Organopolysiloxane
The organopolysiloxane with a specific formula acts as a wetter to improve the solubility and dispersibility of thermally conductive fillers in phenyl-modified silicones, addressing the challenge of maintaining fluidity and workability in high-filler-content heat dissipation materials, thereby enhancing thermal conductivity.
Patent Information
- Application Number
- PCT/JP2024/004936
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge is to develop a heat dissipation material with high thermal conductivity for electronic components that maintains fluidity and workability, as increasing the filling rate of thermally conductive fillers in silicone-based greases leads to poor fluidity and viscosity issues, particularly with phenyl-modified silicones, where the thermal conductivity of fillers is influenced by their volume fraction exceeding 0.6, and organopolysiloxanes with trialkoxysilyl groups have poor solubility.
An organopolysiloxane with a specific general formula, characterized by monovalent aromatic hydrocarbon and alkyl groups, is used as a wetter to enhance the solubility and dispersibility of thermally conductive fillers in phenyl-modified silicones, maintaining fluidity and suppressing viscosity increases, even with high filler content.
The organopolysiloxane effectively improves the dispersibility and solubility of thermally conductive fillers in phenyl-modified silicones, allowing for higher filler loading without significant viscosity increases, thus enhancing the thermal conductivity of silicone compositions while maintaining their fluidity and workability.
Smart Images

Figure JP2024004936_03102024_PF_FP_ABST
Abstract
Description
organopolysiloxane
[0001] The present invention relates to organopolysiloxanes.
[0002] The performance of electronic components, such as highly integrated circuits like CPUs, is significantly degraded by heat generation during use. To solve this problem, heat-dissipating materials are used, which improve heat transfer efficiency when introduced into the air gap between the heat-generating and cooling components. Silicone heat-dissipating materials, in particular, are used in a wide range of fields due to their high heat resistance, weather resistance, and electrical insulation properties inherent to silicone. In addition, as electronic devices have become increasingly miniaturized and highly integrated in recent years, it is important to more efficiently cool the generated heat, which has led to a demand for heat-dissipating materials with high thermal conductivity.
[0003] The thermal conductivity of materials containing silicone oil and thermally conductive fillers is affected by the thermal conductivity of the thermally conductive filler itself when the volume fraction of the thermally conductive filler exceeds 0.6. Therefore, increasing the thermal conductivity of heat-dissipating materials is crucial. However, simply increasing the filler content significantly reduces the fluidity of the conductive grease, making it difficult to process. To solve this problem, a method has been proposed in which the thermally conductive filler is surface-treated with a silane coupling agent (wetter) to disperse it in the silicone base oil and maintain the fluidity of the thermally conductive grease.
[0004] Phenyl-modified silicones, which have a structure in which some methylsilicones have been replaced with phenyl groups, have better heat resistance, cold resistance, and oxidation resistance than methylsilicones. Furthermore, because they have high gas barrier properties and a high refractive index, phenyl-modified silicones are used in cosmetics, light-emitting diode encapsulants, and other applications (Patent Documents 1 and 2). Therefore, it is believed that using phenyl-modified silicones as base oils and applying them to heat-dissipating materials can achieve properties that cannot be achieved with methylsilicones. On the other hand, the introduction of phenyl groups makes the silicone skeleton rigid, which causes a problem of significantly increased viscosity, particularly in high-phenyl-modified silicones (Patent Document 3).
[0005] Therefore, when a phenyl-modified silicone is used as a base oil and a thermally conductive filler is added to form a grease, the fluidity of the thermally conductive grease is significantly reduced. Furthermore, organopolysiloxanes having trialkoxysilyl groups, which are often used as wetters, have poor solubility in phenyl-modified silicones (Patent Documents 4 and 5). Therefore, there has been a need for the development of a wetter that is highly soluble in phenyl-modified silicones and that can suppress an increase in viscosity when a thermally conductive filler is added.
[0006] Japanese Patent Application Laid-Open No. 2004-162039 Japanese Patent Application Laid-Open No. 2007-039621 Japanese Patent Application Laid-Open No. 2004-262919 Japanese Patent Application Laid-Open No. 2004-262972 Japanese Patent Application Laid-Open No. 2005-162975
[0007] An object of the present invention is to provide a novel organopolysiloxane that acts as a wetter that allows resin materials, particularly phenyl-modified silicones, to be highly loaded with a highly thermally conductive filler.
