Urethane foam molded body

The urethane foam molded article with oriented composite particles of expanded graphite and magnetic particles addresses the limitations of thermal conductivity and flame retardancy in soundproofing materials, achieving enhanced heat dissipation and electrical insulation.

WO2024202354A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO RIKO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/046983
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-12-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Urethane foam soundproofing materials face limitations in thermal conductivity and flame retardancy, with existing thermally conductive fillers like expanded graphite not sufficiently enhancing heat dissipation and potentially compromising flame retardancy when magnetic particles are blended.

Method used

A urethane foam molded article with composite particles, where expanded graphite particles and magnetic particles are adhered with a binder, forming separate composite particles that are oriented to create a heat transfer path, enhancing thermal conductivity and flame retardancy without inhibiting each other's effects.

Benefits of technology

The solution achieves improved thermal conductivity and flame retardancy, suitable for applications requiring both heat dissipation and electrical insulation, such as in electronic devices and vehicle components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The urethane foam molded body comprises a base material made of polyurethane foam and composite particles oriented and contained in the base material. The composite particles comprise: first composite particles having expandable graphite particles and magnetic particles bonded to the surface of the expandable graphite particles with a binder; and second composite particles having expanded graphite particles and magnetic particles bonded to the surface of the expanded graphite particles with a binder. When the total mass of the expandable graphite particles and the expanded graphite particles in the base material in the urethane foam molded body is taken to be 100 mass%, the content of the expandable graphite particles is 20-80 mass% inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Urethane foam molding

[0001] The present disclosure relates to a urethane foam molded article having high thermal conductivity.

[0002] In automobiles and other vehicles, measures are taken to reduce noise generated by engines, transmissions, and other components in order to reduce noise leaking outside the vehicle or into the passenger compartment. In electric vehicles (EVs) and hybrid electric vehicles (HEVs), the driving noise of the electric powertrain, which consists of an inverter, motor, gearbox, and other components, is also a target for reduction. Soundproofing materials made of foams such as polyurethane foam are used as noise countermeasures. Foams have a large number of internal cells (air bubbles) and therefore have low thermal conductivity. Therefore, if they are placed around a heat-generating noise source, heat may accumulate, causing problems.

[0003] From the viewpoint of improving the heat dissipation properties of soundproofing materials using foams, for example, Patent Document 1 describes a urethane foam molded body in which composite particles, which are a composite of thermally conductive particles, magnetic particles, and insulating inorganic particles, are oriented and arranged in polyurethane foam, thereby forming a heat transfer path in the direction of the orientation, thereby improving the heat dissipation properties. Examples of the thermally conductive particles described include expanded graphite. Patent Document 2 describes a polyurethane foam containing a thermally conductive filler. Examples of the thermally conductive filler described include expanded graphite and expanded graphite.

[0004] International Publication No. 2013 / 042611 Japanese Patent Application Laid-Open No. 2022-72896

[0005] Depending on the application, soundproofing materials may require flame retardancy in addition to thermal conductivity. For example, flame-retardant polyurethane foams have a dropping effect, which drops embers and prevents the spread of fire when exposed to flames. In the urethane foam molded product described in Patent Document 1, composite particles are used in which magnetic particles are adhered to the surface of thermally conductive particles to orient the particles with relatively high thermal conductivity. Adding magnetic particles to polyurethane foam may impair the dropping effect and reduce self-extinguishing properties. Therefore, considering flame retardancy, expanded graphite, which has flame retardant properties due to the insertion of a substance that generates gas upon heating between the layers of flake graphite, is suitable as the thermally conductive particles. Thus, using expanded graphite as the thermally conductive particles in the composite particles improves the flame retardancy of urethane foam molded products. However, in recent years, higher thermal conductivity has been required for soundproofing materials. In this case, the thermal conductivity of expanded graphite is not sufficiently high, and there is a limit to the improvement in thermal conductivity that can be achieved by using expanded graphite alone.

[0006] In this regard, Patent Document 2 lists expanded graphite and expanded graphite as thermally conductive fillers. Expanded graphite is produced by heating and expanding expanded graphite, followed by pulverization, and has high purity due to the disappearance of intercalation materials. Therefore, the thermal conductivity of expanded graphite is higher than that of expanded graphite. However, as described in paragraph

[0006] , Patent Document 2 aims to perform foam molding without applying a magnetic field. Therefore, the thermally conductive filler in the polyurethane foam is not oriented, and even if expanded graphite or expanded graphite is used as the thermally conductive filler, it is merely dispersed as a single substance. According to the inventor's research, it has been found that simply dispersing expanded graphite in polyurethane foam only slightly improves thermal conductivity.

[0007] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a urethane foam molded article having excellent thermal conductivity and flame retardancy.

[0008] (1) In order to solve the above-mentioned problems, the urethane foam molded product of the present disclosure has a substrate made of polyurethane foam and composite particles contained and oriented in the substrate, the composite particles including first composite particles having expanded graphite particles and magnetic particles bonded to the surfaces of the expanded graphite particles with a binder, and second composite particles having expanded graphite particles and magnetic particles bonded to the surfaces of the expanded graphite particles with a binder, and is characterized in that, when the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is taken as 100 mass%, the content of the expanded graphite particles is 20 mass% or more and 80 mass% or less.

