Composite magnetic material, dust core, and power choke coil

By coating inorganic insulating particles with amphiphilic molecules, the composite magnetic material achieves improved relative magnetic permeability and withstand voltage, addressing the issue of agglomeration and filling rate in conventional materials.

WO2024202529A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/003457
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-02
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional composite magnetic materials experience a decrease in relative magnetic permeability and withstand voltage when electrically insulating components are added, due to agglomeration of insulating particles, which reduces the filling rate of soft magnetic alloy particles.

Method used

The use of inorganic insulating particles coated with amphiphilic molecules, which have a hydrophobic group with a hydrocarbon chain and a hydrophilic group including a phosphate group, prevents agglomeration and allows for a higher filling rate of iron-based soft magnetic alloy particles, maintaining relative magnetic permeability while improving withstand voltage.

Benefits of technology

The approach enhances both the relative magnetic permeability and withstand voltage of the composite magnetic material, making it suitable for applications in electronic components and power choke coils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024003457_03102024_PF_FP_ABST
    Figure JP2024003457_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This composite magnetic material comprises: iron-based soft magnetic alloy particles; inorganic insulating particles; and a thermosetting resin. The surface of each of the inorganic insulating particles is coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. The hydrophobic group has a hydrocarbon chain, and the hydrophilic group has of a phosphate group and / or a phosphoric acid salt.
Need to check novelty before this filing date? Find Prior Art

Description

Composite magnetic materials, powder magnetic cores, and power choke coils

[0001] The present disclosure relates to a composite magnetic material, a powder magnetic core, and a power choke coil, and more particularly to a composite magnetic material, a powder magnetic core including a cured composite magnetic material, and a power choke coil.

[0002] Patent Document 1 discloses a composite magnetic body containing, for example, a metal magnetic powder and a thermosetting resin, with the metal magnetic powder filling rate being 65% by volume or more and 90% by volume or less. It also describes that this composite magnetic body may further contain an electrically insulating material other than the thermosetting resin, and that the electrically insulating material is in the form of plate-like or needle-like particles.

[0003] Japanese Patent Application Laid-Open No. 2002-305108

[0004] A composite magnetic material according to one embodiment of the present disclosure includes iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. The surfaces of the inorganic insulating particles are coated with amphiphilic molecules having hydrophobic and hydrophilic groups. The hydrophobic groups have hydrocarbon chains. The hydrophilic groups include at least one of phosphate groups and phosphate salts.

[0005] The powder magnetic core of the present disclosure includes a cured product of the composite magnetic material.

[0006] The power choke coil of the present disclosure includes a cured composite magnetic material and a coil conductor, the coil conductor being covered with the cured composite magnetic material.

[0007] The present disclosure has the advantage that the withstand voltage of the composite magnetic material can be improved while suppressing a decrease in the relative permeability.

[0008] FIG. 1 is a schematic cross-sectional view of a compact including a composite magnetic material according to an embodiment. FIG. 2A is a schematic exploded perspective view showing an example of a magnetic element including a powder magnetic core according to an embodiment. FIG. 2B is a schematic perspective view showing an example of a magnetic element including the powder magnetic core in FIG. 2A. FIG. 3A is an X-X cross-sectional view showing an example of a power choke coil according to an embodiment. FIG. 3B is a perspective view showing an outline of the power choke coil according to the embodiment. FIG. 4 is a cross-sectional view showing a modified example of the power choke coil according to the embodiment. FIG. 5 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 2, and Example 1. FIG. 6 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 3, and Example 2. FIG. 7 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 4, Example 3, and Example 4. FIG. 8 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 5, and Example 5. FIG. 9 is a graph showing evaluation results of the composite magnetic material according to an embodiment. FIG. 10 is a graph showing evaluation results of the composite magnetic material according to an embodiment. FIG. 11 is a graph showing evaluation results of the composite magnetic material according to an embodiment.

[0009] 1. Overview One embodiment of the present disclosure will be described below. Note that the following embodiment is merely one of various embodiments of the present disclosure. The following embodiment can be modified in various ways depending on the design as long as the object of the present disclosure can be achieved.

[0010] The composite magnetic material of this embodiment contains iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. The surface of each inorganic insulating particle is coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. The hydrophobic group has a hydrocarbon chain. The hydrophilic group includes at least one of a phosphate group and a phosphate salt.

[0011] According to the composite magnetic material of this embodiment, even if inorganic insulating particles, which are an electrically insulating component, are contained in the composite magnetic material, it is possible to improve the withstand voltage while suppressing a decrease in relative permeability. The reason for this is presumed to be as follows. However, this embodiment is not bound by the explanation of the reason below.

[0012] In the past, when electrically insulating components were blended into a composite magnetic material, the electrically insulating components tended to aggregate in the compact, which reduced the packing density of the soft magnetic alloy particles and the like, resulting in a decrease in the relative magnetic permeability of the compact. Furthermore, aggregation of the electrically insulating components also tended to reduce the withstand voltage. In contrast, the inorganic insulating particles of this embodiment are coated with amphiphilic molecules having both hydrophobic and hydrophilic groups. Specifically, the surface of the inorganic insulating particles is bonded to at least one of the hydrophilic groups, phosphate groups and phosphate salts, through acid-base interactions, resulting in the adsorption of the amphiphilic molecules. Hydrophobic hydrocarbon chains are present on the surface of the inorganic insulating particles opposite the adsorption side (i.e., the side where the hydrophilic groups are adsorbed). This reduces the likelihood of aggregation between the inorganic insulating particles. The fact that the inorganic insulating particles are less likely to aggregate and more easily disperse in the composite magnetic material compact facilitates an increase in the packing density of the iron-based soft magnetic alloy particles in the cured composite magnetic material. Furthermore, it is believed that increasing the filling rate of the iron-based soft magnetic alloy particles leads to a relative increase in the proportion of iron-based soft magnetic alloy particles that have an effect on magnetic force, thereby improving the relative permeability. Furthermore, the inorganic insulating particles coated with amphiphilic molecules are less likely to aggregate with each other in the cured composite magnetic material and are interposed between the iron-based soft magnetic alloy particles. This can increase the electrical resistivity of the cured composite magnetic material. It is believed that this can improve the insulation resistance, i.e., the voltage resistance, of the molded body made from the composite magnetic material.

[0013] The composite magnetic material of the present embodiment can be hardened to form a hardened product, and since it has excellent relative magnetic permeability and voltage resistance as described above, it can be suitably used to produce electronic components such as powder magnetic cores and magnetic elements such as power choke coils.

[0014] 2. Details The composite magnetic material, the powder magnetic core, and the power choke coil according to this embodiment will be described in detail below.

[0015] (1) Composite Magnetic Material As already described, the composite magnetic material of this embodiment contains iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. Details of the components that can be contained in the composite magnetic material will be described.

