Light emitting element, display device, and quantum dot additive
The quantum dot adduct configuration, with a carbon-containing compound and a discontinuous or porous silica coating, addresses the insulating issues of silica-coated quantum dots, enhancing carrier injection and luminous efficiency in light-emitting devices, resulting in improved performance and extended service life.
Patent Information
- Application Number
- PCT/JP2023/012829
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
The insulating nature of silica coatings on quantum dots inhibits carrier injection, and introducing organic cyclic structures to improve carrier injection efficiency is insufficient, leading to suboptimal performance in light-emitting devices.
A quantum dot adduct configuration is developed, where the quantum dots are partially surrounded by a compound containing carbon, hydrogen, nitrogen, or oxygen, with the adduct being a discontinuous film, non-uniform in thickness, or porous, allowing for enhanced carrier injection and luminous efficiency.
This configuration significantly improves carrier injection efficiency and luminous efficiency of light-emitting elements, extending their service life and maintaining high external quantum efficiency over time.
Smart Images

Figure JP2023012829_03102024_PF_FP_ABST
Abstract
Description
Light-emitting device, display device, and quantum dot adduct
[0001] The present disclosure relates to a light-emitting device, a display device, and a quantum dot adduct.
[0002] To improve durability, research is being conducted into covering quantum dots with silica (silicon oxide). Non-Patent Document 1 discloses a structure in which quantum dots are covered with silica having an organic ring structure introduced therein.
[0003] "Blue-Emitting InP / GaP / ZnS Quantum Dots with Enhanced Stability by Siloxane Capping: Implication for Electroluminescent Devices" (ACS Appl. Nano Mater. 2022, 5, 2801-2811)
[0004] Since silica is insulating, covering quantum dots with silica hinders carrier injection into the quantum dots. Non-Patent Document 1 attempts to improve the carrier injection efficiency by introducing an organic ring structure into silica, but carrier injection is still insufficient.
[0005] A light-emitting element according to one aspect of the present disclosure comprises: a first electrode and a second electrode facing each other; and a light-emitting layer provided between the first electrode and the second electrode, the light-emitting layer including quantum dots, an additive located at least partially around the quantum dots, and a compound including carbon and one or more of hydrogen, nitrogen, and oxygen provided between the quantum dots and the additive, the additive being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion having a thickness of 1 nm or less.
[0006] A quantum dot adduct according to one aspect of the present disclosure includes a quantum dot, an adduct located at least partially around the quantum dot, and a compound containing carbon and one or more of hydrogen, nitrogen, and oxygen, provided between the quantum dot and the adduct, wherein the adduct is at least one of a discontinuous film, a non-uniform thickness, a porous film, and a film having a thickness of 1 nm or less.
[0007] According to the configuration according to one aspect of the present disclosure, the efficiency of carrier injection into quantum dots can be improved.
[0008] 1 is a cross-sectional view showing an example of the configuration of a light-emitting device according to an embodiment of the disclosure. FIG. 1 is a cross-sectional view showing an example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 2 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 3 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 4 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 5 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 6 is a diagram showing a method for manufacturing a quantum dot-added body according to an embodiment of the present disclosure. FIG. 7 is a diagram showing a method for manufacturing a quantum dot-added body according to an embodiment of the present disclosure. FIG. 8 is a graph showing the voltage-luminance characteristics of light-emitting devices according to Example 1 and Comparative Examples 1 and 2. FIG. 9 is a graph showing the voltage-current density characteristics of light-emitting devices according to Example 1 and Comparative Examples 1 and 2. FIG. 10 is a graph showing the current density-luminance characteristics of light-emitting devices according to Example 1 and Comparative Examples 1 and 2. FIG. 11 is a graph showing the current density-EQE characteristics of light-emitting devices according to Example 1 and Comparative Examples 1 and 2. FIG. 12 is a graph showing the luminance and driving voltage over time for the light-emitting device according to Example 1 in a constant current test. FIG. 13 is a graph showing the luminance and driving voltage over time for the light-emitting device according to Comparative Example 1 in a constant current test. FIG. 14 is a graph showing an estimated useful life of the light-emitting device according to Example 1. Fig. 1 is a diagram showing an estimated value of the useful life of a light-emitting element according to Comparative Example 1. Fig. 2 is a diagram showing the result of FTIR of a solution of a quantum dot adduct according to Example 1. Fig. 3 is a diagram showing the result of FTIR of a solution of a quantum dot adduct according to Comparative Example 1. Fig. 4 is a diagram showing the result of FTIR of a solution of a quantum dot adduct according to Comparative Example 2. Fig. 5 is a cross-sectional view showing an example of the configuration of a display device according to an embodiment of the present disclosure.
