Roller and manufacturing method therefor

The roller's two-layer structure with polyether-containing polymers improves welding strength and durability, addressing the challenges of wear resistance and mechanical strength in harsh environments.

WO2024201723A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI ELECTRIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/012564
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Rollers with resin tires used in harsh environments, such as escalators and walking sidewalks, face challenges in achieving sufficient wear resistance and elasticity, particularly in maintaining strong welding between the outer circumferential and base portions with different hardness levels.

Method used

The roller features a two-layer structure with a base portion and an outer peripheral portion, both containing polymers with hard and soft segments, including polyether, which are welded together to enhance the welding strength, using specific resin compositions and manufacturing methods to ensure improved mechanical strength and abrasion resistance.

Benefits of technology

The enhanced welding strength between the layers improves the roller's durability and reduces peeling, leading to better performance under high-speed rotation and high loads, while maintaining flexibility and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023012564_03102024_PF_FP_ABST
    Figure JP2023012564_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A roller (1) comprises: bearings (40); and resin tires (10) that are respectively disposed at the outer peripheries of the bearings (40). The tires (10) each comprise an outer peripheral part (12) and a base part (11) disposed concentrically with respect to the bearings (40). The base parts (11) are each welded to the bearing (40)-side of the corresponding outer circumferential part (12), and have a different hardness from the outer peripheral parts (12). The base parts (11) and the outer peripheral parts (12) each individually contain a polymer comprising a hard segment and a soft segment, which is constituted by a polyol unit. The base parts (11) and the outer peripheral parts (12) also contain a polyether.
Need to check novelty before this filing date? Find Prior Art

Description

Roller and manufacturing method thereof

[0001] The present disclosure relates to rollers and methods of manufacturing the same.

[0002] Escalators, walkways, and the like sometimes use rollers with resin tires attached to the outer periphery of a bearing. Because such rollers are exposed to harsh environments involving high-speed rotation and heavy loads, they are required to have wear resistance and appropriate elasticity. From this perspective, it is known that the tire placed on the outer periphery of the bearing has a two-layer structure consisting of an outer periphery and a base portion located inside the outer periphery, with the outer periphery being soft and the base portion being hard (e.g., Patent Documents 1 and 2). Patent Documents 1 and 2 disclose that the outer periphery and the base portion can be welded together by supplying a molten resin material into a space formed between the bearing and the outer periphery to form the base portion.

[0003] JP 2000-167871 A JP 2015-55329 A

[0004] In a tire having two layers with different hardness as described above, it is required to further improve the welding strength between the layers.

[0005] The present disclosure aims to provide a roller with improved welding strength between the outer circumferential portion of a tire and a base portion, and a method for manufacturing the same.

[0006] The roller of the present disclosure includes a bearing and a resin tire disposed on the outer periphery of the bearing. The tire has a base portion and an outer periphery disposed concentrically with the bearing. The base portion is welded to the bearing side of the outer periphery and has a different hardness from that of the outer periphery. The base portion and the outer periphery each independently contain a polymer having a hard segment and a soft segment that is a polyol unit. The base portion and the outer periphery further contain a polyether.

[0007] The roller manufacturing method of the present disclosure is a method for manufacturing a roller having a bearing and a resin tire disposed on the outer periphery of the bearing. The roller manufacturing method includes a step of forming a tire, in which a second layer is formed using a second resin composition so as to be welded to a first layer formed using a first resin composition. The first layer and the second layer are formed concentrically around the bearing. The first resin composition and the second resin composition each independently contain a polymer having a hard segment and a soft segment that is a polyol unit. At least one of the first resin composition and the second resin composition further contains a polyether.

[0008] According to the present disclosure, it is possible to provide a roller with improved welding strength between the outer circumferential portion of a tire and the base portion.

[0009] Fig. 1 is a cross-sectional view of a roller in embodiment 1. Fig. 2 is a cross-sectional view of a roller in embodiment 2. Fig. 3 is a perspective view schematically showing test pieces obtained in examples and comparative examples.

[0010] Embodiment 1 (Roller) Fig. 1 is a cross-sectional view of a roller in embodiment 1. Roller 1 can be used under conditions where it rotates at high speed while being subjected to a high load. Roller 1 is used, for example, in escalators, walkways, elevators, etc.

[0011] The roller 1 has a bearing 40 and a resin tire 10 arranged on the outer periphery of the bearing 40. The tire 10 has a base portion 11 and an outer periphery portion 12 arranged concentrically with the bearing 40. The base portion 11 is welded to the bearing 40 side of the outer periphery portion 12 and has a different hardness from that of the outer periphery portion 12. The base portion 11 and the outer periphery portion 12 each independently contain a polymer (hereinafter sometimes referred to as "polymer (P)") having a hard segment and a soft segment that is a polyol unit. The base portion 11 and the outer periphery portion 12 further contain a polyether.

