are arranged. Arranging two or more temperature sensors in this way is preferable because even if one temperature sensor becomes unusable due to expansion of the exterior body or the like, the other temperature sensors can be used.

[0054] Furthermore, although there is an adhesive region on the side where the wiring 1005a and the wiring 1005b are arranged, there is no adhesive region on the side where the wiring 1005a and the wiring 1005b are not arranged because the exterior body is folded back. Therefore, even if the exterior body expands, the expansion is suppressed on the side where the wiring 1005a and the wiring 1005b are not arranged, and the first temperature sensor 1006a is more unlikely to peel off than the second temperature sensor 1006b, which is preferable.

[0055] The dashed ellipse in FIG. 1B represents the area where the nail 1003 penetrates the secondary battery 1004 during the nail penetration operation. The first temperature sensor 1006a and the second temperature sensor 1006b provided on the secondary battery 1004 are preferably provided equidistant from the area where the nail 1003 penetrates. Typically, the first temperature sensor 1006a and the second temperature sensor 1006b are provided within 5 cm, preferably within 2 cm, of the area where the nail 1003 penetrates. By providing the sensors in this manner, it is possible to grasp temperature changes in the area where the nail 1003 penetrates and its vicinity, which is preferable. Here, "vicinity" refers to an area within 1 cm of the penetration area. When two or more temperature sensors are provided, it is preferable to start the nail penetration operation after confirming that the difference in temperature indicated by the temperature sensors is within ±5°C, preferably within ±2°C.

[0056] <Secondary Battery in Nail Penetration Test> Next, the state of the secondary battery in the nail penetration test will be described again with reference to FIGS. 2A and 2B . The nail penetration test is a test in which a secondary battery 1004 is fully charged and a nail 1003 is inserted into the secondary battery 1004 at a predetermined speed. The diameter of the nail 1003 is 2 mm or more and 10 mm or less. FIG. 2A shows a cross-sectional view of the secondary battery 1004 with the nail 1003 inserted therein. The secondary battery 1004 has a structure in which a positive electrode 503, a separator 508, a negative electrode 506, and an electrolyte 530 are housed in an exterior case 531. The positive electrode 503 has a positive electrode current collector 501 and positive electrode active material layers 502 formed on both sides thereof, and the negative electrode 506 has a negative electrode current collector 511 and negative electrode active material layers 512 formed on both sides thereof. The positive electrode active material layer is a layer containing at least a positive electrode active material, for example, a conductive material and / or a binder. The negative electrode active material layer is a layer containing at least a negative electrode active material, for example, a conductive material and / or a binder. Figure 2B shows an enlarged view of the nail 1003, the positive electrode current collector 501, and their vicinity, and also clearly shows the positive electrode active material 100 and the conductive material 553 contained in the positive electrode active material layer 502.

[0057] As shown in Figures 2A and 2B, a nail 1003 is inserted into a secondary battery 1004, and the nail 1003 penetrates the positive electrode 503 and the negative electrode 506, causing an internal short circuit. Then, the potential of the nail 1003 becomes equal to the potential of the negative electrode 506, and electrons (e − ) flows to the positive electrode 503, and Joule heat is generated at the internal short circuit location and its vicinity. In addition, due to the internal short circuit, carrier ions, typically lithium ions (Li + ) are released into the electrolyte as indicated by the white arrow. However, because the temperature of the secondary battery rises rapidly due to Joule heat generated by the internal short circuit, the electrolyte begins to reductively decompose on the surface of the anode before all the lithium ions are released from the anode. This is an electrochemical reaction, and is called the reduction reaction of the electrolyte by the anode.

[0058] Furthermore, when the temperature of the secondary battery 1004 rises due to Joule heat, if lithium cobalt oxide is used as the positive electrode active material, the lithium cobalt oxide may undergo a phase change (i.e., a structural change) to an H1-3 type crystal structure or an O1 type crystal structure, and heat may be generated as a result of the phase change. Note that the H1-3 type crystal structure and the O1 type crystal structure will be described later. When an internal short circuit occurs, heat is generated one after another.

[0059] As shown in FIGS. 2A and 2B, the electrons (e − ) reduces the tetravalent Co in the charged lithium cobalt oxide to trivalent or divalent Co, and this reduction reaction releases oxygen from the lithium cobalt oxide, which then decomposes the electrolyte 530 through an oxidation reaction caused by the oxygen. This is an electrochemical reaction, and is called an oxidation reaction of the electrolyte by the positive electrode. The rate at which current flows into the positive electrode active material 100, etc., is thought to affect the electrochemical reaction, and the insulating properties of the positive electrode active material can slow the rate at which current flows.

[0060] As mentioned above, when an internal short circuit occurs in a secondary battery, it is believed that the temperature will change as shown in the graph in Figure 3. Figure 3 is a partially modified version of the graph shown on page 70 [Figures 2-12] of Non-Patent Document 13, and is a graph of the temperature (specifically, the internal temperature) of the secondary battery versus time. When an internal short circuit occurs at (P0), the temperature of the secondary battery rises over time. As shown at (P1), heat generation due to Joule heat continues until the temperature of the secondary battery reaches 100°C or close to that temperature, exceeding the reference temperature (Ts) of the secondary battery. Then, at (P2), the negative electrode (when graphite is used, the negative electrode is C 6 In (P3), the electrolyte is oxidized by the positive electrode and heat is generated, and in (P4), heat is generated due to thermal decomposition of the electrolyte. This causes the secondary battery to go into thermal runaway and catch fire.

[0061] <Thermal Runaway of Secondary Batteries> Figure 4 shows a partially revised version of the graph shown on page 69 [Figures 2-11] of Non-Patent Document 13, which illustrates the principle of thermal runaway in secondary batteries. When the temperature (specifically, the internal temperature) of the above-mentioned secondary battery rises, for example, during charging, it passes through several states and then goes into thermal runaway. Figure 4 is a graph of the temperature of the secondary battery against time. For example, when the temperature of the secondary battery reaches or is close to 100°C, (1) the SEI (Solid Electrolyte Interface) of the negative electrode collapses and heat is generated. Furthermore, when the temperature of the secondary battery exceeds 100°C, (2) the negative electrode (when graphite is used, the negative electrode becomes C 6 (3) At or near 150°C, oxidation of the electrolyte by the positive electrode occurs, and heat is generated. When the temperature of the secondary battery reaches or near 180°C, (4) thermal decomposition of the electrolyte occurs, and (5) oxygen is released from the positive electrode and thermal decomposition of the positive electrode (this thermal decomposition includes a structural change in the positive electrode active material). When the temperature of the secondary battery then exceeds 200°C, (6) decomposition of the negative electrode occurs, and finally, (7) direct contact between the positive electrode and the negative electrode occurs. Through these states, particularly states (5), (6), or (7), the secondary battery reaches thermal runaway.

[0062] To prevent thermal runaway, it is considered effective to suppress the temperature rise of the secondary battery and to have stable characteristics at high temperatures for the negative electrode, positive electrode, and / or electrolyte. A configuration that suppresses temperature rise can be achieved by having a structure that slows the rate of current flow to the positive electrode active material. A specific example of a configuration that allows the positive electrode to exhibit stable characteristics at high temperatures is a structure in which the positive electrode active material 100 does not release oxygen at high temperatures. This is expected to have significant effects on secondary batteries, such as reducing the risk of thermal runaway and fire. The positive electrode active material of one embodiment of the present invention can have both the stable structure and a structure that slows the rate of current flow.

[0063] [Positive Electrode Active Material] A positive electrode active material 100 according to one embodiment of the present invention will be described. The positive electrode active material 100 contains carrier ions, typically lithium ions (Li +A compound containing a transition metal and oxygen capable of inserting and extracting ions may be used. The transition metal may be one or more selected from the group consisting of cobalt (Co), nickel (Ni), manganese (Mn), and iron (Fe). FIG. 5A shows an example of the cross-sectional structure of a positive electrode active material 100. The positive electrode active material 100 has a surface portion 100a and an interior portion 100b, and the (001) plane, which is the diffusion plane of lithium ions, is indicated by a dashed line.

[0064] <Main Component> The positive electrode active material 100 of one embodiment of the present invention preferably uses cobalt as the main component of the transition metal M responsible for the oxidation-reduction reaction. Note that in this specification and the like, the main component of the transition metal M refers to the transition metal M having the highest atomic ratio. For example, lithium cobalt oxide can be used as the positive electrode active material 100 as a compound using Co as the transition metal. Alternatively, the positive electrode active material 100 can be lithium cobalt oxide (LiCoO 2 However, the positive electrode active material 100 of one embodiment of the present invention preferably has a crystal structure described later. Therefore, the composition of lithium cobalt oxide is not strictly limited to Li:Co:O=1:1:2.

[0065] The positive electrode active material 100 of one embodiment of the present invention preferably has an insulating region or a high-resistance region. The region preferably has a narrow width of 1 nm to 20 nm, preferably 2 nm to 10 nm, and more preferably 2 nm to 5 nm, in a cross-sectional view of the positive electrode active material 100. The narrow region may be referred to as a "shell" in this specification and elsewhere. A cross-sectional scanning transmission electron microscope (STEM) image can be used for the cross-sectional view.

[0066] During the nail penetration test, electrons rapidly flow into the positive electrode active material, causing cobalt to be reduced from tetravalent to divalent, resulting in a reaction in which oxygen is released from the positive electrode active material. This reaction is exothermic, accelerating thermal runaway. In order to suppress the above reaction, for example, the positive electrode active material 100 of the present invention has a structure that makes it difficult to release oxygen by using a shell 100s described below. If oxygen is not released from the positive electrode active material, the above reduction reaction (for example, Co 4+ From Co 2+ The reaction that results in the

[0067] 5B shows the positive electrode active material 100 having a shell 100s. The positive electrode active material 100 having the shell 100s has increased resistance, and therefore, even when a nail penetration test is performed, the rate at which current flows into the positive electrode active material 100 can be slowed down, which is preferable because fire and the like can be suppressed. In order to slow down the rate at which current flows into the positive electrode active material 100, it is more preferable that the shell 100s, which has high resistance, is located in the surface layer portion 100a.

[0068] <Additive Element> The positive electrode active material 100 preferably contains an additive element. Examples of the additive element include magnesium, fluorine, nickel, aluminum, titanium, zirconium, vanadium, iron, manganese, chromium, niobium, arsenic, zinc, silicon, sulfur, phosphorus, boron, bromine, and beryllium, and it is preferable to use one or more additive elements selected from these.

[0069] The additive elements do not necessarily include magnesium, fluorine, nickel, aluminum, titanium, zirconium, vanadium, iron, manganese, chromium, niobium, arsenic, zinc, silicon, sulfur, phosphorus, boron, bromine, and beryllium. For example, if the cathode active material 100 is substantially free of manganese, the advantages of relatively easy synthesis and handling, and excellent cycle characteristics, as described above, are enhanced. The weight of manganese contained in the cathode active material 100 is preferably, for example, 600 ppm or less, and more preferably 100 ppm or less.

[0070] Magnesium is one of the elements suitable for forming the shell 100s. Specifically, magnesium is suitable as an additive element that is less likely to release oxygen because the closer the magnesium is to oxygen, the greater the energy required to desorb it. Magnesium also has the function of stabilizing the crystal structure of the positive electrode active material, making it suitable as an additive element. Magnesium can stabilize the crystal structure while slowing down the rate of current flowing into the positive electrode active material 100.

[0071] In a cross-sectional view of the positive electrode active material 100, magnesium is preferably present in a narrow width of 1 nm to 20 nm, preferably 2 nm to 10 nm, and more preferably 2 nm to 5 nm from the surface. Magnesium is preferably present in greater amounts, i.e., at a higher concentration, in the shells 100s of the edge surfaces than in the shells 100s of the basal surfaces.

[0072] Since the shell 100s contains at least magnesium, oxygen release from this region is suppressed, improving thermal stability and thus reducing the likelihood of thermal runaway. Therefore, the shell 100s is preferably provided so as to sufficiently cover the entire cathode active material 100, as shown in FIG. 5A , but it is preferable that the shell 100s be formed over 60% or more, preferably 80% or more, of the cross-sectional area. Furthermore, although a uniform shell 100s is preferred, it may be formed so that a specific region of the cathode active material 100, such as a surface other than the (001) plane, is thicker.

[0073] However, as long as the shell 100s does not ignite in a nail penetration test, the shell 100s may be provided in any manner relative to the positive electrode active material 100, and the lithium ion (Li + As long as the speed of current flow due to an internal short circuit can be slowed while allowing insertion and removal of the magnesium, the magnesium may be present somewhere other than the shell 100s, for example, in the interior 100b.

[0074] Furthermore, in consideration of rapid charge and discharge, it may be preferable that the positive electrode active material 100 has a region where the shell 100s is not provided.

[0075] When magnesium is added to the positive electrode active material 100, it is preferable to use magnesium fluoride as a magnesium source, and using magnesium fluoride allows fluorine to also be added to the positive electrode active material 100. In other words, it may be preferable for the positive electrode active material 100 to contain fluorine in addition to magnesium as an added element. Lithium and fluorine may react during a nail penetration test, etc., but this reaction generates less heat than when lithium reacts with oxygen, and therefore the temperature rise of the secondary battery can be suppressed.

[0076] Furthermore, it may be preferable for the positive electrode active material 100 of one embodiment of the present invention to contain nickel in addition to magnesium as an additive element. In other words, it is preferable for nickel to be present in the shell 100s. It is preferable for nickel to be present in a larger amount, i.e., at a higher concentration, in the edge surface shell 100s than in the basal surface shell 100s. This configuration can suppress oxygen detachment from the positive electrode active material or suppress structural changes in the positive electrode active material.

[0077] It is preferable that all of the above-mentioned additive elements are present at least in the shell 100s. In other words, it is preferable that the above-mentioned additive elements are present at least in the surface layer portion 100a. The additive elements that contribute to the stability of the crystal structure of the positive electrode active material 100 are preferably present in the surface layer portion 100a, where deterioration is likely to begin. It is preferable that the additive elements are present in greater amounts, i.e., at a higher concentration, in the shell 100s of the edge surface than in the shell 100s of the basal surface.

[0078] One method for determining whether or not a shell 100s is formed on the positive electrode active material 100 is to measure the resistance (called powder resistance) of the powder that becomes the positive electrode active material. When a shell 100s is formed on the positive electrode active material 100, the powder resistance value is higher than when the shell 100s is not formed. Typically, if the powder resistance of a positive electrode active material containing an additive element exhibits a higher value than the powder resistance of a positive electrode active material without the additive element, there is a possibility that the shell 100s has been formed.

[0079] It is preferable that the shell 100s contains cobalt in addition to the additive element. By containing at least cobalt, the shell 100s can effectively absorb lithium ions (Li+ The shell 100s can slow down the rate of current flow caused by an internal short circuit. + In terms of enabling the insertion and desorption of cobalt, it is preferable that the surface layer portion 100a also contains the additional element and cobalt.

[0080] The magnesium concentration in the lithium cobalt oxide shell 100s should be greater than 0 and less than 10 atomic%, preferably greater than 0 and less than 5 atomic%, and more preferably greater than 0 and less than 2 atomic%. The magnesium concentration can be determined by linear analysis using energy dispersive X-ray spectroscopy (EDX). If magnesium is present throughout the entire surface layer 100a at a high concentration, the insulating properties will be high, making it difficult to obtain favorable battery characteristics in charge-discharge cycle tests and the like. On the other hand, the presence of magnesium in the surface layer 100a, particularly in an appropriate region for the shell 100s, at an appropriate concentration can stabilize the lithium cobalt oxide and suppress ignition and other problems during the nail penetration test described above. Furthermore, the presence of magnesium at an appropriate concentration in the shell 100s is expected to improve the hardness of the lithium cobalt oxide.

[0081] FIG. 5C also shows a positive electrode active material 100 having a crystal grain boundary 101. The crystal grain boundary 101 refers to, for example, a portion where particles of the positive electrode active material 100 adhere to each other, a portion where the crystal orientation changes within the positive electrode active material 100, i.e., a portion where the repetition of bright and dark lines in an STEM image or the like becomes discontinuous, a portion containing many crystal defects, a portion where the crystal structure is disordered, etc. Furthermore, the crystal defect refers to a defect that can be observed in a cross-sectional TEM, cross-sectional STEM image, etc., i.e., a structure in which other atoms have entered between the lattices, a cavity, etc. The crystal grain boundary 101 can be considered one type of planar defect. Furthermore, the vicinity of the crystal grain boundary 101 refers to a region within 10 nm of the crystal grain boundary 101.

[0082] FIG. 5C also shows a positive electrode active material 100 having a crack 102. A crack includes a region where a crystal plane is displaced or a region where a crystal plane is broken, and cracks often occur along the (001) plane. While it is preferable that such cracks 102 are not observed, cracks 102 may be present as long as they do not ignite during a nail penetration test. To prevent ignition during a nail penetration test, it is preferable that a shell is also formed on the newly formed surface layer when the crack 102 occurs. The vicinity of the crack 102 refers to a region within 10 nm of the crack 102.

[0083] <Crystallinity> The positive electrode active material 100 preferably has high crystallinity, and is more preferably single crystalline or polycrystalline. In particular, when the positive electrode active material 100 has single crystallinity, cracks are less likely to occur even when a volume change occurs in the positive electrode active material 100 due to charge and discharge, which is preferable. In other words, when the positive electrode active material 100 is single crystalline, a secondary battery using the positive electrode active material 100 is thought to be less likely to ignite, thereby improving safety. After undergoing the initial heating described below, the crystallinity of the positive electrode active material 100 becomes high, which is preferable. Furthermore, the positive electrode active material 100 is preferably a single particle (also called a primary particle) rather than a secondary particle.

[0084] <Median Diameter (D50) of Positive Electrode Active Material> The median diameter (D50) of the positive electrode active material possessed by a highly safe secondary battery will be described. If the positive electrode active material is too small, it may be difficult to coat the positive electrode during production. Furthermore, if the positive electrode active material is too small, the surface area may become too large, which may result in excessive reaction between the positive electrode active material surface and the electrolyte. Furthermore, if the positive electrode active material is too small, it may be necessary to mix a large amount of conductive material, which may result in a decrease in capacity. In these respects, the median diameter (D50) of the positive electrode active material is preferably 1 μm or more, preferably 5 μm or more, and more preferably 9 μm or more. A positive electrode active material with a small median diameter (D50) is preferred because it is less likely to produce a misaligned region. Furthermore, a positive electrode active material with a small median diameter (D50) is preferred because it is less likely to produce cracks even after undergoing a pressing process.

[0085] On the other hand, if the active materials are too small, there are concerns that the density of the positive electrode active material layer will decrease, side reactions with the electrolyte will increase, etc. In this respect, the median diameter (D50) of the positive electrode active material is 20 μm or less, preferably 18 μm or less, and more preferably 15 μm or less.

[0086] That is, the median diameter (D50) of the positive electrode active material can be any combination of the above upper and lower limits. For example, the median diameter is 1 μm or more and 20 μm or less, preferably 1 μm or more and 18 μm or less, and more preferably 1 μm or more and 15 μm or less.

[0087] The above-mentioned median diameter (D50) can be measured, for example, by observation using an SEM or TEM, or by a particle size distribution analyzer using a laser diffraction / scattering method. When measured by a particle size distribution analyzer using a laser diffraction / scattering method, the median diameter (D50) is the particle diameter at which the integrated amount in a cumulative curve of the particle size distribution measurement results accounts for 50%. Note that, as a method for measuring the median diameter (D50) by analysis using an SEM or TEM, for example, 20 or more particles are measured, a cumulative curve is created, and the particle diameter at which the integrated amount accounts for 50% is determined.

[0088] <Surface of the Positive Electrode Active Material> The surface of the positive electrode active material 100 refers to the surface of the composite oxide including the surface layer portion 100a and the interior portion 100b. Such a surface can be confirmed in a cross-sectional view. Therefore, the surface of the positive electrode active material 100 is made of aluminum oxide (Al 2 O 3 The positive electrode active material 100 does not include, for example, metal oxides having no lithium sites that can contribute to charging and discharging, carbonates chemically adsorbed after the preparation of the positive electrode active material, hydroxyl groups, etc. The attached metal oxides refer to, for example, metal oxides whose crystal structure does not match that of the interior 100b.

[0089] Since the positive electrode active material 100 is a composite oxide containing a transition metal and oxygen capable of lithium insertion / extraction, the interface between a region where the transition metal M (e.g., Co, Ni, Mn, Fe, etc.) that is oxidized and reduced upon lithium insertion / extraction and oxygen is present and a region where it is not present is defined as the surface of the positive electrode active material. When the positive electrode active material is subjected to analysis, a protective film may be attached to the surface, but the protective film is not included in the positive electrode active material. As the protective film, a single-layer film or a multilayer film of carbon, metal, oxide, resin, etc. may be used.

[0090] Therefore, the reference point in the STEM-EDX-ray analysis is the average value M of the detected amount of characteristic X-rays of the transition metal M inside the positive electrode active material. AVE When the left side of the reference point is described as the outside of the positive electrode active material and the right side of the reference point is described as the inside of the positive electrode active material, the reference point may be referred to as the position of the surface of the positive electrode active material. In addition, in STEM-EDX-ray analysis, if the amount of detected characteristic X-rays of the transition metal M does not decrease sufficiently to the left of the reference point, the amount of detected characteristic X-rays of the transition metal M to the left of the reference point is called background, and the average value M of the amount of detected characteristic X-rays of the transition metal M in the background is used. BG and the average detected amount of transition metal M inside AVE The reference point may be the point where the detected amount of characteristic X-rays of oxygen inside the positive electrode active material is 50% of the sum of the transition metal M and the transition metal M. The reference point can be determined by replacing the transition metal M with oxygen. However, since oxygen is an element that is easily affected by the outside of the positive electrode active material, the reference point is the average value M of the detected amount of characteristic X-rays of the transition metal M. AVE It is preferable to calculate it from 50% of the average value M of the detected amount of characteristic X-rays of the transition metal M inside. AVE 50% of the average value of the detected amount of characteristic X-rays of oxygen inside M AVE If the position of the reference point is different in 50% of the above cases, it is considered to be the influence of metal oxides, carbonates, etc. containing oxygen attached to the surface. Therefore, the average value M of the detected amount of characteristic X-rays inside the transition metal M is used. AVE In the case of a positive electrode active material containing a plurality of transition metals M, it is preferable to adopt the 50% point of the element M with the largest amount of characteristic X-rays detected inside. AVE , or M AVE and MBG The reference point can be found using

[0091] Average value of internal characteristic X-ray detection amount M AVE can be determined by averaging a range of 2 nm or more, preferably 3 nm or more, in a region where the detected amount of characteristic X-rays of the transition metal M or oxygen is stable, in other words, a saturated region, specifically, a region where the detected amount of characteristic X-rays of the transition metal M or oxygen starts to increase, and a depth of 30 nm or more, preferably 50 nm or more, from the region where the detected amount of characteristic X-rays of the transition metal M or oxygen starts to increase. BG can be obtained by averaging a range of 2 nm or more, preferably 3 nm or more, in a stable region avoiding the vicinity where the detected amount of characteristic X-rays of the transition metal M starts to increase.

[0092] Furthermore, the surface of the positive electrode active material 100 in a cross-sectional STEM image or the like is the boundary between an area where an image derived from the crystalline structure of the positive electrode active material is observed and an area where an image is not observed, and is the outermost area of ​​an area where atomic columns derived from the atomic nuclei of metal elements having atomic numbers larger than that of lithium among the metal elements constituting the positive electrode active material are confirmed.

[0093] Furthermore, the minimum spatial resolution of STEM-EDX is about 1 nm. Therefore, the peak position (also called the maximum value) of the detected amount of characteristic X-rays corresponding to the added element may be shifted by about 1 nm. For example, even if the peak position of the detected amount of characteristic X-rays corresponding to an added element such as magnesium is located to the left of the surface obtained above, the difference between the peak and the surface can be considered an error as long as it is less than 1 nm.

[0094] The peak in STEM-EDX-ray analysis refers to the maximum or local maximum value of the characteristic X-rays corresponding to each element. Note that noise in STEM-EDX-ray analysis may be a measured value with a half-width less than the spatial resolution (R), for example, R / 2 or less.

[0095] The influence of noise can be reduced by scanning the same location multiple times under the same conditions. For example, the integrated values ​​measured over six scans can be used to graph the characteristic X-rays of each element. The number of scans is not limited to six, and more scans can be performed, and the average can be used to graph the characteristic X-rays of each element.

[0096] STEM-EDX analysis can be performed, for example, as follows: First, a protective film is vapor-deposited on the surface of the positive electrode active material in the atmosphere. For example, carbon can be vapor-deposited using a carbon coating unit of an ion sputtering device (MC1000 manufactured by Hitachi High-Technologies).

[0097] Next, the positive electrode active material is thinned to prepare a STEM cross-sectional sample. For example, the thinning process can be performed using an FIB-SEM device (Hitachi High-Tech XVision 200TBS). The pickup is performed using an MPS (micro-probing system), and the finishing process can be performed under conditions such as an acceleration voltage of 10 kV.

[0098] For example, STEM-EDX analysis can be performed using an EDAX Octane T Ultra W (Dual EDS) as the EDX detector mounted on the STEM device. During EDX analysis, the acceleration voltage of the STEM device is set to 200 kV, and the emission current is set to 6 μA or more and 10 μA or less, and a portion of the thinned sample with minimal depth and unevenness is measured. The magnification is, for example, approximately 150,000 times. The EDX analysis conditions can be drift correction, a line width of 42 nm, a pitch of 0.2 nm, and six or more frames.

