Metal material and sliding component

The use of an amorphous Ni plating layer on one metal material and a crystalline Ni layer on another in sliding parts addresses wear issues, enhancing wear resistance and reducing transmission loss for high-frequency applications.

WO2024202237A1PCT designated stage expired Publication Date: 2024-10-03JX ADVANCED METALS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/042409
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-11-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Metal materials used in sliding parts often experience significant wear when rubbed against other metal materials, leading to reduced performance and lifespan, particularly in high-frequency applications where low friction and corrosion resistance are crucial.

Method used

A metal material with a base material and a plating layer, where the plating layer includes an amorphous Ni layer and the opposing material has a crystalline Ni layer, which provides excellent wear resistance by suppressing wear through the difference in hardness between the two layers.

Benefits of technology

The solution effectively reduces wear and transmission loss, making the metal materials suitable for high-frequency applications with improved durability and performance in sliding components like connectors and switches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023042409_03102024_PF_FP_ABST
    Figure JP2023042409_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This metal material 1 has a base material 2 and a plating layer 3 formed on the base material 2. The plating layer 3 contains an amorphous layer 4 containing Ni. The metal material 1 is used for a sliding component 101 that slides, at the surface 5 of the plating layer 3, against the surface 55 of another metal material 51. The other metal material 51 includes a crystalline layer 54 containing Ni.
Need to check novelty before this filing date? Find Prior Art

Description

Metal materials and sliding parts

[0001] This specification discloses a technique relating to a metal material having a plated layer formed on a substrate and a sliding part.

[0002] In sliding parts in which one metal material slides against another metal material during use, such as connectors, switches, gears, bearings, washers, etc., the metal material may have a plating layer formed on the base material in order to suppress metal diffusion, etc.

[0003] In this regard, for example, Patent Document 1 states that "...nickel-phosphorus alloy coatings, among others, have characteristics such as high corrosion resistance, high lubricity, high hardness, and high resistivity, and are used as plating coatings for sliding members and piping equipment used under severe conditions, as well as being widely used as thin-film resistors in the electronics industry or as a substitute for gold in connectors."

[0004] Furthermore, Patent Document 2 states that "from the bath of Composition Example 1 (paragraph

[0016] ), a Ni-P alloy-CNT composite plating having a high phosphorus concentration, so-called high-phosphorus type (P concentration: 12 to 13 mass%), is obtained, and these composite plating films exhibit a low coefficient of friction and high hardness. On the other hand, in terms of electromagnetic wave shielding properties, a film in which CNT is composited with a low-phosphorus type Ni-P alloy (P concentration: 2 to 4 mass%) is desired."

[0005] JP 03-010086 A JP 2010-215977 A

[0006] The metal materials used in the above-mentioned sliding parts are required to have excellent wear resistance, so that the plating layer is unlikely to wear even when other metal materials are repeatedly rubbed against them.

[0007] This specification provides a metal material having excellent wear resistance and a sliding part in which wear of the metal material is suppressed.

[0008] The metallic material disclosed in this specification has a substrate and a plating layer formed on the substrate, the plating layer including an amorphous layer containing Ni, and the metallic material is used in a sliding part in which the surface of the plating layer slides against the surface of another metallic material, the other metallic material including a crystalline layer containing Ni.

[0009] Another metal material disclosed in this specification has a substrate and a plating layer formed on the substrate, the plating layer including an amorphous layer, and the metal material is used in a sliding part that slides on the surface of the plating layer against the surface of another metal material, the other metal material including a crystalline layer that is softer than the amorphous layer.

[0010] The sliding component disclosed in this specification comprises a first metal material and a second metal material, wherein the first metal material has a substrate and a plating layer formed on the substrate, the plating layer of the first metal material includes an amorphous layer containing Ni, and the second metal material includes a crystalline layer containing Ni, and the first metal material and the second metal material are used by sliding against each other on their respective surfaces.

[0011] The above-mentioned metal material has excellent wear resistance, and the above-mentioned sliding component is one in which wear of the metal material is suppressed.

[0012] 1 is a partial cross-sectional view taken along a direction perpendicular to the surface, schematically illustrating a metal material according to an embodiment; FIG. 2 is a similar cross-sectional view schematically illustrating the sliding behavior of the metal material of FIG. 1 and another metal material when used as sliding components; FIG. 3 is a similar cross-sectional view showing another example of a plating layer formed on a metal material substrate; FIG. 4 is a schematic diagram illustrating a microstrip line of a sample used in measuring the transmission loss of a metal material; FIG. 5 is a diagram illustrating the shape and dimensions of a terminal and a flat plate used in Test Example 1; FIG. 6 is a graph illustrating the relationship between frequency and transmission loss for each metal material in Test Example 2; FIG. 7 is a graph illustrating the relationship between frequency and transmission loss for each metal material in Test Example 3; and FIG. 8 is a TEM image and a diffraction image of each metal material in Test Example 4.