[0009] [Embodiment 1] (Configuration of Light-Emitting Device) Fig. 1 is a cross-sectional view showing an example of the configuration of a light-emitting device according to an embodiment of the present disclosure. As shown in Fig. 1, a light-emitting device 10 according to the present disclosure includes a first electrode 12 and a second electrode 16 facing each other, and a light-emitting layer 14 provided between the first electrode 12 and the second electrode 16, the light-emitting layer 14 including quantum dots QDs, an adduct 2 located at least partially around the quantum dots QDs, and a compound 4 provided between the quantum dots QDs and the adduct 2, the compound 4 including carbon and one or more of hydrogen, nitrogen, and oxygen, the adduct 2 being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion with a thickness of 1 nm or less. The quantum dots QDs, the adduct 2, and the compound 4 constitute the quantum dot adduct 1.
[0010] In this configuration, the additive 2 does not hinder carrier injection into the quantum dots QD, as compared with the conventional configuration in which the additive covering the periphery of the quantum dots is a continuous film with a uniform thickness and a dense structure, thereby improving the efficiency of carrier injection into the quantum dots QD in the light-emitting element 10 and the luminous efficiency of the light-emitting element 10.
[0011] One of the first electrode 12 and the second electrode 16 is an anode, and the other is a cathode. At least one of the first electrode 12 and the second electrode 16 is a transparent electrode. The light-emitting element 10 may include additional components, such as a substrate 11 on which the first electrode 12 is formed, a sealing film 17 covering the second electrode 16, a charge transport layer 13 located between the first electrode 12 and the light-emitting layer 14, and a charge transport layer 15 located between the second electrode 16 and the light-emitting layer 14.
[0012] Compound 4 can passivate surface defects of quantum dots (QDs). Compound 4 may further contain sulfur and / or a metal element of the same type as the metal element contained in the quantum dots. Compound 4 may be an organic substance. Compound 4 may be coordinated to the quantum dots (QDs) or may have a modifying group capable of coordinating to the quantum dots (QDs). For example, compound 4 may be bonded to a metal element contained in the quantum dots (QDs) via a thiol bond or may have a thiol group at one end. Compound 4 may be bonded to adduct 2 or may have a modifying group capable of bonding to adduct 2 at another end.
[0013] It is beneficial for compound 4 to have a short molecular length so that hopping conduction via compound 4 does not become dominant in the charge transfer from the outside of adduct 2 to the quantum dots (QDs). Compound 4 may also have carbon-carbon bonds, and the carbon-carbon bonds may be continuous in a chain or ring. Carbon in compound 4 may be an element constituting the main chain of an organic material. When compound 4 has more than 5 carbon atoms, steric hindrance tends to obscure surface defects in the quantum dots (QDs), resulting in insufficient defect passivation. Therefore, it is desirable for compound 4 to have 5 or less carbon atoms. Experiments have shown that when compound 4 has less than 3 carbon atoms, the density of methoxysilane is high and silicon oxide tends to form a dense film. Therefore, it is desirable for compound 4 to have 3 or more carbon atoms.
[0014] The band gap of the additive 2 is wider than the band gap of the constituent material of the quantum dot QD. When the quantum dot QD has a core and a shell surrounding the core, the band gap of the additive 2 is wider than the band gap of the constituent material of the shell. Usually, the additive 2 is insulating.
[0015] The additive 2 may be an inorganic material. For example, the additive 2 may be silicon oxide (SiO 2 ), and may further contain silicic acid ([SiO x (OH) 4-2x ] n Additive 2 may contain titanium oxide (TiO 2 The additive 2 may contain aluminum oxide (Al 2 O 3Adduct 2 may contain zinc chloride (ZnCl 2 The additive 2 may include silicon nitride (Si 3 N 4 ). Additive 2 may include, for example, boron oxide (B 2 O 3 ), phosphorus oxide (P 2 O 5 ), germanium oxide (GeO 2 ), beryllium fluoride (BeF 2 ), arsenic sulfide (As 2 S 3 ), silicon selenide (SiSe 2 ), germanium sulfide (GeS), tellurium oxide (TeO 2 ), bismuth oxide (Bi 2 O 3 ), vanadium oxide (V 2 O 5 ), antimony oxide (Sb 2 O 5 ), lead oxide (PbO), copper oxide (CuO), zirconium fluoride (ZrF 4 ), aluminum fluoride (AlF 3 ), indium fluoride (InF 3 ), and zinc bromide (ZnBr 2 ) may contain one or more selected from the group consisting of. The chemical formulas written in parentheses after the compound names are representative examples. The composition ratios written in the chemical formulas may be stoichiometric, but do not necessarily have to be stoichiometric.