[0099] <Continuous Change in Crystal Structure> Furthermore, due to the concentration gradient of the added element as described above, it is preferable that the crystal structure continuously changes from the interior 100b toward the surface. Alternatively, it is preferable that the crystal orientation of the surface layer 100a and the interior 100b are approximately the same.

[0100] For example, it is preferable that the crystal structure continuously change from the interior 100b of the layered rock salt type toward the surface and surface layer 100a, which has characteristics of the rock salt type or both the rock salt type and the layered rock salt type. Alternatively, it is preferable that the crystal orientation of the surface layer 100a, which has characteristics of the rock salt type or both the rock salt type and the layered rock salt type, and the interior 100b of the layered rock salt type are approximately the same.

[0101] In this specification, the layered rock-salt crystal structure belonging to the space group R-3m, which is possessed by a composite oxide containing lithium and a transition metal such as cobalt, refers to a crystal structure having a rock-salt ion arrangement in which cations and anions are alternately arranged, and in which the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Defects such as vacancies of cations or anions may also be present. Furthermore, strictly speaking, the layered rock-salt crystal structure may have a distorted lattice structure of the rock-salt crystal, which may result in a lower symmetry than the rock-salt crystal structure.

[0102] The rock salt crystal structure refers to a cubic crystal structure, such as a crystal structure belonging to the space group Fm-3m, in which cations and anions are arranged alternately, and may contain cation or anion defects.

[0103] The fact that it has both the characteristics of the layered rock salt type and the rock salt type crystal structure can be determined by electron diffraction, TEM images, cross-sectional STEM images, and the like.

[0104] In the rock salt type, there is no distinction in the cation sites, but in the layered rock salt type, there are two types of cation sites in the crystal structure, one of which is mostly occupied by lithium and the other by a transition metal. The layered structure in which two-dimensional planes of cations and two-dimensional planes of anions are alternately arranged is the same for both the rock salt type and the layered rock salt type. Among the bright spots in the electron diffraction pattern corresponding to the crystal planes that form this two-dimensional plane, when the central spot (transmitted spot) is set as the origin 000, the bright spot closest to the central spot is, for example, the (111) plane in the ideal rock salt type, and, for example, the (003) plane in the layered rock salt type. For example, rock salt type MgO and layered rock salt type LiCoO 2 When comparing the electron diffraction patterns of LiCoO 2 The distance between the bright spots on the (003) plane of LiCoO is observed to be about half the distance between the bright spots on the (111) plane of MgO. 2In the case of a material having these two phases, the electron diffraction pattern shows a plane orientation in which bright spots with strong brightness and bright spots with weak brightness are arranged alternately. Bright spots common to both the rock salt type and the layered rock salt type have strong brightness, while bright spots occurring only in the layered rock salt type have weak brightness.

[0105] Furthermore, when a layered rock-salt crystal structure is observed from a direction perpendicular to the c-axis in cross-sectional STEM images, layers observed with high brightness and layers observed with low brightness are observed alternately. This characteristic is not observed in the rock-salt structure, as there is no distinction in the cation sites. In the case of a crystal structure that has the characteristics of both the rock-salt and layered rock-salt structures, when observed from a specific crystal orientation, layers observed with high brightness and layers observed with low brightness are observed alternately in cross-sectional STEM images, and furthermore, metals with atomic numbers higher than that of lithium are present in some of the low-brightness layers, i.e., the lithium layers.

[0106] Layered rock salt crystals and anions in rock salt crystals have a cubic close-packed structure (face-centered cubic lattice structure). It is presumed that anions in the O3'-type and monoclinic O1(15) crystals described below also have a cubic close-packed structure. Therefore, when a layered rock salt crystal and a rock salt crystal come into contact, there are crystal faces where the cubic close-packed structure composed of anions is aligned.

[0107] It can also be explained as follows: Anions on the {111} plane of a cubic crystal structure have a triangular lattice. Layered rock salt has a space group of R-3m and a rhombohedral structure, but to make the structure easier to understand, it is generally expressed as a compound hexagonal lattice, and the (0001) plane of the layered rock salt has a hexagonal lattice. The triangular lattice on the cubic {111} plane has the same atomic arrangement as the hexagonal lattice on the (0001) plane of the layered rock salt. The compatibility of the two lattices can be said to be the alignment of the cubic close-packed structure.

[0108] However, the space group of the layered rock salt crystal and the O3'-type crystal is R-3m, which is different from the space group Fm-3m of the rock salt crystal (the space group of a general rock salt crystal), and therefore the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt crystal and the O3'-type crystal and the rock salt crystal. In this specification, when the orientations of the cubic close-packed structures formed by anions in the layered rock salt crystal, the O3'-type crystal and the rock salt crystal are aligned, it may be said that the crystal orientations are approximately the same. In addition, having a three-dimensional structural similarity such that the crystal orientations are approximately the same, or having the same crystallographic orientation, is called topotaxis.

[0109] The fact that the crystal orientations of the two regions roughly coincide can be determined from TEM images, STEM images, HAADF-STEM (High-angle Annular Dark Field STEM, high-angle scattering annular dark-field scanning transmission electron microscope) images, ABF-STEM (Annular Bright-Field STEM, annular bright-field scanning transmission electron microscope) images, electron diffraction patterns, FFT patterns of TEM images and STEM images, etc. XRD, electron diffraction, neutron diffraction, etc. can also be used as materials for determination.

[0110] 6 shows an example of a TEM image in which the orientations of the layered rock salt crystals LRS and the rock salt crystals RS are roughly the same. Images reflecting the crystal structure can be obtained in TEM images, STEM images, HAADF-STEM images, ABF-STEM images, etc.

[0111] For example, in high-resolution TEM images, contrast originating from crystal planes can be observed. When an electron beam is incident perpendicularly to the c-axis of a layered rock-salt type composite hexagonal lattice, for example, due to the diffraction and interference of the electron beam, the contrast originating from the (0003) plane is observed as a repetition of bright bands (bright strips) and dark bands (dark strips). Therefore, a repetition of bright and dark lines is observed in the TEM image, and the bright lines (for example, the L shown in Figure 6) RS and L LRSWhen the angle between the dark lines is 5 degrees or less, or 2.5 degrees or less, it can be determined that the crystal planes are roughly aligned, i.e., the crystal orientations are roughly aligned. Similarly, when the angle between the dark lines is 5 degrees or less, or 2.5 degrees or less, it can be determined that the crystal orientations are roughly aligned.

[0112] Furthermore, in HAADF-STEM images, contrast proportional to atomic number is obtained, with elements with higher atomic numbers being observed brighter. For example, in the case of layered rock-salt lithium cobaltate belonging to the space group R-3m, cobalt (atomic number 27) has the highest atomic number, so the electron beam is strongly scattered at the position of the cobalt atoms, and the arrangement of the cobalt atoms is observed as a bright line or an arrangement of highly bright dots. Therefore, when lithium cobaltate having a layered rock-salt crystal structure is observed perpendicular to the c-axis, the arrangement of the cobalt atoms perpendicular to the c-axis is observed as a bright line or an arrangement of highly bright dots, while the arrangements of lithium atoms and oxygen atoms are observed as dark lines or low-brightness regions. The same is true when lithium cobaltate contains fluorine (atomic number 9) and magnesium (atomic number 12) as additive elements.

[0113] Therefore, in an HAADF-STEM image, when repetitions of bright and dark lines are observed in two regions with different crystal structures and the angle between the bright lines is 5 degrees or less or 2.5 degrees or less, it can be determined that the atomic arrangements are roughly consistent, i.e., the crystal orientations are roughly consistent. Similarly, when the angle between the dark lines is 5 degrees or less or 2.5 degrees or less, it can also be determined that the crystal orientations are roughly consistent.

[0114] In ABF-STEM, elements with smaller atomic numbers are observed brighter, but like HAADF-STEM, contrast according to the atomic number is obtained, so the crystal orientation can be determined in the same way as with HAADF-STEM images.

[0115] Figure 7A shows an example of an STEM image in which the orientations of the layered rock salt crystal LRS and the rock salt crystal RS are roughly the same. Figure 7B shows the FFT pattern of the region of the rock salt crystal RS, and Figure 7C shows the FFT pattern of the region of the layered rock salt crystal LRS. The left side of Figures 7B and 7C shows the composition, JCPDS card number, and d value and angle calculated from the JCPDS card data. The right side shows the measured values. The spot marked with O is the zeroth order diffraction.

[0116] The spot marked A in Figure 7B is derived from the 11-1 reflection of the cubic crystal. The spot marked A in Figure 7C is derived from the 0003 reflection of the layered rock salt type. From Figures 7B and 7C, it can be seen that the orientation of the 11-1 reflection of the cubic crystal and the orientation of the 0003 reflection of the layered rock salt type roughly coincide. In other words, it can be seen that the line passing through AO in Figure 7B is roughly parallel to the line passing through AO in Figure 7C. Here, "roughly coincident" and "roughly parallel" mean that the angle between the lines is 5 degrees or less, or 2.5 degrees or less.

[0117] In this way, in the FFT pattern and the electron beam diffraction pattern, when the orientations of the layered rock salt type crystal and the rock salt type crystal are roughly the same, the <0003> orientation of the layered rock salt type and the <11-1> orientation of the rock salt type may roughly coincide. In this case, it is preferable that these reciprocal lattice points are spot-like, that is, not continuous with other reciprocal lattice points. A reciprocal lattice point being spot-like and not continuous with other reciprocal lattice points means high crystallinity.

[0118] Furthermore, as described above, when the orientation of the 11-1 reflection of the cubic crystal and the orientation of the 0003 reflection of the layered rock salt crystal are approximately the same, depending on the incident orientation of the electron beam, spots not originating from the 0003 reflection of the layered rock salt crystal may be observed in a reciprocal lattice space different from the orientation of the 0003 reflection of the layered rock salt crystal. For example, the spot marked B in FIG. 7C originates from the 1014 reflection of the layered rock salt crystal. This spot may be observed at an angle of 52° to 56° (i.e., ∠AOB is 52° to 56°) from the orientation of the reciprocal lattice point (A in FIG. 7C) originating from the 0003 reflection of the layered rock salt crystal, and at a location where the d value is 0.19 nm to 0.21 nm. Note that this index is merely an example and does not necessarily have to be identical. For example, reciprocal lattice points equivalent to 0003 and 1014 may also be used.

[0119] Similarly, spots not originating from the 11-1 reflection of the cubic crystal may be observed in a reciprocal lattice space other than the orientation where the 11-1 reflection of the cubic crystal is observed. For example, the spot marked B in FIG. 7B originates from the 200 reflection of the cubic crystal. This is a location at an angle of 54° or more and 56° or less (i.e., ∠AOB is 54° or more and 56° or less) from the orientation of the reciprocal lattice point (A in FIG. 7B) originating from the 11-1 reflection of the cubic crystal, and a diffraction spot may be observed at this location. Note that this index is merely an example and does not necessarily have to match this. For example, a reciprocal lattice point equivalent to 11-1 and 200 may also be used.

[0120] It is known that layered rock salt type positive electrode active materials, including lithium cobalt oxide, tend to have the (0003) plane and its equivalents, as well as the (10-14) plane and its equivalents, as crystal planes. Therefore, when observing the (0003) plane using a TEM or the like, first select positive electrode active material particles in which a crystal plane expected to be the (0003) plane is observed using a SEM or the like, and then thin-section the positive electrode active material particles using a FIB (Focused Ion Beam) or the like so that the (0003) plane can be observed in a TEM or the like with an electron beam incident in the [12-10] direction. When determining whether the crystal orientation is consistent, it is preferable to thin-section the layered rock salt type so that the (0003) plane can be easily observed.

[0121] <Characteristic 1 of Secondary Battery in Nail Penetration Test> When AC impedance measurement is performed on a secondary battery in a fully charged state, it is preferable that the internal resistance of the secondary battery exhibits an AC impedance value of 100 mΩ or less, preferably less than 90 mΩ, at a frequency of 1 kHz. A secondary battery having such an internal resistance can be said to be highly safe. When fully charged, the charge capacity of the secondary battery is preferably 2000 mAh or more, preferably 2400 mAh or more. Because a fully charged secondary battery may discharge over time, AC impedance measurement should be performed within 24 hours, preferably within 12 hours, and more preferably within 6 hours after being fully charged.

[0122] <Characteristic 2 of Secondary Battery in Nail Penetration Test> When a nail penetration test is performed, the temperature rise of the secondary battery, i.e., the difference between the temperature before the nail penetration test and the maximum temperature reached after the nail penetration (also referred to as temperature rise ΔT), is preferably 100°C or less, more preferably 70°C or less, and even more preferably 50°C or less. The temperature is measured within 5 cm, preferably within 2 cm, of the nail hole, and specifically, is the value output by a temperature sensor located within 5 cm, preferably within 2 cm, of the nail hole. When the temperature sensor is provided so as to be in contact with the exterior body of the secondary battery, this temperature is equal to the temperature of the exterior body.

[0123] The temperature of the nail 1003 is preferably 100° C. or less, more preferably 80° C. or less, and even more preferably 60° C. or less. This is a value output by a temperature sensor disposed on the nail 1003.

[0124] Furthermore, the maximum temperature of the secondary battery during the nail penetration test is preferably 150°C or lower, more preferably 100°C or lower, and even more preferably 80°C or lower. It is more preferable that the maximum temperature is lower than the temperature at which oxidation of the electrolyte occurs due to the positive electrode. It is even more preferable that the maximum temperature is lower than the flash point of the mixed organic solvent used in the electrolyte. If the flash point of the mixed organic solvent is unknown, the flash point of each organic solvent can be used as a reference.

[0125] <Characteristics of secondary battery in nail penetration test 3> The amount of positive electrode active material carried in the positive electrode of the secondary battery is 15 mg / cm 2 25mg / cm or more 2 Preferably 18 mg / cm or less2 23mg / cm or more 2 or less, more preferably 20 mg / cm 2 22mg / cm or more 2 It is preferable that the amount of support is as follows: With such a supported amount, a highly safe secondary battery can be provided.

[0126] In the secondary battery, the positive / negative electrode capacity ratio is preferably 75% or more and 100% or less, and more preferably 80% or more and 90% or less. With such a positive / negative electrode capacity ratio, a highly safe secondary battery can be provided. The positive / negative electrode capacity ratio will be described in detail in the Examples.

[0127] <Characteristic 4 of Secondary Battery in Nail Penetration Test> The positive electrode active material particles of the secondary battery preferably have very few cracks. For example, when the positive electrode active material particles are observed with a surface SEM or a cross-section SEM, the number of observable cracks per positive electrode active material particle should be between 0 and 5.

[0128] The cracks may be caused by pressure applied after the positive electrode slurry is applied to the positive electrode current collector. Therefore, in the manufacturing process of the positive electrode of the present invention, the pressure of the press is, for example, a linear pressure of 500 kN / m or less, preferably a linear pressure of 300 kN / m or less, and more preferably a linear pressure of 250 kN / m or less.

[0129] After the pressing, the thickness of the positive electrode active material layer is preferably 70 μm or more and 80 μm or less, and more preferably 75 μm or more and 78 μm or less.

[0130] <Crystal Structure of Positive Electrode Active Material> The crystal structure of the positive electrode active material 100 of one embodiment of the present invention will be described in comparison with that of a conventional positive electrode active material.

[0131] <Li x MO 2 When x is 1 in the graph, the crystal structure of the positive electrode active material 100 according to one embodiment of the present invention is shown in FIG. x MO 2In the case where x = 1 (M is a transition metal, specifically cobalt and / or nickel), it is preferable that the layered rock salt type composite oxide has a layered rock salt type crystal structure belonging to the space group R-3m. Layered rock salt type composite oxides have a high discharge capacity, have two-dimensional lithium ion diffusion paths, are suitable for lithium ion insertion and desorption, and are excellent as positive electrode active materials for secondary batteries. Therefore, it is particularly preferable that the inner portion 100b, which occupies most of the volume of the positive electrode active material 100, has a layered rock salt type crystal structure. Figure 8 shows the layered rock salt type crystal structure labeled R-3m O3. R-3m O3 has a lattice constant a = 2.81610 × 10 −10 (m), b=2.81610×10 −10 (m), c=14.05360×10 −10 (m), α = 90.0000, β = 90.0000, γ = 120.0000, and the coordinates of lithium, cobalt, and oxygen in the unit cell are Li(0,0,0), Co(0,0,0.5), and O(0,0,0.23951) (Non-Patent Document 10). In Figure 8, O3 is added under the space group, and in this crystal structure, lithium occupies an octahedral site and MO is present in the unit cell. 2 Because there are three layers, this crystal structure is sometimes called an O3 type crystal structure. 2 The layer refers to a structure in which an octahedron structure in which oxygen is six-coordinated to a transition metal M is continuous on a plane in an edge-sharing state. This is sometimes referred to as a layer consisting of octahedra of transition metal M and oxygen. Also, in Figure 8, lithium ions are shown to exist at all lithium sites, but as mentioned above, ions of an added element, such as magnesium ions, may also be located at the lithium sites.

[0132] On the other hand, the surface layer portion 100a of the cathode active material 100 according to one embodiment of the present invention preferably has a function of reinforcing the inner portion 100b so that the layered structure of the transition metal M and oxygen octahedra is not broken even when lithium is removed from the cathode active material 100 upon charging. Alternatively, the surface layer portion 100a preferably functions as a barrier film for the cathode active material 100. Alternatively, the surface layer portion 100a, which is the outer periphery of the cathode active material 100, preferably reinforces the cathode active material 100. Here, "reinforcement" refers to suppressing structural changes in the surface layer portion 100a and inner portion 100b of the cathode active material 100, such as oxygen desorption and / or shifting of the layered structure of the transition metal M and oxygen octahedra, and / or suppressing decomposition of an organic electrolyte solution or the like on the surface of the cathode active material 100.

[0133] Therefore, the surface layer portion 100a preferably has a different crystal structure from the interior portion 100b. Furthermore, the surface layer portion 100a preferably has a composition and a crystal structure that are more stable at room temperature (25°C) than the interior portion 100b. For example, at least a part of the surface layer portion 100a of the positive electrode active material 100 of one embodiment of the present invention preferably has a rock salt crystal structure. Alternatively, the surface layer portion 100a preferably has both a layered rock salt crystal structure and a rock salt crystal structure. Alternatively, the surface layer portion 100a preferably has characteristics of both a layered rock salt crystal structure and a rock salt crystal structure.

[0134] The surface layer 100a is the region from which lithium ions are first released during charging, and is a region where the lithium concentration is likely to be lower than that of the interior 100b. In addition, it can be said that the atoms on the surface of the particles of the positive electrode active material 100 in the surface layer 100a are in a state where some of the bonds are broken. Therefore, the surface layer 100a is likely to become unstable, and is a region where deterioration of the crystal structure is likely to begin. For example, if the crystal structure of the layered structure consisting of transition metal M and oxygen octahedra in the surface layer 100a is displaced, this influence is transmitted to the interior 100b, causing the layered crystal structure in the interior 100b to also be displaced, which is thought to lead to deterioration of the crystal structure of the entire positive electrode active material 100. On the other hand, if the surface layer 100a can be sufficiently stabilized, Li x CoO 2Even when x is small, for example, 0.24 or less, the layered structure of the inner portion 100b made of the transition metal M and oxygen octahedra can be made less likely to break. Furthermore, displacement of the layer made of the transition metal M and oxygen octahedra in the inner portion 100b can be suppressed.

[0135] Furthermore, it is preferable that the interior 100b of the positive electrode active material 100 has a low density of defects such as dislocations. It is also preferable that the crystallite size of the positive electrode active material 100 measured by XRD is large. In other words, it is preferable that the interior 100b has high crystallinity. It is also preferable that the surface of the positive electrode active material 100 is smooth. These characteristics are important factors that support the reliability of the positive electrode active material 100 when used in a secondary battery. If the reliability of the positive electrode active material is high, the upper limit of the charge voltage of the secondary battery can be increased, resulting in a secondary battery with a high discharge capacity.

[0136] Dislocations in the interior 100b can be observed, for example, by a TEM. If the density of defects such as dislocations is sufficiently low, defects such as dislocations may not be observed in a specific 1 μm square of the observation sample. Note that dislocations are a type of crystal defect and are different from point defects.

[0137] The crystallite size measured by XRD is preferably 300 nm or more. The larger the crystallite size, the more Li x CoO 2 When x in the crystal structure is small, the O3' type crystal structure is easily maintained, and shortening of the c-axis length is easily suppressed.

[0138] It is believed that the fewer defects such as dislocations observed by TEM, the larger the crystallite size measured by XRD.

[0139] When calculating the crystallite size, the XRD diffraction pattern is preferably obtained from the positive electrode active material alone. However, it may also be obtained from the positive electrode, which includes a current collector, binder, conductive material, etc., in addition to the positive electrode active material. However, in the positive electrode state, due to the influence of pressure, etc., during the manufacturing process, the particles of the positive electrode active material may be oriented so that the crystal planes of the particles of the positive electrode active material are aligned in one direction. If the orientation is too strong, the crystallite size may not be accurately calculated. Therefore, it is more preferable to obtain the XRD diffraction pattern by removing the positive electrode active material layer from the positive electrode, removing some of the binder, etc., in the positive electrode active material layer using a solvent, etc., and then loading the sample into a sample holder. Another method is to apply grease to a silicon non-reflective plate and attach a powder sample of the positive electrode active material, etc., to the silicon non-reflective plate.

[0140] The crystallite size can be determined, for example, from the following Scherrer formula.

[0141]

[0142] The crystallite size can be calculated using, for example, a Bruker D8 ADVANCE, with CuKa radiation as X-rays, 2θ of 15° to 90° increments of 0.005, and a LYNXEYE XE-T detector, using a diffraction pattern acquired from the detector, and ICSD Coll. Code. 172909 as the literature value for lithium cobalt oxide. Analysis can be performed using DIFFRAC. TOPAS ver. 6 as crystal structure analysis software, and can be set, for example, as follows: Emission Profile: CuKa5. lam Background: Chebychev polynomial, 5th Instrument Primary radius: 280mm Secondary radius: 280mm Linear PSD 2Th angular range: 2.9 FDS angle: 0.3 Full Axial Convolution Filament length: 12mm Sample length: 15mm Receiving Slit length: 12mm Primary Sollers: 2.5 Secondary Sollers: 2.5 Corrections Specimen displacement: Refine LP Factor: 0

[0143] It is preferable to use the value of LVol-IB, which is the crystallite size calculated by the above method, as the crystallite size. Note that if the calculated preferred orientation is less than 0.8, the sample may be unsuitable for determining the crystallite size because the orientation of the sample is too strong.

[0144] [Distribution] The distribution of the additive elements in the positive electrode active material 100 will be described using the discharged state as an example. To ensure that the surface layer 100a has a stable composition and crystalline structure, the surface layer 100a preferably contains an additive element, and more preferably contains multiple additive elements. Furthermore, the surface layer 100a preferably has a higher concentration of one or more selected additive elements than the interior 100b. Furthermore, the one or more selected additive elements contained in the positive electrode active material 100 preferably have a concentration gradient. Furthermore, it is more preferable that the distribution of the additive elements in the positive electrode active material 100 differs depending on the additive element. For example, it is more preferable that the depth from the surface of the peak of the detected amount differs depending on the additive element. Here, the detected amount peak refers to the maximum detected amount, and the detected amount peak in the surface layer 100a refers to the maximum detected amount in the surface layer 100a. The detected amount may be referred to, for example, as the intensity when the vertical axis is counts in EDX analysis, or as the concentration when the vertical axis is atomic %.

[0145] Of the additive elements, it is preferable that the detected amount of magnesium in the surface layer portion 100a is greater than that in the interior portion 100b. Furthermore, it is preferable that the detected amount of magnesium has a peak in the surface layer portion 100a in a region closer to the surface.

[0146] Of the additive elements, fluorine, like magnesium, preferably has a greater detectable amount in the surface layer portion 100a than in the interior portion 100b. Furthermore, it is preferable that the detectable amount of fluorine has a peak in the surface layer portion 100a in a region closer to the surface.

[0147] Of the additive elements, it is preferable that the detected amount of nickel in the surface layer portion 100a is greater than the detected amount in the interior portion 100b. Furthermore, it is preferable that the detected amount of nickel has a peak in a region closer to the surface of the surface layer portion 100a. For example, it is preferable that the detected amount of nickel in the shell of the surface layer portion 100a is greater than the detected amount of nickel in a region deeper than the shell, and that the detected amount of nickel has a peak in the shell. Here, the ratio (Ni / Co) of the number of nickel (Ni) atoms in the shell of the surface layer portion 100a to the number of cobalt (Co) atoms is less than 1. In other words, the number of nickel (Ni) atoms in the shell of the surface layer portion 100a is less than the number of cobalt (Co) atoms. Furthermore, the ratio (Ni / Co) of the number of nickel (Ni) atoms to the number of cobalt (Co) atoms at the peak of detected nickel is less than 1. Furthermore, the ratio of the number of nickel (Ni) atoms to the number of cobalt (Co) atoms in the region inside the shell (Ni / Co) is smaller than the ratio of the number of nickel (Ni) atoms to the number of cobalt (Co) atoms in the shell (Ni / Co). The amount of nickel detected in the interior 100b may be significantly smaller than that in the surface layer 100a. Therefore, the number of nickel (Ni) atoms is smaller than the number of cobalt (Co) atoms in both the surface layer 100a and the interior 100b. Furthermore, the number of nickel (Ni) atoms in the positive electrode active material 100 is smaller than the number of cobalt (Co) atoms.

