Resin composition for injection molding, injection molded article, and method for producing injection molded article
The resin composition, with specific copolymer ratios, addresses the high viscosity and warpage issues in poly(3-hydroxyalkanoate) resin molding by enhancing impact resistance and bending properties, resulting in improved injection moldability and mechanical strength.
Patent Information
- Application Number
- PCT/JP2024/005105
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-03
AI Technical Summary
Poly(3-hydroxyalkanoate) resin compositions used in injection molding exhibit high viscosity, leading to difficulties in adjusting molding conditions and causing warpage due to residual stress in molded products, while also compromising impact resistance and bending properties.
A resin composition combining copolymers with specific content ratios of 3-hydroxybutyrate units and other hydroxyalkanoate units, including Copolymer (A) with 5-24 mol% content, Copolymer (B) with 24 mol% or more, and Copolymer (C) with 1-5 mol% content, optimized to improve injection moldability and mechanical strength.
The composition achieves excellent impact resistance, bending properties, and injection moldability, reducing the likelihood of warpage and enhancing the mechanical strength of injection molded articles.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Resin composition for injection molding, injection molded article, and method for manufacturing injection molded article
[0001] The present invention relates to a resin composition for injection molding, an injection-molded article, and a method for producing an injection-molded article.
[0002] Large amounts of petroleum-derived plastics are discarded every year, and environmental pollution caused by these large amounts of waste has become a serious problem. In recent years, microplastics have also become a major issue in the marine environment.
[0003] Poly(3-hydroxyalkanoate) resins have excellent biodegradability in soil and seawater, and are materials that can solve environmental problems caused by discarded plastics. For example, the mechanical properties of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), a type of poly(3-hydroxyalkanoate) resin, can be flexibly controlled by changing the composition ratio of 3-hydroxyhexanoate.
[0004] As an injection-molded article containing a poly(3-hydroxyalkanoate)-based resin component, for example, an injection-molded article having good moldability and excellent impact resistance has been proposed, which contains a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the average content of which is 1 mol % to 6 mol %, and a copolymer (B) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the average content of which is 24 mol % or more (see Patent Document 1). However, the poly(3-hydroxyalkanoate)-based resin component used in the production of this proposed injection-molded article has a high viscosity, making it difficult to adjust the conditions during injection molding, and the molded article may be prone to warpage due to residual stress, leaving room for improvement.
[0005] International Publication No. 2022 / 054758
[0006] The present invention aims to solve the above-mentioned problems in the prior art and to achieve the following object: That is, the present invention aims to provide an injection-molding resin composition that can be used to produce injection-molded articles that are excellent in impact resistance and bending properties, and that has excellent injection moldability.
[0007] The means for solving the above problems are as follows: That is, the resin composition for injection molding of the present invention is a resin composition for injection molding containing a poly(3-hydroxyalkanoate)-based resin component, wherein the poly(3-hydroxyalkanoate)-based resin component is a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content of 5 mol% or more and less than 24 mol%, a copolymer (B) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content of 24 mol% or more, and a copolymer (C) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content of 1 mol% or more and less than 5 mol%. and a copolymer (C) having a carboxylate unit, wherein the content of the copolymer (A) is 5 parts by mass or more and 45 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C), the content of the copolymer (B) is 35 parts by mass or more and 55 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C), and the content of the copolymer (C) is 20 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C).
[0008] According to the present invention, the above-mentioned conventional problems can be solved, the above-mentioned object can be achieved, and an injection-molded resin composition can be provided that can produce an injection-molded article that is excellent in impact resistance and bending properties and that is excellent in injection moldability.
[0009] Hereinafter, embodiments of the present invention will be described in detail. Note that the embodiments are not limited by the following description and can be modified as appropriate within the scope of the present invention. Furthermore, in this specification, unless otherwise specified, the term "to" indicating a range of values means that the values before and after it are included as the lower and upper limits.
[0010] (Resin Composition for Injection Molding) The resin composition for injection molding of the present invention contains a poly(3-hydroxyalkanoate)-based resin component, and further contains other components as required.
[0011] <Poly(3-hydroxyalkanoate)-based resin component> The poly(3-hydroxyalkanoate)-based resin component is a mixture of at least three types of poly(3-hydroxyalkanoate)-based resins having different content ratios of constituent monomers, and contains copolymer (A), copolymer (B), and copolymer (C), and further contains other poly(3-hydroxyalkanoate)-based resins as necessary.
[0012] Highly crystalline poly(3-hydroxyalkanoate) resins have excellent injection moldability but poor mechanical strength. On the other hand, low-crystalline poly(3-hydroxyalkanoate) resins have poor injection moldability but excellent mechanical strength. Therefore, by mixing a highly crystalline poly(3-hydroxyalkanoate) resin with a low-crystalline poly(3-hydroxyalkanoate) resin, the highly crystalline poly(3-hydroxyalkanoate) resin forms fine resin crystal layers, and the low-crystalline poly(3-hydroxyalkanoate) resin forms tie molecules that connect the resin crystal layers together, which is expected to improve injection moldability and mechanical strength. However, simply mixing a highly crystalline poly(3-hydroxyalkanoate) resin with a low-crystalline poly(3-hydroxyalkanoate) resin results in a very high viscosity, making it difficult to adjust the injection molding conditions during injection molding to produce an injection-molded article, and residual stress in the molded article can easily cause warpage, leaving room for improvement. The present inventors have therefore discovered that by mixing a highly crystalline poly(3-hydroxyalkanoate) resin with a low-crystalline poly(3-hydroxyalkanoate) resin and a medium-crystalline poly(3-hydroxyalkanoate) resin with a crystallinity between these two, it is possible to produce an injection-molded article that is excellent in injection moldability and has excellent impact resistance and bending properties. Other molding methods, such as inflation molding, typically use high-viscosity resin compositions. However, in the case of injection molding, if the viscosity of the resin composition is high, areas of the mold product shape are insufficiently filled during injection molding, making the molded article more susceptible to warpage.
[0013] In this specification, the term "poly(3-hydroxyalkanoate) resin" refers to a resin containing one or more types of 3-hydroxyalkanoate units as structural units of the polymer. The 3-hydroxyalkanoate units are units represented by the following general formula (1): [-CHR-CH 2 -CO-O-] ... General formula (1)
[0014] In the general formula (1), R is C p H 2p+1 and p is an integer of 1 to 15.
[0015] R in the general formula (1) is C p H 2p+1
[0039] The alkyl group is not particularly limited as long as it is represented by the formula (I) and can be appropriately selected depending on the purpose. Examples thereof include linear or branched alkyl groups such as a methyl group, an ethyl group, a propyl group, a methylpropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, and a hexyl group.
[0016] In the general formula (1), p is not particularly limited as long as it is an integer of 1 to 15, and can be appropriately selected depending on the purpose.
[0017] The poly(3-hydroxyalkanoate) resin is preferably a poly(3-hydroxyalkanoate) resin produced by a microorganism, in which all 3-hydroxyalkanoate units are contained as (R)-3-hydroxyalkanoate units.
[0018] The poly(3-hydroxyalkanoate) resin preferably contains 3-hydroxyalkanoate units, preferably units represented by the general formula (1), in an amount of 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more, based on all structural units. The poly(3-hydroxyalkanoate) resin may contain only one or more types of 3-hydroxyalkanoate units as structural units of the polymer, or may contain one or more types of 3-hydroxyalkanoate units as well as other units (e.g., 4-hydroxyalkanoate units).