[0016] The additive 2 may include at least one of polycrystalline and amorphous. The maximum thickness of the additive 2 may be 2 nm or more.
[0017] (Structure of Quantum Dot Addendum) FIG. 2 is a cross-sectional view showing an example of the structure of the quantum dot addendum shown in FIG. 1. As shown in FIG. 2, the addendum 2 may be solid or may include a discontinuous film arranged around the quantum dot QD in a cross section passing through the quantum dot QD. The discontinuous film has one or more discontinuous points in the circumferential direction centered on the quantum dot QD. With this structure, the addendum 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through the discontinuous points of the addendum 2. "Solid" may mean that there is no deficiency of the constituent elements of the addendum 2, or that the deficiency is negligibly small, typically meaning that the size of the deficient region is 5 nm or less. "Discontinuous points" may be regions where one or more of the constituent elements of the addendum 2 are deficient, typically having a size of more than 8 nm. The discontinuous points may penetrate the addendum 2 three-dimensionally. Furthermore, when the addendum 2 for one quantum dot is composed of multiple parts that are separated and independent from each other, the discontinuous points may include gaps between the multiple parts. A "solid discontinuous film" may refer to a film that has discontinuities and is solid in areas other than the discontinuities.
[0018] Furthermore, "surrounding" refers to a region extending around an object (here, quantum dots QDs), and the distance from the object is not particularly limited. However, "surrounding" may refer to a region extending outward from the surface of an object to a given width, or may refer to a region from the quantum dots QDs having a width approximately equal to or less than the distance between adjacent quantum dots QDs. Furthermore, "disposed around" does not necessarily mean continuously surrounding an object, but also includes cases where the object is intermittently surrounded, and cases where the object is disposed in only a portion of the region extending around the object.
[0019] FIG. 3 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in FIG. 1 . As shown in FIG. 3 , the adduct 2 may be solid and may include a continuous film of non-uniform thickness surrounding the quantum dot QD in a cross section passing through the quantum dot QD. The thickness of the adduct 2 is the size in the radial direction centered on the quantum dot QD. With this configuration, the adduct 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through the thin portion of the adduct 2. The minimum thickness of the adduct 2 may be 1 nm or less. By setting the thickness to 1 nm or less, carriers can pass through the thin portion more efficiently, allowing carriers to be injected into the quantum dot QD more efficiently. Furthermore, the entire continuous film may have a thickness of 1 nm or less, allowing carriers to be injected into the quantum dot QD more efficiently. Alternatively, the entire continuous film may be a uniform continuous film with a thickness of 1 nm or less.
[0020] 4 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in FIG. 1. As shown in FIG. 4, the adduct 2 may be porous and may include a continuous film surrounding the quantum dot QDs in a cross section passing through the quantum dot QDs. With this configuration, the adduct 2 protects the quantum dot QDs, and carriers can be injected into the quantum dot QDs through the pores of the adduct 2. The porous pores may be regions in which one or more of the constituent elements of the adduct 2 are deficient, and typically have a size of more than 5 nm and not more than 8 nm. The pores may penetrate the adduct 2 three-dimensionally.
[0021] Figure 5 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in Figure 1. As shown in Figure 5, the adduct 2 may be porous and may include a discontinuous film arranged around the quantum dot QD in a cross section passing through the quantum dot QD. With this configuration, the adduct 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through discontinuities or pores in the adduct 2. A "porous discontinuous film" may mean a film having discontinuities and having porous regions other than the discontinuities.
[0022] 6 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in FIG. 6. As shown in FIG. 6, the adduct 2 may be porous and may include a continuous film with a non-uniform thickness that surrounds the quantum dot QD in a cross section passing through the quantum dot QD. With this configuration, the adduct 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through the pores of the adduct 2 or through thin portions of the adduct 2. The minimum thickness of the adduct 2 may be 1 nm or less.