[0012] The bearing 40 is connected to a shaft provided on a cart (not shown). The bearing 40 supports the shaft so that it can rotate freely around a rotation axis. The bearing 40 may be configured using a ball bearing or a roller bearing. The bearing 40 may be made of metal, for example. As shown in FIG. 1 , the bearing 40 may include an inner ring 41, an outer ring 42 arranged on the outer periphery of the inner ring 41, and rolling elements 43 arranged between the inner ring 41 and the outer ring 42.

[0013] The tire 10 is an annular body and is concentrically disposed on the outer periphery of the bearing 40. The tire 10 can have a two-layer structure in which, from the bearing 40 side, a base portion 11 and an outer periphery portion 12 are laminated. The base portion 11 and the outer periphery portion 12 are also annular bodies. The base portion 11 and the outer periphery portion 12 are formed using a resin such as a synthetic resin and are welded to each other. The entire contact surfaces of the base portion 11 and the outer periphery portion 12 are preferably welded together to form an integrated unit. The welded surfaces of the base portion 11 and the outer periphery portion 12 can be curved surfaces without any steps. The base portion 11 may be directly fixed to the bearing 40. For example, as shown in FIG. 1 , the base portion 11 may be fixed to an outer ring 42 of the bearing 40.

[0014] The hardness of the base portion 11 may be different from the hardness of the outer peripheral portion 12, and may be either smaller or larger than the hardness of the outer peripheral portion 12. The hardness of the base portion 11 and the outer peripheral portion 12 can be compared by hardness measured with a durometer.

[0015] The base portion 11 may be required to have mechanical strength sufficient to withstand the high-speed rotation and high load applied to the roller 1 via the shaft. Therefore, the base portion 11 preferably has greater mechanical strength than the outer peripheral portion 12. The outer peripheral portion 12 can form the rolling surface of the roller 1 and can contact a rail or the like when the roller 1 rotates. Therefore, the outer peripheral portion 12 preferably has better wear resistance and is softer than the base portion 11. From this perspective, the hardness (Ho) of the outer peripheral portion 12 measured with a durometer is preferably smaller than the hardness (Hs) of the base portion 11 measured with a durometer. The hardness (Hs) of the base portion 11 and the hardness (Ho) of the outer peripheral portion 12 can be measured using a durometer specified in JIS-K-7215. When comparing hardness, hardnesses measured using the same type of durometer are compared. When measuring hardness, it is desirable to disassemble the tire 10 into the base portion 11 and the outer peripheral portion 12 and measure the surface opposite the welded surface. The hardness of the base portion 11 and the outer periphery 12 may be measured on the side surface of the roller without disassembling the base portion 11 and the outer periphery 12. When measuring the hardness, in addition to disassembling the base portion 11 and the outer periphery 12, cutting may be performed as necessary. However, it is not preferable to use the cut surface for hardness measurement.

[0016] The hardness (Hs) of the base portion 11 and the hardness (Ho) of the outer peripheral portion 12 can be adjusted by one or more selected from the group consisting of the type and content of the polymer (P) contained in the base portion 11 and the outer peripheral portion 12, the type, number average molecular weight, and content of the polyether described below, and the type and content of the additives. Different types of polymer (P) mean different types of structural units such as hard segments and soft segments and different content ratios thereof.

[0017] The hardness (Hs) of the base portion 11 and the hardness (Ho) of the outer peripheral portion 12 may each independently be A60 or more and A100 or less, A70 or more and A99 or less, A75 or more and A98 or less, or A80 or more and A95 or less, as measured with a type A durometer described in JIS-K-7215.

[0018] The hardness (Hs) of the base portion 11 and the hardness (Ho) of the outer peripheral portion 12 may each independently be D20 or more and D90 or less, D65 or more and D85 or less, or D70 or more and D80 or less, as measured with a type D durometer described in JIS-K-7215.

[0019] The base portion 11 and the outer peripheral portion 12 contain a polymer (P). The polymer (P) has hard segments and soft segments in its molecular chain, and the soft segments are polyol units. The polymer (P) is preferably thermoplastic. The polymer (P) is, for example, a thermoplastic elastomer such as a thermoplastic polyurethane elastomer, a thermoplastic polyamide elastomer, or a thermoplastic polyester elastomer. The polymer (P) contained in the base portion 11 and the outer peripheral portion 12 is preferably both a thermoplastic polyurethane elastomer or a thermoplastic polyamide elastomer, and more preferably a thermoplastic polyurethane elastomer.

