Powder containing anionic modified cellulose nanofibers

The anion-modified cellulose nanofiber powder addresses the agglomeration and handling issues of dried cellulose nanofibers by optimizing particle size, moisture, and pH, resulting in a stable, efficient, and cost-effective product with improved redispersibility and transfer efficiency.

WO2024202689A1PCT designated stage expired Publication Date: 2024-10-03NIPPON PAPER IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/005691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-22
Filing Date
2024-02-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Dried cellulose nanofibers tend to agglomerate and solidify during storage and use, leading to handling issues and increased costs, and require high water content for stability, which is costly and inefficient.

Method used

An anion-modified cellulose nanofiber powder with specific particle size distribution, moisture content, and pH levels is developed, ensuring the powder remains stable, non-agglomerative, and easy to handle, with improved redispersibility and reduced water absorption.

Benefits of technology

The anion-modified cellulose nanofiber powder maintains stability and handling efficiency, suppresses agglomeration, and reduces transportation costs by optimizing particle size, moisture, and pH, enhancing transfer efficiency and redispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000035_0000
    Figure 00000035_0000
  • Figure 00000035_0001
    Figure 00000035_0001
Patent Text Reader

Abstract

Provided is a powder containing anionic modified cellulose nanofibers having an average fiber diameter of 3-500 nm, the powder having a moisture content of 20 mass% or less, an average particle diameter of less than 45 μm, and a cumulative 10% diameter (D10) of 10 μm or less in a volume-based particle size distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Anion-modified cellulose nanofiber-containing powder

[0001] The present invention relates to a powder containing anionically modified cellulose nanofibers.

[0002] It is known that introducing anionic groups such as carboxyl groups or carboxymethyl groups into cellulose molecular chains and mechanically processing (defibrating) them can convert them into cellulose nanofibers with nanoscale fiber diameters. Because cellulose nanofibers are light, strong, and biodegradable, their applications in a variety of fields are being explored.

[0003] Generally, cellulose nanofibers into which anionic groups have been introduced are produced in a stably dispersed state in water, and are usually used in the form of a cellulose nanofiber dispersion of a predetermined concentration for various purposes, such as industrial materials or additives for foods and cosmetics. To maintain the cellulose nanofiber state stably, water is required that is several tens of times the amount of cellulose nanofiber, but this high water content increases the costs of packaging, storage, transportation, etc. of the cellulose nanofiber, so the cellulose nanofiber is dried to produce a dried product, and when ready to use, water is added to redisperse it and used as a redispersion.

[0004] When an aqueous dispersion of cellulose nanofibers is dried to form a dry solid, hydrogen bonds are formed between the fine cellulose fibers. Therefore, even if water is added to this dry solid to redisperse it, the viscosity and other properties do not return to the same level as before drying, and drying methods are being investigated (Patent Document 1, etc.).

[0005] International Publication No. 2019 / 189318

[0006] Dried cellulose nanofibers are commercialized by subjecting cellulose nanofibers dispersed in water (wet state) to processes such as drying, crushing, classification, and recovery. The commercialized cellulose nanofibers are compressed, bagged, and distributed, but when the cellulose nanofibers are used at their destination, they may be aggregated and solidified, which can easily lead to lumps during the redispersion process. Furthermore, due to the high hydrophilicity of the dried cellulose nanofiber products, they rapidly absorb water during use, resulting in problems with adhesion to various parts of the process. Furthermore, with the growing demand for dried cellulose nanofiber products, further cost reductions have been required.

[0007] Therefore, the present invention aims to provide a powder containing anion-modified cellulose nanofibers that can suppress aggregation and solidification of powder particles even when compressed and packed in bags, does not absorb water rapidly, is easy to handle during processing, and has excellent transport efficiency and low transport costs.

[0008] As a result of extensive research into achieving this object, the present inventors have found that producing a powder having a specific particle size is extremely effective, and have completed the present invention.

[0009] The present invention provides the following: (1) A powder containing anion-modified cellulose nanofibers having an average fiber diameter of 3 nm to 500 nm, the powder having a moisture content of 20% by mass or less, an average particle diameter of less than 45 μm, and a cumulative 10% diameter (D10) in a volume-based particle size distribution of 10 μm or less. (2) The anion-modified cellulose nanofiber-containing powder according to (1), having an angle of repose of 40 to 55°. (3) The anion-modified cellulose nanofiber-containing powder according to (1), having a collapse angle of 20 to 28°. (4) The anion-modified cellulose nanofiber-containing powder according to (1), having a difference angle of 20 to 30°. (5) The powder according to any one of (1) to (4), having a pH of 8 or higher when dispersed in 1% water.

[0010] According to the present invention, it is possible to provide a powder containing anion-modified cellulose nanofibers that can suppress aggregation and solidification of powder particles even when compressed and packed in a bag, does not absorb water rapidly, is easy to handle in the process, and has excellent transport efficiency and low transport costs.

[0011] 1 is a photograph showing an example determined to be graded A in the evaluation of initial water absorbency; and 2 is a photograph showing an example determined to be graded B in the evaluation of initial water absorbency.

[0012] The present invention will be described in detail below. In the present invention, "to" includes the end values. That is, "X to Y" includes the values ​​X and Y at both ends.

[0013] (Anion-modified cellulose nanofiber-containing powder) The present invention provides a powder containing anion-modified cellulose nanofibers (anion-modified CNF) having an average fiber diameter of 3 nm to 500 nm, wherein the powder has a moisture content of 20 mass% or less, an average particle diameter of less than 45 μm, and a cumulative 10% diameter (D10) in the volume-based particle diameter distribution of 10 μm or less.

[0014] (Moisture content) From the viewpoint of storage stability, the anion-modified CNF-containing powder of the present invention has a moisture content of 20% by mass or less, preferably 0 to 15% by mass, more preferably 0 to 10% by mass, and even more preferably 0 to 9.5% by mass. If the moisture content is higher than the upper limit, there is a problem of increased risk of spoilage. The powder may be dried to a moisture content of 0% (absolutely dry).

[0015] (Average particle size) From the viewpoint of transfer efficiency, the anion-modified CNF-containing powder of the present invention has an average particle size of less than 45 μm, preferably 5 μm or more and less than 20 μm. If the average particle size is too large above the upper limit, there is a problem that the powder becomes bulky and transfer efficiency decreases. Furthermore, if the average particle size is too large above the upper limit, there is a risk of poor redispersibility during weak stirring (e.g., 1000 rpm). Here, the average particle size (D50) is the particle size that includes 50% of the particle size distribution based on volume, calculated from the minimum value. The particle size distribution can be measured using a laser diffraction / scattering particle size distribution analyzer.

[0016] (Cumulative 10% Diameter) From the viewpoint of packing ratio, the anion-modified CNF-containing powder of the present invention has a cumulative 10% diameter (D10) of 10 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less. If D10 is too large above the upper limit, there is a problem that voids increase and the packing ratio decreases. It is also preferable that it is 0.1 μm or more. Here, the cumulative 10% diameter (D10) is the particle diameter that includes 10% of the particle diameter in the volume-based particle diameter distribution, calculated from the minimum value. The particle diameter distribution can be measured using a laser diffraction / scattering particle size distribution analyzer.

