Positively chargeable toner for electrostatic charge image development, toner set, and image forming method

The use of a styrene acrylic-polyester resin combination with ester wax and optimized surfactant levels in the toner formulation addresses the balance of low-temperature fixability and heat-resistant storage, preventing fogging and ensuring uniform gloss and stability in image formation.

WO2024202238A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP

Patent Information

Application Number
PCT/JP2023/042523
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-11-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Toner formulations face challenges in achieving a balance between low-temperature fixability and heat-resistant storage stability, often resulting in issues like fogging and uneven gloss, particularly when using hydrocarbon waxes as mold release agents.

Method used

A positively chargeable toner is developed using a combination of styrene acrylic resin and polyester resin as binder resins, with ester wax as the mold release agent and a nonionic surfactant as the release agent dispersant, optimizing the amount of surfactant on toner particles to enhance dispersibility and prevent moisture absorption.

Benefits of technology

The toner achieves excellent low-temperature fixability, heat-resistant storage stability, and uniform gloss, reducing the likelihood of fogging and peeling in multi-color images, while maintaining charging stability across varying environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023042523_03102024_PF_FP_ABST
    Figure JP2023042523_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a toner which has an excellent balance between low-temperature fixability and thermal storage stability, is not susceptible to the occurrence of fogging, and is capable of forming images that are excellent in terms of gloss uniformity. Specifically provided is a positively chargeable toner for electrostatic charge image development, the positively chargeable toner containing colored resin particles which contain a binder resin, a coloring agent, a mold release agent, a mold release agent dispersant and a charge control agent. This positively chargeable toner for electrostatic charge image development contains: a styrene acrylic resin and a polyester resin as the binder resin; an ester wax as the mold release agent; and a nonionic surfactant as the mold release agent dispersant. The mass of the nonionic surfactant present on the surfaces of the toner particles is 0.1-500 ppm relative to the mass of the toner particles.
Need to check novelty before this filing date? Find Prior Art

Description

Positively charged toner for developing electrostatic images, toner set, and image forming method

[0001] The present disclosure relates to a positively charged toner for developing electrostatic images used to develop electrostatic latent images in electrophotography, electrostatic recording, electrostatic printing, etc. The present disclosure also relates to a toner set combining the positively charged toners for developing electrostatic images, and an image forming method using the toner set.

[0002] In image forming apparatuses such as electrophotographic apparatuses, electrostatic recording apparatuses, and electrostatic printing apparatuses, an electrostatic latent image formed on a photosensitive member is developed with toner, the toner image is transferred to a transfer material such as paper, and then fixed by heating or the like to form a fixed image. In such image forming apparatuses, there is a demand for a toner for developing electrostatic images (simply referred to as "toner" in this disclosure) that can be thermally fixed at a lower temperature for purposes such as reducing power consumption by reducing thermal energy during fixing, reducing environmental impact, and increasing printing speed.

[0003] For example, Patent Document 1 discloses a toner having excellent low-temperature fixing property, heat resistance, fixing separation property, and durability, in which toner particles contain a binder resin, a colorant, a release agent, and a plasticizer, and the binder resin contains a styrene-acrylic resin, and the average aspect ratio (Aw) of the domain portion of the release agent in the cross section of the toner particle is made larger than the average aspect ratio (Ac) of the domain portion of the plasticizer. The toner disclosed in Patent Document 1 uses a microcrystalline wax as the release agent.

[0004] Patent Document 2 aims to provide an image forming apparatus that simultaneously satisfies low-temperature fixability and environmental stability, and discloses a toner containing a monoester compound having a specific structure as a wax as a toner to be used in the image forming apparatus.

[0005] Patent Document 3 aims to provide a toner that can obtain high image density and excellent charging stability, and discloses a toner containing, as a resin constituting a binder resin, a polyester resin segment, an addition polymerization resin segment which is an addition polymerization product of raw material monomers including a styrene compound, and a composite resin containing a structural unit derived from a bireactive monomer bonded to the polyester resin segment and the addition polymerization resin segment via a covalent bond. The toner disclosed in Patent Document 3 uses a hydrocarbon wax as a release agent.

[0006] JP 2016-206387 A JP 2021-86067 A JP 2022-164798 A

[0007] Toners are required to have a good balance between low-temperature fixability and heat-resistant storage stability. However, toners with good low-temperature fixability and heat-resistant storage stability are prone to other problems, such as fogging. Furthermore, when a hydrocarbon wax is used alone as a release agent, gloss unevenness is likely to occur.

[0008] An object of the present disclosure is to provide a toner that has an excellent balance of low-temperature fixability and heat-resistant storage stability, is less likely to cause fogging, and is capable of forming images with excellent gloss uniformity.A further object of the present disclosure is to provide a toner set that is capable of forming multi-color images with excellent gloss uniformity and in which toner layer peeling is less likely to occur in the formed multi-color images, and to provide an image forming method using the toner set.

[0009] The present inventors have conducted extensive research to achieve the above-mentioned object, and have found that when a positively charged toner contains a combination of a styrene acrylic resin and a polyester resin as a binder resin and uses a specific amount of a nonionic surfactant as a dispersant for the ester wax, the toner has an excellent balance of low-temperature fixability and heat-resistant storage stability, is less likely to cause fogging, and can form images with excellent gloss uniformity, leading to the present disclosure.

[0010] That is, the positively charged toner for developing electrostatic images of the present disclosure is a positively charged toner for developing electrostatic images, which contains colored resin particles including a binder resin, a colorant, a release agent, a release agent dispersant, and a charge control agent, and is characterized in that the binder resin contains a styrene acrylic resin and a polyester resin, the release agent contains an ester wax, and the release agent dispersant contains a nonionic surfactant, and the mass of the nonionic surfactant present on the surface of the toner particles is 0.1 to 500 ppm relative to the mass of the toner particles.

[0011] In one embodiment of the present disclosure, the charge control agent contains a charge control resin.

[0012] In one embodiment of the present disclosure, the mass ratio of the styrene acrylic resin to the polyester resin (styrene acrylic resin:polyester resin) is 96:4 to 70:30.

[0013] In one embodiment of the present disclosure, the colored resin particles further contain a styrene-based thermoplastic elastomer.

[0014] In one embodiment of the present disclosure, the toner particles have an average circularity of 0.96 or more, and a particle size distribution (Dv / Dp) which is the ratio of the volume average particle size (Dv) to the number average particle size (Dp) of the toner particles is less than 1.3.

[0015] In one embodiment of the present disclosure, the ester wax contains a polyfunctional ester compound of a fatty acid having 10 to 22 carbon atoms and a polyhydric alcohol.

[0016] The present inventors have also found that a toner set combining the toners of the present disclosure can form a multi-color image with excellent gloss uniformity, and that peeling of the toner layer is unlikely to occur in the formed multi-color image. That is, the toner set of the present disclosure is a color toner set containing positively charged toners for electrostatic image development of multiple colors, characterized in that the positively charged toners for electrostatic image development of multiple colors include at least a yellow toner, a magenta toner, and a cyan toner, and all of the positively charged toners for electrostatic image development of the multiple colors are the positively charged toners for electrostatic image development of the present disclosure.

[0017] The image forming method of the present disclosure is characterized in that an image is formed using the toner set of the present disclosure.

[0018] According to the present disclosure, it is possible to provide a toner that has excellent low-temperature fixability and heat-resistant storage stability, is less likely to cause fogging, and is capable of forming images with excellent gloss uniformity. Furthermore, according to the present disclosure, it is possible to provide a toner set that is capable of forming multi-color images with excellent gloss uniformity and that is less likely to cause peeling of the toner layer in the formed multi-color images. Furthermore, according to the present disclosure, there is provided an image forming method using the toner set.

[0019] FIG. 1 is a schematic diagram illustrating an example of an image forming apparatus that can be used to form an image using a toner set according to the present disclosure.

[0020] The positively charged toner for developing electrostatic images of the present disclosure is a positively charged toner for developing electrostatic images containing colored resin particles including a binder resin, a colorant, a release agent, a release agent dispersant, and a charge control agent, wherein the binder resin contains a styrene acrylic resin and a polyester resin, the release agent contains an ester wax, and the release agent dispersant contains a nonionic surfactant, and the mass of the nonionic surfactant present on the surface of the toner particles is 0.1 to 500 ppm relative to the mass of the toner particles. Hereinafter, the positively charged toner for developing electrostatic images of the present disclosure may be simply referred to as the "toner of the present disclosure."

[0021] The toner of the present disclosure contains a combination of a styrene-acrylic resin and a polyester resin as a binder resin, thereby achieving both fixability and charge stability under environmental changes, resulting in excellent low-temperature fixability and reduced fogging. Furthermore, the toner of the present disclosure uses an ester wax as a release agent and a specific amount of a nonionic surfactant as a release agent dispersant, thereby improving the dispersibility of the ester wax in the colored resin particles. As a result, the low-temperature fixability is further improved while suppressing deterioration of heat-resistant storage stability. Furthermore, the toner of the present disclosure uses an ester wax as a release agent, which slows the crystallization rate of the release agent when the toner is rapidly cooled after fixing, thereby reducing gloss unevenness and enabling the formation of images with excellent gloss uniformity. Furthermore, by using a specific amount of nonionic surfactant within the toner of the present disclosure, the dispersibility of the ester wax can be improved while sufficiently reducing the amount of surfactant remaining on the toner particle surface. If a large amount of surfactant is present on the toner particle surface, the toner particle surface absorbs moisture, resulting in poor chargeability, which can lead to problems such as increased fogging and blocking. In high-temperature, high-humidity environments, the toner particle surface is more likely to absorb moisture, making such problems more likely to occur. In contrast, the toner of the present disclosure has a sufficiently low amount of nonionic surfactant present on the toner particle surface, resulting in excellent charge stability, less fogging, less blocking, and excellent heat-resistant storage stability. As described above, the toner of the present disclosure uses a specific binder resin, release agent, and release agent dispersant, and by adjusting the amount of the nonionic surfactant used as the release agent dispersant so that the amount present on the toner particle surface of the nonionic surfactant used as the release agent dispersant falls within a specific range, the toner has an excellent balance of low-temperature fixability and heat-resistant storage stability and is less likely to cause fogging. Furthermore, by using the toner of the present disclosure, images with excellent gloss uniformity can be formed. In this disclosure, the heat-resistant storage stability of a toner may also be simply referred to as "storage stability."The following describes the manufacturing method of the colored resin particles used in the toner of the present disclosure, the colored resin particles, the external additives used in the toner of the present disclosure, and the toner particles that constitute the toner of the present disclosure. Note that in this disclosure, the term "to" in a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit, respectively.

[0022] 1. Manufacturing Method of Colored Resin Particles Generally, manufacturing methods of colored resin particles are roughly divided into dry methods such as pulverization methods, and wet methods such as emulsion polymerization aggregation methods, suspension polymerization methods, and dissolution suspension methods, with wet methods being preferred because they are more likely to produce toners with excellent printing properties such as image reproducibility. Among the wet methods, polymerization methods such as emulsion polymerization aggregation methods and suspension polymerization methods are preferred because they are more likely to produce toners with a relatively small particle size distribution on the order of microns, and among polymerization methods, suspension polymerization is more preferred.

[0023] The emulsion polymerization aggregation method involves polymerizing an emulsified polymerizable monomer to obtain a resin fine particle emulsion, which is then aggregated with a colorant dispersion or the like to produce colored resin particles. The solution suspension method involves forming droplets of a solution in which toner components such as a binder resin and a colorant are dissolved or dispersed in an organic solvent in an aqueous medium, and then removing the organic solvent to produce colored resin particles. Any known method can be used for either method.

[0024] The colored resin particles used in the present disclosure can be produced by employing a wet method or a dry method, but a wet method is preferred, and among the wet methods, a suspension polymerization method is particularly preferred, and the colored resin particles can be produced by the following process.

[0025] (A) Suspension Polymerization Method (A-1) Preparation of Polymerizable Monomer Composition First, a polymerizable monomer, a polyester resin, a colorant, a release agent, a release agent dispersant, and a charge control agent are mixed, and, if necessary, other additives such as an acidic group-containing acrylic resin, a styrene-based thermoplastic elastomer, and a molecular weight modifier are mixed to prepare a polymerizable monomer composition. For example, a disperser such as an in-line emulsifying disperser or a media-type emulsifying disperser is used for mixing when preparing the polymerizable monomer composition. The polymerizable monomer composition is preferably prepared, for example, by mixing the polymerizable monomer, the polyester resin, the colorant, and the molecular weight modifier using a media-type disperser, wet-grinding the mixture, and then adding the charge control agent, the release agent, and the release agent dispersant, and further mixing the mixture. This method makes it easy to obtain a toner with excellent low-temperature fixability and heat-resistant storage stability.

[0026] (Polymerizable Monomer) In the present disclosure, the term "polymerizable monomer" refers to a monomer or macromonomer having a polymerizable functional group. The polymerizable monomer contained in the polymerizable monomer composition is polymerized to form a styrene-acrylic resin, which is a binder resin. In the present disclosure, the styrene-acrylic resin is a copolymer of an aromatic vinyl monomer and a (meth)acrylic monomer. Other monomers different from the aromatic vinyl monomer and the (meth)acrylic monomer may also be copolymerized within the scope of the present disclosure. Here, the (meth)acrylic monomer is a monomer containing at least one selected from an acryloyl group and a methacryloyl group. The aromatic vinyl monomer, (meth)acrylic monomer, and other monomers used in the synthesis of the styrene-acrylic resin may be monovinyl monomers, crosslinkable polymerizable monomers, or macromonomers, but preferably contain a monovinyl monomer as the main component. Specifically, the content of the monovinyl monomer is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, even more preferably 90 parts by mass or more, still more preferably 95 parts by mass or more, and particularly preferably 98 parts by mass or more, relative to 100 parts by mass of the total amount of polymerizable monomers.

[0027] Examples of the monovinyl monomer include aromatic vinyl monomers such as styrene and styrene derivatives such as vinyltoluene and α-methylstyrene; acrylic acid esters such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and dimethylaminoethyl acrylate; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and dimethylaminoethyl methacrylate; (meth)acrylic monomers such as acrylamide, methacrylamide, acrylic acid, and methacrylic acid; nitrile compounds such as acrylonitrile and methacrylonitrile; olefins such as ethylene, propylene, and butylene; etc. These monovinyl monomers can be used alone or in combination of two or more. In particular, from the viewpoint of improving charging stability when the environment is changed and thereby suppressing the occurrence of fogging, it is preferable that the monovinyl monomer contains an aromatic vinyl monomer and at least one selected from the group consisting of acrylic acid esters and methacrylic acid esters, and it is more preferable that the monovinyl monomer contains styrene and at least one selected from the group consisting of acrylic acid esters and methacrylic acid esters. Furthermore, among the acrylic acid esters, at least one selected from the group consisting of n-butyl acrylate, propyl acrylate, and 2-ethylhexyl acrylate is preferred. Among the methacrylic acid esters, at least one selected from the group consisting of n-butyl methacrylate, propyl methacrylate, and 2-ethylhexyl methacrylate is preferred. In a total of 100 parts by mass of monovinyl monomers, the total content of aromatic vinyl monomers, acrylic acid esters, and methacrylic acid esters is preferably 60 parts by mass or more, more preferably 70 parts by mass or more, even more preferably 80 parts by mass or more, still more preferably 90 parts by mass or more, and particularly preferably more than 99.95 parts by mass.

[0028] In order to obtain a good balance between the low-temperature fixability and heat-resistant storage stability of the toner and to suppress the occurrence of fogging, the monovinyl monomer preferably contains styrene and at least one selected from the group consisting of acrylic acid esters and methacrylic acid esters, and the mass ratio of styrene to the total of the acrylic acid esters and methacrylic acid esters (styrene:(meth)acrylic acid ester) is preferably within a range of 50:50 to 90:10, more preferably within a range of 60:40 to 80:20. The structure and ratio of each monomer unit constituting the resin can be determined from the composition of the polymerizable monomers used in the synthesis of the resin, and 1 It can be calculated from the integral value obtained by H-NMR measurement.

[0029] The polymerizable monomer may contain a macromonomer in addition to the monovinyl monomer. By incorporating a macromonomer into the polymerizable monomer, the balance between the storage stability and low-temperature fixability of the toner can be improved. Examples of macromonomers include reactive oligomers and polymers having a polymerizable carbon-carbon unsaturated double bond at the end of the molecular chain, and having a number-average molecular weight of typically 1,000 to 30,000. Examples of the macromonomer include styrene macromonomers, styrene-acrylonitrile macromonomers, polyacrylic acid ester macromonomers, and polymethacrylic acid ester macromonomers. Among these, at least one selected from polyacrylic acid ester macromonomers and polymethacrylic acid ester macromonomers is preferably used because it allows for easy control of the glass transition temperature (Tg) of the toner. Examples of acrylic acid esters used in polyacrylic acid ester macromonomers include the same acrylic acid esters usable as the monovinyl monomers, and examples of methacrylic acid esters used in polymethacrylic acid ester macromonomers include the same methacrylic acid esters usable as the monovinyl monomers. As the macromonomer, it is preferable to appropriately select and use one that, when incorporated into the polymerizable monomer, increases the glass transition temperature (Tg) of the resulting binder resin compared to when not incorporated, since this makes it easier to bring the glass transition temperature (Tg) of the toner within the preferred range. Commercially available macromonomers may be used. Examples of commercially available macromonomers include the macromonomer series AA-6, AS-6, AN-6S, AB-6, and AW-6S manufactured by Toagosei Co., Ltd. The macromonomers may be used alone or in combination of two or more.

[0030] When the polymerizable monomer contains the macromonomer, the content of the macromonomer is not particularly limited, but is preferably 0.03 parts by mass or more and 5 parts by mass or less, and more preferably 0.05 parts by mass or more and 1 part by mass or less, relative to 100 parts by mass of the monovinyl monomer.

[0031] The polymerizable monomer may contain a crosslinkable polymerizable monomer in addition to the monovinyl monomer. The inclusion of a crosslinkable polymerizable monomer in the polymerizable monomer is preferred because it facilitates improving the storage stability and hot offset resistance of the toner. Here, the crosslinkable polymerizable monomer refers to a monomer having two or more polymerizable functional groups. Examples of crosslinkable polymerizable monomers include aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof; ester compounds in which two or more carboxylic acids are ester-bonded to an alcohol having two or more hydroxyl groups, such as ethylene glycol dimethacrylate and diethylene glycol dimethacrylate; other divinyl compounds such as N,N-divinylaniline and divinyl ether; and compounds having three or more vinyl groups. Among these, aromatic divinyl compounds are preferred. The crosslinkable polymerizable monomers may be used alone or in combination of two or more.