[0016] (Iron-based soft magnetic alloy particles) The iron-based soft magnetic alloy particles have electrical conductivity and are dispersed in the composite magnetic material.

[0017] The iron-based soft magnetic alloy particles are soft magnetic alloy particles containing iron (Fe) as the main atom. Here, the main atom refers to the atom that has the highest mass ratio in terms of mass among the atoms contained in the soft magnetic alloy particles. For example, it is preferable that the iron atoms account for 50 mass% or more of the mass of all atoms contained in the iron-based soft magnetic alloy particles.

[0018] The iron-based soft magnetic alloy constituting the iron-based soft magnetic alloy particles can be an alloy having an appropriate composition, and may contain, for example, at least one atom selected from the group consisting of silicon (Si), chromium (Cr), and aluminum (Al) as an atom other than iron, although the atoms other than iron are not limited to these.

[0019] Soft magnetic alloy particles are particles of a soft magnetic alloy in particulate form. In the present disclosure, a particulate soft magnetic alloy also includes a powder form. The particulate form of soft magnetic alloy particles can be determined by measuring the particle diameter and confirming whether the particle diameter is 100 μm or less. The average particle diameter of the iron-based soft magnetic alloy particles in the present disclosure refers to the median diameter D50 (50% particle diameter). The average particle diameter of the iron-based soft magnetic alloy particles is obtained by measuring the particle size distribution of the iron-based soft magnetic alloy particles using a laser diffraction / scattering method and calculating the volume-based particle size corresponding to 50% of the integrated value obtained from the particle size distribution. The average particle diameter of the iron-based soft magnetic alloy particles is, for example, 3 μm or more and 40 μm or less. When the average particle diameter of the iron-based soft magnetic alloy particles is within this range, a high filling rate of the iron-based soft magnetic alloy particles in the composite magnetic material compact is easily achieved. Furthermore, when the average particle size of the iron-based soft magnetic alloy particles is 40 μm or less, even when a compact made from the composite magnetic material is used in the high frequency band, loss in the compact (e.g., a magnetic core) can be reduced, and overcurrent loss in particular can be reduced. Furthermore, the iron-based soft magnetic alloy particles can contain alloy particles from multiple particle groups each having a different particle size distribution. In this case, it is easier to increase the filling rate of the iron-based soft magnetic alloy in the compact of the composite magnetic material. As an example, the iron-based soft magnetic alloy particles may include alloy particles (A1) from a particle group having an average particle size of 3 μm or more and 20 μm or less, and alloy particles (A2) from a particle group having an average particle size of 20 μm or more and 40 μm or less. However, the average particle size of the iron-based soft magnetic alloy particles is not limited to the above.

[0020] Specific examples of iron-based soft magnetic alloys include soft magnetic iron-silicon (Fe—Si) alloys, soft magnetic iron-aluminum (Fe—Al) alloys, soft magnetic iron-aluminum-silicon (Fe—Al—Si) alloys, soft magnetic iron-silicon-chromium (Fe—Si—Cr) alloys, soft magnetic iron-chromium (Fe—Cr) alloys, soft magnetic iron-nickel (Fe—Ni) alloys, soft magnetic iron-silicon-boron (Fe—Si—B) alloys, soft magnetic iron-nitrogen (Fe—N) alloys, soft magnetic iron-carbon (Fe—C) alloys, soft magnetic iron-boron (Fe—B) alloys, soft magnetic iron-phosphorus (Fe—P) alloys, permendur (Fe—Co), soft magnetic iron-cobalt-vanadium (Fe—Co—V) alloys, Fe-based amorphous alloys, and Fe-based nanocrystalline alloys.

[0021] The proportion of iron-based soft magnetic alloy particles to the total solid content of the composite magnetic material is preferably 89% by mass or more and 99% by mass or less. At 89% by mass or more, it is possible to prevent a decrease in saturation magnetic flux density when a compact (e.g., a magnetic core) is produced from the composite magnetic material. Furthermore, at 99% by mass or less, it is easy to bond the iron-based soft magnetic alloy particles together, and it is easy to maintain the shape of the magnetic core. In the present disclosure, the total solid content of the composite magnetic material refers to the total amount of components that can be contained in the composite magnetic material, excluding volatile components, such as solvents.

[0022] The iron-based soft magnetic alloy particles can be produced by any suitable method, such as mechanical pulverization, molten metal pulverization, physical pulverization, or chemical pulverization. Examples of mechanical pulverization include stamp milling, ball milling, and hammer milling. Examples of molten metal pulverization include high-pressure water atomization (water atomization), ultra-high-pressure water atomization, gas atomization (gas atomization), rotating electrode pulverization, and vacuum atomization. Examples of physical or chemical pulverization include electrolysis, gas reduction, solid reduction, carbonyl pulverization, hydride decomposition, evaporation condensation, and amalgamation. However, the production method of the iron-based soft magnetic alloy particles is not limited to the above methods. The iron-based soft magnetic alloy particles may be previously surface-treated with an appropriate dispersant, modifier, or the like.

[0023] (Inorganic insulating particles) The inorganic insulating particles have electrical insulating properties. Specifically, the inorganic insulating particles are particles made by granulating an inorganic material having electrical insulating properties. In this embodiment, the surface of the inorganic insulating particles is coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. Note that the inorganic material referred to here does not include the above-mentioned iron-based soft magnetic alloy. In this embodiment, the entire surface of the inorganic insulating particles is coated with amphiphilic molecules.

[0024] An amphiphilic molecule is a compound having a hydrophobic group and a hydrophilic group. In this embodiment, the hydrophobic group has a hydrocarbon chain. The hydrophilic group has at least one of a phosphate group and a phosphate salt. The hydrocarbon chain in the hydrophilic group is a hydrocarbon group in which hydrocarbons are linked in a linear or branched manner. The amphiphilic molecule may further have a group other than the hydrocarbon group as the hydrophobic group, and may further have a group other than a phosphate group or a phosphate salt as the hydrophilic group.

[0025] In this embodiment, the inorganic insulating particles can be present between the iron-based soft magnetic alloy particles in the cured composite magnetic material. That is, the inorganic insulating particles can be present in the cured composite magnetic material in a dispersed state so that the iron-based soft magnetic alloy particles are less likely to come into contact with each other. Therefore, the inorganic insulating particles can contribute to improving the withstand voltage of the cured composite magnetic material.

[0026] In the present disclosure, the term "particulate inorganic insulating particles" also includes powder (powder). Furthermore, the average particle size of inorganic insulating particles in the present disclosure refers to the median diameter D50 (50% particle size), as with iron-based soft magnetic alloy particles. Specifically, the average particle size of inorganic insulating particles is obtained by measuring the particle size distribution of the inorganic insulating particles using a laser diffraction / scattering method and calculating the volume-based particle size corresponding to 50% of the integrated value obtained from the particle size distribution. The average particle size of the inorganic insulating particles is preferably 0.8 μm or more and 4 μm or less. In this case, the relative permeability and withstand voltage of the molded body can be further improved.