[0023] 2 to 6 , the quantum dot adduct 1 according to the present disclosure includes a quantum dot QD, an adduct 2 located at least partially around the quantum dot QD, and a compound 4 containing carbon and one or more of hydrogen, nitrogen, and oxygen provided between the quantum dot QD and the adduct 2, wherein the adduct 2 is at least one of a discontinuous film, an uneven thickness, a porous film, and a film having a thickness of 1 nm or less. The quantum dot adduct 1 may further include an element 6 for passivating surface defects of the quantum dot QD. The element 6 may be a halogen.
[0024] (Manufacturing Method) The manufacturing method of the light-emitting element 10 according to the present disclosure may be any manufacturing method, and the light-emitting element 10 may be manufactured using common materials and common film-forming and sealing processes. For example, an alcohol solution in which the quantum dot adduct 1 is dispersed may be applied by spin coating, slit coating, or the like to form the light-emitting layer 14. For example, the quantum dot adduct 1 may be mixed with a solvent for viscosity control, and an ink containing the quantum dot adduct 1 may be printed by inkjet printing, screen printing, or the like to form the light-emitting layer 14. The printing method is suitable for producing light-emitting panels and display panels because it can uniformly form the light-emitting layer 14 over a large area.
[0025] Example 1 A quantum dot adduct 1 and a light-emitting device 10 according to an example of the present disclosure will be described below. A quantum dot adduct 1 and a light-emitting device 10 were prepared using commercially available red quantum dots as the quantum dots QD and zinc chloride (ZnCl ) as the halogen source. 2 ) 0.02 [mol / L] of ethanol (C 2 H 6A solution of 3-(mercaptopropyl)trimethoxysilane (MPS) containing compound 4 and a precursor of adduct 2, and tetramethyl orthosilicate (TMOS) as a precursor of adduct 2 were prepared. The red quantum dots had a core of ZeSeTe and a shell of ZeS, coordinated with an organic ligand different from that of compound 4. The following chemical formula (1) represents MPS, and chemical formula (2) represents TMOS. Octane (C) was used as the solvent. 8 H 18 ) and N-methylformamide (NMF) were prepared.
[0026] 7 and 8 are diagrams illustrating a method for manufacturing a quantum dot adduct according to one embodiment of the present disclosure. As shown in FIG. 7 , a first liquid L1 containing quantum dots (QDs) dispersed in octane was mixed with a zinc chloride ethanol solution and held at room temperature for approximately one hour. Stirring may be performed using a stirrer or similar device. This process inactivates chlorine in the remaining defects (not deactivated by ligands) on the surface of the quantum dots (QDs). In FIG. 7 , active defects are indicated by crosses, and deactivated defects or chlorine in the defects are indicated by circles. In the first liquid L1, chlorine was coordinated to the quantum dots (QDs) in addition to the organic ligands described above. The first liquid L1 could be used directly in subsequent processes, or the first liquid L1 could be centrifuged to separate the quantum dots (QDs) coordinated with the organic ligands and chlorine, which could then be dispersed in pure octane again to form a new first liquid L1 for subsequent processes. A second liquid L2 was also prepared by dissolving MPS and TMOS in NMF. In the first liquid L1, the concentrations of MPS in the second liquid L2 were 0.2 [mol / L] and 0.02 [mol / L] of TMOS.
[0027] Next, as shown in Figure 8, the first liquid L1 and the second liquid L2 were thoroughly stirred and mixed. During the stirring process, the ligands for the quantum dots QDs were exchanged. Specifically, the aforementioned organic ligands were released from the quantum dots QDs, and MPS coordinated to the quantum dots QDs. The thiol groups of MPS easily bond with sulfur (S) vacancies on the shell surface of the quantum dots QDs, and MPS inactivates the defects in the quantum dots QDs. At the same time, halogens also coordinated to the quantum dots QDs, inactivating the defects that MPS could not coordinate. Due to the ligand exchange, the quantum dots QDs no longer dispersed in octane, and the quantum dots QDs migrated from the first liquid L1 to the second liquid L2.
[0028] In the second liquid L2, quantum dot adduct 1 was formed. Specifically, the trimethoxysilane group of MPS and TMOS reacted to synthesize silicon oxide. In addition, some silicon atoms bonded with hydroxyl groups (—OH) and / or some silicon oxide was converted to water (H 2 O) to synthesize silicic acid. An inorganic film containing silicon oxide and silicic acid was disposed at least partially around the quantum dots (QDs). The propyl group of MPS was positioned between the quantum dots (QDs) and adduct 2, resulting in compound 4, which contains carbon and hydrogen.