[0009] The urethane foam molded article of the present disclosure contains at least two types of composite particles, first and second. Both composite particles have magnetic particles bonded to the surface of a core particle with a binder. The core particles of the first composite particles are expanded graphite particles with a higher thermal conductivity than expanded graphite particles, primarily contributing to improving the thermal conductivity of the urethane foam molded article. The core particles of the second composite particles are expanded graphite particles that exhibit flame retardancy, primarily contributing to improving the flame retardancy of the urethane foam molded article. These composite particles are oriented in a substrate made of polyurethane foam. The composite particles are aligned in a series, forming a heat transfer path in the substrate. This facilitates heat transfer to the composite particles, making it easier for the expanded graphite particles and expanded graphite particles to exert their respective effects compared to when each particle is contained alone. Furthermore, both the expanded graphite particles and expanded graphite particles are graphite-based materials, have thermal conductivity anisotropy, and are highly compatible with polyurethane.

[0010] The urethane foam molded article of the present disclosure contains expanded graphite particles and expanded graphite particles, which have different functions, as separate, independent composite particles. This allows each particle to fully exert its respective effects without interfering with the other's function. As a result, desired thermal conductivity and flame retardancy can be achieved. However, the urethane foam molded article of the present disclosure does not exclude a form that includes composite particles in which magnetic particles are adhered to the surface of particles formed by integrating expanded graphite particles and expanded graphite particles.

[0011] (2) In the above configuration, the average particle size of the expanded graphite particles may be 100 μm or more and 3000 μm or less. This configuration reduces the effect on the moldability and brittleness of the urethane foam molded body, and allows the expanded graphite particles to exhibit the effect of improving thermal conductivity.

[0012] (3) In any of the above configurations, the purity of the expanded graphite particles may be 99% or more. With this configuration, the effect of improving thermal conductivity can be enhanced.

[0013] (4) In any of the above configurations, the average particle size of the expanded graphite particles may be 100 μm or more and 3000 μm or less. This configuration reduces the effect on the moldability and brittleness of the urethane foam molded body, and allows the expanded graphite particles to exert their flame retardant effect.

[0014] (5) In any of the above configurations, the content of the composite particles may be 5% by volume or more and 50% by volume or less, based on the volume of the urethane foam molded body taken as 100% by volume. This configuration is suitable for achieving both improved moldability of the urethane foam molded body and improved thermal conductivity and flame retardancy.

[0015] (6) In any of the above configurations, the binder constituting the first composite particles and the second composite particles may be a water-soluble polymer. This configuration has little effect on foam molding and is environmentally friendly when producing a urethane foam molded article.

[0016] (7) In the above (6), the water-soluble polymer may be one or more selected from the group consisting of methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and starch. The water-soluble polymer of this configuration has good adhesive properties, is relatively inexpensive, and is easily available.

[0017] (8) In any of the above configurations, the content of the magnetic particles constituting the first composite particles and the second composite particles may be 20% by mass or more and 80% by mass or less, when the total mass of the expanded graphite particles and the expanded graphite particles in the base material is 100% by mass. With this configuration, the amount of magnetic particles is relatively small, which allows for cost reduction and weight reduction.

[0018] (9) In any of the above configurations, the magnetic particles constituting the first composite particles and the second composite particles may be one or more selected from iron particles and iron-based alloy particles, which have high saturation magnetization and are readily available as fine particles.

[0019] (10) In any of the above configurations, at least one of the first composite particles and the second composite particles may have insulating inorganic particles bonded to the surfaces of the expanded graphite particles or the expanded graphite particles with a binder.

[0020] In this configuration, the insulating inorganic particles may be directly bonded to the surface of the core expanded graphite particles or expanded graphite particles, or indirectly bonded via magnetic particles, i.e., to the surface of magnetic particles bonded to each particle. Ferromagnetic materials such as stainless steel and iron are used as magnetic particles. Therefore, composite particles formed by combining expanded graphite particles or expanded graphite particles with magnetic particles have high electrical conductivity. When insulating inorganic particles are bonded to such composite particles, even if the composite particles are oriented in contact with each other, the core particles and magnetic particles (conductive particles) between adjacent composite particles are less likely to come into contact with each other. This increases the electrical resistance between the composite particles. Furthermore, contact between the composite particles via the insulating inorganic particles can interrupt electrical continuity between the composite particles. As a result, the urethane foam molded product of the present disclosure can achieve electrical insulation. Thus, this configuration can impart electrical insulation in addition to high thermal conductivity and flame retardancy. Therefore, the urethane foam molded product of this configuration is suitable for applications requiring both heat dissipation and electrical insulation, such as heat dissipation components in electronic devices.

[0021] (11) In the configuration of (10) above, the insulating inorganic particles may be one or more selected from aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, and silica. The insulating inorganic particles of this configuration have a relatively high thermal conductivity and therefore are unlikely to impair thermal conductivity between composite particles. In addition, they are relatively inexpensive and easily available.

