Solid state battery
The integration of an oxide glass-based solid electrolyte with a specific density ratio in the negative electrode layer of solid-state batteries addresses interfacial resistance issues, enhancing energy density and charge/discharge efficiency.
Patent Information
- Application Number
- PCT/JP2023/047055
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional solid-state batteries face challenges in reducing interfacial resistance between the negative electrode active material and the solid electrolyte, which limits the volumetric energy density and charge/discharge efficiency due to porosity and poor contact between garnet-type oxide-based solid electrolytes and negative electrode materials.
A solid-state battery design incorporating a negative electrode layer with a Li composite oxide and an oxide glass-based solid electrolyte, where the solid electrolyte content is between 20% to 60% by mass, and the actual density ratio of the negative electrode active material to its true density is maintained between 0.3 and 0.6, enhancing the contact interface and lithium ion conduction.
This configuration reduces interfacial resistance, improves lithium ion mobility, and increases the volumetric energy density and charge/discharge efficiency, achieving efficiencies of 85% or higher.
Smart Images

Figure JP2023047055_03102024_PF_FP_ABST
Abstract
Description
solid state battery
[0001] The present invention relates to a solid-state battery.
[0002] Secondary batteries that can be repeatedly charged and discharged have been used for various purposes, such as power sources for electronic devices such as smartphones and laptop computers.
[0003] In secondary batteries, a liquid electrolyte is generally used as a medium for ion migration, which contributes to charging and discharging. In other words, a so-called electrolytic solution is used in secondary batteries. However, such secondary batteries generally require safety in terms of preventing leakage of the electrolytic solution. In addition, organic solvents and the like used in the electrolytic solution are flammable, so safety is also required in this respect. Therefore, research is being conducted on solid-state batteries that use solid electrolytes instead of electrolytic solutions.
[0004] The solid-state battery comprises a battery element including a positive electrode layer, a negative electrode layer, and a solid electrolyte interposed between the positive electrode layer and the negative electrode layer. The positive electrode layer includes a positive electrode active material and the solid electrolyte, and the negative electrode layer includes a negative electrode active material and the solid electrolyte.
[0005] JP 2015-144061 A JP 2019-77573 A JP 2020-068188 A
[0006] The inventors of the present application have newly discovered that there are areas in which conventional solid-state batteries can be improved, and that there is a need to take measures to achieve this.
[0007] Specifically, in solid-state batteries, the electrode layer, particularly the negative electrode layer, may be composed of a combination of a negative electrode active material containing a Li composite oxide and a garnet-type oxide-based solid electrolyte. However, it is difficult for the garnet-type oxide-based solid electrolyte to form a dense interface with the particles of the negative electrode active material, making it difficult to reduce the porosity within the electrode. This increases the interfacial resistance between the active material and the solid electrolyte in the negative electrode, making it difficult for lithium ions to cross this interface. As a result, it may be difficult to increase the volumetric energy density of the solid-state battery.
[0008] The present invention has been made in view of the above-mentioned problems. That is, an object of the present invention is to provide a solid-state battery including a negative electrode layer that can reduce the interfacial resistance between the active material and the solid electrolyte.
[0009] In order to achieve the above object, one embodiment of the present invention provides a solid-state battery including: an anode layer including an anode active material containing a Li composite oxide; and an oxide glass-based solid electrolyte; wherein a content of the solid electrolyte in the anode layer is 20 mass % or more and 60 mass % or less with respect to a total amount of the anode active material and the solid electrolyte; and wherein a ratio (B / A) of an actual density B of the anode active material to a true density A of the anode active material is 0.3 or more and 0.6 or less.
[0010] According to the solid state battery according to one embodiment of the present invention, it is possible to provide a negative electrode layer that can reduce the interface resistance between the active material and the solid electrolyte.
[0011] Fig. 1 is a perspective view showing a schematic external appearance of a solid-state battery according to an embodiment of the present invention, and Fig. 2 is a schematic cross-sectional view of the solid-state battery taken along line AA in Fig. 1 as viewed in the direction of the arrows.
[0012] The solid-state battery of the present invention will be described in detail below. While the description will be made with reference to the drawings as necessary, the contents shown in the drawings are merely schematic and illustrative for understanding the present invention, and the appearance and dimensional ratios may differ from the actual product.
[0013] The term "cross-sectional view" as used herein refers to the shape of a solid-state battery viewed from a direction substantially perpendicular to the stacking direction (in other words, the shape of a solid-state battery cut along a plane parallel to the thickness direction of the layers). The terms "planar view" and "planar shape" as used herein refer to a sketch of an object viewed from above or below along the thickness direction of the layers (i.e., the stacking direction).
[0014] The terms "upper and lower directions" and "left and right directions" used directly or indirectly in this specification correspond to the upper and lower directions and left and right directions in the drawings, respectively. Unless otherwise specified, the same symbols or signs indicate the same members or parts or the same meanings. In a preferred embodiment, the vertical downward direction (i.e., the direction in which gravity acts) can be considered to correspond to the "downward direction," and the opposite direction to that can be considered to correspond to the "upward direction."
[0015] In the present invention, the term "solid-state battery" refers in a broad sense to a battery whose components are made of solids, and in a narrow sense to an all-solid-state battery whose components (particularly preferably all components) are made of solids. In a preferred embodiment, the solid-state battery of the present invention is a stacked-type solid-state battery in which each layer constituting a battery unit is stacked on top of each other, and preferably each such layer is made of a sintered body. A "solid-state battery" is a so-called "secondary battery" that can be repeatedly charged and discharged. The term "secondary battery" should not be overly limited to its name, and can also include, for example, an electricity storage device.
[0016] A feature of the present invention relates to a positive electrode layer included in a solid-state battery. Below, we will first explain the basic configuration of the solid-state battery of the present invention in order to understand the overall structure of the solid-state battery. However, the configuration of the solid-state battery described here is merely an example for understanding the invention and does not limit the invention.
[0017] [Basic Structure of Solid-State Battery] Fig. 1 is a perspective view showing a schematic external appearance of a solid-state battery according to one embodiment of the present invention. Fig. 2 is a schematic cross-sectional view of the solid-state battery of Fig. 1 taken along the line A-A in the direction of the arrow. A solid-state battery has at least positive and negative electrode layers and a solid electrolyte. Specifically, as shown in Figs. 1 and 2, a solid-state battery 200 includes a solid-state battery stack 100 including battery structural units each consisting of a positive electrode layer 10A, a negative electrode layer 10B, and a solid electrolyte 20 interposed at least between them.