[0032] When the polymerizable monomer contains the crosslinkable polymerizable monomer, the content of the crosslinkable polymerizable monomer is not particularly limited, but is preferably 0.05 parts by mass or more and 5 parts by mass or less, more preferably 0.06 parts by mass or more and 1.5 parts by mass or less, and even more preferably 0.08 parts by mass or more and 0.8 parts by mass or less, relative to 100 parts by mass of the monovinyl monomer.

[0033] The content of the polymerizable monomer is not particularly limited, but from the viewpoint of achieving a good balance between the low-temperature fixability and heat-resistant storage stability of the toner and suppressing the occurrence of fogging, it is preferably 60 parts by mass or more and 90 parts by mass or less, more preferably 65 parts by mass or more and 85 parts by mass or less, and even more preferably 70 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the total solid content contained in the polymerizable monomer composition. In the present disclosure, the solid content refers to all components other than the solvent, and includes liquid monomers and the like. The content of the polymerizable monomer relative to 100 parts by mass of the total solid content contained in the polymerizable monomer composition corresponds to the content of the styrene-acrylic resin relative to 100 parts by mass of the colored resin particles.

[0034] (Polyester Resin) As the polyester resin, a polyester resin generally used as a binder resin for toner can be used, and although not particularly limited, a polyester resin obtained by polycondensation of a carboxylic acid component containing a polycarboxylic acid compound and an alcohol component containing a polyhydric alcohol is preferably used. The carboxylic acid component is a compound containing a carboxyl group or a carboxylic acid derivative group, and the polycarboxylic acid compound is a compound having two or more carboxyl groups or carboxylic acid derivative groups in one molecule. Examples of the carboxylic acid derivative group include an amide group, an ester group, an acid anhydride group, and an acid halide. In the synthesis of the polyester resin, the carboxylic acid component and the alcohol component can each be used alone or in combination of two or more.

[0035] The polycarboxylic acid compound used in the synthesis of the polyester resin preferably contains at least a cyclic dicarboxylic acid component (B), since this makes it easier to obtain a toner that has an excellent balance between low-temperature fixability and heat-resistant storage stability, is excellent in environmental stability, and is less susceptible to fogging. Examples of the cyclic dicarboxylic acid compound (B) include aromatic dicarboxylic acid compounds, alicyclic dicarboxylic acid compounds, and derivatives thereof, and among these, alicyclic dicarboxylic acid compounds and derivatives thereof are preferred.

[0036] Examples of aromatic dicarboxylic acid compounds include 1,5-naphthalic acid, 2,6-naphthalic acid, diphenic acid, terephthalic acid, isophthalic acid, phthalic acid, and alkyl-substituted derivatives thereof, as well as derivatives thereof such as acid anhydrides, halides, esters, and amides.

[0037] Alicyclic dicarboxylic acid compounds are compounds in which an alicyclic structure and two carboxyl groups exist in the molecular structure. Derivatives of alicyclic dicarboxylic acid compounds are compounds in which at least one carboxyl group in an alicyclic dicarboxylic acid compound is replaced with a carboxylic acid derivative group. Examples of alicyclic structures include monocyclic structures such as a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, and a cyclohexene ring; and polycyclic structures such as a norbornane ring and a norbornene ring. Suitable alicyclic dicarboxylic acid compounds and their derivatives include alicyclic dicarboxylic acid compounds in which a carboxyl group or a carboxylic acid derivative group is bonded to each of two carbon atoms constituting an alicyclic ring. In particular, alicyclic dicarboxylic acids represented by the following general formula (1) or (2), and anhydrides thereof, in which an alkyl group is bonded as a substituent to the alicyclic ring, are preferred. The alkyl group bonded as a substituent to the alicyclic ring is preferably an alkyl group having 1 to 8 carbon atoms, with methyl, ethyl, propyl, and isopropyl groups being more preferred.

[0038]

[0039]

[0040] In the formulas (1) and (2), R is an alkyl group.

[0041] Alicyclic dicarboxylic acid compounds can be obtained, for example, by reacting a diene compound such as butadiene, isoprene, piperylene, or cyclopentadiene with maleic anhydride, followed by hydrogenation as necessary. Examples of alicyclic dicarboxylic acid compounds include tetrahydroterephthalic acid, tetrahydroisophthalic acid, tetrahydrophthalic acid; hexahydroterephthalic acid, hexahydroisophthalic acid, hexahydrophthalic acid; 3-alkyltetrahydroterephthalic acid, 4-alkyltetrahydroterephthalic acid, 3-alkyltetrahydroisophthalic acid, 4-alkyltetrahydroisophthalic acid, 3-alkyltetrahydrophthalic acid, 4-alkyltetrahydrophthalic acid; 3-alkylhexahydrophthalic acid, 4-alkyltetrahydrophthalic acid; Terephthalic acid, 4-alkylhexahydroterephthalic acid, 3-alkylhexahydroisophthalic acid, 4-alkylhexahydroisophthalic acid, 3-alkylhexahydrophthalic acid, 4-alkylhexahydrophthalic acid; bis(β-hydroxyethyl) hexahydroterephthalate; 3,6-endomethylene-tetrahydroterephthalic acid, 3,6-endomethylene-tetrahydroisophthalic acid, 3,6-endomethylene-tetrahydrophthalic acid; 3,6-endomethylene-hexahydroterephthalic acid Phthalic acid, 3,6-endomethylene-hexahydroisophthalic acid, 3,6-endomethylene-hexahydrophthalic acid; 2-alkyl-3,6-endomethylene-tetrahydroterephthalic acid, 3-alkyl-3,6-endomethylene-tetrahydroterephthalic acid, 2-alkyl-3,6-endomethylene-tetrahydroisophthalic acid, 3-alkyl-3,6-endomethylene-tetrahydroisophthalic acid, 2-alkyl-3,6-endomethylene-tetrahydrophthalic acid, 3-alkyl- Examples thereof include 3,6-endomethylene-tetrahydrophthalic acid; 2-alkyl-3,6-endomethylene-hexahydroterephthalic acid, 3-alkyl-3,6-endomethylene-hexahydroterephthalic acid; 2-alkyl-3,6-endomethylene-hexahydroisophthalic acid, 3-alkyl-3,6-endomethylene-hexahydroisophthalic acid, 2-alkyl-3,6-endomethylene-hexahydrophthalic acid, 3-alkyl-3,6-endomethylene-hexahydrophthalic acid; and the like.

[0042] Examples of the derivatives of alicyclic dicarboxylic acid compounds include acid anhydrides such as tetrahydrophthalic anhydride, hexahydrophthalic anhydride, 3-alkyltetrahydrophthalic anhydride, 3-alkylhexahydrophthalic anhydride, 4-alkyltetrahydrophthalic anhydride, and 4-alkylhexahydrophthalic anhydride, as well as halides, esters, and amides.

[0043] As the alicyclic dicarboxylic acid compound and its derivative, from the viewpoint of improving the low-temperature fixability of the toner and suppressing the occurrence of fogging, 3-alkyltetrahydrophthalic acid, 3-alkylhexahydrophthalic acid, 4-alkyltetrahydrophthalic acid, 4-alkylhexahydrophthalic acid, and anhydrides thereof are particularly preferred.

[0044] The cyclic dicarboxylic acid compound (B) may also contain a polycarboxylic acid compound (A1) containing an amino group or a salt thereof. Examples of the polycarboxylic acid compound (A1) containing an amino group or a salt thereof include aromatic polycarboxylic acids such as aminoterephthalic acid, 5-aminoisophthalic acid, 5-aminoisophthalic acid methyl ester, 4-aminophthalic acid, 4-aminophthalic anhydride, 4-aminonaphthalene-2,7-dicarboxylic acid, and 5-[4-aminophenoxy]isophthalic acid; and alicyclic polycarboxylic acids such as 5-aminohexahydroisophthalic acid, 5-aminohexahydroisophthalic acid methyl ester, 5-aminohexahydroisophthalic acid dimethyl ester, 4-aminohexahydrophthalic acid, 4-aminohexahydrophthalic anhydride, 5-aminotetrahydroisophthalic acid, 5-aminotetrahydroisophthalic acid methyl ester, 4-aminotetrahydrophthalic acid, and 4-aminotetrahydrophthalic anhydride.

[0045] The amount of the cyclic dicarboxylic acid compound (B) is preferably 70 to 100 mol %, more preferably 80 to 100 mol %, based on the total carboxylic acid components. When the amount of the cyclic dicarboxylic acid compound (B) is within this range, a toner having an excellent balance between low-temperature fixability and heat-resistant storage stability, excellent environmental stability, and little fogging is likely to be obtained.

[0046] The carboxylic acid component used in the synthesis of the polyester resin may further contain at least one selected from a chain dicarboxylic acid compound (D) and a trivalent or higher carboxylic acid compound (F), as necessary. Examples of the chain dicarboxylic acid compound (D) include succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, fumaric acid, maleic acid, and itaconic acid. Examples of the trivalent or higher carboxylic acid compound (F) include trimellitic acid, pyromellitic acid, and trimesic acid. The proportion of the chain dicarboxylic acid compound (D) is preferably 30 mol% or less of the total carboxylic acid components. If this proportion is high, the glass transition temperature and melt viscosity may decrease, resulting in a decrease in the blocking resistance of the toner and the occurrence of hot offset. The proportion of the trivalent or higher carboxylic acid compound (F) is preferably 5 mol% or less of the total carboxylic acid components. If this proportion is high, the weight-average molecular weight of the polyester resin increases, which may increase the melt viscosity of the toner and result in poor toner fixability.

[0047] The polyhydric alcohol used in the synthesis of the polyester resin preferably contains at least a cyclic dihydric alcohol (C), since this makes it easier to obtain a toner that has an excellent balance between low-temperature fixability and heat-resistant storage stability, is excellent in environmental stability, and is less susceptible to fogging. Examples of the cyclic dihydric alcohol (C) include aromatic dihydric alcohols and alicyclic dihydric alcohols, and among these, alicyclic dihydric alcohols are preferred.

[0048] Examples of aromatic dihydric alcohols include paraxylylene glycol, metaxylylene glycol, orthoxylylene glycol, ethylene oxide adducts of 1,4-phenylene glycol, ethylene oxide adducts and propylene oxide adducts of bisphenol A, and the like.

[0049] Examples of alicyclic dihydric alcohols include 2,2-bis(4-hydroxycyclohexyl)-propane (i.e., hydrogenated bisphenol A), 1,4-bis(hydroxymethyl)cyclohexane, 1,3-bis(hydroxymethyl)cyclohexane, 1,2-bis(hydroxymethyl)cyclohexane, 2,2,4,4-tetramethyl-1,3-cyclohexanediol, 1,4-cyclohexanediol, ethylene oxide adducts and propylene oxide adducts of hydrogenated bisphenol A, tricyclodecane diol, tricyclodecane dimethanol, dicyclohexyl 4,4'-diol, etc. Of these, bis(hydroxycyclohexyl)-alkanes such as hydrogenated bisphenol A are preferred.

[0050] The amount of the cyclic dihydric alcohol (C) is preferably 2 to 100 mol % of the total alcohol components, more preferably 10 to 60 mol %, and even more preferably 20 to 50 mol %. If the amount of the cyclic dihydric alcohol (C) is too small, the glass transition temperature and melt viscosity may decrease, resulting in reduced blocking resistance and hot offset. By reducing the amount of the alicyclic dihydric alcohol, the fixability of the toner may be improved.

[0051] The alcohol component used in the synthesis of the polyester resin preferably further contains a chain dihydric alcohol (E). It may also further contain a trihydric or higher alcohol (G). Examples of the chain dihydric alcohol (E) include linear aliphatic glycols such as ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, polyethylene glycol, and polytetramethylene glycol; and branched aliphatic glycols such as propylene glycol, dipropylene glycol, polypropylene glycol, neopentyl glycol, 2,2,4-trimethyl-1,3-pentanediol, and 2-ethyl-2-butyl-1,3-propanediol. Among these, linear aliphatic glycols are preferred, and ethylene glycol is particularly preferred. The amount of the chain dihydric alcohol (E) is preferably 40 to 98 mol %, and more preferably 50 to 97 mol %, of the total polyhydric alcohol components constituting the polyester-based resin. If the amount of the chain dihydric alcohol (E) is too small, the melt viscosity may increase, resulting in poor fixability. Conversely, if the amount of the chain dihydric alcohol is too large, the glass transition temperature and melt viscosity may decrease, resulting in poor blocking resistance and hot offset. Examples of the trihydric or higher alcohol (G) include trimethylolpropane, glycerin, pentaerythritol, dipentaerythritol, trimethylolethane, cyclohexanetriol, tris(hydroxymethyl)cyclohexane, and 2,4-bis(hydroxyethyl)-1-aminocyclohexane. The proportion of the trihydric or higher alcohol (G) is preferably 5 mol % or less of the total alcohol components. If this proportion is too large, the weight-average molecular weight of the polyester-based resin increases, resulting in a high melt viscosity of the toner and poor fixability of the toner.

[0052] The cyclic dihydric alcohol (C) or chain dihydric alcohol (E) may contain a polyhydric alcohol (A2) containing an amino group or a salt thereof. Examples of the polyhydric alcohol (A2) containing an amino group or a salt thereof include chain aliphatic polyhydric alcohols such as 2-amino-2-methyl-1,3-propanediol and diethanolamine; aromatic polyhydric alcohols such as 2-amino-4-hydroxymethylbenzyl alcohol, 2-amino-3-hydroxymethylbenzyl alcohol, 4-amino-2-hydroxymethylbenzyl alcohol and 5-amino-3-hydroxymethylbenzyl alcohol; and ammonium salts thereof.

[0053] The polyester resin contained in the toner of the present disclosure is preferably a polyester resin obtained by polycondensation of at least one selected from a polycarboxylic acid compound (A1) containing an amino group or a salt thereof and a polyhydric alcohol (A2) containing an amino group or a salt thereof, since this tends to improve the low-temperature fixability of the toner and reduces the occurrence of fogging. The polyester resin is preferably a polyester resin having an amino group or an ammonium salt. The polyester resin having an ammonium salt may be a polyester resin obtained by copolycondensation of one or more selected from a polycarboxylic acid compound (A1) containing an ammonium salt and a polyhydric alcohol (A2) containing an ammonium salt, or may be a polyester resin obtained by copolycondensation of one or more selected from a polycarboxylic acid compound (A1) containing an amino group and a polyhydric alcohol (A2) containing an amino group, followed by conversion to an ammonium salt. In the polyester resin contained in the toner of the present disclosure, the total amount of the polycarboxylic acid compound (A1) containing an amino group or a salt thereof and the polyhydric alcohol (A2) containing an amino group or a salt thereof is usually 0.2 to 30 mol %, preferably 0.5 to 10 mol %, and more preferably 1.0 to 5 mol %, relative to 100 mol % of all monomers constituting the polyester resin (the sum of all carboxylic acid components and all alcohol components). By containing at least one selected from the polycarboxylic acid compound (A1) containing an amino group or a salt thereof and the polyhydric alcohol (A2) containing an amino group or a salt thereof as a polycondensation component, the dispersibility of the pigment in the toner is improved, and the chargeability of the toner can be controlled.

[0054] The molecular weight of the polyester resin contained in the toner of the present disclosure is preferably a number-average molecular weight Mn of 1,500 to 20,000, more preferably 2,000 to 10,000, and even more preferably 2,500 to 8,000, and a weight-average molecular weight Mw of 5,000 to 300,000, more preferably 7,000 to 100,000, and even more preferably 8,000 to 20,000. Having a molecular weight within this range enables the production of a toner with excellent low-temperature fixability and hot offset resistance. If the number-average molecular weight Mn or weight-average molecular weight Mw is smaller than the above range, the cohesive strength of the polyester resin may decrease, resulting in poor storage stability. Conversely, if it is larger, productivity may decrease and the fixability of the toner may deteriorate. In the present disclosure, the weight-average molecular weight Mw and number-average molecular weight Mn of the resin can be determined in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF).

[0055] The glass transition temperature of the polyester resin is preferably 40 to 90°C, particularly preferably 50 to 80°C. If the glass transition temperature is in the above range, the storage stability of the toner is improved. In the present disclosure, the glass transition temperature (Tg) of the resin can be determined, for example, in accordance with ASTM D3418-82. Specifically, a sample is heated at a heating rate of 10°C / min using a differential scanning calorimeter (Seiko Electronics Industries Co., Ltd.: SSC5200) or the like, and the temperature showing the maximum endothermic peak in the DSC curve obtained during this process can be taken as the glass transition temperature.

[0056] The hydroxyl value of the polyester resin is usually 1 to 100 mgKOH / g, preferably 5 to 80 mgKOH / g. A low hydroxyl value can result in poor fixability, large irregularities on the image surface, and reduced smoothness. A high hydroxyl value can lower the temperature at which hot offset occurs and increase hydrophilicity, making the charge amount more susceptible to changes in environmental conditions and increasing the likelihood of fogging. In addition, to reduce the impact of moisture in high-temperature, high-humidity environments, it is preferable to reduce the amount of aromatic rings contained in the polyester resin.

[0057] The polyester resin contained in the toner of the present disclosure can be produced by a known method, i.e., a polycondensation method. When polycondensing a carboxylic acid component and an alcohol component, it is preferable to perform the polycondensation under conditions such that the total number of hydroxyl values ​​of the alcohol-reactive groups [X] in the total monomers, i.e., the carboxylic acid component and the alcohol component, is not smaller than the total number of acid values ​​of the carboxylic acid-reactive groups [Y], since this facilitates adjustment of the molecular weight and hydroxyl value of the polyester within a preferred range. The ratio of the total number of hydroxyl values ​​of the alcohol-reactive groups [X] to the total number of acid values ​​of the carboxylic acid-reactive groups [Y] (equivalent ratio) [X] / [Y] is preferably 1.00 or greater, more preferably 1.01 to 1.5, and particularly preferably 1.03 to 1.3. Here, the alcohol-reactive group refers to an alcoholic functional group that forms an ester bond, typically a hydroxyl group. The carboxylic acid-reactive group refers to a carboxylic acid functional group that forms an ester bond, typically a carboxyl group or a carboxylic acid derivative group.

[0058] The polycondensation reaction is carried out, for example, at a reaction temperature of 100 to 300°C, preferably 150 to 280°C, and is particularly preferably carried out in the presence of an inert gas. If necessary, a water-insoluble organic solvent that forms an azeotrope with water, such as toluene or xylene, may be used. The polycondensation reaction may also be carried out under reduced pressure (usually 0.1 to 500 mmHg, preferably 0.5 to 200 mmHg, more preferably 1 to 50 mmHg). An esterification catalyst is usually used in this polycondensation reaction. Examples of the esterification catalyst include Bronsted acids such as paratoluenesulfonic acid, sulfuric acid, and phosphoric acid; calcium acetate, zinc acetate, manganese acetate, and zinc stearate; iron and zinc acetylacetonates; metal alkoxides; organometallic compounds such as alkyltin oxides, dialkyltin oxides, and organotitanium compounds; metal oxides such as tin oxide, antimony oxide, titanium oxide, and vanadium oxide; and heteropolyacids. Titanium alkoxides such as tetrabutoxytitanate, heteropolyacids, and iron acetylacetonates are preferred because they can increase the molecular weight of the resulting polyester resin.