[0013] The following describes in detail embodiments of the above-mentioned metal material and sliding component. The metal material 1 shown in Fig. 1 has a substrate 2 and a plating layer 3 formed on the substrate 2. The metal material 1 is used in a sliding component 101 together with another metal material 51, as shown in Fig. 2.

[0014] In many cases, the other metallic material 51 is formed by forming a plating layer 53 on a base material 52, like the metallic material 1. However, the plating layer 3 of the metallic material 1 includes an amorphous layer 4. On the other hand, the other metallic material 51 includes a crystalline layer 54. In one embodiment, the amorphous layer 4 of the metallic material 1 and the crystalline layer 54 of the other metallic material 51 both contain Ni. In another embodiment, the crystalline layer 54 of the other metallic material 51 is softer than the amorphous layer 4 of the metallic material 1. The sliding component 101 is used by sliding the metallic material 1 and the other metallic material 51 on the surfaces 5, 55 of the plating layers 3, 53, respectively, as shown by the arrows in FIG. 2 .

[0015] As described above, a new finding has been obtained: when the plating layer 3 of the metal material 1 includes an amorphous layer 4, while the other metal material 51 that slides against it includes a crystalline layer 54, and when the amorphous layer 4 and the crystalline layer 54 contain Ni and / or the crystalline layer 54 is softer than the amorphous layer 4, the metal material 1 and the other metal material 51 exhibit excellent wear resistance. In this case, as will be described in detail later in the Examples section, wear of the plating layers 3, 53 is significantly suppressed when the metal material 1 slides against the other metal material 51. Therefore, the metal material 1 of the embodiment described here exhibits excellent wear resistance, and the sliding component 101 can be said to be one in which wear of the metal materials 1, 51 is suppressed.

[0016] Here, when it is necessary to distinguish between the two metal materials 1, 51 included in the sliding element 101, one of them, the metal material 1, will be referred to as the "metal material" or the "first metal material," and the other metal material 51 will be referred to as the "other metal material" or the "second metal material." In a description common to both the two metal materials 1, 51, they may be simply referred to as the "metal material."

[0017] (Substrate) The material of the substrate 2, 52 of the metal material 1, 51 is not particularly limited and may be any metal or alloy. The material of the substrate 2, 52 may be, for example, Cu (copper), Al (aluminum), Fe (iron), or an alloy containing at least one of these.

[0018] From the viewpoint of having high conductivity and strength, the material of the substrates 2, 52 is preferably Cu or a Cu alloy, more specifically, phosphor bronze, brass, Corson copper, oxygen-free copper, tough pitch copper, etc. In particular, the materials of the substrates 2, 52 may be C11000, C10200, C19400, C70250, C26000, C52100, etc., as specified by the Copper Development Association (CDA).

[0019] The substrate 2 of the metal material 1 and the substrate 52 of the other metal material 51 may be made of the same material, but may also be made of different materials. The dimensions and shapes of the substrates 2 and 52 may be changed as appropriate depending on the sliding part in which the metal materials 1 and 51 are used.

[0020] (Amorphous Layer) The amorphous layer 4 constitutes at least a part of the plating layer 3 of the metal material 1. Typically, the amorphous layer 4 contains Ni (nickel) as a main component, which is an element of more than 50 mass %, but is not limited thereto.

[0021] The Ni-containing amorphous layer 4 preferably further contains P (phosphorus). The Ni-P amorphous layer 4 has a dense amorphous structure (non-crystalline structure), and therefore tends to be harder than the crystalline layer 54 described below, which contains mainly Ni. The metal material 1, which is used in sliding contact with another metal material 51 including a crystalline layer 54 whose main component is Ni, preferably contains Ni and P.

[0022] Furthermore, the amorphous layer 4 containing Ni and P is non-magnetic, and therefore exhibits small dielectric loss in transmission loss. Therefore, the metal material 1 including such an amorphous layer 4 is particularly suitable for use in high-frequency components, as described below, in which a predetermined high-frequency internal signal flows, among other sliding components 101.

