Negative electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery using same

The use of SiO_x combined with optimized carbon-based active materials in the negative electrode of lithium ion secondary batteries addresses the limitations of graphite by minimizing expansion and contraction, resulting in improved energy density and cycle stability.

WO2024202298A1PCT designated stage expired Publication Date: 2024-10-03AESC JAPAN LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/044960
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-12-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional lithium ion secondary batteries using graphite as the negative electrode active material face limitations in further improving energy density and cycle characteristics due to expansion and contraction during charging and discharging, which affects the lifespan and capacity retention.

Method used

A negative electrode for non-aqueous electrolyte secondary batteries comprising a silicon-based active material (SiO_x) combined with specific carbon-based active materials, where the average particle diameters are optimized to minimize expansion and contraction, enhancing packing density and cycle stability.

Benefits of technology

The optimized negative electrode structure improves energy density and cycle capacity retention by suppressing expansion and contraction, leading to enhanced performance in lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

An objective of the present invention is to suppress the expansion and contraction when charging and discharging a nonaqueous electrolyte secondary battery, including lithium ion secondary batteries, when an Si-based negative electrode active material is used, to improve the lifespan (cycle characteristics) of the nonaqueous electrolyte secondary battery, and to improve rapid charging properties. The negative electrode active material contains: a silicon-based active material (A) containing SiOx (in the formula, x is a number satisfying 0.5≤x≤1.6); a carbon-based active material (B) composed of secondary particles formed by aggregating primary particles; and a carbon-based active material (C) composed of primary particles different from the primary particles of the carbon-based active material (B). If the value of the maximum average particle diameter among the average particle diameters is D50max and the value of the minimum average particle diameter among the average particle diameters is D50 min, the value of D50max / D50min is smaller than 2.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery using the same

[0001] The present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery using the negative electrode for a non-aqueous electrolyte secondary battery.

[0002] Non-aqueous electrolyte secondary batteries have been put to practical use as automotive batteries, including hybrid vehicles and electric vehicles, and are also used as batteries for small electronic devices, including mobile terminals. Lithium-ion secondary batteries, in particular, are widely used as such batteries. Lithium-ion secondary batteries are required to combine various characteristics, such as output characteristics, energy density, capacity, lifespan, and high-temperature stability. In particular, improving the volumetric energy density and increasing the capacity of batteries is an urgent issue, particularly in order to reduce the size of batteries. In particular, lithium-ion secondary batteries for electric vehicles are required to have improved energy density in order to further extend the driving range. To this end, various improvements have been made to the battery configuration, including the electrodes and electrolyte.

[0003] Graphite is known to be used as a negative electrode active material for lithium-ion secondary batteries. Graphite is widely used because it is inexpensive, exhibits little degradation during battery charge-discharge cycles, and is highly safe. However, conventional lithium-ion secondary batteries using graphite as a negative electrode active material are unlikely to achieve further improvements in energy density, and therefore, a search for higher-capacity negative electrode active materials has begun. Silicon-based negative electrode active materials containing silicon or silicon oxide (hereinafter, sometimes referred to as "Si-based negative electrode active materials" or "Si-based negative electrode active materials") have attracted attention as high-capacity negative electrode active materials.

[0004] For example, Patent Document 1 discloses a negative electrode active material, SiO x Patent Document 2 discloses a lithium ion secondary battery using three types of negative electrode active materials, including graphite having an average particle size of more than 15 μm and not more than 25 μm, and graphite having an average particle size of 8 μm or more and 15 μm or less, the surfaces of which are coated with amorphous carbon. xA negative electrode containing particles and a carbon material including flake graphite is disclosed.

[0005] JP 2016-219275 A JP 2019-29311 A

[0006] In Patent Document 1, when Li ions are introduced into the negative electrode, SiO x In addition, Patent Document 2 also describes the use of graphite particles having an average particle size of 8 μm or more and 15 μm or less, and graphite particles having an average particle size of 8 μm or more and 15 μm or less, and the use of graphite particles in combination improves cycle characteristics. x It is disclosed that the most preferable lower limit of the ratio of the particle diameter (rc) of the flake graphite to the D50 particle diameter (rs) of the particles, rc / rs, is 2.3. However, these conditions are not sufficient to suppress the loss of contact between the active material particles due to repeated expansion and contraction of the negative electrode during charging and discharging of the lithium ion secondary battery.

[0007] An object of the present invention is to suppress expansion and contraction during charge and discharge of nonaqueous electrolyte secondary batteries, including lithium ion secondary batteries, when a Si-based negative electrode active material is used, and to improve the life (cycle characteristics) of the nonaqueous electrolyte secondary batteries.