[0059] To obtain a polyester resin, the carboxylic acid component and the alcohol component may be charged in the desired composition ratio and reacted all at once, or may be reacted stepwise to adjust the molecular weight. When using at least one selected from a polycarboxylic acid compound (A1) containing an amino group or a salt thereof and a polyhydric alcohol (A2) containing an amino group or a salt thereof, the reaction can be carried out stepwise by the following method. That is, a precursor is obtained by polycondensing a carboxylic acid component containing a cyclic dicarboxylic acid compound (B) with an alcohol component containing a cyclic dihydric alcohol (C). Here, the carboxylic acid component and the alcohol component used in the precursor preferably do not contain the polycarboxylic acid compound (A1) containing an amino group or a salt thereof and the polyhydric alcohol (A2) containing an amino group or a salt thereof. Furthermore, the carboxylic acid component and the alcohol component used in the precursor preferably further contain at least one selected from a chain dicarboxylic acid compound (D) and a chain dihydric alcohol (E). Next, the obtained precursor is polycondensed with at least one selected from a polycarboxylic acid compound (A1) containing an amino group or a salt thereof and a polyhydric alcohol (A2) containing an amino group or a salt thereof, and at least one selected from a polycarboxylic acid compound (H) and a polyhydric alcohol (I).

[0060] The precursor has a number average molecular weight of 1,500 to 5,000, preferably 2,000 to 4,000, in terms of polystyrene, as measured by gel permeation chromatography (GPC). Having a molecular weight within this range enhances the dispersibility of the polyester resin. The precursor preferably has a glass transition temperature of 40°C or higher, particularly preferably 50 to 80°C. A glass transition temperature of 40°C or higher improves the storage stability of the toner.

[0061] The polycarboxylic acid compound (H) is not particularly limited, and examples thereof include cyclic dicarboxylic acid compounds (B) such as aromatic dicarboxylic acid compounds and alicyclic dicarboxylic acid compounds, chain dicarboxylic acid compounds (D), and trivalent or higher carboxylic acid compounds (F), as described above. Among these, cyclic dicarboxylic acid compounds in which a carboxyl group or a carboxylic acid derivative group is bonded to each of two non-adjacent carbon atoms constituting a ring, such as terephthalic acid, tetrahydroterephthalic acid, and hexahydroterephthalic acid, are preferred. The polyhydric alcohol (I) is also not particularly limited, and examples thereof include cyclic dihydric alcohols (C) such as aromatic dihydric alcohols and alicyclic dihydric alcohols, chain dihydric alcohols (E), and trivalent or higher alcohols (G), as described above. The total amount of the polycarboxylic acid compound (H) or polyhydric alcohol (I) used in the copolycondensation with the precursor is preferably 10 to 50 parts by mass, particularly preferably 20 to 40 parts by mass, per 100 parts by mass of the precursor. The amount of the polycarboxylic acid compound or polyhydric alcohol is preferably within the above range, since it is possible to increase the molecular weight without impairing the melting properties.

[0062] The content of the polyester resin is preferably adjusted so that the mass ratio of the styrene-acrylic resin to the polyester-based resin (styrene-acrylic resin:polyester-based resin) is within the range of 96:4 to 70:30. This mass ratio is more preferably 96:4 to 80:20, and even more preferably 96:4 to 90:10. Here, the mass of the styrene-acrylic resin corresponds to the mass of the polymerizable monomer. When the content of the polyester resin is equal to or greater than the lower limit, the melt viscosity of the toner is sufficiently reduced, thereby improving the fixability of the toner. When the content of the polyester resin is equal to or less than the upper limit, the charge stability of the toner is good even in high-temperature, high-humidity environments, thereby suppressing the occurrence of fogging and reducing degradation in image quality. By keeping the content of the polyester resin within the above range, both the fixability of the toner and the charge stability when the environment is changed are achieved.

[0063] (Colorant) The colorant contained in the polymerizable monomer composition can be appropriately selected from colorants conventionally used in toners and is not particularly limited, and black, cyan, yellow, or magenta colorants can be used. Examples of black colorants that can be used include carbon black, titanium black, and magnetic powders such as iron zinc oxide and iron nickel oxide. Examples of cyan colorants that can be used include cyan pigments such as copper phthalocyanine pigments and their derivatives, anthraquinone pigments, and cyan dyes. Specific examples include C.I. Pigment Blue 2, 3, 6, 15, 15:1, 15:2, 15:3, 15:4, 16, 17:1, and 60; C.I. Solvent Blue 70, and the like. Examples of yellow colorants that can be used include azo pigments such as monoazo pigments and disazo pigments, yellow pigments such as condensed polycyclic pigments, and yellow dyes. Specific examples include C.I. Pigment Yellow 3, 12, 13, 14, 15, 17, 62, 65, 73, 74, 83, 93, 97, 120, 138, 155, 180, 181, 185, 186, 213, 214; C.I. Solvent Yellow 98, 162, etc. Examples of magenta colorants that can be used include azo pigments such as monoazo pigments and disazo pigments, magenta pigments such as condensed polycyclic pigments, and magenta dyes.Specifically, for example, C.I. Pigment Red 31, 48, 57:1, 58, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 144, 146, 149, 150, 163, 170, 184, 185, 187, 202, 206, 207, 209, 237, 238, 251, 254, 255, 269; C.I. Pigment Violet 19; C.I. Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; C.I. Disperse Red 9; C.I. Examples of the colorants include Solvent Violet 8, 13, 14, 21, and 27; C.I. Disper Violet 1; C.I. Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, and 40; and C.I. Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, and 28. The colorants can be used alone or in combination of two or more. In order to improve image quality, a pigment and a dye may be used in combination as the colorant. When two or more pigments are used in combination, it is preferable that the two or more pigments are mixed crystal pigments, as this allows for the formation of high-quality images. Specific examples of mixed crystal pigments include C.I. Pigment Violet 19 and C.I. Pigment Violet 20, which will be described later. Pigment Red 122 and the like.

[0064] In the case of black toner, it is preferable to contain carbon black as a colorant from the viewpoint of forming high-quality images, and in the case of cyan toner, it is preferable to contain copper phthalocyanine pigment and its derivatives as a colorant from the viewpoint of forming high-quality images.

[0065] In the yellow toner, it is preferable to contain as a colorant at least one selected from the group consisting of disazo pigments such as C.I. Pigment Yellow 93, 155, 180, 214, 219, and yellow dyes such as C.I. Solvent Yellow 98, 162, from the viewpoint of easily improving storage stability and being able to form high-quality images, and it is more preferable to contain at least one of C.I. Pigment Yellow 155, 214, and C.I. Solvent Yellow 98, and it is even more preferable to contain at least one of C.I. Pigment Yellow 214 and C.I. Solvent Yellow 98. Furthermore, in the yellow toner, it is preferable to contain as a colorant a combination of a disazo pigment and a yellow dye, from the viewpoint of easily improving storage stability and being able to form high-quality images, and it is more preferable to contain at least one of C.I. Pigment Yellow 155 and C.I. Pigment Yellow 214, and C.I. It is more preferable to contain C.I. Pigment Yellow 214 in combination with C.I. Solvent Yellow 98, and even more preferable to contain C.I. Pigment Yellow 214 in combination with C.I. Solvent Yellow 98. In addition, in the yellow toner, the mass ratio of the yellow pigment to the yellow dye contained in the yellow colorant (yellow pigment:yellow dye) is preferably within a range of 50:50 to 95:5, and more preferably within a range of 60:40 to 90:10. Here, the yellow pigment contained in the yellow colorant is preferably a disazo pigment, more preferably at least one of C.I. Pigment Yellow 155 and C.I. Pigment Yellow 214, and even more preferably C.I. Pigment Yellow 214. The yellow dye contained in the yellow colorant is preferably C.I. Solvent Yellow 98.

[0066] In magenta toners, it is preferable to contain C.I. Pigment Red 122 as a colorant, since it is possible to form high-quality images. Furthermore, it is more preferable to use C.I. Pigment Red 122 and C.I. Pigment Violet 19 in combination, and a mixed crystal of C.I. Pigment Violet 19 and C.I. Pigment Red 122 is particularly preferable. A mixed crystal of C.I. Pigment Violet 19 and C.I. Pigment Red 122 can be produced, for example, by the method described in U.S. Pat. No. 3,160,510, in which the mixed crystal components are simultaneously recrystallized from sulfuric acid or other suitable solvent, and if necessary, salt-ground and then treated with a solvent, or by the method described in German Patent Application Publication No. 1,217,333, in which a substituted diaminoterephthalic acid mixture is cyclized and then treated with a solvent. When a magenta toner contains C.I. Pigment Violet 19 and C.I. Pigment Violet 19 as colorants, it is more preferable to use C.I. Pigment Violet 19 and C.I. Pigment Violet 122 in combination. When C.I. Pigment Violet 19 and C.I. Pigment Red 122 are contained, the mass ratio of C.I. Pigment Violet 19 to C.I. Pigment Red 122 is preferably 80:20 to 20:80, more preferably 70:30 to 30:70, and even more preferably 60:40 to 40:60.

[0067] The content of the colorant is adjusted appropriately depending on the type of colorant so as to obtain a desired color, and is not particularly limited, but is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 5 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the styrene-acrylic resin contained as the binder resin.

[0068] (Release Agent) As the release agent, an ester wax is used. As the ester wax, a synthetic ester wax obtained by esterifying an alcohol and a carboxylic acid is preferred, and a polyfunctional ester wax or a monoester wax can be preferably used. The alcohol and the carboxylic acid used in synthesizing the ester wax can each be used alone or in combination of two or more. As the ester wax, a long-chain fatty acid ester wax using a long-chain fatty acid having 10 or more carbon atoms as a raw material is preferred. Since the long-chain fatty acid ester wax has a high dispersibility improving effect due to the styrene-based thermoplastic elastomer, when used in combination with the styrene-based thermoplastic elastomer, the low-temperature fixability of the toner can be particularly improved.

[0069] Among the polyfunctional ester waxes, polyfunctional ester compounds of a fatty acid having 10 to 22 carbon atoms and a polyhydric alcohol are preferred. The number of carbon atoms of the fatty acid used in the polyfunctional ester compound is more preferably 14 to 22, and even more preferably 16 to 22. The fatty acid may be a saturated fatty acid or an unsaturated fatty acid, with saturated fatty acids being preferred because of their high stability. The fatty acid may also be a monocarboxylic acid or a polycarboxylic acid, with monocarboxylic acids being preferred. Preferred examples of monocarboxylic acids include lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, and oleic acid, with stearic acid, arachidic acid, and behenic acid being preferred.

[0070] Examples of polyhydric alcohols used in the polyfunctional ester wax include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 2,4-dimethyl-2-ethylhexane-1,3-diol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1,3-propanediol, 1,3-butanediol, and 1,4-butanediol. Examples of suitable alcohols include dihydric alcohols such as hexanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, and 2,2,4-trimethyl-1,6-hexanediol; trihydric alcohols such as glycerin, trimethylolethane, and trimethylolpropane; tetrahydric alcohols such as pentaerythritol, erythritol, and diglycerin; pentahydric alcohols such as xylitol and triglycerol; hexahydric alcohols such as sorbitol and dipentaerythritol, and octahydric alcohols such as hexaglycerol. Among these, tetrahydric to octahydric polyhydric alcohols are preferred.

[0071] The polyfunctional ester wax may preferably be at least one selected from the group consisting of pentaerythritol ester compounds, glycerin ester compounds, and dipentaerythritol ester compounds. Examples of such preferred polyfunctional ester waxes include pentaerythritol ester compounds such as pentaerythritol tetrapalmitate, pentaerythritol tetrabehenate, and pentaerythritol tetrastearate; glycerin ester compounds such as hexaglycerin tetrabehenate tetrapalmitate, hexaglycerin octabehenate, pentaglycerin heptabehenate, tetraglycerin hexabehenate, triglycerin pentabehenate, diglycerin tetrabehenate, and glycerin tribehenate; and dipentaerythritol ester compounds such as dipentaerythritol hexamyristate and dipentaerythritol hexapalmitate. Among these, glycerin ester compounds are preferred. The glycerin ester compound is preferably used because it has a high effect of improving the dispersibility of the styrene-based thermoplastic elastomer and can particularly improve the low-temperature fixability of the toner when used in combination with the styrene-based thermoplastic elastomer.

[0072] Among the monoester waxes, monoester compounds of monocarboxylic acids having 10 to 22 carbon atoms and monohydric alcohols having 10 to 22 carbon atoms are preferred. The number of carbon atoms of the monocarboxylic acid is more preferably 14 to 22, even more preferably 16 to 22. The number of carbon atoms of the monohydric alcohol is also more preferably 14 to 22, even more preferably 16 to 22. Preferred examples of monocarboxylic acids include lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid (eicosanoic acid), behenic acid, and oleic acid, with palmitic acid, stearic acid, arachidic acid, and behenic acid being preferred. Preferred examples of monohydric alcohols include lauryl alcohol, myristyl alcohol, palmityl alcohol (1-hexadecanol), stearyl alcohol, arachidyl alcohol (eicosyl alcohol), behenyl alcohol, and oleyl alcohol, with palmityl alcohol, stearyl alcohol, arachidyl alcohol, and behenyl alcohol being preferred.

[0073] The monoester wax is not particularly limited, but from the viewpoint of improving the balance between the storage stability and low-temperature fixability of the toner, behenyl palmitate, behenyl stearate, behenyl eicosanoate, behenyl behenate, eicosyl palmitate, eicosyl stearate, eicosyl eicosanoate, eicosyl behenate, stearyl stearate, stearyl eicosanoate, stearyl behenate, hexadecyl eicosanoate, hexadecyl behenate, etc. are preferably used. Among these, behenyl stearate, behenyl palmitate, and stearyl behenate are particularly preferred.

[0074] The molecular weight of the ester wax is preferably in the range of 400 to 3500, more preferably in the range of 500 to 3000. When the molecular weight of the ester wax is equal to or greater than the lower limit, bleeding out of the ester wax can be suppressed, and the generation of UFP derived from the ester wax can be suppressed. When the molecular weight of the ester wax is equal to or less than the upper limit, the low-temperature fixability of the toner can be improved.

[0075] In order to improve the balance between the storage stability and low-temperature fixability of the toner, the melting point of the release agent is preferably in the range of 50°C or higher and 90°C or lower, more preferably in the range of 60°C or higher and 85°C or lower, and even more preferably in the range of 65°C or higher and 80°C or lower.

[0076] The toner of the present disclosure may further contain a release agent other than ester wax, provided that the object of the present disclosure is not impaired. Examples of release agents other than ester wax include those commonly used as toner release agents, and are not particularly limited. Examples include, for example, hydrocarbon waxes such as polyolefin waxes (e.g., polyethylene wax, polypropylene wax), synthetic waxes (e.g., Fischer-Tropsch wax), petroleum waxes (e.g., paraffin, microcrystalline wax, and petrolatum), natural waxes (e.g., candelilla, carnauba, rice, Japan wax, and jojoba), and mineral waxes (e.g., montan, ceresin, and ozokerite). When a release agent other than ester wax is contained, the content of the ester wax is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and even more preferably 99% by weight or more, based on 100% by weight of the total amount of the release agent. When the content of the ester wax is equal to or greater than the above-mentioned lower limit, deterioration of toner performance can be sufficiently suppressed. Specifically, it is possible to sufficiently suppress the deterioration of the balance between the storage stability and low-temperature fixability of the toner, the occurrence of fogging, the occurrence of uneven gloss, and the bleeding of the release agent.

[0077] In addition, from the viewpoint of improving the balance between the storage stability and low-temperature fixability of the toner, the content of the glycerin ester compound is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on 100% by mass of the release agent.

[0078] Furthermore, from the viewpoint of improving the balance between the storage stability and low-temperature fixability of the toner, the glycerin ester compound is preferably a polyglycerin ester compound such as hexaglycerin tetrabehenate tetrapalmitate, hexaglycerin octabehenate, pentaglycerin heptabehenate, tetraglycerin hexabehenate, triglycerin pentabehenate, etc. The polyglycerin used in the polyglycerin ester compound is a dehydration condensation product of glycerin, and its degree of polymerization is preferably 3 to 9.

[0079] The content of the release agent is not particularly limited, but from the viewpoint of improving the balance between the storage stability and low-temperature fixability of the toner and suppressing the occurrence of fogging, it is preferably from 1 part by mass to 30 parts by mass, more preferably from 5 parts by mass to 20 parts by mass, and even more preferably from 10 parts by mass to 15 parts by mass, relative to 100 parts by mass of the styrene-acrylic resin contained as the binder resin. The release agent may be used alone or in combination of two or more kinds.

[0080] (Release Agent Dispersant) As the release agent dispersant, a nonionic surfactant is used. The nonionic surfactant is not particularly limited, but examples thereof include polyoxyalkylene alkyl aryl ether surfactants, polyoxyalkylene distyrenated aryl ether surfactants, polyoxyalkylene alkyl ether surfactants, polyoxyalkylene alkenyl ether surfactants, polyoxyalkylene fatty acid ester surfactants, sorbitan fatty acid ester surfactants, silicone surfactants, acetylene alcohol surfactants, and fluorine-containing surfactants.

[0081] Examples of polyoxyalkylene alkyl aryl ether surfactants include polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene dodecylphenyl ether, etc. Examples of polyoxyalkylene distyrenated aryl ether surfactants include polyoxyethylene distyrenated phenyl ether, etc.

[0082] Examples of polyoxyalkylene alkyl ether surfactants include polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, and polyoxyethylene stearyl ether. Examples of polyoxyalkylene alkenyl ether surfactants include polyoxyethylene oleyl ether and polyoxyethylene methylbutenyl ether. Examples of polyoxyalkylene fatty acid ester surfactants include polyoxyethylene oleate, polyoxyethylene laurate, and polyoxyethylene distearate. Specific examples of the above-mentioned nonionic surfactants containing a polyoxyalkylene group include those in which the polyoxyalkylene group is a polyoxyethylene group, but are not limited to these. In the present disclosure, the above-mentioned nonionic surfactants containing a polyoxyethylene group in which some or all of the polyoxyethylene groups have been replaced with other polyoxyalkylene groups such as polyoxypropylene groups or polyoxybutylene groups can also be used. Examples of sorbitan fatty acid ester surfactants include sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, polyoxyethylene monooleate, and polyoxyethylene stearate.

[0083] Examples of silicone surfactants include dimethylpolysiloxane, etc. Examples of acetylene alcohol surfactants include 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, 3,5-dimethyl-1-hexyne-3-ol, etc. Examples of fluorine-containing surfactants include fluorine alkyl esters, etc.