[0017] (Angle of repose) From the viewpoint of handleability and workability, the anion-modified CNF-containing powder of the present invention preferably has an angle of repose of 40 to 55°, more preferably 42 to 52°. If the angle of repose is too large, deposition is likely to occur in the hopper, and if it is too small, the powder will not stop flowing from the feeder outlet, etc. The angle of repose can be measured using a powder property tester.

[0018] (Collapse angle) From the viewpoint of handleability and workability, the collapse angle of the anion-modified CNF-containing powder of the present invention is preferably 20 to 28°, more preferably 22 to 25°. If the collapse angle is too large, a large impact is required to break up the powder pile, and if it is too small, the powder will not stop flowing from the feeder outlet, etc. The collapse angle can be measured using a powder property tester.

[0019] (Difference angle) From the viewpoint of ease of handling and workability, the anion-modified CNF-containing powder of the present invention preferably has a difference angle of 20 to 30°, more preferably 22 to 28°. If the difference angle is too large beyond the above range, the powder tends to be highly jet-like and easily scatters, while if it is too small, a large force is required to discharge the powder, making it difficult to control the discharge amount. The difference angle can be calculated from the angle of repose and angle of collapse measured using a powder property tester using the following formula: Difference angle = angle of repose - angle of collapse

[0020] (Circularity) From the viewpoint of workability during packaging, the anion-modified CNF-containing powder of the present invention has a lower limit of circularity of preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more. The upper limit of circularity is preferably 1.0 or less, more preferably 0.9 or less. The upper limit of circularity is 1. If the circularity is too lower than the above lower limit, aggregation is likely to occur during packaging. The circularity can be measured, for example, using a particle image analyzer (Morphologi G3, manufactured by Marvern Panalytical).

[0021] (pH after redispersion) From the viewpoint of improving redispersibility during weak stirring (e.g., 1000 rpm), the anion-modified CNF-containing powder of the present invention preferably has a pH of 7.0 or more, more preferably a pH of 8.0 or more, when dispersed in 1% water. The upper limit of the pH is preferably 10 or less.

[0022] (Anion-modified cellulose nanofiber) In the present invention, anion-modified cellulose nanofiber (anion-modified CNF) is a fine fiber having an average fiber diameter (fiber width) of 3 to 500 nm and an aspect ratio of 100 or more, and can be obtained by defibrating anion-modified cellulose.

[0023] (Cellulose Raw Material) Examples of cellulose raw materials for producing anion-modified cellulose include those derived from plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animal materials (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), microbial products, etc., and any of these can be used. Cellulose fibers derived from plants or microorganisms are preferred, and plant-derived cellulose fibers are more preferred.

[0024] (Anionic Modification) In the present invention, anionic modification refers to the introduction of anionic groups into cellulose, specifically the introduction of anionic groups into the pyranose ring of cellulose by carboxylation (oxidation) or substitution reaction. In the present invention, the carboxylation (oxidation) reaction refers to a reaction in which the hydroxyl group of the pyranose ring is directly oxidized to a carboxy group. In addition, in the present invention, substitution reaction refers to a reaction in which anionic groups are introduced into the pyranose ring by a substitution reaction other than the carboxylation (oxidation).

[0025] Examples of anionic modification include carboxylation (oxidation), carboxymethylation, esterification, etc. Among these, carboxylation (oxidation), carboxymethylation, and phosphate esterification are more preferred, and carboxylation (oxidation) is particularly preferred.

[0026] (Carboxylation) In the present invention, when carboxylated (oxidized) cellulose is used as the anion-modified cellulose, the carboxylated cellulose (also called oxidized cellulose) can be obtained by carboxylating (oxidizing) the above-mentioned cellulose raw material by a known method. Although not particularly limited, during carboxylation, the amount of carboxy groups is preferably adjusted to 0.6 to 2.0 mmol / g, and more preferably 1.0 mmol / g to 2.0 mmol / g, relative to the bone dry mass of the anion-modified cellulose nanofiber.

[0027] An example of a carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the surface of the cellulose, leaving aldehyde groups and carboxy groups (—COOH) or carboxylate groups (—COO) on the surface. - The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less.

[0028] An N-oxyl compound refers to a compound capable of generating a nitroxy radical. Any compound can be used as the N-oxyl compound as long as it promotes the target oxidation reaction. Examples include 2,2,6,6-tetramethylpiperidine-1-oxyl radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO).

[0029] The amount of the N-oxyl compound used is not particularly limited, as long as it is a catalytic amount that can oxidize the raw material cellulose. For example, the amount is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.05 to 0.5 mmol, per 1 g of bone-dry cellulose. The amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.

[0030] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose.

[0031] Known oxidizing agents can be used, such as halogens, hypohalous acids, halous acids, perhalogen acids or their salts, halogen oxides, and peroxides. Among these, sodium hypochlorite is preferred because it is inexpensive and has a low environmental impact. The appropriate amount of oxidizing agent used is, for example, preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, even more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. Furthermore, for example, 1 to 40 mol is preferred per 1 mol of the N-oxyl compound.

[0032] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature, about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, resulting in a decrease in the pH of the reaction solution. To efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably about 10 to 11. Water is preferred as the reaction medium because it is easy to handle and is less likely to cause side reactions.

[0033] The reaction time in the oxidation reaction can be appropriately set depending on the degree of progress of the oxidation, and is usually from 0.5 to 6 hours, for example, from about 0.5 to 4 hours.

[0034] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after the completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, thereby enabling efficient oxidation without reaction inhibition by sodium chloride produced as a by-product in the first-stage reaction.

[0035] Another example of a carboxylation (oxidation) method is a method in which cellulose raw materials are oxidized by contacting them with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m. 3 It is preferable that the density is 50 to 220 g / m 3It is more preferable that the ozone addition amount relative to the cellulose raw material is preferably 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solids content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is approximately 1 to 360 minutes, and preferably approximately 30 to 360 minutes. When the ozone treatment conditions are within these ranges, excessive oxidation and decomposition of cellulose can be prevented, resulting in a good yield of oxidized cellulose. After the ozone treatment, a further oxidation treatment may be performed using an oxidizing agent. The oxidizing agent used in the further oxidation treatment is not particularly limited, but examples include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, the further oxidation treatment can be performed by dissolving these oxidizing agents in water or a polar organic solvent such as alcohol to prepare an oxidizing agent solution, and then immersing the cellulose raw material in the solution.

[0036] The amount of carboxy groups in the oxidized cellulose can be adjusted by controlling the reaction conditions, such as the amount of oxidizing agent added and the reaction time.