[0019] Among these, the poly(3-hydroxyalkanoate) resin is preferably a homopolymer or copolymer containing 3-hydroxybutyrate (hereinafter, sometimes referred to as "3HB") units, more preferably a homopolymer or copolymer in which all of the 3-hydroxybutyrate units are (R)-3-hydroxybutyrate units, and even more preferably a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units.
[0020] Specific examples of poly(3-hydroxyalkanoate) resins include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (hereinafter, sometimes referred to as "P3HB3HV"), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter, sometimes referred to as "P3HB3HH"). Examples of such polyhydroxybutyrates include poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (hereinafter, sometimes referred to as "P3HB4HB"). These may be used alone or in combination of two or more. Among these, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and the like are preferred from the viewpoints of the injection moldability and mechanical properties of injection-molded articles obtained from the resin composition for injection molding.
[0021] When the poly(3-hydroxyalkanoate)-based resin component contains a copolymer of a 3-hydroxyalkanoate unit and another hydroxyalkanoate unit, the average content of the other hydroxyalkanoate units in all the monomer units constituting the poly(3-hydroxyalkanoate)-based resin component is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of productivity of the resin composition for injection molding, however, it is preferably 9 mol % or more and less than 16 mol %, more preferably 10 mol % or more and 15 mol % or less, and even more preferably 11 mol % or more and 14 mol % or less.
[0022] In this specification, the "average content of the other hydroxyalkanoate units in all the monomer units constituting the poly(3-hydroxyalkanoate)-based resin component" means the molar ratio of each monomer unit in all the monomer units constituting the poly(3-hydroxyalkanoate)-based resin component, and when the poly(3-hydroxyalkanoate)-based resin component is a mixture of two or more poly(3-hydroxyalkanoate)-based resins, it means the molar ratio of each monomer unit contained in the entire mixture.
[0023] The average content ratio of the other hydroxyalkanoate units in all the monomer units constituting the poly(3-hydroxyalkanoate)-based resin component can be adjusted by adjusting the blending ratio of the copolymer (A), the copolymer (B), and the copolymer (C).
[0024] <<Copolymer (A)>> The copolymer (A) is a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, in which the average content of the other hydroxyalkanoate units is 5 mol % or more and less than 24 mol %. In this specification, the copolymer (A) refers to the moderately crystalline poly(3-hydroxyalkanoate) resin.
[0025] In this specification, the "average content of other hydroxyalkanoate units" in the copolymer (A) means the molar ratio of the other hydroxyalkanoate units to all monomer units constituting the copolymer (A).
[0026] The average content of the other hydroxyalkanoate units in the copolymer (A) is 5 mol% or more and less than 24 mol%, preferably 5 mol% or more and 22 mol% or less, more preferably 5 mol% or more and 20 mol% or less, and even more preferably 5 mol% or more and 18 mol% or less.
[0027] The other hydroxyalkanoate units in the copolymer (A) are not particularly limited and can be appropriately selected depending on the purpose. Examples include 3-hydroxyhexanoate units, 3-hydroxypropionate units, 3-hydroxyvalerate units, 3-hydroxyheptanoate units, 3-hydroxyoctanoate units, 3-hydroxyoctanoate units, 3-hydroxynanoate units, 3-hydroxydecanoate units, 3-hydroxyundecanoate units, and 4-hydroxybutyrate units. The copolymer (A) may contain only one type of these, or two or more types. Among these, the 3-hydroxyhexanoate unit is preferred as the other hydroxyalkanoate unit in the copolymer (A) from the viewpoint of compatibility with other 3-hydroxyalkanoate resins.
[0028] Specific examples of the copolymer (A) include poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) and poly(3-hydroxybutyrate-co-4-hydroxybutyrate). These may be used alone or in combination of two or more. Among these, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred as the copolymer (A).
[0029] The weight-average molecular weight of the copolymer (A) is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of achieving both the impact resistance and bending elasticity of the injection-molded article and injection moldability, it is preferably 500,000 or less, more preferably 480,000 or less, and even more preferably 450,000 or less. The lower limit of the weight-average molecular weight of the copolymer (A) is also not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of the breaking strength of the material, it is preferably 200,000 or more, more preferably 250,000 or more, and even more preferably 300,000 or more. The upper and lower limits of the weight-average molecular weight of the copolymer (A) can be appropriately combined, but it is preferably 200,000 or more and 500,000 or less, more preferably 250,000 or more and 480,000 or less, and even more preferably 300,000 or more.
[0030] The weight average molecular weight of the copolymer (A) can be adjusted, for example, by lowering the molecular weight by hydrolysis of a high weight average molecular weight product.
[0031] The content of the copolymer (A) is 5 to 45 parts by mass, preferably 5 to 35 parts by mass, and more preferably 5 to 25 parts by mass, per 100 parts by mass of the total mass of the copolymers (A), (B), and (C). If the content of the copolymer (A) is less than 5 parts by mass per 100 parts by mass of the total mass of the copolymers (A), (B), and (C), the viscosity of the injection molding resin composition increases, resulting in poor injection moldability. If the content of the copolymer (A) is more than 45 parts by mass per 100 parts by mass of the total mass of the copolymers (A), (B), and (C), the mechanical strength of the resulting injection-molded article decreases, resulting in poor impact resistance.
[0032] <<Copolymer (B)>> The copolymer (B) is a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, in which the average content of the other hydroxyalkanoate units is 24 mol % or more. In this specification, the copolymer (B) refers to the low-crystalline poly(3-hydroxyalkanoate) resin.
[0033] The copolymer (B) has an average content of the other hydroxyalkanoate units of 24 mol% or more, preferably 24 mol% or more and 99 mol% or less, more preferably 24 mol% or more and 50 mol% or less, even more preferably 24 mol% or more and 35 mol% or less, and particularly preferably 24 mol% or more and 30 mol% or less.
[0034] In this specification, the "average content of other hydroxyalkanoate units" in the copolymer (B) means the molar ratio of the other hydroxyalkanoate units to all monomer units constituting the copolymer (B).
[0035] The other hydroxyalkanoate units in the copolymer (B) are not particularly limited and can be appropriately selected depending on the purpose. Examples include 3-hydroxyhexanoate units, 3-hydroxypropionate units, 3-hydroxyvalerate units, 3-hydroxyheptanoate units, 3-hydroxyoctanoate units, 3-hydroxyoctanoate units, 3-hydroxynanoate units, 3-hydroxydecanoate units, 3-hydroxyundecanoate units, and 4-hydroxybutyrate units. Only one of these may be contained in the copolymer (B), or two or more may be contained. Among these, the 3-hydroxyhexanoate unit is preferred as the other hydroxyalkanoate unit in the copolymer (B) from the viewpoint of compatibility with other 3-hydroxyalkanoate resins.
[0036] Specific examples of the low-crystalline poly(3-hydroxyalkanoate) resin include poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) and poly(3-hydroxybutyrate-co-4-hydroxybutyrate). These may be used alone or in combination of two or more. Among these, the copolymer (B) is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0037] The weight-average molecular weight of the copolymer (B) is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of achieving both the impact resistance and bending elasticity of the injection-molded article and injection moldability, it is preferably 2.5 million or less, more preferably 2.3 million or less, even more preferably 2 million or less, and particularly preferably 1 million or less. The lower limit of the weight-average molecular weight of the copolymer (B) is also not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of material strength, it is preferably 200,000 or more, more preferably 250,000 or more, even more preferably 300,000 or more, and particularly preferably 500,000 or more. The upper and lower limits of the weight-average molecular weight of the copolymer (B) can be appropriately combined, but it is preferably 200,000 or more and 2.5 million or less, more preferably 250,000 or more and 2.3 million or less, even more preferably 300,000 or more and 2 million or less, and particularly preferably 500,000 or more and 1 million or less.