[0084] Further examples of the nonionic surfactant include polyethylene glycol fatty acid esters, polyethylene glycol phosphate esters, fatty acid monoglycerides, polyglycerin fatty acid esters, propylene glycol fatty acid esters, sucrose fatty acid esters, polyoxyethylene-polyoxypropylene block copolymers, polyoxyethylene-polyoxypropylene alkyl ethers, ethylene oxide derivatives of alkylphenol-formalin condensates, polyoxyethylene glycerin fatty acid esters, polyoxyethylene hydrogenated castor oil, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid alkanolamides, and polyoxyethylene fatty acid amides.

[0085] Among the nonionic surfactants, polyoxyalkylene alkyl aryl ether surfactants, polyoxyalkylene distyrenated aryl ether surfactants, polyoxyalkylene alkyl ether surfactants, polyoxyalkylene alkenyl ether surfactants, and polyoxyalkylene fatty acid esters are preferred, polyoxyalkylene alkyl aryl ether surfactants and polyoxyalkylene distyrenated aryl ether surfactants are more preferred, and polyoxyalkylene distyrenated aryl ether surfactants are particularly preferred.

[0086] Furthermore, as the nonionic surfactant, a nonionic surfactant containing a polyoxyalkylene group is preferred because of its excellent effect in improving the dispersibility of ester wax. The number of repeating units of the polyoxyalkylene group is preferably 10 to 20, more preferably 12 to 18. Furthermore, examples of the polyoxyalkylene group include a polyoxyethylene group, a polyoxypropylene group, and a polyoxybutylene group, with a polyoxyethylene group being particularly preferred. Examples of the nonionic surfactant containing a polyoxyalkylene group include a polyoxyalkylene alkyl aryl ether surfactant, a polyoxyalkylene alkyl ether surfactant, a polyoxyalkylene alkenyl ether surfactant, a polyoxyalkylene distyrenated aryl ether surfactant, and a polyoxyalkylene fatty acid ester.

[0087] As the nonionic surfactant, commercially available products may be used. Examples of commercially available nonionic surfactants include those manufactured by Kao Corporation under the trade name "Emulgen A-60" (polyoxyethylene (distyrenated phenyl) ether, the average number of moles of polyoxyethylene added is 13), the trade name "Emulgen 120" (polyoxyethylene lauryl ether), the trade name "Emulgen 109P" (polyoxyethylene lauryl ether), the trade name "Emulgen 106" (polyoxyethylene lauryl ether), the trade name "Emulgen 150" (polyoxyethylene lauryl ether), the trade name "Emulgen 108" (polyoxyethylene lauryl ether), and the trade name "Latemul PD" series (polyoxyalkylene alkenyl ether having an alkenyl group having a terminal double bond, a butylene oxide group, and an ethylene oxide group), as well as those manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. under the trade name "Polyoxyethylene (20) Cetyl Ether".

[0088]

[0033] As long as the object of the present disclosure is not impaired, the release agent dispersant may further contain a cationic, anionic, or amphoteric ionic surfactant. From the viewpoints of suppressing a decrease in the charge stability of the toner, suppressing the occurrence of fog, suppressing a decrease in the storage stability of the toner, and suppressing uneven gloss in the formed image, the content of the ionic surfactant contained in the polymerizable monomer composition is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 10% by mass or less, still more preferably 5% by mass or less, and particularly preferably 1% by mass or less, relative to 100% by mass of the total amount of surfactants. That is, the content of the nonionic surfactant contained in the polymerizable monomer composition is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, and particularly preferably 99% by mass or more, relative to 100% by mass of the total amount of surfactants.

[0089] The molecular weight of the surfactant used as a release agent dispersant is preferably 100 to 500 in order to provide excellent dispersibility of the release agent.

[0090] The content of the release agent dispersant is not particularly limited, but is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 0.7 to 13 parts by mass, relative to 100 parts by mass of the release agent. The content of the nonionic surfactant is also not particularly limited, but is preferably 0.1 to 20 parts by mass, more preferably 0.4 to 15 parts by mass, and even more preferably 0.7 to 12 parts by mass, relative to 100 parts by mass of the release agent. This makes it easy for the mass of the nonionic surfactant present on the surface of the toner particles to fall within the range of 0.1 to 500 ppm relative to the mass of the toner particles.

[0091] (Charge Control Agent) The charge control agent contained in the polymerizable monomer composition can be appropriately selected from positively charged charge control agents generally used to improve the chargeability of toner, and is not particularly limited. Examples of positively charged charge control agents include charge control compounds such as nigrosine dyes, quaternary ammonium salts, triaminotriphenylmethane compounds, and imidazole compounds, as well as positively charged charge control resins. Among these, the charge control agent preferably contains a positively charged charge control resin, because it has high compatibility with the polymerizable monomer, can impart stable chargeability to toner particles, and has excellent charge stability. A functional group-containing copolymer can be used as the positively charged charge control resin. Specifically, a functional group-containing copolymer containing a structural unit containing a functional group such as an amino group, a quaternary ammonium group, or a quaternary ammonium salt-containing group can be used.

[0092] In the functional group-containing copolymer used as a positively charged charge control resin, the content of the functional group-containing structural unit relative to all structural units (sometimes simply referred to as the "functional group amount" in the present disclosure) is preferably 0.3% by mass or more and 20% by mass or less, more preferably 0.3% by mass or more and 10% by mass or less. When the functional group amount is equal to or greater than the lower limit, the toner chargeability is improved and fogging is less likely to occur, while when the functional group amount is equal to or less than the upper limit, the toner tends to have a good balance between low-temperature fixability and heat-resistant storage stability. Furthermore, when the functional group amount is too large, charging stability deteriorates and fogging is more likely to occur, but when the functional group amount is equal to or less than the upper limit, fogging is less likely to occur.

[0093] The functional group-containing copolymer may contain a combination of two or more functional group-containing copolymers with different amounts of functional groups. When two or more functional group-containing copolymers with different amounts of functional groups are contained in the colored resin particles as a charge control resin, the desired chargeability can be imparted to the toner while improving the dispersibility of the colorant. This allows the colorant to be incorporated at a high concentration, resulting in improved print density. When copolymer A, which has a relatively high amount of functional groups, and copolymer B, which has a relatively low amount of functional groups, are used in combination, the difference in functional group amounts is thought to result in a distribution in which copolymer B is unevenly distributed relatively toward the center of the colored resin particles, and copolymer A is unevenly distributed toward the surface of the colored resin particles. Since copolymer A has a higher amount of functional groups than copolymer B, it has a stronger charge-imparting effect and is unevenly distributed toward the surface of the colored resin particles, and therefore the chargeability of the toner is thought to be mainly influenced by copolymer A. On the other hand, copolymer B not only exhibits a charge-imparting effect, but is also thought to be more effective at dispersing the colorant within the colored resin particles. It is presumed that the effects of copolymer A and copolymer B impart the desired chargeability to the toner and improve the dispersibility of the colorant.

[0094] When the charge control agent contains two or more functional group-containing copolymers with different functional group contents, it is preferable to include copolymer A having a functional group content of 5% to 10% by weight and copolymer B having a functional group content of 0.3% to less than 5% by weight. The functional group content of copolymer A is preferably 5% by weight or more, more preferably 6% by weight or more, from the viewpoint of imparting a desired chargeability to the toner and improving the dispersibility of the colorant, and the upper limit is preferably 10% by weight or less, more preferably 9% by weight or less. The functional group content of copolymer B is preferably 0.3% by weight or more, more preferably 0.5% by weight or more, and the upper limit is preferably less than 5% by weight, more preferably 4% by weight or less, and even more preferably 3% by weight or less, from the viewpoint of imparting a desired chargeability to the toner and improving the dispersibility of the colorant. On the other hand, when one type of functional group-containing copolymer is used alone, the lower limit of the amount of functional groups in the functional group-containing copolymer is preferably 0.3 mass% or more, more preferably 0.5 mass% or more, and the upper limit is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 3 mass% or less, still more preferably 2.5 mass% or less, and particularly preferably 2 mass% or less.

[0095] The functional group-containing copolymer used as the positively charged charge control resin is preferably a styrene-acrylic resin because of its high compatibility with the polymerizable monomer. Here, the styrene-acrylic resin is preferably a copolymer of two or more monomers including an aromatic vinyl monomer and a (meth)acrylate monomer. In particular, the total of the structural units derived from the aromatic vinyl monomer and the structural units derived from the (meth)acrylate monomer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, of the total structural units.

[0096] The charge control resin preferably has a glass transition temperature (Tg) in the range of 50° C. to 110° C., more preferably in the range of 60° C. to 100° C. When the glass transition temperature (Tg) of the charge control resin is within the above range, the toner tends to have a good balance between low-temperature fixability and heat-resistant storage stability.

[0097] The charge control resin preferably has a weight average molecular weight Mw in the range of 5,000 to 30,000, more preferably in the range of 10,000 to 25,000. When the charge control resin has a weight average molecular weight Mw in the above range, the toner tends to have a good balance between low-temperature fixability and heat-resistant storage stability.

[0098] The content of the charge control agent is not particularly limited, but is preferably 0.01 to 15 parts by mass, and more preferably 0.03 to 8 parts by mass, relative to 100 parts by mass of the styrene-acrylic resin contained as the binder resin. When the content of the charge control agent is equal to or greater than the lower limit, the occurrence of fogging can be suppressed, while when the content is equal to or less than the upper limit, print smearing can be suppressed. The charge control agents can be used singly or in combination of two or more.

[0099] (Acidic Group-Containing Acrylic Resin) The polymerizable monomer composition may contain an acidic group-containing acrylic resin. This makes it easier to control the particle size of the colored resin particles and to suppress the generation of coarse particles. The acidic group-containing acrylic resin is preferably a copolymer of at least one selected from acrylic acid esters and methacrylic acid esters with at least one selected from acrylic acid and methacrylic acid, and more preferably a copolymer of an acrylic acid ester, a methacrylic acid ester, and acrylic acid. Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, sec-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, and neohexyl (meth)acrylate. Examples of suitable acrylic esters include alkyl (meth)acrylates such as sec-hexyl (meth)acrylate, tert-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate, as well as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, and 4-hydroxybutyl acrylate glycidyl ether. Among these, alkyl (meth)acrylates are preferred. The acrylic ester used in the acidic group-containing acrylic resin is preferably at least one selected from the group consisting of ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and n-butyl acrylate, and more preferably at least one selected from ethyl acrylate and n-butyl methacrylate.The methacrylic acid ester used in the acidic group-containing acrylic resin is preferably at least one selected from the group consisting of methyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, and n-butyl methacrylate, and more preferably methyl methacrylate.

[0100] In the acidic group-containing acrylic resin, the proportion of (meth)acrylic acid relative to 100% by mass of the total amount of the (meth)acrylic acid ester and (meth)acrylic acid used in the synthesis of the acidic group-containing acrylic resin is preferably 0.05 to 1% by mass, more preferably 0.1 to 0.6% by mass, and even more preferably 0.3 to 0.5% by mass, from the viewpoints of high compatibility with the polymerizable monomer, ease of control of the particle size of the colored resin particles, and ease of suppression of the generation of coarse particles.

[0101] The acidic group-containing acrylic resin is preferably a copolymer of monomers containing 50.0% by mass or more of methyl methacrylate relative to 100% by mass of the total mass of the monomers used in the synthesis of the copolymer, because it has high compatibility with the polymerizable monomer, makes it easy to control the particle size of the colored resin particles, and makes it easy to suppress the generation of coarse particles. The acidic group-containing acrylic resin is more preferably a copolymer of a monomer containing 50.0 to 99.9% by mass of methyl methacrylate and 0.1 to 5.0% by mass of (meth)acrylic acid, even more preferably a copolymer of a monomer containing 50.0 to 99.0% by mass of methyl methacrylate and 0.1 to 5.0% by mass of (meth)acrylic acid, still more preferably a copolymer of a monomer containing 50.0 to 98.0% by mass of methyl methacrylate, 1.0 to 5.0% by mass of an alkyl (meth)acrylate other than methyl methacrylate, and 0.1 to 5.0% by mass of (meth)acrylic acid, and particularly preferably a copolymer of a monomer containing 50.0 to 98.0% by mass of methyl methacrylate, 1.0 to 5.0% by mass of an alkyl (meth)acrylate other than methyl methacrylate, and 0.2 to 3.0% by mass of (meth)acrylic acid. As the alkyl (meth)acrylate other than methyl methacrylate, at least one selected from ethyl acrylate and butyl acrylate is preferred from the viewpoint of being able to control the glass transition temperature.

[0102] The acidic group-containing acrylic resin may contain a small amount of monomer units derived from other monomers other than (meth)acrylic acid esters and (meth)acrylic acid. From the viewpoints of easily controlling the particle size of the colored resin particles and easily suppressing the generation of coarse particles, the content of the other monomers is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the total amount of monomers used in the synthesis of the acidic group-containing acrylic resin. It is most preferable that the acidic group-containing acrylic resin does not contain the other monomers. Examples of the other monomers include halogenated aromatic vinyl monomers, polar group-containing aromatic vinyl monomers, vinyl carboxylic acid ester monomers, halogenated vinyl monomers, vinylidene halogenated monomers, vinylpyridine, ethylenically unsaturated carboxylic acid monomers, allyl glycidyl ether, aromatic vinyl monomers, monoolefin-based monomers, and diene-based monomers.

[0103] The acid value of the acidic group-containing acrylic resin is preferably 0.5 to 7.0 mgKOH / g, more preferably 1.0 to 5.0 mgKOH / g, and even more preferably 1.5 to 3.0 mgKOH / g. When the acid value of the acidic group-containing acrylic resin is within the above range, the effect of improving the heat-resistant storage stability, low-temperature fixability, and print durability of the toner is high, and the effect of suppressing the generation of coarse particles is also high.

[0104] The weight average molecular weight Mw of the acidic group-containing acrylic resin is preferably 8,000 to 45,000, more preferably 9,000 to 45,000, and even more preferably 10,000 to 40,000. When the weight average molecular weight Mw of the acidic group-containing acrylic resin is equal to or greater than the lower limit, the heat-resistant storage stability and durability of the toner can be improved, and when it is equal to or less than the upper limit, an increase in the fixing temperature of the toner can be suppressed.

[0105] The glass transition temperature (Tg) of the acidic group-containing acrylic resin is preferably 60 to 95° C., more preferably 65 to 90° C., and even more preferably 70 to 80° C. When the glass transition temperature of the acidic group-containing acrylic resin is equal to or higher than the lower limit, the heat-resistant storage stability of the toner can be improved, and when the glass transition temperature is equal to or lower than the upper limit, the low-temperature fixability of the toner can be improved.

[0106] The acidic group-containing acrylic resin may be commercially available, or may be produced by polymerizing a monomer containing the above-mentioned monomer by a known method such as solution polymerization, aqueous solution polymerization, ionic polymerization, high-temperature high-pressure polymerization, or suspension polymerization. When the acidic group-containing acrylic resin is a copolymer, the copolymer may be a random copolymer, a block copolymer, or a graft copolymer, but is preferably a random copolymer. The acidic group-containing acrylic resin is preferably pulverized to improve solubility.

[0107] The content of the acidic group-containing acrylic resin is preferably 0.5 to 2.5 parts by mass, more preferably 0.8 to 2.2 parts by mass, and even more preferably 1.0 to 2.0 parts by mass, relative to 100 parts by mass of the styrene-acrylic resin contained as the binder resin. When the content of the acidic group-containing acrylic resin is equal to or greater than the lower limit, the particle size of the colored resin particles is easily controlled and the generation of coarse particles is easily suppressed. On the other hand, when the content of the acidic group-containing acrylic resin is equal to or less than the upper limit, an increase in the fixing temperature of the toner can be suppressed.

[0108] (Styrene-based thermoplastic elastomer) The polymerizable monomer composition may further contain a styrene-based thermoplastic elastomer. The styrene-based thermoplastic elastomer can improve the dispersibility of the release agent, and thus by including the styrene-based thermoplastic elastomer, the fixability of the toner can be improved while maintaining the heat resistance temperature of the toner. Here, the styrene-based thermoplastic elastomer refers to a random, block, graft, or other copolymer of a styrene-based monomer and at least one other monomer selected from monoolefins, diolefins, and the like that can be copolymerized with the styrene-based monomer, as well as a hydrogenated product of such a copolymer.

[0109] Representative examples of the styrene-based thermoplastic elastomer used in the present disclosure include styrene-butadiene-styrene type block copolymers, styrene-butadiene type block copolymers, styrene-isoprene-styrene type block copolymers, styrene-isoprene type block copolymers, styrene-butadiene-isoprene-styrene type block copolymers, and hydrogenated products thereof; styrene-ethylene-butylene-styrene type block copolymers, styrene-ethylene-propylene-styrene type block copolymers, and styrene-ethylene-ethylene-propylene-styrene type block copolymers. Among these styrene-based thermoplastic elastomers, styrene-isoprene-styrene type block copolymers can be preferably used from the viewpoint of optimizing the balance between the storage stability and low-temperature fixability of the toner.

[0110] The content of styrene units in the styrene-based thermoplastic elastomer is preferably 15 to 70% by mass, more preferably 15 to 60% by mass, and even more preferably 20 to 40% by mass. When the styrene content is equal to or greater than the lower limit, the proportion of hydrocarbon units is not too high, making it difficult for the fixed toner to peel from the fixing surface, thereby suppressing a decrease in fixability. On the other hand, when the styrene content is equal to or less than the upper limit, compatibility with the binder resin is not too high, suppressing a decrease in the storage stability of the toner.

[0111] The weight average molecular weight Mw of the styrene-based thermoplastic elastomer is not particularly limited, but is preferably 50,000 to 350,000, and more preferably 80,000 to 250,000, from the viewpoint of being excellent in the effect of improving the fixability of the toner while maintaining the heat resistance temperature of the toner.

[0112] The styrene-based thermoplastic elastomer may be a commercially available product, such as the Quintac (registered trademark) series manufactured by Zeon Corporation and the Septon (registered trademark) series manufactured by Kuraray Co., Ltd.

[0113] The content of the styrene-based thermoplastic elastomer is not particularly limited, but is preferably 0.5 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 2 to 6 parts by mass, relative to 100 parts by mass of the styrene-acrylic resin contained as the binder resin. The styrene-based thermoplastic elastomer may be used alone or in combination of two or more types.

[0114] (Other Additives) The polymerizable monomer composition may further contain other additives as needed, as long as the object of the present disclosure is not impaired. For example, a molecular weight modifier can be preferably used as the other additive. The molecular weight modifier is not particularly limited as long as it is a molecular weight modifier that is generally used for toners. Examples include mercaptans such as t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, and 2,2,4,6,6-pentamethylheptane-4-thiol; and thiuram disulfides such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, N,N'-dimethyl-N,N'-diphenylthiuram disulfide, and N,N'-dioctadecyl-N,N'-diisopropylthiuram disulfide. The molecular weight modifiers can be used alone or in combination of two or more.