[0020] The hard segment may be, for example, one or more selected from the group consisting of a polyurethane unit, a polyamide unit, and a polyester unit. From the viewpoint of hydrolysis resistance in a high-temperature, high-humidity environment, the hard segment is preferably at least one of a polyurethane unit and a polyamide unit, and more preferably a polyurethane unit or a polyamide unit.

[0021] The polyurethane unit is a partial structure of polyurethane obtained by polymerization of diisocyanate and short-chain diol, and has a diisocyanate unit and a short-chain diol unit. Examples of the diisocyanate unit include one or more units selected from the group consisting of methyl isocyanate unit, diphenylmethane diisocyanate unit, hexamethylene diisocyanate unit, and toluene diisocyanate unit. Examples of the short-chain diol unit include one or more units selected from the group consisting of ethylene glycol unit, propylene glycol unit, and 1,4-butanediol unit.

[0022] The polyamide unit may be, for example, one or more units selected from the group consisting of nylon 6 units, nylon 66 units, nylon 11 units, and nylon 12 units.

[0023] The polyester unit is a partial structure of a polyester obtained by polymerizing an aromatic diester and a short-chain diol, and has an aromatic diester unit and a short-chain diol unit. Examples of the aromatic diester unit include a polybutylene terephthalate unit. Examples of the short-chain diol unit include those exemplified as the short-chain diol unit contained in the polyurethane unit.

[0024] The polyol unit of the soft segment may be, for example, one or more selected from the group consisting of an ester polyol unit, an ether polyol unit, and a carbonate polyol unit. From the viewpoint of hydrolysis resistance in a high-temperature, high-humidity environment and affinity with polyether, the soft segment is preferably an ether polyol unit. The polyol unit may contain an ester polyol unit and an ether polyol unit, and in this case, may be a partial structure of a copolymer of an ester polyol and an ether polyol.

[0025] The ether-based polyol unit may be, for example, one or more units selected from the group consisting of a polypropylene glycol unit, a polyethylene glycol unit, a polytetramethylene glycol unit, a polytrimethylolpropanol unit, and a polypentaerythritol unit.

[0026] The ester-based polyol unit may be a partial structure of a polyol compound obtained by dehydration condensation of a carboxylic acid and a polyhydric alcohol, and may have a carboxylic acid unit and a polyhydric alcohol unit. The carboxylic acid unit may be at least one of an aliphatic carboxylic acid unit and an aromatic carboxylic acid unit. The carboxylic acid unit may be, for example, one or more units selected from the group consisting of a succinic acid unit, an adipic acid unit, a sepacic acid unit, an azelaic acid unit, a phthalic acid unit, and a dimer acid unit. The polyhydric alcohol unit may be, for example, one or more units selected from the group consisting of an ethylene glycol unit, a butylene glycol unit, and a propylene glycol unit.

[0027] The carbonate-based polyol unit may be a partial structure of a polyol compound obtained by reacting a carbonate diester with an alkanediol, and may have a carbonate diester unit and an alkanediol unit. The carbonate diester unit may be, for example, one or more units selected from the group consisting of a diphenyl carbonate unit, a dinaphthyl carbonate unit, a bis(diphenyl)carbonate unit, a dimethyl carbonate unit, a diethyl carbonate unit, and a dibutyl carbonate unit. The alkanediol unit may be, for example, one or more units selected from the group consisting of a 1,6-hexanediol unit, a 1,5-pentanediol unit, a 1,4-butanediol unit, and a 2-methyl-1,3-propanediol unit.

[0028] The polymer (P) preferably has a hard segment that is one or more selected from the group consisting of polyurethane units, polyamide units, and polyester units, and a soft segment that is one or more selected from the group consisting of ester-based polyol units, ether-based polyol units, and carbonate-based polyol units. From the viewpoints of hydrolysis resistance in a high-temperature, high-humidity environment and affinity with polyether, the polymer (P) is more preferably a polymer in which the hard segment is a polyurethane unit or polyamide unit and the soft segment is an ether-based polyol unit.

[0029] The content of the polymer (P) in the base portion 11 is preferably 40 parts by mass or more and 100 parts by mass or less, based on 100 parts by mass of the base portion 11 .

[0030] The content of the polymer (P) in the outer peripheral portion 12 is preferably 50 parts by mass or more and 100 parts by mass or less, when the outer peripheral portion 12 is taken as 100 parts by mass.

[0031] Both the base portion 11 and the outer peripheral portion 12 further contain a polyether, such as at least one of polyethylene glycol and polypropylene glycol.

[0032] The number average molecular weight of the polyether is preferably 1,000 or more, more preferably 2,000 or more, even more preferably 3,000 or more, and may be 4,000 or more, and is usually 10,000 or less. The number average molecular weight can be determined as a value converted into standard polystyrene by gel permeation chromatography (GPC), and can be measured by the method described in the examples below.