[0038] The weight average molecular weight of the copolymer (B) can be adjusted, for example, by lowering the molecular weight by hydrolysis of a high weight average molecular weight product.
[0039] The content of the copolymer (B) is 35 to 55 parts by mass, preferably 35 to 50 parts by mass, and more preferably 35 to 45 parts by mass, per 100 parts by mass of the total mass of the copolymers (A), (B), and (C). If the content of the copolymer (B) is less than 35 parts by mass per 100 parts by mass of the total mass of the copolymers (A), (B), and (C), the mechanical strength of the resulting injection-molded article will be reduced, resulting in poor impact resistance. On the other hand, if the content of the copolymer (B) is more than 55 parts by mass per 100 parts by mass of the total mass of the copolymers (A), (B), and (C), the viscosity of the injection-molding resin composition will increase, resulting in poor injection moldability.
[0040] <<Copolymer (C)>> The copolymer (C) is a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, in which the average content of the other hydroxyalkanoate units is 1 mol % or more and less than 5 mol %. In this specification, the copolymer (C) refers to the highly crystalline poly(3-hydroxyalkanoate) resin.
[0041] The copolymer (C) has an average content of the other hydroxyalkanoate units of 1 mol % or more and less than 5 mol %, preferably 2 mol % or more and 4 mol % or less.
[0042] In this specification, the "average content of other hydroxyalkanoate units" in the copolymer (C) means the molar ratio of the other hydroxyalkanoate units to all monomer units constituting the copolymer (C).
[0043] The other hydroxyalkanoate units in the copolymer (C) are not particularly limited and can be appropriately selected depending on the purpose. Examples include 3-hydroxyhexanoate units, 3-hydroxypropionate units, 3-hydroxyvalerate units, 3-hydroxyheptanoate units, 3-hydroxyoctanoate units, 3-hydroxyoctanoate units, 3-hydroxynanoate units, 3-hydroxydecanoate units, 3-hydroxyundecanoate units, and 4-hydroxybutyrate units. Only one of these may be contained in the copolymer (C), or two or more may be contained. Among these, the 3-hydroxyhexanoate unit is preferred as the other hydroxyalkanoate unit in the copolymer (C) from the viewpoint of compatibility with other 3-hydroxyalkanoate resins.
[0044] Specific examples of the copolymer (C) include poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) and poly(3-hydroxybutyrate-co-4-hydroxybutyrate). These may be used alone or in combination of two or more. Among these, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred as the copolymer (C).
[0045] The weight-average molecular weight of the copolymer (C) is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of achieving both the impact resistance and bending elasticity of the injection-molded article and injection moldability, it is preferably 1,000,000 or less, more preferably 800,000 or less, and even more preferably 700,000 or less. The lower limit of the weight-average molecular weight of the copolymer (C) is also not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of material strength, it is preferably 200,000 or more, more preferably 250,000 or more, and even more preferably 500,000 or more. The upper and lower limits of the weight-average molecular weight of the copolymer (C) can be appropriately combined, but it is preferably 200,000 or more to 1,000,000 or less, more preferably 250,000 or more to 800,000 or less, and even more preferably 500,000 or more to 700,000 or less.
[0046] The weight average molecular weight of the copolymer (C) can be adjusted, for example, by lowering the molecular weight by hydrolysis of a high weight average molecular weight product.
[0047] The content of the copolymer (C) is 20 parts by mass or more and 50 parts by mass or less, preferably 25 parts by mass or more and 45 parts by mass or less, and more preferably 30 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C). If the content of the copolymer (C) is less than 20 parts by mass relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C), the flexural modulus becomes low and the injection moldability becomes poor. On the other hand, if the content of the copolymer (C) is more than 50 parts by mass relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C), the impact resistance becomes poor.
[0048] <<Other Poly(3-hydroxyalkanoate)-Based Resins>> The other poly(3-hydroxyalkanoate)-based resins other than the copolymers (A), (B), and (C) are not particularly limited as long as they do not impair the effects of the present invention and can be appropriately selected depending on the purpose. Examples include homopolymers consisting of only 3-hydroxyalkanoate units, copolymers of 3-hydroxyalkanoate units other than 3-hydroxybutyrate and the other hydroxyalkanoate units, and copolymers of 3-hydroxybutyrate units and the other hydroxyalkanoate units, the average content of the other hydroxyalkanoate units of which differs from that of the copolymers (A), (B), and (C). These may be used alone or in combination of two or more.
[0049] The content of the other poly(3-hydroxyalkanoate) resin is not particularly limited as long as it does not impair the effects of the present invention, and can be appropriately selected depending on the purpose.
[0050] The average content of each monomer unit relative to all monomer units constituting the poly(3-hydroxyalkanoate)-based resin component can be determined by methods known to those skilled in the art, for example, the method described in paragraph
[0047] of WO 2013 / 147139. Specifically, 2 mL of a sulfuric acid-methanol mixed solution (volume ratio of sulfuric acid:methanol = 15:85) and 2 mL of chloroform are added to 20 mg of the dried poly(3-hydroxyalkanoate)-based resin component, the mixture is sealed, and heated at 100°C for 140 minutes to obtain a methyl ester of a decomposition product of the poly(3-hydroxyalkanoate)-based resin component. After cooling, 1.5 g of sodium bicarbonate is added little by little to neutralize the mixture, and the mixture is allowed to stand until the evolution of carbon dioxide gas ceases. 4 mL of diisopropyl ether is added and mixed thoroughly, followed by centrifugation, and the monomer unit composition of the polyester decomposition product in the supernatant is analyzed by capillary gas chromatography. The gas chromatograph may be, for example, a GC-17A (manufactured by Shimadzu Corporation), and the capillary column may be, for example, a NEUTRA BOND-1 (column length: 25 m, column inner diameter: 0.25 mm, liquid film thickness: 0.4 μm, manufactured by GL Sciences Co., Ltd.). He is used as the carrier gas, the column inlet pressure is 100 kPa, and 1 μL of sample is injected. The temperature conditions are as follows: the initial temperature is raised from 100°C to 200°C at a rate of 8°C / min, and then further raised from 200°C to 290°C at a rate of 30°C / min.
[0051] The weight-average molecular weight of the poly(3-hydroxyalkanoate) resin component as a whole is not particularly limited and can be selected appropriately depending on the purpose. From the viewpoint of achieving both the impact resistance and flexural modulus of the injection-molded article and injection moldability, it is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. The lower limit of the weight-average molecular weight of the poly(3-hydroxyalkanoate) resin component as a whole is also not particularly limited and can be selected appropriately depending on the purpose. From the viewpoint of material strength, it is preferably 200,000 or more, more preferably 250,000 or more, and even more preferably 300,000 or more. The upper and lower limits of the weight-average molecular weight of the poly(3-hydroxyalkanoate) resin component as a whole can be combined appropriately, but is preferably 200,000 or more and 2,000,000 or less, more preferably 250,000 or more and 1,500,000 or less, and even more preferably 300,000 or more.
[0052] In this specification, the weight-average molecular weight of Copolymer (A), Copolymer (B), Copolymer (C), or the poly(3-hydroxyalkanoate)-based resin component can be measured in terms of polystyrene using gel permeation chromatography (GPC) with a chloroform solution. A column suitable for measuring weight-average molecular weights can be used as the column in the gel permeation chromatography. A specific example is a method in which the weight-average molecular weight is measured in terms of polystyrene standards using a gel permeation chromatography system (e.g., Shodex (registered trademark) GPC-101, manufactured by Showa Denko K.K.) with two columns (e.g., Shodex (registered trademark) KM-806M, manufactured by Showa Denko K.K.) connected together, using chloroform as the mobile phase.