[0023] The amorphous layer 4 containing Ni and P often has an amorphous structure when the P content is 8% by mass or more. The P content of the amorphous layer 4 is preferably 8% by mass to 15% by mass. If the P content is 15% by mass or less, it is possible to suppress a decrease in the electrical conductivity of the amorphous layer 4 due to the inclusion of P. More preferably, the P content is 10% by mass to 13% by mass.

[0024] Furthermore, when the amorphous layer 4 contains Ni, it is also preferable that it further contains W (tungsten). This is because the Ni-W amorphous layer 4 also has a dense amorphous structure and is harder than the Ni crystalline layer 54, and is expected to have the effect of improving wear resistance, similar to Ni-P. The W content of the amorphous layer 4 containing Ni and W is preferably 20% to 40% by mass. Furthermore, when the amorphous layer 4 contains Ni, it may further contain P and W.

[0025] To measure the P content, an electron probe microanalyzer (EPMA, JXA-8500F manufactured by JEOL Ltd.) can be used. More specifically, the X-ray intensity at the P peak position (197.235 mm) is measured for each of the standard specimen and the sample using the electron probe microanalyzer, and the P content is calculated using the formula: P content (at%) = (average value of X-ray intensity of sample) ÷ (average value of X-ray intensity of standard specimen) × 50. The measurement conditions for the standard specimen are as follows: standard specimen: InP wafer (P content 50 at%), crystal used: PETH, X-ray used: Kα, acceleration voltage: 15 kV, irradiation current: 1 × 10 -7 A, and a beam diameter of 10 μm. Under these measurement conditions, the X-ray intensity at the P peak position (197.235 mm) of the standard sample is measured five times, and the average value is calculated. For the sample measurement, the central portion of the sample, which is the metal material 1 having an amorphous layer 4 formed on a substrate 2, is measured five times under the same measurement conditions as the standard sample, and the average X-ray intensity at the P peak position (197.235 mm) is calculated. The W content can be measured by TEM-EDX (energy dispersive X-ray spectroscopy) using a JEM-2100F manufactured by JEOL Ltd. More specifically, the W content is measured at the central portion of the Ni-W layer in the thickness direction. Measurement of the W content by TEM-EDX (energy dispersive X-ray spectroscopy) can be performed as follows. Equipment (TEM): JEOL Ltd., field emission transmission electron microscope (JEM-2100F) Equipment (EDX): JEOL Ltd., energy dispersive X-ray analyzer (JED-2300T) STEM image observation + EDX analysis Mode: STEM mode Acceleration voltage: 200 kV Spot size: 0.15 nm Magnification: 80,000 times

[0026] In the amorphous layer 4 containing Ni and P or W, the remainder other than P or W is often substantially composed of Ni, but at least one element selected from the group consisting of Cu, Pb, and Zn may be contained as an impurity in a total amount of 15 mass ppm or less.

[0027] The amorphous structure of the amorphous layer 4 can be confirmed by processing a cross section of the metal material 1 using an FIB-SIM (SMI3050SE manufactured by Hitachi High-Tech Corporation) and observing the cross section using a TEM (JEM-2100F manufactured by JEOL Ltd.).

[0028] The amorphous layer 4 of the metal material 1 may be harder than the crystalline layer 54 of the other metal material 51. The Vickers hardness of the amorphous layer 4 may be 500 Hv to 600 Hv. The Vickers hardness of the crystalline layer 54 will be described later, but the difference in Vickers hardness between the amorphous layer 4 and the crystalline layer 54 is preferably 100 Hv or more, more preferably 150 Hv or more, and particularly preferably 150 Hv to 300 Hv. It is believed that wear of the metal materials 1, 51 during sliding on the sliding component 101 is suppressed due to such a difference in hardness between the amorphous layer 4 and the crystalline layer 54.

[0029] The Vickers hardness of the amorphous layer 4 and the crystalline layer 54 can be measured using a microhardness tester MHT-2 manufactured by Matsuzawa Seiki Mfg. Co., Ltd. (currently Matsuzawa Corporation). More specifically, the metal materials 1 and 51 are embedded in acrylic resin while standing vertically, then scraped down to the measurement point and polished. After that, a square pyramidal diamond indenter is pressed into the amorphous layer 4 and the crystalline layer 54, and the diagonal length of the depression created after the test force is released is measured. The test conditions are a test force of 500 gf and a holding time of 10 seconds, and the diagonal length measurement is the average of the X and Y measurements. The median of five measurements is used as the measurement value, and the hardness is calculated from a Vickers hardness calculation table based on this median and the test force.