[0008] In order to achieve the above object, the present invention provides the following novel organopolysiloxane.
[0009] That is, the present invention provides a compound represented by the following general formula (1): (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The siloxane units enclosed in parentheses in the general formula (1) may be bonded in either block or random fashion.
[0010] Such organopolysiloxanes are suitable as wetters, and for example, phenyl-modified silicones can be highly loaded with highly thermally conductive fillers.
[0011] The organopolysiloxane is preferably one represented by the following general formula (2). (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bonding of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bonding of two types of siloxane units enclosed in parentheses with x forms a block polymer.
[0012] Such organopolysiloxanes have high solubility in phenyl-modified silicones.
[0013] R shown in the above general formula (1) and general formula (2) 1 is a phenyl group, and R 2 is preferably a methyl group. From the viewpoint of organopolysiloxane synthesis, these groups are preferred.
[0014] The present invention provides a wetter comprising the organopolysiloxane described above. By using the organopolysiloxane described above in the wetter, it is possible to further disperse the thermally conductive filler in the phenyl-modified silicone.
[0015] The organopolysiloxane of the present invention is useful as a silane coupling agent (wetter) that improves the dispersibility of thermally conductive fillers in phenyl-modified silicones. Therefore, a phenyl-modified silicone composition containing the organopolysiloxane of the present invention has a reduced viscosity and maintains fluidity, even when it contains a large amount of thermally conductive filler. Therefore, when the organopolysiloxane of the present invention is incorporated into a silicone composition, a thermally conductive silicone composition can be obtained in which an increase in viscosity is suppressed, even when the thermally conductive filler is highly loaded.
[0016] The organopolysiloxane synthesized in Example 1 29 This is a Si-NMR chart.
[0017] The present inventors have searched for organopolysiloxanes suitable for wetters that enable resin materials, particularly phenyl-modified silicones, to be highly loaded with highly thermally conductive fillers, and have found that those represented by the following general formula (1) are useful for this purpose, leading to the completion of the present invention. (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The siloxane units enclosed in parentheses in the general formula (1) may be bonded in block or random fashion.) In particular, the organopolysiloxane is characterized by being represented by the following general formula (2): (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer satisfying 1≦x≦30, m' is an integer satisfying 1≦m'≦3, and n' is an integer satisfying 0≦n'≦2, with the proviso that m'+n' is 3. The siloxane units enclosed in parentheses with m' and n' may be bonded in block or random fashion, and the bond between two types of siloxane units enclosed in parentheses with x forms a block polymer.
[0018] The present invention will be described in detail below.
[0019] In the above general formula (1), R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms. 1 Specific examples of include aryl groups such as phenyl, tolyl, xylyl, and mesityl groups, and among these, phenyl is preferred from the viewpoint of ease of synthesis.
[0020] In the above general formula (1), R 2 are independently alkyl groups having 1 to 10 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 3 carbon atoms.2 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a nonyl group, and a decyl group. Among these, a methyl group or an ethyl group is preferred from the viewpoint of ease of synthesis.
[0021] In the above general formula (1), R 3 are independently an alkyl group having 1 to 4 carbon atoms, and are preferably a methyl group or an ethyl group. 3 Examples of a include methyl, ethyl, propyl, isopropyl, butyl, and tert-butyl groups. Of these, methyl and ethyl groups are particularly preferred from the viewpoint of the hydrolysis property of the organopolysiloxane compound of the present invention. In addition, in the above general formula (1), a is 2 or 3, but from the viewpoint of ease of synthesis and economic efficiency, a is preferably 3.
[0022] In the general formula (1), m is typically an integer satisfying the following conditions: 1≦m≦30, preferably 3≦m≦20, and more preferably 5≦m≦18. If m exceeds 30, the viscosity of the organopolysiloxane increases significantly, which is undesirable. Furthermore, in the general formula (1), n is typically an integer satisfying the following conditions: 0≦n≦60, preferably 5≦n≦50, and more preferably 10≦n≦40. Values outside the above range are undesirable because compatibility with the phenyl-modified silicone decreases. Furthermore, m+n satisfies the following conditions: 3≦m+n≦90, and preferably 6≦m+n≦60. Values outside the above range are undesirable because the product becomes difficult to handle during synthesis of this compound. Furthermore, the bonding of the siloxane units enclosed in parentheses in the general formula (1) may be block or random.