[0018] A solid-state battery 200 according to the present invention comprises a solid-state battery stack 100 including, along a stacking direction L, at least one battery structural unit composed of a positive electrode layer 10A, a negative electrode layer 10B, and a solid electrolyte layer 20 interposed therebetween; and a positive electrode terminal 40A and a negative electrode terminal 40B provided on opposing side surfaces of the solid-state battery stack 100. In the solid-state battery stack 100, the positive electrode layers 10A and the negative electrode layers 10B are alternately stacked with the solid electrolyte layer 20 interposed therebetween.
[0019] In the solid-state battery, each of the constituent layers may be formed by firing, and the positive electrode layer, negative electrode layer, solid electrolyte layer, etc. may form fired layers. Preferably, the positive electrode layer, negative electrode layer, and solid electrolyte layer are each fired together, and the solid-state battery laminate forms a fired body.
[0020] The positive electrode layer is an electrode layer containing at least a positive electrode active material. The positive electrode layer may further contain a solid electrolyte. In a preferred embodiment, the positive electrode layer is composed of a sintered body containing at least positive electrode active material particles and solid electrolyte particles. On the other hand, the negative electrode layer is an electrode layer containing at least a negative electrode active material. The negative electrode layer may further contain a solid electrolyte. In a preferred embodiment, the negative electrode layer is composed of a sintered body containing at least negative electrode active material particles and solid electrolyte particles. A positive electrode layer having such a configuration is referred to as a "composite positive electrode body," and similarly, a negative electrode layer may be referred to as a "composite negative electrode body."
[0021] The positive electrode active material and the negative electrode active material are materials involved in the transfer of electrons in a solid-state battery. Charge and discharge are performed by the transfer of electrons through the transfer (conduction) of ions between the positive electrode layer and the negative electrode layer via the solid electrolyte. It is preferable that each electrode layer, the positive electrode layer and the negative electrode layer, is a layer capable of absorbing and releasing lithium ions or sodium ions in particular. In other words, the solid-state battery is preferably an all-solid-state secondary battery in which lithium ions or sodium ions transfer between the positive electrode layer and the negative electrode layer via the solid electrolyte to charge and discharge the battery.
[0022] The positive electrode active material contained in the positive electrode layer can be selected from, for example, lithium-containing layered oxides, lithium-containing oxides having a spinel structure, etc. An example of the lithium-containing layered oxide is LiCoO 2 , LiCo 1/3 Ni 1/3 Mn 1/3 O 2 An example of a lithium-containing oxide having a spinel structure is LiMn 2 O 4 , LiNi 0.5 Mn 1.5 O 4 etc.
[0023] The positive electrode active material capable of absorbing and releasing sodium ions can be selected from sodium-containing layered oxides, sodium-containing oxides having a spinel structure, and the like.
[0024] The positive electrode layer and / or the negative electrode layer may contain a conductive material, which may include at least one of metal materials such as silver, palladium, gold, platinum, aluminum, copper, and nickel, and carbon.
[0025] Furthermore, the positive electrode layer and / or the negative electrode layer may contain a sintering aid, such as at least one selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, boron oxide, silicon oxide, bismuth oxide, and phosphorus oxide.
[0026] There are no particular limitations on the thickness of the positive electrode layer and the negative electrode layer, but for example, they may each independently be 2 μm or more and 50 μm or less, particularly 5 μm or more and 30 μm or less.
[0027] (Positive electrode current collecting layer / negative electrode current collecting layer) Although not essential elements of the electrode layer, the positive electrode layer and the negative electrode layer may include a positive electrode current collecting layer 11A and a negative electrode current collecting layer 11B, respectively. The positive electrode current collecting layer and the negative electrode current collecting layer may each have the form of a foil. However, if emphasis is placed on improving electronic conductivity through co-firing, reducing the manufacturing cost of the solid-state battery, and / or reducing the internal resistance of the solid-state battery, the positive electrode current collecting layer and the negative electrode current collecting layer may each have the form of a sintered body.
[0028] The positive electrode current collector constituting the positive electrode current collecting layer and the negative electrode current collector constituting the negative electrode current collector are preferably made of a material with high electrical conductivity, such as silver, palladium, gold, platinum, aluminum, copper, and / or nickel. The positive electrode current collector and the negative electrode current collector may each have an electrical connection part for electrical connection to the outside and may be configured to be electrically connectable to a terminal.
[0029] When the positive electrode current collecting layer and the negative electrode current collecting layer are in the form of a sintered body, they may be composed of a sintered body containing a conductive material and a sintering aid. The conductive material contained in the positive electrode current collecting layer and the negative electrode current collecting layer may be selected from, for example, the same materials as the conductive materials that may be contained in the positive electrode layer and the negative electrode layer. The sintering aid contained in the positive electrode current collecting layer and the negative electrode current collecting layer may be selected from, for example, the same materials as the sintering aids that may be contained in the positive electrode layer and the negative electrode layer.
[0030] (Solid Electrolyte) The solid electrolyte is a material capable of conducting lithium ions or sodium ions. This solid electrolyte may form a layer capable of conducting lithium ions between the positive electrode layer and the negative electrode layer. The solid electrolyte may also be contained within the positive electrode layer and the negative electrode layer.
[0031] The solid electrolyte layer may contain a sintering aid. The sintering aid contained in the solid electrolyte layer may be selected from the same materials as the sintering aids that may be contained in the positive electrode layer and the negative electrode layer, for example.
[0032] The thickness of the solid electrolyte layer is not particularly limited. The thickness of the solid electrolyte layer located between the positive electrode layer and the negative electrode layer may be, for example, 1 μm to 15 μm, particularly 1 μm to 5 μm.
[0033] (Electrode Separation Portion) The solid state battery 200 of the present invention may further have an electrode separation portion (also referred to as a "blank layer" or "blank portion") 30 (30A, 30B).
[0034] The electrode separator 30A (positive electrode separator) is disposed around the positive electrode layer 10A, thereby separating the positive electrode layer 10A from the negative electrode terminal 40B. The electrode separator 30B (negative electrode separator) is disposed around the negative electrode layer 10B, thereby separating the negative electrode layer 10B from the positive electrode terminal 40A. Although not particularly limited, the electrode separator 30 may be made of one or more materials selected from the group consisting of, for example, a solid electrolyte, an insulating material, a mixture thereof, and the like.
[0035] The solid electrolyte that can form the electrode separator 30 can be made of the same material as the solid electrolyte that can form the solid electrolyte layer.