[0030] The thickness of the amorphous layer 4 is preferably 1 μm to 6 μm. If the thickness of the amorphous layer 4 is less than 1 μm, pits and pinholes are likely to occur, which may result in reduced corrosion resistance. On the other hand, if the thickness of the amorphous layer 4 exceeds 6 μm, there is a concern that cracks may occur when the metal material 1 is bent due to the hardness of the amorphous layer 4. The thickness of the amorphous layer 4 can be measured using a fluorescent X-ray film thickness meter. The thickness of layers other than the amorphous layer 4 in the plating layer 3, as well as the thickness of other plating layers described below, can also be measured in a similar manner. Measurement of plating thickness using a fluorescent X-ray film thickness meter can be performed as follows. Apparatus: FT9500X fluorescent X-ray film thickness meter manufactured by Hitachi High-Tech Corporation X-ray tube: Mo Detector: Drift-type semiconductor detector X-ray optical system: Polycapillary method Beam diameter (diameter): 30 μm Measurement method: Thin film FP (fundamental parameter) method

[0031] In order to form the amorphous layer 4 on the substrate 2 during the production of the metal material 1, for example, a plating bath is used for the substrate 2 as a nickel sulfate bath, and nickel (II) sulfate hexahydrate or the like is added to the nickel sulfate concentration of 205 g / L to 295 g / L, a phosphorous acid concentration of 68 g / L to 95 g / L, and a current density of 7 A / dm 2 ~13 A / dm 2 The amorphous layer 4 can be formed by setting the solution temperature at 55° C. to 65° C. Alternatively, the amorphous layer 4 can be formed by electroless plating instead of electrolytic plating.

[0032] (Crystalline Layer) When the other metal material 51 is a plated layer 53 formed on a base material 52 , at least a portion of the plated layer 53 includes a crystalline layer 54 .

[0033] The crystalline layer 54 has, for example, the same main component as the main component of the amorphous layer 4, and typically contains Ni as the main component, but is not limited to this. Furthermore, in this case, the Ni content may be approximately 100 mass % and the crystalline layer 54 may be made of only Ni. However, the crystalline layer 54 may also contain other elements. The Ni content can be measured using an electron probe microanalyzer (EPMA, JXA-8500F manufactured by JEOL Ltd.).

[0034] The crystalline layer 54 may be softer than the above-described amorphous layer 4. The Vickers hardness of the crystalline layer 54 may be 200 Hv to 400 Hv.

[0035] The thickness of the crystalline layer 54 is preferably 1 μm to 6 μm. If the thickness of the crystalline layer 54 is less than 1 μm, pits and pinholes are likely to occur, which may result in reduced corrosion resistance. On the other hand, if the thickness of the amorphous layer 4 exceeds 6 μm, there is a concern that cracks may occur when the other metal material 51 is bent.

[0036] The crystalline layer 54 can be formed by, but not limited to, applying matte, semi-bright, or roughened Ni plating to the substrate 52. For example, a nickel sulfamate plating solution may be used as the plating solution, and the current density may be 3 A / dm 2 ~20 A / dm 2 The liquid temperature may be set to 40°C to 60°C.

[0037] (Outermost layer) The plating layer 3, 53 of the metal material 1, 51 may include an outermost layer containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd, and Cu. For example, Fig. 3 shows an example of the metal material 11 in which an outermost layer 16 is further formed on an amorphous layer 14 on a substrate 12. Note that an outermost layer may also be formed on other metal materials.

[0038] In this case, the outermost layer 16 is exposed on the surface 15 of the plating layer 13, and since the outermost layer 16 made of the above-mentioned material is relatively soft and thin, it is thought that it will have almost no effect on wear resistance. When the outermost layer 16 is provided, transmission loss can be further reduced due to high electrical conductivity, making the metal material 11 even more suitable for use in sliding parts that are also high-frequency parts. This is because the influence of the skin effect is strong in high-frequency parts.

[0039] The thickness of the outermost layer 16 may be 0.005 μm to 5 μm. If the thickness of the outermost layer 16 is too thin, the transmission loss may not be reduced significantly, whereas if the thickness is too thick, there is a concern that the transmission loss may not change, that there may be a slight effect on the abrasion resistance, and that the cost of precious metals may increase.