[0027] It is preferable that the average particle size of the inorganic insulating particles and the average particle size of the iron-based soft magnetic alloy particles satisfy the following relationship: InsThe average particle diameter D of the iron-based soft magnetic alloy particles Cond Ratio D to Ins / D Cond It is preferable that the relationship of the following formula (1) is satisfied.

[0028] 0.09≦D Ins / D Cond ≦0.5 (1) The ratio D Ins / D Cond If the ratio D is 0.09 or more, the inorganic insulating particles are more likely to penetrate and intervene between the iron-based soft magnetic alloy particles in the cured composite magnetic material, and the packing rate of the iron-based soft magnetic alloy particles is more likely to be increased. Therefore, the relative permeability of the cured composite magnetic material is more likely to be increased. Ins / D Cond If D is 0.5 or less, the withstand voltage can be further improved while maintaining a high filling rate of the iron-based soft magnetic alloy particles in the hardened composite magnetic material. Ins / D Cond is more preferably 0.2 or more.

[0029] In the composite magnetic material, when the volume of the iron-based soft magnetic alloy particles is taken as 100 (volume %), the ratio of the inorganic insulating particles to the total volume of the iron-based soft magnetic alloy particles is preferably 1.3 volume % or more and 4.0 volume % or less. When the ratio of the inorganic insulating particles is within the above range, the filling efficiency of the iron-based soft magnetic alloy particles in the composite magnetic material can be improved. Therefore, the relative permeability of the compact of the composite magnetic material can be further improved, and the withstand voltage can also be further improved.

[0030] The inorganic material constituting the inorganic insulating particles can be an inorganic component having appropriate insulating properties. The inorganic material includes at least one selected from the group consisting of talc (hydrated magnesium silicate), silica (silicon oxide), alumina (aluminum oxide), boron nitride, magnesium oxide, titanium oxide, zirconium oxide, and mica. The boron nitride preferably includes hexagonal boron nitride (h-BN).

[0031] In the present disclosure, inorganic insulating particles whose surfaces are coated with amphiphilic molecules can be produced, for example, as follows: However, the method for producing inorganic insulating particles whose surfaces are coated with amphiphilic molecules is not limited to the method described below.

[0032] A particulate inorganic material having insulating properties as inorganic insulating particles and a dispersant are prepared.

[0033] The dispersant contains the above-mentioned amphipathic molecules. Therefore, the surfaces of the inorganic insulating particles are particularly easily coated with the amphipathic molecules. The dispersant is preferably, for example, a phosphate ester-based dispersant. The phosphate ester-based dispersant has amphipathic molecules, the hydrophobic group has a hydrocarbon chain, and the hydrophilic group has at least one of a phosphate group and a phosphate salt. More specifically, the dispersant is, for example, a phosphate ester-based wetting dispersant.

[0034] Next, the inorganic insulating particles, a dispersant, and, if necessary, a solvent such as an organic solvent are mixed, and the inorganic insulating particles are dispersed in the mixture. In this case, the ratio of the amphiphilic molecules to 100% by mass of the inorganic insulating particles is preferably 10% by mass or more and 100% by mass or less. When the ratio of the amphiphilic molecules is 10% by mass or more, the composite magnetic material molding can maintain a high relative permeability and improve the withstand voltage. Furthermore, when the ratio of the amphiphilic molecules is 100% by mass or less, the surfaces of the inorganic insulating particles can be coated with a sufficient amount of amphiphilic molecules, making it easier to achieve particularly excellent relative permeability and withstand voltage. The ratio of the amphiphilic molecules is more preferably 30% by mass or more. The upper limit of the ratio of the amphiphilic molecules is not particularly limited, and is, for example, 100% by mass.

[0035] This results in inorganic insulating particles coated with amphiphilic molecules.

[0036] (Thermosetting resin) The thermosetting resin functions as a so-called binder (binding agent) in the cured composite magnetic material. That is, the thermosetting resin has the function of binding the iron-based soft magnetic alloy particles together in the cured composite magnetic material. However, in this embodiment, as described above, since inorganic insulating particles are interposed between the iron-based soft magnetic alloy particles in the cured composite magnetic material, the binding is not limited to binding all of the iron-based soft magnetic alloy particles together.

[0037] The thermosetting resin can have electrical insulation properties, and therefore, when the composite magnetic material is cured, the thermosetting resin can penetrate to fill the gaps between the soft magnetic alloy particles, thereby improving the electrical insulation properties of the compact of the composite magnetic material. Furthermore, the thermosetting resin can ensure moldability when the composite magnetic material is molded to produce a cured product.

[0038] Examples of the thermosetting resin include, but are not limited to, epoxy resin, phenol resin, phenoxy resin, silicone resin, polyimide, and organic phosphoric acid compound.

[0039] Examples of epoxy resins include alkylphenol novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; naphthol novolac type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, biphenylene skeleton, or the like; biphenyl aralkyl type epoxy resins; naphthol aralkyl type epoxy resins having a phenylene skeleton, biphenylene skeleton, or the like; polyfunctional epoxy resins such as triphenol methane type epoxy resins and alkyl-modified triphenol methane type epoxy resins; triphenyl methane type epoxy resins; tetrakisphenol ethane type epoxy resins; dicyclopentadiene bisphenol-type epoxy resins such as bisphenol A-type epoxy resins and bisphenol F-type epoxy resins; biphenyl-type epoxy resins; naphthalene-type epoxy resins; alicyclic epoxy resins; bromine-containing epoxy resins such as bisphenol A-type bromine-containing epoxy resins; glycidylamine-type epoxy resins obtained by reacting epichlorohydrin with polyamines such as diaminodiphenylmethane or isocyanuric acid; and glycidyl ester-type epoxy resins obtained by reacting epichlorohydrin with polybasic acids such as phthalic acid or dimer acid.

[0040] The thermosetting resin may be, for example, liquid or solid.

[0041] The composite magnetic material may contain a curable component other than a thermosetting resin, for example, a photocurable component.

[0042] The ratio of the thermosetting resin to the total amount of iron-based soft magnetic alloy particles may be adjusted as appropriate depending on the shape of the composite magnetic material, the type of thermosetting resin, and the properties required for the molded body, but is, for example, 1% by mass to 10% by mass. Within this range, the electrical insulation of the molded body of the composite magnetic material can be easily maintained at a good level.

[0043] The composite magnetic material may contain components other than those described above without departing from the scope of the present disclosure. For example, the composite magnetic material may contain additives as components other than those described above. Examples of additives include modifiers, lubricants, and hardeners.