[0036] The insulating material that can form the electrode separator 30 may be a material that does not conduct electricity, i.e., a non-conductive material. Although not particularly limited, the insulating material may be, for example, a glass material, a ceramic material, or the like. For example, a glass material may be selected as the insulating material. Although not particularly limited, the glass material may be at least one selected from the group consisting of soda-lime glass, potash glass, borate-based glass, borosilicate-based glass, barium borosilicate-based glass, zinc borate-based glass, barium borate-based glass, bismuth borosilicate-based glass, bismuth zinc borate-based glass, bismuth silicate-based glass, phosphate-based glass, aluminophosphate-based glass, and zinc phosphate-based glass. Furthermore, although not particularly limited, the ceramic material may be aluminum oxide (Al 2 O 3 ), boron nitride (BN), silicon dioxide (SiO 2 ), silicon nitride (Si 3 N 4 ), zirconium oxide (ZrO 2 ), aluminum nitride (AlN), silicon carbide (SiC), and barium titanate (BaTiO 3 ) can be mentioned as at least one selected from the group consisting of
[0037] (Terminals) The solid-state battery 200 of the present invention generally has terminals (external terminals) 40 (40A, 40B). In particular, positive and negative terminals 40A, 40B are provided in pairs on the side surfaces of the solid-state battery. More specifically, the positive terminal 40A connected to the positive electrode layer 10A and the negative terminal 40B connected to the negative electrode layer 10B are provided in pairs. The terminals 40A, 40B may also be referred to as "end electrodes" because they can be provided to cover at least one side surface of the solid-state battery. Such terminals 40 (40A, 40B) can be made of a material with high conductivity. The material of the terminal 40 is not particularly limited, but may include at least one conductive material selected from the group consisting of silver, gold, platinum, aluminum, copper, tin, and nickel.
[0038] The terminal 40 (40A, 40B) may further contain a sintering aid. Examples of the sintering aid include the same materials as the sintering aid that may be contained in the positive electrode layer 10A. In a preferred embodiment, the terminal 40 (40A, 40B) is made of a sintered body that contains at least a conductive material and a sintering aid.
[0039] (Outer Layer Material) The solid-state battery 200 of the present invention typically further includes an outer layer material 60. The outer layer material 60 is generally formed on the outermost surface of the solid-state battery to provide electrical, physical, and / or chemical protection. The material constituting the outer layer material 60 preferably has excellent insulating properties, durability, and / or moisture resistance, and is environmentally safe. For example, glass, ceramics, thermosetting resin, photocurable resin, and mixtures thereof can be used.
[0040] The glass that can be used to form the outer layer material can be the same material as the glass material that can be used to form the electrode separator, and the ceramic material that can be used to form the outer layer material can be the same material as the ceramic material that can be used to form the electrode separator.
[0041] [Features of the Solid-State Battery of the Present Invention] The present inventors have conducted extensive research into solutions for reducing the interfacial resistance between the active material and the solid electrolyte in the negative electrode layer of a solid-state battery, and as a result, have devised the present invention, which has technical features relating to a specific combination of the negative electrode active material and the solid electrolyte in the negative electrode layer, as well as specific ranges of the density of the negative electrode active material and the content of the solid electrolyte.
[0042] Specifically, the present invention has a technical feature in that the anode layer contains an anode active material containing a Li composite oxide and an oxide glass-based solid electrolyte, the content of the solid electrolyte is 20 mass % or more and 60 mass % or less with respect to the total amount of the anode active material and the solid electrolyte in the anode layer, and the ratio (B / A) of the actual density B of the anode active material to the true density A of the anode active material is 0.3 or more and 0.6 or less.
[0043] In this specification, the term "negative electrode active material and solid electrolyte in the negative electrode layer" refers to the negative electrode active material and solid electrolyte located in a region other than voids that may be formed in the negative electrode layer of the final solid-state battery (corresponding to the finished product).
[0044] According to the above technical feature, when the content of the solid electrolyte in the negative electrode layer is 20% by mass or more and 60% by mass or less, it is possible to ensure a predetermined ratio (0.3 or more and 0.6 or less) of the actual density B of the negative electrode active material in the fabricated battery to the true density A of the negative electrode active material. For example, the true density A of the above negative electrode active material is 3.0 g / cm 3 4.0g / cm or more 3 or less, for example 3.5 g / cm 3 Furthermore, when the content of the solid electrolyte in the negative electrode layer is 20 mass % or more, a predetermined amount of solid electrolyte is ensured compared to when the content is less than 20 mass %.
[0045] As a result, the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer can be made dense, and a conductive path for lithium ions can be suitably formed. That is, the interfacial resistance between the negative electrode active material and the solid electrolyte in the negative electrode layer can be reduced, and lithium ions can easily move across this interface. As a result, the internal resistance of the battery can be reduced, and the volumetric energy density can be improved.
[0046] Furthermore, when the content of the solid electrolyte in the negative electrode layer is 60 mass % or less, a ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material can be ensured to be 0.3 or more, compared to when the content exceeds 60 mass %. As a result, in the fabricated battery, a predetermined amount of the negative electrode active material is contained in the negative electrode layer, and therefore the interparticle distance of the negative electrode active material in the negative electrode layer can be kept to a distance that allows the formation of a suitable electron path.
[0047] As a result, it is possible to ensure a discharge capacity that can achieve a charge / discharge efficiency equal to or higher than a predetermined reference value (85% or higher), and it is possible to suitably improve the battery characteristics of the solid-state battery.
[0048] As used herein, the term "true density of the negative electrode active material" refers to the density inherent to a specific type of negative electrode active material, and the term "true density of the solid electrolyte" refers to the density inherent to a specific type of solid electrolyte. The true densities of the negative electrode active material and the solid electrolyte can be calculated by a gas-phase displacement method using helium gas. The true density can be calculated by changing the pressure and volume to determine the volume of the object to be measured and then measuring the weight. Furthermore, the term "real density of the negative electrode active material" refers to the volume density of the negative electrode active material in the negative electrode layer of the solid-state battery after fabrication.
[0049] Furthermore, the actual density B of the negative electrode active material after the battery is fabricated can be calculated using the true density A of the negative electrode active material, the true density C of the solid electrolyte, the porosity E in the negative electrode, the content F of the negative electrode active material in the negative electrode layer, and the content G of the solid electrolyte. The calculation formulas are as follows: Volumetric blending ratio of negative electrode active material (V1) = (100 - E) x F / A / (F / A + G / C) Actual density of negative electrode active material after molding (B) = (A x V1) / 100
[0050] The porosity within the electrode can be calculated by forming a smooth cross section of the obtained solid-state battery by ion milling and observing the cross section at 5000x magnification using an SEM, using software called Image J. The content F of the negative electrode active material and the content G of the solid electrolyte can also be calculated in a similar manner.