[0040] For example, if the outermost layer 16 is formed with Au-Co plating (hard plating), the Au content of the outermost layer 16 may be approximately 99.7% by mass. Alternatively, if the outermost layer 16 is formed with pure Au plating (soft plating), the Au content of the outermost layer 16 may be approximately 100% by mass. Alternatively, if the outermost layer 16 contains another metal (Ag, Sn, Pd, or Cu), the content of that metal may be approximately 100% by mass. Alternatively, the outermost layer 16 may further contain Co, such as Au-Co. It is also possible to form two or more outermost layers made of different materials. The metal content of the outermost layer 16 can be measured using X-ray photoelectron spectroscopy (XPS, ULVAC-PHI 5600MC). The XPS measurement conditions can be as follows: ultimate vacuum: 5.7 x 10 -7 Pa Detection diameter: 800 μm Excitation source: MgK Output: 400 W Incident angle: 81 degrees Take-off angle: 45 degrees Neutralization gun: None Sputtering conditions Ion species: Ar+ Acceleration voltage: 2 kV Sweep area: 3 mm × 3 mm Rate: 1.7 nm / min (SiO2 equivalent)

[0041] During the production of the metal material 11, in order to form the outermost layer 16, the substrate 12 on which the amorphous layer 14 has been formed can be plated using an appropriate plating solution depending on the material of the outermost layer 16. As the plating solution, for example, Silbrex Bright HS manufactured by EEJA can be suitably used in the case of the outermost layer 16 containing Ag, and a hard Au plating solution can be suitably used in the case of the outermost layer 16 containing Au. For example, in Ag plating, the current density is set to 5 A / dm 2 ~25 A / dm 2 The solution temperature may be set to 30 to 60°C. For example, in Au plating, the current density is set to 5 A / dm 2 ~60 A / dm2 The liquid temperature may be set to 50°C to 60°C.

[0042] (Transmission Loss) The metal material 1 has low transmission loss, and preferably has an absolute value of 4 dB or less when a current of a frequency of 10 GHz is passed through it. Transmission loss is often measured as a negative value, and the smaller the absolute value is and the closer to zero it is, the smaller the transmission loss is, and the more desirable the metal material 1 is for the sliding part 101, which is also a high-frequency part.

[0043] The transmission loss of the metal material 1 can be measured using a network analyzer. More specifically, as shown in FIG. 4 , a microstrip line is used as the sample to be set in the network analyzer. The microstrip line includes a copper foil on which a dielectric layer is provided, and copper wiring with a plating layer formed around the periphery of the dielectric layer. This sample is prepared by bonding a metal foil made of the material of the substrate 2 to each side of the dielectric layer using a heat press at 300°C. Then, the metal foil on one side is turned into wiring by circuit etching, and plating corresponding to the plating layer 3 is applied around the wiring. The wiring corresponds to the substrate. This sample is set in a network analyzer (Keysight N5247A) to measure the transmitted and reflected power of an AC current passed through the sample. The transmission loss can be calculated from the voltages P1 and P2 measured using the formula: Transmission loss = 10 × log(P2 / P1). Measurements are performed on four microstrip lines of the sample, and the average of the measured values ​​is taken as the transmission loss.

[0044] (Sliding Component) The sliding component 101 includes a first metallic material 1 as the metallic material 1 and a second metallic material 51 as another metallic material 51 .

[0045] In the sliding part 101, the surface 5 of the plating layer 3 of the first metal material 1 and the surface 55 of the plating layer 53 of the second metal material 51 are pressed together in a direction perpendicular to the surfaces 5 and 55 (the up-down direction in Figure 2), and as shown in Figure 2, the first metal material 1 and the second metal material 51 may be displaced relatively in opposite directions to each other in a direction roughly along the surfaces 5 and 55 (the left-right direction in Figure 2).

[0046] When the first metallic material 1 and the second metallic material 51 are caused to slide against each other on the surfaces 5, 55 of the plating layers 3, 53 in this manner, the plating layers 3, 53 may rub against each other and wear. In contrast, as described above, when the plating layer 3 of the first metallic material 1 includes the amorphous layer 4 and the plating layer 53 of the second metallic material 51 includes the crystalline layer 54, and when the amorphous layer 4 and the crystalline layer 54 contain Ni and / or the crystalline layer 54 is softer than the amorphous layer 4, wear of the plating layers 3, 53 can be effectively suppressed.

[0047] If one of the metal materials 1 or 51 in the sliding component 101 has a convex portion protruding toward the surface 55 or 5 of the opposing metal material 51 or 1, it is preferable that the first metal material 1 has a convex portion provided on the surface 5. This is because, when the first metal material 1 including the hard amorphous layer 4 is provided with a convex portion and is caused to slide against the second metal material 51 including the soft crystalline layer 54, wear is suppressed compared to when the second metal material 51 has a convex portion. Therefore, when the first metal material 1 is used in the sliding component 101, it is preferable that the first metal material 1 has a convex portion protruding toward the surface 55 of the second metal material 51 and sliding against the surface 55 while being pressed against the surface 55.