[0022] In the urethane foam molded article of the present disclosure, the expanded graphite particles and the expanded graphite particles are arranged as separate composite particles oriented in the substrate, which results in the urethane foam molded article of the present disclosure having excellent thermal conductivity and flame retardancy.

[0023] The following describes embodiments of the urethane foam molded article of the present disclosure. Note that the embodiments are not limited to the following embodiments, and various modifications and improvements that can be made by those skilled in the art are possible.

[0024] <Urethane Foam Molded Article> The urethane foam molded article of the present disclosure has a substrate made of polyurethane foam and composite particles contained and oriented in the substrate.

[0025] [Substrate] The polyurethane foam substrate is produced from urethane foam resin raw materials such as a polyisocyanate component and a polyol component. The urethane foam resin raw materials may be prepared from known raw materials such as polyol and polyisocyanate. The polyol may be appropriately selected from polyhydric hydroxy compounds, polyether polyols, polyester polyols, polymer polyols, polyether polyamines, polyester polyamines, alkylene polyols, urea-dispersed polyols, melamine-modified polyols, polycarbonate polyols, acrylic polyols, polybutadiene polyols, phenol-modified polyols, etc. The polyisocyanate may be appropriately selected from, for example, tolylene diisocyanate, phenylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, triphenylmethane triisocyanate, polymethylene polyphenyl isocyanate, naphthalene diisocyanate, and derivatives thereof (for example, prepolymers obtained by reaction with polyols, modified polyisocyanates), and the like.

[0026] The urethane foam resin raw material may further contain catalysts, blowing agents, foam stabilizers, plasticizers, crosslinking agents, chain extenders, flame retardants, antistatic agents, viscosity reducers, stabilizers, fillers, colorants, etc. Examples of catalysts include amine catalysts such as tetraethylenediamine, triethylenediamine, and dimethylethanolamine, and organometallic catalysts such as tin laurate and tin octoate. Water is also suitable as a blowing agent. Other than water, other suitable blowing agents include methylene chloride, chlorofluorocarbons, CO 2 As the foam stabilizer, a silicone-based foam stabilizer is suitable, and as the crosslinking agent, triethanolamine, diethanolamine, etc. are suitable.

[0027] The shape, size, etc. of the substrate are not particularly limited and may be determined appropriately depending on the application. The composite particles contained in the substrate may be arranged with a certain regularity. For example, they may be arranged in a straight line or a curved line between one end and the other end of the urethane foam molded body (the ends do not have to be 180° opposite to the one end). Alternatively, they may be arranged radially from the center toward the periphery.

[0028] [Composite Particles] The composite particles contained in an oriented state in the substrate are particles in which magnetic particles or the like are bonded to the surface of a non-magnetic particle serving as a core with a binder, and include first composite particles and second composite particles. The first composite particles include expanded graphite particles and magnetic particles bonded to the surface of the expanded graphite particles with a binder. The second composite particles include expanded graphite particles and magnetic particles bonded to the surface of the expanded graphite particles with a binder. The non-magnetic particle serving as a core may be a single particle or multiple particles. For example, the expanded graphite particle constituting the first composite particle may be a single expanded graphite particle or an aggregate particle in which multiple expanded graphite particles are integrated. The expanded graphite particle constituting the second composite particle may be a single expanded graphite particle or an aggregate particle in which multiple expanded graphite particles are integrated. Furthermore, the composite particles may include particles of a form other than the first composite particles and the second composite particles, such as a form in which magnetic particles are adhered to the surface of a particle in which expanded graphite particles and expanded graphite particles are integrated together, or a form in which magnetic particles are adhered to the surface of other graphite particles or metal particles.

[0029] The content of the composite particles may be determined taking into consideration thermal conductivity, flame retardancy, the effect on the foaming reaction of the polyurethane foam, moldability, etc. In order to achieve the desired thermal conductivity and flame retardancy, the content of the composite particles is preferably 5% by volume or more, based on the volume of the urethane foam molded product being 100% by volume. 10% by volume or more is more preferable. On the other hand, from the viewpoint of not inhibiting the foaming reaction, the content of the composite particles is preferably 50% by volume or less, and more preferably 20% by volume or less.

[0030] Furthermore, when the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is taken as 100% by mass, the content of the expanded graphite particles is set to 20% by mass or more and 80% by mass or less. If the content of the expanded graphite particles is less than 20% by mass, the effect of improving thermal conductivity is small. 30% by mass or more is more preferable. Conversely, if the content of the expanded graphite particles is more than 80% by mass, flame retardancy decreases. 60% by mass or less is more preferable.

[0031] The expanded graphite particles constituting the first composite particles may be produced by heating and expanding expanded graphite, forming it into a sheet, and then pulverizing the sheet. The expanded graphite particles have a multilayer structure in which multiple graphenes are stacked. From the viewpoint of enhancing the effect of improving thermal conductivity, the purity of the expanded graphite particles (the carbon component content) is desirably 99% or more. The thermal conductivity of the expanded graphite particles is desirably 200 W / m·K or more.