[0051] In the present invention, the content of the solid electrolyte is preferably 30% by mass or more and 50% by mass or less relative to the total amount of the negative electrode active material and the solid electrolyte. In this case, the content of the solid electrolyte in the negative electrode layer is increased by 10% by mass compared to when the content is 20% by mass, thereby making the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer denser and more suitably forming a conduction path for lithium ions.
[0052] When the solid electrolyte content in the negative electrode layer is 50 mass% or less, the amount of negative electrode active material increases by 10 mass% compared to when the solid electrolyte content is 60 mass%, thereby making it possible to more suitably reduce the interparticle distance of the negative electrode active material in the negative electrode layer to a distance that allows for the formation of an electron path. As a result, it is possible to ensure a discharge capacity that can achieve a charge / discharge efficiency equal to or higher than a predetermined standard value (95% or higher), and it is possible to more suitably improve the battery characteristics of the solid-state battery.
[0053] Furthermore, when the content of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte in the negative electrode layer is a uniform predetermined amount (for example, 40 mass%), the ratio (C / A) of the true density C of the solid electrolyte to the true density A of the negative electrode active material can be 0.55 or more and 0.9 or less. For example, the true density C of the solid electrolyte can be 2.0 g / cm 3 3.0g / cm or more 3 Preferably 2.0 g / cm or less 3 2.5g / cm or more 3 It can be:
[0054] If the ratio C / A is within this range, it is possible to ensure that the actual density B of the negative electrode active material in the battery after fabrication is a predetermined ratio (0.3 to 0.6) relative to the true density A of the negative electrode active material. On the other hand, if the ratio C / A is outside this range (specifically, 0.51), it is not possible to ensure that the actual density B of the negative electrode active material in the battery after fabrication is a predetermined ratio (0.3 to 0.6) relative to the true density A of the negative electrode active material.
[0055] As a result, in the fabricated battery, a predetermined amount of the negative electrode active material (and solid electrolyte) is secured in the negative electrode layer, and therefore the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer can be made dense, and a conductive path for lithium ions can be suitably formed.
[0056] Furthermore, when the ratio C / A is 0.6 or more and 0.75 or less, the ratio B / A can be 0.35 or more and 0.5 or less. In this case, the ratio B / A can be made higher than when the ratio C / A is less than 0.6. This allows a predetermined amount of the negative electrode active material (and solid electrolyte) to be more suitably secured in the negative electrode layer after fabrication, thereby making the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer denser and more suitably forming a conduction path for lithium ions.
[0057] The Li composite oxide contained in the above-mentioned negative electrode active material can be an oxide containing Li and a transition metal element, and for example, can be an oxide containing Li and at least one metal element selected from the group consisting of titanium (Ti), silicon (Si), tin (Sn), chromium (Cr), iron (Fe), niobium (Nb), and molybdenum (Mo). For example, the Li composite oxide contained in the above-mentioned negative electrode active material can be an oxide containing Li and Ti. When an oxide containing Li and Ti is used, a high energy density can be obtained while suppressing the expansion and contraction of the negative electrode layer during charge and discharge.
[0058] The oxide glass-based solid electrolyte of the negative electrode layer has the advantage of being able to contribute to reducing the porosity in the negative electrode, and can be, for example, lithium borosilicate glass. Lithium borosilicate glass is an oxide glass material containing at least lithium (Li), silicon (Si), and boron (B) as constituent elements, and can be, for example, 50Li 4 SiO 4 ・50Li 3 BO 3 Lithium borosilicate glass can be advantageous in that it has a low glass transition temperature and can form a dense negative electrode layer.
[0059] Furthermore, the solid electrolyte may contain, in addition to the lithium borosilicate glass as a glass-based solid electrolyte, a solid electrolyte used in other known solid-state batteries. Examples of such solid electrolytes include one or more of a crystalline solid electrolyte, a glass-based solid electrolyte other than lithium borosilicate glass, and a glass-ceramic solid electrolyte. The crystalline solid electrolyte may be, for example, an oxide-based crystalline material. Examples of oxide-based crystalline materials include lithium-containing phosphate compounds having a Nasicon structure, oxides having a perovskite structure, oxides having a garnet-type or garnet-like structure, and oxide glass-ceramic lithium ion conductors.
[0060] The lithium-containing phosphate compound having a Nasicon structure includes Li x M y (P.O. 4 ) 3 (1≦x≦2, 1≦y≦2, M is at least one selected from the group consisting of titanium (Ti), germanium (Ge), aluminum (Al), gallium (Ga) and zirconium (Zr). An example of a lithium-containing phosphate compound having a Nasicon structure is, for example, Li 1.2 Al 0.2 Ti 1.8 (P.O. 4 ) 3 Examples of oxides having a perovskite structure include La 0.55 Li 0.35 TiO3 Examples of oxides having a garnet-type or garnet-like structure include Li 7 La 3 Zr 2 O 12 The crystalline solid electrolyte may include a polymer material (for example, polyethylene oxide (PEO)).
[0061] As a glass-based solid electrolyte other than lithium borosilicate glass, 30Li 2 S・26B 2 S 3 ・44LiI, 63Li 2 S・36SiS 2 ・1Li 3 P.O. 4 , 57Li 2 S・38SiS 2 ・5Li 4 SiO 4 , 70Li 2 S・30P 2 S 5 and 50Li 2 S・50GeS 2 etc.
[0062] The glass ceramic solid electrolyte is, for example, an oxide-based glass ceramic material. Examples of the oxide-based glass ceramic material include a phosphate compound containing lithium, aluminum, and titanium as constituent elements (LATP) and a phosphate compound containing lithium, aluminum, and germanium as constituent elements (LAGP). LATP is, for example, a phosphate compound containing Li, 1.07 Al 0.69 Ti 1.46 (P.O. 4 ) 3 LAGP is, for example, Li 1.5 Al 0.5 Ge 1.5 (P.O. 4 ) etc.
[0063] For example, the solid electrolyte may further contain, in addition to the lithium borosilicate glass, an oxide having a garnet-type or garnet-like structure from the viewpoint of improving ion conductivity.
[0064] [Method for Manufacturing a Solid-State Battery] The solid-state battery of the present invention can be manufactured by a printing method such as a screen printing method, a green sheet method using a green sheet, or a combination of these methods. Below, the cases where the printing method and the green sheet method are used will be described in detail for the purpose of understanding the present invention, but the present invention is not limited to these methods. In other words, the solid-state battery may be manufactured according to a conventional method for manufacturing a solid-state battery. Furthermore, the chronological matters, such as the order of description below, are merely for the convenience of explanation and are not necessarily bound by them.