[0048] Furthermore, when either one of the metal materials 1 or 51 has a pressing portion that is pressed against the surface 55 or 5 of the opposing other metal material 51 or 1 by a force such as a spring material and rubs against the surface 55 or 5, it is preferable that the first metal material 1 has a pressing portion provided on the surface 5. Such a pressing portion may be the above-mentioned convex portion.

[0049] For example, when the sliding element 101 is a board-to-board connector, it is preferable that the receptacle having the convex portion of the board-to-board connector is made of the first metal material 1, and the plug is made of the second metal material 51. In addition, it may be preferable that one of the two metal materials of the sliding element 101, which is biased toward the other metal material by a spring material such as a leaf spring, is made of the metal material 1.

[0050] The sliding part 101 described above is not particularly limited as long as two metal materials 1, 51 slide against each other when in use, but specifically, it can be a connector, a switch, a gear, a bearing, a washer, etc.

[0051] In particular, the embodiment described herein may be able to reduce transmission loss in the metal materials 1, 51, and is therefore effective when applied to a sliding component 101, which is a high-frequency component through which a current flows at a frequency of 1 GHz to 15 GHz, typically a frequency of 7 GHz to 15 GHz. Examples of such high-frequency components include connectors and switches mounted on communication devices such as automotive radar and mobile phones, typified by so-called smartphones. In recent communication devices, electrical signals in such high-frequency bands are used due to the increasing communication speed, amount of information, and diversification of information. In the transmission of high-frequency electrical signals, it is necessary to reduce transmission loss not only during propagation through space but also inside the communication device.

[0052] The effects of the above-mentioned metal materials and sliding parts were confirmed through tests, and are described below. However, the description here is for illustrative purposes only and is not intended to be limiting.

[0053] Test Example 1: A terminal and a flat plate were prepared with the shape and dimensions shown in Figure 5. The protrusion of the terminal protruded 30 μm from the flat surface. Both the terminal and the flat plate had a base material made of a copper alloy containing 0.12 mass% Sn (NKE012 manufactured by JX Nippon Mining & Metals Corporation) and having a thickness of 0.15 mm. The longitudinal direction of both the terminal and the flat plate was perpendicular to the rolling direction of the base material.

[0054] In Example 1, the flat plate was plated with Ni to a thickness of 1.5 μm, and the terminals were plated with Ni—P to a thickness of 1.5 μm (P concentration: 11% by mass). In Example 2, the flat plate was plated with Ni—P to a thickness of 1.5 μm (P concentration: 11% by mass), and the terminals were plated with Ni to a thickness of 1.5 μm.

[0055] In Comparative Example 1, both the flat plate and the terminal were plated with Ni to a thickness of 1.5 μm. In Comparative Example 2, both the flat plate and the terminal were plated with Ni—P to a thickness of 1.5 μm (P concentration: 11% by mass).

[0056] For each of the terminals and flat plates of Examples 1 and 2 and Comparative Examples 1 and 2, a load was applied to the terminal with the protruding portion of the terminal in contact with the flat plate, and the terminal was slid under the following conditions: Load: 200 g Sliding direction: Perpendicular to the rolling direction of the substrate Sliding distance: 24 mm / reciprocation Sliding speed: 960 mm / min Number of slides: 20 reciprocations

[0057] The plate after sliding was observed with a laser microscope (Keyence Corporation's VK-X1000 shape analysis laser microscope) to measure the scraped area in the cross section. The measurement conditions were: scan mode: laser confocal, imaging magnification: 1200x, measurement size: standard (1024 x 768), measurement pitch: 0.13 μm.

[0058] As a result, the scraped area in Example 1 was 33 μm 2 , 425 μm in Example 2 2 , and 1981 μm in Comparative Example 1 2 , and 1079 μm in Comparative Example 2 2 The appearances of the flat plates and terminals after the tests in Examples 1 and 2 and Comparative Examples 1 and 2, as well as the scraped areas of the cross sections of the flat plates, are shown in FIG.

[0059] It has been thought that the harder each of the two metal materials that slide against each other is, the higher the wear resistance will be. In contrast, the results of Test Example 1 above show that wear resistance is improved when one substrate is plated with Ni—P and the other substrate is plated with Ni, compared to when both substrates are plated with Ni—P, which is harder than Ni. The layer formed on the substrate by Ni—P plating is an amorphous layer, and the layer formed on the substrate by Ni plating is a crystalline layer.