[0008] One embodiment of the present invention is a negative electrode for a non-aqueous electrolyte secondary battery, including a negative electrode active material layer containing a negative electrode active material, a binder, and a conductive additive. The negative electrode contains a negative electrode active material, a binder, and a conductive additive, and the negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6), a carbon-based active material (B) consisting of secondary particles formed by aggregation of primary particles, and a carbon-based active material (C) consisting of primary particles different from the primary particles of the carbon-based active material (B), wherein the average particle diameters of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) are each D50 A [μm], D50 B [μm], and D50 C The largest average particle diameter among these average particle diameters is defined as D50 [μm]. maxThe smallest average particle diameter among these average particle diameters is defined as D50 min When this is done, D50 max / D50 min The value of is smaller than 2.

[0009] The negative electrode for a non-aqueous electrolyte secondary battery of the present invention suppresses expansion and contraction even when a Si-based negative electrode active material is used, and it is possible to provide a negative electrode for a non-aqueous electrolyte secondary battery that is excellent in rapid charge and discharge, and a non-aqueous electrolyte secondary battery using the negative electrode.

[0010] Embodiments of the present invention are described below. One embodiment is a negative electrode for a non-aqueous electrolyte secondary battery, which includes a negative electrode active material layer containing a negative electrode active material, a binder, and a conductive additive. The negative electrode contains a negative electrode active material, a binder, and a conductive additive, and the negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6), a carbon-based active material (B) consisting of secondary particles formed by aggregation of primary particles, and a carbon-based active material (C) consisting of primary particles different from the primary particles of the carbon-based active material (B), wherein the average particle diameters of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) are each D50 A [μm], D50 B [μm], and D50 C The largest average particle diameter among these average particle diameters is defined as D50 [μm]. max The smallest average particle diameter among these average particle diameters is defined as D50 min When this is done, D50 max / D50 min The value of is smaller than 2.

[0011] In the embodiment, a nonaqueous electrolyte secondary battery is a battery that uses mainly an organic solvent-based electrolyte and can be repeatedly charged and discharged. Examples of nonaqueous electrolyte secondary batteries include lithium-ion secondary batteries. A nonaqueous electrolyte secondary battery includes a negative electrode for a nonaqueous electrolyte secondary battery as a component. In the embodiment, the negative electrode is a thin plate-like or sheet-like battery component in which a mixture containing a negative electrode active material is applied or rolled and dried to a negative electrode current collector, which is a metal foil such as copper foil, to form a negative electrode active material layer. That is, the negative electrode is composed of a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material applied to both sides of the negative electrode current collector. In the embodiment, the negative electrode active material layer preferably includes a negative electrode active material, a binder, and a conductive additive. The negative electrode active material is a substance used in a negative electrode that participates in a reaction that generates electrical energy. The binder is generally a substance that binds negative electrode active material particles to ensure electrical contact between particle-shaped negative electrode active materials. The conductive additive is a material that reduces the resistance of the electrode.

[0012] In an embodiment, the negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6), and a carbon-based active material. Here, the silicon-based active material (A) has the chemical formula SiO x The silicon oxide in the formula is a silicon oxide represented by the formula: where x is a number satisfying 0.5≦x≦1.6. The silicon-based active material may be a single compound or a mixture of multiple compounds. The silicon-based active material (A) is preferably in the form of particles having approximately uniform or irregular sizes. The negative electrode active material may further contain a lithium silicon compound. The lithium silicon compound is represented by the chemical formula: Li 4.4 Si, Li 3.75 Si and Li 4 SiO 4The lithium silicon compound is a compound containing lithium and silicon, such as lithium silicate. Lithium silicon compounds are stable compounds and do not release lithium during charging and discharging of a non-aqueous electrolyte secondary battery. Therefore, by using them in combination with a silicon-based active material that is prone to volume changes during charging and discharging of a non-aqueous electrolyte secondary battery, it is possible to suppress volume changes in the negative electrode active material layer. Furthermore, the silicon-based active material (A) may be doped with lithium in advance. When a lithium silicon compound or lithium-doped silicon is present, the average particle size of the silicon-based active material (A) refers to the overall average particle size of these silicon-containing compounds, unless otherwise specified. In this specification, the average particle size of the silicon-based active material (A) is defined as D50 A It is expressed as "Da". A silicon-based active material having an average particle diameter of 7 μm to 13 μm can be used as the silicon-based active material (A) of this embodiment. In this specification, the particle diameter of the particles of the negative electrode active material is represented as Da [μm], which is the particle diameter when the cumulative particle volume from the small particle side reaches a [%] of the previous particle volume based on the volume-based particle size distribution. D50 is the particle diameter (unit: μm) when the cumulative particle volume from the small particle side reaches 50 [%] of the previous particle volume based on the volume-based particle size distribution, and this refers to the average particle diameter.