[0065] (Step of forming a solid battery laminate precursor) In this step, several types of pastes are used as inks, such as a paste for a positive electrode layer, a paste for a negative electrode layer, a paste for a solid electrolyte layer, a paste for a positive electrode current collector layer, a paste for a negative electrode current collector layer, a paste for an electrode separator, and a paste for an outer layer material, etc. That is, the pastes are applied by a printing method and dried to form a solid battery laminate precursor having a predetermined structure on a support substrate.
[0066] In printing, a solid state battery laminate precursor corresponding to a predetermined solid state battery structure can be formed on a substrate by sequentially stacking printed layers with a predetermined thickness and pattern shape. The type of pattern formation method is not particularly limited as long as it is a method capable of forming a predetermined pattern, and may be, for example, one or more of a screen printing method, a gravure printing method, etc.
[0067] The paste can be prepared by wet mixing predetermined constituent materials for each layer appropriately selected from the group consisting of positive electrode active material particles, negative electrode active material particles, conductive material, solid electrolyte material, current collecting layer material, insulating material, sintering aid, and other materials mentioned above, with an organic vehicle in which an organic material is dissolved in a solvent.
[0068] The paste for the positive electrode layer contains, for example, positive electrode active material particles, a solid electrolyte material, an organic material and a solvent, and, if desired, a sintering aid.
[0069] The paste for the negative electrode layer contains, for example, negative electrode active material particles, a solid electrolyte material, an organic material and a solvent, and, if desired, a sintering aid.
[0070] The paste for the solid electrolyte layer contains, for example, a solid electrolyte material, an organic material, a solvent, and, if desired, a sintering aid.
[0071] The paste for the positive electrode current collector layer contains a conductive material, an organic material, a solvent, and, if desired, a sintering aid.
[0072] The paste for the negative electrode current collector layer contains a conductive material, an organic material, a solvent, and, if desired, a sintering aid.
[0073] The paste for the electrode separator contains, for example, a solid electrolyte material, an insulating material, an organic material, a solvent, and, if desired, a sintering aid.
[0074] The paste for the outer layer material contains, for example, an insulating material, an organic material, a solvent, and, if desired, a sintering aid.
[0075] The organic material contained in the paste is not particularly limited, but at least one polymer material selected from the group consisting of polyvinyl acetal resin, cellulose resin, polyacrylic resin, polyurethane resin, polyvinyl acetate resin, and polyvinyl alcohol resin can be used.
[0076] The type of solvent is not particularly limited, but may be, for example, one or more of organic solvents such as butyl acetate, N-methyl-pyrrolidone, toluene, terpineol, and N-methyl-pyrrolidone.
[0077] In the wet mixing, media can be used, specifically, a ball mill method, a viscomill method, etc. Alternatively, a wet mixing method without using media can be used, such as a sand mill method, a high-pressure homogenizer method, or a kneader dispersion method.
[0078] The support substrate is not particularly limited as long as it is a support capable of supporting each paste layer, and may be, for example, a release film with one surface subjected to a release treatment. Specifically, a substrate made of a polymer material such as polyethylene terephthalate can be used. When the paste layer is subjected to the firing step while being held on the substrate, a substrate that is heat resistant to the firing temperature may be used.
[0079] Alternatively, each paste may be formed into a green sheet, and the resulting green sheets may be stacked to form a solid state battery laminate precursor.
[0080] Specifically, the support base coated with each paste is dried on a hot plate heated to 30°C or higher and 90°C or lower, thereby forming a positive electrode layer green sheet, a negative electrode layer green sheet, a solid electrolyte layer green sheet, a positive electrode current collector layer green sheet, a negative electrode current collector layer green sheet, an electrode separator green sheet, and / or an outer layer material green sheet, each having a predetermined shape and thickness, on each support base (e.g., a PET film).
[0081] Next, each green sheet is peeled off from the substrate. After peeling, the green sheets of each component are stacked in order along the stacking direction to form a solid state battery laminate precursor. After stacking, a solid electrolyte layer, an insulating layer, and / or a protective layer may be provided on the side regions of the electrode green sheets by screen printing.
[0082] (Firing Step) In the firing step, the solid battery laminate precursor is subjected to firing. For illustrative purposes, firing is performed by heating in an oxygen-containing nitrogen gas atmosphere or in the air, for example, at 200°C or higher to remove organic materials, and then heating in a nitrogen gas atmosphere or in the air, for example, at 300°C or higher and 500°C or lower. Firing can be performed while applying pressure of 20 to 100 MPa to the solid battery laminate precursor in the stacking direction (and in some cases, in the stacking direction and a direction perpendicular to the stacking direction).
[0083] Through such firing, a solid state battery stack is formed, and ultimately a desired solid state battery is obtained.
[0084] (Step of forming positive and negative electrode terminals) For example, a positive electrode terminal is attached to the solid battery stack using a conductive adhesive, and a negative electrode terminal is attached to the solid battery stack using a conductive adhesive. In this way, the positive electrode terminal and the negative electrode terminal are respectively attached to the solid battery stack. As a result, a desired solid battery can finally be obtained.
[0085] Although the embodiments of the present invention have been described above, they are merely typical examples. Therefore, the present invention is not limited to these, and it will be readily understood by those skilled in the art that various modifications are possible within the scope of the present invention.
[0086] Examples will be described below.
[0087] Example 1 (Process for Producing Green Sheet for Solid Electrolyte Layer) First, a halogen-containing lithium borosilicate glass (60Li) was used as a solid electrolyte. 2 O-10SiO 2 -30B 2 O 3 The solid electrolyte used in Example 1 had a true density of 2.5 g / cm. 3 It was.
[0088] The resulting mixture was then mixed with butyl acetate as a solvent to a solid content of 30% by mass, and the resulting mixture was stirred for 4 hours with zirconia balls having a diameter of 5 mm to obtain a paste for a solid electrolyte layer. The paste was then applied to a release film and dried at 80°C for 20 minutes to produce a green sheet for a solid electrolyte layer as a solid electrolyte layer precursor.
[0089] (Process for Producing Green Sheet for Positive Electrode Material Layer) First, lithium cobalt oxide (LiCoO 2 Next, LiCoO 2 The solid electrolyte used in the above-mentioned green sheet for the solid electrolyte layer and an acrylic binder are mixed with LiCoO 2 The mixture was mixed at a mass ratio of 70:20:10: solid electrolyte: binder. The resulting mixture was then mixed with terpineol to achieve a solid content of 60 mass%. The resulting mixture was stirred for 1 hour with zirconia balls having a diameter of 5 mm to obtain a cathode layer paste. This paste was then applied to a release film and dried at 80°C for 20 minutes to produce a cathode layer green sheet as a cathode layer precursor.