[0148] Furthermore, when both magnesium and nickel are present, it is preferable that the distributions of magnesium and nickel overlap. Note that overlapping of the distributions includes the case where the peaks of the detected amounts of magnesium and nickel are the same or the difference between the peaks is 3 nm or less, and the peaks do not have to overlap entirely. For example, the peak of the detected amount of magnesium may be closer to the surface, or the peak of the detected amount of nickel may be closer to the surface.

[0149] Of the additional elements, it is also preferable that the detected amount of titanium in the surface layer portion 100a is greater than the detected amount in the interior portion 100b. Furthermore, it is preferable that the detected amount of titanium has a peak in the surface layer portion 100a in a region closer to the surface.

[0150] Of the additive elements, it is also preferable that the detected amount of silicon, phosphorus, boron, and / or calcium in the surface layer portion 100a is greater than the detected amount in the interior portion 100b. It is also preferable that the detected amount of silicon, phosphorus, boron, and / or calcium has a peak in a region closer to the surface of the surface layer portion 100a.

[0151] Of the additive elements, aluminum preferably has a peak of detected amount further inward than magnesium. The distributions of magnesium and aluminum may overlap, or there may be little overlap between the distributions of magnesium and aluminum. Note that overlapping distributions includes the peaks of detected amount of magnesium and aluminum being the same or the difference between the peaks being 3 nm or less, and the peaks do not have to overlap entirely. The peak of detected amount of aluminum may be present in the surface layer 100a or may be deeper than the surface layer 100a. If the peak of detected amount of aluminum is deeper than the surface layer 100a, there may be little overlap between the distributions of magnesium and aluminum. For example, aluminum preferably has a peak in the region of 5 nm to 30 nm from the surface toward the interior. The reason aluminum is distributed more inward than magnesium is thought to be because aluminum diffuses more easily than magnesium.

[0152] The distribution of aluminum may not be a normal distribution. For example, if the curve of the distribution of aluminum is Al When divided by the length, the length of the tail may differ between the surface side and the inside side. Al ) height 1 / 5 (1 / 5 Max Al When the peak width at the surface side is divided into two by a perpendicular line drawn from the maximum value to the horizontal axis, the peak width at the surface side (W s ) than the inner peak width (W c ) may be large.

[0153] On the other hand, the reason why the amount of aluminum detected is small in the region closest to the surface is presumably because aluminum exists more stably in the region where magnesium and the like are not present in solid solution at a high concentration than in the region where magnesium and the like are not present in solid solution at a high concentration. More specifically, in the region of the layered rock salt type of space group R-3m or the rock salt type of cubic crystal system, in the region where magnesium is present in solid solution at a high concentration, layered rock salt type LiAlO 2 Compared to the case of cobalt, the distance between the cation and oxygen is long, making it difficult for aluminum to exist stably. + is Mg 2+ The valence change due to substitution to Co 3+ From Co 2+ However, since Al can only be trivalent, it is thought that it is difficult for it to coexist with magnesium in a rock salt or layered rock salt structure.

[0154] Of the added elements, manganese preferably has a peak of detectable amount inside magnesium, similar to aluminum.

[0155] However, the distribution of the additive element does not necessarily have to be the same throughout the entire surface layer portion 100 a of the positive electrode active material 100 .

[0156] For example, the distribution of the additive element may be different in a region of the positive electrode active material 100 having a (001)-oriented surface compared to a region having a surface other than the (001)-oriented surface. For example, the (001)-oriented surface and its surface layer 100a may have a lower detected amount of one or more selected from the additive elements compared to a surface other than the (001)-oriented surface. Specifically, the detected amount of nickel may be low. In particular, in the case of an analytical method for detecting characteristic X-rays such as EDX, the Kβ of cobalt and the Kα of nickel are close in energy, making it difficult to detect trace amounts of nickel in a material in which cobalt is the main element. Therefore, it is preferable to confirm the presence of nickel using point analysis in addition to line analysis. Alternatively, the region having a (001)-oriented surface may have one or more peaks selected from the additive elements positioned shallower from the surface compared to a region having a surface other than the (001)-oriented surface. Specifically, the peaks for magnesium and aluminum may be positioned shallower from the surface. The region having the above-mentioned surface is included in the surface layer 100a.

[0157] The reason why the positions of the magnesium and aluminum peaks are shallower from the surface in the region with a (001) oriented surface is considered. In the layered rock salt type crystal structure of R-3m, cations are arranged parallel to the (001) plane. This is due to CoO 2 It can be said that the structure is one in which the CoO layer and the lithium layer are alternately stacked parallel to the (001) plane. Therefore, the diffusion path of lithium ions also exists parallel to the (001) plane. 2 Since the layer is relatively stable, it is more stable for the surface of the positive electrode active material 100 to have a (001) orientation. Therefore, magnesium and aluminum are less likely to diffuse, and the positions of these peaks become shallower from the surface.

[0158] Furthermore, the main diffusion path of lithium ions during charge and discharge is not exposed on the (001) plane. On the other hand, the diffusion path of lithium ions is exposed on surfaces other than the (001) orientation. Therefore, the surface other than the (001) orientation and its surface layer 100a are important regions for maintaining the diffusion path of lithium ions, and at the same time, they are prone to instability because they are the regions from which lithium ions are first desorbed. Therefore, in order to maintain the crystal structure of the entire positive electrode active material 100, it is preferable to reinforce at least the surface other than the (001) orientation and its surface layer 100a.

[0159] Therefore, in the positive electrode active material 100, attention may be paid to the concentration distribution of the additive element on the surface other than the (001) orientation and on the surface layer 100a thereof. Among the additive elements, it is preferable that magnesium, in particular, be detected on the surface other than the (001) orientation and on the surface layer 100a thereof. On the other hand, as described above, the concentration of the additive element on the (001) oriented surface and on the surface layer 100a thereof may be low or absent. Nickel may not be present on the (001) oriented surface and on the surface layer 100a thereof.

[0160] For example, the half-width of the magnesium distribution in the (001)-oriented surface and its surface layer portion 100a is preferably 10 nm to 200 nm, more preferably 50 nm to 150 nm, and even more preferably 80 nm to 120 nm. Furthermore, the half-width of the magnesium distribution in the non-(001)-oriented surface and its surface layer portion 100a is preferably 200 nm to 500 nm, more preferably 200 nm to 300 nm, and even more preferably 230 nm to 270 nm. In other words, the half-width of the magnesium distribution may be wider in the non-(001)-oriented surface and its surface layer portion 100a than in the (001)-oriented surface and its surface layer portion 100a.

[0161] The half-width of the nickel distribution in the non-(001) oriented surface and its surface layer 100a is preferably 30 nm or more and 150 nm or less, more preferably 50 nm or more and 130 nm or less, and even more preferably 70 nm or more and 110 nm or less.

[0162] In a manufacturing method in which the additive element is mixed and then heated, which will be described in a later embodiment, the additive element may spread through the diffusion path of lithium ions. Therefore, in order to make the distribution of the additive element in the surface other than the (001) orientation and the surface layer portion 100a thereof within a preferred range, it is better to mix the additive element and heat it after manufacturing lithium cobalt oxide with high purity or lithium cobalt oxide with a smooth surface.

[0163] [Magnesium] Magnesium is divalent, and in the layered rock-salt crystal structure, since the added element aluminum or nickel is stably present at the cobalt site, magnesium ions tend to be present at the lithium site rather than the cobalt site, i.e., they tend to enter the lithium site. The presence of magnesium at an appropriate concentration at the lithium site of the surface layer 100a makes it easier to maintain the layered rock-salt crystal structure. This is because magnesium present at the lithium site is easily absorbed by CoO 2 It is presumed that this is because it functions as a pillar supporting the layers. x CoO 2 When x in the formula (1) is, for example, 0.24 or less, the desorption of oxygen from the surroundings of magnesium can be suppressed, thereby suppressing the thermal decomposition reaction. Furthermore, the presence of magnesium is expected to increase the density of the positive electrode active material 100. Furthermore, a high magnesium concentration in the surface layer portion 100a is expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of an organic electrolyte solution or the like.

[0164] At an appropriate concentration, magnesium does not adversely affect the intercalation and deintercalation of lithium during charging and discharging, providing the above benefits. However, excessive magnesium may adversely affect the intercalation and deintercalation of lithium. Furthermore, the effect on stabilizing the crystal structure may be reduced. This is thought to be due to magnesium occupying the cobalt site in addition to the lithium site. In addition, unnecessary magnesium compounds (e.g., oxides and fluorides) that do not substitute for either the lithium or cobalt site may segregate on the surface of the positive electrode active material and become resistance components in the secondary battery. Furthermore, as the magnesium concentration in the positive electrode active material increases, the discharge capacity of the positive electrode active material may decrease. This is thought to be due to excessive magnesium occupancy at the lithium site, reducing the amount of lithium contributing to charging and discharging.

[0165] Therefore, it is preferable that the amount of magnesium contained in the entire positive electrode active material 100 is appropriate. For example, the number of magnesium atoms is preferably 0.002 to 0.06 times the number of cobalt atoms, more preferably 0.005 to 0.03 times, and even more preferably about 0.01 times. The amount of magnesium contained in the entire positive electrode active material 100 referred to here may be a value obtained by performing elemental analysis of the entire positive electrode active material 100 using, for example, glow discharge mass spectrometry (GD-MS) or inductively coupled plasma mass spectrometry (ICP-MS), or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material 100.

[0166] [Fluorine] Fluorine is a monovalent anion, and when fluorine is adsorbed on the surface of the positive electrode active material 100, the energy required for lithium desorption from the positive electrode active material 100 is reduced. As long as this energy is reduced, fluorine may replace part of the oxygen in the surface layer 100a. This is because the redox potential of cobalt ions accompanying lithium desorption differs depending on the presence or absence of fluorine. That is, in the absence of fluorine, cobalt ions change from trivalent to tetravalent upon lithium desorption. On the other hand, in the presence of fluorine, cobalt ions change from divalent to trivalent upon lithium desorption. The redox potential of cobalt ions differs between the two. Therefore, desorption and insertion of lithium ions near the fluorine is more likely to occur smoothly, and it is preferable to have fluorine on the surface or surface layer of the positive electrode active material 100. When the fluorine-containing positive electrode active material 100 is used in a secondary battery, the charge / discharge characteristics, large current characteristics, etc. can be improved. Furthermore, the presence of fluorine on the surface or surface layer that is in contact with the electrolyte, or the adsorption or adhesion of fluoride to the surface, can suppress excessive reaction between the positive electrode active material 100 and the electrolyte, and can also effectively improve corrosion resistance to hydrofluoric acid.

[0167] [Nickel] Nickel can exist on either the cobalt site or the lithium site. When present on the cobalt site, nickel has a lower redox potential than cobalt, which means that it is easier to release lithium during charging, for example. This is expected to result in faster charge and discharge speeds.

[0168] Furthermore, when nickel exists at the lithium site, the layer structure consisting of octahedra of cobalt and oxygen can be prevented from shifting. Also, the change in volume caused by charging and discharging is prevented. Also, the elastic modulus increases, that is, the material becomes hard. This is because nickel existing at the lithium site can also be prevented from shifting to CoO 2 This is presumably because they function as pillars supporting the layers together. Therefore, it is expected that the crystal structure will be more stable, particularly in a charged state at high temperatures, for example, 45° C. or higher, which is preferable.

[0169] Nickel can exist on both the cobalt and lithium sites. When nickel exists on the cobalt site, it has a lower redox potential than cobalt, so it can easily release lithium during discharge. This can be expected to increase the charge / discharge speed, i.e., improve the charge / discharge rate characteristics.

[0170] The distance between the cations and anions of nickel oxide (NiO) is larger than that of LiCoO compared with MgO and CoO. 2 The average distance between the cations and anions is close to that of LiCoO 2 The orientation is likely to match.

[0171] In addition, the ionization tendency decreases in the order of magnesium, aluminum, cobalt, and nickel (Mg>Al>Co>Ni). Therefore, nickel is thought to be less likely to dissolve into the electrolyte than the other elements listed above during charging. Therefore, it is thought to be highly effective in stabilizing the crystalline structure of the surface layer when in a charged state.

[0172] Furthermore, nickel is Ni 2+ , Ni 3+ , Ni 4+ Of which Ni 2+ is the most stable, and nickel has a higher trivalent ionization energy than cobalt. Therefore, it is known that nickel and oxygen alone do not form a spinel-type crystal structure. Therefore, nickel is thought to have the effect of suppressing the phase change from the layered rock salt type to the spinel-type crystal structure.

[0173] On the other hand, an excess of nickel is undesirable because it increases the influence of strain due to the Jahn-Teller effect, and may also adversely affect the insertion and extraction of lithium.

[0174] Therefore, it is preferable that the total amount of nickel in the positive electrode active material 100 is appropriate. For example, the number of nickel atoms in the positive electrode active material 100 is smaller than the number of cobalt atoms, and is preferably more than 0% but not more than 7.5%, preferably 0.05% to 4%, preferably 0.1% to 2%, and more preferably 0.2% to 1% of the total number of cobalt atoms. Alternatively, more than 0% but not more than 4% is preferable. Alternatively, more than 0% but not more than 2% is preferable. Alternatively, 0.05% to 7.5% is preferable. Alternatively, 0.05% to 2% is preferable. Alternatively, 0.1% to 7.5% is preferable. Alternatively, 0.1% to 4% is preferable. The amount of nickel shown here may be, for example, a value obtained by performing elemental analysis of the entire positive electrode active material using GD-MS, ICP-MS, or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.

[0175] [Aluminum] Aluminum can also be present at the cobalt site in a layered rock salt crystal structure. Because aluminum is a trivalent typical element and its valence does not change, lithium around the aluminum is less likely to move during charging and discharging. Therefore, the aluminum and its surrounding lithium function as pillars, suppressing changes in the crystal structure. Therefore, as described below, even if the positive electrode active material 100 experiences a force that causes it to expand and contract in the c-axis direction due to the insertion and desorption of lithium ions, i.e., even if a force that causes it to expand and contract in the c-axis direction due to changes in the charge depth or charge rate occurs, deterioration of the positive electrode active material 100 can be suppressed.

[0176] Aluminum also has the effect of suppressing the elution of surrounding cobalt and improving continuous charge durability. Furthermore, since the Al—O bond is stronger than the Co—O bond, it can suppress the desorption of oxygen from the aluminum's surroundings. These effects improve thermal stability. Therefore, the presence of aluminum as an additive element can improve safety when the positive electrode active material 100 is used in a secondary battery. Furthermore, the positive electrode active material 100 can be made to have a crystal structure that is resistant to collapse even after repeated charge and discharge.

[0177] On the other hand, an excess of aluminum may adversely affect the intercalation and deintercalation of lithium.

[0178] Therefore, it is preferable that the aluminum content of the entire cathode active material 100 is an appropriate amount. For example, the number of aluminum atoms contained in the entire cathode active material 100 is preferably 0.05% to 4% of the number of cobalt atoms, preferably 0.1% to 2%, and more preferably 0.3% to 1.5%. Alternatively, 0.05% to 2% is preferable. Alternatively, 0.1% to 4% is preferable. The amount contained in the entire cathode active material 100 referred to here may be, for example, a value obtained by performing elemental analysis of the entire cathode active material 100 using GD-MS, ICP-MS, or the like, or may be based on the value of the composition of raw materials in the process of producing the cathode active material 100.

[0179] Titanium oxide is also known to have superhydrophilic properties. Therefore, by providing the cathode active material 100 with titanium oxide in the surface layer 100a, it is possible that the cathode active material 100 may have good wettability with highly polar solvents. When used in a secondary battery, this may improve the contact at the interface between the cathode active material 100 and a highly polar electrolyte, thereby suppressing an increase in internal resistance.

[0180] Furthermore, when phosphorus is present in the surface layer 100a, Li x CoO 2 When the value of x in the formula (100a) is kept small, it is possible to suppress short circuits, which is preferable. For example, it is preferable that the compound containing phosphorus and oxygen is present in the surface layer portion 100a.

[0181] When the positive electrode active material 100 contains phosphorus, the phosphorus reacts with hydrogen fluoride generated by decomposition of the electrolyte or lithium salt, which may reduce the concentration of hydrogen fluoride in the electrolyte, which is preferable.

[0182] The lithium salt is LiPF 6 In the case where the organic electrolyte solution contains the above-mentioned fluorine-containing polymer, hydrogen fluoride may be generated by hydrolysis. Furthermore, hydrogen fluoride may be generated by a reaction between polyvinylidene fluoride (PVDF), which is used as a component of the positive electrode, and an alkali. By reducing the hydrogen fluoride concentration in the organic electrolyte solution, corrosion of the current collector and / or peeling of the coating portion 104 (see FIG. 15 ) may be suppressed. Furthermore, a decrease in adhesion due to gelation and / or insolubilization of PVDF may be suppressed.

[0183] When the positive electrode active material 100 contains phosphorus together with magnesium, Li x CoO 2 This is preferable because the stability of the crystal structure is extremely high when x is small. When the positive electrode active material 100 contains phosphorus, the number of phosphorus atoms is preferably 1% to 20% of the number of cobalt atoms, more preferably 2% to 10%, and even more preferably 3% to 8%. Or 1% to 10% is preferable. Or 1% to 8% is preferable. Or 2% to 20% is preferable. Or 2% to 8% is preferable. Or 3% to 20% is preferable. Or 3% to 10% is preferable. In addition, the number of magnesium atoms is preferably 0.1% to 10% of the number of cobalt atoms, more preferably 0.5% to 5%, and more preferably 0.7% to 4%. Or 0.1% to 5% is preferable. Or 0.1% to 4% is preferable. Or 0.5% to 10% is preferable. Or 0.5% to 4% is preferable. Or 0.7% to 10% is preferable. The concentrations of phosphorus and magnesium shown here may be values ​​obtained by performing elemental analysis of the entire cathode active material 100 using, for example, GD-MS, ICP-MS, or the like, or may be based on values ​​of the composition of raw materials in the process of producing the cathode active material 100.

[0184] Furthermore, when a crack 102 is formed on a portion of the surface of the positive electrode active material 100, the progression of the crack can be suppressed by the presence of phosphorus, more specifically, a compound containing, for example, phosphorus and oxygen, in the embedded portion in contact with the portion of the surface.

[0185] [Synergistic Effect of Multiple Elements] Furthermore, when the surface layer portion 100a contains both magnesium and nickel, there is a possibility that divalent nickel can exist more stably near divalent magnesium. x CoO 2 Even when the value of x in the formula is small, the elution of magnesium can be suppressed, which can contribute to the stabilization of the surface layer portion 100a.

[0186] For the same reason, in the manufacturing process, when adding an additive element to lithium cobalt oxide, it is preferable that magnesium be added in a step before nickel. Alternatively, it is preferable that magnesium and nickel be added in the same step. Magnesium has a large ionic radius and tends to remain in the surface layer of lithium cobalt oxide regardless of the step in which it is added, whereas nickel can diffuse widely into the interior of lithium cobalt oxide in the absence of magnesium. Therefore, if nickel is added before magnesium, there is a concern that nickel will diffuse into the interior of the lithium cobalt oxide and not remain in the surface layer in a desired amount.

[0187] Furthermore, the inclusion of additive elements with different distributions is preferable because it stabilizes the crystal structure in a wider region. For example, if the positive electrode active material 100 contains magnesium, nickel, and aluminum, it can stabilize the crystal structure in a wider region than if it contains only one of these elements. In this way, when the positive electrode active material 100 contains additive elements with different distributions, magnesium, nickel, etc. can sufficiently stabilize the surface, so aluminum is not essential to the surface. Rather, it is preferable for aluminum to be distributed widely in a deeper region. For example, it is preferable for aluminum to be continuously detected in a region from 1 nm to 25 nm in the depth direction from the surface. A wide distribution in a region from 0 nm to 100 nm from the surface, preferably a region from 0.5 nm to 50 nm from the surface, is preferable because it stabilizes the crystal structure in a wider region.

[0188] When a plurality of additive elements are contained as described above, the effects of the respective additive elements are synergistic, which can contribute to further stabilization of the surface layer portion 100 a. In particular, when magnesium, nickel, and aluminum are contained, the effect of providing a stable composition and crystal structure is high, which is preferable.

[0189] However, if the surface layer 100a is occupied only by a compound of the additive element and oxygen, it is not preferable because it makes it difficult to insert and extract lithium. For example, it is not preferable for the surface layer 100a to be occupied only by MgO, a structure in which MgO and NiO(II) are solid-solved, and / or a structure in which MgO and CoO(II) are solid-solved. Therefore, the surface layer 100a must contain at least cobalt, and in the discharged state, it must also contain lithium, and it must have a path for the insertion and extraction of lithium.

[0190] In order to ensure sufficient paths for lithium insertion and desorption, the surface layer portion 100a preferably has a higher cobalt concentration than magnesium. For example, when measured from the surface of the positive electrode active material 100 using XPS (X-ray photoelectron spectroscopy), the ratio Mg / Co of the number of magnesium atoms Mg to the number of cobalt atoms Co is preferably 0.62 or less. The surface layer portion 100a preferably has a higher cobalt concentration than nickel. The surface layer portion 100a preferably has a higher cobalt concentration than aluminum. The surface layer portion 100a preferably has a higher cobalt concentration than fluorine.

[0191] Furthermore, since an excessive amount of nickel may inhibit the diffusion of lithium, it is preferable that the concentration of magnesium is higher than that of nickel in the surface layer portion 100 a. For example, when measured from the surface of the positive electrode active material 100 by XPS, the number of nickel atoms is preferably 1 / 6 or less of the number of magnesium atoms.

[0192] Furthermore, it is preferable that some of the added elements, particularly magnesium, nickel, and aluminum, have a higher concentration in the surface layer 100a than in the interior 100b, but it is also preferable that they are present randomly and in a sparse manner in the interior 100b. When magnesium and aluminum are present at appropriate concentrations at the lithium sites in the interior 100b, it has the effect of making it easier to maintain the layered rock-salt crystal structure, as described above. Furthermore, when nickel is present at an appropriate concentration in the interior 100b, it is possible to suppress the deviation of the layered structure consisting of the transition metal M and oxygen octahedra, as described above. Furthermore, when magnesium and nickel are present together, a synergistic effect of suppressing the elution of magnesium can be expected, as described above.

[0193] <Li x MO2 The positive electrode active material 100 of one embodiment of the present invention has the above-described distribution of the additional element and / or the crystal structure, and therefore, x MO 2 The crystal structure in the state where x is small, i.e., in the charged state at a high voltage, differs from that of conventional positive electrode active materials. Here, "small x" means 0.1 < x ≦ 0.24. Furthermore, "high voltage in the charged state" means 4.5 V or higher, preferably 4.6 V or higher, and more preferably 4.8 V or higher.

[0194] 8 and 9, Li x MO 2 The change in the crystal structure accompanying the change in x in the positive electrode active material 100 will be described by comparing a conventional positive electrode active material with the positive electrode active material 100 of one embodiment of the present invention.

[0195] The change in the crystal structure of a conventional positive electrode active material is shown in FIG. 9. The conventional positive electrode active material shown in FIG. 9 is a lithium cobalt oxide (LiCoO 2 In particular, changes in the crystal structure of lithium cobalt oxide that does not contain any added elements are described in Non-Patent Documents 1 to 3, etc.

[0196] In Figure 9, R-3m O3 is added to show the discharge state, i.e., Li x CoO 2 1 shows the crystal structure of lithium cobalt oxide where x = 1. In a discharged state, conventional lithium cobalt oxide has the same crystal structure as the positive electrode active material 100 of one embodiment of the present invention.

[0197] It is also known that conventional lithium cobalt oxide has a crystal structure that has high lithium symmetry when x is about 0.5 and belongs to the monoclinic space group P2 / m. This structure has CoO 2 There is one layer, so it is sometimes called O1 type or monoclinic (indicated as monoclinic in the figure) O1 type.

[0198] When x = 0, the positive electrode active material has a crystal structure of the trigonal space group P-3m1, and also contains CoO 2There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal (indicated as trigonal in the figure) O1 type. In addition, the trigonal crystal is sometimes converted into a composite hexagonal lattice and called hexagonal O1 type.

[0199] Furthermore, when x is about 0.12, conventional lithium cobalt oxide has a crystal structure of the space group R-3m. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m O 2 It can also be said that the structure of and the structure of are stacked alternately. Therefore, this crystal structure is sometimes called the H1-3 type crystal structure (denoted as H1-3 in the figure). Note that, since the actual insertion and desorption of lithium does not necessarily occur uniformly within the positive electrode active material and the lithium concentration may become uneven, the H1-3 type crystal structure is experimentally observed from about x = 0.25. In addition, in reality, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures.

[0200] As an example of the H1-3 type crystal structure, as described in Non-Patent Document 3, the coordinates of cobalt and oxygen in a unit cell can be expressed as Co (0,0,0.42150±0.00016), O1 (0,0,0.27671±0.00045), and O2 (0,0,0.11535±0.00045). O1 and O2 are each oxygen atoms. Which unit cell should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of the XRD pattern. For example, it is preferable to adopt a unit cell with a GOF (goodness of fit) value close to 1.