[0044] The modifier or lubricant can improve the dispersibility of the iron-based soft magnetic alloy particles in the cured composite magnetic material or modify the surface of the iron-based soft magnetic alloy particles. Examples of the modifier include coupling agents and surfactants. Examples of the coupling agent include at least one component selected from the group consisting of silane coupling agents, titanium-based coupling agents, titanium alkoxides, and titanium chelates. Examples of the surfactant include ionic surfactants and nonionic surfactants.

[0045] The lubricant may be, for example, an organic metal soap, and the organic metal soap may be, for example, at least one component selected from the group consisting of zinc stearate, calcium stearate, magnesium stearate, and barium stearate. Note that the modifier and the lubricant are not limited to the above components.

[0046] The curing agent is not particularly limited as long as it is a component capable of curing a thermosetting resin. In the present disclosure, the curing agent also includes a curing accelerator, a curing catalyst, and a curing aid. Specific examples of the curing agent include phenol-based curing agents, acid anhydride-based curing agents, aliphatic amine-based curing agents, aromatic amine-based curing agents, imidazole-based curing accelerators, tertiary amines, and phosphorus compounds.

[0047] (2) Preparation of Composite Magnetic Material and Compact The composite magnetic material of this embodiment can be prepared, for example, as follows.

[0048] First, iron-based soft magnetic alloy particles, inorganic insulating particles coated with amphiphilic molecules on their surfaces (hereinafter sometimes referred to as "coated inorganic insulating particles"), and a thermosetting resin are prepared. The iron-based soft magnetic alloy particles may be previously surface-treated with an appropriate dispersant, modifier, lubricant, etc., as necessary.

[0049] Then, for example, the iron-based soft magnetic alloy particles and the coated inorganic insulating particles are added to a kneadable container and mixed to be dispersed uniformly.

[0050] Next, the iron-based soft magnetic alloy particles and the coated inorganic insulating particles are mixed, and then a thermosetting resin is added, and if necessary, additives, a solvent, etc. are further added, and the mixture is kneaded. When adding the thermosetting resin, the thermosetting resin may be added to the iron-based soft magnetic alloy particles and the coated inorganic insulating particles in a state where it has been dissolved in a solvent in advance. Furthermore, an appropriate kneading device can be used for kneading. The kneading conditions can be adjusted appropriately depending on the type of thermosetting resin, the melting start temperature, etc., but for example, the heating temperature can be set to a temperature lower than the temperature at which the thermosetting resin starts to harden. This results in a composite magnetic material.

[0051] The kneaded composite magnetic material may be dried by heating it at an appropriate temperature. When a solvent such as an organic solvent is added during kneading, it is preferable to dry the composite magnetic material by heating it at a temperature at which the solvent can volatilize.

[0052] The dried composite magnetic material may be pulverized using an appropriate pulverizer or the like to produce a powder of the composite magnetic material. Pulverization may be performed using a stamp mill, a ball mill, a hammer mill, or the like. Furthermore, the composite magnetic material may be pulverized and then further classified to produce a composite magnetic material having an appropriate particle size. The particle size of the composite magnetic material may be, for example, 100 μm or more and 500 μm or less, but is not limited to this.

[0053] As described above, the shape or properties of the composite magnetic material are not particularly limited. When the composite magnetic material is in powder form (powder), it is easy to improve moldability. Therefore, the powder of the composite magnetic material is particularly suitable for use as a material for producing a compact, for example. To produce a compact, first, the powder composite magnetic material is placed in a mold and pressure-molded into an appropriate shape. The pressure conditions can be adjusted as appropriate, but for example, 1 ton / cm 2 More than 10ton / cm 2 It can be more than that.

[0054] Next, the pressure-molded composite magnetic material is heated to harden the thermosetting resin. The heating conditions, such as the heating temperature and heating time, may be adjusted as appropriate depending on the type of thermosetting resin, but the heating temperature is, for example, 150° C. or higher and 300° C. or lower, and the heating time is, for example, 1 minute or higher and 10 hours or lower.

[0055] This results in a cured composite magnetic material. In the present disclosure, the term "molded body of a composite magnetic material" refers to a cured composite magnetic material.

[0056] FIG. 1 shows a schematic cross-sectional view of a compact 1 made from the composite magnetic material of this embodiment. As shown in FIG. 1, the compact 1 contains iron-based soft magnetic alloy particles 2, inorganic insulating particles 3, and a cured thermosetting resin 4. That is, the compact 1 contains the composite magnetic material described above. Furthermore, inorganic insulating particles 3 are interposed between the iron-based soft magnetic alloy particles 2. Furthermore, the surface of each inorganic insulating particle 3 is coated with amphiphilic molecules having a hydrophobic group with a hydrocarbon chain and at least one hydrophilic group selected from a phosphate group and a phosphate salt. Therefore, a compact containing the composite magnetic material can achieve improved voltage resistance while suppressing a decrease in relative permeability.

[0057] (Characteristics of Molded Product and Cured Product) The initial relative permeability of the cured product of the composite magnetic material is the relative permeability when no magnetic field is applied (i.e., magnetic field of 0 kA / m). The initial relative permeability of the composite magnetic material in the present disclosure and the relative permeability when a magnetic field is applied can be measured and calculated by the method described in Example "(2-1) Evaluation 1: Initial Relative Permeability and Relative Permeability" below.

[0058] The withstand voltage of the cured composite magnetic material is preferably 70 V / mm or more. In this case, when the cured composite magnetic material is used as the magnetic core of an inductor component, the leakage current of the magnetic core can be effectively reduced. The withstand voltage of the cured composite material in this disclosure can be measured and calculated by the method described in Example "(2-2) Evaluation 2: Withstand Voltage" below.

[0059] As described above, the composite magnetic material of this embodiment can achieve both improvements in the relative permeability and the withstand voltage of the compact even though it contains an electrically insulating component. Therefore, the composite magnetic material of this embodiment can be suitably used to manufacture magnetic elements and magnetic cores for the magnetic elements by, for example, pressing the material into a desired shape.

[0060] For example, the composite magnetic material can be used to manufacture magnetically responsive electronic components, such as inductor components, which are magnetic elements. Examples of inductor components include inductors, noise filters, reactors, and transformers. Furthermore, applications of the magnetic elements are not particularly limited, but include, for example, noise filter components and impedance matching circuit components. The inductor component includes, for example, a coil-shaped conductor portion and a coating layer that coats the coil-shaped conductor portion. Therefore, an inductor component can be manufactured by using a compact manufactured from the composite magnetic material as the coating layer. In particular, the compact 1 of the composite magnetic material of this embodiment can be suitably used for powder magnetic cores 10, power choke coils 110, and the like. However, this does not mean that the applications of the composite magnetic material are limited to those described above.