[0032] The shape of the expanded graphite particles is not particularly limited, and may be flaky, fibrous, spherical, or the like. The average particle size of the expanded graphite particles is desirably 100 μm or more, from the viewpoint of increasing thermal conductivity. 700 μm or more is more preferable. On the other hand, if the expanded graphite particles are too large, cracks may occur from the expanded graphite particles, making the molded body brittle. Therefore, the average particle size of the expanded graphite particles is desirably 3000 μm or less, and more preferably 2000 μm or less. Unless otherwise specified, the average particle size in this specification refers to the median diameter (D ) calculated from the volume-based particle size distribution measured by laser diffraction / scattering method. 50 For commercially available products, the catalogue value may be used.

[0033] The expanded graphite particles constituting the second composite particles are obtained by inserting a substance that generates gas when heated between layers of scaly graphite, for example, by acid treatment. When heat is applied to the expanded graphite particles, the generated gas expands the spaces between the layers and forms a layer that is stable against heat and chemicals. This stable layer acts as a heat insulating layer, preventing the transfer of heat and thereby providing a flame retardant effect. The expanded graphite particles may be appropriately selected taking into consideration the expansion start temperature, expansion coefficient, etc. The expansion start temperature must be higher than the heat generation temperature during molding of the urethane foam molded body, so expanded graphite particles with an expansion start temperature of 150°C or higher are suitable, for example.

[0034] The shape of the expanded graphite particles is not particularly limited, and may be flaky, fibrous, spherical, or the like. Taking into consideration dispersibility in polyurethane foam, the average particle size of the expanded graphite particles is desirably 100 μm or more, and more desirably 700 μm or more. On the other hand, as with the expanded graphite particles, if the expanded graphite particles are too large, cracks may occur from the expanded graphite particles, making the molded body brittle. Therefore, the average particle size of the expanded graphite particles is desirably 3000 μm or less, and more desirably 2000 μm or less. When the size of the expanded graphite particles and the size of the expanded graphite particles are comparable, there is an advantage in that the composite particles can be granulated together.

[0035] In the first composite particle and the second composite particle, the magnetic particles adhered to the surface of the expanded graphite particle or expanded graphite particle (either or both of these may be collectively referred to as "core particle") as the core may be the same or different. The magnetic particles may be any particles capable of orienting the composite particles, and may be, for example, ferromagnetic materials such as iron, nickel, cobalt, gadolinium, stainless steel, magnetite, maghemite, manganese zinc ferrite, barium ferrite, and strontium ferrite, MnO, Cr 2 O 3 , FeCl 2Particles of antiferromagnetic materials such as MnAs and alloys using these are preferred. Among these, iron, nickel, cobalt, and iron-based alloys thereof (including stainless steel) are preferred from the viewpoints of easy availability as fine particles and high saturation magnetization. Iron, in particular, is relatively inexpensive and easily available, allowing for reduced manufacturing costs and making it suitable for mass production.

[0036] The magnetic particles may be directly adhered to the surface of the core particle, or may be indirectly adhered via other particles such as insulating inorganic particles, as described below. The magnetic particles may be adhered to only a portion of the surface of the core particle, or may be adhered so as to cover the entire surface. The size of the magnetic particles may be determined appropriately, taking into consideration the size of the core particle, the orientation of the composite particles, and the thermal conductivity between the composite particles. For example, the particle diameter of the magnetic particles is preferably 1 / 10 or less of the particle diameter of the core particle. As the size of the magnetic particles decreases, the saturation magnetization of the magnetic particles tends to decrease. Therefore, in order to orient the composite particles with a smaller amount of magnetic particles, it is desirable that the average particle diameter of the magnetic particles be 100 nm or more. It is more preferable to set the average particle diameter of the magnetic particles to 1 μm or more, and even more preferably to set the average particle diameter to 5 μm or more.

[0037] The shape of the magnetic particles is not particularly limited. For example, when the magnetic particles are flat, the distance between adjacent core particles is shorter than when the magnetic particles are spherical. This improves the thermal conductivity between adjacent composite particles. As a result, the thermal conductivity of the urethane foam molded body is improved. Furthermore, when the magnetic particles are flat, the magnetic particles and core particles come into contact with each other through their surfaces. In other words, the contact area between the two is increased. This improves the adhesive strength between the magnetic particles and core particles. Therefore, the magnetic particles are less likely to peel off. In addition, the thermal conductivity between the magnetic particles and core particles is also improved. For these reasons, it is desirable to use flaky particles as the magnetic particles.

[0038] From the viewpoint of enabling the composite particles to be oriented even in a relatively weak magnetic field, the content of the magnetic particles is desirably 20% by mass or more, where the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is 100% by mass. Furthermore, from the viewpoint of achieving cost reduction and weight reduction, the content of the magnetic particles is desirably 130% by mass or less. 100% by mass or less, and even 80% by mass or less, is more preferable. In the urethane foam molded product of the present disclosure, expanded graphite particles with high thermal conductivity are contained as the first composite particles, so that thermal conductivity is not likely to decrease even if the content of the magnetic particles is reduced.