[0115] When the polymerizable monomer composition contains a molecular weight modifier, the content of the molecular weight modifier is appropriately adjusted so that the binder resin has a desired molecular weight, and is not particularly limited, but is usually 0.01 parts by mass or more and 10 parts by mass or less, and may be 0.1 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the monovinyl monomer.

[0116] The polymerizable monomer composition may further contain a polymerization initiator, which may be added to the dispersion obtained in the droplet formation step described below. In particular, it is preferable to add the polymerization initiator to the dispersion obtained by dispersing the polymerizable monomer composition in an aqueous solvent in the droplet formation step described below, in order to easily control the molecular weight of the polymer.

[0117] (A-2) Suspension Step for Obtaining a Suspension (Droplet Formation Step) Next, the polymerizable monomer composition is dispersed in an aqueous medium containing a dispersion stabilizer, a polymerization initiator is added, and then droplets of the polymerizable monomer composition are formed. As described above, the polymerization initiator may be added after the polymerizable monomer composition is dispersed in the aqueous medium and before droplet formation, or it may be added to the polymerizable monomer composition before dispersion in the aqueous medium. The method for droplet formation is not particularly limited, and may be performed using an apparatus capable of strong stirring, such as an (in-line type) emulsifying disperser (manufactured by Pacific Machinery Works, trade name: Milder) or a high-speed emulsifying disperser (manufactured by Primix Corporation, trade name: T.K. Homomixer MARK II Type).

[0118] Examples of the polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; azo compounds such as 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide), 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobisisobutyronitrile; and organic peroxides such as di-t-butyl peroxide, benzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylbutanoate, t-hexylperoxy-2-ethylbutanoate, diisopropyl peroxydicarbonate, di-t-butylperoxyisophthalate, and t-butylperoxyisobutyrate. Among these, organic peroxides are preferred because they can reduce the amount of residual polymerizable monomers and provide excellent print durability for the resulting toner. Among organic peroxides, peroxyesters are preferred because they have good initiator efficiency and can reduce the amount of residual polymerizable monomers, and non-aromatic peroxyesters, i.e., peroxyesters without an aromatic ring, are more preferred. These polymerization initiators can be used alone or in combination of two or more.

[0119] The amount of the polymerization initiator used in the polymerization reaction of the polymerizable monomer composition is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and particularly preferably 1 to 10 parts by mass, relative to 100 parts by mass of the monovinyl monomer.

[0120] In the present disclosure, the aqueous medium refers to a medium containing water as a main component. In the present disclosure, it is preferable that the aqueous medium contains a dispersion stabilizer. Examples of the dispersion stabilizer include sulfates such as barium sulfate and calcium sulfate; carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates such as calcium phosphate; metal oxides such as aluminum oxide and titanium oxide; metal hydroxides such as aluminum hydroxide, magnesium hydroxide, and ferric hydroxide; inorganic compounds such as silicon dioxide; water-soluble polymers such as polyvinyl alcohol, methyl cellulose, and gelatin; anionic surfactants; nonionic surfactants; amphoteric surfactants; and other organic compounds. These dispersion stabilizers can be used alone or in combination of two or more.

[0121] Among the above dispersion stabilizers, inorganic compounds are preferred, and as the aqueous medium containing a dispersion stabilizer, colloidal metal hydroxides of poor water solubility are particularly preferred. By using an inorganic compound, particularly a colloidal metal hydroxide of poor water solubility, it is possible to narrow the particle size distribution of the colored resin particles and reduce the amount of dispersion stabilizer remaining after washing, so that the resulting toner can reproduce images clearly and does not deteriorate in environmental stability.

[0122] (A-3) Polymerization Step After droplets of the polymerizable monomer composition are formed as described above in (A-2), the polymerizable monomer composition is subjected to a polymerization reaction in the presence of a polymerization initiator to form colored resin particles. That is, the aqueous dispersion medium in which droplets of the polymerizable monomer composition are dispersed is heated to initiate polymerization and prepare an aqueous dispersion of colored resin particles. The heating conditions are not particularly limited, but the heating temperature is preferably 50°C or higher, and more preferably 60 to 95°C. The heating time is preferably 1 to 20 hours, and more preferably 2 to 15 hours.

[0123] The colored resin particles may be used as a toner as they are or with the addition of an external additive, but it is preferable to use the colored resin particles as the core layer of so-called core-shell type (also called "capsule type") colored resin particles. Core-shell type colored resin particles have a structure in which the outside of a core layer is covered with a shell layer formed of a material different from the core layer. By covering a core layer made of a material with a low softening point with a material with a higher softening point, it is possible to improve the low-temperature fixability and storage stability of the toner in a well-balanced manner.

[0124] The method for producing the core-shell type colored resin particles using the above-mentioned colored resin particles is not particularly limited, and they can be produced by a conventionally known method. In terms of production efficiency, an in situ polymerization method or a phase separation method is preferred.

[0125] A method for producing core-shell type colored resin particles by in situ polymerization is described below: A polymerizable monomer for forming a shell layer (shell polymerizable monomer) and a polymerization initiator are added to an aqueous medium in which colored resin particles are dispersed, and the resulting mixture is polymerized to obtain core-shell type colored resin particles.

[0126] As the polymerizable monomer for the shell, the same polymerizable monomers as those described above can be used. Among them, it is preferable to use, alone or in combination, monomers that can give polymers with a Tg of more than 80°C, such as styrene, acrylonitrile, and methyl methacrylate.

[0127] Examples of the polymerization initiator used in the polymerization of the shell polymerizable monomer include water-soluble polymerization initiators such as metal persulfates, such as potassium persulfate and ammonium persulfate; and azo initiators, such as 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide) and 2,2'-azobis-(2-methyl-N-(1,1-bis(hydroxymethyl)2-hydroxyethyl)propionamide). These can be used either alone or in combination of two or more. The amount of the polymerization initiator is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, per 100 parts by mass of the shell polymerizable monomer.

[0128] The polymerization temperature for the shell layer is preferably 50° C. or higher, more preferably 60 to 95° C. The polymerization reaction time is preferably 1 to 20 hours, more preferably 2 to 15 hours.

[0129] (A-4) Washing, Filtration, Dehydration, and Drying Steps After the polymerization is completed, the aqueous dispersion of colored resin particles obtained by polymerization is preferably subjected to filtration, washing to remove the dispersion stabilizer, dehydration, and drying in a conventional manner, which are repeated several times as necessary.

[0130] As for the above-mentioned washing method, when an inorganic compound is used as the dispersion stabilizer, it is preferable to add an acid or alkali to the aqueous dispersion of the colored resin particles to dissolve and remove the dispersion stabilizer in water. When a poorly water-soluble inorganic hydroxide colloid is used as the dispersion stabilizer, it is preferable to add an acid to adjust the pH of the aqueous dispersion of the colored resin particles to 6.5 or less. The acid to be added may be an inorganic acid such as sulfuric acid, hydrochloric acid, or nitric acid, or an organic acid such as formic acid or acetic acid, but sulfuric acid is particularly preferred because of its high removal efficiency and small burden on the production equipment.

[0131] The colored resin particles are washed until the electrical conductivity of the filtrate is preferably 300 μS / cm or less, more preferably 200 μS / cm or less, and even more preferably 50 μS / cm or less. This makes it easier for the electrical conductivity of the toner extract to fall within the preferred range described below. The filtrate refers to the filtrate obtained in a series of washing steps, and is the filtrate immediately before the end of the washing steps.

[0132] The dehydration and filtration methods can be any of various known methods, and are not particularly limited. Examples include centrifugal filtration, vacuum filtration, pressure filtration, etc. The drying method is also not particularly limited, and various methods can be used.

[0133] (B) Pulverization Method When colored resin particles are produced by the pulverization method, the process is, for example, as follows. First, the binder resin, colorant, release agent, release agent dispersant, charge control agent, and other additives, such as an acidic group-containing acrylic resin and a styrene-based thermoplastic elastomer, which are added as needed, are mixed using a mixer such as a ball mill, V-type mixer, FM mixer (trade name), high-speed dissolver, internal mixer, or Fallberg mixer. Next, the mixture obtained above is kneaded while heating using a pressure kneader, a twin-screw extrusion mixer, a roller, or the like. The kneaded product is coarsely pulverized using a pulverizer such as a hammer mill, a cutter mill, or a roller mill. The resulting mixture is then finely pulverized using a pulverizer such as a jet mill or a high-speed rotary pulverizer, and then classified to the desired particle size using a classifier such as an air classifier or an airflow classifier to obtain colored resin particles produced by the pulverization method.

[0134] The binder resin, colorant, release agent, release agent dispersant, and charge control agent used in the pulverization method, as well as the acidic group-containing acrylic resin and styrene-based thermoplastic elastomer added as needed, may be the same as those listed in the (A) suspension polymerization method. Furthermore, the colored resin particles obtained by the pulverization method can also be used in a method such as in situ polymerization to produce core-shell type colored resin particles, similar to the colored resin particles obtained by the (A) suspension polymerization method.

[0135] 2. Colored Resin Particles The colored resin particles contained in the toner of the present disclosure can be obtained by the above-mentioned manufacturing method such as (A) suspension polymerization method or (B) pulverization method. The colored resin particles contained in the toner will be described below. Note that the colored resin particles described below include both core-shell type and non-core-shell type particles.

[0136] The colored resin particles contained in the toner of the present disclosure include a binder resin, a colorant, a release agent, a release agent dispersant, and a charge control agent, and may further contain other additives, such as an acidic group-containing acrylic resin or a styrene-based thermoplastic elastomer, as necessary. The binder resin includes at least a styrene-acrylic resin obtained by polymerizing the polymerizable monomers used in the suspension polymerization method described above (A) and the polyester-based resin described above. In the toner of the present disclosure, the styrene-acrylic resin and polyester-based resin contained as the binder resin are not crosslinked by covalent bonds, and relatively weak forces, such as π-π interactions or hydrogen bonds, act between the resins. This allows for the achievement of both low-temperature fixing performance and hot offset resistance, which are normally trade-offs. The acid value of the styrene-acrylic resin contained as the binder resin is typically less than 0.5 mgKOH / g and may be 0 mgKOH / g.

[0137] In the toner of the present disclosure, in addition to the above-mentioned styrene acrylic resin and polyester resin, resins such as polystyrene and epoxy resin, which have conventionally been widely used in toners, can be used as the binder resin, as long as the object of the present disclosure is not impaired. In the toner of the present disclosure, the total amount of the styrene acrylic resin and polyester resin relative to 100% by mass of the binder resin is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass.

[0138] The colorant, release agent, release agent dispersant, charge control agent, acidic group-containing acrylic resin, and styrene-based thermoplastic elastomer contained in the colored resin particles are as described above in (A) Suspension polymerization method.

[0139] The toner of the present disclosure can be prepared by using the colored resin particles as they are. However, from the viewpoint of adjusting the chargeability, fluidity, storage stability, and the like of the toner, the colored resin particles may be mixed and stirred with an external additive to perform an external addition treatment, thereby causing the external additive to adhere to the surfaces of the colored resin particles, thereby preparing the toner of the present disclosure.

[0140] The agitator used for the external addition treatment is not particularly limited as long as it is an agitator that can adhere an external additive to the surface of the colored resin particles. For example, the external addition treatment can be performed using an agitator that is capable of mixing and stirring, such as an FM Mixer (trade name, manufactured by Nippon Coke and Engineering Co., Ltd.), a Super Mixer (trade name, manufactured by Kawada Manufacturing Co., Ltd.), a Q Mixer (trade name, manufactured by Nippon Coke and Engineering Co., Ltd.), a Mechanofusion System (trade name, manufactured by Hosokawa Micron Corporation), and a Mechano Mill (trade name, manufactured by Okada Seiko Co., Ltd.).

[0141] Examples of external additives include inorganic fine particles such as silica, titanium oxide, aluminum oxide, zinc oxide, tin oxide, calcium carbonate, calcium phosphate, cerium oxide, barium titanate, and strontium titanate; and organic fine particles such as polymethyl methacrylate resin, silicone resin, and melamine resin. Among these, inorganic fine particles are preferred, and among inorganic fine particles, at least one fine particle selected from silica fine particles and titanium oxide fine particles is preferred, and silica fine particles are particularly preferred. These external additives can be used alone, but it is preferred to use two or more of them in combination.

[0142] In the toner of the present disclosure, the external additive is typically used in an amount of 0.05 to 6 parts by mass, and preferably 0.2 to 5 parts by mass, relative to 100 parts by mass of the colored resin particles. When the content of the external additive is 0.05 part by mass or more, the occurrence of transfer residue can be suppressed, and when the content of the external additive is 6 parts by mass or less, the occurrence of fogging can be suppressed.

[0143] 4. Toner Particles The toner of the present disclosure is an aggregate of “toner particles.” Each toner particle may consist of only colored resin particles, or may contain colored resin particles and an external additive attached to the surface of the colored resin particles.

[0144] In the toner of the present disclosure, the mass of the nonionic surfactant present on the surface of the toner particles is 0.1 to 500 ppm, preferably 30 to 500 ppm, relative to the mass of the toner particles. The mass of the nonionic surfactant present on the surface of the toner particles is an indicator of the amount of nonionic surfactant added as a release agent dispersant during the production of the colored resin particles. The lower limit of the mass of the nonionic surfactant present on the surface of the toner particles is 0.1 ppm or more, but is preferably 20 ppm or more, more preferably 30 ppm or more, and even more preferably 40 ppm or more. If the mass of the nonionic surfactant present on the surface of the toner particles is equal to or greater than the above lower limit, a sufficient amount of nonionic surfactant is added, and the release agent dispersibility is good, thereby reducing the melt viscosity of the toner and improving the low-temperature fixability of the toner. On the other hand, if the mass of the nonionic surfactant present on the surface of the toner particles is 500 ppm or less, deterioration of toner properties due to the surfactant present on the surface of the toner particles is suppressed. Specifically, since deterioration of charging stability is suppressed, fogging is less likely to occur. Furthermore, since blocking is suppressed, heat-resistant storage stability is improved. Furthermore, bleeding of the release agent is suppressed. The mass of the nonionic surfactant present on the surface of the toner particles is preferably less than 400 ppm, more preferably less than 300 ppm, even more preferably less than 200 ppm, still more preferably less than 100 ppm, and particularly preferably less than 90 ppm.

[0145] The mass of surfactant present on the surface of toner particles can be measured using a toner extract. The toner extract refers to a liquid obtained by adding toner to an aqueous medium and stirring the mixture to extract the water-soluble components present on the surface of the toner particles into the aqueous medium. A mixed solvent of alcohol and water is preferably used as the aqueous medium. The toner extract used to measure the mass of surfactant present on the surface of toner particles is specifically obtained by dispersing 10 g of toner in 100 mL of a mixed solvent of IPA (isopropyl alcohol) and ion-exchanged water (IPA / ion-exchanged water = 80 / 20 (volume ratio)), stirring at 50°C for 30 minutes, and then separating the liquid. When the toner extract contains a nonionic surfactant and an ionic surfactant, and the mass of only the nonionic surfactant is to be measured, the toner extract is treated with an anion exchange resin and a cation exchange resin to remove the ionic surfactant from the toner extract, and the amount of surfactant is then measured for the treated toner extract.

[0146] The mass of the surfactant contained in the toner extract can be measured by a method appropriately selected from known methods such as LC / MS (liquid chromatography-mass spectrometry), IC (ion exchange chromatography), and GC / MS (gas chromatography-mass spectrometry), depending on the type of surfactant. The mass of the nonionic surfactant used in the present disclosure can be measured by LC / MS (liquid chromatography-mass spectrometry). A specific measurement method using LC / MS is as described in the examples below.

[0147] The mass of the ionic surfactant present on the surface of the toner particles is preferably 40 ppm or less, more preferably 30 ppm or less, even more preferably 20 ppm or less, still more preferably 10 ppm or less, and particularly preferably 1 ppm or less, from the viewpoint of suppressing a decrease in the charging stability of the toner, suppressing the occurrence of fogging, suppressing a decrease in the storage stability of the toner, and suppressing uneven gloss in the formed image.

[0148] The toner of the present disclosure has a volume average particle size (Dv) of toner particles of preferably 3 to 15 μm, more preferably 4 to 12 μm. By having Dv equal to or greater than the above lower limit, the fluidity of the toner can be improved, and deterioration of transferability and reduction in image density can be suppressed. By having Dv equal to or less than the above upper limit, reduction in image resolution can be suppressed.

[0149] The particle size distribution (Dv / Dp), which is the ratio of the volume average particle size (Dv) to the number average particle size (Dp) of the toner particles, is preferably 1.0 or more and less than 1.3, and more preferably 1.0 or more and 1.2 or less. When Dv / Dp is less than 1.3, it is possible to suppress deterioration in transferability, image density, and resolution. The volume average particle size and number average particle size of the toner particles can be measured using, for example, a particle size distribution analyzer (manufactured by Beckman Coulter, product name: Multisizer) or the like.

[0150] From the viewpoint of image reproducibility, the average circularity of the toner particles is preferably 0.96 to 1.00, more preferably 0.97 to 1.00, and even more preferably 0.98 to 1.00. By having the average circularity of the toner particles equal to or greater than the above lower limit, the reproducibility of thin lines in printing can be improved. The average circularity of the toner particles is 1 or less, and when the measurement sample is a perfect sphere, the average circularity is 1. In the present disclosure, circularity is the value obtained by dividing the perimeter of a circle having the same projected area as the particle image by the perimeter of the projected image of the particle. The average circularity is an index indicating the degree of unevenness on the surface of the measurement sample and can be used as a simple method for quantitatively expressing the shape of the particles. The more complex the surface shape of the measurement sample, the smaller the average circularity value. The circularity of the toner particles can be determined, for example, by using an aqueous solution in which toner particles are dispersed as a sample liquid, taking a projected image of the toner particles in the sample liquid using a flow particle image analyzer (for example, FPIA-2100 manufactured by CIMEX Corporation), measuring the perimeter of a circle equal to the projected area of ​​the particle and the perimeter of the projected image of the particle from the projected image, and then using the following calculation formula 1. The average circularity is the average value of the circularities of the toner particles contained in the sample liquid. Calculation formula 1: (Circularity) = (Perimeter of a circle equal to the projected area of ​​the particle) / (Perimeter of the projected image of the particle)

[0151] The volume average particle diameter (Dv), number average particle diameter (Dp) and average circularity of the toner particles do not show any significant difference depending on whether or not an external additive is used. Therefore, the volume average particle diameter (Dv), number average particle diameter (Dp) and average circularity of the toner containing an external additive and the colored resin particles not containing an external additive can be considered to be the same.