[0090] (Process for Producing a Green Sheet for Negative Electrode Material Layer) First, Li was used as a negative electrode active material. 4 Ti 5 O 12 (Merck, product number 915939), the solid electrolyte used in the above-mentioned green sheet for the solid electrolyte layer as the solid electrolyte, and an acrylic binder were mixed with Li 4 Ti 5 O 12 The negative electrode active material was mixed in a mass ratio of 72:18:10. The true density of the negative electrode active material used was 3.5 g / cm 3 It was.
[0091] The resulting mixture was then mixed with terpineol to a solids content of 60% by mass. The resulting mixture was stirred for 1 hour with zirconia balls having a diameter of 5 mm to obtain a paste for the negative electrode layer. The paste was then applied to a release film and dried at 80°C for 20 minutes to produce a green sheet for the negative electrode layer as a precursor for the negative electrode layer.
[0092] (Process for Producing a Positive Electrode Current Collector Green Sheet) First, carbon powder (manufactured by Resonac, product number VGCF (registered trademark)-F) was mixed as a conductive material, the solid electrolyte used in the above-described solid electrolyte layer green sheet as a solid electrolyte, and an acrylic binder in a mass ratio of carbon powder:solid electrolyte:binder = 70:20:10. Next, the resulting mixture was mixed with terpineol to achieve a solid content of 60 mass%. The resulting mixture was then stirred for 1 hour with zirconia balls having a diameter of 5 mm to obtain a positive electrode current collector layer paste. Next, this paste was applied to a release film and dried at 80°C for 20 minutes to produce a positive electrode current collector layer green sheet as a positive electrode current collector layer precursor.
[0093] (Process for Producing Green Sheet for Negative Electrode Current Collector Layer) A green sheet for a negative electrode current collector layer was produced in the same manner as in the process for producing the green sheet for a positive electrode current collector layer described above.
[0094] (Process for Producing Green Sheets for Outer Layer Materials) First, alumina particle powder (manufactured by Kojundo Chemical Research Co., Ltd., product number γ-Al 2 O3 Alumina), the solid electrolyte used in the solid electrolyte layer green sheet, and an acrylic binder were mixed in a mass ratio of carbon powder:solid electrolyte:binder = 70:20:10. The resulting mixture was then mixed with terpineol to achieve a solid content of 60 mass%. The resulting mixture was then stirred for 1 hour with zirconia balls having a diameter of 5 mm to obtain a paste for a main surface exterior material. This paste was then applied to a release film and dried to produce a green sheet for an outer layer material as an outer layer material precursor.
[0095] (Step of Producing Green Sheet for Electrode Separation Portion) In the same manner as the step of producing the green sheet for the outer layer material described above, a green sheet for the electrode separation portion was produced as an electrode separation portion precursor.
[0096] (Laminate Fabrication Process) Using each green sheet obtained as described above, a laminate having the configuration shown in Figures 1 and 2 was fabricated as follows. Specifically, first, each green sheet was processed into the shape shown in Figures 1 and 2, and then released from the release film. Next, each green sheet was laminated in order so as to correspond to the configuration of the battery element shown in Figures 1 and 2, and then thermocompression bonded by heating to 100°C while applying pressure in the thickness direction. This resulted in a laminate as a battery element precursor.
[0097] (Steps for degreasing and sintering the laminate) The obtained laminate was heated at 300°C for 10 hours to remove the acrylic binder contained in each green sheet, and then the laminate from which the acrylic binder had been removed was heated at 350°C for 10 minutes while applying pressure in the thickness direction under conditions of 20 to 100 MPa, and then cooled in the atmosphere for 1 hour to obtain a sintered laminate.
[0098] (Process for Producing Terminals) Next, a silver plate was attached to the first and second end faces (or side faces) of the laminate, where the positive electrode current collecting layer and the negative electrode current collecting layer were exposed, using a conductive adhesive (thermosetting silver paste), to form positive and negative electrode terminals, thereby producing a solid-state battery.
[0099] In addition, in conjunction with, or in place of, the above-mentioned laminate preparation, degreasing, and sintering processes, multiple green sheets for the solid electrolyte layer punched to a diameter of 16 mm and the above-mentioned green sheet for the negative electrode layer punched to a diameter of 8 mm were laminated on SUS304 (φ16 mm, thickness 0.3 mm). Then, using a muffle furnace KDF P-90 (manufactured by Denken Co., Ltd.), the binder contained in the green sheets was degreased at 300 °C. Using a pressure sintering machine P-5058-00 (manufactured by NPA Systems Co., Ltd.), the degreased sample was heated at 350 °C for 10 minutes while applying pressure in the thickness direction under conditions of 20 to 100 MPa, and then cooled in air for 30 minutes to sinter and obtain a cell element. Then, a 100 μm thick Li foil was punched to a diameter of 10 mm and attached to the cell element to produce the half cell used in this evaluation. In the fabricated cell, the mass ratio of the negative electrode active material to the solid electrolyte was 80:20 due to the removal of the acrylic binder.
[0100] Example 2 In Example 2, in the process of producing a green sheet for a negative electrode material layer in Example 1, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 63:27:10. Except for this, a solid battery was manufactured in the same manner as in Example 1. In the manufactured cell, the mass ratio of the negative electrode active material to the solid electrolyte was 70:30 due to the removal of the acrylic binder.
[0101] Example 3 In Example 3, in the process of producing a green sheet for a negative electrode material layer in Example 1, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 54:36:10. Except for this, a solid battery was manufactured in the same manner as in Example 1. In the manufactured cell, the mass ratio of the negative electrode active material to the solid electrolyte was 60:40 due to the removal of the acrylic binder.
[0102] Example 4 In Example 4, in the process of producing a green sheet for a negative electrode material layer in Example 1, Li 4 Ti5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 45:45:10. Except for this, a solid battery was manufactured in the same manner as in Example 1. In the manufactured cell, the mass ratio of the negative electrode active material to the solid electrolyte became 50:50 due to the removal of the acrylic binder.
[0103] Example 5 In Example 5, in the process of producing a green sheet for a negative electrode material layer in Example 1, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 36:54:10. Except for this, a solid battery was manufactured in the same manner as in Example 1. In the manufactured cell, the mass ratio of the negative electrode active material to the solid electrolyte was 40:60 due to the removal of the acrylic binder.