[0061] Preferred aspects of the powder magnetic core 10 and power choke coil 110 of this embodiment will be described with reference to the drawings (FIGS. 2A to 4).

[0062] (3) Powder Magnetic Core The powder magnetic core 10 is used in, for example, a magnetic element including a magnetic core. The powder magnetic core 10 is also sometimes called a dust core.

[0063] The powder magnetic core 10 includes a molded body 1 (cured product) of the composite magnetic material described above. The powder magnetic core 10 of this embodiment is a molded body obtained by, for example, pressure-molding the composite magnetic material described above and heating it.

[0064] The shape of the powder magnetic core 10 may be set according to an appropriate shape for use in electronic components such as magnetic elements, and is not particularly limited, but may be, for example, a cylindrical shape, a polygonal prism shape, a toroidal shape, a disk shape, etc.

[0065] Specifically, the powder magnetic core 10 shown as an example in Fig. 2A has a coil conductor portion 20 formed by winding a copper wire so as to have an air core, and is formed with a protrusion 102 passing through the air core of the coil conductor portion 20, and a main body portion 101 that covers the periphery of the wound portion of the coil conductor portion 20. In Fig. 2A, the coil conductor portion 20 is, for example, an edgewise coil formed by winding a rectangular copper wire, but is not limited to this.

[0066] 2A shows an exploded perspective view of a choke coil 100 in which two powder cores 10 (11, 12) having similar shapes sandwich a coil conductor 20 from above and below the air core, with a protrusion 102 arranged so that the coil conductor 20 passes through the air core of the coil conductor 20. That is, the choke coil 100 is produced from the coil conductor 20 and the powder cores 10 (11, 12) (see FIG. 2B). Of the coil conductor 20 sandwiched between the powder cores 11, 12, the tip 200 (first tip 201 and second tip 202) may protrude from each powder core 11, 12 when the powder cores 11, 12 are stacked. However, the first tip 201 and the second tip 202 can serve as terminals (connection terminals) that can be connected to an external circuit. The connection terminals can be produced by stacking the powder cores 11 and 12 with the coil conductor 20 sandwiched between them, and then bending the tip portions 201 and 202 of the coil conductor 20 in opposite directions. 2B , the housing 50 may be formed by stacking the powder cores 11 and 12 with the coil conductor 20 sandwiched between them, and then molding the powder cores 11 and 12 with resin to cover the entire main body 101 of the powder core 10 (11, 12).

[0067] (4) Power Choke Coil A power choke coil is a passive element that stores electrical energy flowing between terminals as magnetic energy. Specifically, the power choke coil 110 includes, for example, a coil conductor 20. The coil conductor 20 has two terminals (a first end 211 and a second end 212) (see FIG. 3A ). The power choke coil 110 can generate magnetic energy by a current flowing between the first terminal 211 and the second terminal 212 in the coil conductor 20. The coil conductor 20 is, for example, an edgewise coil formed by winding a rectangular copper wire.

[0068] As described above, the composite magnetic material can impart high relative permeability and high withstand voltage to the compact 1, and therefore can be suitably used to fabricate the power choke coil 110. The power choke coil 110 of this embodiment includes a hardened composite magnetic material and a coil conductor portion 20. The coil conductor portion 20 is covered with the hardened composite magnetic material. Note that the hardened composite magnetic material is the compact 1 of the composite magnetic material, and therefore may be the above-described powder magnetic core 10.

[0069] While the choke coil 100 shown in FIG. 2B above can be considered a type of power choke coil 110, the power choke coil 110 shown in FIGS. 3A and 3B has a composite magnetic material and a coil conductor 20 integrally molded. Specifically, as shown in the cross-sectional view of FIG. 3A, in the power choke coil 110, the coil conductor 20 is embedded inside the compact 1 by being covered with the composite magnetic material. That is, the choke coil 100 shown in FIGS. 2A and 2B is a coil-assembled magnetic element in which the composite magnetic material compact (powder core 10) and the coil conductor 20 are prepared separately and assembled, whereas the power choke coil 110 shown in FIGS. 3A and 3B can be considered a coil-embedded magnetic element in which the composite magnetic material and the coil conductor 20 are integrally molded to enclose the coil conductor 20.

[0070] As shown in Figures 3A and 3B, the power choke coil 110 has a coil conductor portion 20 with an air core inside the molded body 1, and is applicable to applications where a large current flows and can be made smaller.

[0071] The coil conductor portion 20 has a first end 211 and a second end 212. The first end 211 and the second end 212 are connected to the respective connection terminals 30. Specifically, the first end 211 is connected to the first connection terminal 31, and the second end 212 is connected to the second connection terminal 32. The air-core portion of the coil conductor portion 20 is filled with a hardened product (molded body 1) of the composite magnetic material, and therefore, the part of the coil conductor portion 20 that was air-core can become a magnetic path.

[0072] The connection terminals 30 (first connection terminal 31 and second connection terminal 32) are connected to external electrodes, allowing current to flow through the power choke coil 110. When current flows through the power choke coil 110, a magnetic field is generated, but by including the composite magnetic material compact 1 in the magnetic path, the relative permeability is less likely to decrease, allowing the power choke coil 110 to effectively convert electrical energy into magnetic energy and store the magnetic energy. The power choke coil 110 also has excellent voltage resistance.

[0073] As shown in Figure 3B, the housing 51 may be formed by molding the outer surfaces of the hardened composite magnetic material (molded body 1) and the first end 211 and second end 212 of the coil conductor portion 20 with an appropriate resin.

[0074] (Modification) The power choke coil 110 shown in FIG. 4 is also a coil-buried magnetic element in which a composite magnetic material and a coil conductor portion 20 are integrally molded, similar to FIGS. 3A and 3B . In the power choke coil 110 shown in FIG. 4 , the coil conductor portion 20 is, for example, a coil wire, specifically, a winding coil 20A. In the power choke coil 110, the winding coil 20A and the composite magnetic material are integrally molded. The winding coil 20A has a first end and a second end (not shown), and the first end and the second end of the winding coil 20A are connected to the respective connection terminals 30, allowing current to flow through the power choke coil 110. The power choke coil 110 of this modification also has a low relative permeability and excellent withstand voltage.

[0075] (5) Summary As is clear from the above-described embodiments, the present disclosure includes the following aspects. In the following, reference numerals are given in parentheses only to clarify the correspondence with the embodiments.

[0076] A composite magnetic material according to a first aspect includes iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. The surfaces of the inorganic insulating particles are coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. The hydrophobic group comprises a hydrocarbon chain, and the hydrophilic group comprises at least one of a phosphate group and a phosphate salt.

[0077] According to this aspect, the withstand voltage of the molded body can be improved while preventing the relative magnetic permeability from decreasing.