[0037] (Carboxymethylation) When carboxymethylated cellulose is used as the anion-modified cellulose in the present invention, the carboxymethylated cellulose may be obtained by carboxymethylating the above-mentioned cellulose raw material using a known method, or a commercially available product may be used. In either case, the carboxymethyl group substitution degree per anhydroglucose unit of the cellulose is preferably 0.01 to 0.50. An example of a method for producing such carboxymethylated cellulose is the following. Cellulose is used as the starting material, and 3 to 20 times by mass of water and / or a lower alcohol, specifically water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., is used as a solvent, or a mixture of two or more of these. When a lower alcohol is mixed, the mixing ratio of the lower alcohol is 60 to 95% by mass. As the mercerizing agent, 0.5 to 20 times the molar amount of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, is used per anhydroglucose residue of the starting material. The starting material, solvent, and mercerizing agent are mixed and subjected to mercerization treatment at a reaction temperature of 0 to 70°C, preferably 10 to 60°C, for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Thereafter, a carboxymethylating agent is added at 0.05 to 10.0 times the moles per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90°C, preferably 40 to 80°C, for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.

[0038] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I in carboxymethylated cellulose is preferably 50% or more, more preferably 60% or more. The crystallinity of cellulose type I in carboxymethylated cellulose can be controlled by the concentration of the mercerizing agent during production, the temperature during treatment, and the degree of carboxymethylation. Since high concentrations of alkali are used in mercerization and carboxymethylation, cellulose type I crystals are likely to be converted to type II crystals. However, the desired crystallinity can be maintained by, for example, adjusting the amount of alkali (mercerizing agent) used to adjust the degree of conversion. The upper limit of the crystallinity of cellulose type I is not particularly limited. In reality, it is thought that the upper limit is about 90%. The crystallinity of cellulose type I in carboxymethylated cellulose and the crystallinity of cellulose type I in carboxymethylated CNF obtained by defibrating it are usually the same.

[0039] In this specification, "carboxymethylated cellulose," a type of anion-modified cellulose used in preparing anion-modified CNF, refers to a material that maintains at least a portion of its fibrous shape when dispersed in water. Therefore, it is distinguished from carboxymethyl cellulose, a type of water-soluble polymer described below. When observing an aqueous dispersion of "carboxymethylated cellulose" with an electron microscope, fibrous material can be observed. On the other hand, when observing an aqueous dispersion of carboxymethyl cellulose, a type of water-soluble polymer, no fibrous material is observed. Furthermore, when "carboxymethylated cellulose" is measured by X-ray diffraction, peaks of cellulose type I crystals can be observed, but cellulose type I crystals are not observed in the water-soluble polymer carboxymethyl cellulose.

[0040] (Esterification) In the present invention, when esterified cellulose is used as the anion-modified cellulose, the esterified cellulose can be obtained by a method of mixing a powder or an aqueous solution of phosphoric acid compound A with the above-mentioned cellulose raw material, or a method of adding an aqueous solution of phosphoric acid compound A to a slurry of the cellulose raw material.

[0041] Examples of the phosphoric acid compound A include phosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, polyphosphonic acid, and esters thereof. These may be in the form of a salt. Among these, compounds having a phosphoric acid group are preferred because they are low cost, easy to handle, and can introduce phosphoric acid groups into the cellulose of the pulp fibers to improve defibration efficiency. Examples of compounds having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. These compounds can be used alone or in combination of two or more. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are more preferred from the viewpoints of high efficiency of introducing phosphoric acid groups, ease of defibration in the defibration step described below, and ease of industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is preferable to use the phosphoric acid compound A as an aqueous solution, since this increases the uniformity of the reaction and the efficiency of introducing the phosphoric acid group. The pH of the aqueous solution of phosphoric acid compound A is preferably 7 or less, since this increases the efficiency of introducing the phosphoric acid group, but from the viewpoint of suppressing hydrolysis of the pulp fiber, a pH of 3 to 7 is preferred.

[0042] The following method can be mentioned as an example of a method for producing phosphated cellulose. A phosphoric acid compound A is added to a dispersion of a cellulose raw material having a solids concentration of 0.1 to 10% by mass while stirring, to introduce phosphate groups into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of phosphoric acid compound A added is preferably 0.2 to 500 parts by mass, and more preferably 1 to 400 parts by mass, in terms of the amount of phosphorus element. If the proportion of phosphoric acid compound A is equal to or greater than the lower limit, the yield of fine cellulose fibers can be further improved. However, if the proportion exceeds the upper limit, the effect of improving the yield reaches a plateau, which is not preferable from a cost perspective.

[0043] In this case, in addition to the cellulose raw material and phosphoric acid compound A, a powder or aqueous solution of compound B may be mixed. Compound B is not particularly limited, but a basic nitrogen-containing compound is preferred. "Basic" here is defined as an aqueous solution exhibiting a pink to red color in the presence of a phenolphthalein indicator, or a pH of the aqueous solution greater than 7. The basic nitrogen-containing compound used in the present invention is not particularly limited as long as it achieves the effects of the present invention, but a compound having an amino group is preferred. Examples include, but are not limited to, urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea is preferred due to its low cost and ease of handling. The amount of compound B added is preferably 2 to 1,000 parts by mass, more preferably 100 to 700 parts by mass, per 100 parts by mass of the solid content of the cellulose raw material. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is about 1 to 600 minutes, and more preferably 30 to 480 minutes. When the esterification reaction conditions are within these ranges, it is possible to prevent the cellulose from being excessively esterified and becoming more soluble, resulting in a good yield of phosphated cellulose. After dehydrating the resulting phosphated cellulose suspension, it is preferably heat-treated at 100 to 170°C in order to suppress cellulose hydrolysis. Furthermore, it is preferable to heat the suspension at 130°C or lower, preferably 110°C or lower, while it contains water, and then, after removing the water, to heat the suspension at 100 to 170°C.

[0044] The degree of phosphate substitution per glucose unit of the phosphate-esterified cellulose is preferably 0.001 to 0.40. Introducing phosphate group substituents into cellulose causes electrical repulsion between cellulose molecules. Therefore, cellulose with phosphate groups introduced therein can be easily defibrated. If the degree of phosphate substitution per glucose unit is less than 0.001, it cannot be sufficiently defibrated. On the other hand, if the degree of phosphate substitution per glucose unit is greater than 0.40, it may swell or dissolve, making it impossible to obtain fine cellulose fibers. To efficiently defibrate, the phosphate-esterified cellulose raw material obtained above is preferably washed by boiling and then washing with cold water. The modification by these esterifications is a modification by a substitution reaction. The degree of substitution in the esterified cellulose and the degree of substitution when the esterified cellulose is defibrated are usually the same.

[0045] Phosphate-esterified cellulose can be described as cellulose into which an anionic phosphorus oxoacid group or a substituent derived from a phosphorus oxoacid group (sometimes simply referred to as a "phosphorus oxoacid group") has been introduced. Here, the phosphorus oxoacid group is, for example, a divalent functional group obtained by removing a hydroxy group from phosphoric acid, specifically -PO 3 H 2 The substituent derived from the phosphorus oxo acid group includes salts of the phosphorus oxo acid group, phosphorus oxo acid ester groups, and other substituents. The substituent derived from the phosphorus oxo acid group may be contained in the cellulose nanofiber as a group in which a phosphate group is condensed (e.g., a pyrophosphate group). The phosphorus oxo acid group may also be, for example, a phosphorous acid group (phosphonic acid group), and the substituent derived from the phosphorus oxo acid group may be a salt of the phosphorous acid group, or the like.