[0033] The polyether is preferably polyethylene glycol, more preferably polyethylene glycol having a number average molecular weight in the above-mentioned range, for example, polyethylene glycol having a number average molecular weight of 1,000 or more. The number average molecular weight of the polyethylene glycol for polymer (P) may be in the range of the number average molecular weight of the polyether described above. When the number average molecular weight of the polyethylene glycol is in the above-mentioned range, it is easily kneaded with the polymer (P).

[0034] The content of the polyether in the base 11 is 0 parts by mass or more and 20 parts by mass or less, preferably more than 0 parts by mass or more than 10 parts by mass or more than 0 parts by mass or less, relative to 100 parts by mass of the polymer (P) contained in the base 11. If the content of the polyether is too large, the mechanical strength of the base 11 decreases, and the durability of the roller 1 tends to decrease.

[0035] The content of polyether in the outer circumferential portion 12 may be 0 parts by mass or more and 50 parts by mass or less, preferably 10 parts by mass or more and 50 parts by mass or less, and may be 10 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the polymer (P) contained in the outer circumferential portion 12. If the content of polyether is too small, it becomes difficult to impart flexibility to the outer circumferential portion 12, and it tends to be difficult to obtain a roller 1 having flexibility on the rolling surface. If the content of polyether is too large, the mechanical strength of the outer circumferential portion 12 tends to decrease.

[0036] The hard segments of the polymer (P) have a higher melting point and a more rigid molecular chain structure than the soft segments, while the soft segments of the polymer (P) have a lower melting point and a more flexible molecular chain structure than the hard segments. Therefore, when a welded surface is formed between the base portion 11 and the outer peripheral portion 12, it is thought that the soft segments of the polymer (P) melt and diffuse, forming a welded surface in which the soft segments of the polymer (P) are entangled with each other.

[0037] In addition, the polyether contained in the base portion 11 and the outer peripheral portion 12 also has a low melting point and a flexible molecular structure. When the welded surface between the base portion 11 and the outer peripheral portion 12 is formed, the polyether melts and diffuses along with the soft segments of the polymer (P), and it is believed that the soft segments become entangled with the polyether at the welded surface. As a result, in the roller 1, peeling at the welded surface between the base portion 11 and the outer peripheral portion 12 is suppressed and the weld strength is improved compared to rollers in which neither the base portion nor the outer peripheral portion contains polyether. In this way, the improved weld strength at the welded surface between the base portion 11 and the outer peripheral portion 12 of the tire 10 is believed to suppress surface wear that would be revealed by peeling of the welded surface when the roller 1 rolls, and to suppress the generation of abnormal noise from the roller 1.

[0038] The base portion 11 and the outer peripheral portion 12 have different hardnesses. When different types of polymers (P) are used to achieve different hardnesses, polymers with different ratios of hard segments to soft segments may be used. In this case, the entanglement of the soft segments of the polymer (P) may be reduced at the welded surface between the base portion 11 and the outer peripheral portion 12. Even in such a case, the polyether in the roller 1 can be entangled with the soft segments of the polymer (P), thereby improving the weld strength at the welded surface between the base portion 11 and the outer peripheral portion 12.

[0039] As described above, the tire 10 contains polyether in both the base portion 11 and the outer circumferential portion 12. The base portion 11 and the outer circumferential portion 12 may contain polyether entirely. Alternatively, one of the base portion 11 and the outer circumferential portion 12 may contain polyether entirely, and the other may contain polyether on the welding surface side, but not on the surface opposite the welding surface.

[0040] More specifically, the outer peripheral portion 12 may contain polyether throughout its entirety, and the base portion 11 may contain polyether on the welding surface side but not on the surface opposite the welding surface side. Alternatively, the base portion 11 may contain polyether throughout its entirety, and the outer peripheral portion 12 may contain polyether on the welding surface side but not on the surface opposite the welding surface side. The presence of polyether in the base portion 11 and the outer peripheral portion 12 can be analyzed by, for example, gel permeation chromatography (GPC) or nuclear magnetic resonance (NMR).

[0041] The base portion 11 and the outer peripheral portion 12 may each independently further contain additives such as a filler, an antioxidant, an ultraviolet absorber, a hydrolysis-resistant stabilizer, and a flame retardant.

[0042] The filler can improve the rigidity of the base portion 11 and the outer peripheral portion 12. The filler may be contained in the base portion 11 but not in the outer peripheral portion 12. By blending a filler into the base portion 11 and improving the rigidity of the base portion 11, a roller 1 with excellent durability can be obtained. Examples of the filler include one or more selected from the group consisting of fibrous fillers such as glass fiber and cellulose fiber, and particulate fillers such as inorganic fillers.