[0078] The composite magnetic material according to the second aspect is the same as that according to the first aspect, except that the average particle diameter D of the inorganic insulating particles is Ins and the average particle diameter D of the iron-based soft magnetic alloy particles Cond satisfies the relationship of formula (1).

[0079] 0.09≦D Ins / D Cond ≦0.5 (1) According to this embodiment, it is easy to further increase the relative magnetic permeability of the compact, and the withstand voltage can be further improved.

[0080] A composite magnetic material according to a third aspect is the composite magnetic material of the first or second aspect, wherein the inorganic insulating particles have an average particle size of 0.8 μm or more and 4 μm or less.

[0081] According to this embodiment, the relative magnetic permeability and the withstand voltage of the molded body can be further improved.

[0082] The composite magnetic material according to a fourth aspect is any one of the first to third aspects, wherein the volume ratio of the inorganic insulating particles to the total volume of the iron-based soft magnetic alloy particles is 1.3 volume % or more and 4.0 volume % or less.

[0083] According to this embodiment, the molded body can maintain a high relative magnetic permeability, and the withstand voltage can be further improved.

[0084] A composite magnetic material according to a fifth aspect is any one of the first to fourth aspects, wherein the proportion of the amphiphilic molecules relative to the total mass of the inorganic insulating particles is 10 mass % or more and 100 mass % or less.

[0085] According to this aspect, the molded body of the composite magnetic material can maintain a high relative magnetic permeability and improve the withstand voltage. Furthermore, if the proportion of the amphiphilic molecules is 100 mass % or less, the surfaces of the inorganic insulating particles can be coated with a sufficient amount of amphiphilic molecules, making it easy to achieve particularly excellent relative magnetic permeability and withstand voltage.

[0086] A composite magnetic material according to a sixth aspect is any one of the first to fifth aspects, wherein the inorganic insulating particles include coated particles obtained by adding the amphiphilic molecules in a ratio of 10% by mass or more and 100% by mass or less to 100% by mass of the inorganic insulating particles.

[0087] According to this aspect, the molded body of the composite magnetic material can maintain a high relative magnetic permeability and improve the withstand voltage. Furthermore, if the proportion of the amphiphilic molecules is 100 mass % or less, the surfaces of the inorganic insulating particles can be coated with a sufficient amount of amphiphilic molecules, making it easy to achieve particularly excellent relative magnetic permeability and withstand voltage.

[0088] A powder magnetic core (10) according to a seventh aspect includes a cured product of the composite magnetic material according to any one of the first to sixth aspects.

[0089] According to this aspect, a powder magnetic core (10) can be obtained that can achieve both an improvement in withstand voltage while making it difficult for the relative magnetic permeability to decrease.

[0090] A power choke coil (110) according to an eighth aspect includes the cured composite magnetic material of any one of the first to sixth aspects and a coil conductor portion (20). The coil conductor portion (20) is coated with the cured composite magnetic material.

[0091] According to this aspect, a power choke coil (110) can be obtained that can achieve both a reduction in relative permeability and an improvement in withstand voltage.

[0092] EXAMPLES The present disclosure will be specifically described below with reference to examples, although the present disclosure is not limited to the following examples.

[0093] (1) Experiment 1 (Preparation of Composite Magnetic Material) [Comparative Example 1] Fe-Si-Cr metal powder (FeSiCr metal powder) with an average particle diameter D50 of 9 μm was prepared as iron-based soft magnetic alloy particles (hereinafter also referred to as "alloy particles"). 4 mass% of epoxy resin as a thermosetting resin and MEK (methyl ethyl ketone) as an organic solvent were mixed with 100 mass% of the prepared alloy particles. In Comparative Example 1, no inorganic insulating particles were added. After kneading the mixture, the solvent was removed by drying at 50°C for 30 minutes, and a composite magnetic material (dried product) was prepared.

[0094] The dried product was pulverized in a pulverizer and then classified to obtain a powder of a composite magnetic material having a particle size of 100 μm to 500 μm.

[0095] Next, the powder was added to a compression molding die and pressed at a pressure of 2 t / cm 2 The compaction was carried out under the conditions of 1000 to 1500 MPa. For the evaluation described later, a toroidal shaped compact and a disk shaped compact were prepared as quasi-test pieces. Subsequently, each quasi-test piece was heated at 175°C for 3 hours to harden the compacted body, thereby preparing a hardened composite magnetic material. In this way, a toroidal shaped hardened test piece and a disk shaped hardened test piece were obtained. The density of the hardened test piece and the packing ratio (volume %) of the alloy particles are shown in Figure 9 as "density (g / cm)", respectively. 3 "), and "Alloy particle filling rate (volume %)." The density of the hardened test piece was calculated by dividing the mass of the test piece by the volume of the test piece measured with a micrometer. The alloy particle filling rate was calculated from the following formula (2). The same applies below. In the following formula (2), the density of the test piece is expressed as d Mea , the true density of the alloy particles is d Met , the true density of the inorganic insulating particles is d Ins , the true density of the thermosetting resin is d Res , the packing ratio of the alloy particles is a Met , the mass % of inorganic insulating particles is M with respect to 100 mass % of alloy particles in the composite magnetic material. Ins , the mass% of the thermosetting resin is M Res , the mass % of the amphiphilic molecules is M Amp , respectively.

[0096] aMet = d Mea × (100 / d Met ) / (100+M Ins +M Res +M Amp ) × 100 (2) [Example 1, Comparative Example 2] In Example 1, FeSiCr-based metal powder having an average particle size (D50) of 9 μm was prepared as the alloy particles. Furthermore, talc having an average particle size D50 of 2 μm was prepared as the inorganic insulating particles, and 33 mass % of a phosphate ester-based wetting and dispersing agent and an appropriate amount of MEK as an organic solvent were added to 100 mass % of the inorganic insulating particles, followed by stirring to subject the inorganic insulating particles to a surface treatment, thereby preparing coated inorganic insulating particles.

[0097] Next, the alloy particles and the coated inorganic insulating particles were mixed, and then 4% by mass of epoxy resin as a thermosetting resin and MEK as an organic solvent were mixed with 100% by mass of the alloy particles. The mixture was then kneaded and dried at 50°C for 30 minutes to remove the solvent, preparing a composite magnetic material (dried product). The dried product was pulverized in a pulverizer and then classified to obtain a powder of the composite magnetic material having a particle size of 100 μm to 500 μm.

[0098] In Comparative Example 2, the inorganic insulating particles were talc, as in Example 1, but the inorganic insulating particles were not surface-treated. Otherwise, similar to Example 1, the materials were mixed, kneaded, dried, pulverized, and classified to obtain a powder of a composite magnetic material having a particle size of 100 μm to 500 μm.