[0029] Subsequently, the solvent was replaced with alcohol. Specifically, the first liquid L1 was removed, and ethyl acetate was added to the second liquid L2 to precipitate and separate the quantum dot adduct 1. The quantum dot adduct 1 was then dispersed in ethanol. Other alcohols such as methanol and IPA may be used instead of ethanol. The alcohol converts silicon oxide and silicic acid into water (H 2 O) to prevent water from corroding the quantum dots QDs.
[0030] The quantum dot adduct 1 was again precipitated and separated with ethyl acetate, and dispersed in alcohol. Because silicon oxide and silicic acid tend to retain water, it is desirable to repeat alcohol dehydration multiple times. In this example, alcohol dehydration was performed twice. Hereinafter, "the quantum dot adduct according to Example 1" refers to the quantum dot adduct 1 after the second alcohol dehydration.
[0031] Next, the quantum dot adduct 1 according to Example 1 was used to manufacture the light emitting device 10 according to Example 1, and the device characteristics and service life of the light emitting device 10 were measured. In addition, a solution of the quantum dot adduct 1 according to Example 1 was analyzed by Fourier transform infrared spectroscopy (FTIR).
[0032] Comparative Example 1 In Comparative Example 1, the commercially available red quantum dots described above were used instead of the quantum dot adduct 1, and otherwise a light-emitting device according to Comparative Example 1 was manufactured in the same manner as the light-emitting device 10 according to Example 1, and the device characteristics and service life were measured. In addition, a solution of the commercially available red quantum dots was analyzed by Fourier transform infrared spectroscopy (FTIR). Hereinafter, "quantum dots according to Comparative Example 1" refers to the commercially available red quantum dots.
[0033] (Comparative Example 2) In Comparative Example 2, the TMOS concentration was increased tenfold compared to Example 1, and otherwise a quantum dot-adduct according to Comparative Example 2 was produced in the same manner as quantum dot-adduct 1 according to Example 1. Then, using the quantum dot-adduct according to Comparative Example 2, a light-emitting device according to Comparative Example 2 was produced in the same manner as light-emitting device 10 according to Example 1, and the device characteristics were measured. In addition, a solution of the quantum dot-adduct according to Comparative Example 2 was analyzed by Fourier transform infrared spectroscopy (FTIR).
[0034] 9 to 12 are graphs showing the element characteristics (voltage-luminance characteristics, voltage-current density characteristics, current density-luminance characteristics, and current density-luminous efficiency characteristics) of the light-emitting elements according to Example 1 and Comparative Examples 1 and 2. In each figure, points for Example 1, Comparative Example 1, and Comparative Example 2 are shown as triangles, circles, and diamonds, respectively, and the points are connected by solid lines.
[0035] 9 to 12, the EQE (external quantum efficiency) of Example 1 is significantly higher than that of Comparative Example 2. The EQE of Example 1 is approximately 2%, while the EQE of Comparative Example 2 is nearly 0%. Since the light-emitting devices of Example 1 and Comparative Example 2 have the same configuration except for the quantum dot adduct, the difference in EQE is presumed to be due to the efficiency of carrier injection into the quantum dot adduct (more precisely, the quantum dots therein).
[0036] Although the quantum dots QDs are protected by insulating silicon oxide, the light-emitting device according to Example 1 has a turn-on voltage in the luminance-voltage characteristics (see FIG. 9 ) that is only about 2 V higher than that of Comparative Example 1. Furthermore, similar to Comparative Example 1, the luminance of the light-emitting device according to Example 1 increases with increasing voltage at voltages higher than the turn-on voltage. This result is thought to indicate that in Example 1, the additive 2 protecting the quantum dots QDs is at least one of a discontinuous film, an uneven thickness, a porous film, and a film having a thickness of 1 nm or less, and therefore no excessive voltage is required for carrier transport to the QDs.
[0037] On the other hand, the light-emitting device according to Comparative Example 2 showed a tendency for its luminance to decrease in the high voltage region of 14 V or more, which is presumably due to the influence of heat loss proportional to the square of the voltage. Therefore, the luminance and EQE of Comparative Example 2 were significantly lower than those of Example 1, and it is considered that protecting the quantum dots by introducing an excessive amount of TMOS as in Comparative Example 2 is not suitable for practical use.