[0201] Li, which can be experimentally confirmed to have an H1-3 type crystal structure x CoO 2 When charging and discharging are repeated so that x in the formula is 0.24 or less, conventional lithium cobalt oxide undergoes repeated changes in crystal structure (i.e., non-equilibrium phase changes) between the H1-3 type crystal structure and the R-3m O3 structure in the discharged state.

[0202] These two crystal structures are CoO 2 As shown by the dotted line in FIG. 9, in the H1-3 type crystal structure, CoO2 The layer is significantly different from the R-3m O3 in the discharged state. Such dynamic structural changes can adversely affect the stability of the crystal structure.

[0203] Furthermore, the difference in volume between these two crystal structures is large: per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the discharged R-3mO3 crystal structure is greater than 3.5%, typically 3.9% or more.

[0204] In addition, the H1-3 type crystal structure has CoO like the trigonal O1 type. 2 A structure with continuous layers is likely to be unstable.

[0205] Therefore, when charging and discharging are repeated so that x is 0.24 or less, the crystal structure of conventional lithium cobalt oxide collapses. This collapse of the crystal structure causes a deterioration in cycle characteristics. This is because the collapse of the crystal structure reduces the number of sites where lithium can exist stably and makes it difficult for lithium to be inserted and extracted.

[0206] On the other hand, in the positive electrode active material 100 according to one embodiment of the present invention shown in FIG. x MO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less is smaller than that of conventional positive electrode active materials. 2 The layer misalignment can be reduced. When the cathode active material 100 having the same number of transition metal M atoms is compared with a conventional cathode active material, the volume change of the cathode active material 100 is smaller than that of the conventional cathode active material. Therefore, the crystal structure of the cathode active material 100 of one embodiment of the present invention is not easily broken even when charging and discharging are repeated so that x is 0.24 or less, and sites where lithium can stably exist are maintained, thereby achieving excellent cycle characteristics.

[0207] The positive electrode active material 100 according to one embodiment of the present invention is Li x MO 2 When x is 0.24 or less, the positive electrode active material 100 can have a more stable crystal structure than conventional positive electrode active materials. x MO2 Even when the value of x in the positive electrode active material 100 is kept at 0.24 or less, oxygen is unlikely to be released, and a thermal decomposition reaction can be suppressed. In other words, a secondary battery using the positive electrode active material 100 of one embodiment of the present invention is preferable because it has improved safety.

[0208] Li x MO 2 The crystal structure of the inner portion 100b of the positive electrode active material 100 when x is 1, approximately 0.2, and approximately 0.15 is shown in FIG. 8. The inner portion 100b occupies the majority of the volume of the positive electrode active material 100 and is the portion that contributes greatly to charge and discharge. 2 The most problematic areas are layer misalignment and volume changes.

[0209] As described above, the cathode active material 100 has the same R-3m O3 crystal structure as conventional lithium cobalt oxide when x = 1. However, when x is 0.24 or less, for example, approximately 0.2 or 0.15, which is the value at which conventional lithium cobalt oxide has an H1-3 type crystal structure, the cathode active material 100 has a different crystal structure.

[0210] The positive electrode active material 100 of one embodiment of the present invention when x is about 0.2 has a crystal structure belonging to the trigonal space group R-3m. 2 The layer symmetry is the same as that of O3. Therefore, this crystal structure will be referred to as an O3'-type crystal structure. Alternatively, although it is not a spinel structure, a pattern similar to a spinel structure may appear in the XRD pattern, and this crystal structure may be referred to as a pseudo-spinel structure. This crystal structure is shown in FIG. 8 with R-3m O3'. As will be described later, it may become an H1-3-type crystal structure via the O3'-type crystal structure. However, the positive electrode active material 100 that has passed through the O3'-type crystal structure can exhibit the effect of suppressing oxygen release even if it becomes an H1-3-type crystal structure, for example. Therefore, it is estimated that even if a nail penetration test is performed on a lithium ion secondary battery using this positive electrode active material 100, ignition will be suppressed.

[0211] In the O3' type crystal structure, when M is cobalt, the coordinates of cobalt and oxygen in the unit cell can be expressed in the range of Co(0,0,0.5), O(0,0,x), 0.20≦x≦0.25. The lattice constant of the unit cell is 2.797×10 for the a-axis. −10 ≦a≦2.837×10 −10 (m) is preferred, and 2.807 × 10 −10 ≦a≦2.827×10 −10 (m) is more preferable, and typically a=2.817×10 −10 (m). The c-axis is 13.681 × 10 −10 ≦c≦13.881×10 −10 (m) is preferred, and 13.751 × 10 −10 ≦c≦13.811×10 −10 (m) is more preferable, and typically c=13.781×10 −10 (m).

[0212] Furthermore, the positive electrode active material 100 of one embodiment of the present invention when x is about 0.15 has a crystal structure belonging to the monoclinic space group P2 / m. 2 There is one layer. Furthermore, when x = 0.15, it can be considered that the lithium present in the positive electrode active material 100 is about 15 atomic % in the discharged state. Therefore, this crystal structure is called a monoclinic O1(15) type crystal structure. This crystal structure is shown in Figure 9, labeled P2 / m monoclinic O1(15).

[0213] In the monoclinic O1(15) crystal structure, when M is cobalt, the coordinates of cobalt and oxygen in the unit cell are Co1(0.5,0,0.5), Co2(0,0.5,0.5), O1(X O1 , 0, Z O1 ), 0.23≦X O1 ≦0.24, 0.61≦Z O1 ≦0.65, O2(X O2 , 0.5, Z O2 ), 0.75≦X O2 ≦0.78, 0.68≦Z O2The lattice constants of the unit cell are a = 0.4880 ± 0.005 nm, b = 0.2817 ± 0.005 nm, c = 0.4839 ± 0.005 nm, α = 90°, β = 109.6 ± 0.1°, and γ = 90°.

[0214] In addition, this crystal structure can show the lattice constant even in the space group R-3m if a certain degree of error is allowed in the Rietveld analysis etc. In this case, the coordinates of cobalt and oxygen in the unit cell are Co(0,0,0.5), O(0,0,Z O ), 0.21≦Z O The lattice constants of the unit cell are a = 0.2817 ± 0.002 nm and c = 1.368 ± 0.01 nm.

[0215] In both the O3' and monoclinic O1(15) crystal structures, ions of cobalt, nickel, magnesium, etc. occupy hexacoordinated oxygen sites, although lighter elements such as lithium and magnesium may occupy tetracoordinated oxygen sites.

[0216] In the discharged state, R-3m O3, O3', and the monoclinic O1(15) type crystal structure, MO 2 There is almost no layer misalignment.

[0217] The difference in volume per the same number of cobalt atoms between R-3m O3 in a discharged state and the O3' type crystal structure is 2.5% or less, more specifically 2.2% or less, typically 1.8%.

[0218] The difference in volume per the same number of cobalt atoms between R-3m O3 in a discharged state and the monoclinic O1(15) type crystal structure is 3.3% or less, more specifically 3.0% or less, typically 2.5%.

[0219] The table below shows the difference in volume per cobalt atom between discharged R-3m O3, O3', monoclinic O1(15), H1-3, and trigonal O1. For the lattice constants of the crystal structures of discharged R-3m O3 and trigonal O1 used in the calculations in the table below, ICSD Coll. Code. 172909 and 88721 can be referenced. For H1-3, Non-Patent Document 3 can be referenced. For O3' and monoclinic O1(15), calculations can be made from experimental XRD values.

[0220]

[0221] As described above, in the positive electrode active material 100 according to one embodiment of the present invention, Li x CoO 2 When x is small, i.e., when a large amount of lithium is released, the change in the crystal structure is suppressed compared to conventional cathode active materials. Comparing the cathode active material 100 having the same number of cobalt atoms with a conventional cathode active material, the volume change of the cathode active material 100 is smaller than that of the conventional cathode active material. Therefore, the cathode active material 100 is less likely to collapse in crystal structure even when repeatedly charged and discharged so that x is 0.24 or less. Therefore, the cathode active material 100 suppresses the decrease in charge / discharge capacity during charge / discharge cycles. Furthermore, because it can stably utilize more lithium than conventional cathode active materials, the cathode active material 100 has a large discharge capacity per weight and per volume. Therefore, by using the cathode active material 100, a secondary battery with a high discharge capacity per weight and per volume can be fabricated.

[0222] The positive electrode active material 100 is Li x MO 2 It has been confirmed that when x is 0.15 or more and 0.24 or less, the O3' type crystal structure may be formed, and it is estimated that the O3' type crystal structure may also be formed when x is more than 0.24 and 0.27 or less. x MO 2 It has been confirmed that when x is greater than 0.1 and less than 0.2, typically 0.15 or more and less than 0.17, the crystal structure may be monoclinic O1(15) type. However, the crystal structure is x MO 2The range of x is not necessarily limited to the above range, since it is affected not only by x in the formula but also by the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, etc.

[0223] Therefore, the positive electrode active material 100 is Li x MO 2 When x is greater than 0.1 and equal to or less than 0.24, the positive electrode active material 100 may have only the O3' type, only the monoclinic O1(15) type, or both crystal structures. Furthermore, all of the particles in the interior 100b of the positive electrode active material 100 do not necessarily have the O3' type and / or the monoclinic O1(15) type crystal structure. Other crystal structures may be included, or a portion may be amorphous.

[0224] Also Li x MO 2 To make the value of x small, it is generally necessary to charge at a high charging voltage. x MO 2 A state where x is small can be rephrased as a state where the battery is charged at a high charging voltage. For example, when CC / CV charging is performed at a voltage of 4.6 V or higher relative to the potential of lithium metal in an environment of 25°C, a H1-3 crystal structure appears in conventional positive electrode active materials. Therefore, a charging voltage of 4.6 V or higher relative to the potential of lithium metal can be said to be a high charging voltage. Furthermore, in this specification and the like, unless otherwise specified, charging voltages are expressed relative to the potential of lithium metal.

[0225] Therefore, the positive electrode active material 100 of one embodiment of the present invention can be said to be preferable because it can maintain a crystal structure with R-3m O3 symmetry even when charged at a high charge voltage, for example, a voltage of 4.6 V or higher at 25° C. In other words, it can be said to be preferable because it can adopt an O3′-type crystal structure when charged at a higher charge voltage, for example, a voltage of 4.65 V or higher and 4.7 V or lower at 25° C. In other words, it can be said to be preferable because it can adopt a monoclinic O1(15)-type crystal structure when charged at an even higher charge voltage, for example, a voltage of more than 4.7 V and 4.8 V or lower at 25° C.

[0226] Even in the positive electrode active material 100 of one embodiment of the present invention, when the charge voltage is further increased, the H1-3 crystal structure may finally be observed. Furthermore, as described above, the crystal structure is affected by the number of charge / discharge cycles, the charge / discharge current, the temperature, the electrolyte, and the like. Therefore, when the charge voltage is lower, for example, even when the charge voltage is 4.5 V or more and less than 4.6 V at 25° C., the positive electrode active material 100 of one embodiment of the present invention may be able to adopt the O3′ crystal structure. Similarly, when charged at a voltage of 4.65 V or more and 4.7 V or less at 25° C., the positive electrode active material 100 may be able to adopt the monoclinic O1(15) crystal structure.

[0227] In addition, when graphite is used as the negative electrode active material in a secondary battery, the voltage of the secondary battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.05 V to 0.2 V with respect to the potential of lithium metal. Therefore, in the case of a secondary battery using graphite as the negative electrode active material, when the voltage is the above voltage minus the potential of graphite, the secondary battery has the same crystal structure as above.

[0228] In addition, in the O3′ and monoclinic O1(15) of FIG. 8, lithium is shown to exist at all lithium sites with equal probability, but this is not limited to this. It may exist unevenly at some lithium sites, or, for example, the monoclinic O1(Li 0.5 CoO 2 The lithium distribution can be analyzed by, for example, neutron diffraction.

[0229] The O3' and monoclinic O1(15) crystal structures have random lithium between layers, but CdCl 2 It can be said that this crystal structure is similar to that of the CdCl type. 2 A similar crystal structure to the Li-type is lithium nickel oxide. 0.06 NiO 2 However, pure lithium cobaltate or layered rock salt cathode active materials containing a large amount of cobalt usually have a crystal structure similar to that of CdCl 2 It is known that it does not have a typical crystal structure.

[0230] As described above, the conventional lithium cobalt oxide and the positive electrode active material 100 according to one embodiment of the present invention have the same change in charge depth, i.e., Li x CoO 2 The crystal structure changes depending on the change in x in the graph. The change in the c-axis length of conventional lithium cobalt oxide described in Non-Patent Document 12 is shown in Figure 10. The round markers represent the hexagonal phase, and the diamond markers represent the monoclinic phase.

[0231] The change in the c-axis length of lithium cobalt oxide corresponds to the change in the angle at which the peak of, for example, the (003) plane of lithium cobalt oxide appears in the XRD pattern. 1 ray (CuKα ray to CuKα 2 It is known that in XRD (excluding the line), the peak of the (003) plane of lithium cobalt oxide occurs at 2θ of approximately 19° to 20°.

[0232] <Grain Boundary> In addition to the above distribution, at least a part of the additive element contained in the positive electrode active material 100 of one embodiment of the present invention is preferably unevenly distributed in and around the grain boundary 101. Again, the vicinity of the grain boundary 101 refers to a region within 10 nm from the grain boundary 101.

[0233] For example, the magnesium concentration at and near the grain boundaries 101 of the positive electrode active material 100 is preferably higher than that in other regions of the interior 100b. The fluorine concentration at and near the grain boundaries 101 is also preferably higher than that in other regions of the interior 100b. The nickel concentration at and near the grain boundaries 101 is also preferably higher than that in other regions of the interior 100b. The aluminum concentration at and near the grain boundaries 101 is also preferably higher than that in other regions of the interior 100b.

[0234] The grain boundaries 101 are one type of planar defect. Therefore, like the grain surfaces, they tend to become unstable and are prone to change in the crystal structure. Therefore, if the concentration of the added element at and near the grain boundaries 101 is high, the change in the crystal structure can be more effectively suppressed.

[0235] Furthermore, when the magnesium concentration and fluorine concentration are high at and near the grain boundaries 101, even if cracks occur along the grain boundaries 101 of the positive electrode active material 100 of one embodiment of the present invention, the magnesium concentration and fluorine concentration are high on the surface where the cracks occur and in the vicinity thereof. Therefore, even in the positive electrode active material after the cracks occur, the corrosion resistance to hydrofluoric acid can be improved.

[0236] <Analysis method> A certain positive electrode active material is x CoO 2 When x in the formula (I) is small, whether the positive electrode active material 100 of one embodiment of the present invention has an O3′-type and / or monoclinic O1(15)-type crystal structure can be determined by Li x CoO 2 This can be determined by analyzing a positive electrode having a positive electrode active material with a small x using XRD, electron beam diffraction, neutron beam diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), or the like.

[0237] In particular, XRD is preferable in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, it can obtain sufficient accuracy even when measuring the positive electrode obtained by disassembling the secondary battery as it is, etc. Among XRD methods, powder XRD can obtain diffraction peaks that reflect the crystalline structure of the interior 100b of the positive electrode active material 100, which occupies the majority of the volume of the positive electrode active material 100.

[0238] When analyzing the crystallite size by powder XRD, it is preferable to measure the crystallite size while excluding the influence of the orientation of the positive electrode active material particles due to pressure or the like. For example, it is preferable to measure the crystallite size after removing the positive electrode active material layer from the positive electrode obtained by disassembling the secondary battery. Alternatively, the positive electrode active material may be removed from the positive electrode active material layer before measurement.

[0239] As described above, the positive electrode active material 100 according to one embodiment of the present invention is x CoO 2 The characteristic of this material is that there is little change in the crystal structure when x is 1 and when it is 0.24 or less. Materials in which the crystal structure that undergoes large changes when charged at high voltage accounts for 50% or more of the crystal structure are not preferable because they cannot withstand repeated high-voltage charging and discharging.

[0240] It should be noted that simply adding an additive element may not result in an O3'-type or monoclinic O1(15)-type crystal structure. For example, even if lithium cobalt oxide containing magnesium and fluorine or lithium cobalt oxide containing magnesium and aluminum has something in common, depending on the concentration and distribution of the additive element, Li x CoO 2 In some cases, x is 0.24 or less and the O3' type and / or monoclinic O1(15) type crystal structure accounts for 60% or more, and in other cases the H1-3 type crystal structure accounts for 50% or more.

[0241] Furthermore, even in the positive electrode active material 100 of one embodiment of the present invention, an H1-3 type or trigonal O1 type crystal structure may be formed when x is too small, such as 0.1 or less, or under conditions where the charge voltage exceeds 4.9 V. Therefore, to determine whether or not the positive electrode active material 100 of one embodiment of the present invention is the positive electrode active material 100, analysis of the crystal structure, such as XRD, and information such as the charge capacity or the charge voltage are required.

[0242] However, when a positive electrode active material with a small x is exposed to the air, its crystal structure may change. For example, the crystal structure may change from O3'-type and monoclinic O1(15)-type to H1-3-type. Therefore, it is preferable to handle all samples used for crystal structure analysis in an inert atmosphere such as an argon atmosphere.

[0243] Furthermore, whether the distribution of the additive elements contained in a certain positive electrode active material is in the state described above can be determined by analysis using, for example, XPS, EDX, EPMA (electron probe microanalysis), or the like.

[0244] The crystal structure of the surface layer 100 a, the grain boundaries 101 , etc. can be analyzed by electron beam diffraction of a cross section of the positive electrode active material 100 .

[0245] Whether a certain composite oxide is the positive electrode active material 100 of one embodiment of the present invention can be determined by, for example, fabricating a coin cell (CR2032 type, diameter 20 mm, height 3.2 mm) using the composite oxide for the positive electrode and lithium metal for the counter electrode, and charging the coin cell. The coin cell includes an electrolyte, a separator, a positive electrode can, and a negative electrode can.

[0246] More specifically, the positive electrode may be prepared by coating a positive electrode current collector made of aluminum foil with a slurry containing the composite oxide as a positive electrode active material, a conductive material, and a binder.

[0247] As described above, lithium metal can be used for the counter electrode, but materials other than lithium metal may also be used. When a material other than lithium metal is used, the potential of the secondary battery differs from the potential of the positive electrode. Unless otherwise specified, the voltage and potential in this specification refer to the potential of the positive electrode.

[0248] The lithium salt contained in the electrolyte solution is 1 mol / L lithium hexafluorophosphate (LiPF 6 ) is used, and the electrolyte may be a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 with 2 wt % vinylene carbonate (VC).

[0249] The separator may be a 25 μm thick porous polypropylene film.

[0250] The positive electrode can and the negative electrode can may be made of stainless steel (SUS).

[0251] The coin cell prepared under the above conditions is charged to a desired voltage (e.g., 4.5 V, 4.55 V, 4.6 V, 4.65 V, 4.7 V, 4.75 V, or 4.8 V). The charging method is not particularly limited as long as it allows sufficient time for charging to the desired voltage. For example, when charging by CCCV, the CC charging current can be set to 20 mA / g or more and 100 mA / g or less. CV charging can be terminated at 2 mA / g or more and 10 mA / g or less. To observe the phase change of the positive electrode active material, it is desirable to charge at such a low current value. Because XRD measurements are difficult to perform below 0°C, the temperature is set to 25°C. Note that the temperature of 25°C is an example. After charging in this manner, the coin cell can be disassembled in a glove box under an argon atmosphere and the positive electrode removed to obtain a positive electrode active material with the desired charge capacity. When performing various subsequent analyses, it is preferable to seal the cell in an argon atmosphere to prevent reactions with external components. For example, XRD measurement can be performed with the positive electrode active material sealed in a sealed container under an argon atmosphere. After charging is completed, the positive electrode is preferably removed promptly and the XRD analysis described below is started. Specifically, the XRD analysis is preferably performed within 1 hour, more preferably within 30 minutes, after charging is completed.

[0252] When analyzing the crystal structure in the charged state after multiple charge / discharge cycles, the conditions for the multiple charge / discharge cycles may be different from the above-mentioned conditions for charge / discharge. For example, charging can be performed by constant current charging at a current value of 20 mA / g or more and 100 mA / g or less up to a given voltage (e.g., 4.6 V, 4.65 V, 4.7 V, 4.75 V, or 4.8 V), followed by constant voltage charging until the current value reaches 2 mA / g or more and 10 mA / g or less, and then discharging by constant current discharging at a current value of 20 mA / g or more and 100 mA / g or less up to 2.5 V.

[0253] Furthermore, when analyzing the crystal structure in the discharged state after multiple charge / discharge cycles, the discharge conditions for the multiple charge / discharge cycles can be, for example, constant current discharge at 2.5 V and a current value of 20 mA / g or more and 100 mA / g or less.

[0254] <XRD> As long as proper adjustment and calibration are performed, the XRD measurement device and conditions are not particularly limited. For example, the measurement can be performed using the following device and conditions. XRD device: D8 ADVANCE manufactured by Bruker AXS X-ray: Cukα radiation, Cukα 1 Line output: 40 kV, 40 mA Divergence angle: Div. Slit, 0.5° Detector: LynxEye Scan method: 2θ / θ continuous scan Measurement range (2θ): 15° to 90° Step width (2θ): Set to 0.01° Counting time: 1 second / step Sample stage rotation: 15 rpm The standard sample used for adjustment and calibration can be, for example, NIST (National Institute of Standards and Technology) standard aluminum oxide sintered plate SRM 1976.

[0255] If the measurement sample is a powder, it can be set by placing it on a glass sample holder, or by sprinkling the sample on a greased silicone non-reflective plate, etc. If the measurement sample is a positive electrode, the positive electrode can be attached to the substrate with double-sided tape, and the positive electrode active material layer can be set to match the measurement surface required by the device.

[0256] The characteristic X-rays may be monochromated using a filter or by using software for XRD data analysis after obtaining an XRD pattern. For example, CuKα 2 Excluding the peak due to the line, CuKα 1 It is possible to extract only the line peaks. The software can also be used to remove background noise.

[0257] In this specification, data processing when referring to the 2θ value of a certain diffraction peak will be described. First, a calculation model is fitted to the XRD pattern using crystal structure analysis software to obtain a calculated pattern. In the calculated pattern, the 2θ value at which the peak top of the diffraction peak appears is referred to as the 2θ value of the diffraction peak. The crystal structure analysis software used for fitting is not particularly limited, but for example, TOPAS ver. 3 (crystal structure analysis software manufactured by Bruker) can be used.

[0258] FIG. 11 shows CuKα 1 12 shows the XRD patterns corresponding to the O3 type crystal structure, the O3' type crystal structure, and the monoclinic O1(15) type crystal structure when using the CuKα 1 CuKα calculated from the ideal powder XRD pattern with X-rays and the trigonal O1 crystal structure with x = 0 1 13A and 13B show all of the XRD patterns described above. The range of 2θ is 18° or more and 21° or less, and the range of 2θ is 42° or more and 46° or less. 2 (O3) and CoO 2 The pattern of (O1) was created using Reflex Powder Diffraction, one of the modules of Materials Studio (BIOVIA), based on the crystal structure information obtained from the Inorganic Crystal Structure Database (ICSD) (see Non-Patent Document 5). The 2θ range was set to 15° to 75°, with a step size of 0.01 and a wavelength λ of 1.54 × 10. −10 The monochromator was single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 3. The patterns of the O3' type and monoclinic O1(15) type crystal structures were obtained by estimating the crystal structure from the XRD pattern of the positive electrode active material 100 of one embodiment of the present invention and fitting it using TOPAS ver. 3 (crystal structure analysis software manufactured by Bruker).

[0259] As shown in Figures 11, 13A and 13B, in the O3' type crystal structure, diffraction peaks appear at 2θ = 19.25 ± 0.12° (19.13° or more and less than 19.37°) and 2θ = 45.47 ± 0.10° (45.37° or more and less than 45.57°).

[0260] In addition, in the monoclinic O1(15) type crystal structure, diffraction peaks appear at 2θ=19.47±0.10° (19.37° or more and 19.57° or less) and 2θ=45.62±0.05° (45.57° or more and 45.67° or less).

[0261] However, as shown in Figures 12, 13A and 13B, in the H1-3 type crystal structure and trigonal O1, no peaks appear at these positions. x CoO 2 When x is small, peaks appear at 2θ positions of 19.13° or more and less than 19.37° and / or 19.37° or more and 19.57° or less, and 45.37° or more and less than 45.57° and / or 45.57° or more and 45.67° or less. This can be said to be a characteristic of the positive electrode active material 100 of one embodiment of the present invention.

[0262] This can also be said to be because the positions at which XRD diffraction peaks appear are close between the crystal structures of x = 1 and x ≦ 0.24. More specifically, among the main diffraction peaks of the crystal structures of x = 1 and x ≦ 0.24, the difference in 2θ between the peaks appearing at 2θ of 42° or more and 46° or less is 0.7° or less, more preferably 0.5° or less.