[0043] The antioxidant may be, for example, one or more selected from the group consisting of phenol-based antioxidants, hindered phenol-based antioxidants, and hindered amine-based antioxidants.

[0044] Examples of the ultraviolet absorber include one or more selected from the group consisting of benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, and benzophenone-based ultraviolet absorbers.

[0045] The hydrolysis-resistant stabilizer may be, for example, a compound having a carbodiimide group.

[0046] Examples of the flame retardant include one or more selected from the group consisting of phosphoric acid ester compounds such as tricresyl phosphate and triphenyl phosphate, and halogen-based compounds such as decabromodiphenyl ether and brominated polystyrene.

[0047] The above describes a case where the tire 10 has a two-layer structure of the base portion 11 and the outer circumferential portion 12, but the tire 10 may have further layers as long as it has the base portion 11 and the outer circumferential portion 12.

[0048] As described above, since the polymer (P) has thermoplasticity, the base portion 11 and the outer peripheral portion 12 can be formed by injection molding. The method for manufacturing the roller 1 is not particularly limited, and the roller 1 can be manufactured by, for example, the manufacturing method described in the embodiment described later.

[0049] Embodiment 2 (Roller) Figure 2 is a cross-sectional view of a roller in embodiment 2. In Figure 2, the same or corresponding members as in Figure 1 are designated by the same reference numerals, and description thereof will not be repeated.

[0050] The roller 2 shown in Fig. 2 has a base portion 21 and an outer periphery 22 instead of the base portion 11 and outer periphery 12 of the roller 1 shown in Fig. 1. In the roller 2 shown in Fig. 2, the shape of the welded surface between the base portion 21 and the outer periphery 22 is different from the shape of the welded surface between the base portion 11 and the outer periphery 12 of the roller 1 shown in Fig. 1. Except for the shape of the welded surface, the base portion 21 and the outer periphery 22 can be similar to the base portion 11 and the outer periphery 12 shown in Fig. 1.

[0051] As shown in Fig. 2, the roller 2 has an uneven shape on the welded surface between the base portion 21 and the outer periphery 22. The uneven shape may have steps, and the shape and number of the steps are not limited. By having an uneven shape on the welded surface, the welded area can be increased compared to when the welded surface does not have steps as shown in Fig. 1, and therefore the weld strength between the base portion 21 and the outer periphery 22 can be improved. This makes it possible to further suppress peeling at the welded surface between the base portion 21 and the outer periphery 22.

[0052] Embodiment 3 (Roller Manufacturing Method) The roller manufacturing method can be, for example, a method for manufacturing the rollers 1 and 2 (FIGS. 1 and 2) described above. The rollers manufactured by the roller manufacturing method may be rollers other than the rollers 1 and 2.

[0053] The roller has a bearing and a resin tire arranged on the outer periphery of the bearing. The method for manufacturing the roller includes a step of forming a tire (hereinafter sometimes referred to as "step (S)"). In step (S), a second layer is formed using a second resin composition so as to be welded to a first layer formed using a first resin composition. The first layer and the second layer are formed concentrically with respect to the bearing. The first resin composition and the second resin composition each independently contain a polymer having a hard segment and a soft segment that is a polyol unit. At least one of the first resin composition and the second resin composition further contains a polyether.

[0054] The bearing may be any of those described above. The tire may have, for example, the base body 11, 21 and the outer peripheral portion 12, 22 described above. The polymer (P) and the polyether may be any of those described above.

[0055] In step (S), the second layer is formed so as to be welded to the first layer. In step (S), the second layer may be formed by injection molding of the second resin composition. In step (S), the first layer may be formed using the first resin composition, or may be formed by injection molding of the first resin composition. For example, when the first layer is formed so as to be fixed to the bearing, the first layer may be formed by pouring a molten first resin composition onto the outer periphery of a bearing placed in a mold and molding it.

[0056] The second layer can be formed by, for example, placing the first layer in a mold and pouring a molten second resin composition into the mold so that it contacts the first layer. When the second layer is formed so that it is welded to the surface of the first layer opposite the bearing side, the second layer can be formed by placing the first layer or the first layer integrated with the bearing in the mold and pouring a molten second resin composition into the surface of the first layer. When the second layer is formed between the bearing and the first layer, the bearing and the first layer can be concentrically placed in the mold so that a gap is formed therebetween, and the molten second resin composition can be poured into the gap to form the second layer. The first layer and the second layer can be welded together by pouring a molten second resin composition into the mold so that it contacts the first layer to form the second layer.