[0013] The negative electrode active material further includes a carbon-based active material. The carbon-based active material is preferably natural graphite, artificial graphite, hard carbon, soft carbon, or any mixture thereof. Here, graphite is a carbon material with hexagonal plate-like crystals, and is sometimes called graphite, etc. Natural graphite and artificial graphite include natural graphite coated with amorphous carbon and artificial graphite coated with amorphous carbon. Here, amorphous carbon refers to a carbon material that is amorphous overall, with a random network structure of microcrystals, which may have a structure similar to that of graphite in part. Examples of amorphous carbon include carbon black, coke, activated carbon, carbon fiber, hard carbon, soft carbon, and mesoporous carbon. When artificial graphite is used, the interlayer distance d value (d 002) is preferably 0.33 nm or more. The crystal structure of artificial graphite is generally thinner than that of natural graphite. When artificial graphite is used as a negative electrode active material for a non-aqueous electrolyte secondary battery, particularly a lithium ion secondary battery, it is necessary that the artificial graphite has an interlayer distance that allows lithium ions to be inserted. The interlayer distance that allows lithium ions to be inserted and removed is the d value (d 002 ), and if the d value is 0.33 nm or more, lithium ions are inserted and extracted without any problems. In the embodiment, it is preferable to include at least two types of carbon-based active materials. The two types of carbon-based active materials are referred to as carbon-based active material (B) and carbon-based active material (C), respectively. The carbon-based active material (B) is preferably a carbon-based active material consisting of secondary particles formed by aggregation of primary particles. The carbon-based active material (B) is preferably artificial graphite whose surface is coated with amorphous carbon. The carbon-based active material (C) is a carbon-based active material whose primary particles are different from the primary particles of the carbon-based active material (B), and the primary particles do not aggregate to form secondary particles. The carbon-based active material (C) is preferably artificial graphite whose surface is not coated. In this specification, the average particle diameter of the carbon-based active material (B) is defined as D50 B and the average particle diameter of the carbon-based active material (C) is expressed as D50 C (both units are μm). A carbon-based active material having an average particle size of 10 to 30 μm can be used as the carbon-based active material (B) of this embodiment, and a carbon-based active material having an average particle size of 6 to 25 μm can be used as the carbon-based active material (C) of this embodiment.

[0014] In this embodiment, the average particle diameter D50 of each of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C) A [μm], D50 B [μm], and D50 C The maximum average particle diameter of [μm] is D50 max The smallest average particle diameter among these average particle diameters is defined as D50 min When this is done, D50 max / D50 minIt is preferable that the value of is smaller than 2. By combining negative electrode active materials having such an average particle size relationship, the packing density of the negative electrode active material particles is optimized, and it becomes possible to suppress expansion and contraction during charge and discharge.

[0015] Furthermore, with regard to the composition of the negative electrode active material, it is particularly preferable that the content of the silicon-based active material (A) is greater than 5% by mass and less than 50% by mass relative to the total amount of the negative electrode active material in the negative electrode active material layer. More preferably, the content of the silicon-based active material (A) is greater than 10% by mass and less than 20% by mass. If the content of the silicon-based active material (A) is too high, the volume change of the negative electrode active material during charge and discharge of the nonaqueous electrolyte secondary battery becomes large, which is undesirable. Furthermore, if the content of the silicon-based active material (A) is too low, it is difficult to achieve the effect of increasing energy density.

[0016] The above-mentioned negative electrode active material can improve electrical contact by binding particles together with a binder. The binder preferably contains poly(meth)acrylic acid, a metal salt of poly(meth)acrylic acid, an alkyl ester of poly(meth)acrylic acid, or any mixture thereof. Compounds suitable as binders include, for example, polyacrylic acid, polymethacrylic acid; sodium polyacrylate, potassium polyacrylate, sodium polymethacrylate, potassium polymethacrylate; ethyl polyacrylate, ethyl polyacrylate, butyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, and butyl polymethacrylate, and any mixture thereof may also be used. The binder content is preferably 2% by mass or more and less than 10% by mass with respect to the total solid content of the negative electrode active material layer. If the binder content is too high, a large portion of the active material surface will be covered with the binder, which may result in a decrease in ionic conductivity and electronic conductivity. Furthermore, if the binder content is too low, there is a risk that the electrical contact between the negative electrode active material particles will not be properly achieved.

[0017] In addition to the above compounds, it is particularly preferred that the binder component further contains carboxymethylcellulose (referred to as "CMC"), a cellulose derivative, or a metal salt of carboxymethylcellulose (e.g., sodium carboxymethylcellulose, potassium carboxymethylcellulose). Carboxymethylcellulose or a metal salt of carboxymethylcellulose serves to stabilize the binder compound and also stabilize the electrical contact of the negative electrode active material. When CMC or a metal salt of CMC is further added as a binder component, the content of CMC or a metal salt of CMC is preferably 0.05% by mass or more and 1.5% by mass or less, particularly 0.08% by mass or more and 0.8% by mass or less, and even more preferably 0.15% by mass or more and 0.30% by mass or less, based on the total solid content of the negative electrode active material layer.