[0099] Next, the powders of each composite magnetic material of Example 1 and Comparative Example 2 were compression-molded under the same conditions as Comparative Example 1 to produce toroidal-shaped compacts and disk-shaped compacts as quasi-test pieces, and the compacts serving as quasi-test pieces were cured by heating at 175°C for 3 hours. This resulted in toroidal-shaped hardened test pieces and disk-shaped hardened test pieces. The density and alloy particle packing ratio (volume %) of the hardened test pieces are shown in Figure 9.

[0100] [Example 2, Comparative Example 3] In Example 2, a powder of a composite magnetic material was produced under the same conditions as in Example 1, except that the inorganic insulating particles in Example 1 were changed to silica having an average particle diameter D50 of 4 μm, and the amount of phosphate ester-based wetting and dispersing agent used in the surface treatment of the inorganic insulating particles was changed to 35 mass %.

[0101] In Comparative Example 3, powder of a composite magnetic material was produced under the same conditions as in Comparative Example 2, except that the inorganic insulating particles in Comparative Example 2 were changed to silica having an average particle diameter D50 of 4 μm.

[0102] Next, the powders of each composite magnetic material of Example 2 and Comparative Example 3 were compression-molded under the same conditions as Comparative Example 1 to produce toroidal-shaped compacts and disk-shaped compacts as quasi-test pieces, and the compacts serving as quasi-test pieces were cured by heating at 175°C for 3 hours. This resulted in toroidal-shaped hardened test pieces and disk-shaped hardened test pieces. The density and alloy particle packing ratio (volume %) of the hardened test pieces are shown in Figure 9.

[0103] [Examples 3-4, Comparative Example 4] In Example 3, a powder of a composite magnetic material was produced under the same conditions as in Example 1, except that the inorganic insulating particles in Example 1 were changed to alumina having an average particle diameter D50 of 3 μm, and the amount of phosphate ester-based wetting and dispersing agent used in the surface treatment of the inorganic insulating particles was changed to 23 mass %.

[0104] In Example 4, powder of a composite magnetic material was produced under the same conditions as in Example 3, except that the amount of the phosphate ester-based wetting and dispersing agent in Example 3 was changed to 35 mass %.

[0105] In Comparative Example 4, powder of a composite magnetic material was produced under the same conditions as in Comparative Example 2, except that the inorganic insulating particles in Comparative Example 2 were changed to alumina having an average particle diameter D50 of 3 μm.

[0106] Next, the powders of each composite magnetic material of Examples 3-4 and Comparative Example 4 were compression-molded under the same conditions as Comparative Example 1 to produce a toroidal-shaped compact and a disk-shaped compact as quasi-test pieces, and the quasi-test piece compacts were cured by heating at 175°C for 3 hours. As a result, a toroidal-shaped hardened test piece and a disk-shaped hardened test piece were obtained. The density of the hardened test piece and the packing ratio (volume %) of the alloy particles are as shown in Figure 9.

[0107] [Example 5, Comparative Example 5] In Example 5, a powder of a composite magnetic material was produced under the same conditions as in Example 1, except that the inorganic insulating particles in Example 1 were changed to boron nitride (hexagonal boron nitride) having an average particle diameter D50 of 3 μm, and the amount of phosphate ester-based wetting and dispersing agent used in the surface treatment of the inorganic insulating particles was changed to 41 mass %.

[0108] In Comparative Example 5, a powder of a composite magnetic material was produced under the same conditions as in Comparative Example 2, except that the inorganic insulating particles in Comparative Example 2 were changed to boron nitride (hexagonal boron nitride) having an average particle diameter D50 of 3 μm.

[0109] Next, the powders of each composite magnetic material of Example 5 and Comparative Example 5 were compression-molded under the same conditions as Comparative Example 1 to produce a toroidal-shaped compact and a disk-shaped compact as quasi-test pieces, and the quasi-test piece compacts were cured by heating at 175°C for 3 hours. This resulted in a toroidal-shaped hardened test piece and a disk-shaped hardened test piece. The density and alloy particle filling rate (volume %) of the hardened test pieces are shown in Figure 9.

[0110] (2) Evaluation of Experiment 1 (2-1) Evaluation 1: Initial Relative Permeability and Relative Permeability In each Example and Comparative Example, a silver-plated annealed copper wire having a diameter of 0.6 mm and a coating thickness of 0.15 mm was wound 30 times around a test piece of the cured product of a toroidal molded body having dimensions of an outer diameter of 14 mm, an inner diameter of 10 mm, and a thickness of approximately 2 mm, and then connected to an LCR meter, and the inductance was measured at 10 kHz and a current of 0 A. From the obtained results, the relative permeability was calculated based on the following formula (3). In formula (3), L is inductance [H], μ0 is the magnetic permeability in vacuum [H / m], μi is the relative permeability, le is the magnetic path length [m], and Ae is the cross-sectional area [m 2 ] and n indicate the number of turns of the coil, and the words in [ ] indicate units. The calculated values ​​are shown in Figure 9.

[0111] L=(μi)×(μ0)×n 2 × Ae / le (3) Subsequently, in order to measure the inductance when a magnetic field was applied, a DC bias current was applied to the above-mentioned test piece, which was wound with a copper wire under the same conditions, and the inductance was measured at 10 kHz using an LCR meter, in the same manner as for the initial relative permeability.

[0112] The DC current required for the applied magnetic field was calculated based on the following formula (4): In formula (4), Hx is the applied magnetic field [A / m], l e is the magnetic path length [m], Ix is the applied current [A], and n is the number of turns of the coil, and the words in brackets [ ] are units.

[0113] Hx = n / le × Ix (4) Figure 9 shows the relative permeability (also referred to as the initial relative permeability) when no magnetic field is applied (0 kA / m) and the relative permeability when the magnetic field is 12.4 kA / m. Graphs showing the relationship between the applied magnetic field and the relative permeability are shown in Figures 5 to 8. In Figures 5 to 8, the horizontal axis represents the magnetic field [kA / m] and the vertical axis represents the relative permeability. Figure 5 shows the results for Comparative Example 1, Comparative Example 2, and Example 1. Figure 6 shows the results for Comparative Example 1, Comparative Example 3, and Example 2. Figure 7 shows the results for Comparative Example 1, Comparative Example 4, Example 3, and Example 4. Figure 8 shows the results for Comparative Example 1, Comparative Example 5, and Example 5.

[0114] (2-2) Evaluation 2: Withstand Voltage In each example and comparative example, a test piece of a cured disc-shaped molded product having a diameter of 12 mm and a thickness of approximately 1 mm was clamped between probes on both sides near the center, and a DC voltage of 10 V was applied in stages using an ultra-high resistance / microcurrent meter. The discharge time was 1 second, and the charge time was 10 seconds. The withstand voltage was calculated from the "voltage [V] at which the leakage current reached 10 mA or more" obtained in this manner based on the following formula (5). In formula (5), Ex represents the withstand voltage [V / mm], Ez represents the "voltage [V] at which the leakage current reached 10 mA or more," d represents the thickness [mm] of the test piece, and the words in brackets [ ] represent units. The results are shown in the "Withstand voltage (V / mm)" column in Figure 9.