[0053] The poly(3-hydroxyalkanoate)-based resin component is preferably one that has not been crosslinked using a crosslinking agent such as an organic peroxide, i.e., the poly(3-hydroxyalkanoate)-based resin component is preferably a resin component that does not have a crosslinked structure.
[0054] -Method for producing poly(3-hydroxyalkanoate)-based resin- The method for producing the poly(3-hydroxyalkanoate)-based resin is not particularly limited and can be appropriately selected depending on the purpose, and may be a production method by chemical synthesis or a production method using a microorganism. Among these, as the method for producing the poly(3-hydroxyalkanoate)-based resin, the production method using a microorganism is preferred because it allows efficient production of a poly(3-hydroxyalkanoate)-based resin having an (R)-3-hydroxyalkanoate unit.
[0055] The poly(3-hydroxyalkanoate) resin can be produced by any known method using a microorganism. For example, the following microorganisms are known to produce copolymers of 3-hydroxybutyrate and other hydroxyalkanoates: Examples of producing bacteria for poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (P3HB3HV) and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) include Aeromonas caviae and Cupriavidus necator into which genes for P3HA synthases have been introduced (see T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997), WO 2019 / 142845, and JP 57-150393 A). Known examples of bacteria that produce poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4HB) include Alcaligenes eutrophus. Among these, as a producer of P3HB3HH, in order to improve the productivity of P3HB3HH, Alcaligenes eutrophus AC32 strain (Alcaligenes eutrophus AC32, FERM BP-6038) into which the genes of the P3HA synthase group have been introduced (see T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997)), Cupriavidus necator into which the genes of the P3HA synthase group have been introduced (see WO 2019 / 142845) is preferred.
[0056] In producing a poly(3-hydroxyalkanoate) resin, microbial cells obtained by culturing these microorganisms under appropriate conditions and accumulating a poly(3-hydroxyalkanoate) resin such as P3HB3HH within the cells can be used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxyalkanoate) resin synthesis-related genes have been introduced may be used depending on the poly(3-hydroxyalkanoate) resin to be produced, or the culture conditions, including the type of substrate, may be optimized.
[0057] The method for obtaining a mixture of three or more poly(3-hydroxyalkanoate) resins, including the copolymer (A), the copolymer (B), and the copolymer (C), and, if necessary, the other poly(3-hydroxyalkanoate) resin, is not particularly limited and can be appropriately selected depending on the purpose. The method may be a method for obtaining the mixture using a microorganism, or a method for obtaining the mixture by chemical synthesis. Alternatively, the mixture may be obtained by melt-kneading three or more resins using an extruder, kneader, Banbury mixer, roll, or the like, or by dissolving three or more resins in a solvent, mixing, and drying the resins.
[0058] <Other Components> The other components in the resin composition for injection molding are not particularly limited as long as they do not impair the effects of the present invention and can be appropriately selected depending on the purpose, and examples thereof include other resins other than the poly(3-hydroxyalkanoate)-based resin component, inorganic fillers, various other additives, etc. These may be used alone or in combination of two or more.
[0059] <<Other Resins>> The other resins are not particularly limited as long as they do not impair the effects of the present invention, and examples thereof include aliphatic polyester-based resins such as polybutylene succinate adipate, polybutylene succinate, polycaprolactone, and polylactic acid; and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate, polybutylene sebacate terephthalate, and polybutylene azelate terephthalate. These may be used alone or in combination of two or more.
[0060] The content of the other resin in the resin composition for injection molding is not particularly limited as long as it does not impair the effects of the present invention and can be appropriately selected depending on the purpose, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the total of the poly(3-hydroxyalkanoate)-based resin components. The lower limit of the content of the other resin is not particularly limited, and may be 0 parts by mass.
[0061] <<Inorganic Filler>> The resin composition for use in injection molding may contain an inorganic filler from the viewpoint of improving the mechanical strength of the injection-molded article to be obtained.
[0062] The inorganic filler is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include silica-based inorganic fillers, alumina, zircon, iron oxide, zinc oxide, titanium oxide, silicon nitride, boron nitride, aluminum nitride, silicon carbide, glass, silicone rubber, silicone resin, titanium oxide, carbon fiber, mica, graphite, carbon black, ferrite, graphite, diatomaceous earth, clay, talc, calcium carbonate, manganese carbonate, magnesium carbonate, barium sulfate, and silver powder. Examples of silica-based inorganic fillers include quartz, fumed silica, silicic acid anhydride, fused silica, crystalline silica, amorphous silica, fillers formed by condensing alkoxysilanes, and ultrafine amorphous silica. These inorganic fillers may be used alone or in combination of two or more.
[0063] Among these, silica-based inorganic fillers are preferred because they can improve the mechanical properties of injection-molded articles obtained from the injection-molding resin composition. The type of silica-based inorganic filler is not particularly limited, and from the viewpoint of versatility, examples include synthetic amorphous silica produced by a dry method or a wet method. Furthermore, either hydrophobic or non-hydrophobic treated fillers can be used. These may be used alone or in combination of two or more.
[0064] The inorganic filler may be surface-treated to improve dispersibility in the resin material. The treating agent used for the surface treatment is not particularly limited and can be appropriately selected from known treating agents, such as higher fatty acids, silane coupling agents, titanate coupling agents, sol-gel coating agents, and resin coating agents. These may be used alone or in combination of two or more.
[0065] The water content of the inorganic filler is not particularly limited and can be appropriately selected from known treatment agents, but from the viewpoint of easily suppressing hydrolysis of the poly(3-hydroxyalkanoate)-based resin, it is preferably 0.01% by mass to 10% by mass, more preferably 0.01% by mass to 5% by mass, and even more preferably 0.01% by mass to 1% by mass. The water content of the inorganic filler can be determined in accordance with JIS-K5101-15-1:2004 (Testing methods for pigments - Part 15: Loss on heating).
[0066] The volume average particle diameter of the inorganic filler is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 μm to 100 μm, more preferably 0.1 μm to 50 μm, from the viewpoint of excellent mechanical properties and injection moldability of an injection-molded article obtained from the resin composition for injection molding. The volume average particle diameter of the inorganic filler can be measured using a laser diffraction / scattering device (for example, Microtrac MT3100II, manufactured by Nikkiso Co., Ltd.).
[0067] The content of the inorganic filler in the resin composition for injection molding is not particularly limited as long as the effects of the present invention are not impaired and can be appropriately selected depending on the purpose, but is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, and even more preferably 30 parts by mass or less, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin component. Although the inorganic filler does not need to be blended into the resin composition for injection molding, blending the inorganic filler has the advantage of improving the strength of the injection-molded article obtained from the resin composition for injection molding. Therefore, the lower limit of the content of the inorganic filler in the resin composition for injection molding is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin component. The upper and lower limits of the content of the inorganic filler in the resin composition for injection molding can be appropriately combined, but is preferably 1 part by mass or more and 40 parts by mass or less, more preferably 5 parts by mass or more and 35 parts by mass or less, and even more preferably 10 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin component.
[0068] For the purpose of improving the dispersibility of the silica, it is preferable to use a dispersing aid in combination with the silica.