[0018] In an embodiment, it is preferable that the content of the silicon-based active material (A) is 5% by mass or more and 50% by mass or less, and the content of the binder is 2% by mass or more and 8% by mass or less, relative to the total solid content of the negative electrode active material layer. It is more preferable that the content of the silicon-based active material (A) is 10% by mass or more and 20% by mass or less, relative to the total solid content of the negative electrode active material layer, and the content of the binder is 2% by mass or more and 6% by mass or less, relative to the total solid content of the negative electrode active material layer. It is even more preferable that the content of the silicon-based active material (A) is 15% by mass or more and 20% by mass or less, relative to the total solid content of the negative electrode active material layer, and the content of the binder is 2.5% by mass or more and 3.8% by mass or less, relative to the total solid content of the negative electrode active material layer. By appropriately adjusting the contents of the silicon-based active material (A) and the binder, the energy density of the nonaqueous electrolyte secondary battery can be improved.

[0019] The negative electrode active material layer preferably further contains a conductive additive. Examples of the conductive additive include carbon fibers such as carbon nanofibers, carbon blacks such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, and carbon nanotubes. In an embodiment, it is particularly preferable to use carbon nanotubes (hereinafter referred to as "CNTs") as the conductive additive. CNTs are substances in which a six-membered ring network of carbon atoms (graphene) has a single-layer or multi-layer coaxial tubular structure, and include single-wall carbon nanotubes (hereinafter referred to as "single-layered" or "SWCNTs") and multi-walled carbon nanotubes (hereinafter referred to as "multi-layered" or "MWCNTs"). While any CNT may be used, it is preferable to use an aggregated SWCNT, in which SWCNTs are aggregated and have a shape longer in diameter and length than a single SWCNT, so that the conductive network in the negative electrode does not break when the negative electrode active material layer expands or contracts. The SWCNTs are dispersed in a solvent and mixed with at least one of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C), and the SWCNTs are attached to the surface of the at least one active material, thereby allowing the SWCNTs to be arranged between at least two of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C). Furthermore, carbon black may be used in combination with the SWCNTs to enhance the conductivity of the negative electrode active material layer.

[0020] When CNTs are used as the conductive additive, the content of CNTs is preferably 0.01 mass % or more and 1 mass % or less, particularly preferably 0.03 mass % or more and 0.8 mass % or less, and even more preferably 0.1 mass % or more and 0.5 mass % or less, relative to the total solid content of the negative electrode active material layer.

[0021] In addition, the negative electrode active material layer may contain appropriate electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.

[0022] Another embodiment of the present invention is a nonaqueous electrolyte secondary battery including at least the negative electrode for a nonaqueous electrolyte secondary battery of one embodiment, a positive electrode for a nonaqueous electrolyte secondary battery, a separator, and a nonaqueous electrolyte. The nonaqueous electrolyte secondary battery of the embodiment includes, as its constituent components, at least the negative electrode for a nonaqueous electrolyte secondary battery, the positive electrode for a nonaqueous electrolyte secondary battery, a separator, and a nonaqueous electrolyte. In the embodiment, the positive electrode is a thin plate-like or sheet-like battery component formed by applying or rolling and drying a mixture containing a positive electrode active material to a positive electrode current collector, which is a metal foil such as aluminum foil, to form a positive electrode active material layer. That is, the positive electrode is composed of a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material applied to one or both sides of the positive electrode current collector. In the embodiment, the positive electrode active material layer preferably includes a positive electrode active material and a binder. The positive electrode active material is a substance used in a positive electrode that is involved in a reaction that generates electrical energy. The binder is generally a substance that binds particles of the positive electrode active material together so that the particles of the positive electrode active material are in electrical contact with each other.

[0023] The positive electrode active material used in the embodiment preferably contains a lithium-nickel based composite oxide as the positive electrode active material. The lithium-nickel based composite oxide is represented by the general formula Li x Ni y Me (1-y) O 2 (wherein Me is at least one metal selected from the group consisting of Al, Mn, Na, Fe, Co, Cr, Cu, Zn, Ca, K, Mg, and Pb).) It is particularly preferable to include a lithium-manganese composite oxide. The lithium-manganese composite oxide is, for example, lithium manganese oxide (LiMnO 2 ), spinel-type lithium manganese oxide (LiMn 2 O 4 The positive electrode active material is particularly a material represented by the general formula Li x Ni y Co z Mn (1-y-z) O 2The lithium-nickel-manganese-cobalt composite oxide has a layered crystal structure represented by the formula: where x in the general formula is 1≦x≦1.2, y and z are positive numbers satisfying y+z<1, and the value of y is 0.5 or greater. Since a high manganese content makes it difficult to synthesize a single-phase composite oxide, it is desirable to satisfy 1-y-z≦0.4. To obtain a high-capacity battery, it is particularly preferable to satisfy y>1-y-z and y>z. The lithium-nickel-based composite oxide having this general formula is a lithium-nickel-cobalt-manganese composite oxide (hereinafter, sometimes referred to as "NCM"). NCM is a lithium-nickel-based composite oxide that is suitable for use in increasing the capacity of batteries.

[0024] Examples of binders that form a positive electrode active material layer together with the positive electrode active material include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF); conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles; synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR); and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin.