[0104] Example 6 In Example 6, similarly to Example 3, in the process of producing a green sheet for a negative electrode material layer, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 54:36:10. That is, in the fabricated cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte was 60:40 due to the removal of the acrylic binder. Meanwhile, in Example 6, unlike Example 3, the composition ratio of the Li, B, and Si components, which are the main components of the solid electrolyte, was adjusted. For example, by reducing the content ratio of Si, the true density of the solid electrolyte was increased to 2.2 g / cm. 3 The following was used.
[0105] Example 7 In Example 7, similarly to Example 3, in the process of producing a green sheet for a negative electrode material layer, Li 4 Ti 5 O 12The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 54:36:10. That is, in the fabricated cell, the mass ratio of the negative electrode active material to the solid electrolyte was 60:40 due to the removal of the acrylic binder. On the other hand, in Example 7, unlike Example 3, by adjusting the composition ratio of the Li, B, and Si components that are the main components of the solid electrolyte, for example, by further reducing the Si content, the true density of the solid electrolyte was increased to 2.0 g / cm. 3 The following was used.
[0106] Comparative Example 1 In Comparative Example 1, in the process of producing a green sheet for a negative electrode material layer in Example 1, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 81:9:10. Except for this, a solid battery was manufactured in the same manner as in Example 1. In the manufactured cell, the mass ratio of the negative electrode active material to the solid electrolyte was 90:10 due to the removal of the acrylic binder.
[0107] Comparative Example 2 In Comparative Example 2, in the process of producing a green sheet for a negative electrode material layer in Example 1, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 27:63:10. Except for this, a solid battery was manufactured in the same manner as in Example 1. In the manufactured cell, the mass ratio of the negative electrode active material to the solid electrolyte was 30:70 due to the removal of the acrylic binder.
[0108] Comparative Example 3 In Comparative Example 3, similarly to Example 3, in the process of producing a green sheet for a negative electrode material layer, Li 4 Ti 5 O 12 The negative electrode active material and the solid electrolyte were mixed at a mass ratio of 54:36:10. That is, in the fabricated cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte was 60:40 due to the removal of the acrylic binder. On the other hand, in Comparative Example 3, unlike Example 3, by adjusting the composition ratio of the Li, B, and Si components that are the main components of the solid electrolyte, for example, by further reducing the Si content ratio, the true density of the solid electrolyte was 1.8 g / cm3 The following was used.
[0109] [Measurement Contents] (Measurement of Battery Characteristics) The above half cell was placed in a low-temperature incubator (manufactured by Yamato Scientific Co., Ltd., model number: IQ822), and then a charge / discharge test was performed using a charge / discharge evaluation device (manufactured by Toyo Systems Co., Ltd., model number: TOSCAT-3100). The charge / discharge conditions were as follows. The rated capacity of the cell was 1 C, and it was charged to a predetermined potential at a constant current of 0.05 C (cut-off voltage: 4 V). In addition, it was discharged to a predetermined potential at a constant current of 0.05 C, and after reaching the predetermined potential, it was discharged in a constant voltage mode until the current was reduced to 0.005 C (cut-off voltage: 1.0 V). The charge / discharge capacity of the half cell was confirmed by this charge / discharge test.
[0110] [Measurement Results 1] Table 1 shows the measurement results for Examples 1 to 5 and Comparative Examples 1 and 2. In these Examples and Comparative Examples, the charge capacity was approximately 170 mAh / g. Using this value as a reference, the charge / discharge efficiency was calculated from the ratio of the discharge capacity to the charge capacity. A charge / discharge efficiency of 85% or higher was evaluated as ◯, a charge / discharge efficiency of 95% or higher was evaluated as ⊚, and a charge / discharge efficiency of less than 85% or one for which the discharge capacity could not be measured was evaluated as ×.
[0111]
[0112] As shown in Examples 1 to 5 in Table 1, it was found that in the obtained batteries, when the content ratio (by mass) of the negative electrode active material to the solid electrolyte was 80:20 to 40:60, that is, the content of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte was 20 mass % or more and 60 mass % or less, and the ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material was 0.3 or more and 0.6 or less, the charge-discharge efficiency was 85% or more.
[0113] In particular, when the content ratio of the negative electrode active material to the solid electrolyte is 70:30 to 50:50, that is, when the content of the solid electrolyte is 30% by mass or more and 50% by mass or less with respect to the total amount of the negative electrode active material and the solid electrolyte, it was found that the charge-discharge efficiency is 95% or more. In this case, the density of the negative electrode active material B after preparation is 0.3 g / cm 3 0.5g / cm or more3 It was as follows.
[0114] On the other hand, as shown in Comparative Example 1, when the mass content ratio of the negative electrode active material to the solid electrolyte was 90:10, i.e., the content of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte was 10 mass %, and the porosity in the negative electrode layer was 20.0 volume % or less, a battery could be fabricated, but the discharge capacity could not be measured. From the above, it was found that because the content of the negative electrode active material was high and the content of the solid electrolyte was low, the contact interface between the negative electrode active material and the solid electrolyte could not be made dense, and a conduction path for lithium ions could not be formed.
[0115] Furthermore, as shown in Comparative Example 2, it was found that when the mass content ratio of the negative electrode active material to the solid electrolyte was 30:70, that is, the content of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte was 70 mass%, and the ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material was less than 0.3, the charge-discharge efficiency was less than 85%. From the above, it was found that when the content of the solid electrolyte in the negative electrode layer exceeded 60 mass% and the ratio (B / A) was less than 0.3, the interparticle distance of the negative electrode active material could not be made large enough to form an electron path.
[0116] From the above, it was found that within the range of Examples 1 to 5 described above, the contact interface between the negative electrode active material and the solid electrolyte can be made dense, a conduction path for lithium ions can be suitably formed, and the distance between particles of the negative electrode active material in the negative electrode layer can be made to be a distance that allows the formation of a suitable electron path.
[0117] [Measurement Results 2] Table 2 shows the measurement results for Examples 3, 6, and 7, and Comparative Example 3. In these Examples and Comparative Examples, as in Example 1, the charge capacity was approximately 170 mAh / g, and the charge / discharge efficiency was calculated from the ratio of the discharge capacity to the charge capacity using this value as a reference. A charge / discharge efficiency of 85% or more was evaluated as ◯, a charge / discharge efficiency of 95% or more was evaluated as ⊚, and a charge / discharge efficiency of less than 85% or one for which the discharge capacity could not be measured was evaluated as ×.