[0046] The amount of phosphorus oxoacid groups, such as phosphate groups or phosphite groups, introduced into the phosphated cellulose is not particularly limited. During phosphate esterification, the amount of phosphorus oxoacid groups is preferably adjusted to 0.5 to 5 mmol / g, and more preferably 0.5 to 2.5 mmol / g, relative to the bone dry mass of the anion-modified cellulose nanofiber.

[0047] (Defibrillation) The device used to defibrate anionically modified cellulose is not particularly limited, and devices such as high-speed rotation, colloid mill, high-pressure, roll mill, and ultrasonic devices can be used. During defibration, it is preferable to apply a strong shear force to the aqueous dispersion of anionically modified cellulose. In particular, for efficient defibration, it is preferable to apply a pressure of 50 MPa or more to the aqueous dispersion and to use a wet high-pressure or ultra-high-pressure homogenizer capable of applying a strong shear force. The pressure is more preferably 100 MPa or more, and even more preferably 140 MPa or more. Furthermore, prior to the defibration and dispersion treatment using the high-pressure homogenizer, the aqueous dispersion may be subjected to a pretreatment, if necessary, using a known mixing, stirring, emulsifying, or dispersing device such as a high-speed shear mixer.

[0048] (Dispersant) The anion-modified cellulose nanofiber-containing powder of the present invention may contain a dispersant from the viewpoint of improving redispersibility. Examples of dispersants include water-soluble polymers, surfactants, etc., and it is preferable to use a water-soluble polymer because it covers areas of low charge density on the surface of the anion-modified cellulose nanofiber, suppresses the formation of hydrogen bonds, and prevents aggregation of the cellulose nanofibers during drying.

[0049] (Water-Soluble Polymer) In the present invention, examples of water-soluble polymers include cellulose derivatives (carboxymethylcellulose, methylcellulose, hydroxypropylcellulose, ethylcellulose), xanthan gum, xyloglucan, dextrin, dextran, carrageenan, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, arrowroot flour, modified starch (cationized starch, phosphorylated starch, phosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch, hydroxypropyl starch, hydroxypropylated phosphate cross-linked starch, acetylated adipate cross-linked starch, acetylated phosphate cross-linked starch, acetylated oxidized starch, starch sodium octenylsuccinate, starch acetate, oxidized starch), corn starch, gum arabic, and gellan. Examples of the modified cellulose nanofibers include gum, polydextrose, pectin, chitin, water-soluble chitin, chitosan, casein, albumin, soy protein lysate, peptone, polyvinyl alcohol, polyacrylamide, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl acetate, polyamino acids, polylactic acid, polymalic acid, polyglycerin, latex, rosin-based sizing agents, petroleum resin-based sizing agents, urea resin, melamine resin, epoxy resin, polyamide resin, polyamide-polyamine resin, polyethyleneimine, polyamine, vegetable gum, polyethylene oxide, hydrophilic crosslinked polymers, polyacrylates, starch-polyacrylic acid copolymers, tamarind gum, guar gum, and colloidal silica, as well as mixtures of one or more thereof. Among these, cellulose derivatives are preferred in terms of compatibility with anion-modified cellulose nanofibers, and carboxymethyl cellulose and its salts are particularly preferred. It is thought that water-soluble polymers such as carboxymethyl cellulose and its salts penetrate between the anion-modified cellulose nanofibers and increase the distance between the CNFs, thereby improving redispersibility.

[0050] When carboxymethyl cellulose or a salt thereof is used as the water-soluble polymer, it is preferable to use a carboxymethyl cellulose having a degree of carboxymethyl group substitution per anhydroglucose unit of 0.55 to 1.6, more preferably 0.55 to 1.1, and even more preferably 0.65 to 1.1. Furthermore, carboxymethyl cellulose with longer molecules (higher viscosity) is preferred because it is more effective at widening the distance between CNFs. The Brookfield viscosity of a 1% by mass aqueous solution of carboxymethyl cellulose at 25°C and 600 rpm is preferably 3 to 14,000 mPa s, more preferably 7 to 14,000 mPa s, and even more preferably 1,000 to 8,000 mPa s. Note that the "carboxymethyl cellulose or a salt thereof" referred to here as the water-soluble polymer is completely soluble in water, and is therefore distinguished from the carboxymethylated cellulose described above, the fibrous shape of which can be confirmed in water.

[0051] In the present invention, when a dispersant is contained in the anion-modified cellulose nanofiber-containing powder, the blending ratio of anion-modified CNF (bone dry solids) to dispersant is preferably 2:8 to 8:2, and more preferably 5:5 to 7:3, from the viewpoint of obtaining an improved effect on redispersibility. If the blending ratio of the dispersant is too much higher than the upper limit, problems such as reduced viscosity characteristics such as thixotropy, which are characteristic of anion-modified CNF, and reduced dispersion stability may occur. If the blending ratio of the dispersant is too much lower than the lower limit, sufficient redispersibility cannot be obtained.

[0052] (Method for producing powder) The method for producing the anion-modified CNF-containing powder of the present invention is not particularly limited. For example, an aqueous suspension containing anion-modified CNF and a dispersant, if necessary, is dehydrated and dried to obtain a dry solid, which is then pulverized using a pulverizer or the like, and the resulting pulverized material is classified as necessary and recovered to obtain a powder; or a method in which the aqueous suspension is spray-dried to simultaneously dehydrate, dry, and powderize the suspension, and the resulting powder is then classified as necessary and recovered to obtain a powder. Examples of spray methods include an atomizer, a one-fluid nozzle, and a two-fluid nozzle.

[0053] In addition, from the viewpoint of achieving good redispersibility, it is preferable to adjust the pH of the aqueous suspension containing anion-modified CNF to 7 to 12, more preferably 7.5 to 11, using an alkali such as sodium hydroxide, sodium bicarbonate, or potassium hydroxide before dehydrating and drying it.

[0054] The processing conditions for spray drying vary depending on the spraying method and cannot be generalized. However, for example, processing conditions such as the concentration, viscosity, spray pressure, temperature, amount of drying air, and amount of liquid fed can be adjusted, a calibration curve showing the relationship between the processing conditions and the particle size can be prepared, and appropriate processing conditions can be determined based on the calibration curve so as to obtain the desired average particle size.

[0055] Methods for dehydrating and drying aqueous suspensions containing anion-modified CNF may be conventionally known, such as spray drying, freeze drying, squeezing, air drying, hot air drying, and vacuum drying. Specific examples of drying apparatuses that can be used include the following: continuous tunnel dryers, band dryers, vertical dryers, vertical turbo dryers, multi-stage disk dryers, through-flow dryers, rotary dryers, flash dryers, spray dryer dryers, spray dryers, cylindrical dryers, drum dryers, reduced-pressure belt dryers, screw conveyor dryers, rotary dryers with heating tubes, vibration transport dryers, fluidized bed dryers, etc.; batch-type box dryers, through-flow dryers, vacuum box dryers, agitator dryers, shelf dryers, freeze dryers, etc., can be used alone or in combination of two or more. Among these, drum dryers and belt dryers are preferred, and from the viewpoint of energy efficiency, drum dryers, which directly and uniformly supply heat energy to the material to be dried, are even more preferred.