[0152] In order to suppress the occurrence of fogging, the toner of the present disclosure preferably has an electrical conductivity of 50 μS / cm or less, more preferably 40 μS / cm or less, and even more preferably 30 μS / cm or less, of the toner extract. The electrical conductivity of the toner extract can be used as an indicator of the degree of cleaning. The weaker the cleaning, the more dispersion stabilizer remains in the toner. Since dispersion stabilizers usually contain ionic components, the more dispersion stabilizer remains in the toner, the higher the electrical conductivity of the toner extract. Specifically, the toner extract used to measure electrical conductivity is obtained by dispersing 10 g of toner in 100 mL of a mixed solvent of IPA and ion-exchanged water (IPA / ion-exchanged water = 80 / 20 (volume ratio)), stirring at 50°C for 30 minutes, and then separating the liquid.

[0153] The toner of the present disclosure may be used as a one-component developer consisting of only toner particles, or may be used as a two-component developer by further mixing and stirring together with carrier particles.

[0154] 5. Toner Set The toner set of the present disclosure is a color toner set including positively charged toners for developing electrostatic images of multiple colors, wherein the positively charged toners for developing electrostatic images of multiple colors include at least a yellow toner, a magenta toner, and a cyan toner, and all of the positively charged toners for developing electrostatic images of multiple colors are the positively charged toners for developing electrostatic images of the present disclosure described above. In other words, the toner set of the present disclosure is a toner set that combines the toners of the present disclosure described above.

[0155] In images containing multi-colors formed using the toner set of the present disclosure (sometimes simply referred to as "multi-color images" in this disclosure), peeling of toner layers is unlikely to occur. The reason for this is presumed to be as follows. In the toner set of the present disclosure, each toner constituting the toner set contains a combination of a styrene-acrylic resin and a polyester-based resin as the binder resin. This results in a lower melt viscosity and easier melting than when the binder resin is composed solely of a styrene-acrylic resin. Furthermore, each toner contains an ester wax as a release agent, and a specific amount of a nonionic surfactant as a release agent dispersant. This provides excellent dispersibility of the ester wax in the colored resin particles, resulting in a high plasticizing effect and easier melting. Because each toner constituting the toner set of the present disclosure is thus prone to melting, adhesion of the individual toner layers is facilitated when a multi-color image is formed using the toner set of the present disclosure. This prevents peeling of the toner layers, resulting in good multilayer fixation of the toner layers. Peeling of the toner layer refers to, for example, peeling at the interface between the toner layer and the paper surface, peeling between toner layers, and peeling within the toner layer. When at least one toner included in a toner set contains a hydrocarbon wax alone as a release agent, the compatibility between the binder resin and the release agent in the toner is so high that the release agent easily seeps onto the surface of the toner particles during toner fixation. As a result, interfacial peeling is likely to occur between toner particles forming the toner layer, which makes peeling within the toner layer more likely to occur. Furthermore, the toner set of the present disclosure can form multicolor images with excellent gloss uniformity. The reason for this is presumed to be as follows: Each toner constituting the toner set of the present disclosure uses an ester wax as a release agent, which slows the crystallization rate of the release agent when the toner is rapidly cooled after fixation. Therefore, gloss unevenness is less likely to occur in each toner layer formed using the toner set of the present disclosure. Meanwhile, in multicolor images formed using the toner set, the thickness of the entire toner layer increases due to the stacking of multiple toner layers. When a multi-color image is fixed onto a recording material, if the toner layer is not melted uniformly throughout, unevenness occurs at the interface of the toner layer, resulting in uneven gloss.In contrast, since the toners constituting the toner set of the present disclosure are prone to melting as described above, the melting of each toner layer proceeds easily during fixing, and the melting of the entire toner layer is highly uniform, so that unevenness is unlikely to occur at the interface of the toner layers. As a result, the multi-color image formed using the toner set of the present disclosure has excellent gloss uniformity.

[0156] The toner set of the present disclosure may further include, in addition to the basic color toners of yellow, cyan, and magenta, a toner of yellow, cyan, or magenta that differs in some color element such as hue, color density, brightness, or vividness, and may further include a black toner. Even when the toner set of the present disclosure includes a toner different from the basic color toners of yellow, cyan, or magenta, all of the toners constituting the toner set are the toners of the present disclosure described above. Note that the individual toners included in the toner set of the present disclosure typically exhibit different colors from each other.

[0157] 6. Image Forming Method The toner set disclosed herein is a color toner set for electrostatic image development, typically used to form a full-color image using an electrostatic image development method. Methods for forming full-color images using an electrostatic image development method can be broadly divided into the following two types based on the difference in the transfer process: (1) A method in which an original image is color-separated to obtain data for each color component, multiple single-color toner images are formed based on the data for each color component, these images are sequentially transferred onto a single transfer medium, and a full-color image is formed by color superposition on the transfer medium, and the full-color image is then transferred from the transfer medium to a recording material. (2) A method in which an original image is color-separated to obtain data for each color component, multiple single-color toner images are formed based on the data for each color component, these images are sequentially transferred onto a single recording material, and a full-color image is formed by color superposition on the recording material. The toner set disclosed herein can form multi-color images with excellent gloss uniformity and with little toner layer peeling in either method.

[0158] The present disclosure also includes the following two image forming methods. The former is a method of overlaying colors on a transfer medium, and the latter is a method of overlaying colors on a recording material. The first method is a method of forming an image using an electrostatic charge development type full-color printer with the toner set of the present disclosure, and is characterized by comprising the steps of: developing a first image, which is a primary color image formed with a first toner (first image developing step); developing a second image, which is a primary color image of each color formed with a second toner (second image developing step); transferring the first image onto the transfer medium and then transferring the second image onto the transfer medium to form an image including multi-colors on the transfer medium (color overlaying step on transfer medium); transferring the image including multi-colors formed on the transfer medium onto a recording material (multi-color image transfer step); and fixing the image including multi-colors transferred onto the recording material (fixing step).

[0159] The second method is a method of forming an image using an electrostatic charge development type full-color printer with the toner set of the present disclosure, and is characterized by having a step of developing a first image which is a primary color image formed with a first toner (first image developing step), a step of developing a second image which is a primary color image of each color formed with a second toner (second image developing step), a step of transferring the first image onto a recording material, and then transferring the second image to form an image including multi-colors on the recording material (color overlaying step on recording material), and a step of fixing the image including multi-colors formed on the recording material onto the recording material (fixing step).

[0160] In this disclosure, a "primary color" refers to a color obtained when a toner of each color is printed alone; a "secondary color" refers to a color obtained when two primary color toner images of different colors are superimposed; and a "multi-color" refers to a color obtained when primary color toner images of multiple colors are superimposed. In this disclosure, the term "toner image" literally refers to an image formed with toner, but is used particularly to emphasize that it is a visual image of the state in which toner is distributed on an image-bearing surface such as a photoreceptor, transfer medium, or recording material in accordance with the image to be reproduced. In this disclosure, a "leading color" refers to the color of the primary color toner image transferred first onto a transfer receiving material when a full-color image is formed by color superposition on a transfer receiving material by forming primary color toner images of each color using multiple toner developing machines and sequentially transferring them onto a single transfer receiving material (recording material or transfer medium). In this disclosure, a "leading developing machine" refers to a developing machine that develops the primary color toner image of the leading color. When multiple toner developing units are arranged in series along the transport path of the transfer receiving material (recording material or transfer medium) in a developing device, the first developing unit encountered by the transfer receiving material moving along the transport path is the "leading developing unit."

[0161] The toner set disclosed herein is suitable for a printing method in which electrostatic latent images corresponding to the individual primary colors are developed using multiple primary color toners, such as yellow, cyan, and magenta toners, to form individual primary color toner images on a developing machine, and the resulting individual primary color toner images are then sequentially transferred onto a transfer receiving material selected from the group consisting of a recording material and a transfer medium, thereby forming a full-color image by color superposition on the transfer receiving material. When color superposition is performed on the recording material, the individual primary color toner images are sequentially transferred onto the recording material, either directly or via an intermediate transfer process from the toner image forming surface of the developing machine to the transfer medium, to form a full-color image including multiple colors on the recording material. When color superposition is performed on the transfer medium, the individual primary color toner images are sequentially transferred onto one transfer medium, either directly or via an intermediate transfer process from the toner image forming surface of the developing machine to another transfer medium, to form a full-color image including multiple colors on the transfer medium, and then the full-color image on the transfer medium is subsequently transferred onto the recording material, either directly or via an intermediate transfer process to another transfer medium.

[0162] One of the toners contained in the toner set of the present disclosure is used as a first toner, and the other toner is used as a second toner. The first toner is a primary color toner that is transferred first onto a transfer receiving material selected from the group consisting of a recording material and a transfer medium in a process of color overlay on a transfer receiving material. The second toner is a primary color toner that is transferred second or later in the process of color overlay on a transfer receiving material. The first toner is typically selected from the group consisting of a yellow toner, a cyan toner, and a magenta toner, and the second toner is typically selected from the group consisting of a yellow toner, a cyan toner, a magenta toner, and a black toner. Note that each toner typically exhibits a different color.

[0163] Examples of the transfer medium on which color superposition is performed include an intermediate transfer belt, an intermediate transfer roll, etc. In addition, examples of the recording material include recording paper such as plain paper, as well as coated paper, art paper, and OHP sheets, and are not particularly limited.

[0164] An example of an image forming apparatus capable of carrying out the above-described procedure is a full-color printer in which multiple developing units corresponding to the respective colors of toner contained in a toner set are arranged in series, and primary color images (color separation images) of each color generated by each developing unit are transferred onto a single recording material, either directly from the individual developing units or sequentially via a transfer medium, to form an image including secondary or higher colors on the recording material. This is a type of printer with a so-called tandem arrangement. FIG. 1 is a schematic diagram illustrating an example of the structure of an image forming apparatus to which the toner set of the present disclosure can be applied. Note that the image forming method of the present disclosure is not limited to that shown in the figure. Furthermore, the structure, dimensions, and shape of the materials used in the method of the present disclosure are not limited to those shown in these figures.

[0165] The image forming apparatus 100 shown in FIG. 1 is a tandem printer. The image forming apparatus 100 includes a conveyance path 4 for the recording material R, four developing units (1Y, 1M, 1C, and 1K) corresponding to the colors yellow (Y), magenta (M), cyan (C), and black (K), pairs of transfer media (2Y, 2M, 2C, and 2K) and support rolls (3Y, 3M, 3C, and 3K) for each developing unit, an exposure device 5 that irradiates laser light in accordance with primary color image data obtained by color separation of an original image, and pairs of fixing rolls 6 and support rolls 7. The four developing units (1Y, 1M, 1C, and 1K) corresponding to each color are arranged in series along the conveyance direction D of the recording material R within the image forming apparatus. The four developing units are arranged in the following order from the upstream side of the conveyance direction: yellow developing unit 1Y, magenta developing unit 1M, cyan developing unit 1C, and black developing unit 1K.

[0166] The configuration of the developing machine will be described using the yellow developing machine 1Y as an example. The developing machine 1Y has a drum-shaped photoconductor 11Y, and is surrounded by a charging roll 12Y that charges the surface of the photoconductor to a predetermined potential, a laser light irradiation unit 13Y that irradiates the photoconductor 11Y with laser light generated by an exposure device to form an electrostatic image, a developing unit 14Y that supplies charged toner to the electrostatic image to develop it, a roll-shaped transfer medium 2Y to which the developed toner image is transferred, and a cleaning unit 15Y that removes toner remaining on the photoconductor 11Y after the toner image has been transferred to the transfer medium. The developing unit 14Y is also connected to a toner storage unit 16Y by a yellow toner supply path. Similarly, the developing machines for the other colors are equipped with photosensitive members (11M, 11C, 11K), charging rolls (12M, 12C, 12K), laser light irradiation units (13M, 13C, 13K), developing units (14M, 14C, 14K), cleaning units (15M, 15C, 15K), and toner storage units (16M, 16C, 16K), and transfer media (2M, 2C, 2K) are arranged around the photosensitive members together with these components.

[0167] A method for forming an image using the image forming apparatus 100 will now be described. In this apparatus, yellow toner is selected as the first toner and used in the first developing unit 1Y. Magenta (M), cyan (C), and black (K) toners are used as second toners in the second and subsequent developing units. First, in the yellow developing unit 1Y, the surface of the photoconductor 11Y is uniformly charged by the charging roll 12Y. Photoconductors typically have high resistance (the resistance of ordinary resins), but when irradiated with laser light, the resistivity of the irradiated portion changes. Therefore, the exposure device 5 generates a laser beam according to the yellow primary color image data, and the laser beam irradiation unit 13Y irradiates the charged surface of the photoconductor 1Y. The laser beam irradiates the photosensitive layer on the surface of the photoconductor 11Y, thereby forming an electrostatic latent image corresponding to the yellow primary color image on the surface of the photoconductor 11Y. The electrostatic latent image is a negative latent image because it is formed by the residual charge in the areas not irradiated with the laser beam.

[0168] The electrostatic latent image on the photoconductor 11Y moves to the position of the developing unit 14Y as the photoconductor rotates, where it is developed to obtain a yellow primary color toner image. The yellow primary color toner image on the photoconductor moves to the primary transfer position as the photoconductor rotates. At the primary transfer position, the surface of the photoconductor 11Y and the surface of the transfer medium 2Y come into contact, where the yellow primary color toner image on the photoconductor is primarily transferred to the surface of the transfer medium 2Y. The yellow primary color toner image on the transfer medium 2Y moves to a position where the yellow is secondary transferred as the transfer medium rotates. At the secondary transfer position, the recording material R on the conveying path 4 is sandwiched between the transfer medium 2Y and the support roll 3Y, where the surface of the transfer medium 2Y comes into contact with the image receiving surface of the recording material R, where the yellow primary color toner image on the transfer medium 2Y is secondary transferred to the recording material R.

[0169] Next, the magenta developing unit 1M performs a procedure similar to that for forming the yellow primary color toner image. That is, in the magenta developing unit 1M, a magenta primary color toner image is formed on the surface of the photoreceptor 11M, and is primarily transferred to the surface of the transfer medium 2M. The rotation of the transfer medium 2M moves the magenta primary color toner image to a position for secondary transfer. Meanwhile, from the upstream side of the conveying path 4, the portion of the recording material R on which the yellow primary color toner image has been formed moves to a position for secondary transfer of magenta. There, the magenta primary color toner image on the transfer medium 2M is aligned with the yellow primary color toner image on the recording material R and is secondary transferred to the recording material R.

[0170] Next, the cyan developing unit 1C and the black developing unit 1K perform a procedure similar to that for forming a yellow primary color toner image. Then, primary color toner images of yellow (Y), magenta (M), cyan (C), and black (K) are superimposed in this order on the recording material R moving along the conveyance path, thereby obtaining a full-color image including multiple colors. After the recording material R passes through the developing units of all colors and an image including multiple colors is formed, the recording material R moves to a position where a fixing process is performed. There, the recording material R is sandwiched between the fixing roll 6 and the support roll 7, where the image including multiple colors is fixed onto the recording material.

[0171] The present disclosure will be further described in detail below with reference to examples and comparative examples, but the present disclosure is not limited to these examples. Note that parts and percentages are by mass unless otherwise specified. Furthermore, the weight-average molecular weight Mw and number-average molecular weight Mn of the resin were determined in polystyrene equivalent terms by GPC. The sample for measurement was prepared by dissolving the polymer in tetrahydrofuran (THF) to a concentration of 2 mg / mL, sonicating for 10 minutes, and then passing the solution through a 0.45 μm membrane filter. The measurement conditions were: temperature: 40°C, solvent: tetrahydrofuran, flow rate: 1.0 mL / min, concentration: 0.2 wt%, sample injection volume: 100 μL, and a GPC TSKgel Multipore HXL-M (30 cm x 2 columns) manufactured by Tosoh Corporation was used.

[0172] [Production Example 1: Production of Magenta Pigment A] 2,9-dimethylquinacridone (C.I. Pigment Red 122) was synthesized by cyclization of 2,5-di-(4-methylphenylamino)terephthalic acid in phosphoric acid. Water was added to the resulting phosphoric acid dispersion of 2,9-dimethylquinacridone, which was then filtered and washed with water. Water was added again to the washed 2,9-dimethylquinacridone to prepare an aqueous dispersion with a 20% solids content. Similarly, an aqueous dispersion of quinacridone (C.I. Pigment Violet 19) with a 20% solids content was prepared using 2,5-diphenylaminoterephthalic acid. 250 parts of ethanol were added to 250 parts of the aqueous dispersion of dimethylquinacridone (C.I. Pigment Red 122) with a 20% solids content and 250 parts of the aqueous dispersion of quinacridone (C.I. Pigment Violet 19) with a 20% solids content to prepare a pigment mixture. This mixture was transferred to a vessel equipped with a condenser, and the pigment was reacted for 5 hours under heating and reflux while being ground. After the reaction was completed, the pigment was filtered out from the reaction mixture, washed, dried, and then ground to obtain Magenta Pigment A, which is a magenta pigment mixed crystal (i.e., a mixed crystal of C.I. Pigment Red 122 and C.I. Pigment Violet 19). The mass ratio of the pigments contained in the mixed crystal was C.I. Pigment Red 122:C.I. Pigment Violet 19=1:1.

[0173] [Production Example 2: Production of Polyester Resin (1)] 536 parts of 4-methyl-hexahydrophthalic anhydride, 100 parts of bis(β-hydroxyethyl)hexahydroterephthalate, 30 parts of dimethyl 5-aminohexahydroisophthalate, 284 parts of hydrogenated bisphenol A, and 150 parts of ethylene glycol were placed in a three-neck flask equipped with a stirrer, thermometer, reflux condenser, water separator, and nitrogen gas inlet. The ratio of the total hydroxyl value [X] to the total acid value [Y] was 1.07. The mixture was stirred while introducing nitrogen gas, and the reaction was carried out at 200°C for 3 hours while removing the alcohol produced during the reaction. Next, 5 parts of tetrabutoxy titanate was added, the reaction temperature was raised to 220°C, and the pressure in the flask was gradually reduced to 5 mmHg or less after 1.5 hours. The reaction was then continued for another 3 hours to obtain Polyester Resin (1). The resulting polyester resin (1) had a number average molecular weight of 3,000, a weight average molecular weight of 14,000, a hydroxyl value of 38 mgKOH / g, and a glass transition temperature of 65°C.