[0057] When a resin composition is heated and melted to form a mold, the resin composition may shrink after curing. If a molten second resin composition is poured onto the bearing side of the first layer to form the second layer, the second layer will shrink toward the bearing, i.e., in a direction away from the first layer, making it more likely to peel off from the first layer. Therefore, it is preferable to form the second layer so that it is welded to the surface of the first layer opposite the bearing side. This allows the second layer to be formed so that it shrinks in a direction that brings it into close contact with the first layer, thereby preventing a decrease in the weld strength between the first and second layers. For the same reason, it is preferable to form the first layer by pouring the first resin composition onto the outer periphery of the bearing so that the first layer is formed so that it shrinks in a direction that brings it into close contact with the bearing. This allows the bearing to be firmly held by the first layer, integrating the first layer and the bearing.

[0058] When the second layer is molded by pouring the second resin composition into the gap between the bearing and the first layer, it is possible to adjust the molding conditions to suppress shrinkage of the resin composition after curing. This can prevent a decrease in the welding strength between the first layer and the second layer, but because shrinkage of the resin composition after curing is suppressed, there is a risk that the holding strength of the bearing by the second layer will decrease. Therefore, as described above, it is preferable to mold the first layer on the outer periphery of the bearing and then mold the second layer on the outer periphery of this first layer (the surface opposite the bearing side).

[0059] As described above, the first resin composition and the second resin composition contain a polymer (P), and at least one of the first resin composition and the second resin composition contains a polyether. The soft segment of the polymer (P) has a lower melting point and is more easily melted than the hard segment, and the polyether also melts easily. When forming the second layer, the soft segment of the polymer (P) near the surface of the first layer that contacts the second layer can be melted by pouring the molten second resin composition so that it contacts the first layer. At this time, if the first layer is formed from a first resin composition containing a polyether, the polyether on the surface of the first layer also melts. As a result, it is presumed that the soft segment of the polymer (P) contained in the first layer, the soft segment of the polymer (P) contained in the second resin composition, and the polyether contained in at least one of the first layer and the second resin composition diffuse and become entangled with each other. As a result, at the welding surface between the first layer and the second layer, the soft segments of the polymer (P) contained in the first layer and the soft segments of the polymer (P) contained in the second resin composition become entangled, and these soft segments and the polyether become entangled, which is thought to enable the first layer and the second layer to be welded with excellent welding strength.

[0060] The first layer to which the second layer is welded can become the base portion 11, 21 or the outer circumferential portion 12, 22 of the tires 10, 20 of the rollers 1, 2 described above. For example, if the first layer to which the second layer is welded becomes the base portion 11, 21, the second layer becomes the outer circumferential portion 12, 22. If the first layer to which the second layer is welded becomes the outer circumferential portion 12, 22, the second layer becomes the base portion 11, 21. In this way, the first layer can become the base portion 11, 21 or the outer circumferential portion 12, 22 by welding it to the second layer. Because the second layer is formed so as to be welded to the first layer, the formed second layer can become the base portion 11, 21 or the outer circumferential portion 12, 22 as it is. If the second layer is formed so as to be welded to the surface of the first layer opposite the bearing side, the first layer to which the second layer is welded becomes the base portion 11, 21, and the second layer becomes the outer circumferential portion 12, 22. When the second layer is formed so as to be welded to the bearing side surface of the first layer, the first layer to which the second layer is welded becomes the outer peripheral portion 12, 22, and the second layer becomes the base portion 11, 21.

[0061] The first layer and the second layer may have different hardnesses. The hardness of the first layer may be greater or less than the hardness of the second layer. The hardnesses of the first layer and the second layer can be compared based on the hardness measured with a durometer, for example, a durometer as described in JIS-K-7215. When comparing hardnesses, the hardnesses are compared based on the hardness measured using the same type of durometer.

[0062] The hardness of the first layer and the second layer can be adjusted by one or more selected from the group consisting of the type and content of the polymer (P) contained in the first resin composition and the second resin composition, the type, number average molecular weight, and content of the polyether, and additives, etc. Examples of different types of polymer (P) include polymers having different structural units and polymers having different content ratios of hard segments and soft segments.

[0063] The first resin composition and the second resin composition may have the same composition, but preferably have different compositions. The first resin composition and the second resin composition have different compositions means that the first resin composition and the second resin composition differ from each other in at least one of the types and contents of components contained therein, and preferably differ from each other in at least one of the type of polymer (P) and the content of polyether.