[0069] The dispersing aid is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include glycerin ester compounds, adipate ester compounds, polyether ester compounds, phthalate ester compounds, isosorbide ester compounds, and polycaprolactone compounds. These may be used alone or in combination of two or more. Among these, modified glycerin compounds such as glycerin diacetomonolaurate, glycerin diacetomonocaprylate, and glycerin diacetomonodecanoate are preferred because they have excellent affinity with poly(3-hydroxyalkanoate) resin components and are less likely to bleed; adipate compounds such as diethylhexyl adipate, dioctyl adipate, and diisononyl adipate; and polyether ester compounds such as polyethylene glycol dibenzoate, polyethylene glycol dicaprylate, and polyethylene glycol diisostearate. Dispersing aids containing a large amount of biomass-derived components are even more preferred because they can increase the biomass content of the entire injection-molding resin composition.
[0070] Examples of such dispersing aids include the "Rikemal" (registered trademark) PL series from Riken Vitamin Co., Ltd. and the Polysorb series from Roquette.
[0071] The content of the dispersing aid in the resin composition for use in injection molding is not particularly limited as long as the effects of the present invention are not impaired, and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass to 20 parts by mass per 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin components in total. The dispersing aid does not necessarily have to be blended into the resin composition for use in injection molding.
[0072] <<Additives>> Examples of the additives include nucleating agents, lubricants, plasticizers, antistatic agents, flame retardants, conductive agents, heat insulating agents, crosslinking agents, antioxidants, ultraviolet absorbers, colorants, inorganic fillers, organic fillers, and hydrolysis inhibitors. These may be used alone or in combination of two or more. Among these, biodegradable additives are preferred as the additives.
[0073] -Crystal Nucleating Agent- The crystal nucleating agent is not particularly limited as long as it does not impair the effects of the present invention and can be appropriately selected depending on the purpose. Examples include pentaerythritol, orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, boron nitride, etc. These may be used alone or in combination of two or more. Among these, pentaerythritol is preferred as the crystal nucleating agent because it is particularly effective in promoting the crystallization of the poly(3-hydroxyalkanoate) resin component.
[0074] The content of the crystal nucleating agent in the resin composition for injection molding is not particularly limited as long as the effects of the present invention are not impaired, and can be appropriately selected depending on the purpose. However, the content is preferably 0.1 parts by mass to 5 parts by mass, more preferably 0.5 parts by mass to 3 parts by mass, and even more preferably 0.7 parts by mass to 1.5 parts by mass, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin components in total.
[0075] -Lubricant- The lubricant is not particularly limited as long as it does not impair the effects of the present invention and can be appropriately selected depending on the purpose. Examples include behenamide, oleamide, erucamide, stearamide, palmitamide, N-stearylbehenamide, N-stearylerucamide, ethylenebisstearamide, ethylenebisoleamide, ethylenebiserucamide, ethylenebislauricamide, ethylenebiscapricamide, p-phenylenebisstearamide, and polycondensates of ethylenediamine, stearic acid, and sebacic acid. These may be used alone or in combination of two or more. Among these, behenamide and erucamide are preferred as the lubricant because they have particularly excellent lubricating effect on the poly(3-hydroxyalkanoate)-based resin component.
[0076] The content of the lubricant in the resin composition for injection molding is not particularly limited as long as the effects of the present invention are not impaired, and can be appropriately selected depending on the purpose. However, the content is preferably 0.01 parts by mass to 5 parts by mass, more preferably 0.05 parts by mass to 3 parts by mass, and even more preferably 0.1 parts by mass to 1.5 parts by mass, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin components in total.
[0077] -Plasticizer- The plasticizer is not particularly limited as long as it does not impair the effects of the present invention and can be appropriately selected depending on the purpose. Examples include glycerin ester compounds, citrate ester compounds, sebacic acid ester compounds, adipate ester compounds, polyether ester compounds, benzoic acid ester compounds, phthalic acid ester compounds, isosorbide ester compounds, polycaprolactone compounds, and dibasic acid ester compounds. These may be used alone or in combination of two or more. Among these, glycerin ester compounds, citrate ester compounds, sebacic acid ester compounds, and dibasic acid ester compounds are preferred as the plasticizer because they have a particularly excellent plasticizing effect on the poly(3-hydroxyalkanoate) resin component.
[0078] The glycerin ester compound is not particularly limited, and examples thereof include glycerin diacetomonolaurate. The citrate ester compound is not particularly limited, and examples thereof include acetyl tributyl citrate. The sebacic acid ester compound is not particularly limited, and examples thereof include dibutyl sebacate. The dibasic acid ester compound is not particularly limited, and examples thereof include benzyl methyl diethylene glycol adipate.
[0079] The content of the plasticizer in the resin composition for injection molding is not particularly limited as long as the effects of the present invention are not impaired, and can be appropriately selected depending on the purpose. However, the content is preferably 1 part by mass to 20 parts by mass, more preferably 2 parts by mass to 15 parts by mass, and even more preferably 3 parts by mass to 10 parts by mass, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin components in total.
[0080] [Melt Viscosity] The melt viscosity of the resin composition for injection molding is not particularly limited and can be appropriately selected depending on the purpose, but the melt viscosity measured at 165°C and a shear rate of 608 / s is preferably 400 Pa s or more and 500 Pa s or less, more preferably 410 Pa s or more and 480 Pa s or less, and even more preferably 420 Pa s or more and 470 Pa s or less. When the melt viscosity of the resin composition for injection molding is 400 Pa s or more, it is easy to reduce flash during molding, and when it is 500 Pa s or less, injection moldability is improved.
[0081] Specifically, the melt viscosity of the resin composition for injection molding is measured by the following method: A capillograph (for example, 1D PMD-C, manufactured by Toyo Seiki Seisaku-sho, Ltd.) equipped with an orifice having a diameter of 1 mm, a length of 10 mm, and an inlet angle of 45° and heated to 165°C is filled with 15 g of the resin composition for injection molding, and after preheating for 5 minutes, the piston is lowered at a rate of 50 mm / min (shear rate of 608 / s), and the melt viscosity at a shear rate of 608 / s is calculated from the stress applied to the piston when the molten resin is extruded through the orifice.
[0082] The resin composition for injection molding of the present invention can be used to produce injection-molded articles that are excellent in impact resistance and bending properties, and has excellent injection moldability, so it is preferably used for producing injection-molded articles, and particularly preferably used for the method for producing injection-molded articles of the present invention described below.
[0083] (Injection Molded Article) An injection molded article according to one embodiment of the present invention contains the resin composition for injection molding of the present invention. An injection molded article according to another embodiment of the present invention is an injection molded article containing a poly(3-hydroxyalkanoate)-based resin component, and has a Charpy impact strength of 10 kJ / m 2 or more, and the flexural modulus is 520 MPa or more. Hereinafter, when an injection molded article according to one embodiment of the present invention and an injection molded article according to another embodiment of the present invention are described without distinction, they may be simply referred to as "injection molded article." The injection molded article of the present invention is excellent in impact resistance and flexural properties.
[0084] <Injection-molded article according to one embodiment> The injection-molded article according to one embodiment contains the resin composition for use in injection molding of the present invention and may further contain other components as necessary. Note that the injection-molded article according to the one embodiment may be made of the resin composition for use in injection molding of the present invention.
[0085] The impact resistance and flexural modulus of the injection-molded article according to the one embodiment are not particularly limited and can be appropriately selected depending on the properties of the resin composition for injection molding. However, it is preferable that the impact resistance and flexural modulus are in the same numerical range as those of the injection-molded article according to another embodiment described below.