[0174] [Production Example 3: Production of Polyester Resin (2)] 93 parts of 1,4-cyclohexanedicarboxylic acid, 7 parts of 1,3,5-cyclohexanetricarboxylic acid, 60 parts of hydrogenated bisphenol A, and 40 parts of 1,4-cyclohexanediol were placed in a three-neck flask equipped with a stirrer, thermometer, reflux condenser, water separator, and nitrogen gas inlet. The mixture was stirred while introducing nitrogen gas, and the reaction was carried out at 200°C for 5 hours while removing water generated during the reaction. Next, 0.5 parts of iron acetylacetonate was added, the reaction temperature was raised to 220°C, and the pressure in the flask was gradually reduced to 5 mmHg or less after 1.5 hours. The reaction was continued for another 5 hours to obtain Polyester Resin (2). The resulting Polyester Resin (2) was a pale yellow, transparent solid with a number average molecular weight of 8,500, a weight average molecular weight of 28,000, and a glass transition temperature of 62°C.

[0175] [Production Example 4: Production of Acidic Group-Containing Acrylic Resin P1] 200 parts of toluene were charged into a reaction vessel, and the atmosphere inside the reaction vessel was thoroughly purged with nitrogen while stirring the toluene. The toluene was then heated to 90°C. Subsequently, a mixed solution of 97.0 parts of methyl methacrylate, 2.6 parts of ethyl acrylate, 0.4 parts of acrylic acid, and 3 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name: Perbutyl O) was added dropwise to the reaction vessel over 2 hours. The mixture was then held under toluene reflux for 10 hours to complete the polymerization, after which the solvent was distilled off under reduced pressure. In this way, an acidic group-containing acrylic resin P1 (MMA / EA / AA) was obtained. The resulting acidic group-containing acrylic resin P1 had an acid value of 2.5 mgKOH / g, a Tg of 74°C, and an Mw of 12,600.

[0176] Example 1 1. Production of Colored Resin Particles (1) Preparation of Core Polymerizable Monomer Composition: 74 parts of styrene, 26 parts of n-butyl acrylate, 0.1 part of a polymethacrylic acid ester macromonomer (manufactured by Toagosei Chemical Industry Co., Ltd., product name: AA-6, Tg = 94°C) as a binder resin, 5 parts of the polyester resin (1) obtained in Production Example 2 above, 0.50 parts of tetraethyl thiuram disulfide as a molecular weight modifier, and a yellow pigment (6.5 parts of C.I. Pigment Yellow 214 and 1.5 parts of C.I. Solvent Yellow 98) as a colorant were wet-pulverized using a media-type disperser (manufactured by Asada Iron Works Co., Ltd., product name: Picomil). To the mixture obtained by the wet pulverization, 12.0 parts of synthetic ester wax 1 (hexaglycerin octabehenate, melting point 70°C) as a release agent and 0.1 parts of nonionic surfactant A (polyoxyethylene (distyrenated phenyl) ether, trade name: Emulgen A-60, manufactured by Kao Corporation, average number of moles of polyoxyethylene added: 13) as a release agent dispersant were added, and they were mixed. Thereafter, to the resulting mixture, 5.0 parts of a styrene acrylic resin (functional group amount 0.5% by mass) containing a quaternary ammonium salt as a charge control resin, 2.0 parts of a styrene thermoplastic elastomer (styrene-isoprene-styrene type block copolymer, styrene unit content: 24% by mass, weight average molecular weight Mw: 106,000, manufactured by Zeon Corporation, trade name: Quintac 3270), and 1.0 part of the acidic group-containing acrylic resin P1 obtained in Production Example 4 above were added, mixed, and dissolved to prepare a polymerizable monomer composition for a core.

[0177] (2) Preparation of aqueous dispersion medium: On the other hand, an aqueous solution prepared by dissolving 7.3 parts of sodium hydroxide in 50 parts of ion-exchanged water was gradually added to an aqueous solution prepared by dissolving 10.4 parts of magnesium chloride in 280 parts of ion-exchanged water under stirring to prepare a magnesium hydroxide colloidal dispersion.

[0178] (3) Preparation of polymerizable monomer for shell: Separately, 2 parts of methyl methacrylate and 130 parts of water were subjected to a fine dispersion treatment using an ultrasonic emulsifier to prepare an aqueous dispersion of polymerizable monomer for shell.

[0179] (4) Granulation step: The core polymerizable monomer composition was added to the magnesium hydroxide colloidal dispersion (magnesium hydroxide amount: 5.3 parts), and the mixture was further stirred, followed by addition of 6 parts of t-butylperoxy-2-ethylbutanoate as a polymerization initiator. The dispersion containing the polymerization initiator was dispersed at a rotation speed of 15,000 rpm using an in-line emulsifying disperser (manufactured by Pacific Machinery Works, Ltd., trade name: Milder) to form droplets of the core polymerizable monomer composition.

[0180] (5) Suspension polymerization step: A dispersion containing droplets of the core polymerizable monomer composition was placed in a reactor, and the temperature was raised to 90°C to carry out a polymerization reaction. After the polymerization conversion rate reached approximately 100%, a solution prepared by dissolving 0.1 parts of 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide] (manufactured by Wako Pure Chemical Industries, Ltd., trade name: VA-086, water-soluble initiator) as a shell polymerization initiator in the aqueous dispersion of the shell polymerizable monomer was added to the reactor. Next, the temperature was maintained at 95°C for 4 hours to further continue polymerization, and the reaction was then stopped by water cooling to obtain an aqueous dispersion of core-shell type colored resin particles.

[0181] (6) Post-treatment step: While stirring the aqueous dispersion of colored resin particles, sulfuric acid was added to the dispersion until the pH reached 4.5 or less, followed by acid washing (30°C, 10 minutes). The colored resin particles were filtered out, washed with water, and the washed water was filtered. The electrical conductivity of the filtrate was 10 μS / cm. The colored resin particles were then dehydrated and dried to obtain dried colored resin particles.

[0182] 2. Toner Production 0.2 parts of hydrophobized silica fine particles having an average particle size of 7 nm, 0.76 parts of hydrophobized silica fine particles having an average particle size of 20 nm, and 1.91 parts of hydrophobized silica fine particles having an average particle size of 50 nm were added to 100 parts of colored resin particles, and mixed using a high-speed mixer (manufactured by Nippon Coke & Engineering Co., Ltd., product name: FM Mixer) to prepare the toner of Example 1.

[0183] [Examples 2 to 3] Toners of Examples 2 and 3 were obtained in the same manner as in Example 1, except that in "(1) Preparation of Core Polymerizable Monomer Composition" in "1. Production of Colored Resin Particles" above, the type of colorant was changed according to Table 1 below. The cyan pigment used in Example 2 was C.I. Pigment Blue 15:3. The magenta pigment A used in Example 3 was the magenta pigment A obtained in Production Example 1 above.

[0184] [Examples 4 to 7 and Comparative Examples 2, 3, 5, and 6] The toners of Examples 4 to 7 and Comparative Examples 2, 3, 5, and 6 were obtained in the same manner as in Example 1, except that in "(1) Preparation of Core Polymerizable Monomer Composition" in "1. Production of Colored Resin Particles" above, the type and / or amount of the release agent dispersant was changed according to Table 1 or Table 2 below. The nonionic surfactant B used in Example 4 was polyoxyethylene lauryl ether (trade name: EMULGEN 120, manufactured by Kao Corporation). The nonionic surfactant C used in Example 5 was polyoxyethylene lauryl ether (trade name: EMULGEN 109P, manufactured by Kao Corporation). The anionic surfactant A used in Comparative Example 5 was NEOGEN (registered trademark) (trade name, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., linear alkylbenzenesulfonate sodium or alphaolefinsulfonate sodium). The cationic surfactant A used in Comparative Example 6 was alkylbenzyldimethylammonium chloride (trade name: Sanizol (registered trademark) B50, manufactured by Kao Corporation). In Comparative Example 2, no release agent dispersant was added.

[0185] [Examples 8, 9 and Comparative Example 1] Toners of Examples 8 and 9 and a toner of Comparative Example 1 were obtained in the same manner as in Example 1, except that in "(1) Preparation of Core Polymerizable Monomer Composition" in "1. Production of Colored Resin Particles" above, the type or amount of polyester resin added was changed according to Table 1 or Table 2 below. The polyester resin (2) used in Example 9 was the polyester resin (2) obtained in Production Example 3 above. In Comparative Example 1, no polyester resin was added.

[0186] Comparative Example 4 A toner of Comparative Example 4 was obtained in the same manner as in Example 1, except that in "(1) Preparation of Core Polymerizable Monomer Composition" of "1. Production of Colored Resin Particles" above, the type of release agent was changed according to Table 2 below. The hydrocarbon wax used in Comparative Example 4 was a natural gas-based Fischer-Tropsch wax (trade name: FT-100, manufactured by Shell MDS) having an endothermic peak temperature of 93°C, a weight average molecular weight of 1,000, and a number average molecular weight of 670.

[0187] [Example 10] A toner of Example 10 was obtained in the same manner as in Example 1, except that in "(1) Preparation of core polymerizable monomer composition" in "1. Production of colored resin particles" above, the type of colorant was changed according to Table 3 below, and no styrene-based thermoplastic elastomer was added. The magenta pigment A used in Example 10 was the magenta pigment A obtained in Production Example 1 above.

[0188] [Example 11] A toner of Example 11 was obtained in the same manner as in Example 1, except that in the above "(1) Preparation of polymerizable monomer composition for core" of "1. Production of colored resin particles", the amount of nonionic surfactant A added was changed according to Table 3 below.

[0189] Example 12 A toner of Example 12 was obtained in the same manner as in Example 1, except that in Example 1, in "(1) Preparation of polymerizable monomer composition for core" in "1. Production of colored resin particles", 5.0 parts of a styrene acrylic resin containing a quaternary ammonium salt (functional group amount 15% by mass, trade name: FCA-201-PS, manufactured by Fujikura Chemical Industries, Ltd.) was used as the charge control resin instead of 5.0 parts of a styrene acrylic resin containing a quaternary ammonium salt (functional group amount 0.5% by mass).

[0190] [Examples 13 to 14] Toners of Examples 13 to 14 were obtained in the same manner as in Example 1, except that in "(1) Preparation of Core Polymerizable Monomer Composition" of "1. Production of Colored Resin Particles" above, the type of release agent was changed according to Table 3 below. Note that Ester Wax 2 listed in Table 3 below is pentaerythritol tetrabehenate (melting point 76°C), and Ester Wax 3 is behenyl stearate (melting point 67°C).

[0191] [Example 15] A toner of Example 15 was obtained in the same manner as in Example 1, except that in Example 1, 5 parts of C.I. Pigment Blue 15:3 was used instead of the yellow pigment (6.5 parts of C.I. Pigment Yellow 214 and 1.5 parts of C.I. Solvent Yellow 98) in "(1) Preparation of Core Polymerizable Monomer Composition" in "1. Production of Colored Resin Particles".

[0192] [Example 16] A toner of Example 16 was obtained in the same manner as in Example 1, except that in Example 1, 8 parts of C.I. Pigment Red 122 was used instead of the yellow pigment (6.5 parts of C.I. Pigment Yellow 214 and 1.5 parts of C.I. Solvent Yellow 98) in "(1) Preparation of Core Polymerizable Monomer Composition" in "1. Production of Colored Resin Particles".

[0193] [Examples 17 to 18] Toners of Examples 17 to 18 were obtained in the same manner as in Example 1, except that in "(1) Preparation of core polymerizable monomer composition" in "1. Production of colored resin particles", the amounts of ester wax 1 and nonionic surfactant A added were changed according to Table 3 below.

[0194] [Examples 19 and 20] Toners of Examples 19 and 20 were obtained in the same manner as in Example 1, except that in "(1) Preparation of core polymerizable monomer composition" in "1. Production of colored resin particles", the type and amount of release agent added were changed according to the following Table 3. The hydrocarbon wax listed in Table 3 is the same as that used in Comparative Example 4.

[0195] [Examples 21 to 23] Toners of Examples 21 to 23 were obtained in the same manner as in Example 1, except that in "(1) Preparation of Core Polymerizable Monomer Composition" in "1. Production of Colored Resin Particles" above, the type and amount of release agent dispersant added were changed according to Table 3 below. Note that the nonionic surfactant D listed in Table 3 is polyoxyalkylene alkenyl ether (trade name: Latemul PD-420, manufactured by Kao Corporation), the anionic surfactant B is sodium polyoxyethylene lauryl ether sulfate (manufactured by Kao Corporation), and the anionic surfactant C is dodecylbenzenesulfonic acid.

[0196] [Measurement and Evaluation of Toner] (1) Average Circularity 10 ml of ion-exchanged water was placed in a container, 0.2 g of a surfactant aqueous solution (manufactured by Fujifilm Corporation, product name: Drywell) was added as a dispersant, and 0.2 g of toner was then added. The mixture was dispersed in an ultrasonic disperser at 60 W for 3 minutes. The toner particle concentration at the time of measurement was adjusted to 3,000 to 10,000 particles / μL, and 1,000 to 10,000 toner particles with a circle-equivalent diameter of 0.4 μm or more were measured using a flow particle image analyzer (manufactured by Sysmex Corporation, product name: FPIA-2100). The average circularity was calculated from the measured values. The circularity is expressed by the following formula, and the average circularity was taken as the average value: (Circularity) = (Perimeter of a circle equal to the projected area of ​​the particle) / (Perimeter of the projected image of the particle).

[0197] (2) Volume Average Particle Size (Dv), Number Average Particle Size (Dp), and Particle Size Distribution (Dv / Dp) Approximately 0.1 g of toner was weighed and placed in a beaker, and 0.1 mL of a surfactant aqueous solution (manufactured by Fujifilm Corporation, product name: Drywell) was added as a dispersant. 10 to 30 mL of Isoton II was further added to the beaker, and the mixture was dispersed for 3 minutes using a 20 W (Watt) ultrasonic disperser. After that, the volume average particle size (Dv) and number average particle size (Dp) of the toner particles were measured using a particle size distribution analyzer (manufactured by Beckman Coulter, Inc., product name: Multisizer) under the conditions of an aperture diameter of 100 μm, a medium of Isoton II, and a particle number of 100,000 particles, and the particle size distribution (Dv / Dp) was calculated.

[0198] (3) Heat Resistance Temperature 10 g of toner was placed in a 100 mL polyethylene container and sealed. The container was then submerged in a thermostatic water bath whose temperature was set to a predetermined value, varying by 1°C from 50°C. After 8 hours, the container was removed. The toner was transferred from the container onto a 42-mesh sieve, minimizing vibration, and then placed in a powder measuring instrument (manufactured by Hosokawa Micron Corporation, trade name: Powder Tester (registered trademark) PT-R). The sieve amplitude was set to 1.0 mm, and the sieve was vibrated for 30 seconds. The mass of the toner remaining on the sieve was measured and recorded as the mass of the aggregated toner. The maximum temperature at which the mass of the aggregated toner became 0.5 g or less was recorded as the heat resistance temperature of the toner. The higher the heat resistance temperature, the less likely the toner is to block during storage, and the better the storage stability. According to the following evaluation criteria, A, B, and C indicate excellent storage stability, with D being a failure. (Evaluation criteria for heat resistance temperature) A: 59°C or higher B: 56°C or higher but lower than 59°C C: 53°C or higher but lower than 56°C D: Lower than 53°C

[0199] (4) Fixing Temperature: Using a commercially available printer with a non-magnetic single-component development system modified to allow the temperature of the fixing roll to be changed, the temperature of the fixing roll was changed in 5°C increments starting from 120°C, and the toner fixation rate was measured at each temperature. The temperature-fixation rate relationship was determined, and the lowest temperature at which a fixation rate of 80% or higher was obtained was defined as the toner fixation temperature. The lower the fixation temperature, the better the toner's low-temperature fixability. The fixation rate was calculated from the image density ratio before and after a rubbing test on a solid area of ​​a printed test paper. If the image density before the rubbing test is ID(before) and the image density after the rubbing test is ID(after), then the fixation rate (%) = [ID(after) / ID(before)] x 100. The rubbing test was performed by attaching the test area to a fastness tester with adhesive tape, placing a 500g load on it, and rubbing five times back and forth with a rubbing pin wrapped in cotton cloth. According to the following evaluation criteria, A, B, and C indicate excellent low-temperature fixability, with D being a failure. (Evaluation criteria for fixing temperature) A: Less than 155°C B: 155°C or more and less than 170°C C: 170°C or more and less than 185°C D: 185°C or more

[0200] (5) Initial Fog Test: Print paper was loaded into a commercially available non-magnetic single-component development printer (print speed: 30 sheets / min), toner was loaded into the development device, and the printer was left in a high-temperature, high-humidity (H / H) environment at 35°C and 80% RH for 24 hours. Then, three consecutive prints were made at 5% print density under the same conditions. A solid white print (0% print density) was then performed. The printer was stopped midway through the solid white print, and the toner in the non-image area on the photoreceptor after development was transferred to adhesive tape (manufactured by Sumitomo 3M Limited, product name: Scotch Mending Tape 810-3-18), which was then affixed to the print paper. The whiteness (B) of the print paper with the adhesive tape affixed was then measured using a whiteness meter (manufactured by Nippon Denshoku Co., Ltd.). Similarly, unused adhesive tape alone was affixed to the print paper, and its whiteness (A) was measured. The difference in whiteness (B - A) was taken as the fog value. A smaller fog value indicates less fog and better. In the following evaluation criteria, A, B, and C indicate better fog resistance, with D being a failure. (Initial fog evaluation criteria) A: Fog value is 0 or more and less than 2 B: Fog value is 2 or more and less than 4 C: Fog value is 4 or more and less than 8 D: Fog value is 8 or more

[0201] (6) Gloss Unevenness Toner was placed in a commercially available printer using a non-magnetic one-component development method, and a 5 cm x 5 cm square solid print was performed on printing paper in an environment of 23°C temperature and 50% humidity. During this process, the development bias voltage was changed to change the amount of development M / A, which is the amount of toner on the printing paper. The amount of development M / A was calculated using the following formula by removing an unfixed image from the printer and blowing away the toner developed on the printing paper with air. M / A (mg / cm 2 ) = (W 1 -W 2 ) / 25cm 2 W 1 = Weight of the printed paper before toner is blown off (mg) W 2 = Weight of the printed paper after toner has been blown off (mg) M / A = 0.35 mg / cm 2The gloss of a 5 cm x 5 cm square solid printed fixed image was measured. Specifically, the gloss values ​​were measured at a total of five points, the four corners and the center of the resulting 5 cm square solid area, using a gloss meter (manufactured by Nippon Denshoku Industries, product name: VGS-SENSOR) at an incident angle of 60°. The maximum and minimum gloss values ​​of the five points were determined, and the average of the five gloss values ​​was calculated using the following formula: Gloss Unevenness (%) = {(Maximum value - Minimum value) / Average value} x 100. In the following evaluation criteria, A, B, and C indicate less gloss unevenness and are evaluated as good, with D being a failure. (Evaluation criteria for gloss unevenness) A: Gloss unevenness less than 20% B: Gloss unevenness 20% to less than 25% C: Gloss unevenness 25% to less than 30% D: Gloss unevenness 30% or more

[0202] (7) Amount of Surfactant on the Toner Particle Surface (7-1) Extraction of Nonionic Surfactant In Examples 1 to 23 and Comparative Examples 1 to 4, 10 g of toner was dispersed in 100 mL of a mixed solvent of IPA and ion-exchanged water (IPA / ion-exchanged water = 80 / 20 (volume ratio)), stirred at 50°C for 30 minutes, and then the liquid was separated to prepare a toner extract. The resulting toner extract was then treated with a weakly basic anion exchange resin (DIAION WK10, manufactured by Mitsubishi Chemical) and a weakly acidic cation exchange resin (DIAION WK20, manufactured by Mitsubishi Chemical). The treated toner extract was used to measure the amount of surfactant, as described below. The treatment with the ion exchange resin was intended to remove the ionic surfactant. Since no ionic surfactant was used in Examples 1 to 9, Comparative Examples 1 to 4, Examples 10 to 20, and Example 23, the presence or absence of the treatment with the ion exchange resin did not affect the results of the surfactant amount measurement. On the other hand, in Examples 21 and 22, the anionic surfactant was removed by the treatment with the ion exchange resin, and the amount of only the nonionic surfactant could be measured.