[0060] The Ni-P plated amorphous layer had a Vickers hardness of 500 Hv, and the Ni plated crystalline layer had a Vickers hardness of 300 Hv.

[0061] Furthermore, Example 1, in which the terminal with the convex portion includes an amorphous layer and the flat plate includes a crystalline layer, exhibited less wear than Example 2, in which the opposite was true. The reason for this is not entirely clear, but it is thought to be important that the tip of the convex portion (the real contact surface) is hard enough not to deform when shear stress is applied to the convex portion during sliding. If the tip of the convex portion were to deform, the real contact area would increase, and greater stress would be applied, generating wear debris. It is presumed that the convex portion would then engulf this wear debris, making it easier for the flat plate to be scraped.

[0062] In addition to the above tests, it was separately confirmed that applying a 1 μm thick Au plating (outermost layer) to the crystalline Ni plating layer or amorphous Ni-P plating layer of the flat plate and terminal did not affect the magnitude of wear as in Examples 1 and 2 and Comparative Examples 1 and 2. The reason that the provision of the outermost layer did not affect wear resistance is thought to be because outermost layers of Au, Ag, Sn, Pd, Cu, etc. are softer and thinner than Ni or Ni-P. Note that the outermost layer is provided for the purpose of improving electrical conductivity reliability, and even if it wears slightly due to sliding, reliability does not decrease.

[0063] Test Example 2 The transmission loss of a metal material having a base plated with matte Ni and a base plated with Ni—P was measured using a network analyzer (Keysight N5247A).

[0064] In the preparation of the microstrip line, which was the sample to be set in the network analyzer, a 50 μm-thick LCP resin was used as the dielectric layer, and a 12 μm-thick oxygen-free copper foil was used as the metal foil. One side of the oxygen-free copper foil was etched to form a wiring with a width of 124 μm. For plating this wiring, a matte Ni plating was applied using a nickel sulfamate plating solution at a current density of 10 A / dm. 2 The conditions were: solution temperature: 60°C. As a result, a Ni layer was formed around the wiring. On the other hand, Ni-P plating was performed using a Ni sulfate bath as the plating bath, with Ni(II) sulfate hexahydrate: 250 g / L, phosphorous acid: 82 g / L, and a current density of 10 A / dm 2The conditions were: temperature: 60° C. As a result, a Ni—P layer with a P content of 12 mass % was formed around the wiring. The thickness of each Ni layer and Ni—P layer was 2 μm.

[0065] The matte Ni-plated sample and the Ni-P-plated sample were each set in a network analyzer, and the transmission loss was measured using the method described above. The results are shown in Figure 7.

[0066] It can be seen from FIG. 7 that the Ni--P plated sample has a smaller absolute value of transmission loss than the Ni plated sample at frequencies of about 15 GHz or less.

[0067] Test Example 3 For a metal material sample in which an outermost layer was formed by plating Ag or Au to a thickness of 0.3 μm on the Ni layer of the sample of Test Example 2, the transmission loss was measured in the same manner as in Test Example 2. The results are shown in FIG.

[0068] For Ag plating, Silbrex Bright HS manufactured by EEJA was used, and the current density was 10 A / dm 2 The conditions were a solution temperature of 60°C. A hard Au plating solution was used for Au plating, and the current density was 10 A / dm 2 The liquid temperature was 60°C.

[0069] As can be seen from Figure 8, the absolute value of transmission loss tends to decrease by providing a top surface layer. This is presumably because, since the influence of the skin effect is strong in the high frequency range, coating the top surface layer with a highly conductive noble metal reduces the conduction loss in transmission loss. Therefore, Ag, which has a higher conductivity than Au, reduces transmission loss. Figure 8 shows data for a case where the top surface layer is formed on a Ni layer, but from a mechanical perspective, it is believed that similar results would be obtained even if the Ni layer were replaced with a Ni-P layer.

[0070] Test Example 4 A metal material having a crystalline or amorphous plating layer formed thereon was produced by applying matte Ni plating or Ni-P plating to a substrate made of oxygen-free copper (C1020).

[0071] Here, the conditions for the matte Ni plating and the Ni—P plating were the same as those in Test Example 2. The P content of the Ni—P plating was 10 mass %, which is thought to be due to variations.