[0064] When the first resin composition and the second resin composition contain the same type of polymer (P), it is preferable that only one of the first resin composition and the second resin composition contains a polyether, and the other does not. The polymer (P) contained in the first resin composition and the second resin composition may both be a thermoplastic polyurethane elastomer, a thermoplastic polyamide elastomer, or a thermoplastic polyester elastomer. In this case, the hard segment and soft segment content ratios of the thermoplastic elastomers contained in the first resin composition and the second resin composition may be different from each other. It is preferable that both the first resin composition and the second resin composition contain a thermoplastic polyurethane elastomer but have different polyether contents. In this case, the thermoplastic polyurethane elastomers may be the same elastomer or may be elastomers with different hard segment and soft segment content ratios. Alternatively, only one of the first resin composition and the second resin composition may contain a polyether.

[0065] The hardness of the first layer and the second layer, measured with a type A durometer according to JIS-K-7215, may be independently A60 or more and A100 or less, A70 or more and A99 or less, A75 or more and A98 or less, or A80 or more and A95 or less.

[0066] The hardness of the first layer and the second layer may each independently be D20 or more and D90 or less, D65 or more and D85 or less, or D70 or more and D80 or less, as measured with a type D durometer described in JIS-K-7215.

[0067] The content of the polymer (P) in the first resin composition is desirably 40 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the first resin composition.

[0068] The content of the polymer (P) in the second resin composition is desirably 50 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the second resin composition.

[0069] At least one of the first resin composition and the second resin composition further contains a polyether. The polyether may be contained in only one of the first resin composition and the second resin composition, or in both of them.

[0070] When the hardness of the first layer is greater than the hardness of the second layer, the content of the polyether in the first resin composition may be 0 parts by mass or more and 20 parts by mass or less, preferably more than 0 parts by mass or less and 10 parts by mass or less, and may be more than 0 parts by mass or less and 5 parts by mass or less, relative to 100 parts by mass of the polymer (P). The content of the polyether in the second resin composition may be 0 parts by mass or more and 50 parts by mass or less, preferably 10 parts by mass or more and 50 parts by mass or less, and may be 10 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the polymer (P). As the polyether content decreases, the first layer and the second layer tend to become harder, and as the polyether content increases, the first layer and the second layer tend to become softer. The content of the polyether in the first resin composition and the second resin composition may be adjusted depending on the properties required of the first layer and the second layer.

[0071] When the hardness of the first layer is lower than the hardness of the second layer, the content of the polyether in the first resin composition may be 0 to 50 parts by mass, preferably 10 to 50 parts by mass, or 10 to 30 parts by mass, relative to 100 parts by mass of the polymer (P). Also, the content of the polyether in the second resin composition may be 0 to 20 parts by mass, preferably more than 0 to 10 parts by mass, or more than 0 to 5 parts by mass, relative to 100 parts by mass of the polymer (P).

[0072] The first resin composition and the second resin composition may each independently further contain additives such as a filler, an antioxidant, an ultraviolet absorber, a hydrolysis-resistant stabilizer, and a flame retardant, etc. Examples of these additives include those described above.

[0073] When the first resin composition and the second resin composition contain a polyether, the first resin composition and the second resin composition may be a mixture obtained by stirring and mixing a pellet-like polymer (P) with a powdery or liquid polyether, or may be a kneaded product obtained by melting and kneading the polymer (P) and the polyether. The kneaded product may be molded into a pellet shape. The first resin composition and the second resin composition as a mixture can be formed into the first layer and the second layer by heating and melting the kneaded product and molding it. The first resin composition and the second resin composition as a kneaded product can be formed into the first layer and the second layer by heating and melting the kneaded product and molding it.

[0074] Hereinafter, the present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to these examples.

[0075] [Examples 1 to 4, Comparative Examples 1 and 2] FIG. 3 is a perspective view schematically showing the test pieces obtained in the examples and comparative examples.

[0076] A first resin composition and a second resin composition containing each component in the amounts shown in Table 1 were prepared. The first resin composition was melt-molded to form a plate-shaped first layer 31 having a rectangular shape in plan view and measuring 75 mm long, 10 mm wide, and 4 mm thick. Next, the first layer 31 was placed in a mold, and a plate-shaped second layer 32 having a rectangular shape in plan view and measuring 75 mm long, 10 mm wide, and 4 mm thick was molded so as to be welded to one short side of the first layer 31, thereby obtaining a strip-shaped test piece 30 as shown in FIG. 3. Note that when evaluating weld strength, the dimensions of the test piece are not limited to the above, and any shape can be used.