[0203] (7-2) Extraction of Ionic Surfactant In Comparative Examples 5 and 6 and Examples 21 and 22, a toner extract was prepared in the same manner as in the extraction of the nonionic surfactant described above, and the toner extract prepared without treatment with an ion exchange resin was used as is for measuring the amount of surfactant, as described below. In Comparative Examples 5 and 6, only an ionic surfactant was used as the release agent dispersant, which made it possible to measure the amount of ionic surfactant. In Examples 21 and 22, the toner extract contained both a nonionic surfactant and an ionic surfactant, so the amount of the ionic surfactant alone was measured by assigning the peak of the ionic surfactant to the peak of each material alone.

[0204] (7-3) Measurement of surfactant amount The amount of surfactant contained in the toner extract was measured by liquid chromatography-mass spectrometry (LC / MS). The specific measurement method is as follows. First, each material contained in the toner was measured by LC / MS to identify the peak (molecular weight) attributed to each material. Next, the toner extract was measured by LC / MS, and the amount of surfactant was determined by removing the peaks of materials other than the surfactant from the peaks detected in the toner extract based on the results of the individual materials previously measured. The LC / MS measurement conditions are shown below. (LC / MS measurement conditions) Liquid chromatograph mass spectrometer: UPLC H-Class, Xevo G2-XS QTof (Waters) LC conditions Apparatus: UPLC H-Class Column: ACQUITY UPLC C8 1.7 μm, 2.1 × 100 mm Column temperature: 40°C Mobile phase: A: 0.1% formic acid, B: MeOH containing 0.1% formic acid Flow rate: 0.5 mL / min Injection volume: 2 μL MS conditions Apparatus: Xevo G2-XS Q-Tof Ionization mode: ESI positive / negative Capillary voltage: 1.0 kV / 2.5 kV Desolvation gas: 1000 L / hr, 500°C Cone gas: 50 L / hr Cone voltage: 40 V (offset 80 V) Collision energy: 2 eV Measurement range: m / z 100-1000 Measurement mode: MS Sensitivity Mode (resolution / 30,000) MS / MS conditions Collision energy Low Energy: 6 eV High Energy: 30 eV to 50 eV (ramp start to end) The amount of the long-chain fatty acid-polyether nonionic surfactant having 12 to 22 carbon atoms can be approximately determined from the intensity of the peak at m / z = 160-320 derived from the long-chain fatty acid having 12 to 22 carbon atoms.

[0205] (8) Electrical Conductivity of Toner Extract 10 g of toner was dispersed in 100 mL of a mixed solvent of IPA and ion-exchanged water (IPA / ion-exchanged water = 80 / 20 (volume ratio)), stirred at 50°C for 30 minutes, and then the liquid was separated to prepare a toner extract. The electrical conductivity of the obtained toner extract was measured at a temperature of 25±0.5°C using an electrical conductivity meter (manufactured by Horiba, Ltd., product name "ES-12"). The ion-exchanged water used had an electrical conductivity of 0.8 μS / cm or less.

[0206]

[0207]

[0208]

[0209] [Discussion] The toner of Comparative Example 1 did not contain a polyester resin as a binder resin, and therefore had poor low-temperature fixability. The toner of Comparative Example 2 did not contain a release agent dispersant, and therefore also had poor low-temperature fixability. The toner of Comparative Example 3 contained a large amount of nonionic surfactant as a release agent dispersant, and therefore the mass of nonionic surfactant present on the toner particle surface exceeded 500 ppm, resulting in poor heat-resistant storage stability and a tendency for fogging to occur. The toner of Comparative Example 4 did not contain an ester wax as a release agent, but contained a hydrocarbon wax, and the mass of nonionic surfactant present on the toner particle surface exceeded 500 ppm, resulting in a tendency for fogging to occur and gloss unevenness to occur. Hydrocarbon waxes have a fast crystallization rate when rapidly cooled after toner fixing, which is thought to be why they are prone to gloss unevenness. Furthermore, hydrocarbon waxes have difficulty dissolving surfactants, and the surfactants separated and localized on the surface, which is thought to be why the toner of Comparative Example 4 had a high amount of nonionic surfactant present on the toner particle surface. The toners of Comparative Examples 5 and 6 were prone to fog because they used an ionic surfactant instead of a nonionic surfactant as the release agent dispersant. This is thought to be because the ionic surfactant has a greater effect on the toner chargeability than the nonionic surfactant, making the toner chargeability unstable.

[0210] On the other hand, the toners of Examples 1 to 9 were positively charged toners according to the present disclosure, containing a styrene acrylic resin and a polyester resin as the binder resin, an ester wax as the release agent, and a nonionic surfactant as the release agent dispersant, with the mass of the nonionic surfactant present on the toner particle surface being 30 to 500 ppm relative to the mass of the toner particles. Therefore, the toners of Examples 1 to 9 were toners with excellent low-temperature fixability and heat-resistant storage stability, and were less susceptible to fog, enabling the formation of images with minimal gloss unevenness. In particular, a comparison of Examples 1 to 5 showed that when nonionic surfactant A (polyoxyalkylene distyrene-substituted aryl ether surfactant) was used as the release agent dispersant, the resulting toners tended to have excellent low-temperature fixability and heat-resistant storage stability. Furthermore, a comparison of Examples 1 to 6 and 8 to 9 with Example 7 showed that the occurrence of fog was more easily suppressed when the mass of the nonionic surfactant present on the toner particle surface was less than 400 ppm. Furthermore, a comparison between Example 1 and Example 9 showed that when polyester resin (1) having a number average molecular weight of 8,000 or less and a weight average molecular weight of 20,000 or less is used as the polyester resin, the toner obtained tends to have excellent low-temperature fixing properties and is less likely to cause fogging than when polyester resin (2) having a number average molecular weight of more than 8,000 and a weight average molecular weight of more than 20,000 is used.

[0211] The toners of Examples 10 to 23 were positively charged toners according to the present disclosure, containing a styrene-acrylic resin and a polyester-based resin as the binder resin, an ester wax as the release agent, and a nonionic surfactant as the release agent dispersant, with the mass of the nonionic surfactant present on the toner particle surface being 0.1 to 500 ppm relative to the mass of the toner particles. Therefore, the toners of Examples 10 to 23 were toners with excellent low-temperature fixability and heat-resistant storage stability, and were resistant to fog, and were able to form images with little gloss unevenness. Furthermore, Examples 10, 11, and 12 demonstrated that the toners of the present disclosure exhibited an excellent balance between low-temperature fixability and heat-resistant storage stability, were resistant to fog, and were able to form images with excellent gloss uniformity, even when they did not contain a styrene-based thermoplastic elastomer, had a mass of the nonionic surfactant of less than 30 ppm, or had a large amount of functional groups in the charge control resin. Furthermore, a comparison between Example 10 and Example 1 showed that the toner of the present disclosure, when containing a styrene-based thermoplastic elastomer, improved low-temperature fixability and suppressed gloss unevenness. Examples 13 and 14 showed that the above-mentioned effects could be obtained even when a polyfunctional ester wax or monoester compound other than a glycerin ester compound was used as a release agent. On the other hand, a comparison between Examples 13, 14, and 1 showed that using a glycerin ester compound as a release agent provided the best balance between the toner's storage stability and low-temperature fixability. A comparison between Example 15 and Example 2 showed that the above-mentioned effects could be obtained even when the amount of colorant was changed. A comparison between Example 16 and Example 3 showed that the toner of the present disclosure, even when using C.I. Pigment Red 122 alone as a colorant, also provided the above-mentioned effects. Examples 17 and 18 showed that the toner of the present disclosure could improve the dispersibility of the release agent by adjusting the amount of release agent dispersant added depending on the release agent content, thereby achieving a good balance between the toner's storage stability and low-temperature fixability. On the other hand, the results of Example 17 showed that when the content of the release agent is small, the fixing temperature tends to be high, and the results of Example 18 showed that when the content of the release agent is large, blocking and fogging are likely to occur.Examples 19 and 20 show that the toner of the present disclosure can achieve the above-described effects even when the release agent contains two or more ester waxes or a combination of an ester wax and a hydrocarbon wax. Examples 21 and 22 show that the toner of the present disclosure can achieve the above-described effects even when the release agent dispersant contains a combination of a nonionic surfactant and an ionic surfactant. Example 23 shows that the toner of the present disclosure can achieve the above-described effects even when the release agent dispersant contains two or more nonionic surfactants.

[0212] [Toner Set] Toner sets 1 to 10 were prepared by combining the top color toner to be transferred first, the other color toner 1 to be transferred second, and the other color toner 2 to be transferred third according to Table 4. Each toner set was evaluated as follows.

[0213] [Evaluation of Gloss Unevenness] A commercially available non-magnetic single-component development printer (printing speed: 20 pages / min) was loaded with print paper and a developing device equipped with multiple toner developers. Each toner developer was loaded with a leading color toner, other color toner 1, or other color toner 2 according to Table 4. Overlapping printing was performed under an environment of 23°C temperature and 50% humidity, resulting in a 5 cm x 5 cm square tertiary color solid print (print density 100%) at a position 0.5 cm from the leading edge in the paper feed direction. A primary color image formed with the leading color toner, a primary color image formed with other color toner 1, and a primary color image formed with other color toner 2 were transferred onto the print paper in this order to form a tertiary color image. The development bias voltage was also changed to change the amount of development M / A, which is the amount of toner on the print paper. The amount of development M / A was calculated by removing the unfixed image from the printer, blowing off the toner developed on the print paper with air, and using the following formula: M / A (mg / cm 2 ) = (W 1 -W 2 ) / 25cm 2 W 1 = weight of the printed paper before toner is blown off (mg), W 2 = weight (mg) of the printed paper after the toner has been blown off. M / A = 0.70 mg / cm 2The unfixed tertiary color image was fixed onto the print paper using a fixing roll at 160°C, obtaining a 5 cm x 5 cm square tertiary color solid print fixed image. A total of five points, the four corners and the center of the resulting 5 cm square solid area, were measured for gloss using a gloss meter (manufactured by Nippon Denshoku Industries, product name: VGS-SENSOR) at an incident angle of 60°. The maximum and minimum gloss values ​​were determined from the five points, and the average of the five gloss values ​​was calculated using the following formula: Gloss Unevenness (%) = {(Maximum value - Minimum value) / Average value} x 100. According to the following evaluation criteria, A, B, and C indicate less gloss unevenness and are evaluated as good, with D being a failure. (Evaluation criteria for gloss unevenness) A: Gloss unevenness less than 20% B: Gloss unevenness 20% to less than 25% C: Gloss unevenness 25% to less than 30% D: Gloss unevenness 30% or more

[0214] [Peeling Evaluation] A commercially available non-magnetic single-component development printer (printing speed: 20 pages / min) was modified to allow the temperature of the fixing roll to be changed. Printing paper and a developing device equipped with multiple toner developers were installed in each printer. The leading color toner, other color toner 1, or other color toner 2 was loaded into each toner developer according to Table 4. Overlapping printing was performed under an environment of 23°C temperature and 50% humidity, resulting in a 5 cm x 20 cm rectangular tertiary color solid print (print density 100%) located 0.5 cm from the leading edge in the paper feed direction. The primary color image formed with the leading color toner, the primary color image formed with other color toner 1, and the primary color image formed with other color toner 2 were transferred onto the printing paper in this order to form a tertiary color image. The temperature of the fixing roll was also changed in 5°C increments from 200°C to 150°C, and tertiary color solid prints were obtained for each fixing temperature. The obtained solid prints of tertiary colors were visually inspected for the occurrence of peeling at the interface between the toner layer and the paper surface, peeling between toner layers, or peeling within the toner layer. The temperature of the fixing roll (fixing temperature) during printing of the print where peeling occurred was determined as the peeling temperature. The evaluation method was rated into four levels: A, B, C, and D. The lower the peeling temperature, the better the multilayer fixing of the toner layer is, and the more peeling can be evaluated as being suppressed. Therefore, the order of excellent multilayer fixing can be evaluated as A, B, and C, with D being a failure. (Evaluation criteria for peeling) A: Peeling temperature is 160°C or lower B: Peeling temperature is greater than 160°C and less than 165°C C: Peeling temperature is greater than 165°C and less than 170°C D: Peeling temperature is greater than 170°C

[0215]

[0216] [Discussion] In Toner Sets 1 to 6, all of the color toners constituting the toner sets were toners of the present disclosure, and therefore, in the multi-color images (solid prints of tertiary colors) formed using Toner Sets 1 to 6, there was little uneven gloss and the peeling temperature was low, i.e., peeling of the toner layer was suppressed.

[0217] On the other hand, because Toner Set 7 contained the toner (Y-8) of Comparative Example 1, which did not contain a polyester resin as a binder resin, the multi-color image formed using Toner Set 7 had greater gloss unevenness than the images formed using Toner Sets 1 to 6. This is presumably because the toner (Y-8) of Comparative Example 1 was difficult to melt, causing unevenness at the interface of the toner layer formed with this toner (Y-8). Furthermore, the multi-color image formed using Toner Set 7 was prone to toner layer peeling. This is presumably because the toner (Y-8) was difficult to melt, resulting in insufficient adhesion at the interface of the toner layer formed with this toner (Y-8). Because Toner Set 8 contained the toner (Y-9) of Comparative Example 2, which did not use a release agent dispersant, the multi-color image formed using Toner Set 8 had greater gloss unevenness than the images formed using Toner Sets 1 to 6. This is presumably because the dispersion of the ester wax in the toner (Y-9) of Comparative Example 2 was non-uniform, making it difficult for the toner (Y-9) to melt, resulting in unevenness at the interface of the toner layer formed by the toner (Y-9). Furthermore, the multi-color image formed using Toner Set 8 was prone to toner layer peeling. This is presumably because the toner (Y-9) was difficult to melt, resulting in insufficient adhesion of the toner layer formed by the toner (Y-9). Because Toner Set 9 contained the toner (Y-10) of Comparative Example 3, in which the mass of nonionic surfactant present on the surface of the toner particles exceeded 500 ppm, the multi-color image formed using Toner Set 9 was prone to toner layer peeling. This is presumably because the amount of nonionic surfactant added in the toner (Y-10) of Comparative Example 3 was too large, causing the dispersion of the release agent to become too fine, which made it easier for the release agent to seep out to the surface of the toner particles when the toner was fixed, resulting in interfacial peeling between the toner particles forming the toner layer. Toner set 10 contained the toner (Y-11) of Comparative Example 4, which contained only a hydrocarbon wax as a release agent, and therefore the multi-color image formed using toner set 10 had significant gloss unevenness. This is presumably because the crystallization rate of the hydrocarbon wax contained in the toner (Y-11) of Comparative Example 4 was fast.Furthermore, the multi-color image formed using Toner Set 10 was more susceptible to toner layer peeling than the images formed using Toner Sets 1 to 6. This is thought to be because, in the toner (Y-11) of Comparative Example 4, the compatibility between the binder resin and the release agent was too high, causing the release agent to bleed onto the surface of the toner particles when the toner was fixed, resulting in interfacial peeling between the toner particles.

Claims

1. A positively charged toner for developing electrostatic images, which contains colored resin particles including a binder resin, a colorant, a release agent, a release agent dispersant, and a charge control agent, wherein the binder resin contains a styrene acrylic resin and a polyester resin, the release agent contains an ester wax, and the release agent dispersant contains a nonionic surfactant, and the mass of the nonionic surfactant present on the surface of the toner particles is 30 to 500 ppm relative to the mass of the toner particles.

2. A positively charged toner for developing electrostatic images, which contains colored resin particles including a binder resin, a colorant, a release agent, a release agent dispersant, and a charge control agent, wherein the binder resin contains a styrene acrylic resin and a polyester resin, the release agent contains an ester wax, and the release agent dispersant contains a nonionic surfactant, and the mass of the nonionic surfactant present on the surface of the toner particles is 0.1 ppm or more and less than 30 ppm relative to the mass of the toner particles.

3. The positively charged toner for developing electrostatic images according to claim 1 or 2, wherein the charge control agent contains a charge control resin.

4. The positively charged toner for developing electrostatic images according to claim 1 or 2, wherein the mass ratio of the styrene-acrylic resin to the polyester-based resin (styrene-acrylic resin:polyester resin) is from 96:4 to 70:

30.

5. The positively charged toner for developing electrostatic images according to claim 1 or 2, wherein the colored resin particles further contain a styrene-based thermoplastic elastomer.

6. A positively charged toner for developing electrostatic images according to claim 1 or 2, wherein the toner particles have an average circularity of 0.96 or more, and the particle size distribution (Dv / Dp), which is the ratio of the volume average particle size (Dv) to the number average particle size (Dp) of the toner particles, is less than 1.

3.

7. The positively charged toner for developing electrostatic images according to claim 1 or 2, wherein the ester wax contains a polyfunctional ester compound of a fatty acid having 10 to 22 carbon atoms and a polyhydric alcohol.

8. A color toner set including a plurality of colored positively charged toners for developing electrostatic images, the plurality of colored positively charged toners for developing electrostatic images including at least a yellow toner, a magenta toner and a cyan toner, and all of the plurality of colored positively charged toners for developing electrostatic images being the positively charged toner for developing electrostatic images according to any one of claims 1 to 7.

9. An image forming method, comprising forming an image using the toner set according to claim 8.

Citation Information

Patent Citations

  • Fuel vacuum cleaner

    DE1217333B

  • Toner for electrostatic charge image development

    JP2016206387A

  • Image forming apparatus and process cartridge

    JP2021086067A

  • toner

    JP2022164798A

  • Quinacridone pigment compositions

    US3160510A

Cited By

  • Toner set for developing electrostatic images

    JP2026177343A