[0025] The positive electrode active material layer may optionally contain a conductive additive. Examples of the conductive additive that may be used include carbon fibers such as carbon nanofibers, carbon blacks such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, and carbon nanotubes. In an embodiment, it is particularly preferable to use carbon nanotubes (CNTs) as the conductive additive. CNTs are substances in which a six-membered ring network of carbon atoms (graphene) has a single- or multi-layered coaxial tubular structure, and include single-walled carbon nanotubes (single-walled, SWCNTs) and multi-walled carbon nanotubes (multi-layered, MWCNTs). While any CNT may be used, it is preferable to use a collective SWCNT in which SWCNTs are aggregated and have a longer diameter and longer length than a single SWCNT, so that the conductive network in the positive electrode does not break when the positive electrode active material layer expands or contracts. Furthermore, carbon black may be used in addition to the SWCNTs to support the conductivity of the positive electrode active material layer. In addition, the positive electrode active material layer may contain appropriate electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.

[0026] The nonaqueous electrolyte secondary battery of the embodiment includes a separator as a constituent member. The separator can be, for example, a polyolefin film. Polyolefins are compounds obtained by polymerizing or copolymerizing α-olefins such as ethylene, propylene, butene, pentene, and hexene. Examples include polyethylene, polypropylene, polybutene, polypentene, and polyhexene, as well as copolymers thereof. When using a polyolefin film as the separator, it is advantageous to use a polyolefin film with a structure having pores that are blocked when the battery temperature rises, i.e., a porous or microporous polyolefin film. This structure of the polyolefin film allows the separator to block (shutdown) and disrupt ion flow even if the battery temperature rises. In other words, uniaxially oriented polyolefin films shrink and block the pores when the battery is heated, preventing short circuits between the positive and negative electrodes. To achieve the shutdown effect, a porous polyethylene film is highly preferable.

[0027] Crosslinked films can also be used as separators. Porous or microporous polyolefin films have the property of shrinking when heated, causing the film to shrink and shut down when the battery overheats. However, if the film's thermal shrinkage rate is too high, the film's area will change significantly, which could result in a large current flow. Crosslinked polyolefin films have an appropriate thermal shrinkage rate, allowing them to shrink enough to close the pores without significantly changing their area when overheated.

[0028] The separator used in the embodiment may have a heat-resistant fine particle layer on one or both sides of the separator. In this case, the heat-resistant fine particle layer provided to prevent overheating of the battery is composed of inorganic fine particles that have a heat resistance temperature of 150°C or higher and are stable in electrochemical reactions. Examples of such inorganic fine particles include inorganic oxides such as silica, alumina (α-alumina, β-alumina, θ-alumina), iron oxide, titanium oxide, barium titanate, and zirconium oxide; and minerals such as boehmite, zeolite, apatite, kaolin, spinel, mica, and mullite.

[0029] The nonaqueous electrolyte secondary battery of the embodiment includes a nonaqueous electrolyte. The nonaqueous electrolyte is an electrically conductive material obtained by dissolving an ionic substance in an organic solvent. The above-mentioned negative electrode for a nonaqueous electrolyte secondary battery and positive electrode for a nonaqueous electrolyte secondary battery are stacked together, with a separator disposed therebetween. This nonaqueous electrolyte secondary battery element, including this and the nonaqueous electrolyte, is one unit of the main components of the nonaqueous electrolyte secondary battery. Typically, a stack formed by stacking multiple negative electrodes for a nonaqueous electrolyte secondary battery and multiple positive electrodes for a nonaqueous electrolyte secondary battery with multiple separators interposed therebetween, is immersed in the nonaqueous electrolyte. The non-aqueous electrolyte that can be used in the embodiment is mainly a non-aqueous electrolytic solution, and is preferably a mixture containing a chain carbonate such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), di-n-propyl carbonate, di-t-propyl carbonate, di-n-butyl carbonate, di-isobutyl carbonate, or di-t-butyl carbonate, and a cyclic carbonate such as propylene carbonate (PC) or ethylene carbonate (EC). The non-aqueous electrolytic solution is preferably a mixture of such a carbonate mixture and lithium hexafluorophosphate (LiPF 6 ), lithium fluoroborate (LiBF 4 ), LiFSI, lithium perchlorate (LiClO 4 ) or other lithium salts dissolved therein.

[0030] The non-aqueous electrolyte may also contain a cyclic carbonate compound other than the above-mentioned cyclic carbonate as an additive. Examples of cyclic carbonates used as additives include vinylene carbonate (VC). Furthermore, a cyclic carbonate compound containing a halogen may also be used as an additive. These cyclic carbonates also form protective coatings on the negative electrode of a non-aqueous electrolyte secondary battery and the positive electrode of a non-aqueous electrolyte secondary battery during the charge / discharge process of the non-aqueous electrolyte secondary battery. In particular, they are compounds that can prevent attack of a positive electrode active material containing a lithium-nickel composite oxide by sulfur-containing compounds such as the above-mentioned disulfonic acid compounds or disulfonic acid ester compounds. Examples of cyclic carbonate compounds containing a halogen include fluoroethylene carbonate (FEC), difluoroethylene carbonate, trifluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, and trichloroethylene carbonate. Fluoroethylene carbonate, a cyclic carbonate compound containing a halogen and an unsaturated bond, is particularly preferred.