[0263] The positive electrode active material 100 according to one embodiment of the present invention is Li x CoO 2When x in is small, the particles have an O3'-type and / or monoclinic O1 (15)-type crystal structure, but not all of the particles have an O3'-type and / or monoclinic O1 (15)-type crystal structure. Other crystal structures may be included, or some may be amorphous. However, when Rietveld analysis is performed on the XRD pattern, the O3'-type and / or monoclinic O1 (15)-type crystal structure is preferably 50% or more, more preferably 60% or more, and even more preferably 66% or more. If the O3'-type and / or monoclinic O1 (15)-type crystal structure is 50% or more, more preferably 60% or more, and even more preferably 66% or more, the positive electrode active material can have sufficiently excellent cycle characteristics.

[0264] Furthermore, even after 100 or more charge / discharge cycles from the start of measurement, when Rietveld analysis is performed, the O3' type and / or monoclinic O1(15) type crystal structure is preferably 35% or more, more preferably 40% or more, and even more preferably 43% or more.

[0265] Similarly, when Rietveld analysis is performed, the H1-3 type and O1 type crystal structures are preferably 50% or less, more preferably 34% or less, or more preferably substantially not observed.

[0266] Furthermore, the sharpness of the diffraction peaks in the XRD pattern indicates the degree of crystallinity. Therefore, it is preferable that each diffraction peak after charging is sharp, i.e., the half-width, for example, the full width at half maximum, is narrow. The half-width varies depending on the XRD measurement conditions and the value of 2θ, even for peaks arising from the same crystalline phase. Under the above-mentioned measurement conditions, for peaks observed at 2θ = 43° or more and 46° or less, the full width at half maximum is preferably, for example, 0.2° or less, more preferably 0.15° or less, and even more preferably 0.12° or less. Note that not all peaks necessarily meet this requirement. If some peaks meet this requirement, it can be said that the crystallinity of the crystalline phase is high. Such high crystallinity contributes to the stabilization of the crystal structure after charging.

[0267] The crystallite size of the O3'-type and monoclinic O1(15) crystal structures of the positive electrode active material 100 is approximately equal to that of LiCoO in a discharged state.2 Therefore, even under the same XRD measurement conditions as the positive electrode before and after charging and discharging, the x CoO 2 When x in the formula is small, clear peaks of the O3' type and / or monoclinic O1(15) crystal structure can be confirmed. 2 In this case, even if some of the crystal structure resembles the O3' type and / or monoclinic O1(15) crystal structure, the crystallite size will be small and the peaks will be broad and small. The crystallite size can be determined from the half-width of the XRD peak.

[0268] As described above, the positive electrode active material 100 of one embodiment of the present invention preferably has a small influence of the Jahn-Teller effect. As long as the influence of the Jahn-Teller effect is small, the positive electrode active material 100 may contain a transition metal such as nickel or manganese as an additive element in addition to cobalt.

[0269] In the positive electrode active material, the range of the proportions of nickel and manganese and the lattice constants in which the influence of the Jahn-Teller effect is presumed to be small is considered using XRD analysis.

[0270] 14A to 14C show the results of calculating the a-axis and c-axis lattice constants by XRD when the positive electrode active material 100 of one embodiment of the present invention has a layered rock-salt crystal structure and contains cobalt and nickel. FIG. 14A shows the a-axis result, and FIG. 14B shows the c-axis result. Note that the XRD patterns used in these calculations are for powder after synthesis of the positive electrode active material, but before incorporation into the positive electrode. The nickel concentration on the horizontal axis represents the nickel concentration when the sum of the number of cobalt and nickel atoms is taken as 100%.

[0271] FIG. 14C shows the value obtained by dividing the a-axis lattice constant by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active materials whose lattice constant results are shown in FIGS. 14A and 14B.

[0272] 14C shows that the a-axis / c-axis tends to change significantly at nickel concentrations of 5% and 7.5%, and the a-axis distortion increases at a nickel concentration of 7.5%. This distortion may be due to the Jahn-Teller distortion of trivalent nickel. This suggests that an excellent positive electrode active material with small Jahn-Teller distortion can be obtained at nickel concentrations of less than 7.5%.

[0273] The above-mentioned range of nickel concentration does not necessarily apply to the surface layer 100a, that is, the concentration in the surface layer 100a may be higher than the above-mentioned range.

[0274] As a result of considering a preferable range of the lattice constant from the above, it was found that in the positive electrode active material of one embodiment of the present invention, the layered rock-salt crystal structure of the positive electrode active material 100 in a state where no charge and discharge are performed or in a discharged state, which can be estimated from the XRD pattern, has an a-axis lattice constant of 2.814 × 10 −10 m is greater than 2.817 x 10 −10 m and the lattice constant of the c-axis is 14.05 × 10 −10 m or larger, 14.07 x 10 −10 It has been found that the value is preferably smaller than m. The state in which no charge and discharge are performed may be, for example, the state of powder before the positive electrode of the secondary battery is produced.

[0275] Alternatively, in the layered rock-salt crystal structure of the positive electrode active material 100 in a state where no charge or discharge is performed or in a discharged state, it is preferable that the value obtained by dividing the lattice constant of the a-axis by the lattice constant of the c-axis (a-axis / c-axis) is greater than 0.20000 and smaller than 0.20049.

[0276] Alternatively, when XRD analysis is performed on the layered rock salt type crystal structure of the positive electrode active material 100 in a state where no charge or discharge is performed or in a discharged state, a first peak may be observed at 2θ of not less than 18.50° and not more than 19.30°, and a second peak may be observed at 2θ of not less than 38.00° and not more than 38.80°.

[0277] <<XPS>> In the case of inorganic oxides, when monochromatic aluminum Kα rays are used as X-rays, XPS can analyze a region from the surface to a depth of about 2 to 8 nm (usually 5 nm or less), so that the concentration of each element can be quantitatively analyzed in a region about half the depth of the surface layer 100 a. Furthermore, narrow scan analysis can be performed to analyze the bonding state of the elements.

[0278] In the cathode active material 100 according to one embodiment of the present invention, the concentration of one or more selected additive elements is preferably higher in the surface layer portion 100a than in the interior portion 100b. This is equivalent to saying that the concentration of one or more selected additive elements in the surface layer portion 100a is preferably higher than the average concentration throughout the cathode active material 100. Therefore, for example, it can be said that the concentration of one or more selected additive elements in the surface layer portion 100a measured by XPS or the like is preferably higher than the average concentration of the additive elements throughout the cathode active material 100 measured by ICP-MS, GD-MS, or the like. For example, the magnesium concentration of at least a portion of the surface layer portion 100a measured by XPS or the like is preferably higher than the average magnesium concentration throughout the cathode active material 100. Furthermore, the nickel concentration of at least a portion of the surface layer portion 100a is preferably higher than the average nickel concentration throughout the cathode active material 100. Furthermore, the aluminum concentration of at least a portion of the surface layer portion 100a is preferably higher than the average aluminum concentration throughout the cathode active material 100. It is also preferable that the fluorine concentration in at least a part of the surface layer portion 100 a is higher than the average fluorine concentration in the entire positive electrode active material 100 .

[0279] Note that the surface and surface layer portion 100a of the positive electrode active material 100 according to one embodiment of the present invention do not contain carbonates, hydroxyl groups, or the like that are chemically adsorbed after the preparation of the positive electrode active material 100. Furthermore, the surface of the positive electrode active material 100 also does not contain an electrolyte, a binder, a conductive material, or compounds derived therefrom that are attached to the surface of the positive electrode active material 100. Therefore, when quantifying the elements contained in the positive electrode active material, correction may be made to exclude carbon, hydrogen, excess oxygen, excess fluorine, and the like that can be detected by surface analysis such as XPS. For example, XPS can separate the types of bonds by analysis, and correction may be made to exclude C—F bonds derived from the binder.

[0280] Furthermore, before subjecting the sample to various analyses, the sample of the positive electrode active material and the positive electrode active material layer may be washed or the like to remove the electrolyte, binder, conductive material, or compounds derived therefrom that adhere to the surface of the positive electrode active material. At this time, lithium may dissolve in the solvent or the like used for washing, but even in this case, the added element is unlikely to dissolve, and therefore the atomic ratio of the added element is not affected.

[0281] The concentration of the added element may also be compared in terms of its ratio to cobalt. Using the ratio to cobalt is preferable because it allows comparisons to be made while reducing the influence of carbonates and other substances chemically adsorbed after the preparation of the positive electrode active material. For example, the ratio of magnesium to cobalt atoms (Mg / Co) determined by XPS analysis is preferably 0.4 to 1.5. Meanwhile, the ratio of Mg / Co determined by ICP-MS analysis is preferably 0.001 to 0.06.

[0282] Similarly, in order to ensure sufficient lithium insertion / extraction paths, the positive electrode active material 100 preferably has a higher concentration of lithium and cobalt in the surface layer portion 100a than the concentrations of the respective additive elements. This means that the concentrations of lithium and cobalt in the surface layer portion 100a are preferably higher than the concentrations of one or more additive elements selected from the additive elements contained in the surface layer portion 100a as measured by XPS or the like. For example, the concentration of cobalt in at least a portion of the surface layer portion 100a as measured by XPS or the like is preferably higher than the concentration of magnesium in at least a portion of the surface layer portion 100a as measured by XPS or the like. Similarly, the concentration of lithium is preferably higher than the concentration of magnesium. Furthermore, the concentration of cobalt is preferably higher than the concentration of nickel. Similarly, the concentration of lithium is preferably higher than the concentration of nickel. Furthermore, the concentration of cobalt is preferably higher than the concentration of aluminum. Similarly, the concentration of lithium is preferably higher than the concentration of aluminum. Furthermore, the concentration of cobalt is preferably higher than the concentration of fluorine. Similarly, the concentration of lithium is preferably higher than the concentration of fluorine.

[0283] Furthermore, it is more preferable that the additive elements such as aluminum are widely distributed in a deep region, for example, a region having a depth of 5 nm to 50 nm from the surface. Therefore, in an analysis of the entire cathode active material 100 using ICP-MS, GD-MS, or the like, the additive elements such as aluminum are detected, but the concentration may differ from the analysis result obtained by XPS, etc., which targets a region about 5 nm from the surface.

[0284] Furthermore, when XPS analysis was performed on the positive electrode active material 100 of one embodiment of the present invention, the number of magnesium atoms relative to the number of cobalt atoms was preferably 0.4 to 1.2 times, more preferably 0.65 to 1.0 times. The number of nickel atoms relative to the number of cobalt atoms was preferably 0.15 times, more preferably 0.03 to 0.13 times. The number of aluminum atoms relative to the number of cobalt atoms was preferably 0.12 times, more preferably 0.09 times. The number of fluorine atoms relative to the number of cobalt atoms was preferably 0.1 to 1.1 times, more preferably 0.3 to 0.9 times. The above ranges indicate that these additive elements are not attached to a narrow area on the surface of the positive electrode active material 100 but are widely distributed at preferred concentrations in the surface layer 100a of the positive electrode active material 100.

[0285] When performing XPS analysis, for example, monochromated aluminum Kα rays can be used as X-rays. The take-off angle is, for example, 45°, and measurement can be performed using, for example, the following equipment and conditions: Measurement equipment: Quantera II manufactured by PHI Corporation X-ray: monochromated Al Kα (1486.6 eV) Detection area: 100 μmφ Detection depth: approximately 4 to 5 nm (take-off angle 45°) Measurement spectrum: wide scan, narrow scan of each detected element

[0286] Furthermore, when the positive electrode active material 100 of one embodiment of the present invention is analyzed by XPS, the peak representing the bond energy between fluorine and another element is preferably greater than or equal to 682 eV and less than 685 eV, and more preferably about 684.3 eV, which is different from both the bond energy of lithium fluoride (685 eV) and the bond energy of magnesium fluoride (686 eV).

[0287] Furthermore, when the positive electrode active material 100 of one embodiment of the present invention is analyzed by XPS, the peak representing the bond energy between magnesium and another element is preferably greater than or equal to 1302 eV and less than 1304 eV, and more preferably about 1303 eV, which is a value different from the bond energy of magnesium fluoride, 1305 eV, and is close to the bond energy of magnesium oxide.

[0288] <EDX> Preferably, one or more selected from the additive elements contained in the positive electrode active material 100 have a concentration gradient. More preferably, the depth from the surface of the concentration peak varies depending on the additive element in the positive electrode active material 100. The concentration gradient of the additive element can be evaluated, for example, by exposing a cross section of the positive electrode active material 100 using an FIB or the like and analyzing the cross section using EDX, EPMA, or the like.

[0289] Among EDX measurements, EDX area analysis is performed by scanning an area and evaluating the area two-dimensionally. EDX area analysis is performed by linear scanning and evaluating the distribution of atomic concentrations within the positive electrode active material. Linear analysis is also used to refer to data extracted from a linear area of ​​EDX area analysis. Point analysis is used to measure an area without scanning.

[0290] EDX area analysis (e.g., element mapping) can quantitatively analyze the concentration of the added element in the surface layer 100a, the interior 100b, the grain boundary 101, and the vicinity thereof of the positive electrode active material 100. Furthermore, EDX ray analysis can analyze the concentration distribution and maximum value of the added element. Furthermore, analysis using a thinned sample, such as STEM-EDX, is more suitable because it can analyze the concentration distribution in the depth direction from the surface to the center of the positive electrode active material in a specific region without being affected by the distribution in the depth direction.

[0291] Therefore, when EDX area analysis or EDX point analysis is performed on the positive electrode active material 100 of one embodiment of the present invention, the concentration of the additive element such as magnesium in the surface layer portion 100a is preferably higher than that in the interior portion 100b.

[0292] For example, when EDX area analysis or EDX point analysis is performed on a cathode active material 100 containing magnesium as an additive element, the magnesium concentration in the surface layer 100a is preferably higher than the magnesium concentration in the interior 100b. Furthermore, when EDX analysis is performed, the magnesium concentration peak in the surface layer 100a preferably exists within a depth of 3 nm from the surface of the cathode active material 100 toward the center, more preferably within a depth of 1 nm, and even more preferably within a depth of 0.5 nm. Furthermore, the magnesium concentration preferably decays to 60% or less of the peak at a depth of 1 nm from the peak top. Furthermore, it is preferable that the magnesium concentration decays to 30% or less of the peak at a depth of 2 nm from the peak top. Note that the "peak concentration" referred to here refers to the maximum concentration value.

[0293] In addition, in the positive electrode active material 100 containing magnesium and fluorine as additive elements, the distribution of fluorine preferably overlaps with the distribution of magnesium. For example, the difference in the depth direction between the peak of the fluorine concentration and the peak of the magnesium concentration is preferably within 10 nm, more preferably within 3 nm, and even more preferably within 1 nm.

[0294] Furthermore, when EDX-ray analysis is performed, the fluorine concentration peak of the surface layer portion 100a preferably exists at a depth of 3 nm from the surface toward the center of the positive electrode active material 100, more preferably at a depth of 1 nm, and even more preferably at a depth of 0.5 nm. Furthermore, if the fluorine concentration peak exists slightly closer to the surface than the magnesium concentration peak, resistance to hydrofluoric acid is increased, which is more preferable. For example, the fluorine concentration peak is more preferably 0.5 nm or more closer to the surface than the magnesium concentration peak, and even more preferably 1.5 nm or more closer to the surface.

[0295] Furthermore, in the positive electrode active material 100 containing nickel as an additive element, the nickel concentration peak in the surface layer 100a preferably exists within a depth of 3 nm from the surface toward the center of the positive electrode active material 100, more preferably exists within a depth of 1 nm, and even more preferably exists within a depth of 0.5 nm. Furthermore, in the positive electrode active material 100 containing magnesium and nickel, the nickel distribution preferably overlaps with the magnesium distribution. For example, the difference in depth between the nickel concentration peak and the magnesium concentration peak is preferably within 10 nm, more preferably within 3 nm, and even more preferably within 1 nm.

[0296] Furthermore, when the positive electrode active material 100 contains aluminum as an additive element, it is preferable that the peak of the magnesium, nickel, or fluorine concentration is closer to the surface than the peak of the aluminum concentration in the surface layer portion 100 a when EDX-ray analysis is performed. For example, the peak of the aluminum concentration is preferably present at a depth of 0.5 nm to 50 nm, more preferably at a depth of 5 nm to 50 nm, from the surface toward the center of the positive electrode active material 100.

[0297] Furthermore, when EDX-ray analysis, area analysis, or point analysis is performed on the positive electrode active material 100, the ratio of magnesium (Mg) to the number of cobalt (Co) atoms (Mg / Co) at the peak of the magnesium concentration is less than 1, preferably 0.05 to 0.6, and more preferably 0.1 to 0.4. The ratio of aluminum (Al) to cobalt (Co) atoms (Al / Co) at the peak of the aluminum concentration is less than 1, preferably 0.05 to 0.6, and more preferably 0.1 to 0.45. The ratio of nickel (Ni) to cobalt (Co) atoms (Ni / Co) at the peak of the nickel concentration is less than 1, preferably 0 to 0.2, and more preferably 0.01 to 0.1. Alternatively, Ni / Co is preferably 0.1 to 0.5. The atomic ratio of cobalt (Co) to nickel (Ni) is preferably Co:Ni=90:10, Co:Ni=80:20, Co:Ni=70:30, or any ratio therebetween. The atomic ratio of fluorine (F) to cobalt (Co) (F / Co) at the peak of the fluorine concentration is less than 1, preferably 0 to 1.6, and more preferably 0.1 to 1.4.

[0298] The surface of the positive electrode active material 100 in the EDX analysis results can be estimated, for example, as follows: For an element that is uniformly present in the interior 100b of the positive electrode active material 100, such as oxygen or cobalt, the point where the detected amount is half that of the interior 100b is defined as the surface.

[0299] Since the positive electrode active material 100 is a composite oxide, the surface can be estimated using the detected amount of oxygen. Specifically, first, the average oxygen concentration O ave At this time, oxygen O, which is thought to be due to chemical adsorption or background, is found in the area that can be clearly determined to be outside the surface. bg If detected, O bg The average oxygen concentration O ave This average value O ave Half the value of O ave The measurement point showing the measurement value closest to / 2 can be estimated to be the surface of the positive electrode active material.

[0300] The surface can also be estimated in the same manner as above using the detected amount of cobalt. Alternatively, the sum of the detected amounts of multiple transition metals can be used to similarly estimate the surface. The detected amounts of transition metals, including cobalt, are suitable for estimating the surface because they are less susceptible to chemical adsorption.

[0301] Furthermore, when the positive electrode active material 100 is subjected to linear or area analysis, the ratio of the number of atoms of the added element A to the number of atoms of cobalt Co (A / Co) at or near the grain boundary 101 is preferably 0.020 or more and 0.50 or less. It is further preferably 0.025 or more and 0.30 or less. It is further preferably 0.030 or more and 0.20 or less. It is also preferably 0.020 or more and 0.30 or less. It is also preferably 0.020 or more and 0.20 or less. It is also preferably 0.025 or more and 0.50 or less. It is also preferably 0.025 or more and 0.20 or less. It is also preferably 0.030 or more and 0.50 or less. It is also preferably 0.030 or more and 0.30 or less.

[0302] For example, when the added element is magnesium, when linear analysis or area analysis is performed on the positive electrode active material 100, the ratio of the number of magnesium atoms to cobalt atoms (Mg / Co) at or near the grain boundary 101 is preferably 0.020 or more and 0.50 or less. It is further preferably 0.025 or more and 0.30 or less. It is further preferably 0.030 or more and 0.20 or less. It is also preferably 0.020 or more and 0.30 or less. It is also preferably 0.020 or more and 0.20 or less. It is also preferably 0.025 or more and 0.50 or less. It is also preferably 0.025 or more and 0.20 or less. It is also preferably 0.030 or more and 0.50 or less. It is also preferably 0.030 or more and 0.30 or less. Furthermore, when the above-mentioned range is achieved at multiple locations, for example, three or more locations, of the positive electrode active material 100, it can be said that this indicates that the added element is not attached to a narrow area on the surface of the positive electrode active material 100, but is widely distributed at a preferred concentration in the surface layer portion 100a of the positive electrode active material 100.

[0303] Furthermore, a coating portion may be attached to at least a portion of the surface of the positive electrode active material 100. Figures 15A and 15B show structures in which a coating portion 104 is attached to the positive electrode active material 100 shown in Figures 5A and 5C, respectively.

[0304] The coating portion 104 is preferably formed by the accumulation of decomposition products of lithium salt, organic electrolyte solution, etc., during charging and discharging, for example. x CoO 2 When repeated charging is performed such that x in the formula is 0.24 or less, it is expected that the charge-discharge cycle characteristics will be improved by having a coating portion derived from an organic electrolyte on the surface of the positive electrode active material 100. This is due to reasons such as suppressing an increase in impedance on the surface of the positive electrode active material or suppressing cobalt elution. The coating portion 104 preferably contains, for example, carbon, oxygen, and fluorine. Furthermore, when LiBOB and / or SUN (suberonitrile) are used as the electrolyte, a high-quality coating portion is easily obtained. Therefore, a coating portion 104 containing one or more elements selected from boron, nitrogen, sulfur, and fluorine may be a high-quality coating portion and is therefore preferable. Furthermore, the coating portion 104 does not have to cover the entire positive electrode active material 100. For example, it is sufficient for the coating portion 104 to cover 50% or more of the surface of the positive electrode active material 100, with 70% or more being more preferable and 90% or more being even more preferable. Fluorine may be adsorbed on the surface of the positive electrode active material 100 in areas where the coating portion 104 is not present.

[0305] <Laminated Secondary Battery> A secondary battery according to one embodiment of the present invention will be described. First, a typical laminated secondary battery will be described with reference to FIGS.

[0306] As shown in FIG. 16A , the secondary battery 1004 includes a plurality of positive electrodes 503, a plurality of negative electrodes 506, and a plurality of separators 508. The separators 508 are provided between the positive electrodes 503 and the negative electrodes 506, and are shown by dotted lines in FIG. 16A for ease of viewing. The separators 508 may include an electrolyte, specifically, a liquid electrolyte (also referred to as an electrolyte solution). Note that when a solid electrolyte or a semi-solid electrolyte is used as the electrolyte, the secondary battery 1004 does not need to include the separators 508.

[0307] The positive electrode 503 and the negative electrode 506 each have a protruding tab portion and a portion other than the tab portion. The tab portion can be electrically connected to wiring 1005a, wiring 1005b, etc. in a nail penetration test device. The positive electrode 503 has a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer is preferably formed on both sides of the positive electrode current collector. The negative electrode 506 has a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector, and the negative electrode active material layer is preferably formed on both sides of the negative electrode current collector.

[0308] As shown in FIG. 16B , multiple positive electrodes 503, multiple negative electrodes 506, and multiple separators 508 are stacked, and this may be referred to herein as a laminate. The tab portions of the multiple negative electrodes 506 are joined together with leads 512b at joints 515b and electrically connected to each other. The tab portions of the multiple positive electrodes 503 are joined together with leads 512a at joints 515a and electrically connected to each other. Compared to the positive electrode current collector and the negative electrode current collector (collectively referred to as current collectors), the positive electrode active material layer and the negative electrode active material layer (collectively referred to as active material layer) have higher insulating properties, so it is preferable not to form an active material layer on the tab portions. The leads 512a and 512b can be made of a material selected from aluminum, nickel, copper, titanium, or alloys thereof. Ultrasonic welding can be used for joining the joints. In the nail penetration test, it is not necessary to provide the leads 512a and 512b, but if provided, the wires 1005a and 1005b are electrically connected to the leads 512a and 512b, respectively.

[0309] Furthermore, the secondary battery 1004 has an exterior body (not shown), and the laminate shown in FIG. 16A is housed in the exterior body. Then, an electrolyte solution containing a dissolved lithium salt is injected into the exterior body. In other words, the electrolyte solution contains carrier ions, typically lithium ions. A secondary battery containing such lithium ions is called a lithium-ion secondary battery.

[0310] The exterior body is preferably in the form of a film from the viewpoint of weight reduction, and a secondary battery having a film-shaped exterior body is called a laminate-type secondary battery. Furthermore, from the viewpoint of excellent cooling performance, the exterior body may have a laminated structure of a polymer and a metal, which have excellent thermal conductivity. Specifically, polypropylene is preferably used as the polymer and aluminum as the metal, and nylon or the like may be further disposed on the exterior of the exterior body. A metal can case may also be used as the exterior body, and when a circular can case is used, the battery is called a coin-type secondary battery.

[0311] This embodiment can be used in combination with other embodiments.

[0312] Embodiment 2 In this embodiment, an example of a method for manufacturing a positive electrode active material 100, which is one embodiment of the present invention, will be described.

[0313] In order to prepare the positive electrode active material 100 having the distribution, composition, and / or crystalline structure of the additive elements as described in the previous embodiment, the method of adding the additive elements is important. At the same time, it is also important that the crystallinity of the inner portion 100b is good.

[0314] In the manufacturing process of the positive electrode active material 100, there is a method in which lithium cobalt oxide is synthesized, and then an additive element source is mixed and heat-treated. Alternatively, a method in which the additive element source is mixed in the same step as the cobalt source and the lithium source to synthesize lithium cobalt oxide containing the additive element may be used. Furthermore, it is preferable to not only mix the lithium cobalt oxide and the additive element source but also to heat the mixture, since this allows the additive element to dissolve in the lithium cobalt oxide. Furthermore, sufficient heating is preferable to ensure good distribution of the additive element. Therefore, the heat treatment after mixing the additive element source is important. The heat treatment after mixing the additive element source is sometimes called firing or annealing.