[0056] The method for pulverizing the anion-modified CNF-containing dry solid to obtain a pulverized product is not particularly limited. For example, the pulverized product can be obtained by pulverizing the anion-modified CNF-containing dry solid with a pulverizer. Examples of pulverizers include cutting mills: mesh mill (manufactured by HORAI Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Manufacturing Co., Ltd.), knife mill (manufactured by Parman Co., Ltd.), cutter mill (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), CS cutter (manufactured by Mitsui Mining Co., Ltd.), rotary cutter mill (manufactured by Nara Machinery Manufacturing Co., Ltd.), turbo cutter (manufactured by Freund Corporation), pulp crusher (manufactured by Zuiko Co., Ltd.), shredder (manufactured by Kobe Steel Pantech Co., Ltd.), hammer mills: jaw crusher (manufactured by Makino Corporation), etc. (manufactured by Makino Sangyo Co., Ltd.), hammer crusher (manufactured by Makino Sangyo Co., Ltd.), impact mill: Pulverizer (manufactured by Hosokawa Micron Corporation), Fine Impact Mill (manufactured by Hosokawa Micron Corporation), Super Micron Mill (manufactured by Hosokawa Micron Corporation), Inomizer (manufactured by Hosokawa Micron Corporation), Fine Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), CUM-type centrifugal mill (manufactured by Mitsui Mining Co., Ltd.), Exceed Mill (manufactured by Makino Sangyo Co., Ltd.), Ultraplex (manufactured by Makino Sangyo Co., Ltd.), Contraplex (manufactured by Makino Sangyo Co., Ltd.) Co., Ltd.), Coroplex (Makino Sangyo Co., Ltd.), Sample Mill (Seishin Co., Ltd.), Bantam Mill (Seishin Co., Ltd.), Atomizer (Seishin Co., Ltd.), Tornado Mill (Nikkiso Co., Ltd.), Nea Mill (Dalton Co., Ltd.), HT-type fine grinder (Horai Co., Ltd.), Free Grinding Mill (Nara Machinery Manufacturing Co., Ltd.), New Cosmomizer (Nara Machinery Manufacturing Co., Ltd.), Turbo Mill (Freund Corporation), Gather Mill (Nishimura Machinery Manufacturing Co., Ltd.), Super Powder Mill (Nishimura Machinery Manufacturing Co., Ltd.), Blade Mill (Nisshin Engineering Inc.), Super Rotor (Nisshin Engineering Inc.), Npa Crusher (Sansho Industry Co., Ltd.), Wheeley Grinding Mill (Sanki Manufacturing Co., Ltd.), Pulp Grinding Mill (Zuiko Co., Ltd.), Jacobson Fine Grinding Mill (Kobe Pantech Co., Ltd.), Universal Mill (Tokuju Kogyosho Co., Ltd.), Atomizer (Tokyo Atomizer Manufacturing Co., Ltd.), Mill Star Dam (Tokyo Atomizer Manufacturing Co., Ltd.),Airflow type mills: Stream Mill (manufactured by Nippon Coke Engineering Co., Ltd.), CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), Micron Jet (manufactured by Hosokawa Micron Corporation), Counter Jet Mill (manufactured by Hosokawa Micron Corporation), Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.), Supersonic Jet Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), Current Jet (manufactured by Nisshin Engineering Inc.), Jet Mill (manufactured by Sansho Industry Co., Ltd.), Ebara Jet Micronizer (manufactured by Ebara Corporation), Ebara Triad Jet (manufactured by Ebara Corporation), Selenium Mirror (manufactured by Masuko Sangyo Co., Ltd.), New Micro Sic Examples include matte (manufactured by Masuno Manufacturing Co., Ltd.), Kryptron (manufactured by Kawasaki Heavy Industries, Ltd.), disc mills: vibrating disc mill (manufactured by Retsch), centri-cutter (manufactured by Nippon Coke Engineering Co., Ltd.), turbo disc mill (manufactured by Freund Turbo Corporation), mortar-type high-speed crusher (manufactured by Makino Sangyo Co., Ltd.), vertical roller mills: vertical roller mill (manufactured by Chinon Co., Ltd.), vertical roller mill (manufactured by Schaeffler Japan Co., Ltd.), roller mill (manufactured by Kotobuki Giken Kogyo Co., Ltd.), VX mill (manufactured by Kurimoto Iron Works Co., Ltd.), KVM-type vertical mill (manufactured by Earth Technica Co., Ltd.), and IS mill (manufactured by IHI Plant Engineering Co., Ltd.). The processing conditions for these crushers cannot be uniformly determined because the principles of crushing differ. However, for example, a method can be used in which processing conditions that affect the crushing process, such as the screen diameter at the crusher outlet and the rotation speed of the classification rotor, are adjusted, a calibration curve showing the relationship between processing conditions and particle size is created, and appropriate processing conditions are determined based on the calibration curve to achieve the desired average particle size.

[0057] The pulverized material containing anion-modified CNF may be classified as needed. When classification is performed, it can be performed using a classifier attached to or attached to a pulverizer.

[0058] The type of device used to collect the pulverized material containing anion-modified CNF and the granulated material obtained by spray drying is not particularly limited. Examples of the collection device include a cyclone and a bag filter.

[0059] The anion-modified CNF-containing powder may be classified after collection.

[0060] The anion-modified CNF-containing powder of the present invention has an average particle size of less than 45 μm and a cumulative 10% diameter (D10) of 10 μm or less, so that even when compressed and packed, it can suppress agglomeration of the powder particles, does not rapidly absorb water, is easy to handle in the process, has high loose bulk density and packed bulk density, has excellent transport efficiency, and low transport costs.In addition, the anion-modified CNF-containing powder of the present invention is particularly excellent in redispersibility when weakly stirred at about 1000 rpm.

[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0062] (Average Fiber Diameter and Average Fiber Length of CNF) The powder was redispersed in water to prepare a suspension, which was then diluted. 200 randomly selected fibers were analyzed using an atomic force microscope (AFM) and the average was calculated. The aspect ratio was calculated using the following formula: Aspect ratio = Average fiber length / Average fiber diameter

[0063] (Carboxy group amount) The carboxy group amount was calculated using the following formula: 60 mL of a 0.5 mass% slurry (aqueous dispersion) of carboxylated cellulose was prepared, 0.1 M aqueous hydrochloric acid was added to adjust the pH to 2.5, 0.05 N aqueous sodium hydroxide was added dropwise, and the electrical conductivity was measured until the pH reached 11. The amount of carboxy groups was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of a weak acid, where the change in electrical conductivity was gradual: Carboxy group amount [mmol / g carboxylated cellulose] = a [mL] × 0.05 / mass of carboxylated cellulose [g].