[0023] Specific examples of organopolysiloxanes represented by the general formula (1) include, but are not limited to, the following compounds: In the formulas shown below, "Me" represents a methyl group and "Ph" represents a phenyl group.
[0024] The organopolysiloxane represented by the general formula (1) above can be synthesized, for example, according to the following reaction formula.
[0025] Reaction scheme:
[0026] In the formula, m and n are 29 Identified by Si-NMR.
[0027] An organopolysiloxane compound such as that shown in general formula (1) above is synthesized by heating and stirring silanol and 1,1-diphenyl-3,3,5,5-tetramethyltrisiloxane (hereinafter sometimes referred to as phenyl-modified cyclic siloxane) in acetonitrile solvent in the presence of bis(1,2-benzenediolate)phenylsilicate sodium salt (NAS, formula above) as a catalyst, and then reacting with 2-(trimethoxysilyl)ethyl propionate (ECMS, formula above) as a reaction terminator. A polar solvent such as acetonitrile (MeCN) or N,N-dimethylformamide (DMF) is preferred as the solvent for this reaction. The reaction temperature is typically 60 to 65°C, and the reaction time is approximately 2 hours for each step.
[0028] By changing the equivalent weight of the phenyl-modified cyclic siloxane relative to the silanol, the length of the main chain (m+n) of the organopolysiloxane compound, i.e., the degree of polymerization, can be adjusted.
[0029] The resulting organopolysiloxane exhibits high solubility in phenyl-modified silicone.
[0030] The phenyl-modified silicone composition of the present invention containing the organopolysiloxane described above can be highly loaded with thermally conductive fillers while maintaining their dispersibility, and therefore can be suitably used as a wetter.
[0031] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. In the following examples, the kinematic viscosity is a value measured at 25°C using a Canon-Fenske viscometer according to JIS Z8803::2011. The refractive index is a value measured at 25°C using an Abbe refractometer according to JIS K0062:1992. D In the following formula, Me represents a methyl group, and Ph represents a phenyl group.
[0032] [Example 1] A 300 mL round separable flask was equipped with a stirrer, a thermometer, and a coiled condenser through a four-neck separable cover. Trimethylsilanol (9.0 g, 0.1 mol), phenyl-modified cyclic siloxane (103.8 g, 0.3 mol), and acetonitrile (60.8 g) were added to the separable flask, and the mixture was heated and stirred at 65°C to dissolve the phenyl-modified cyclic siloxane. After the phenyl-modified cyclic siloxane was completely dissolved, NAS (61 mg, 0.0178 mmol) was added, and the reaction solution was heated and stirred at 65°C for 2 hours. The progress of the reaction was 1 After tracking with H-NMR spectroscopy and confirming the disappearance of the signal of the phenyl-modified cyclic siloxane, the reaction terminator ECMS (29.1 g, 0.13 mol) was added, and the mixture was heated and stirred at 65°C for an additional 2 hours. After confirming the disappearance of the peak corresponding to silanol by infrared spectroscopy, methanol was added to the reaction solution, and the mixture was heated and stirred at 65°C for an additional 1 hour. The reaction solution was returned to room temperature, washed with methanol, and the oil layer was extracted. The solvent and low molecular weight siloxane contained in the resulting oil layer were removed under reduced pressure to obtain an organopolysiloxane compound. This compound was a colorless, transparent liquid with a kinematic viscosity of 314 mm 2 ・s ―1 The refractive index was 1.505. 29 Si-NMR spectrum analysis revealed that it had the following structure (NMR chart is shown in FIG. 1). 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ = 7.9 (SiMe 3 ), -17.8 to -21.1 (SiMe 2 ), -46.7 to -47.8 (SiPh 2 ), -84.7 to -85.0 (Si(OMe) 3 )
[0033] [Example 2] An organopolysiloxane compound was obtained in the same manner as above, except that 5 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinematic viscosity of 552 mm 2 ・s -1The refractive index was 1.509. 29 Si-NMR spectrum analysis revealed the following structure: 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ = 7.9 (SiMe 3 ), -17.8 to -21.3 (SiMe 2 ), -46.7 to -47.7 (SiPh 2 ), -84.7 to -85.0 (Si(OMe) 3 ).