[0038] 13 and 14 are graphs showing the emission luminance and driving voltage over time of the light-emitting elements according to Example 1 and Comparative Example 1 in a constant current test. The horizontal axis in each diagram indicates time from the start of light emission. The left vertical axis indicates relative luminance, with the emission luminance of each light-emitting element at the start of light emission taken as 100%. The right vertical axis indicates relative voltage, with the driving voltage of each light-emitting element at the start of light emission taken as 100%. In each diagram, the relationship between luminance and time is shown by a solid line, and the relationship between voltage and time is shown by a dashed line. In this constant current test, a current of 25 mA / cm was applied to the light-emitting elements. 2 A current of 295 [cd / m s] was applied at 25° C. In addition, the light emitting device 10 according to Example 1 had a luminance of 295 [cd / m s] at the start of light emission in this constant current test. 2 ], and the light emitting device according to Comparative Example 1 had a luminance of 157 [cd / m 2 〕 was the case.
[0039] As shown in FIG. 13, the light-emitting device according to Example 1 exhibited a characteristic in which the luminance increased from the start of emission until about 20 hours later (so-called "positive aging"). This is thought to be due to the improvement in the EQE according to Example 1 due to the application of current. The luminance was about 295 [cd / m 2 ] to about 1474 [cd / m 2 ], which is a significant improvement of about 5 times, or EQE equivalent to the initial 2% to 10%. Note that the light extraction efficiency of a light-emitting element is determined by the refractive index of each material, and the light extraction efficiency of light-emitting elements using a glass substrate and a general organic carrier transport material, metal oxide, etc. does not exceed 20%. Therefore, in the light-emitting element of Example 1, the IQE (internal quantum efficiency) after 20 hours of application of electricity exceeds 50%.
[0040] This positive aging is a phenomenon specific to Example 1, and is thought to be the result of the halogen or MPS present in a free state inside the additive 2 gradually inactivating the surface defects of the quantum dots QDs through electrochemical reactions or electrophoresis caused by the passage of electricity.
[0041] 14, the light-emitting device according to Comparative Example 1 does not exhibit positive aging, and the luminance rapidly and monotonically decreases with the passage of current. 2 ] to about 13 [cd / m 2 ], which is approximately one-twelfth of the original value. This is thought to be because the quantum dots of Comparative Example 1 were only protected by organic ligands, and so degradation progressed rapidly when a current was applied. The degradation may include degradation of the organic ligand itself or dissociation of the organic ligand from the quantum dots. Because the degradation was so rapid, it is thought that practical use in display panels and the like would be difficult.
[0042] For the relationship between luminance and time in Example 1, a fitting function using the least squares method was applied to the measured values from 20 hours to 130 hours so that the application results would form a straight line on a semi-logarithmic graph. For the relationship between luminance and time in Comparative Example 1, a fitting function using the least squares method was similarly applied to the measured values from 20 hours to 130 hours so that the application results would form a straight line on a semi-logarithmic graph. LT50 and LT95 were calculated from the application results. "LT95" indicates an estimated value of the lifetime until the emission luminance of the light-emitting element reaches 95% of its initial value, and "LT50" indicates an estimated value of the lifetime until the emission luminance of the light-emitting element reaches 50% of its initial value.
[0043] 15 and 16 are diagrams showing estimated values of useful life of the light emitting elements according to Example 1 and Comparative Example 1, respectively. Generally, in a nanoLED, the initial value of the light emission luminance is L 0 The lifetime LT(x, P) until the luminance reaches x [%] of the initial value when (P) is reached, and the initial value of the luminance is L 0 (Q) and the lifetime LT(x, Q) until the luminance reaches x [%] of the initial value. 0 (P), L 0 It is known that the following relational expression holds regardless of (Q) and x: This relational expression is called the "reliability calculation formula."
[0044] LT(x, P) × {L 0 (P)} n =LT(x,Q)×{L 0 (Q)} n = constant n is a coefficient that depends on the nanoLED, and n=1.8.
[0045] As shown in FIGS. 15 and 16, when the initial luminance is 100 [cd / m 2 ], the L50 of Comparative Example 1 was about 0.1 hours, whereas the LT50 of Example 1 was about 23,000 hours, achieving reliability more than 100,000 times higher. Therefore, Example 1 was able to improve the efficiency of carrier injection into the quantum dots QD, thereby realizing a light-emitting element 10 with a high EQE and a long service life.