[0077] In Table 1, each symbol represents the following component: (Polymer (P)) P-1: Thermoplastic polyurethane elastomer ("Elastollan 1174D" manufactured by BASF) P-2: Thermoplastic polyurethane elastomer ("Elastollan 1180A" manufactured by BASF) P-3: Thermoplastic polyurethane elastomer ("Elastollan ET385" manufactured by BASF)

[0078] (Polyether) B-1: Polyethylene glycol ("Polyethylene Glycol 4000" manufactured by Tokyo Chemical Industry Co., Ltd., number average molecular weight: 4000)

[0079] [Measurement of number average molecular weight] The number average molecular weight was measured as a standard polystyrene equivalent value by gel permeation chromatography (GPC). Specifically, a high-speed GPC device ("HLC-8320" manufactured by Tosoh Corporation) was used, and the following column and mobile phase were used, with the column temperature set to 25°C. Column: TSKgel ODS-80Ts (4.6 mmφ×25 cm) (manufactured by Tosoh Corporation) Mobile phase: water / acetonitrile Column temperature: 40°C Flow rate: 1 mL / min Sample concentration: 1 mg / mL Injection volume: 10 μL

[0080] [Measurement of durometer hardness] Using a type A or type D durometer as specified in JIS-K-7215, the durometer hardness of the first layer and the second layer of the test piece was measured at 25°C. The results are shown in Table 1. In Table 1, the letters "A" and "D" before the numerical values ​​indicate the type of durometer used for the measurement. When measurements were performed using both type A and type D durometers, both values ​​are shown in Table 1.

[0081] [Measurement of Weld Strength] A tensile test was performed using a tensile testing machine ("AG-X20kN" manufactured by Shimadzu Corporation) with a distance between grippers of 50 mm and a pulling speed of 50 mm / min, in which the first layer 31 and the second layer 32 were pulled in opposite directions to each other, and the breaking strength [MPa] was measured when the first layer 31 and the second layer 32 of the test piece 30 broke at the welded surface. The tensile test was performed under conditions of 25°C.

[0082]

[0083] The results shown in Table 1 show that as the content of polyether in the second resin composition increases, the hardness of the second layer decreases, but the weld strength of the test piece improves. A comparison between Example 3 and Comparative Example 1, and a comparison between Example 4 and Comparative Example 2, shows that even if the hardness of the second layer is similar, the inclusion of polyether in the test piece can improve the weld strength.

[0084] The embodiments and examples disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims.

[0085] REFERENCE SIGNS LIST 1, 2 Roller, 10 Tire, 11 Base portion, 12 Outer peripheral portion, 20 Tire, 21 Base portion, 22 Outer peripheral portion, 30 Test piece, 31 First layer, 32 Second layer, 40 Bearing, 41 Inner ring, 42 Outer ring, 43 Rolling element.

Claims

1. A roller comprising: a bearing; and a resin tire arranged on the outer periphery of the bearing, wherein the tire has a base portion and an outer periphery arranged concentrically with the bearing, wherein the base portion is welded to the bearing side of the outer periphery and has a different hardness from that of the outer periphery, wherein the base portion and the outer periphery each independently contain a polymer having a hard segment and a soft segment which is a polyol unit, and wherein the base portion and the outer periphery further contain a polyether.

2. The roller according to claim 1, wherein the hardness (Ho) of the outer peripheral portion measured with a durometer is smaller than the hardness (Hs) of the base portion measured with a durometer.

3. The roller according to claim 1 or 2, wherein the polyether is a polyethylene glycol having a number average molecular weight of 1000 or more.

4. The roller according to any one of claims 1 to 3, wherein the hard segment is a polyurethane unit or a polyamide unit, and the soft segment is an ether-based polyol unit.

5. A roller according to any one of claims 1 to 4, wherein the welded surface between the base portion and the outer periphery has an uneven shape.

6. A method for manufacturing a roller having a bearing and a resin tire placed on the outer periphery of the bearing, comprising the step of forming the tire, wherein the step comprises forming a second layer using a second resin composition so as to be welded to a first layer formed using a first resin composition, the first layer and the second layer being formed concentrically around the bearing, the first resin composition and the second resin composition each independently containing a polymer having a hard segment and a soft segment which is a polyol unit, and at least one of the first resin composition and the second resin composition further contains a polyether.

7. The method for manufacturing a roller according to claim 6, wherein the step of forming the tire includes forming the second layer so as to be fused to a surface of the first layer opposite to the bearing side.

8. A method for manufacturing a roller according to claim 6 or 7, comprising the steps of: forming the first layer by injection molding the first resin composition; and forming the second layer by injection molding the second resin composition.

9. A method for manufacturing a roller according to any one of claims 6 to 8, wherein the first layer has a different hardness than the second layer.

10. A method for manufacturing a roller according to any one of claims 6 to 9, wherein only one of the first resin composition and the second resin composition contains a polyether.

Citation Information

Patent Citations

  • Step roller for escalator or moving walk

    JP1998279244A

  • Structure

    JP2020051615A

  • tire

    WO2017104187A1