[0064] (Degree of Carboxymethyl Substitution) The degree of carboxymethyl substitution was measured by the following method. Approximately 2.0 g of sample was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 100 mL of a solution of 1000 mL of nitric acid methanol and 100 mL of special-grade concentrated nitric acid was added, and the mixture was shaken for 3 hours to convert the carboxymethylated cellulose CNF salt (CMC) into H-CMC (hydrogen-type carboxymethylated CNF). 1.5 to 2.0 g of the bone-dried H-CMC was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. The H-CMC was moistened with 15 mL of 80% methanol, 100 mL of 0.1 N NaOH was added, and the mixture was shaken at room temperature for 3 hours. Phenolphthalein was used as an indicator, and the 0.1 N-H 2 SO 4 The excess NaOH was back-titrated with 0.05% NaOH, and the degree of carboxymethyl substitution (DS value) was calculated by the following formula: A = [(100 × F' - 0.1N - H 2 SO 4 (mL) × F × 0.1] / (bone dry mass (g) of H-CMC) Degree of carboxymethyl substitution = 0.162 × A / (1 - 0.058 × A) F': Factor of 0.1N-NaOH F: 0.1N-H 2 SO 4 Factor

[0065] The degree of carboxymethyl substitution in the CNF of carboxymethyl cellulose is usually the same as the degree of carboxymethyl substitution in the carboxymethyl cellulose before being converted into CNF.

[0066] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I of carboxymethylated cellulose nanofibers was measured by the following method. A sample was placed in a glass cell and measured using an X-ray diffraction measurement device (LabX XRD-6000, manufactured by Shimadzu Corporation). The crystallinity was calculated using the method of Segal et al., and was calculated using the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous portion at 2θ = 18.5°, using the diffraction intensity from 2θ = 10° to 50° in the X-ray diffraction pattern as the baseline, using the following formula:

[0067] Xc = (I002c - Ia) / I002c × 100 Xc = Crystallinity (%) of cellulose type I I002c: 2θ = 22.6°, diffraction intensity of 002 plane Ia: 2θ = 18.5°, diffraction intensity of amorphous part

[0068] The proportion of type I crystals in carboxymethylated cellulose nanofibers is usually the same as that in the carboxymethyl cellulose before it is made into CNF.

[0069] (Amount of phosphorus oxoacid groups) The amount of phosphorus oxoacid groups (amount of phosphate groups or phosphite groups) was measured by the following method. First, ion-exchanged water was added to the target CNF to prepare a slurry with a solids concentration of 0.2 mass%. The obtained slurry was treated with an ion-exchange resin, and then titrated with an alkali to measure the amount of phosphorus oxoacid groups.

[0070] Treatment with ion exchange resin was carried out by adding 1 / 10 by volume of a strongly acidic ion exchange resin (Amberjet 1024; Organo Corporation, conditioned) to the above CNF-containing slurry, shaking for 1 hour, and then pouring it onto a mesh with 90 μm openings to separate the resin and slurry.

[0071] In addition, the alkali titration was performed by adding 10 μL of 0.1 N sodium hydroxide solution to the CNF-containing slurry after ion exchange resin treatment every 5 seconds while measuring the change in the pH value of the slurry. Nitrogen gas was bubbled into the slurry 15 minutes before the start of the titration. In this neutralization titration, two maximum points of increment (differential value of pH with respect to the amount of alkali added) were observed on the curve plotting the measured pH against the amount of alkali added. Of these, the maximum point of increment obtained first after starting the addition of alkali is called the first endpoint, and the maximum point of increment obtained next is called the second endpoint. The amount of alkali required from the start of the titration to the first endpoint is equal to the amount of first dissociated acid in the slurry used for titration. Furthermore, the amount of alkali required from the start of the titration to the second endpoint is equal to the total amount of dissociated acid in the slurry used for titration. The amount of alkali (mmol) required from the start of titration to the first endpoint was divided by the solid content (g) in the slurry to be titrated, and the value was taken as the amount of phosphorus oxo acid groups (mmol / g).

[0072] (Water Content) The water content of the powder was calculated as the difference between the mass of the obtained powder after drying at 105° C. for 3 hours or more (bone dry mass) and the mass before drying.

[0073] (Particle diameter) The average particle diameter (D50) of the powders used in the examples and comparative examples is the particle diameter that includes 50% of the particles when accumulated from the minimum value in the volume-based particle diameter distribution, and the cumulative 10% diameter (D10) is the particle diameter that includes 10% of the particles when accumulated from the minimum value.

[0074] The particle size was measured using a laser diffraction / scattering particle size distribution analyzer (Mastersizer 3000, manufactured by Spectris Co., Ltd.) under the condition of a particle refractive index of 1.5. The measurement was performed by directly putting the dry powder sample into the device.

[0075] (Angle of Repose) The angle of repose of the powders obtained in the Examples and Comparative Examples was determined as the value of the angle of repose (angle of elevation) when the powder was dropped and deposited from the hole of a funnel onto a horizontal plate of a certain area until it took on a certain shape using a powder property testing device (Powder Tester PT-X model, manufactured by Hosokawa Micron Corporation) to form conical granules.

[0076] (Collapse Angle) The collapse angle of the powders obtained in the Examples and Comparative Examples was measured using a powder property tester (Powder Tester PT-X, manufactured by Hosokawa Micron Corporation) by dropping and depositing the powder from the holes of a funnel onto a horizontal plate of a certain area until a certain shape was achieved, forming conical granules. Next, a weight of a certain weight placed on the same base as the horizontal plate was dropped to apply a certain impact to the powder, and after some of the powder naturally flowed and fell off the horizontal plate, the angle of elevation of the remaining conical granules from a point on the outer periphery of the base to the apex of the cone was taken as the collapse angle.

[0077] (Difference Angle) Using the angle of repose and angle of collapse measured above, the difference angle was calculated according to the following formula: Difference Angle = Angle of Repose - Angle of Collapse

[0078] (Loose Bulk Density) The loose bulk density of the powders obtained in the Examples and Comparative Examples was measured using a powder property tester (Powder Tester PT-X, manufactured by Hosokawa Micron Corporation). Specifically, a sample was filled into a container of a fixed capacity by gravity, and the sample was weighed to determine the density.

[0079] (Packed Bulk Density) The packed bulk density of the powders obtained in the Examples and Comparative Examples was measured using a powder property tester (Powder Tester PT-X, manufactured by Hosokawa Micron Corporation). Specifically, the samples were closely packed into a container of a fixed capacity while tapping, and then the samples were weighed to determine the density.

[0080] (Compressibility) The compressibility of the powders obtained in the examples and comparative examples was calculated by the following formula: Compressibility (%) = (packed bulk density - loose bulk density) / packed bulk density x 100

[0081] (Circularity) The circularity of the powders obtained in the examples and comparative examples was measured using a Morphologi G3 (manufactured by Malvern Panalytical). 3 An image of the powder was taken at an objective magnification of 10 times, and the circularity was determined by image analysis. The number of particles (N) measured was 257,614 in Example 1 and 7,106 in Comparative Example 1.