[0315] However, if the heating temperature is too high, cation mixing occurs, increasing the possibility that an added element, for example, magnesium, enters the cobalt site. x CoO 2When the value of x in the formula is small, the layered rock salt crystal structure of R-3m is not maintained. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as the reduction of cobalt to divalent and the evaporation of lithium.

[0316] Therefore, it is preferable to mix a material that functions as a flux together with or as the additive element source. A material that functions as a flux can be used that has a melting point lower than that of lithium cobalt oxide. For example, fluorine compounds such as lithium fluoride are suitable as fluxes. Adding a flux lowers the melting points of the additive element source and lithium cobalt oxide. Lowering the melting point facilitates good distribution of the additive element at a temperature where cation mixing is unlikely to occur.

[0317] [Initial Heating] It is more preferable to heat the lithium cobalt oxide after synthesis and before mixing with the additive element. This heating is sometimes called initial heating.

[0318] The initial heating causes lithium to be released from a part of the surface layer 100a of the lithium cobalt oxide, resulting in a more favorable distribution of the additive elements.

[0319] More specifically, it is believed that initial heating facilitates different distributions depending on the additive element through the following mechanism. First, initial heating causes lithium to be desorbed from a portion of the surface layer 100a. Next, the lithium cobalt oxide having this lithium-deficient surface layer 100a is mixed with an additive element source, such as a nickel source, an aluminum source, or a magnesium source, and the mixture is heated. Of the additive elements, magnesium is a divalent typical element, and nickel is a transition metal that is prone to becoming a divalent ion. Therefore, Mg is desorbed from a portion of the surface layer 100a. 2+ and Ni 2+ and Co reduced by lithium deficiency. 2+ However, since this phase is formed only in a part of the surface layer portion 100a, it may not be clearly observed in an electron microscope image such as an STEM or an electron beam diffraction pattern.

[0320] Among the additive elements, nickel is easily dissolved and diffuses into the interior 100b when the surface layer 100a is a layered rock-salt lithium cobaltate, but is more likely to remain in the surface layer 100a when part of the surface layer 100a is a rock-salt lithium cobaltate. Therefore, initial heating can make it easier for divalent additive elements such as nickel to remain in the surface layer 100a. The effect of this initial heating is particularly significant on the surfaces other than the (001)-oriented surface of the positive electrode active material 100 and on the surface layer 100a.

[0321] Furthermore, in these rock salt types, the bond distance between the metal Me and oxygen (Me-O distance) tends to be longer than in the layered rock salt type.

[0322] For example, rock salt type Ni 0.5 Mg 0.5 The Me-O distance in O is 2.09 × 10 −10 m, and the Me-O distance in rocksalt MgO is 2.11 × 10 −10 Even if a spinel-type phase is formed in a part of the surface layer 100a, the spinel-type NiAl 2 O 4 The Me-O distance is 2.0125 × 10 −10 m, spinel-type MgAl 2 O 4 The Me-O distance is 2.02 × 10 −10 In both cases, the Me-O distance is 2 × 10 −10 Exceeds m.

[0323] On the other hand, in the layered rock salt type, the bond distance between metals other than lithium and oxygen is shorter than the above. For example, layered rock salt type LiAlO 2 The Al-O distance in −10 m (Li-O distance is 2.11 × 10 −10 m). Also, layered rock salt LiCoO 2 The Co-O distance in −10 m (Li-O distance is 2.0916 × 10 −10 m).

[0324] According to Shannon's ionic radius, the ionic radius of hexacoordinated aluminum is 0.535 × 10 −10 The ionic radius of hexacoordinated oxygen is 1.4 × 10 −10m, and the sum of these is 1.935 × 10 −10 m.

[0325] From the above, it is considered that aluminum exists more stably in non-lithium sites in the layered rock-salt structure than in the rock-salt structure, and therefore aluminum is more likely to be distributed in the deeper region having the layered rock-salt structure and / or the interior 100b than in the region close to the surface having the rock-salt structure in the surface layer portion 100a.

[0326] Furthermore, the initial heating is expected to have the effect of increasing the crystallinity of the layered rock salt type crystal structure in the inner portion 100b.

[0327] Therefore, especially Li x CoO 2 When x is, for example, 0.15 or more and 0.17 or less, it is preferable to perform this initial heating in order to produce a positive electrode active material 100 having a monoclinic O1(15) type crystal structure.

[0328] However, initial heating is not necessarily required. In other heating steps, the atmosphere, temperature, time, etc. can be controlled to obtain Li x CoO 2 When x in the formula (I) is small, it may be possible to prepare a positive electrode active material 100 having an O3′ type and / or a monoclinic O1(15) type.

[0329] <Eutectic Point> When the melting point of a fluorine compound (sometimes called a fluoride) such as lithium fluoride is lower than the melting point of another additive element source, the fluorine compound can function as a flux (also called a fluxing agent) that lowers the melting point of the other additive element source. 2 As shown in FIG. 17 (quoted and added from FIG. 6 of Non-Patent Document 12), 2 Since the eutectic point P of the alloy is around 742°C (T1), it is preferable to set the heating temperature to 742°C or higher in the heating step after mixing the additive elements.

[0330] Here, DSC measurements of fluorine compounds and mixtures will be described with reference to Fig. 18. The mixture in Fig. 18 contains lithium cobalt oxide as the lithium oxide, LiF and MgF as the fluorine compounds. 2More specifically, the mixture is made by mixing LiCoO 2 :LiF:MgF 2 The fluorine compounds in FIG. 18 were LiF and MgF 2 Specifically, the mixture is LiF:MgF 2 The mixture was mixed so that the molar ratio was 1:3.

[0331] As shown in FIG. 18, an endothermic peak is observed around 735° C. for fluorine compounds. In addition, lithium cobalt oxide, LiF, and MgF 2 In the mixture of , an endothermic peak is observed around 830°C. Therefore, the heating temperature after mixing the additive element is preferably 742°C or higher, more preferably 830°C or higher. Furthermore, a temperature between these temperatures, 800°C (T2 in Figure 17) or higher, is preferable.

[0332] <<Method 1 for Producing Positive Electrode Active Material>> Method 1 for producing positive electrode active material 100 that undergoes initial heating will be described with reference to FIGS. 19A to 19C.

[0333] <Step S11> In step S11 shown in FIG. 19A, a lithium source (Li source) and a cobalt source (Co source) are prepared as starting materials for lithium and transition metal, respectively.

[0334] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. It is preferable that the lithium source has high purity, and it is preferable to use a material with a purity of, for example, 99.99% or higher.

[0335] As the cobalt source, it is preferable to use a compound containing cobalt, for example, cobalt oxide such as tricobalt tetroxide, cobalt hydroxide, or the like.

[0336] The cobalt source preferably has a high purity, for example, a material with a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N (99.995%) or higher, and even more preferably 5N (99.999%) or higher. By using a high-purity material, impurities in the positive electrode active material can be controlled. As a result, the capacity of the secondary battery is increased and / or the reliability of the secondary battery is improved.

[0337] In addition, the cobalt source preferably has high crystallinity, and preferably has, for example, single crystal grains. The crystallinity of the cobalt source can be evaluated using a TEM image, a STEM image, an HAADF-STEM image, an ABF-STEM image, or the like, or by XRD, electron beam diffraction, neutron beam diffraction, or the like. Note that the above-mentioned methods for evaluating crystallinity can be applied not only to the evaluation of cobalt sources but also to the evaluation of the crystallinity of other sources.

[0338] <Step S12> Next, in step S12 shown in FIG. 19A , the lithium source and the cobalt source are pulverized and mixed to prepare a mixed material. The pulverization and mixing can be performed by either a dry or wet method. The wet method is preferred because it allows for smaller pulverization. When using the wet method, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used. It is preferable to mix the lithium source and the cobalt source with dehydrated acetone with a purity of 99.5% or higher, with a water content reduced to 10 ppm or less, and then pulverize and mix them. Using dehydrated acetone with the above purity can reduce potential impurities.

[0339] A ball mill, a bead mill, or the like can be used as a means for pulverizing and mixing. When using a ball mill, it is preferable to use aluminum oxide balls or zirconium oxide balls as media. Zirconium oxide balls are preferred because they emit less impurities. Furthermore, when using a ball mill, a bead mill, or the like, the peripheral speed is preferably 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media. In this embodiment, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm).

[0340] <Step S13> Next, in step S13 shown in FIG. 19A, the mixed material is heated. Heating is preferably performed at a temperature of 800°C or higher and 1100°C or lower, more preferably 900°C or higher and 1000°C or lower, and even more preferably at approximately 950°C. If the temperature is too low, the decomposition and melting of the lithium source and cobalt source may be insufficient. On the other hand, if the temperature is too high, lithium may evaporate from the lithium source and / or cobalt may be excessively reduced, resulting in defects. For example, cobalt may change from trivalent to divalent, inducing oxygen defects.

[0341] If the heating time is too short, lithium cobalt oxide will not be synthesized, but if it is too long, productivity will decrease. For example, the heating time is preferably 1 hour or more and 100 hours or less, and more preferably 2 hours or more and 20 hours or less.

[0342] The temperature rise rate depends on the heating temperature reached, but is preferably 80° C. / h to 250° C. / h. For example, when heating at 1000° C. for 10 hours, the temperature rise rate is preferably 200° C. / h.

[0343] Heating is preferably carried out in an atmosphere with little water, such as dry air, for example, an atmosphere with a dew point of -50°C or less, more preferably an atmosphere with a dew point of -80°C or less. In this embodiment, heating is carried out in an atmosphere with a dew point of -93°C. In addition, in order to suppress impurities that may be mixed into the material, the CH 4 , CO, CO 2 , and H 2The impurity concentrations of the above are preferably 5 ppb (parts per billion) or less.

[0344] The heating atmosphere is preferably an atmosphere containing oxygen. For example, dry air may be continuously introduced into the reaction chamber. In this case, the flow rate of the dry air is preferably 10 L / min. The method of continuously introducing oxygen into the reaction chamber and allowing oxygen to flow through the reaction chamber is called "flow."

[0345] When the heating atmosphere is an atmosphere containing oxygen, it is preferable to use a method that does not allow the gas to flow. For example, a method of preventing the gas from flowing is to reduce the pressure in the reaction chamber and then fill it with oxygen (this can also be called purging) to prevent the oxygen from escaping from the reaction chamber. For example, it is preferable to reduce the pressure in the reaction chamber until a differential pressure gauge in the reaction chamber indicates -970 hPa, and then fill it with oxygen to 50 hPa.

[0346] Cooling after heating may be carried out by natural cooling, but it is preferable that the time required for cooling from the specified temperature to room temperature is within a range of 10 to 50 hours, and for example, the cooling rate (hereinafter also referred to as cooling rate) is preferably 80 to 250° C. / h, more preferably 180 to 210° C. / h. However, cooling to room temperature is not necessarily required, as long as the temperature is cooled to a temperature acceptable for the next step.

[0347] The heating in this step may be carried out using a rotary kiln or a roller hearth kiln. Heating in a rotary kiln can be carried out while stirring, whether in a continuous or batch system.

[0348] The crucible used for heating is preferably an aluminum oxide crucible. Aluminum oxide crucibles are made of a material that does not easily release impurities. In this embodiment, an aluminum oxide crucible with a purity of 99.9% is used. It is preferable to heat the crucible with a lid. This can prevent the material from volatilizing or sublimating. The lid only needs to prevent the material from volatilizing or sublimating from the time the temperature is increased to the time the temperature is decreased in this step, and the crucible does not necessarily have to be sealed with a lid. For example, as described above, by filling the reaction chamber with oxygen, this step can be performed without sealing the crucible.

[0349] In addition, it is preferable to use a used crucible rather than a new one. In this specification, a new crucible refers to one that has undergone the process of heating a material containing lithium, a transition metal M, and / or an additive element two or less times. A used crucible refers to one that has undergone the process of heating a material containing lithium, a transition metal M, and / or an additive element three or more times. This is because when a new crucible is used, there is a risk that some of the materials, including lithium fluoride, may be absorbed, diffused, migrated, and / or adhered to the sheath during heating. If some of the materials are lost as a result of this, there is a growing concern that the distribution of elements, particularly in the surface layer of the positive electrode active material, may not fall within a desirable range. On the other hand, this risk is less likely with a used crucible.

[0350] After heating, the material may be crushed and sieved as necessary. When recovering the heated material, it may be transferred from the crucible to a mortar and then recovered. It is preferable to use an aluminum oxide mortar or a zirconium oxide mortar. An aluminum oxide mortar is a material that does not easily release impurities. Specifically, an aluminum oxide mortar with a purity of 90% or more, preferably 99% or more, is used. Heating conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.

[0351] <Step S14> By the above steps, lithium cobalt oxide (LiCoO 2 When the median diameter (D50) is used as the particle size of lithium cobalt oxide, it is preferable to pulverize the lithium cobalt oxide in order to obtain a positive electrode active material 100 having a relatively small median diameter (D50).

[0352] Although the example of producing the composite oxide by the solid phase method as in steps S11 to S14 has been shown, the composite oxide may also be produced by a coprecipitation method or a hydrothermal method.

[0353] <Step S15> Next, in step S15 shown in FIG. 19A , the lithium cobalt oxide is heated. Because this is the first heating of the lithium cobalt oxide, the heating in step S15 may be referred to as initial heating. Alternatively, because this heating is performed before step S20 described below, it may be referred to as preheating or pretreatment. The crucible and / or lid used in this step are the same as those used in step S13. Although the following effects are expected from the initial heating, the initial heating is not essential for obtaining a positive electrode active material that is one embodiment of the present invention.

[0354] As described above, the initial heating causes lithium to be desorbed from a portion of the surface layer 100a of the lithium cobalt oxide. It is also expected to have the effect of improving the crystallinity of the interior 100b. Furthermore, impurities may be mixed into the lithium source and / or cobalt source prepared in step S11, etc. The initial heating can reduce the amount of impurities in the lithium cobalt oxide completed in step S14.

[0355] Furthermore, initial heating has the effect of smoothing the surface of the lithium cobalt oxide. A smooth surface of a composite oxide means that there are few irregularities, the composite oxide is rounded overall, and the corners are rounded. Furthermore, a smooth surface means that there is little foreign matter adhering to the surface. Foreign matter is thought to be a cause of irregularities, so it is preferable that it does not adhere to the surface.

[0356] For this initial heating, it is not necessary to prepare a lithium source, a source of an additional element, or a material that functions as a flux.

[0357] If the heating time in this step is too short, sufficient effects will not be obtained, but if it is too long, productivity will decrease. For example, the heating conditions can be selected from those described in step S13. In addition to the heating conditions, the heating temperature in this step is preferably lower than the temperature in step S13 in order to maintain the crystalline structure of the complex oxide. Furthermore, the heating time in this step is preferably shorter than the time in step S13 in order to maintain the crystalline structure of the complex oxide. For example, it is preferable to perform heating at a temperature of 700°C or higher and 1000°C or lower for 2 hours or higher and 20 hours or lower.

[0358] The effect of increasing the crystallinity of the inner portion 100b is, for example, the effect of alleviating distortion, displacement, etc. resulting from the difference in shrinkage of the lithium cobalt oxide produced in step S13.

[0359] The heating in step S13 may cause a temperature difference between the surface and the interior of the lithium cobalt oxide. This temperature difference may induce a shrinkage difference. It is also believed that the temperature difference causes a difference in fluidity between the surface and the interior, resulting in a shrinkage difference. The energy associated with the shrinkage difference causes an internal stress difference in the lithium cobalt oxide. This internal stress difference is also called strain, and this energy is sometimes called strain energy. It is believed that the internal stress is removed by the initial heating in step S15; in other words, the strain energy is homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain in the lithium cobalt oxide is alleviated. This may result in a smoother surface for the lithium cobalt oxide. This is also referred to as an improved surface. In other words, it is believed that the shrinkage difference in the lithium cobalt oxide is alleviated and the surface of the composite oxide is smoother after step S15.

[0360] Furthermore, the difference in shrinkage may cause microscopic deviations, such as crystal deviations, in the lithium cobalt oxide. It is preferable to carry out this step in order to reduce such deviations. This step makes it possible to equalize the deviations in the composite oxide. Equalizing the deviations may result in a smoother surface of the composite oxide. This is also referred to as the alignment of crystal grains. In other words, it is believed that step S15 alleviates the deviations of crystals and other particles in the composite oxide, resulting in a smoother surface of the composite oxide.

[0361] When lithium cobalt oxide with a smooth surface is used as the positive electrode active material, deterioration during charge and discharge in a secondary battery is reduced and cracking of the positive electrode active material can be prevented.

[0362] Note that pre-synthesized lithium cobalt oxide may be used in step S14. In this case, steps S11 to S13 can be omitted. By performing step S15 on pre-synthesized lithium cobalt oxide, lithium cobalt oxide with a smooth surface can be obtained.

[0363] <Step S20> Next, as shown in step S20, it is preferable to add the additional element A to the lithium cobalt oxide that has undergone the initial heating. When the additional element A is added to the lithium cobalt oxide that has undergone the initial heating, the additional element A can be added evenly. Therefore, it is preferable to add the additional element A after the initial heating. The step of adding the additional element A will be described with reference to FIGS. 19B and 19C.

[0364] 19B and 19C, the steps of preparing the additional element A source (A source) will be described. A lithium source may be prepared together with the additional element A source.

[0365] The additive element A can be one or more selected from the additive elements described in the previous embodiments, such as magnesium, fluorine, nickel, aluminum, titanium, zirconium, vanadium, iron, manganese, chromium, niobium, arsenic, zinc, silicon, sulfur, phosphorus, and boron. Also, one or two selected from bromine and beryllium can be used.

[0366] <Step S21> Step S21 shown in Fig. 19B will be described. When magnesium is selected as the additive element, the source of the additive element can be called a magnesium source (Mg source). As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, or the like can be used. Furthermore, a plurality of the above-mentioned magnesium sources may be used.

[0367] When fluorine is selected as the additive element, the source of the additive element can be called a fluorine source (F source). Examples of the fluorine source include lithium fluoride (LiF), magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 3 , CeF 4 ), lanthanum fluoride (LaF 3 ), or sodium aluminum hexafluoride (Na 3 AlF 6 Among these, lithium fluoride is preferred because it has a relatively low melting point of 848° C. and is easily melted in the heating step described below.

[0368] Magnesium fluoride can be used as both a fluorine source and a magnesium source, and lithium fluoride can be used as both a fluorine source and a lithium source. Another lithium source that can be used in step S21 is lithium carbonate.

[0369] The fluorine source is preferably a gas, such as fluorine (F 2 ), fluorocarbon, sulfur fluoride, or oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 5 F 2 , O 6 F 2 , O 2 F) or the like may be used and mixed into the atmosphere in the heating step described below. Also, a plurality of the above-mentioned fluorine sources may be used.

[0370] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and the magnesium source. 2Lithium fluoride and magnesium fluoride are prepared as LiF:MgF 2 The effect of lowering the melting point is greatest when the molar ratio of lithium fluoride and magnesium fluoride is about 65:35. On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, the molar ratio of lithium fluoride and magnesium fluoride is set to LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = 0.33 or its vicinity) is more preferable. Here, "or its vicinity" refers to a value that is greater than 0.9 times and less than 1.1 times the value.

[0371] 19B, the magnesium source and the fluorine source are pulverized and mixed. This step can be performed under pulverization and mixing conditions selected from those described in step S12.

[0372] 19B, the pulverized and mixed materials are collected to obtain a source of the additional element A (A source). The source of the additional element A shown in step S23 includes a plurality of starting materials and can be called a mixture.

[0373] The particle size of the mixture is preferably such that the median diameter (D50) is 600 nm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less. Even when a single material is used as the additive element source, the median diameter (D50) is preferably 600 nm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less.

[0374] Such a finely powdered mixture (including the case where only one type of additive element is included) can be easily adhered to the surfaces of the lithium cobalt oxide particles when mixed with the lithium cobalt oxide in a later step. If the mixture is evenly adhered to the surfaces of the lithium cobalt oxide particles, it is preferable because the additive element can be easily distributed or diffused uniformly in the surface layer portion 100a of the composite oxide after heating.

[0375] <Step S21> A step different from that shown in Fig. 19B will be described with reference to Fig. 19C. In step S21 shown in Fig. 19C, four types of additive element sources to be added to lithium cobalt oxide are prepared. That is, Fig. 19C differs from Fig. 19B in the types of additive element sources. A lithium source may be prepared together with the additive element sources.

[0376] As sources of four additive elements, a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source) are prepared. The magnesium source and the fluorine source can be selected from the compounds described in FIG. 19B . Nickel oxide, nickel hydroxide, etc. can be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. can be used as the aluminum source.

[0377] <Steps S22 and S23> Steps S22 and S23 shown in FIG. 19C are similar to the steps described with reference to FIG. 19B.

[0378] 19A , lithium cobalt oxide and a source of additional element A (A source) are mixed together. The ratio of the number of cobalt atoms Co in the lithium cobalt oxide to the number of magnesium atoms Mg in the source of additional element A is preferably Co:Mg=100:y (0.1≦y≦6), and more preferably Co:Mg=100:y (0.3≦y≦3).

[0379] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the shape of the lithium cobalt oxide particles. For example, the mixing conditions are preferably lower in rotation speed or shorter in time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconium oxide balls as the media.

[0380] In this embodiment, dry mixing is performed in a ball mill using zirconium oxide balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.

[0381] <Step S32> Next, in step S32 of Fig. 19A, the mixed materials are collected to obtain a mixture 903. When collecting the materials, they may be crushed and then sieved, if necessary.

[0382] 19A to 19C illustrate a fabrication method in which an additive element is added after initial heating, but the present invention is not limited to the above method. The additive element may be added at a different timing, or may be added multiple times. The timing may be changed depending on the additive element.

[0383] For example, as shown in Figures 20A to 20C, the additive elements may be added to the lithium source and the cobalt source in step S11, i.e., at the stage of the starting material for the composite oxide. Figure 20A shows a flow for adding a magnesium source to a lithium source and a cobalt source. Figure 20B shows a flow for adding a magnesium source and an aluminum source to a lithium source and a cobalt source. Figure 20C shows a flow for adding a magnesium source and a nickel source to a lithium source and a cobalt source. The additive element sources shown in Figures 20A to 20C are examples.

[0384] Subsequently, the process proceeds to step S12, then step S13, and finally step S14, where lithium cobalt oxide containing the additive element can be obtained. The distribution of the additive element can also be controlled depending on the timing of adding the additive element. The additive element added as shown in FIGS. 20A to 20C is expected to be located inside the positive electrode active material 100. Furthermore, in the case of the flow shown in FIGS. 20A to 20C, the above-described steps S11 to S14 and steps S21 to S23 do not need to be separated, making this a simple and highly productive method. Of course, even in the flow shown in FIGS. 20A to 20C, a new additive element may be added in step S20.

[0385] Alternatively, lithium cobalt oxide containing some of the additive elements may be used. For example, if lithium cobalt oxide containing magnesium and fluorine is used, steps S11 to S14 and some of step S20 can be omitted. This method is simple and has high productivity.

[0386] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be heated in step S15, and then a magnesium source and a fluorine source, or a magnesium source, a fluorine source, a nickel source, and an aluminum source may be added as in step S20.

[0387] <Step S33> Next, in step S33 shown in Fig. 19A, the mixture 903 is heated. The heating can be performed under heating conditions selected from those described in step S13. The heating time is preferably 2 hours or more. At this time, the pressure inside the furnace may exceed atmospheric pressure in order to increase the oxygen partial pressure in the heating atmosphere. This is because if the oxygen partial pressure in the heating atmosphere is insufficient, cobalt and the like may be reduced, and the layered rock salt crystal structure of lithium cobalt oxide and the like may no longer be maintained.

[0388] Here, a supplementary note about the heating temperature will be provided. The lower limit of the heating temperature in step S33 must be equal to or higher than the temperature at which the reaction between the lithium cobalt oxide and the additive element source proceeds. The temperature at which the reaction proceeds is preferably a temperature at which interdiffusion between the lithium cobalt oxide and the elements contained in the additive element source occurs, and may be lower than the melting temperature of these materials. An oxide will be used as an example for explanation, but the melting temperature T m 0.757 times (Tammann temperature T d ) solid-phase diffusion occurs. Therefore, the heating temperature in step S33 is preferably 650° C. or higher.

[0389] Of course, the reaction is more likely to proceed if the temperature is equal to or higher than the melting point of one or more of the materials contained in the mixture 903. For example, LiF and MgF are used as the additive element source. 2 When LiF and MgF 2 Since the eutectic point of the molten metal is around 742° C. (see eutectic point P in FIG. 17), the lower limit of the heating temperature in step S33 is preferably set to 742° C. or higher.

[0390] Also, LiCoO 2 :LiF:MgF 2 In the mixture 903 obtained by mixing so that the molar ratio was 100:0.33:1, an endothermic peak was observed around 830° C. in DSC measurement. Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.

[0391] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.

[0392] The upper limit of the heating temperature is set to be lower than the decomposition temperature of lithium cobalt oxide (melting point 1130°C). At temperatures close to the decomposition temperature, there is a concern that lithium cobalt oxide may decompose, albeit only slightly. Therefore, the upper limit of the heating temperature is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 900°C or lower.

[0393] In consideration of these, the heating temperature in step S33 is preferably 650°C or higher and 1130°C or lower, more preferably 650°C or higher and 1000°C or lower, even more preferably 650°C or higher and 950°C or lower, and even more preferably 650°C or higher and 900°C or lower. Also, it is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, it is preferably 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower. The heating temperature in step S33 is preferably lower than the heating temperature in step S13.