[0039] In the first composite particles and the second composite particles, the binder that bonds the core particles and the magnetic particles may be appropriately selected taking into consideration adhesiveness, the effect on foam molding, and the like. Water-soluble polymers are preferred because they have little effect on foam molding and are environmentally friendly. Examples include methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and starch. Among these, starch is preferred because it is relatively inexpensive, has high adhesion, and is excellent in granulation properties. The binder of the first composite particles and the binder of the second composite particles may be the same or different.

[0040] Expanded graphite particles, expanded graphite particles, and magnetic particles are electrically conductive. Therefore, the first composite particles and the second composite particles are aligned and oriented, forming a conductive path in the substrate. For example, composite particles can be formed by adhering insulating inorganic particles to the surface of a core particle in addition to magnetic particles with a binder. By doing so, even if the composite particles are oriented, the electrical resistance between adjacent composite particles can be increased or electrical conduction can be blocked. As a result, electrical insulation can be imparted to the urethane foam molded product. The urethane foam molded product of the present disclosure, in which at least one of the first composite particles and the second composite particles contains insulating inorganic particles, is suitable for applications requiring electrical insulation, such as heat dissipation components in electronic devices.

[0041] The insulating inorganic particles may be particles of an inorganic material having insulating properties. In particular, particles with a relatively high thermal conductivity are desirable from the viewpoint of not inhibiting thermal conductivity between composite particles. For example, it is preferable that the insulating inorganic particles have a thermal conductivity of 5 W / m·K or more. Examples of insulating inorganic materials with a thermal conductivity of 5 W / m·K or more include aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, and silica. One of these can be used alone, or two or more can be used in combination. Among these, talc and mica are preferred because they are flaky and have excellent coating properties.

[0042] The insulating inorganic particles may be directly adhered to the surface of the core particle, or may be indirectly adhered via magnetic particles. The insulating inorganic particles may be adhered to only a portion of the surface of the core particle, or may be adhered so as to cover the entire surface. From the viewpoint of increasing the electrical resistance between the composite particles and improving the electrical insulation of the urethane foam molded product, it is desirable that the insulating inorganic particles be disposed in the outermost layer of the composite particle. The binder that adheres the magnetic particles to the core particle and the binder that adheres the insulating inorganic particles may be the same or different.

[0043] The size of the insulating inorganic particles may be determined appropriately, taking into consideration the adhesiveness to the core particles and magnetic particles, and the electrical insulation and thermal conductivity between the composite particles. If the insulating inorganic particles are too large, the adhesiveness and thermal conductivity between the composite particles will decrease. For example, the particle diameter of the insulating inorganic particles is preferably 1 / 100 to 1 / 10 of the particle diameter of the core particles. The shape of the insulating inorganic particles is not particularly limited. For example, if the insulating inorganic particles have a flat shape, the distance between adjacent core particles can be shorter than when the insulating inorganic particles are spherical. Therefore, the thermal conductivity between adjacent composite particles is less likely to be impaired. Furthermore, the increased contact area makes the insulating inorganic particles less likely to peel off.

[0044] The insulating inorganic particles may be simply dispersed in the substrate rather than as part of the composite particle, or may constitute a composite particle and then be dispersed in the substrate. The insulating inorganic particles dispersed in the substrate may be the same as or different from the insulating inorganic particles added as constituent particles of the composite particle. The insulating inorganic particles dispersed in the substrate may be one type or two or more types. The insulating inorganic particles dispersed in the substrate preferably have a relatively high thermal conductivity, and the aforementioned aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, silica, etc. are suitable. When the insulating inorganic particles are dispersed in the substrate, they penetrate between the composite particles, reducing electrical conductivity between the composite particles. This improves the electrical insulation of the urethane foam molded product. Furthermore, when the insulating inorganic particles have a relatively high thermal conductivity, a heat transfer path is formed by the insulating inorganic particles in addition to the heat transfer path by the composite particles. This further improves the thermal conductivity of the urethane foam molded product. Furthermore, when the insulating inorganic particles have flame retardancy, the flame retardancy of the urethane foam molded article is improved.

[0045] <Method for producing urethane foam molded article> The method for producing the urethane foam molded article of the present disclosure is not particularly limited. As a preferred embodiment of the production method, the method for producing the urethane foam molded article of the present disclosure includes a composite particle production step, a raw material mixture production step, and a foam molding step. Each step will be described below.

[0046] [Composite particle manufacturing process] This process is a process for manufacturing composite particles by stirring a granulation raw material containing a powder of core particles, a powder of magnetic particles, a binder, and water. Regarding the composite particles, the first composite particles containing expanded graphite particles and the second composite particles containing expanded graphite particles may be manufactured together or separately. Since the expanded graphite powder and the expanded graphite powder have similar specific gravities and there is no significant difference in granulation properties, the first composite particles and the second composite particles can be manufactured together, which improves productivity.