[0034] [Example 3] An organopolysiloxane compound was obtained in the same manner as above, except that 10 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinematic viscosity of 1255 mm 2 ・s -1 The refractive index was 1.512. 29 Si-NMR spectrum analysis revealed the following structure: 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ = 7.9 (SiMe 3 ), -17.8 to -21.3 (SiMe 2 ), -46.7 to -47.7 (SiPh 2 ), -84.7 to -85.0 (Si(OMe) 3 ).
[0035] Example 4 An organopolysiloxane compound was obtained in the same manner as above, except that 15 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinematic viscosity of 2158 mm 2 ・s -1 The refractive index was 1.515. 29 Si-NMR spectrum analysis revealed the following structure: 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ = 7.9 (SiMe 3), -17.6 to -21.3 (SiMe 2 ), -47.0 to -48.0 (SiPh 2 ), -84.7 to -85.0 (Si(OMe) 3 ).
[0036] [Compatibility Test] When the following organosiloxane (B-6) was dispersed in a phenyl-modified silicone at a concentration of 25%, clouding and layer separation occurred. On the other hand, when the above novel organosiloxane was dispersed under the same conditions, clouding and layer separation did not occur, indicating that the above novel organosiloxane exhibits high compatibility with the phenyl-modified silicone.
[0037] The compositions of Examples 5 to 11 and Comparative Examples 1 to 4 were obtained by mixing components (A) to (C) described below in the composition ratios shown in Tables 1 and 2.
[0038] Example 5 A thermally conductive phenyl-modified silicone composition was obtained by mixing A-1 as component (A), B-1 as component (B), and component (C). Mixing was carried out by placing plastic containers containing weighed-out components (A) to (C) into a rotation-revolution mixer (product name: Awatori Rentaro, manufactured by THINKY Corporation) and mixing at room temperature at 2,000 rpm for 1 minute twice. The resulting mixture was then cooled to room temperature and the viscosity was measured.
[0039] Example 6 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that component (B) was changed from B-1 to B-2, and the viscosity was measured.
[0040] Example 7 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that component (B) was changed from B-1 to B-3, and the viscosity was measured.
[0041] Example 8 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that component (B) was changed from B-1 to B-4, and the viscosity was measured.
[0042] Comparative Example 1 A composition of Comparative Example 1 was prepared in the same manner as in Example 5, except that the component (B) was changed from B-1 to B-5, and the viscosity was measured.
[0043] Comparative Example 2 A composition of Comparative Example 2 was prepared in the same manner as in Example 5, except that the component (B) was changed from B-1 to B-6, and the viscosity was measured.
[0044] Example 9 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that the component (A) was changed from A-1 to A-2 and the component (B) was changed from B-1 to B-2, and the viscosity was measured.
[0045] Example 10 Thermally conductive phenyl-modified silicone compositions were prepared in the same manner as in Example 5, except that the component (A) was changed from A-1 to A-3 and the component (B) was changed from B-1 to B-2, and the viscosity was measured.
[0046] Example 11 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that the component (B) was changed from B-1 to B-2 and the composition and content of the component (C) (C-1 was changed to C-4), and the viscosity was measured.
[0047] Comparative Example 3 A composition of Comparative Example 3 was prepared in the same manner as in Example 5, except that A-2 was added as component (A) in addition to A-1, and component (B) was not added, and the viscosity was measured.
[0048] Comparative Example 4 A composition of Comparative Example 4 was prepared in the same manner as in Example 5, except that the component (B) was not added and the content of the component (C) was changed, and the viscosity was measured.