[0394] An example of the heating furnace used in step S33 will now be described with reference to FIG.

[0395] The heating furnace 220 shown in FIG. 23 includes a furnace space 202, a hot plate 204, a pressure gauge 221, a heater unit 206, and an insulating material 208. It is preferable to heat a container 216, which corresponds to a crucible or scabbard, with a lid 218 attached. This configuration allows the space 219 defined by the container 216 and lid 218 to be filled with a fluoride-containing atmosphere. By maintaining the lid during heating so that the concentration of gasified fluoride in the space 219 remains constant or does not decrease, fluorine and magnesium can be contained near the particle surfaces of the mixture 903. Because the space 219 has a smaller volume than the furnace space 202, a small amount of fluoride volatilizes, creating a fluoride-containing atmosphere. In other words, the reaction system can be filled with a fluoride-containing atmosphere without significantly reducing the amount of fluoride contained in the mixture 903. Furthermore, using the lid 218 allows the mixture 903 to be heated in a fluoride-containing atmosphere simply and inexpensively.

[0396] Furthermore, before heating in the heating furnace space 202, a step of creating an oxygen-containing atmosphere in the heating furnace space 202 and a step of placing the container 216 containing the mixture 903 in the heating furnace space 202 are performed. By performing these steps in this order, the mixture 903 can be heated in an atmosphere containing oxygen and fluoride. For example, heating can be performed while a gas is flowing (flow). The gas can be introduced from the bottom of the heating furnace space 202 and exhausted to the top. Furthermore, the heating furnace space 202 can be sealed during heating to create a closed space to prevent the gas from being transported to the outside (purging).

[0397] There are no particular limitations on the method for creating an oxygen-containing atmosphere in the heating furnace space 202, but examples include a method of evacuating the heating furnace space 202 and then introducing an oxygen-containing gas such as oxygen gas or dry air, or a method of infusing an oxygen-containing gas such as oxygen gas or dry air for a certain period of time. Among these, it is preferable to evacuate the heating furnace space 202 and then introduce oxygen gas (oxygen substitution). Note that the air in the heating furnace space 202 may be considered to be an oxygen-containing atmosphere.

[0398] Furthermore, fluoride and the like adhering to the inner walls of the container 216 and the lid 218 can be re-flying by heating and can be attached to the mixture 903 .

[0399] There is no particular limitation on the process for heating the heating furnace 220. It is preferable to heat the heating furnace 220 using a heating mechanism provided in the heating furnace 220.

[0400] Furthermore, there are no particular restrictions on how the mixture 903 is arranged when placed in the container 216, but it is preferable to arrange the mixture 903 so that the upper surface of the mixture 903 is flat with respect to the bottom surface of the container 216, in other words, so that the height of the upper surface of the mixture 903 is uniform, as shown in Figure 23.

[0401] The heating in step S33 is preferably performed while controlling the pressure inside the furnace with the pressure gauge 221. The inside of the furnace is preferably kept at atmospheric pressure or pressurized. For example, when exposed to a pressurized state, it is thought that the surface of the lithium cobalt oxide melts. Therefore, LiF and MgF 2 The surface of the lithium cobalt oxide heated together can be melted by applying pressure.

[0402] The cooling after heating in step S33 can be performed by natural cooling, but it is preferable that the time required for the temperature to drop from the specified temperature to room temperature is between 10 and 50 hours. For example, the cooling rate is preferably between 80°C / h and 250°C / h, and more preferably between 180°C / h and 210°C / h. The cooling rate in step S33 is preferably faster than that in step S13. A fast cooling rate is called rapid cooling. Rapid cooling after the melting allows for the appropriate production of a shell. Specifically, it makes it possible to produce a narrow shell. The temperature at the end of the temperature drop does not necessarily have to be room temperature; it is sufficient to cool to a temperature acceptable for the next step.

[0403] Furthermore, when heating the mixture 903, it is preferable to control the partial pressure of fluorine or a fluorine compound resulting from the fluorine source or the like within an appropriate range. The partial pressure can also be controlled by heating the crucible used in this step with a lid. As mentioned above, the lid can prevent the volatilization or sublimation of the material. In other words, it is not necessary to seal the crucible with a lid, as long as it can prevent the volatilization or sublimation of the material from the temperature increase to the temperature decrease in this step. For example, by filling the reaction chamber in which the crucible is placed with oxygen, it is possible to perform this step without sealing the crucible. A positive electrode active material containing an appropriate amount of fluorine or a fluorine compound is preferable because it can suppress heat generation and smoke generation even in the event of an internal short circuit.

[0404] In the manufacturing method described in this embodiment, some materials, for example, LiF as a fluorine source, may function as a flux, which allows the heating temperature to be lowered below the decomposition temperature of lithium cobalt oxide, for example, to 742° C. or higher and 950° C. or lower, and allows additive elements such as magnesium to be distributed in the surface layer, thereby enabling the manufacture of a positive electrode active material with excellent characteristics.

[0405] However, since LiF has a lower specific gravity in a gaseous state than oxygen, there is a possibility that LiF may volatilize or sublime when heated, and if it volatilizes, the amount of LiF in the mixture 903 will decrease. This will weaken its function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiCoO 2 There is a possibility that Li on the surface reacts with F in the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluorine compound with a higher melting point than LiF is used, it is still necessary to suppress volatilization.

[0406] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903. In order to suppress the volatilization of LiF, it is preferable to place a lid on the crucible.

[0407] The heating in this step is preferably performed so as not to cause the particles of the mixture 903 to stick together. If the particles of the mixture 903 stick together during heating, the contact area with oxygen in the atmosphere will decrease and the route along which the added element (e.g., fluorine) diffuses will be blocked, which may result in poor distribution of the added element (e.g., magnesium and fluorine) in the surface layer. In order to promote the reaction with oxygen in the atmosphere, the crucible does not need to be sealed with a lid.

[0408] Furthermore, it is believed that uniform distribution of the additive element (e.g., fluorine) in the surface layer portion results in a smooth cathode active material with few irregularities. Therefore, in order to maintain the smooth state of the surface after the heating in step S15 or to make it even smoother, it is preferable that the particles of mixture 903 do not stick to each other.

[0409] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln during heating. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln. Flowing oxygen may cause the fluorine source to evaporate, which is undesirable in terms of maintaining surface smoothness.

[0410] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by placing a lid on a container containing the mixture 903, for example, in the same way as a lid placed on a crucible.

[0411] Regarding the heating time, the heating time varies depending on conditions such as the heating temperature, the size and composition of the lithium cobalt oxide obtained in step S14, etc. When the lithium cobalt oxide is small, a lower temperature or a shorter heating time may be more preferable than when the lithium cobalt oxide is large.

[0412] When the median diameter (D50) of the lithium cobalt oxide obtained in step S14 of Fig. 19A is about 12 µm, the heating temperature is preferably, for example, 650°C or more and 950°C or less. The heating time is preferably, for example, 3 hours or more and 60 hours or less, more preferably 10 hours or more and 30 hours or less, and even more preferably about 20 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or more and 50 hours or less.

[0413] On the other hand, when the median diameter (D50) of the lithium cobalt oxide obtained in step S14 is about 5 μm, the heating temperature is preferably, for example, 650° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 5 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.

[0414] <Step S34> Next, in step S34 shown in Fig. 19A, the heated material is recovered to obtain the positive electrode active material 100. The recovered particles may be further sieved. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced. The positive electrode active material of one embodiment of the present invention has a smooth surface.

[0415] 21 to 22C , a method for producing a positive electrode active material, which is one embodiment of the present invention and differs from the method for producing a positive electrode active material, will be described. The method for producing a positive electrode active material, which differs from the method for producing a positive electrode active material, is mainly the number of times that an additive element is added and the mixing method. For other details, the description of the method for producing a positive electrode active material, which differs from the method for producing a positive electrode active material, can be referred to.

[0416] In FIG. 21, steps S11 to S15 are carried out in the same manner as in FIG. 19A to prepare lithium cobalt oxide that has undergone initial heating.

[0417] <Step S20a> Next, in step S20a, an additive element A1 source is prepared to be used for adding the additive element A1 to the lithium cobalt oxide that has undergone the initial heating. The process of preparing the additive element A1 source will be described with reference to FIG. 22A.

[0418] <Step S21> Step S21 shown in Fig. 22A will be described. The additional element A1 can be selected from the elements exemplified as the additional element A described in step S21 shown in Fig. 19B and used. For example, one or more elements selected from magnesium, fluorine, and calcium can be suitably used as the additional element A1. Fig. 22A shows an example in which magnesium and fluorine are selected as the additional element A1, and a magnesium source (Mg source) and a fluorine source (F source) are prepared in step S21.

[0419] Steps S21 to S23 shown in Fig. 22A can be performed under the same conditions as steps S21 to S23 shown in Fig. 19B. As a result, an additional element A1 source (A1 source) can be obtained in step S23.

[0420] Furthermore, steps S31 to S33 shown in FIG. 21 can be performed in the same manner as steps S31 to S33 shown in FIG. 19A.

[0421] <Step S34a> Next, the material heated in step S33 is recovered to produce lithium cobalt oxide containing the additional element A1. To distinguish it from the composite oxide in step S14, this is also called a second composite oxide.

[0422] <Step S40> In step S40 shown in Fig. 21, an additive element A2 source used to add the additive element A2 to the second composite oxide is prepared. The steps of preparing the additive element A2 source will be described with reference to Fig. 22B and Fig. 22C.

[0423] <Step S41> Step S41 shown in Fig. 22B will be described. The additional element A2 can be selected from the elements exemplified as the additional element A described in step S21 shown in Fig. 19C. For example, one or more elements selected from nickel, titanium, boron, zirconium, and aluminum can be suitably used as the additional element A2. Fig. 22B shows an example in which a nickel source (Ni source) and an aluminum source (Al source) are prepared in the case where nickel and aluminum are selected as the additional element A2.

[0424] Steps S41 to S43 shown in Fig. 22B can be performed under the same conditions as steps S21 to S23 shown in Fig. 19B. As a result, an additional element A2 source (A2 source) can be obtained in step S43.

[0425] 22C shows a modified example of the step of preparing the additive element A2 source described with reference to FIG. 22B. In step S41 shown in FIG. 22C, a nickel source (Ni source) and an aluminum source (Al source) are prepared, and in step S42a, they are independently pulverized. As a result, in step S43, a plurality of additive element A2 sources (A2 sources) are prepared. The steps in FIG. 22C differ from those in FIG. 22B in that the additive elements are independently pulverized in step S42a.

[0426] <Steps S51 to S54> Next, steps S51 to S54 shown in FIG. 21 can be performed under the same conditions as steps S31 to S34 shown in FIG. 19A , and a mixture 904 is obtained in step S52. Furthermore, the conditions for step S53, which is a heating step, can be a lower temperature and a shorter time than those for step S33. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced in step S54. The positive electrode active material of one embodiment of the present invention has a smooth surface.

[0427] 21 to 22C , in fabrication method 2, an additional element is introduced into lithium cobalt oxide separately as additional element A1 and additional element A2. By introducing the additional elements separately, the positions of the additional elements in the depth direction can be changed. For example, it is possible to position additional element A1 so that its concentration is higher in the surface layer portion than in the interior, and to position additional element A2 so that its concentration is higher in the interior than in the surface layer portion.

[0428] After the initial heating described in this embodiment, a positive electrode active material with a smooth surface can be obtained.

[0429] The initial heating shown in this embodiment is performed on lithium cobalt oxide. Therefore, the initial heating is preferably performed at a temperature lower than that required for obtaining lithium cobalt oxide and for a shorter heating time than that required for obtaining lithium cobalt oxide. The step of adding an additive element to lithium cobalt oxide is preferably performed after the initial heating. This addition step can be performed in two or more steps. Following this order of steps is preferable because it maintains the surface smoothness obtained by the initial heating.

[0430] Positive electrode active material 100 with a smooth surface may be more resistant to physical destruction due to pressure, etc. than positive electrode active material that does not have a smooth surface. For example, positive electrode active material 100 is less likely to be destroyed in a test involving pressure, such as a nail penetration test, and as a result, safety may be improved.

[0431] This embodiment can be used in combination with other embodiments.

[0432] Embodiment 3 In this embodiment, a positive electrode, a negative electrode, and the like of a secondary battery of one embodiment of the present invention will be described.

[0433] 24A shows an example of a cross-sectional view of a positive electrode 503 used in a secondary battery 1004 or the like. The positive electrode 503 has a positive electrode active material layer 502 on a positive electrode current collector 501. The positive electrode active material layer 502 includes a positive electrode active material 100, a positive electrode active material 562, a conductive material 553, a conductive material 554, and an electrolyte solution 530. The positive electrode active material layer 502 also has a binder (not shown). The secondary battery preferably has a configuration including either the conductive material 553 or the conductive material 554.

[0434] The median diameter (D50) of the positive electrode active material 100 is 1 μm or more and 50 μm or less, preferably 5 μm or more and 30 μm or less. To increase the packing density, it is preferable to add a positive electrode active material 562 having a different median diameter (D50). The median diameter (D50) of the positive electrode active material 562 is preferably 1 / 10 to 1 / 6 of the median diameter (D50) of the positive electrode active material 100. When particle size distribution measurement is performed on an active material containing a mixture of the positive electrode active material 100 and the positive electrode active material 562, two peaks with different maximum values ​​are observed. Of course, two or more peaks may be observed. It is possible to increase the packing density without the positive electrode active material 562.

[0435] It is preferable that both the positive electrode active material 100 and the positive electrode active material 562 have a shell. A positive electrode active material with a shell can improve insulation and is less likely to experience thermal runaway. In FIG. 24A , the boundary between the surface layer and the interior is indicated by a dotted line, but the boundary is not necessarily as clear as in FIG. 24A . The shell may have the configuration shown in FIG. 5B or the like. The positive electrode active material is not limited to that shown in FIG. 24A ; for example, either the positive electrode active material 100 or the positive electrode active material 562 may have a shell.

[0436] Positive electrode active material 100 may have the same composition as positive electrode active material 562 or a different composition. The same composition includes positive electrode active materials having the same main composition but differing in the presence or absence of additive elements, etc. The different composition includes positive electrode active materials having different main compositions.

[0437] Again, it is preferable that the positive electrode active material 100 and the positive electrode active material 562 contain an additive element, and it is particularly preferable that the shell contain an additive element. The additive element may be unevenly distributed in the shell or may be sparsely distributed inside. "Uneven distribution" refers to the additive element being present unevenly or unevenly distributed. Therefore, a state in which the concentration of the additive element is higher toward the shell than the inside is sometimes referred to as the additive element being unevenly distributed in the shell.

[0438] The additive element may be present in the surface layer portion. The concentration of the additive element in the surface layer portion may be different from the concentration of the additive element in the interior, and it is preferable that the concentration of the additive element in the surface layer portion is higher than the concentration in the interior. This is sometimes referred to as the additive element being unevenly distributed in the surface layer portion.

[0439] Although the positive electrode active material 100 and the positive electrode active material 562 are sometimes referred to as positive electrode active material particles, the shape of the positive electrode active material can take a variety of forms other than particulate. Unlike FIG. 24A , FIG. 24B shows a positive electrode 503 having a positive electrode active material in a form other than particulate. Since FIG. 24B is the same as FIG. 24A except for the shape of the positive electrode active material, a description thereof will be omitted. Although the positive electrode active material 100 and the positive electrode active material 562 shown in FIGS. 24A and 24B are shown as primary particles, they may also be secondary particles.

[0440] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and may include a conductive material (synonymous with a conductive additive) and a binder. The positive electrode active material may be a positive electrode active material prepared using the preparation method described in the above embodiment. For example, a positive electrode active material having a relatively small median diameter (D50) and a positive electrode active material having a relatively large median diameter (D50) may be mixed and used.

[0441] The positive electrode active material described in the above embodiment may be mixed with another positive electrode active material.

[0442] Other positive electrode active materials include, for example, composite oxides having an olivine-type crystal structure, a layered rock salt-type crystal structure, or a spinel-type crystal structure. For example, LiFePO 4 , LiFeO 2 , LiNiO 2 , LiMn 2 O 4 , V 2 O 5 , Cr 2 O 5 , MnO 2 and the like compounds.

[0443] Other positive electrode active materials include LiMn 2 O 4and lithium-containing materials having a spinel-type crystal structure containing manganese, such as lithium nickel oxide (LiNiO 2 or LiNi 1−x M x O 2 It is preferable to use a mixture of (0<x<1) (M=Co, Al, etc.) This configuration can improve the characteristics of the secondary battery.

[0444] In addition, as another positive electrode active material, the composition formula Li a Mn b M c O d A lithium-manganese composite oxide that can be expressed by the formula (1) can be used. Here, element M is preferably a metal element selected from among lithium and manganese, or silicon or phosphorus, and more preferably nickel. Furthermore, when measuring the entire lithium-manganese composite oxide particle, it is preferable that 0<a / (b+c)<2, c>0, and 0.26≦(b+c) / d<0.5 are satisfied during discharge. The composition of metals, silicon, phosphorus, etc. in the entire lithium-manganese composite oxide particle can be measured using, for example, ICP-MS. The oxygen composition in the entire lithium-manganese composite oxide particle can be measured using, for example, EDX. Furthermore, the composition can be determined by using valence evaluation of fusion gas analysis and XAFS (X-ray absorption fine structure) analysis in combination with ICP-MS analysis. The lithium manganese composite oxide refers to an oxide containing at least lithium and manganese, and may contain one or more elements selected from the group consisting of chromium, cobalt, aluminum, nickel, iron, magnesium, molybdenum, zinc, indium, gallium, copper, titanium, niobium, silicon, phosphorus, and the like.

[0445] [Conductive Material] The conductive material functions to assist the current path between the active material and the current collector, or the current path between multiple active materials. To fulfill such a function, the conductive material preferably has a material with lower resistance than the active material. Due to its role, the conductive material is also called a conductive assistant or a conductivity imparting agent.

[0446] The conductive material is typically a carbon material or a metal material. The conductive material is particulate, and examples of such particulate conductive materials include carbon black (furnace black, acetylene black, graphite, etc.). Many carbon blacks have a particle size smaller than that of the positive electrode active material. The conductive material can be fibrous, and examples of such fibrous conductive additives include carbon nanotubes (CNT) and VGCF (registered trademark). The conductive material can be sheet-shaped, and an example of a sheet-shaped conductive additive is multilayer graphene. Sheet-shaped conductive additives may appear thread-like in the cross section of the positive electrode.

[0447] Particulate conductive materials can penetrate into gaps in the positive electrode active material and are prone to aggregation. Therefore, particulate conductive materials can assist in the conductive paths between adjacent positive electrode active materials. Fibrous conductive materials have bent regions, but are larger than the positive electrode active material. Therefore, fibrous conductive materials can assist in the conductive paths between distant positive electrode active materials in addition to adjacent positive electrode active materials. Thus, it is preferable to mix two or more shapes of conductive additives.

[0448] When multilayer graphene is used as the sheet-like conductive material and carbon black is used as the particulate conductive material, the weight of the carbon black in a mixed slurry state is preferably 1.5 to 20 times, and more preferably 2 to 9.5 times, the weight of the multilayer graphene.

[0449] When the mixing ratio of multilayer graphene to carbon black is within the above range, the carbon black does not aggregate and is easily dispersed. Furthermore, when the mixing ratio of multilayer graphene to carbon black is within the above range, the electrode density can be made higher than when only carbon black is used as the conductive additive. By increasing the electrode density, the capacity per unit weight can be increased.

[0450] Furthermore, by setting the mixing ratio of multilayer graphene and carbon black within the above range, rapid charging can be achieved.

[0451] In this specification, graphene includes multilayer graphene and multigraphene. In other words, graphene refers to a substance that contains carbon, has a shape such as a plate or sheet, and has a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings is sometimes called a carbon sheet. Graphene compounds include graphene oxide, multilayer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, and the like. In other words, graphene compounds may have functional groups. Graphene or graphene compounds preferably have a curved shape. Graphene or graphene compounds may be rolled, and rolled graphene is sometimes called a carbon nanofiber.

[0452] In this specification and the like, graphene oxide refers to a material that contains carbon and oxygen, has a sheet shape, and has a functional group, in particular, an epoxy group, a carboxy group, or a hydroxy group.

[0453] In this specification, reduced graphene oxide refers to a material containing carbon and oxygen, having a sheet-like shape, and having a two-dimensional structure formed by six-membered carbon rings. A single sheet of reduced graphene oxide can function, but multiple sheets may be stacked. Reduced graphene oxide preferably has a portion where the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % or more and 15 atomic % or less. By achieving these carbon and oxygen concentrations, reduced graphene oxide can function as a highly conductive material even in small amounts. Furthermore, reduced graphene oxide preferably has an intensity ratio G / D of the G band to the D band in a Raman spectrum of 1 or more. Reduced graphene oxide with such an intensity ratio can function as a highly conductive material even in small amounts.

[0454] Fluorine-containing graphene may be used as the graphene compound. The fluorine in the graphene compound is preferably adsorbed on the surface. Fluorine-containing graphene can be produced by contacting graphene with a fluorine compound (called a fluorination treatment). The fluorination treatment involves the use of fluorine (F2 ) or a fluorine compound. As the fluorine compound, hydrogen fluoride, halogen fluoride (ClF 3 , IF 5 etc.), gaseous fluorides (BF 3 , N.F. 3 , P.F. 5 , SiF 4 , SF 6 etc.), metal fluorides (LiF, NiF 2 , AlF 3 , MgF 2 For the fluorination treatment, it is preferable to use a gaseous fluoride, and the gaseous fluoride may be diluted with an inert gas. The temperature for the fluorination treatment is preferably room temperature, but is preferably 0°C or higher and 250°C or lower, which includes room temperature. When the fluorination treatment is performed at 0°C or higher, fluorine can be adsorbed on the surface of graphene.

[0455] Graphene compounds may have excellent electrical properties, such as high electrical conductivity, and excellent physical properties, such as high flexibility and high mechanical strength. Graphene compounds may also have a sheet-like shape. Graphene compounds may have curved surfaces, enabling surface contact with low contact resistance. Even when thin, graphene compounds may have very high electrical conductivity, allowing a small amount of graphene to efficiently form a conductive path within an active material layer. Therefore, using a graphene compound as a conductive material can increase the contact area between the active material and the conductive material. The graphene compound preferably covers 80% or more of the active material. It is preferable that the graphene compound wraps around at least a portion of the active material. It is also preferable that the graphene compound overlaps at least a portion of the active material. It is also preferable that the shape of the graphene compound matches at least a portion of the shape of the active material. The shape of the active material refers to, for example, the unevenness of a single active material or the unevenness formed by multiple active materials. It is also preferable that the graphene compound surrounds at least a portion of the active material. The graphene compound may also have holes.

[0456] When an active material having a small particle size, for example, an active material having a particle size of 1 μm or less, is used, a larger number of conductive paths connecting the active materials is required. In such a case, it is preferable to use a graphene compound, which can efficiently form conductive paths even in a small amount.

[0457] Because of the above-described properties, graphene compounds are particularly effective as conductive materials for secondary batteries that require rapid charging and rapid discharging. For example, rapid charging and rapid discharging may be required for secondary batteries for two-wheeled or four-wheeled vehicles, secondary batteries for drones, etc. Furthermore, rapid charging characteristics may be required for mobile electronic devices, etc. Rapid charging and discharging refers to charging and discharging at, for example, 200 mA / g, 400 mA / g, or 1000 mA / g or more.

[0458] 24B , in a longitudinal cross section of the positive electrode active material layer 502, sheet-like graphene or graphene compounds are dispersed approximately uniformly inside the positive electrode active material layer 502. In FIG. 24B , the graphene or graphene compounds are schematically represented by thick lines, but in reality, they are thin films having a thickness corresponding to a single layer or multiple layers of carbon molecules. The plurality of graphene or graphene compounds are formed so as to partially cover the plurality of positive electrode active material particles 100 or to be attached to the surfaces of the plurality of positive electrode active material particles 100, and are therefore in surface contact with each other.

[0459] Here, a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net) can be formed by bonding multiple graphenes or graphene compounds together. When an active material is covered with a graphene net, the graphene net can also function as a binder that bonds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, thereby improving the ratio of the active material to the electrode volume and electrode weight. In other words, the discharge capacity of a secondary battery can be increased.

[0460] Here, graphene oxide is preferably used as the graphene or graphene compound, and the graphene or graphene compound is mixed with an active material to form a layer that becomes the positive electrode active material layer 502, followed by reduction. That is, the completed active material layer preferably contains reduced graphene oxide. By using graphene oxide, which has extremely high dispersibility in a polar solvent, to form the graphene or graphene compound, the graphene or graphene compound can be dispersed approximately uniformly within the positive electrode active material layer 502. The solvent is volatilized and removed from the dispersion medium containing the uniformly dispersed graphene oxide, and the graphene oxide is reduced. Therefore, the graphene or graphene compound remaining in the positive electrode active material layer 502 is dispersed to such an extent that it partially overlaps with and is in surface contact with each other, thereby forming a three-dimensional conductive path. The graphene oxide may be reduced by, for example, heat treatment or using a reducing agent.