[0086] <Injection-molded article according to another embodiment> An injection-molded article according to another embodiment of the present invention is an injection-molded article containing a poly(3-hydroxyalkanoate)-based resin component, and has a Charpy impact strength of 10 kJ / m 2 or more, and the flexural modulus is 520 MPa or more.
[0087] <<Poly(3-hydroxyalkanoate)-based resin component>> The poly(3-hydroxyalkanoate)-based resin component is not particularly limited and can be appropriately selected depending on the purpose, but suitable examples include those described in the section <Poly(3-hydroxyalkanoate)-based resin component> in the above (Resin composition for injection molding).
[0088] [Charpy impact resistance strength] The injection molded article according to the another embodiment has a Charpy impact resistance strength of 10 kJ / m 2 Above 25 kJ / m 2 More than 30 kJ / m is preferable. 2 The higher the Charpy impact strength of the injection molded article according to the another embodiment, the better. Therefore, there is no particular limitation on the upper limit, and it can be appropriately selected depending on the purpose. The Charpy impact strength of the injection molded article according to the another embodiment is 10 kJ / m 2 If the thickness is less than 1 m, the molded product may break when dropped from a height of 1 m or when hit.
[0089] The Charpy impact strength of the injection-molded article according to the another embodiment can be adjusted by adjusting the blending ratios of the high-crystalline poly(3-hydroxyalkanoate) resin, the medium-crystalline poly(3-hydroxyalkanoate) resin, and the low-crystalline poly(3-hydroxyalkanoate) resin. When the injection-molded article according to the another embodiment contains the resin composition for injection molding of the present invention, the Charpy impact strength can be adjusted by adjusting the blending ratios of the copolymer (A), the copolymer (B), and the copolymer (C).
[0090] The Charpy impact strength can be measured in accordance with the notched Charpy impact test described in JIS-K 7111-1:2012 (Plastics - Determination of Charpy impact properties - Part 1: Non-instrumented impact test). Specifically, first, a test specimen (length 80 mm, width 10 mm, thickness 4 mm) for measuring the Charpy impact value is prepared from the injection-molded article according to the other embodiment. The test specimen for measuring the Charpy impact value can be prepared, for example, using an automatic notch processing machine (for example, manufactured by Yasuda Seiki Co., Ltd.). Note that the test specimen for measuring the Charpy impact value is used two weeks after preparation. Using the obtained test specimen, measurement is performed in accordance with the notched Charpy impact test described in JIS-K 7111-1:2012 (Plastics - Determination of Charpy impact properties - Part 1: Non-instrumented impact test) using a Charpy impact testing machine (manufactured by Yasuda Seiki Co., Ltd.). The measurement atmosphere is set to 23°C and 50% RH.
[0091] The flexural modulus of the injection-molded article according to another embodiment is 520 MPa or more, preferably 650 MPa or more, more preferably 700 MPa or more, and even more preferably 850 MPa or more. The upper limit of the flexural modulus of the injection-molded article according to another embodiment is not particularly limited and can be appropriately selected depending on the purpose. However, from the viewpoint of impact resistance, it is preferably 1,200 MPa or less, more preferably 1,100 MPa or more, and even more preferably 1,000 MPa or more. If the flexural modulus of the injection-molded article according to another embodiment is less than 520 MPa, the injection-molded article may become soft and difficult to handle. The upper and lower limits of the flexural modulus of the injection-molded article according to another embodiment can be appropriately combined, but is 520 MPa or more, preferably 650 MPa to 1,200 MPa, more preferably 700 MPa to 1,100 MPa, and even more preferably 850 MPa to 1,000 MPa.
[0092] The flexural modulus of the injection-molded article according to the another embodiment can be adjusted by adjusting the blending ratios of the high-crystalline poly(3-hydroxyalkanoate) resin, the medium-crystalline poly(3-hydroxyalkanoate) resin, and the low-crystalline poly(3-hydroxyalkanoate) resin. When the injection-molded article according to the another embodiment contains the injection-molding resin composition of the present invention, the flexural modulus can be adjusted by adjusting the blending ratios of the copolymer (A), the copolymer (B), and the copolymer (C).
[0093] The flexural modulus can be measured in accordance with JIS-K 7171:2016 (Plastics - Determination of flexural properties). Specifically, it is measured in accordance with JIS-K 7171:2016 (Plastics - Determination of flexural properties) using a three-point bending tester (Autograph AG-X500N, manufactured by Shimadzu Corporation). The test conditions are a test speed of 2 mm / min, a distance between the support bases of 64 mm, and a radius between the indenter and the support base of 5.0 mm. The measurement atmosphere is 23°C and 50% RH. The measurement sample is used two weeks after molding.
[0094] Applications of the injection-molded article of the present invention are not particularly limited. However, due to its excellent impact resistance and bending properties, it can be suitably used for, for example, bottles, containers, and cases for beverages, liquid foods, liquid detergents, and the like, toys, entertainment products, tableware, agricultural materials, office automation parts, home appliance parts, body parts for ships and aircraft structures, automobile parts, daily necessities, stationery products, entertainment products, and the like.
[0095] (Method for producing injection-molded article) The method for producing an injection-molded article of the present invention includes a step of injection-molding the resin composition for injection molding of the present invention to obtain an injection-molded article (hereinafter, this may be referred to as an "injection molding step"), and may further include other steps as necessary. The method for producing an injection-molded article of the present invention uses the resin composition for injection molding of the present invention, which has excellent injection moldability, and therefore is excellent in production efficiency and can produce an injection-molded article that is excellent in impact resistance and bending properties.
[0096] <Injection Molding Step> The injection molding step is a step of obtaining an injection molded article by injection molding the resin composition for injection molding of the present invention.
[0097] The method for injection molding the resin composition for injection molding is not particularly limited and can be appropriately selected from known methods, and examples thereof include injection molding methods generally used when molding thermoplastic resins, as well as gas-assisted molding, injection compression molding, etc. In-mold molding, gas press molding, two-color molding, sandwich molding, push-pull, SCORIM, etc. can also be used.
[0098] A specific example of a method for injection molding the resin composition for injection molding includes a method in which the resin composition for injection molding that has been heated and melted is injected into a mold, the resin composition for injection molding is cooled and solidified in the mold, the mold is opened, and the molded article is released to obtain an injection-molded article.
[0099] <Other Steps> The other steps are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include a step of preparing a poly(3-hydroxyalkanoate)-based resin component and a step of preparing a resin composition for injection molding.
[0100] <<Poly(3-hydroxyalkanoate)-based resin component preparation step>> The poly(3-hydroxyalkanoate)-based resin component preparation step is a step of preparing the poly(3-hydroxyalkanoate)-based resin component, which is a raw material of the resin composition for injection molding. The poly(3-hydroxyalkanoate)-based resin component preparation step can be suitably carried out by the method described in the section "-Method for producing poly(3-hydroxyalkanoate)-based resin-" in the (Resin composition for injection molding) section above.
[0101] <<Step of Preparing Resin Composition for Injection Molding>> The step of preparing a resin composition for injection molding is a step of preparing the resin composition for injection molding to be used in the injection molding step. More specifically, the step of preparing a resin composition for injection molding is a step of melting and kneading a poly(3-hydroxyalkanoate)-based resin component, which is a raw material of the resin composition for injection molding, and, if necessary, other components.
[0102] The method for melting and kneading the raw materials of the resin composition for injection molding is not particularly limited and can be appropriately selected from known methods. Examples include methods of melting and kneading using an apparatus such as an extruder, a kneader, a Banbury mixer, or a roll.