[0046] In Non-Patent Document 1, quantum dots are completely covered with a dense continuous film of silicon oxide. According to Non-Patent Document 1, reliability is improved compared to light-emitting devices using quantum dots protected only with organic ligands, but only by about three times. In the light-emitting device containing quantum dots described in Non-Patent Document 1, positive aging due to current flow is thought to be unlikely because only a small amount of organic ligand is present inside the continuous film. Furthermore, since carrier injection into quantum dots in Non-Patent Document 1 is via π electrons of organic cyclic molecules mixed into silicon oxide, it is speculated that the number of carriers actually injected into the quantum dots is insufficient. Furthermore, since carrier injection into quantum dots in Non-Patent Document 1 is via organic molecules, it is speculated that even cyclic molecules are unable to reduce degradation due to electrochemical reactions.
[0047] 17 to 19 are diagrams showing the results of FTIR (Fourier transform infrared spectroscopy) of the quantum dot adduct of Example 1, the quantum dots of Comparative Example 1, and the quantum dot adduct of Comparative Example 2, respectively. As shown in FIG. 18, in Comparative Example 1, only a peak corresponding to the C-H bond of the organic ligand is observed. On the other hand, as shown in FIGS. 17 and 19, in Example 1 and Comparative Example 2, in addition to the peak corresponding to the C-H bond, a peak corresponding to the Si-O bond of silicon dioxide is observed in the range of 1000 to 1200 [cm -1 ], and a broad peak corresponding to the Si-OH bond of silicic acid is observed at 2600 to 3600 [cm -1 ]. Therefore, it can be seen that in Example 1 and Comparative Example 2, the quantum dots are protected by an inorganic film containing silicon dioxide and silicic acid, while in Comparative Example 1, the quantum dots are not protected by an inorganic film. Hereinafter, for the sake of simplicity, the "peak corresponding to the ... bond" will be referred to as the "... peak."
[0048] Furthermore, while the C—H peaks in Example 1 and Comparative Example 2 have similar intensities, the intensities of the Si—O and Si—OH peaks are different. Compared to Example 1, the Si—O peak intensity in Comparative Example 2 is increased by about three times, and the Si—OH peak intensity is increased by about 1.5 times. Because the TMOS concentration in Comparative Example 2 was 10 times that of Example 1, it is believed that excess TMOS was consumed in the reaction producing silicic acid in Comparative Example 2, resulting in the production of excess silicic acid.
[0049] Silicon oxide naturally (i.e., when only silicon oxide is produced) forms a dense and continuous inorganic film. Silicic acid is insoluble in acid and inhibits the synthesis of silicon oxide. Therefore, an appropriate amount of silicic acid helps form an inorganic film containing silicon oxide and silicic acid so that the inorganic film is at least one of discontinuous, non-uniform in thickness, porous, and / or has portions with a thickness of 1 nm or less. On the other hand, excess silicic acid forms a dense and continuous film with silicon dioxide, surrounding the quantum dots (QDs). Thus, silicic acid plays an important role in protecting and insulating the quantum dots (QDs). The amount of silicic acid produced can be adjusted by the amounts of MPS and TMOS.
[0050] It is estimated that Example 1 contains an appropriate amount of silicic acid, and the inorganic film containing silicon oxide and silicic acid is at least one of a discontinuous film, a non-uniform thickness, a porous film, and a film having a thickness of 1 nm or less, whereas Comparative Example 2 contains an excessive amount of silicic acid, and the inorganic film containing silicon oxide and silicic acid is a dense, thick, continuous film.
[0051] In Non-Patent Document 1, the results of FTIR are about 800 to 3200 [cm -1 ] range, but 3200 [cm -1], it is believed that the material in Non-Patent Document 1 does not contain silicic acid. Furthermore, in Non-Patent Document 1, the quantum dots are protected with silicon dioxide, and the intensity of the C-H peak is similar to the intensity of the Si-O peak, indicating the presence of cyclic organic molecules that contribute to carrier injection into the quantum dots. In contrast, in Example 1 of the present disclosure, the intensity of the C-H peak is less than one-tenth of the Si-O peak, and in Comparative Example 2, the intensity of the C-H peak is less than one-half of the Si-O peak. Therefore, it is believed that the inorganic films of Example 1 and Comparative Example 2 do not contain organic cyclic structures or contain only trace amounts, and that cyclic organic molecules do not contribute to carrier injection into the quantum dots. In particular, the C-H peak in Example 1 is very weak, completely different from that in Non-Patent Document 1.
[0052] [Embodiment 2] Another embodiment of the present disclosure will be described below. For ease of explanation, the same reference numerals will be used to designate components having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0053] Fig. 20 is a cross-sectional view showing an example of the configuration of a display device according to an embodiment of the present disclosure. As shown in Fig. 20, a display device 100 according to the present disclosure includes a light-emitting element 10 according to an embodiment of the present disclosure. The light-emitting element 10 may be the light-emitting element 10 described in the first embodiment above, or may be an improved or modified version of the light-emitting element 10 described in the first embodiment above.