[0118]
[0119] As shown in Examples 3, 6, and 7 in Table 2, in the resulting batteries, the content ratio of the negative electrode active material to the solid electrolyte was uniformly 60:40, i.e., the content of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte was uniformly 40% by mass. When the ratio (C / A) of the true density C of the solid electrolyte to the true density A of the negative electrode active material was 0.55 or more and 0.9 or less, the ratio B / A was 0.3 or more and 0.5 or less, and a charge / discharge efficiency of 85% or more was ensured. In particular, as shown in Examples 3 and 6, when the ratio C / A was 0.6 or more and 0.75 or less, the ratio B / A was 0.35 or more and 0.5 or less, and a charge / discharge efficiency of 95% or more was ensured. On the other hand, when the ratio (C / A) was less than 0.55, the ratio B / A was less than 0.3, and a charge / discharge efficiency of less than 85% was ensured.
[0120] From the above, it has been found that when a predetermined amount of solid electrolyte is contained in the negative electrode layer with respect to the total amount of the negative electrode active material and the solid electrolyte, the ratio (C / A) of the true density C of the solid electrolyte to the true density A of the negative electrode active material is also related to the charge / discharge efficiency, i.e., the battery characteristics.
[0121] The present invention may take the following forms. <1> A solid battery including an anode layer including an anode active material containing a Li composite oxide and an oxide glass-based solid electrolyte, wherein the content of the solid electrolyte in the anode layer is 20% by mass or more and 60% by mass or less with respect to the total amount of the anode active material and the solid electrolyte, and a ratio (B / A) of a real density B of the anode active material to a real density A of the anode active material is 0.3 or more and 0.6 or less. <2> The solid battery according to <1>, wherein the content of the solid electrolyte is 30% by mass or more and 50% by mass or less with respect to the total amount of the anode active material and the solid electrolyte. <3> The solid battery according to <1> or <2>, wherein a ratio (C / A) of a real density C of the solid electrolyte to a real density A of the anode active material is 0.55 or more and 0.9 or less. <4> The solid battery according to <3>, wherein when C / A is 0.6 or more and 0.75 or less, B / A is 0.35 or more and 0.5 or less. <5> The true density A of the negative electrode active material is 3.0 g / cm 3 4.0g / cm or more3 <6> The solid state battery according to any one of <1> to <4>, wherein the true density C of the solid electrolyte is 2.0 g / cm or less. 3 3.0g / cm or more 3 The solid state battery according to <3> or <4>, wherein: <7> The solid state battery according to any one of <1> to <6>, wherein the Li composite oxide is an oxide containing Li and a transition metal element. <8> The solid state battery according to <7>, wherein the Li composite oxide is an oxide containing Li and Ti. <9> The solid state battery according to any one of <1> to <8>, wherein the solid electrolyte is lithium borosilicate glass. <10> The solid state battery according to any one of <1> to <9>, further comprising a positive electrode layer, the positive electrode layer comprising a positive electrode active material containing a Li composite oxide and the oxide glass-based solid electrolyte. <11> The solid state battery according to <10>, wherein the Li composite oxide of the positive electrode active material is an oxide containing Li and Co.
[0122] The solid-state battery of the present invention can be used in various fields where power storage is expected. By way of example only, the solid-state battery of the present invention can be used in the electrical, information, and communications fields where mobile devices are used (for example, the electrical and electronic equipment fields or mobile device fields including small electronic devices such as mobile phones, smartphones, laptops, digital cameras, activity monitors, arm computers, electronic paper, RFID tags, card-type electronic money, and smart watches), household and small industrial applications (for example, power tools, golf carts, and household, nursing care, and industrial robots), large industrial applications (for example, forklifts, elevators, and port cranes), transportation systems (for example, hybrid cars, electric cars, buses, trains, electrically assisted bicycles, and electric motorcycles), power system applications (for example, various power generation systems, road conditioners, smart grids, and general-purpose household power storage systems), medical applications (medical devices such as earphone hearing aids), pharmaceutical applications (medical management systems), IoT, and space and deep-sea applications (for example, space probes and submersible research vessels).
[0123] 10: Electrode layer 10A: Positive electrode layer 10B: Negative electrode layer 11: Electrode current collecting layer 11A: Positive electrode current collecting layer 11B: Negative electrode current collecting layer 20: Solid electrolyte layer 30: Electrode separator 30A: Positive electrode separator 30B: Negative electrode separator 40: Terminal 40A: Positive electrode terminal 40B: Negative electrode terminal 60: Outer layer material 100: Solid battery laminate 200: Solid battery
Claims
1. A solid-state battery comprising an anode layer including an anode active material containing a Li composite oxide and an oxide glass-based solid electrolyte, wherein a content of the solid electrolyte relative to a total amount of the anode active material and the solid electrolyte in the anode layer is 20 mass% or more and 60 mass% or less, and a ratio (B / A) of an actual density B of the anode active material to a true density A of the anode active material is 0.3 or more and 0.6 or less.
2. The solid-state battery according to claim 1, wherein the content of the solid electrolyte is 30% by mass or more and 50% by mass or less based on the total amount of the negative electrode active material and the solid electrolyte.
3. The solid-state battery according to claim 1 or 2, wherein a ratio (C / A) of a true density C of the solid electrolyte to a true density A of the negative electrode active material is 0.55 or more and 0.9 or less.
4. The solid-state battery according to claim 3, wherein when the C / A is 0.6 or more and 0.75 or less, the B / A is 0.35 or more and 0.5 or less.
5. The true density A of the negative electrode active material is 3.0 g / cm 3 4.0g / cm or more 3 The solid state battery according to any one of claims 1 to 4, wherein:
6. The true density C of the solid electrolyte is 2.0 g / cm 3 3.0g / cm or more 3 The solid-state battery according to claim 3 or 4, wherein:
7. The solid-state battery according to any one of claims 1 to 6, wherein the Li composite oxide is an oxide containing Li and a transition metal element.
8. The solid-state battery according to claim 7, wherein the Li composite oxide is an oxide containing Li and Ti.
9. The solid-state battery according to any one of claims 1 to 8, wherein the solid electrolyte is lithium borosilicate glass.
10. The solid-state battery according to any one of claims 1 to 9, further comprising a positive electrode layer, the positive electrode layer comprising a positive electrode active material containing a Li composite oxide and the oxide glass-based solid electrolyte.
11. The solid-state battery according to claim 10, wherein the Li composite oxide of the positive electrode active material is an oxide containing Li and Co.
Citation Information
Patent Citations
Lithium battery
JP2001126757A
Lithium ion cell and method for manufacturing same
WO2018123479A1
All-solid-state battery and method for manufacturing same
WO2018131337A1
Solid-state battery
WO2020250981A1
Solid-state battery
WO2022186087A1