[0082] (Evaluation of cohesion) The cohesion of the powders obtained in the Examples and Comparative Examples was checked before and after packaging. After placing the sample in a polyethylene bag, the bag was tapped to pack it as densely as possible, and the bag was sealed while being pressed by hand to degas, and then stored at a humidity of 80% and 40°C. After one week of storage, the powder was removed from the bag, and the cohesion was evaluated according to the following criteria. A: No powder cohesion, smooth state B: Some powder cohesion observed

[0083] (Evaluation of Initial Water Absorbency) The water absorbency (initial water absorbency) of the powders obtained in the Examples and Comparative Examples was evaluated in a short time. 0.1 g of a specimen was placed flat on a rectangular glass plate. 1 mL of pure water was then evenly dripped onto the specimen using a dropper, and the water absorbency immediately after dripping was evaluated according to the following criteria: A: Water absorption into the powder was moderate immediately after dripping, and little gel layer was formed. B: Water absorption into the powder occurred immediately after dripping, and a thick gel layer was formed. Regarding the above criteria, an example that received a rating of A is shown in Figure 1, and an example that received a rating of B is shown in Figure 2. In Figure 1, it can be seen that most of the water was not absorbed into the powder and separated. On the other hand, in Figure 2, it can be seen that the water was absorbed into the powder and the powder swelled.

[0084] (Preparation of redispersions of dry powder) In the examples and comparative examples, water was added to the obtained dry powder and stirred for 30 minutes using a homodisper to obtain CNF redispersions with a CNF concentration of 1.0% by mass. The redispersions were prepared under two stirring conditions: 1000 rpm (weak stirring) and 3000 rpm (strong stirring). Each of the obtained 1.0% by mass redispersions was used for the following evaluation of redispersibility.

[0085] (Evaluation of Redispersibility) Two drops of ink drop (Kuretake Corporation, solids content 10%) were dropped into the redispersion liquid with a CNF concentration of 1.0% by mass obtained as described above, and the liquid was stirred for 1 minute by setting the rotation speed of a vortex mixer (Iuchi Corporation, equipment name: Automatic Lab-mixer HM-10H) to the maximum. The stirred liquid was sandwiched between two glass plates to give a film thickness of 0.15 mm, and observed at 200x magnification using an optical microscope (KEYENCE Corporation, digital microscope VHX-6000) to confirm the presence or absence of white particles (aggregates of CNF). The redispersibility with weak stirring and strong stirring was evaluated according to the following criteria, and the results are shown in Table 1. A: Almost no white particles were observed. B: A small amount of very small white particles were observed. C: Large white particles were observed.

[0086] (pH of aqueous dispersion after re-dispersion) The pH of the re-dispersion (rotation speed: 3000 rpm) obtained as described above and having a CNF concentration of 1.0 mass % was measured. The results are shown in Table 1.

[0087] (Production Example 1) (Production of Carboxylated CNF1) 500 g (bone-dry) of bleached softwood-derived dissolving kraft pulp (DKP manufactured by Buckeye) was added to 50 L of an aqueous solution containing 7.8 g (0.05 mol) of TEMPO (Sigma-Aldrich) and 75.5 g (0.74 mol) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. 1.6 L of a 2 M aqueous sodium hypochlorite solution was added to the reaction system, and the oxidation reaction was initiated (oxidation treatment). During the reaction, the pH of the system decreased, but was adjusted to pH 10 by successive addition of a 3 M aqueous sodium hydroxide solution. After reacting for 2 hours, the mixture was filtered through a glass filter and thoroughly washed with water to obtain carboxylated cellulose. A 5.0% (w / v) carboxylated cellulose slurry was prepared using water. Hydrogen peroxide was added to the slurry at 2% (w / w) relative to the carboxylated cellulose, and the pH was adjusted to 11.3 with 3M sodium hydroxide. This slurry was then hydrolyzed at 80°C for 2 hours. The resulting slurry was adjusted to 5.0% (w / v) with water and processed five times with an ultra-high-pressure homogenizer (20°C, 140 MPa) to obtain a dispersion of carboxylated CNF1. The pH of the resulting dispersion (solids concentration 1%) was 7.5. The resulting carboxylated CNF1 had a carboxyl group content of 1.7 mmol / g, an average fiber diameter of 3 nm, and an aspect ratio of 117.

[0088] (Production Example 2) (Production of Carboxylated CNF2) 500 g (bone dry) of bleached, unbeaten kraft pulp derived from softwood (brightness 85%) was added to 20 L of an aqueous solution containing TEMPO (Sigma-Aldrich) (0.025 mmol / g relative to the cellulose raw material) and sodium bromide (1 mmol / g relative to the cellulose raw material), and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system to a concentration of 5.2 mmol / g, initiating the oxidation reaction. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The reaction mixture was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain oxidized pulp (carboxylated cellulose). The pulp yield at this time was 90%, the time required for the oxidation reaction was 100 minutes, and the amount of carboxyl groups was 1.4 mmol / g.

[0089] The oxidized pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of carboxylated CNF2. The obtained fibers had an average fiber diameter of 4 nm and an aspect ratio of 220.

[0090] (Production Example 3) (Production of Carboxymethylated CNF) 500 parts of isopropanol (IPA) and a solution of 15 parts of sodium hydroxide dissolved in 200 parts of water were added to a 5 L twin-screw kneader adjusted to 100 rpm, and 100 parts of hardwood pulp (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) was added (based on the dry mass of the pulp dried at 100°C for 60 minutes). The mixture was stirred and mixed at 30°C for 90 minutes to prepare mercerized cellulose. 19 parts of sodium monochloroacetate dissolved in 20 parts of 90% IPA was added with further stirring, and the mixture was stirred at 30°C for 30 minutes. After stirring, the mixture was heated to 70°C and subjected to a carboxymethylation reaction at 70°C for 90 minutes. After the reaction was completed, the mixture was neutralized, washed with 65% aqueous methanol, deliquored, dried, and pulverized to obtain a sodium salt of carboxymethylated cellulose with a carboxymethyl substitution degree of 0.18 and a crystallinity of cellulose type I of 64%. The methods for measuring the degree of carboxymethyl substitution and the crystallinity of cellulose type I are as described above.

[0091] The sodium salt of carboxymethyl cellulose obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of carboxymethylated CNF. The obtained carboxymethylated CNF had an average fiber diameter of 8 nm and an aspect ratio of 60.

[0092] (Production Example 4) (Production of phosphorylated CNF) Bleached unbeaten kraft pulp derived from coniferous trees (brightness 85%, basis weight 245 g / m 2A phosphorus oxo-oxidation treatment was carried out on the raw pulp (sheet form) as follows. First, a mixed aqueous solution of ammonium dihydrogen phosphate and urea was added to 100 parts by mass (bone dry) of the raw pulp to adjust the total weight to 45 parts by mass of ammonium dihydrogen phosphate, 120 parts by mass of urea, and 150 parts by mass of water, to obtain a chemical-impregnated pulp. The resulting chemical-impregnated pulp was then heated in a hot air dryer at 165°C for 250 seconds to introduce phosphate groups into the cellulose in the pulp, thereby obtaining a phosphorylated pulp. 100 g of the resulting phosphorylated pulp (bone dry) was mixed with 10 L of ion-exchanged water to obtain a pulp dispersion. The pulp was stirred to uniformly disperse, and then repeatedly filtered and dehydrated for washing. The washing endpoint was reached when the electrical conductivity of the filtrate reached 100 μS / cm or less. The washed phosphorylated pulp was then diluted with 10 L of ion-exchanged water, and a 1 N aqueous sodium hydroxide solution was added little by little while stirring to obtain a phosphorylated pulp slurry with a pH of 12 to 13. The phosphorylated pulp slurry was dewatered and washed to obtain neutralized phosphorylated pulp.