[0047] When two types of composite particles are produced simultaneously, both the expanded graphite powder and the expanded graphite powder can be stirred together with other raw materials such as water. In this case, the difference between the average particle size of the expanded graphite powder and the average particle size of the expanded graphite powder can be reduced in consideration of granulation properties. Furthermore, the amount of the expanded graphite powder can be set to 20% by mass or more and 80% by mass or less, where the total mass of the expanded graphite powder and the expanded graphite powder is taken as 100% by mass. On the other hand, when two types of composite particles are produced separately, the expanded graphite powder can be stirred together with other raw materials such as water to produce first composite particles, and the expanded graphite powder can be stirred together with other raw materials such as water to produce second composite particles. The composite particles can be produced using a high-speed stirring mixer granulator or the like. The amounts of the magnetic particle powder, binder, and water relative to the core particle powder can be appropriately adjusted in consideration of granulation properties, magnetic field orientation of the composite particles, and the like.

[0048] Considering the magnetic field orientation of the composite particles, the blending amount of magnetic particle powder is preferably 20 parts by mass or more per 100 parts by mass of core particle powder. On the other hand, considering cost and weight reduction, it is preferable to set it to 130 parts by mass or less. 100 parts by mass or less, and even more preferable to set it to 80 parts by mass or less. The blending amount of binder is preferably 2% by mass or more, where the total mass of the powders to be bonded is 100% by mass, as a necessary and sufficient amount for particle adhesion. On the other hand, excessive binder may cause aggregation of the composite particles. Therefore, the blending amount of binder is preferably 10% by mass or less, and more preferably 5% by mass or less. The binder may be solid or liquid. When using a water-soluble powder as the binder, it is recommended to add water after stirring the binder and other powder raw materials in advance. This can suppress particle aggregation.

[0049] When insulating inorganic particles are added as constituent particles of the composite particles, the insulating inorganic particle powder may be included in the granulation raw material. When the insulating inorganic particles are arranged in the outermost layer of the composite particles, this process may be configured to include a first stirring process of stirring a first raw material containing a powder of core particles, a powder of magnetic particles, a binder, and water, and a second stirring process of adding the insulating inorganic particle powder to the stirred first raw material and further stirring the mixture.

[0050] [Mixed Raw Material Manufacturing Process] This process is a process for manufacturing a mixed raw material by mixing the powder of the composite particles (including the first composite particles and the second composite particles) manufactured in the previous process with a urethane foam resin raw material.

[0051] As described above, the urethane foam resin raw material may be prepared from raw materials such as polyol, polyisocyanate, catalyst, blowing agent, and foam stabilizer. In the urethane foam molded product of the present disclosure, insulating inorganic particles may be dispersed in the base material separately from the composite particles. To produce this type of urethane foam molded product, the composite particle powder, the insulating inorganic particle powder, and the urethane foam resin raw material may be mixed. The mixed raw material may be produced, for example, by mechanically stirring the composite particle powder and the urethane foam resin raw material using a stirring blade or the like. Alternatively, the composite particle powder may be added to at least one of the two components of the urethane foam resin raw material (polyol raw material, polyisocyanate raw material) to prepare two types of raw material, and then the two raw materials may be mixed to produce the urethane foam resin raw material.

[0052] [Foam Molding Step] In this step, the mixed raw material produced in the previous step is injected into the cavity of a foaming mold, and foam-molded while applying a magnetic field so that the magnetic flux density in the cavity becomes approximately uniform.

[0053] The magnetic field may be formed in the direction in which the composite particles are oriented. For example, when aligning the composite particles linearly, it is desirable to form the magnetic field lines in the cavity of the foaming mold so that they are approximately parallel from one end to the other end of the cavity. To form such a magnetic field, for example, magnets may be placed near both sides of one end and the other end of the foaming mold, sandwiching the foaming mold. The magnets may be permanent magnets or electromagnets. Using an electromagnet allows the magnetic field to be instantly switched on and off, making it easy to control the strength of the magnetic field. This makes it easy to control the foam molding. It is also desirable that the magnetic field lines that make up the magnetic field form a closed loop. This prevents leakage of the magnetic field lines and allows a stable magnetic field to be formed in the cavity.

[0054] In this process, the magnetic field is formed so that the magnetic flux density within the cavity is approximately uniform. For example, the difference in magnetic flux density within the cavity is preferably within ±10%, more preferably within ±5%, and even more preferably within ±3%. Forming a uniform magnetic field within the cavity of the foaming mold can suppress uneven distribution of the composite particles and achieve the desired orientation state. Furthermore, foam molding is preferably performed at a magnetic flux density of 150 mT or more and 350 mT or less. This ensures that the composite particles in the mixed raw material are aligned. It is desirable to apply the magnetic field while the viscosity of the urethane foam resin raw material is relatively low. If the magnetic field is applied after the urethane foam resin raw material has thickened and foam molding has been completed to a certain extent, the composite particles will not be aligned, making it difficult to achieve the desired thermal conductivity. It is not necessary to apply the magnetic field for the entire duration of foam molding.