[0115] Ex=(Ez-10) / d (5) As is clear from the above results, when comparing Comparative Example 1, in which no inorganic insulating particles were added, with Comparative Example 2-5, in which inorganic insulating particles that had not been surface-treated were added, it was shown that, as is clear from Figures 5 to 8 and 9, in Comparative Example 2-5, regardless of which inorganic insulating particles were used, the relative permeability was lower than in Comparative Example 1.

[0116] In contrast, when comparing Comparative Example 1, in which no inorganic insulating particles were added, with Example 1-5, in which coated inorganic insulating particles were added, as is clear from Figures 5 to 8 and 9, it was found that, although the filling rate of the alloy particles was reduced in Example 1-5, in which coated inorganic insulating particles were added, a relative permeability comparable to that of Comparative Example 1 was obtained regardless of which inorganic insulating particles were used. Furthermore, it was shown that, compared to Comparative Example 1, Example 1-5 was able to achieve a very high withstand voltage.

[0117] Furthermore, when the same type of inorganic insulating particles were used in Comparative Example 2-5 and Example 1-5, it was shown that a high relative magnetic permeability could be achieved by blending coated inorganic insulating particles.

[0118] Furthermore, in Example 1-5 in which coated inorganic insulating particles were added, it was shown that a high withstand voltage could be achieved by blending coated inorganic insulating particles, compared with inorganic insulating particles of the same type.

[0119] (3) Experiment 2 (Preparation of Composite Magnetic Material) Next, for comparison with Experiment 1 above, the following experiment was carried out.

[0120] [Examples 6-21, Comparative Examples 6-10] In Example 6-21, as shown in Figure 10 or Figure 11, one or more of the "type" of inorganic insulating particles, the average particle diameter "D50 (μm)", the "addition amount (relative to alloy particles (volume %))", and the "addition amount (relative to inorganic insulating particles (mass %))" of the dispersant used to coat the surfaces of the inorganic insulating particles were changed from those in Example 1 described above, and a powder of a composite magnetic material was produced under the same conditions as in Example 1.

[0121] In addition, in Comparative Examples 6-10, as shown in Figure 10 or Figure 11, one or more of the "type" of inorganic insulating particles, the average particle diameter "D50 (μm)", and the "addition amount (relative to alloy particles (volume %))" were changed from those in Comparative Example 2 described above, and powder of the composite magnetic material was produced under the same conditions as in Comparative Example 2.

[0122] Then, for the powder of each composite magnetic material of Example 6-21 and Comparative Example 6-10, the powder was compression-molded under the same conditions as in Comparative Example 1 to produce a toroidal-shaped compact and a disk-shaped compact as quasi-test pieces, and the quasi-test piece compacts were hardened by heating at 175°C for 3 hours to obtain a toroidal-shaped hardened product test piece and a disk-shaped hardened product test piece.

[0123] (4) Evaluation of Experiment 2 Under the same conditions as in "(2-1) Evaluation 1: Initial relative permeability and relative permeability," the inductance was measured for Example 6-21 and Comparative Example 6-10, and the initial relative permeability and relative permeability were calculated. The results are shown in Figures 10 and 11.

[0124] Furthermore, under the same conditions as in the above "Evaluation 2: Withstand voltage", the voltage [V] at the point when the leakage current reached 10 mA or more was measured for Example 6-21 and Comparative Example 6-10, and the withstand voltage was calculated. The results are shown in FIGS. 10 and 11. For comparison, FIGS. 10 and 11 also show the results of Experiment 1 (Example 1-5 and Comparative Example 1-5).

[0125] In Experiment 2, a comparison of Comparative Example 1, in which no inorganic insulating particles were added, and Comparative Example 6-10, in which inorganic insulating particles that had not been surface-treated were added, with Example 6-21, in which coated inorganic insulating particles were added, revealed a similar tendency to that of Experiment 1. That is, it was shown that, regardless of which inorganic insulating particles were used in Example 6-21, a high relative permeability comparable to that of Comparative Example 1 and a withstand voltage much higher than that of Comparative Example 1 could be achieved. Furthermore, when Example 6-22 was compared with Comparative Example 6-10, which used the same type of inorganic insulating particles, it was shown that Example 6-21 had a higher relative permeability and a higher withstand voltage than Comparative Example 6-10.

[0126] REFERENCE SIGNS LIST 1 Molded body 2 Iron-based soft magnetic alloy particles 3 Inorganic insulating particles 4 Cured thermosetting resin 10, 11, 12 Powder core 20 Coil conductor 110 Power choke coil

Claims

1. A composite magnetic material containing iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin, wherein the surface of each of the inorganic insulating particles is coated with amphipathic molecules having a hydrophobic group and a hydrophilic group, the hydrophobic group comprises a hydrocarbon chain, and the hydrophilic group comprises at least one of a phosphate group and a phosphate salt.

2. Average particle diameter D of the inorganic insulating particles Ins and the average particle diameter D of the iron-based soft magnetic alloy particles Cond That is, 0.09≦D Ins / D Cond The composite magnetic material according to claim 1 , which satisfies the relationship: ≦0.

5.

3. The composite magnetic material according to claim 1 or 2, wherein the inorganic insulating particles have an average particle size of 0.8 μm or more and 4 μm or less.

4. The composite magnetic material according to any one of claims 1 to 3, wherein the volume ratio of the inorganic insulating particles to the total volume of the iron-based soft magnetic alloy particles is 1.3 volume % or more and 4.0 volume % or less.

5. A composite magnetic material according to any one of claims 1 to 4, wherein the ratio of the amphiphilic molecules to the total mass of the inorganic insulating particles is 10 mass % or more and 100 mass % or less.

6. The composite magnetic material according to any one of claims 1 to 5, wherein the inorganic insulating particles include coated particles obtained by adding the amphiphilic molecules in a ratio of 10 mass% or more and 100 mass% or less to 100 mass% of the inorganic insulating particles.

7. A dust core comprising a cured product of the composite magnetic material according to any one of claims 1 to 6.

8. A power choke coil comprising: a hardened composite magnetic material according to any one of claims 1 to 6; and a coil conductor portion covered with the hardened composite magnetic material.

Citation Information

Patent Citations

  • Soft magnetic material, powder magnetic core, method for producing soft magnetic material, and method for producing powder magnetic core

    JP2007211340A

  • Soft magnetic powder and inductor

    JP2022060995A

  • Magnetic resin composition, magnetic sheet, and inductor component

    WO2023149454A1