[0049] (A) Organosiloxane A-1: Represented by the following formula, having a kinematic viscosity of 700 mm 2 ・s -1 Organosiloxane
[0050] A-2: Represented by the following formula, kinematic viscosity is 380 mm 2 ・s -1 Phenyl-modified organosiloxane
[0051] A-3: Represented by the following formula, kinematic viscosity is 2,000 mm 2 ・s -1 Phenyl-modified organosiloxane
[0052] (B) Wetter B-1: Organosiloxane synthesized in Example 1 and represented by the following formula:
[0053] B-2: Organosiloxane synthesized in Example 2, represented by the following formula:
[0054] B-3: Organosiloxane synthesized in Example 3, represented by the following formula:
[0055] B-4: Organosiloxane synthesized in Example 4, represented by the following formula:
[0056] B-5: Organosiloxane of Comparative Example 1 represented by the following formula
[0057] B-6: Organosiloxane represented by the following formula
[0058] (C) Thermally conductive filler C-1: spherical alumina powder (average particle size 45 μm) C-2: spherical alumina powder (average particle size 10 μm) C-3: irregular alumina powder (average particle size 2 μm) C-4: irregular aluminum nitride powder (average particle size 30 μm)
[0059] [Production Method] Components (A) to (C) were mixed as follows to obtain compositions of the composition examples and comparative examples: Plastic containers containing weighed-out components (A) to (C) were placed in a rotation-revolution mixer (product name: Awatori Rentaro, manufactured by THINKY Corporation) in the composition ratios (parts by volume) shown in Table 1, and the mixture was mixed at room temperature at 2,000 rpm for 1 minute twice, and then cooled to room temperature.
[0060] [Test Methods] The properties of the resulting compositions were measured using the following test methods, and the results are shown in the table below.
[0061] [Viscosity Measurement] The obtained composition was measured using a viscosity / viscoelasticity measuring device (trade name: MARS40 (Thermo Fisher Scientific Co., Ltd.)) at a rotation speed of 10 s -1 The viscosity at 23°C was measured using parallel plates with a gap of 0.5 mm.
[0062]
[0063]
[0064] The results in Tables 1 and 2 demonstrate that the phenyl-modified silicone composition containing the organopolysiloxane of the present invention can reduce the viscosity of the composition, allowing for a high loading of thermally conductive filler. In particular, in Example 10, despite the use of high-viscosity A-3 as component A, the viscosity of the composition was lower than in Comparative Example 1. On the other hand, when B-5, which does not fall within the range represented by general formula (2), was used (Comparative Example 1), and in compositions not containing component (B) (Comparative Examples 3 and 4), the viscosity increased. Furthermore, when B-6, which does not contain a phenyl group, was used (Comparative Example 2), the viscosity of the composition did not increase.
[0065] This specification includes the following aspects: [1]: An organopolysiloxane characterized by being represented by the following general formula (1): (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The siloxane units enclosed in parentheses in the general formula (1) may be bonded in block or random fashion.) [2]: The organopolysiloxane of [1], characterized in that the organopolysiloxane is represented by the following general formula (2): (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bonding of the siloxane units enclosed in parentheses in the general formula (2) may be block or random, and the bonding of two types of siloxane units enclosed in parentheses with x is a block polymer.) [3]: In the general formulas (1) and (2), R 1 is a phenyl group, R 2[4]: A wetter comprising the organopolysiloxane according to any one of [1] to [3] above.
[0066] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.
Claims
1. The following general formula (1) (In the formula, R 1 are each independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms; R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonds of the siloxane units enclosed in parentheses in the general formula (1) may be in blocks or random.
2. The organopolysiloxane is represented by the following general formula (2): (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer satisfying 1≦x≦30, m' is an integer satisfying 1≦m'≦3, and n' is an integer satisfying 0≦n'≦2, with the proviso that m'+n' is 3. The bonds of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bonds of the two types of siloxane units enclosed in parentheses with x form a block polymer.
3. The above R 1 is a phenyl group, and the R 2 3. The organopolysiloxane according to claim 1, wherein is a methyl group.
4. A wetter comprising the organopolysiloxane according to claim 1 or 2.
5. A wetter comprising the organopolysiloxane according to claim 3.
Citation Information
Patent Citations
Organopentasiloxane and its production
JP1994009657A
Heat conductive silicone composition
JP2004262972A
Organosilicon compound, method of producing the same, and curable silicone composition comprising the organosilicon compound as adhesiveness-imparting agent
JP2011136962A
Organopolysiloxane having single terminal functional group and method for manufacturing the same
JP2013136662A
Polysiloxane compound and moisture-curable resin composition
JP2013221135A
Cited By
Thermosoftening and thermally-conductive composition having insulation properties