[0031] The non-aqueous electrolyte may further contain a disulfonic acid compound as an additive. A disulfonic acid compound is a compound having two sulfo groups in one molecule, and includes disulfonate compounds in which the sulfo groups form a salt with a metal ion, and disulfonate ester compounds in which the sulfo groups form an ester. One or two of the sulfo groups in the disulfonic acid compound may form a salt with a metal ion, or may be in an anionic state. Examples of disulfonic acid compounds include methane disulfonic acid, 1,2-ethane disulfonic acid, 1,3-propane disulfonic acid, 1,4-butane disulfonic acid, benzene disulfonic acid, naphthalenedisulfonic acid, biphenyl disulfonic acid, and salts thereof (e.g., lithium methane disulfonate, lithium 1,2-ethane disulfonate, etc.), and anions thereof (e.g., methane disulfonate anion, 1,2-ethane disulfonate anion, etc.). Examples of the disulfonic acid compound include disulfonic acid ester compounds, and include linear disulfonic acid esters such as alkyl diesters or aryl diesters of methane disulfonic acid, 1,2-ethane disulfonic acid, 1,3-propane disulfonic acid, 1,4-butane disulfonic acid, benzene disulfonic acid, naphthalenedisulfonic acid, and biphenyl disulfonic acid; and cyclic disulfonic acid esters such as methylene methane disulfonic acid ester, ethylene methane disulfonic acid ester, and propylene methane disulfonic acid ester.

[0032] The nonaqueous electrolyte secondary battery of the embodiment is usually sealed with an exterior body. Sealed means that at least a portion of the nonaqueous electrolyte secondary battery element is wrapped in an exterior body material so as not to be exposed to the outside air. The exterior body of the nonaqueous electrolyte secondary battery is a housing having gas barrier properties and capable of sealing the nonaqueous electrolyte secondary battery element, or a bag-shaped body made of a flexible material. The exterior body can suitably be an aluminum can or an aluminum laminate sheet formed by laminating aluminum foil and polypropylene or the like. In other words, any material that does not allow the nonaqueous electrolyte to leach out to the outside may be used for the exterior body. The outermost layer of the exterior package can be a heat-resistant protective layer made of polyester, polyamide, liquid crystal polymer, or the like, and the innermost layer can be a laminate film having a sealant layer made of a thermoplastic resin such as polyethylene, polypropylene, ionomer, acid-modified polyethylene such as maleic acid-modified polyethylene, acid-modified polypropylene such as maleic acid-modified polypropylene, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethylene isophthalate (PEI), a blend of PET and PEN, a blend of PET and PEI, a polyamide resin, a blend of polyamide resin and PET, or a blend of xylylene group-containing polyamide and PET. The exterior package can also be formed by bonding or welding one or more of these laminate films together to form a multilayer structure. Aluminum, tin, copper, nickel, or stainless steel can be used as the gas barrier metal layer. The thickness of the metal layer is preferably 30 to 50 μm. An aluminum laminate, which is a laminate of aluminum foil and a polymer such as polyethylene or polypropylene, is particularly preferred. The nonaqueous electrolyte secondary battery of the embodiment may be in various forms such as a coin-type battery, a laminate-type battery, or a wound-type battery.

[0033] The embodiments of the present invention have been described above. Examples of the present invention will be described below. The above embodiments and the examples described below are merely illustrative of the present invention, and are not intended to limit the technical scope of the present invention to any particular embodiment or specific example configuration.

[0034] (Preparation of Positive Electrode, All Examples and Comparative Examples) Li(Ni) as Positive Electrode Active Material 0.9 Co 0.05 Mn 0.05 ) O 2 (97.5% by mass), polyvinylidene fluoride (PVDF, 1.5% by mass) as a positive electrode binder, and carbon nanotubes (multi-walled carbon nanotubes (MWCNT, 1% by mass) as a conductive additive were mixed to prepare a positive electrode active material mixture. The positive electrode active material mixture was dispersed in N-methyl-2-pyrrolidone to prepare a positive electrode slurry. This positive electrode slurry was uniformly applied to one side of an aluminum current collector having a thickness of 12 μm. The initial charge capacity per unit area was 4.0 mAh / cm. 2 After drying, the coating film was compression molded using a roll press to adjust the density of the positive electrode active material layer to 3.5 g / cm. 3 The positive electrode was prepared by adjusting the temperature so that the following condition was satisfied:

[0035] (Fabrication of Negative Electrode, Example 1) A silicon-based active material (A), SiO x (x=1, D 50 = 11.0 μm) and artificial graphite (D) which is a carbon-based active material (B) consisting of secondary particles formed by aggregation of primary particles. 50 13.9 μm) and artificial graphite (D) which is a carbon-based active material (C) consisting of primary particles that do not aggregate to form secondary particles. 50 The negative electrode active material mass ratio (SiO of silicon-based active material (A)) was xThe mass ratio of the carbon-based active material (B) and the artificial graphite (C) of the negative electrode, (denoted as (A) / [(B) + (C)]) was 15 / 85, and the mass ratio of the carbon-based active material (B) to the carbon-based active material (C) was 1 / 1 to obtain a negative electrode active material mixture. This active material mixture (96.6% by mass), a polyacrylic acid binder (trade name: 10CLPAH, Fujifilm Wako Pure Chemical Industries, Ltd., 3.0% by mass) as a negative electrode binder, single-walled carbon nanotubes (SWCNT, 0.3% by mass) as a conductive additive, and carboxymethyl cellulose (CMC, 0.1% by mass) were dissolved and dispersed in an aqueous solvent to prepare a negative electrode slurry. This negative electrode slurry was uniformly applied to a Cu current collector with a thickness of 8 μm. The initial charge capacity per unit area was 4.3 mAh / cm 2 The thickness of the coating film was then adjusted by a roll press to obtain a negative electrode active material layer having a density of 1.65 g / cm. 3 The negative electrode was fabricated by adjusting the SiO x Suitable graphite can be obtained from, for example, Sigma-Aldrich Corporation, High Purity Chemical Laboratory Co., Ltd., Kanto Chemical Co., Ltd., Fujifilm Wako Pure Chemical Industries, Ltd., etc., and the surface coating components, surface conditions such as roughness, particle size, etc. can be adjusted by using these alone or in combination and known methods such as heat treatment such as calcination, chemical treatment such as CVD, mechanical treatment such as crushing and classification, and sputtering. Suitable graphite can be obtained from Nippon Graphite Industries Co., Ltd., Resonac Inc., etc., and the surface coating components, surface conditions such as roughness, particle size, etc. can be adjusted by using these alone or in combination and known methods such as heat treatment such as calcination, chemical treatment such as CVD, mechanical treatment such as crushing and classification, and sputtering.

[0036] The conductive additive used here is a collection of SWCNTs with a length of about 1 μm and a diameter of about 10 nm, which are longer and longer than a single SWCNT. A plurality of SWCNTs are arranged on the surface of the negative electrode active material so as to contact two or more of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C). Such SWCNTs can be obtained, for example, from Meijo Nanocarbon Co., Ltd., Honjo Chemical Co., Ltd., and Kusumoto Chemical Co., Ltd.

[0037] In other examples and comparative examples, the type of negative electrode active material used and the amount of the negative electrode active material mixed were changed as shown in Table 1. Silicon-based active material (A) SiO x The carbon-based active materials (B) and (C) were obtained from the same sources as in Example 1. The mass ratio of the carbon-based active material (B) to the carbon-based active material (C) was 7:3 in Examples 5 and 6, and 1:1 in the other Examples and Comparative Examples, as in Example 1. The types and amounts of the binder and conductive additive, and the method for producing the negative electrode active material layer were also the same as in Example 1 in all Examples and Comparative Examples.

[0038] (Fabrication of Lithium-Ion Secondary Batteries, All Examples and Comparative Examples) A ​​positive electrode and a negative electrode cut into 3 cm x 3 cm pieces were arranged facing each other with a separator interposed therebetween. The separator was a 10 μm-thick microporous polyethylene film with ceramic coating on both sides.

[0039] The non-aqueous electrolyte was prepared by mixing an organic solvent and a supporting salt. The volume ratio of cyclic carbonate (EC) to chain carbonate (DEC, EMC) was adjusted to 1 / 6, and lithium hexafluorophosphate (LiPF ) was used as a supporting salt. 6 ) and fluoroethylene carbonate (FEC) were added.

[0040] The positive electrode, negative electrode, separator, and non-aqueous electrolyte solution were placed in a laminate outer casing, and the laminate was sealed to produce a lithium ion secondary battery, which is a non-aqueous electrolyte secondary battery. The positive electrode and negative electrode were electrically connected from the outside of the laminate by connecting tabs.

[0041] (Evaluation of Lithium Ion Secondary Battery) The lithium ion secondary batteries fabricated in each of the Examples and Comparative Examples were evaluated by measuring the capacity retention rate and the decrease in average voltage during 1 C discharge using the following method.

[0042] (Energy Density) The fabricated battery was charged at 7.2 mA, and after the upper voltage reached 4.2 V, it was charged at a constant voltage until the total charge time reached 12 hours. It was then discharged at a constant current of 7.2 mA until the lower voltage reached 2.5 V. After charging under the same conditions again, it was left in a thermostatic chamber at 45°C for 3 days, discharged under the same conditions again, and then charged and discharged once more. The capacity and average voltage at the final discharge were evaluated. After this evaluation, the thickness of the laminated battery (hereinafter sometimes simply referred to as "cell") was evaluated.

[0043] The sum of the thickness of the positive electrode active material layer, half the thickness of the positive electrode current collector, the thickness of the separator, the thickness of the negative electrode active material layer, and half the thickness of the negative electrode current collector, which are the unit components of the laminate-type battery, was calculated from the thickness of the cell. Specifically, the thickness of the laminate, half the thickness of the positive electrode current collector, and half the thickness of the negative electrode current collector were subtracted from the thickness of the cell.