[0072] For each of the above metal materials, a cross section was processed using an FIB-SIM (SMI3050SE manufactured by Hitachi High-Tech Corporation), and the cross section was observed using a TEM (JEM-2100F manufactured by JEOL Ltd.). As a result, the TEM image and diffraction image shown in Figure 9 were obtained. From Figure 9, it can be seen that the amorphous layer (Ni-P layer) has an amorphous structure, as no crystalline structure can be confirmed in the TEM image. Furthermore, it can also be seen that the amorphous layer (Ni-P layer) has an amorphous structure, as a concentric halo pattern rather than spots can be confirmed in the diffraction image. The fact that the amorphous layer has an amorphous structure can be confirmed by the fact that no crystalline structure can be confirmed in the TEM image of the Ni-P layer. Similarly, the fact that the crystalline layer (Ni layer) has a crystalline structure can be confirmed by the fact that a crystalline structure can be confirmed in the TEM image.

[0073] The results of the above tests, particularly Test Example 1, suggest that the metal material and sliding parts described above have excellent wear resistance and suppress the occurrence of wear of the metal material.

[0074] REFERENCE SIGNS LIST 1, 11 Metal material (first metal material) 2, 12 Base material 3, 13 Plating layer 4, 14 Amorphous layer 5, 15 Surface 16 Outermost layer 51 Other metal material (second metal material) 52 Base material 53 Plating layer 54 Crystalline layer 55 Surface 101 Sliding part

Claims

1. A metallic material having a substrate and a plating layer formed on the substrate, the plating layer including an amorphous layer containing Ni, the metallic material being used in a sliding part in which the surface of the plating layer slides against the surface of another metallic material, the other metallic material including a crystalline layer containing Ni.

2. A metallic material having a substrate and a plating layer formed on the substrate, the plating layer including an amorphous layer, the metallic material being used in a sliding part in which the surface of the plating layer slides against the surface of another metallic material, the other metallic material including a crystalline layer that is softer than the amorphous layer.

3. The metallic material according to claim 2, wherein the main component of the amorphous layer of the metallic material is the same as the main component of the crystalline layer of the other metallic material.

4. The metallic material according to claim 3, wherein the main component is Ni.

5. A metallic material according to any one of claims 1 to 4, wherein the amorphous layer of the metallic material contains P and / or W.

6. A metal material according to any one of claims 1 to 4, wherein the plating layer of the metal material includes an outermost layer containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd and Cu.

7. A metallic material according to any one of claims 1 to 4, wherein the difference between the Vickers hardness of the amorphous layer of the metallic material and the Vickers hardness of the crystalline layer of the other metallic material is 100 Hv or more.

8. A metallic material according to any one of claims 1 to 4, further comprising a pressing part which is pressed against the surface of the other metallic material and slides against the surface.

9. The metallic material according to claim 8, wherein the pressing portion is a protrusion protruding from the surface side of the other metallic material.

10. The metallic material according to any one of claims 1 to 4, wherein the sliding part is a high-frequency part through which a current of a frequency of 1 GHz to 15 GHz flows.

11. The metallic material according to any one of claims 1 to 4, wherein the sliding part is a connector or a switch.

12. A sliding part comprising a first metallic material and a second metallic material, wherein the first metallic material has a substrate and a plating layer formed on the substrate, the plating layer of the first metallic material includes an amorphous layer containing Ni, and the second metallic material includes a crystalline layer containing Ni, and the first metallic material and the second metallic material are used by sliding against each other on their respective surfaces.

13. The sliding component according to claim 12, wherein the amorphous layer of the first metal material contains P and / or W.

14. A sliding component according to claim 12 or 13, wherein the plating layer of the first metal material includes an outermost layer containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd and Cu.

15. The sliding component according to claim 12 or 13, wherein the first metal material has a pressing portion which is pressed against the surface of the second metal material and slides against the surface.

16. The sliding component according to claim 15, wherein the pressing portion is a protrusion protruding from the front surface side of the second metal material.

17. The sliding part according to claim 12 or 13, which is a high-frequency part through which a current having a frequency of 1 GHz to 15 GHz flows.

18. The sliding part according to claim 12 or 13, which is a connector or a switch.

Citation Information

Patent Citations

  • Pulse-electrodeposited Ni-Co-P / HBN composite plating and preparation method thereof

    CN102534732A

  • Arc resistant terminal pair

    JP2003323929A

  • Plating treatment material and slide member

    JP2017186667A

  • Laminate, metal plating liquid, and laminate manufacturing method

    JP2021160117A

  • Plug-in connector

    US20180269603A1