[0461] Therefore, unlike a granular conductive material such as acetylene black that makes point contact with the active material, graphene or a graphene compound enables surface contact with low contact resistance, and therefore, the electrical conductivity between the granular positive electrode active material 100 and the graphene or graphene compound can be improved with a smaller amount than that of a typical conductive material. Thus, the proportion of the positive electrode active material 100 in the positive electrode active material layer 502 can be increased. This can increase the discharge capacity of the secondary battery.

[0462] Furthermore, by using a spray dryer in advance, a graphene compound, which is a conductive material, can be formed as a coating portion that covers the entire active material, and further a conductive path can be formed between the active material particles by the graphene compound.

[0463] In addition, a material used to form the graphene compound may be mixed with the positive electrode active material layer 502 together with the graphene compound. For example, particles used as a catalyst to form the graphene compound may be mixed with the graphene compound. Examples of catalysts used to form the graphene compound include silicon oxide (SiO 2 , SiO x(x<2)), aluminum oxide, iron, nickel, ruthenium, iridium, platinum, copper, germanium, etc. The particles preferably have a median diameter (D50) of 1 μm or less, more preferably 100 nm or less.

[0464] In addition to graphene, acetylene black (abbreviated as AB) can be used as a conductive material. Fluorine-containing acetylene black may also be used. The fluorine in fluorine-containing acetylene black is preferably adsorbed on the surface. Fluorine-containing acetylene black can also be produced by contacting acetylene black with a fluorine compound (called fluorination treatment). The fluorination treatment described for graphene can also be applied to acetylene black.

[0465] In addition to graphene and acetylene black, carbon fiber materials (also referred to as carbon nanotubes or CNTs) can be used as conductive materials. Fluorine-containing carbon nanotubes may also be used. The fluorine in the fluorine-containing carbon nanotubes is preferably adsorbed on the surface. Fluorine-containing carbon nanotubes can also be produced by contacting carbon nanotubes with a fluorine compound (called a fluorination treatment). The fluorination treatment described for graphene can also be applied to carbon nanotubes.

[0466] [Binder] The binder is necessary to firmly bond the powdered active material without covering the surface of the active material. Furthermore, the binder must be adhesive to the current collector. In other words, it is preferable to use a material containing an adhesive component. Furthermore, in consideration of the expansion of the active material, the binder should be sufficiently flexible and able to adapt to changes in the state of the active material. The binder must also be compatible with the electrolyte. Furthermore, since extremely strong oxidation and reduction reactions occur in secondary batteries, a binder that does not deteriorate or has low reactivity in response to these reactions is desirable.

[0467] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Furthermore, as the binder, fluororubber can be used.

[0468] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include one or more of cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, and starch. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.

[0469] Alternatively, it is preferable to use, as the binder, materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose.

[0470] The binder may be a combination of two or more of the above.

[0471] For example, a material with a particularly excellent viscosity adjusting effect may be used in combination with another material. For example, while rubber materials have excellent adhesive strength and / or elasticity, it may be difficult to adjust the viscosity when mixed with a solvent. In such cases, it is preferable to mix them with a material with a particularly excellent viscosity adjusting effect. For example, a water-soluble polymer may be used as a material with a particularly excellent viscosity adjusting effect. Furthermore, as water-soluble polymers with a particularly excellent viscosity adjusting effect, the aforementioned polysaccharides, for example, carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, and diacetyl cellulose, cellulose derivatives such as regenerated cellulose, and starch may be used.

[0472] In addition, the solubility of cellulose derivatives such as carboxymethyl cellulose can be increased by converting them into salts such as sodium and ammonium salts of carboxymethyl cellulose, making them more effective as viscosity adjusters. Higher solubility can also improve the dispersibility of active materials and other components when preparing electrode slurries. In this specification, the cellulose and cellulose derivatives used as electrode binders also include their salts.

[0473] Water-soluble polymers stabilize viscosity by dissolving in water, and can stably disperse active materials and other materials combined as binders, such as styrene-butadiene rubber, in aqueous solutions. Furthermore, because they contain functional groups, they are expected to be easily and stably adsorbed onto the surface of active materials. Furthermore, many cellulose derivatives, such as carboxymethyl cellulose, contain functional groups, such as hydroxyl and carboxyl groups, and because of these functional groups, the polymers are expected to interact with each other and widely cover the surface of the active material.

[0474] When the binder covering or contacting the surface of the active material forms a film, it is expected to function as a passive film and have the effect of suppressing decomposition of the electrolyte. Here, the passive film is a film with no electrical conductivity or a film with extremely low electrical conductivity. For example, when a passive film is formed on the surface of the active material, it can suppress decomposition of the electrolyte at the battery reaction potential. Furthermore, it is more desirable that the passive film suppresses electrical conductivity while still allowing lithium ions to conduct.

[0475] [Current Collector] The current collector can be made of a highly conductive material, such as a metal such as stainless steel, gold, platinum, aluminum, or titanium, or an alloy thereof. It is preferable that the material used for the positive electrode current collector does not dissolve at the potential of the positive electrode. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum, can also be used. The current collector may also be made of a metal element that reacts with silicon to form a silicide. Examples of metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be in the form of a foil, plate, sheet, mesh, punched metal, expanded metal, or the like. It is preferable to use a current collector with a thickness of 5 μm to 30 μm.

[0476] [Negative Electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer may also include a conductive material and a binder.

[0477] [Negative Electrode Active Material] As the negative electrode active material, for example, an alloy-based material and / or a carbon-based material can be used.

[0478] As the negative electrode active material, an element capable of undergoing a charge-discharge reaction by alloying / de-alloying reaction with lithium can be used. For example, a material containing one or more elements selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. Such elements have a larger charge-discharge capacity than carbon, and silicon in particular has a high theoretical capacity of 4200 mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Alternatively, a compound containing these elements may be used. For example, SiO, Mg 2 Si, Mg 2 Ge, SnO, SnO 2 , Mg 2 Sn, SnS 2 , V 2 Sn 3 , FeSn 2 , CoSn 2 , Ni 3 Sn 2 , Cu 6 Sn 5 , Ag 3 Sn, Ag 3 Sb, Ni 2 MnSb, CeSb 3 , LaSn 3 , La 3 Co 2 Sn 7 , CoSb 3 , InSb, SbSn, etc. Here, elements that can undergo charge-discharge reactions by alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloy-based materials.

[0479] In this specification and the like, SiO refers to, for example, silicon monoxide. Alternatively, SiO refers to SiO x For example, x is preferably 0.2 or more and 1.5 or less, more preferably 0.3 or more and 1.2 or less, or preferably 0.2 or more and 1.2 or less, or preferably 0.3 or more and 1.5 or less.

[0480] Examples of carbonaceous materials that can be used include graphite, easily graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon nanotubes, graphene, and carbon black.

[0481] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, spherical graphite having a spherical shape can be used as the artificial graphite. For example, MCMB may have a spherical shape and is preferred. Furthermore, it is relatively easy to reduce the surface area of ​​MCMB and this may be preferred. Examples of natural graphite include flake graphite and spherical natural graphite.

[0482] When lithium ions are inserted into graphite (when a lithium-graphite intercalation compound is formed), graphite exhibits a low potential similar to that of lithium metal (0.05 V to 0.3 V vs. Li / Li + This allows lithium-ion secondary batteries to exhibit high operating voltages. Graphite is also preferred because it has advantages such as a relatively high charge / discharge capacity per unit volume, relatively little volume expansion, low cost, and greater safety than lithium metal.

[0483] Titanium dioxide (TiO 2 ), lithium titanium oxide (Li 4 Ti 5 O 12 ), lithium graphite intercalation compound (Li x C 6 ), niobium pentoxide (Nb 2 O 5 ), tungsten dioxide (WO 2 ), molybdenum dioxide (MoO 2 ) and other oxides can be used.

[0484] In addition, as the negative electrode active material, a nitride of lithium and a transition metal, Li 3 Li with N-type structure 3−x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N has a large charge / discharge capacity (900 mAh / g, 1890 mAh / cm 3 ) and is preferred.

[0485] When a nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so V, which does not contain lithium ions, is used as the positive electrode active material. 2 O 5 , Cr 3 O 8 It is preferable that the material can be combined with a material such as the above. Even when a material containing lithium ions is used as the positive electrode active material, it is possible to use a nitride of lithium and a transition metal as the negative electrode active material by first desorbing the lithium ions contained in the positive electrode active material.

[0486] Furthermore, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, a transition metal oxide that does not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), or iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include Fe 2 O 3 , CuO, Cu 2 O, RuO 2 , Cr 2 O 3 oxides such as CoS 0.89 , sulfides such as NiS and CuS, Zn 3 N 2 , Cu 3 N, Ge 3 N 4 Nitrides such as NiP 2 , FeP 2 , CoP 3 Phosphides such as FeF 3 , BiF 3 Fluorine compounds such as the above can be mentioned.

[0487] The conductive material and binder that can be contained in the negative electrode active material layer can be the same as the conductive material and binder that can be contained in the positive electrode active material layer.

[0488] [Negative electrode current collector] The negative electrode current collector can be made of the same material as the positive electrode current collector. It is preferable that the negative electrode current collector be made of a material that does not alloy with carrier ions such as lithium.

[0489] [Electrolyte Solution] An electrolyte solution can be used as one form of electrolyte. The electrolyte solution contains a solvent and a lithium salt. The solvent (which can also be called an electrolyte solvent) is preferably an aprotic organic solvent, and examples thereof include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, and sultone, or any combination and ratio of two or more of these. Two or more solvents are called mixed organic solvents.

[0490] When the organic solvent contained in the electrolytic solution contains ethylene carbonate (EC) and diethyl carbonate (DEC), a mixed organic solvent can be used in which the volume ratio of ethylene carbonate to diethyl carbonate is x:100-x (where 20≦x≦40) when the ethylene carbonate and diethyl carbonate are 100 vol%. More specifically, a mixed organic solvent containing EC and DEC in a volume ratio of EC:DEC=30:70 can be used.

[0491] Furthermore, when the organic solvent contained in the electrolytic solution contains ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC), a mixed organic solvent can be used in which the volume ratio of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is x:y:100-x-y (where 5≦x≦35 and 0<y<65) when the ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate are 100 vol%. More specifically, a mixed organic solvent containing EC, EMC, and DMC in a volume ratio of EC:EMC:DMC=30:35:35 can be used.

[0492] Furthermore, the organic solvent contained in the electrolyte solution can be a mixed organic solvent containing a fluorinated cyclic carbonate or a fluorinated chain carbonate. Furthermore, it is preferable that the mixed organic solvent contains both a fluorinated cyclic carbonate and a fluorinated chain carbonate. Both the fluorinated cyclic carbonate and the fluorinated chain carbonate have electron-withdrawing substituents, which are preferable because they lower the solvation energy of lithium ions. Therefore, both the fluorinated cyclic carbonate and the fluorinated chain carbonate are suitable for the electrolyte solution, and a mixed organic solvent containing these is also suitable.

[0493] Examples of fluorinated cyclic carbonates that can be used include fluoroethylene carbonate (fluoroethylene carbonate, FEC, F1EC), difluoroethylene carbonate (DFEC, F2EC), trifluoroethylene carbonate (F3EC), and tetrafluoroethylene carbonate (F4EC). DFEC includes isomers such as cis-4,5 and trans-4,5. Since all of these fluorinated cyclic carbonates have electron-withdrawing substituents, they are believed to have low solvation energies for lithium ions.

[0494] The following structural formula (H10) is the structural formula of FEC: In FEC, the electron-withdrawing substituent is an F group.

[0495]

[0496] Methyl 3,3,3-trifluoropropionate is an example of a fluorinated chain carbonate. The following structural formula (H22) is the structural formula of methyl 3,3,3-trifluoropropionate. The abbreviation for methyl 3,3,3-trifluoropropionate is "MTFP." In MTFP, the electron-withdrawing substituent is CF 3 It is the base.

[0497]

[0498] FEC is a cyclic carbonate with a high dielectric constant, and when used in an organic solvent, it promotes the dissociation of lithium salts. On the other hand, because FEC has electron-withdrawing substituents, it is more likely to desolvate with lithium ions than ethylene carbonate (EC). Specifically, the solvation energy of lithium ions in FEC is lower than that of ethylene carbonate (EC), which does not have electron-withdrawing substituents. Therefore, FEC is more likely to release lithium ions from the surfaces of the positive and negative electrode active materials, thereby reducing the internal resistance of the secondary battery. Furthermore, FEC is thought to have a deep highest occupied molecular orbital (HOMO) level. A deep HOMO level reduces oxidation resistance and improves oxidation resistance. On the other hand, there are concerns about the high viscosity of FEC. Therefore, it is recommended to use a mixed organic solvent containing MTFP in addition to FEC in the electrolyte. MTFP is a type of chain carbonate, and can have the effect of reducing the viscosity of the electrolyte solution or maintaining the viscosity at room temperature (typically 25° C.) even at low temperatures (typically 0° C.). Furthermore, MTFP has a lower solvation energy than methyl propionate (abbreviated as "MP"), which does not have an electron-withdrawing substituent, and therefore may form a solvate with lithium ions when used in the electrolyte solution.

[0499] When the mixed organic solvent containing FEC and MTFP having such physical properties is taken as 100 vol %, they are preferably mixed and used in a volume ratio of x:100-x (where 5≦x≦30, preferably 10≦x≦20). In other words, it is preferable to mix MTFP in a larger amount than FEC in the mixed organic solvent.

[0500] Furthermore, by using one or more flame-retardant and non-volatile ionic liquids (room-temperature molten salts) as the solvent for the electrolyte, it is possible to prevent the secondary battery from exploding and / or catching fire even if the internal temperature of the secondary battery rises due to an internal short circuit, overcharging, or the like. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of organic cations used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of anions used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.

[0501] The solvent of the above-mentioned electrolyte solution contains granular dust or molecules other than the constituent molecules of the organic solvent (hereinafter simply referred to as "impurities"), and oxygen (O 2 ), water (H 2 The electrolyte preferably contains a low content of impurities such as 0 or 100 ppm, preferably 50 or less ppm, and more preferably less than 10 ppm. For example, the amount of water can be detected by Karl Fischer titration.

[0502] Furthermore, it is preferable that the above-mentioned organic solvent has almost no peaks due to impurities that can be confirmed by NMR measurement or the like. "Almost no peaks can be confirmed" means that the ratio of the integrated area of ​​the peak due to the impurity to the integrated area of ​​the peak due to the main component (simply referred to as "integral ratio") is 0.005 or less, preferably 0.002 or less. The device used for NMR measurement is not particularly limited, but for example, Bruker's "AVANCEIII 400" can be used. Furthermore, among the five peaks of acetonitrile derived from acetonitrile-d3 used as a solvent in 1H-NMR measurement, the central peak can be located at 1.94 ppm.

[0503] For example, in the case of MTFP, it is known that when 1H-NMR is measured using acetonitrile-d3 solvent, four peaks appear at δ between 3.29 ppm and 3.43 ppm. However, if other peaks appear in this vicinity, for example, if a peak appears at δ between 3.24 ppm and 3.29 ppm, the peak is considered to be derived from impurities. Therefore, if the ratio (integral ratio) of the peak area between 3.24 ppm and 3.29 ppm to the peak area between 3.29 ppm and 3.43 ppm is 0.005 or less, preferably 0.002 or less, it can be said that peaks due to impurities are almost impossible to confirm.

[0504] [Lithium Salt] The lithium salt (also called an electrolyte) to be dissolved in the solvent is, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4 , LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO 2 ), LiN(C 2 F 5 SO 2 ) 2The lithium salt may be used alone or in any combination and ratio of two or more of these. The lithium salt is preferably used in an amount of 0.5 mol / L or more and 3.0 mol / L or less relative to the solvent. 6 , LiBF 4 The use of such improves the safety of lithium ion secondary batteries.

[0505] [Additives] It is preferable to add additives such as vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), or dinitrile compounds such as succinonitrile and adiponitrile to the electrolyte solution. The concentration of the added material is preferably 0.1 wt % or more and 5 wt % or less with respect to the entire solvent. VC or LiBOB is particularly preferable because it is easy to form a good coating portion.

[0506] [Gel Electrolyte] A polymer gel in which a polymer is swollen with an electrolytic solution may be used as the gel electrolyte. By using a polymer gel electrolyte, a semi-solid electrolyte layer can be provided, and safety against leakage and the like can be improved. In addition, it is possible to reduce the thickness and weight of the secondary battery.

[0507] Examples of polymers that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel.

[0508] Examples of polymers that can be used include polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these. For example, PVDF-HFP, which is a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The polymer formed may also have a porous shape.

[0509] [Solid Electrolyte] Instead of an electrolytic solution, a solid electrolyte containing an inorganic material such as a sulfide or oxide, or a solid electrolyte containing a polymer material such as a PEO (polyethylene oxide) can be used. When a solid electrolyte is used, the installation of a separator and / or spacer is unnecessary. Furthermore, since the entire battery can be solidified, there is no risk of leakage, and safety is dramatically improved.

[0510] [Separator] The secondary battery preferably has a separator. Examples of separators that can be used include those made of paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, and polyurethane. The separator is preferably processed into an envelope shape and disposed so as to encase either the positive electrode or the negative electrode.

[0511] The separator may have a multilayer structure. For example, an organic material film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine-based material, a polyamide material, or a mixture thereof. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine-based materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid, para-aramid).

[0512] Coating with ceramic materials improves oxidation resistance, suppressing separator degradation during high-voltage charging and improving the reliability of secondary batteries. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide materials, especially aramid, improves heat resistance, improving the safety of secondary batteries.

[0513] For example, both sides of a polypropylene film may be coated with a mixed material of aluminum oxide and aramid, or the surface of the polypropylene film that contacts the positive electrode may be coated with a mixed material of aluminum oxide and aramid, and the surface that contacts the negative electrode may be coated with a fluorine-based material.

[0514] When a separator with a multilayer structure is used, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the discharge capacity per volume of the secondary battery can be increased.

[0515] [Exterior Body] The exterior body of a secondary battery can be made of a metal material such as aluminum and / or a resin material. A film-like exterior body can also be used. For example, a three-layer film can be used, in which a flexible metal thin film such as aluminum, stainless steel, copper, or nickel is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and a synthetic resin fiber such as polyamide resin or polyester resin is further provided on the metal thin film as the exterior body surface. Fibers made from polyamide resin are called nylon. Such a three-layer film containing aluminum is sometimes referred to as an aluminum laminate film.

[0516] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0517] Embodiment 4 In this embodiment, examples of shapes of secondary batteries other than the laminate type secondary battery described in the previous embodiment will be described in detail.

[0518] <Coin-Type Secondary Battery> An example of a coin-type secondary battery will be described. Fig. 25A is an external view of a coin-type (single-layer flat) secondary battery, and Fig. 25B is a cross-sectional view thereof. Coin-type secondary batteries are mainly used in small electronic devices. In this specification and the like, coin-type batteries include button-type batteries.

[0519] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. A separator 310 is provided between the positive electrode 304 and the negative electrode 307.

[0520] In addition, it is preferable that the active material layer of each of the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 is formed only on one surface of the current collector.

[0521] The positive electrode can 301 and the negative electrode can 302 can be made of a metal such as nickel, aluminum, or titanium that is corrosion-resistant to the electrolyte, or an alloy of these metals and / or alloys of these metals with other metals (e.g., stainless steel). Furthermore, to prevent corrosion by the electrolyte, it is preferable to coat them with nickel and / or aluminum. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.

[0522] These negative electrode 307, positive electrode 304, and separator 310 are impregnated with an electrolyte solution, and as shown in FIG. 25B, the positive electrode 304, separator 310, negative electrode 307, and negative electrode can 302 are stacked in this order with the positive electrode can 301 facing downwards, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303 to produce a coin-shaped secondary battery 300.

[0523] By using the positive electrode active material described in the above embodiment for the positive electrode 304, the coin-type secondary battery 300 can have a high discharge capacity and excellent cycle characteristics.

[0524] Here, we will use Figure 25C to explain the flow of current during charging of a secondary battery. When a lithium-based secondary battery is considered as a closed circuit, the movement of lithium ions and the flow of current are in the same direction. In lithium-based secondary batteries, the anode (positive electrode) and cathode (negative electrode) are interchanged during charging and discharging, and the oxidation and reduction reactions alternate. Therefore, the electrode with a higher reaction potential is called the positive electrode, and the electrode with a lower reaction potential is called the negative electrode. Therefore, in this specification, whether during charging, discharging, when a reverse pulse current is applied, or when a charging current is applied, the positive electrode will be referred to as the "positive electrode" or "+ electrode," and the negative electrode will be referred to as the "negative electrode" or "- electrode." Using the terms anode (positive electrode) and cathode (negative electrode), which are related to oxidation and reduction reactions, may result in the reversed roles during charging and discharging, which could lead to confusion. Therefore, the terms anode (positive electrode) and cathode (negative electrode) will not be used in this specification. If the terms anode and cathode are used, it should be clearly stated whether they are used during charging or discharging, and whether they correspond to the positive electrode (plus pole) or negative electrode (minus pole).

[0525] 25C is connected to a charger to charge the secondary battery 300. As the charging of the secondary battery 300 progresses, the potential difference between the electrodes increases.

[0526] <Cylindrical Secondary Battery> Next, an example of a cylindrical secondary battery will be described with reference to Fig. 26 . Fig. 26A shows an external view of a cylindrical secondary battery 600. Fig. 26B is a schematic diagram showing a cross section of the cylindrical secondary battery 600. As shown in Fig. 26B , the cylindrical secondary battery 600 has a positive electrode cap (battery lid) 601 on the top surface, and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can 602 are insulated by a gasket (insulating packing) 610.

[0527] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a center pin. The battery can 602 is closed at one end and open at the other end. The battery can 602 can be made of a metal, such as nickel, aluminum, or titanium, or an alloy thereof and / or an alloy of these with other metals (e.g., stainless steel), which is corrosion-resistant to the electrolyte. Furthermore, to prevent corrosion by the electrolyte, the battery can 602 is preferably coated with nickel and / or aluminum. Inside the battery can 602, the wound battery element, in which the positive electrode, negative electrode, and separator are wound, is sandwiched between a pair of opposing insulating plates 608 and 609. A nonaqueous electrolyte (not shown) is poured into the battery can 602, in which the battery element is provided. The nonaqueous electrolyte may be the same as that used in coin-type secondary batteries.

[0528] Because the positive and negative electrodes used in cylindrical storage batteries are wound, it is preferable to form active materials on both sides of the current collector. A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. The positive electrode terminal 603 can be made of a metal material such as aluminum. The negative electrode terminal 607 can be made of a metal material such as copper. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 612, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 612 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 612 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the internal pressure of the battery rises above a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases when the temperature rises, and the increase in resistance limits the amount of current to prevent abnormal heat generation. 3 )-based semiconductor ceramics, ...

Claims

A secondary battery having a positive electrode and a negative electrode, The positive electrode has a positive electrode active material, The positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in the surface layer portion of the positive electrode active material is higher than the magnesium concentration in the interior of the positive electrode active material, The negative electrode has a negative electrode active material, The negative electrode active material has a carbon material, When AC impedance measurement is performed on the secondary battery in a state where the secondary battery is charged to a voltage of 4.5 V, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ. A secondary battery having a positive electrode, a negative electrode, a separator, and an electrolyte, The positive electrode has a positive electrode active material, The positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in the surface layer portion of the positive electrode active material is higher than the magnesium concentration in the interior of the positive electrode active material, The negative electrode has a negative electrode active material, The negative electrode active material has a carbon material, the electrolyte solvent comprises ethylene carbonate and diethyl carbonate; The separator comprises polypropylene; When AC impedance measurement is performed on the secondary battery in a state where the secondary battery is charged to a voltage of 4.5 V, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ. A secondary battery having a positive electrode and a negative electrode, The positive electrode has a positive electrode active material, The positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in the surface layer portion of the positive electrode active material is higher than the magnesium concentration in the interior of the positive electrode active material, The negative electrode has a negative electrode active material, The negative electrode active material has a carbon material, When the secondary battery is charged to a voltage of 4.5 V and an AC impedance measurement is performed on the secondary battery in a state in which the capacity is 2000 mAh or more, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ. A secondary battery having a positive electrode, a negative electrode, a separator, and an electrolyte, The positive electrode has a positive electrode active material, The positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in the surface layer portion of the positive electrode active material is higher than the magnesium concentration in the interior of the positive electrode active material, The negative electrode has a negative electrode active material, The negative electrode active material has a carbon material, the electrolyte solvent comprises ethylene carbonate and diethyl carbonate; The separator comprises polypropylene; When the secondary battery is charged to a voltage of 4.5 V and an AC impedance measurement is performed on the secondary battery in a state in which the capacity is 2000 mAh or more, the AC impedance value at a frequency of 1 kHz satisfies the requirement of less than 90 mΩ. In any one of claims 1 to 4, The secondary battery has a temperature rise ΔT of 50° C. or less when a nail penetration test is carried out on the secondary battery with a nail having a diameter of 3 mm and a nail penetration speed of 5 mm / sec. In any one of claims 1 to 4, The lithium cobalt oxide further contains aluminum. In any one of claims 1 to 4, The lithium cobalt oxide further contains nickel. In any one of claims 1 to 4, The lithium cobalt oxide further contains fluorine.

Citation Information

Patent Citations

  • Method for manufacturing lithium-ion secondary batteries

    JP2023033572A

  • Secondary battery and electronic device

    WO2022229776A1