[0055] After foam molding is completed in this step, the mold is removed to obtain the urethane foam molded article of the present disclosure. At this time, depending on the foam molding method, a skin layer is formed on at least one end of the urethane foam molded article. This skin layer may be removed (or, of course, not removed) depending on the application.

[0056] Next, the present disclosure will be described more specifically with reference to examples.

[0057] <Production of Composite Particles> First, eight types of composite particles A to H were produced as follows (composite particle production process). For composite particles B to G, both expanded graphite powder and expanded graphite powder were stirred together to produce two types of composite particles, first and second, at the same time.

[0058] [Composite Particle A] Composite particle A was produced as second composite particles by stirring a granulation raw material containing expanded graphite powder, stainless steel powder, starch powder, talc powder, and water. First, the expanded graphite powder, stainless steel powder, and starch powder were placed in the container of a high-speed stirring mixer granulator and mixed using a blade stirrer. Water was then added and mixed for 1 minute. Next, talc powder was added and mixed for an additional 4 minutes. The stirring speed was 400 rpm. The resulting powder was dried to produce composite particle A. Details of the materials used are summarized in (a) to (d) below, and the blending amounts are shown in Table 1 below (the same applies to composite particles B to H below).

[0059] [Composite Particles B to G] Composite Particles B to G were produced by the same method as the production method of Composite Particle A, except that expanded graphite powder was added as a granulation raw material. Composite Particles B to G were produced by changing the blending ratio of expanded graphite powder and expanded graphite powder, and Composite Particles B to G contain both first composite particles and second composite particles.

[0060] [Composite Particles H] Composite particles H were produced as first composite particles by the same method as that for producing composite particles A, except that expanded graphite powder was used instead of expanded graphite powder.

[0061] (a) Core particles Expanded graphite powder: "SYZR 502FP" manufactured by Shijiazhuang Aidite Trading Co., Ltd., particle size 300 μm or more: 80% or more. Expanded graphite powder: "AED-01" manufactured by Fuji Graphite Industries Co., Ltd., purity 99% or more, particle size 1000 μm or more: 80% or more. (b) Magnetic particles Stainless steel powder: "AKT" manufactured by Mitsubishi Steel Corporation, average particle size 8.5 to 13.0 μm. (c) Binder Starch powder: "Instant Tender Gel C" manufactured by Nippon Cornstarch Co., Ltd. (d) Insulating inorganic particles Talc powder: "Micro Ace (registered trademark) K-1" manufactured by Nippon Talc Co., Ltd., average particle size 8 μm.

[0062]

[0063] <Production of Urethane Foam Molded Articles> Urethane foam molded articles were produced using the produced composite particles A to H. First, a polyol raw material was prepared by mixing 100 parts by mass of polyether polyol (manufactured by Sumika Covestro Urethane Co., Ltd., "SBU (registered trademark) Polyol 0248"), 2 parts by mass of a chain extender diethylene glycol (manufactured by Mitsubishi Chemical Corporation), 2 parts by mass of a blowing agent water, 1.5 parts by mass of a tetraethylenediamine catalyst (manufactured by Kao Corporation, "Kao Raiser (registered trademark) No. 31"), and 0.5 parts by mass of a silicone foam stabilizer (manufactured by Dow Corning Toray Co., Ltd., "SZ-1333") Furthermore, a diphenylmethane diisocyanate (MDI) modified product was prepared as a polyisocyanate raw material. The MDI modified product was produced by mixing polyether polyol (same as above) and 4,4'-diphenylmethane diisocyanate ("Millionate MT" manufactured by Tosoh Corporation) so that the isocyanate (NCO) content was 70% by mass, and reacting the mixture at 100 ° C for 180 minutes under nitrogen purging. Next, 80 parts by mass of composite particles and 60 parts by mass of aluminum hydroxide powder ("SB93" manufactured by Nippon Light Metal Co., Ltd.) as insulating inorganic particles were added to 100 parts by mass of the polyol raw material and mixed to prepare a premix polyol. Subsequently, 100 parts by mass of the premix polyol and 10 parts by mass of the polyisocyanate raw material (MDI modified product) were mixed to obtain a mixed raw material (mixed raw material production process).

[0064] The mixed raw materials were then poured into an aluminum foam mold (cavity: rectangular parallelepiped, 130 mm long x 130 mm wide x 5 mm thick), and the foam mold was sealed. The foam mold was then placed in a magnetic induction foam molding machine to perform foam molding. A uniform magnetic field was formed within the foam mold cavity by approximately parallel magnetic field lines running from top to bottom. The magnetic flux density within the cavity was 200 mT, with the difference in magnetic flux density within the cavity being within ±3%. Foam molding was performed with a magnetic field applied for the first two minutes and without for the next approximately five minutes (foam molding process). After foam molding was completed, the mold was demolded to obtain a urethane foam molded body. The resulting urethane foam molded bodies are referred to as urethane foam molded bodies A to H, corresponding to the type of composite particles used. The composite particle content in urethane foam molded bodies A to H was 10% by volume, assuming the volume of the urethane foam molded body to be 100% by volume. Urethane foam molded bodies C to F are included in the concept of urethane foam molded bodies in this disclosure.