[0054] The display device 100 may include a display unit 30 including a plurality of sub-pixels X, and a driver circuit 25 that drives the plurality of sub-pixels X. At least one of the plurality of sub-pixels X may include a light-emitting element 10 and a pixel circuit 20.
[0055] The present disclosure is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present disclosure.
[0056] REFERENCE SIGNS LIST 1 quantum dot adduct 2 adduct 4 compound 10 light emitting element 12 first electrode 14 light emitting layer 16 second electrode 100 display device QD quantum dot
Claims
1. A light-emitting device comprising: a first electrode and a second electrode facing each other; and a light-emitting layer provided between the first electrode and the second electrode, the light-emitting layer including quantum dots and an additive located at least partially around the quantum dots, and a compound including carbon and one or more of hydrogen, nitrogen and oxygen provided between the quantum dots and the additive, the additive being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion having a thickness of 1 nm or less.
2. The light-emitting element according to claim 1, wherein the compound is bonded to a metal element contained in the quantum dot via a thiol bond or has a thiol group.
3. The light-emitting element according to claim 1 or 2, wherein the compound has 3 or more and 5 or less carbon atoms.
4. The light-emitting element according to any one of claims 1 to 3, wherein the band gap of the additive is wider than the band gap of the material constituting the quantum dots.
5. The light-emitting element according to claim 4, wherein the quantum dot has a core and a shell surrounding the core, and the band gap of the additive is wider than the band gap of a material constituting the shell.
6. The light-emitting device according to claim 4 or 5, wherein the attachment is insulating.
7. The light-emitting element according to any one of claims 1 to 6, wherein the additive contains silicon oxide.
8. The light-emitting device according to claim 7, wherein the additive comprises silicic acid.
9. The light-emitting element according to any one of claims 1 to 6, wherein the additive contains titanium oxide.
10. The light-emitting element according to any one of claims 1 to 6, wherein the additive contains aluminum oxide.
11. The light-emitting device according to any one of claims 1 to 6, wherein the additive contains zinc chloride.
12. The light-emitting device according to any one of claims 1 to 6, wherein the additive comprises silicon nitride.
13. The light-emitting element according to any one of claims 1 to 6, wherein the additive comprises one selected from the group consisting of boron oxide, phosphorus oxide, germanium oxide, beryllium fluoride, arsenic sulfide, silicon selenide, germanium sulfide, tellurium oxide, bismuth oxide, vanadium oxide, antimony oxide, lead oxide, copper oxide, zirconium fluoride, aluminum fluoride, indium fluoride, and zinc bromide.
14. The light-emitting device according to any one of claims 1 to 12, wherein the additive includes at least one of polycrystalline and amorphous.
15. The light-emitting element according to claim 14, wherein the maximum thickness of the additive is 2 nm or more.
16. The light-emitting device according to any one of claims 1 to 15, wherein the additive is porous.
17. The light-emitting device according to claim 16, wherein the appendage comprises a continuous film surrounding the quantum dot at a cross section through the quantum dot.
18. The light-emitting device according to any one of claims 1 to 15, wherein the attachment is solid.
19. The light-emitting device according to claim 16 or 18, wherein the appendage comprises a discontinuous film disposed around the quantum dot in a cross section through the quantum dot.
20. The light-emitting device according to claim 16 or 18, wherein the appendage comprises a continuous film of non-uniform thickness surrounding the quantum dot in a cross section through the quantum dot.
21. The light-emitting element according to claim 20, wherein the minimum thickness of the additive is 1 nm or less.
22. A display device comprising the light-emitting element according to any one of claims 1 to 21.
23. A quantum dot adduct comprising: a quantum dot; an adduct located at least partially around the quantum dot; and a compound containing carbon and containing one or more of hydrogen, nitrogen, and oxygen, provided between the quantum dot and the adduct, wherein the adduct is at least one of a discontinuous film, has a non-uniform thickness, is porous, and has a portion having a thickness of 1 nm or less.
Citation Information
Patent Citations
Core-shell perovskite quantum dot and preparation method thereof, quantum dot composition and quantum dot device with quantum dot composition
CN112521933A
Semiconductor structures having polymer and insulator coatings, and compositions and methods for forming same
JP2020507801A
Light emitting device