[0103] The temperature at which the raw materials of the resin composition for injection molding are melted and kneaded cannot be generally defined because it depends on the melting point and melt viscosity of the poly(3-hydroxyalkanoate) resin component and other resins used, but the resin temperature at the die outlet of the molten kneaded product is preferably 150° C. to 200° C., more preferably 155° C. to 195° C., and even more preferably 160° C. to 190° C. If the resin temperature at the die outlet of the molten kneaded product is 150° C. or higher, the poly(3-hydroxyalkanoate) resin component can be suitably melted, and if it is 200° C. or lower, thermal decomposition of the poly(3-hydroxyalkanoate) resin component can be prevented.
[0104] The resin composition for injection molding obtained by melting and kneading the raw materials for the resin composition for injection molding may be further formed into resin pellets of a desired shape. Specific examples of the method for producing the resin pellets include a method in which the resin composition for injection molding obtained by melting and kneading the raw materials for the resin composition for injection molding is extruded into a strand shape using an extruder, and then cut into resin pellets of a particle shape such as a cylindrical shape, an elliptical cylinder shape, a spherical shape, a cubic shape, or a rectangular parallelepiped shape.
[0105] The resin pellets are preferably subjected to the injection molding step after being thoroughly dried at 40° C. to 80° C. to remove moisture.
[0106] The present invention will be specifically explained below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0107] The materials used in the following Examples 1 to 4 and Comparative Examples 1 to 3 are as follows. [Poly(3-hydroxyalkanoate)-based resin (P3HA)] The following poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) was used as the poly(3-hydroxyalkanoate)-based resin (P3HA). - P3HB3HH-1 (A-1): P3HB3HH (average content ratio: 3HB / 3HH = 95.0 / 5.0 (mol% / mol%), weight average molecular weight (Mw): 670,000 g / mol), produced in accordance with the method of Example 1 of WO 2019 / 142845. P3HB3HH-2(A-2): P3HB3HH (average content ratio: 3HB / 3HH = 95.0 / 5.0 (mol% / mol%), weight average molecular weight (Mw): 440,000 g / mol), produced in accordance with the method of Example 1 of WO 2019 / 142845. P3HB3HH-3(B): P3HB3HH (average content ratio: 3HB / 3HH = 73.6 / 26.4 (mol% / mol%), weight average molecular weight (Mw): 660,000 g / mol), produced in accordance with the method of Example 9 of WO 2019 / 142845. P3HB3HH-4(C): P3HB3HH (average content ratio: 3HB / 3HH = 97.9 / 2.1 (mol% / mol%), weight average molecular weight (Mw): 660,000 g / mol, produced in accordance with the method of Example 2 of WO 2019 / 142845.
[0108] [Additives] Additive 1: Pentaerythritol (Neuraizer P, manufactured by Mitsubishi Chemical Corporation) Additive 2: Behenic acid amide (BNT-22H, manufactured by Nippon Fine Chemical Co., Ltd.)
[0109] Example 1 Preparation of Poly(3-hydroxyalkanoate) Resin Component Various types of P3HA were mixed based on the composition and blending amounts shown in Table 1 below, with the total mass of polyhydroxyalkanoate resin (P3HA) being 100 parts by mass. Note that the unit of blending amount of each component in Table 1 is "parts by mass," and 100 parts by mass is 10 kg. Specifically, using a 75 L Super Mixer (manufactured by Kawata Corporation), 3 kg of P3HB3HH-1 (A-1), 4 kg of P3HB3HH-3 (B), 3 kg of P3HB3HH-4 (C), 100 g of Additive 1, and 50 g of Additive 2 were added and stirred at 300 rpm for 3 minutes, thereby obtaining the P3HA composition of Example 1.
[0110] <Compounding> Using a twin-screw extruder (TEM-26SS (L / D=60): manufactured by Toshiba Machine Co., Ltd.), the barrel and die temperatures were set to 140°C, the screw rotation speed was set to 100 rpm, and the P3HA composition was supplied from the main feeder using a constant mass feeder (KF-CM, manufactured by Kubota Corporation) so that the discharge rate was 10 kg / hour. Strands of the P3HA composition emerging from the tip of the die were passed through a water tank filled with warm water at 45°C to solidify, and then cut with a pelletizer to obtain pelletized P3HA composition (hereinafter sometimes abbreviated as "resin pellets").
[0111] <Preparation of Injection Molded Article> After extrusion molding by compounding, the resin pellets were dried at 60°C for 12 hours. Using an injection molding machine (PLASTAR Si-100IV, manufactured by Toyo Machinery & Metal Co., Ltd.), a rectangular injection molded article of Example 1 having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm was obtained under the following injection molding conditions. The peak pressure during injection molding was also measured. - Injection molding conditions - Nozzle temperature: 160°C Cylinder temperature H1: 160°C Cylinder temperature H2: 150°C Cylinder temperature H3: 130°C Cylinder temperature H4: 110°C Injection speed: 30 mm / sec Dwell pressure: 100 MPa, 20 seconds Mold temperature: 40°C Cooling time: 20 seconds
[0112] (Examples 2 to 4 and Comparative Examples 1 to 3) In the preparation of the poly(3-hydroxyalkanoate)-based resin component of Example 1, except that the composition and blending amounts were changed to the respective compositions and blending amounts shown in Table 1 below, the preparation of the poly(3-hydroxyalkanoate)-based resin component, compounding, and production of injection-molded articles were carried out in the same manner as in Example 1, and the injection-molded articles of Examples 2 to 4 and Comparative Examples 1 to 3 were obtained, respectively.
[0113] [Measurement of Average 3HH Content] The average content of 3-hydroxyhexanoate (3HH) units in all monomer units constituting the poly(3-hydroxyalkanoate) resin component (P3HA) obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was measured by the following method. The results are shown in Table 1 below. 2 mL of a sulfuric acid-methanol mixed solution (volume ratio of sulfuric acid:methanol = 15:85) and 2 mL of chloroform were added to 20 mg of dried poly(3-hydroxyalkanoate) resin component (P3HA), the container was sealed, and heated at 100°C for 140 minutes to obtain the methyl ester of the decomposition product of the poly(3-hydroxyalkanoate) resin component (P3HA). After cooling, 1.5 g of sodium bicarbonate was added little by little to neutralize the mixture, and the mixture was left to stand until the evolution of carbon dioxide gas ceased. After adding 4 mL of diisopropyl ether and mixing thoroughly, the mixture was centrifuged, and the monomer unit composition of the polyester decomposition product in the supernatant was analyzed by capillary gas chromatography under the following analytical conditions: -Analysis conditions- Gas chromatograph: GC-17A (Shimadzu Corporation) Capillary column: NEUTRA BOND-1 (column length: 25 m, column inner diameter: 0.25 mm, liquid film thickness: 0.4 μm, GL Sciences Inc.) Carrier gas: He gas Column inlet pressure: 100 kPa Sample injection amount: 1 μL Temperature conditions: The temperature was raised from an initial temperature of 100°C to 200°C at a rate of 8°C / min, and then from 200°C to 290°C at a rate of 30°C / min.
[0114] <Evaluation> The resin pellets obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were measured for "melt viscosity" by the following method, and the injection molded products obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were measured for "flexural modulus" and "Charpy impact value" by the following methods. Based on these measured values, a comprehensive evaluation was performed by the following method. The results are shown in Table 2 below.