[0065] <Evaluation of Urethane Foam Molded Articles> The thermal conductivity and flame retardancy of the produced urethane foam molded articles were evaluated. The evaluation results for thermal conductivity and flame retardancy are summarized in Table 1 above. The evaluation methods are as follows.

[0066] [Thermal Conductivity] The thermal conductivity of the urethane foam molded article was measured using an "HC-110" manufactured by Eiko Seiki Co., Ltd. in accordance with the heat flow meter method of JIS A1412-2:1999.

[0067] [Flame Retardancy] A vertical flame test according to UL94 standards was carried out. In the vertical flame test, a gas burner flame is applied to the bottom end of a sample held vertically for 10 seconds, and a sample is judged to be at level V-0 if it satisfies all of the following five criteria: (1) The sample does not burn for more than 10 seconds in either of the two flame applications. (2) The total burning time for each of the five samples, after two flame applications, does not exceed 50 seconds. (3) None of the samples burn up to the position of the fixing clamp. (4) None of the samples drip burning particles, which ignites the cotton placed below the sample. (5) After the second flame application, the sample does not remain red-hot for more than 30 seconds.

[0068] As shown in Table 1, urethane foam moldings C to F contain composite particles C to F containing both first composite particles and second composite particles, and the content of expanded graphite particles is 20% to 80% by mass, where the total mass of the expanded graphite particles and the expanded graphite particles is 100% by mass. Therefore, urethane foam moldings C to F have a thermal conductivity of 0.65 W / m·K or higher and a flame retardancy of V-0, confirming that they satisfy both thermal conductivity and flame retardancy. In contrast, urethane foam molding A, which uses composite particles A containing only second composite particles, and urethane foam molding B, which has a low content of expanded graphite particles, satisfied flame retardancy but had poor thermal conductivity. Furthermore, urethane foam molding H, which uses composite particles H containing only first composite particles, and urethane foam molding G, which has a high content of expanded graphite particles, satisfied thermal conductivity but had poor flame retardancy.

[0069] The urethane foam molded article of the present disclosure is suitable as a soundproofing material used in vehicle parts such as inverters, motors, and gearboxes of electric powertrains, engine cylinder heads and cylinder head covers, and electronic devices such as personal computers.

Claims

1. A urethane foam molded product comprising: a substrate made of polyurethane foam; and composite particles contained and oriented in the substrate, the composite particles comprising: first composite particles having expanded graphite particles and magnetic particles bonded to the surfaces of the expanded graphite particles with a binder; and second composite particles having expanded graphite particles and magnetic particles bonded to the surfaces of the expanded graphite particles with a binder, wherein when the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is taken as 100 mass%, the content of the expanded graphite particles is 20 mass% or more and 80 mass% or less.

2. The urethane foam molded article according to claim 1, wherein the average particle size of the expanded graphite particles is from 100 μm to 3,000 μm.

3. The urethane foam molded article according to claim 1 or 2, wherein the purity of the expanded graphite particles is 99% or more.

4. A urethane foam molded article according to any one of claims 1 to 3, wherein the average particle size of the expanded graphite particles is 100 μm or more and 3000 μm or less.

5. A urethane foam molded body according to any one of claims 1 to 4, wherein the content of the composite particles is 5 volume % or more and 50 volume % or less, when the volume of the urethane foam molded body is 100 volume %.

6. A urethane foam molded article according to any one of claims 1 to 5, wherein the binder constituting the first composite particles and the second composite particles is a water-soluble polymer.

7. The urethane foam molded article according to claim 6, wherein the water-soluble polymer is one or more selected from the group consisting of methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and starch.

8. A urethane foam molding described in any one of claims 1 to 7, wherein the content of the magnetic particles constituting the first composite particles and the second composite particles is 20 mass% or more and 80 mass% or less, when the total mass of the expanded graphite particles and the expanded graphite particles in the base material is 100 mass%.

9. A urethane foam molded article according to any one of claims 1 to 8, wherein the magnetic particles constituting the first composite particles and the second composite particles comprise one or more types selected from iron particles and iron-based alloy particles.

10. A urethane foam molding described in any one of claims 1 to 9, wherein at least one of the first composite particles and the second composite particles has insulating inorganic particles adhered to the surface of the expanded graphite particles or the expanded graphite particles by a binder.

11. The urethane foam molded article according to claim 10, wherein the insulating inorganic particles comprise at least one type selected from the group consisting of aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, and silica.

Citation Information

Patent Citations

  • Urethane foam molded body and method for producing the same

    JP2012051986A

  • Method for manufacturing urethane foam molding and apparatus for agitating foamed urethane resin ingredients used for the same

    JP2014188916A

  • Slurry dispersion and refractory material

    JP2022125931A

  • Polyurethane foam, polyol composition and method for producing polyurethane foam

    JP2023016623A

  • Urethane foam molding and method for manufacturing same

    WO2013042611A1