[0044] The energy density of each unit component of the laminated battery was calculated using the following formula: [Mathematical Formula 1] (Capacity during cell discharge) × (Average voltage during cell discharge) / (Area of ​​electrode) / (Thickness of positive electrode active material layer + Half the thickness of positive electrode current collector + Thickness of separator + Thickness of negative electrode active material layer + Half the thickness of negative electrode current collector).

[0045] (Capacity Retention Rate) The fabricated battery was placed in a thermostatic chamber at 45°C and charged at 30 mA. After the upper limit voltage reached 4.2 V, the battery was charged at a constant voltage until the total charging time reached 2.5 hours. The battery was then discharged at a constant current of 30 mA until the lower limit voltage reached 2.5 V. This charge / discharge cycle was repeated 100 times, and the ratio of the 100th discharge capacity to the first discharge capacity was defined as the capacity retention rate after 300 cycles.

[0046] The non-aqueous electrolyte secondary battery using the negative electrode for non-aqueous electrolyte secondary battery of the Example of the present invention has a high energy density and a high capacity retention rate after charge and discharge. On the other hand, the non-aqueous electrolyte secondary battery using the negative electrode for non-aqueous electrolyte secondary battery of the Comparative Example showed a decrease in either the energy density or the capacity retention rate, and it was not possible to improve both the energy density and the lifespan. In the Example, the silicon-based active material SiO x The experiment was conducted using SiO with x = 1, but the SiO with x in the range of 0.5 to 1.6 x By optimizing the compounding ratio of the silicon-based active material to the carbon-based active material and the particle sizes of the silicon-based active material and the two types of carbon-based active materials, an appropriate particle packing density can be obtained in the negative electrode active material layer, and by suppressing electrode expansion, the energy density and cycle capacity retention rate of the non-aqueous electrolyte secondary battery can be improved.

[0047] These are the maximum average particle diameter D50 of the average particle diameters of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C) in a composite negative electrode. max and the minimum average particle size D50 min D50 is the ratio of max / D50 min It is believed that by adjusting D50 within a predetermined range, the packing density of the negative electrode active material particles is optimized and expansion and contraction during charge and discharge are suppressed. In addition, when the average particle diameter of the silicon-based active material (A) and the carbon-based active materials (B) and (C) is large, the capacity retention rate of the battery tends to increase. max / D50 min If the ratio exceeds 2, it is considered that the packing density of the negative electrode active material does not increase, and the expansion and contraction of the negative electrode active material layer cannot be suppressed.

[0048] The negative electrode for a nonaqueous electrolyte secondary battery of the present invention has been described in detail above. However, the present invention is not limited to the above-described embodiments and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.

Claims

1. A negative electrode for a non-aqueous electrolyte secondary battery, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material, a binder, and a conductive assistant, the negative electrode active material being SiO x (wherein x is a number satisfying 0.5≦x≦1.6), a carbon-based active material (B) composed of secondary particles formed by aggregation of primary particles, and a carbon-based active material (C) composed of primary particles different from the primary particles of the carbon-based active material (B), wherein the average particle diameters of each of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) are D50 A [μm], D50 B [μm], and D50 C [μm], and the maximum average particle size among these average particle sizes is D50 max The smallest average particle diameter among these average particle diameters is defined as D50 min When this is done, D50 max / D50 min a value of less than 2.

2. Average particle diameter D50 of the silicon-based active material (A) A The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 , wherein the thickness of the negative electrode is 7 μm or more and 13 μm or less.

3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein the carbon-based active material (B) and the carbon-based active material (C) include artificial graphite, hard carbon, soft carbon, or any mixture thereof.

4. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein the carbon-based active material (B) is artificial graphite the surface of which is coated with amorphous carbon, and the carbon-based active material (C) is artificial graphite the surface of which is not coated.

5. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein the content of the silicon-based active material (A) is 10 mass % or more and 20 mass % or less relative to the total amount of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C) in the negative electrode.

6. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein the conductive assistant contains carbon nanotubes.

7. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 6, wherein the conductive assistant is an aggregate of single-walled carbon nanotubes.

8. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7, wherein a portion of the conductive additive is present in a state of being adhered in advance to a surface of at least one of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C).

9. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 8, wherein the binder contains polyacrylic acid.

10. A non-aqueous electrolyte secondary battery comprising at least the negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 9, a positive electrode for a non-aqueous electrolyte secondary battery, a separator, and an electrolyte.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    JP2016219275A

  • Negative electrode and nonaqueous electrolyte power storage device

    JP2019029311A

  • Electrode and secondary battery including same

    JP2022529987A

  • Negative electrode sheet and method for producing the same, secondary battery, battery module, battery pack and device

    JP2023503706A

  • Non-aqueous electrolyte secondary battery

    WO2015045314A1