[0115] [Measurement of Melt Viscosity] A Capillograph (1D PMD-C, manufactured by Toyo Seiki Seisaku-sho, Ltd.) equipped with an orifice having a diameter of 1 mm, a length of 10 mm, and an inlet angle of 45° and heated to 165°C was filled with 15 g of each of the resin pellets obtained by compounding in Examples 1 to 4 and Comparative Examples 1 to 3, and after preheating for 5 minutes, the piston was lowered at a rate of 50 mm / min (shear rate 608 / s), and the melt viscosity at a shear rate of 608 / s was calculated from the stress applied to the piston when the molten resin was extruded from the orifice.
[0116] [Measurement of flexural modulus] The flexural modulus of the injection molded articles obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was evaluated in accordance with JIS-K 7171:2016 (Plastics - Determination of flexural properties) using a three-point bending tester (Autograph AG-X500N, manufactured by Shimadzu Corporation). The test conditions were a test speed of 2 mm / min, a distance between support tables of 64 mm, and a radius between the indenter and the support table of 5.0 mm. The measurement atmosphere was 23°C and 50% RH. Samples taken two weeks after molding were used for the measurement.
[0117] [Measurement of Charpy Impact Value] Test specimens (length 80 mm, width 10 mm, thickness 4 mm, V-shaped notch, notch depth 2 mm, notch angle 45°) for measuring Charpy impact values were prepared from the injection molded articles obtained in Examples 1 to 4 and Comparative Examples 1 to 3 using an automatic notching machine (manufactured by Yasuda Seiki Co., Ltd.). Using the obtained test specimens, tests were conducted in accordance with the notched Charpy impact test described in JIS-K 7111-1:2012 (Plastics - Determination of Charpy Impact Properties - Part 1: Non-instrumented Impact Test) using a Charpy impact testing machine (manufactured by Yasuda Seiki Co., Ltd.). The measurement atmosphere was 23°C and 50% RH. Test specimens used for measuring Charpy impact values were prepared two weeks after the preparation of the test specimens.
[0118] [Overall Evaluation] The injection molded articles obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were comprehensively evaluated based on the balance between resin properties and molded article properties, in accordance with the following evaluation criteria. -Evaluation criteria- A: Charpy impact strength of 10 kJ / m 2 B: Charpy impact strength is 10 kJ / m or more, the flexural modulus is 520 MPa or more, and the melt viscosity is 500 Pa s or less. 2 C: Charpy impact strength is 10 kJ / m or more, and the flexural modulus is 520 MPa or more. 2 and / or the flexural modulus is less than 520 MPa.
[0119]
[0120]
[0121] Examples of aspects of the present invention include the following: <1> A resin composition for injection molding containing a poly(3-hydroxyalkanoate)-based resin component, wherein the poly(3-hydroxyalkanoate)-based resin component contains: a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content of 5 mol% or more and less than 24 mol%, a copolymer (B) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content of 24 mol% or more, and a copolymer (C) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content of 1 mol% or more and less than 5 mol%, wherein the content of the copolymer (A) is 5 parts by mass or more and 45 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C), The resin composition for injection molding is characterized in that the content of the copolymer (B) is 35 parts by mass or more and 55 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C), and the content of the copolymer (C) is 20 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total mass of the copolymer (A), the copolymer (B), and the copolymer (C). <2> The resin composition for injection molding according to <1> above, in which the weight-average molecular weight of the copolymer (A) is 500,000 or less. <3> The resin composition for injection molding according to <1> or <2> above, in which the average content of the other hydroxyalkanoate units is 9 mol% or more and less than 16 mol% of all monomer units constituting the poly(3-hydroxyalkanoate)-based resin component. <4> The resin composition for injection molding according to any one of <1> to <3> above, in which the other hydroxyalkanoate units are 3-hydroxyhexanoate units. <5> The resin composition for injection molding according to any one of <1> to <4>, having a melt viscosity of 400 Pa·s or more and 500 Pa·s or less, measured at 165°C and a shear rate of 608 / s. <6> An injection-molded article containing the resin composition for injection molding according to any one of <1> to <5>. <7> A Charpy impact strength of 10 kJ / m2 <8> The injection-molded article according to <6> or <7>, having a flexural modulus of 520 MPa or more. <9> An injection-molded article containing a poly(3-hydroxyalkanoate)-based resin component, having a Charpy impact strength of 10 kJ / m or more. 2 <10> A method for producing an injection-molded article, comprising a step of injection-molding the resin composition for injection molding according to any one of <1> to <5> to obtain an injection-molded article.
[0122] As described above, the present invention has been described based on specific embodiments and examples, but these embodiments and examples are presented merely as examples, and the present invention is not limited to the above embodiments and examples. The above embodiments can be embodied in various other forms, and various combinations, omissions, substitutions, additions, modifications, etc. can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are also included in the inventions described in the claims and their equivalents.
[0123] This international application claims priority based on Japanese Patent Application No. 2023-55685, filed on March 30, 2023, the entire contents of which are incorporated herein by reference.
Claims
1. A resin composition for injection molding containing a poly(3-hydroxyalkanoate)-based resin component, the poly(3-hydroxyalkanoate)-based resin component containing: a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content ratio of 5 mol% or more and less than 24 mol%, a copolymer (B) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content ratio of 24 mol% or more, and a copolymer (C) of 3-hydroxybutyrate units and other hydroxyalkanoate units having an average content ratio of 1 mol% or more and less than 5 mol%, the content of the copolymer (A) being 5 parts by mass or more and 45 parts by mass or less relative to 100 parts by mass of the total of the copolymers (A), (B), and (C); A resin composition for injection molding, characterized in that the content of the copolymer (B) is 35 parts by mass or more and 55 parts by mass or less, relative to 100 parts by mass of the total of the copolymers (A), (B), and (C), and the content of the copolymer (C) is 20 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total of the copolymers (A), (B), and (C).
2. The resin composition for injection molding according to claim 1, wherein the weight average molecular weight of said copolymer (A) is 500,000 or less.
3. The resin composition for injection molding according to claim 1, wherein the average content of the other hydroxyalkanoate units in all monomer units constituting the poly(3-hydroxyalkanoate) resin component is 9 mol % or more and less than 16 mol %.
4. The injection molding resin composition according to claim 1, wherein said other hydroxyalkanoate units are 3-hydroxyhexanoate units.
5. The resin composition for injection molding according to claim 1, having a melt viscosity measured at 165°C and a shear rate of 608 / s of 400 Pa·s or more and 500 Pa·s or less.
6. An injection molded article comprising the resin composition for injection molding according to claim 1.
7. Charpy impact strength is 10kJ / m 2 The injection molded article according to claim 6 .
8. The injection molded article according to claim 6, having a flexural modulus of 520 MPa or more.
9. An injection molded article containing a poly(3-hydroxyalkanoate) resin component, having a Charpy impact strength of 10 kJ / m 2 and a flexural modulus of elasticity of 520 MPa or more.
10. A method for producing an injection molded article, comprising the step of injection molding the resin composition for injection molding according to claim 1.
Citation Information
Patent Citations
PHA blend
JP2011140656A
Copolymer resin composition, molded article, and method of producing the copolymer resin composition
JP2012087207A
Resin composition and resin molding
JP2018131484A
Transformed microorganism for producing PHA copolymer comprising 3HH monomer unit at high composition rate and method for producing PHA using same
WO2019142845A1
Blow molded body and injection molded body
WO2022054758A1
Cited By
Polyhydroxyalkanoate composition, polyhydroxyalkanoate forming body and preparation method of polyhydroxyalkanoate forming body
CN121086491A
Biodegradable polymeric composition comprising pha
WO2026126201A1
Resin composition for air bubble cushioning material and resin film
WO2026126915A1