[0093] The obtained phosphorylated pulp was subjected to infrared absorption spectroscopy using FT-IR. -1 The absorption due to P=O of the phosphate group was observed around the 2θ=14° to 17° angle and the 2θ=22° to 23° angle.

[0094] The phosphorylated pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a phosphorylated CNF dispersion. The obtained fibers had an average fiber diameter of 4 nm and an aspect ratio of 200.

[0095] X-ray diffraction confirmed that the obtained CNF maintained cellulose type I crystal structure. The amount of phosphate groups (amount of first dissociated acid) was 1.45 mmol / g. The total amount of dissociated acid was 2.45 mmol / g.

[0096] (Example 1) (Production of dried body) A 5.0 mass% aqueous suspension (pH 7.5) of carboxylated CNF1 (carboxy group amount: 1.7 mmol / g, average fiber diameter: 3 nm, aspect ratio: 117) obtained in Production Example 1 was prepared as anion-modified CNF, and dried using a two-fluid nozzle spray dryer (Okawahara Chemical Engineering Co., Ltd., OUDT-25) at an inlet temperature of 160°C, an outlet temperature of 70°C, a drying air flow rate of 80 kg / h, and a liquid feed rate of 54.2 kg / h to obtain a powdery dried CNF body.

[0097] The resulting dried product was classified and collected using a cyclone to obtain an anion-modified CNF powder, which had a moisture content of 4.4% by mass.

[0098] Example 2 (Production of Dried Body) The carboxymethylated CNF obtained in Production Example 3 (degree of carboxymethyl substitution: 0.18, average fiber diameter: 8 nm, aspect ratio: 60) was used as the anion-modified CNF. Carboxymethyl cellulose (manufactured by Nippon Paper Industries Co., Ltd., product name: F350HC-4, viscosity (1% by mass, 25°C, 60 rpm) approximately 3000 mPa s, degree of carboxymethyl substitution approximately 0.90) was added to a 0.7% by mass aqueous suspension of carboxymethylated CNF in an amount of 40% by mass relative to the carboxymethylated CNF (i.e., so that the solid content of carboxymethyl cellulose was 40 parts by mass per 100 parts by mass of the solid content of carboxymethylated CNF), and the mixture was stirred for 60 minutes with a TK Homomixer (12,000 rpm) to prepare an aqueous dispersion (solid content concentration 1.0%) containing carboxymethylated CNF as anion-modified CNF. The pH of this aqueous dispersion was adjusted to 9.0 with a 5% aqueous sodium hydroxide solution, and then the dispersion was dried in a spray dryer in the same manner as in Example 1. The anion-modified CNF-containing powder was obtained by classification and recovery using a cyclone. The moisture content of the obtained powder was 8.2% by mass.

[0099] Example 3: The anion-modified CNF was the phosphorylated CNF (phosphate group amount: 1.45 mmol / g, average fiber diameter: 4 nm, aspect ratio: 200) obtained in Production Example 4, and the aqueous suspension was adjusted to pH 10.2 with a 5% aqueous sodium hydroxide solution before drying. The procedure was the same as in Example 1, except that the suspension was dried using a spray dryer, and then classified and recovered using a cyclone to obtain anion-modified CNF powder. The moisture content of the resulting phosphorylated CNF powder was 8.5% by mass.

[0100] Example 4: A 5.0% by mass aqueous suspension (pH 7.5) of carboxylated CNF1 (carboxy group content: 1.7 mmol / g, average fiber diameter: 3 nm, aspect ratio: 117) obtained in Production Example 1 was prepared as anion-modified CNF. The pH was adjusted to 11.0 using 5% sodium hydroxide. This aqueous suspension was dried using a two-fluid nozzle spray dryer (Okawahara Chemical Engineering Co., Ltd., OUDT-25) at an inlet temperature of 160°C, an outlet temperature of 70°C, a drying air flow rate of 80 kg / h, and a liquid feed rate of 54.2 kg / h. The resulting suspension was then classified and recovered in a cyclone, yielding a powdered dried CNF. The moisture content of the resulting powder was 6.4% by mass.

[0101] (Example 5) A powdery dried CNF body was obtained in the same manner as in Example 4, except that 5% sodium bicarbonate was used instead of 5% sodium hydroxide to adjust the pH of the aqueous suspension before drying to 7.9. The moisture content of the obtained powder was 5.1% by mass.

[0102] Comparative Example 1 (Production of Dried Product) Carboxylated CNF2 (carboxyl group amount: 1.4 mmol / g, average fiber diameter: 4 nm, aspect ratio: 220) obtained in Production Example 2 was used as anion-modified CNF. Carboxymethyl cellulose (trade name: F350HC-4, viscosity (1%, 25°C) approximately 3000 mPa·s, degree of carboxymethyl substitution approximately 0.9) was added to a 0.7% by mass aqueous suspension of carboxylated CNF2 in an amount of 40% by mass relative to the anion-modified CNF (i.e., so that the solid content of carboxymethyl cellulose was 40 parts by mass per 100 parts by mass of the solid content of the anion-modified CNF), and the mixture was stirred for 60 minutes with a TK Homomixer (12,000 rpm) to prepare an aqueous dispersion of anion-modified CNF. The pH of this dispersion was approximately 7 to 8. This aqueous dispersion was added with 5% aqueous sodium hydroxide solution to adjust the pH to 9.0, and then coated on the drum surface of a drum dryer D0405 (manufactured by Katsuragi Kogyo Co., Ltd.) to form a thin film with a thickness of approximately 100 to 200 μm.The film was then dried at a drum surface temperature of 80°C, an internal pressure of the dryer of 2 kPa, and a drum rotation speed of 2 rpm, yielding a dried anion-modified CNF with a moisture content of 5% by mass.

[0103] The dried CNF obtained as described above was pulverized using a hammer mill (Hammer Mill TAP-3, manufactured by Tokyo Atomizer Co., Ltd.) to produce a pulverized product. The particle size of the pulverized product obtained was adjusted by adjusting the screen diameter at the outlet of the pulverizer. The pulverized product after particle size adjustment was collected using a cyclone to obtain an anion-modified CNF powder. The moisture content of the obtained powder was 8% by mass.

[0104] (Comparative Example 2) A pulverized product was obtained in the same manner as in Comparative Example 1, except that the dried product containing CNF obtained in Comparative Example 1 was pulverized using a Turbo Mill (manufactured by Freund Corporation) as the pulverizer. The particle size of the obtained pulverized product was adjusted by adjusting the gap between the rotor and the liner. The pulverized product after particle size adjustment was collected using a cyclone, and a powder containing anion-modified CNF was obtained. The moisture content of the obtained powder was 7.8% by mass.

[0105]

[0106] As can be seen from Table 1, the powders containing anion-modified cellulose nanofibers with an average fiber diameter of 3 nm to 500 nm in Examples 1 to 5, which had a moisture content of 20% by mass or less, an average particle diameter of less than 45 μm, and a cumulative 10% diameter (D10) in the volume-based particle size distribution of 10 μm or less, had high circularity and were able to suppress aggregation due to particle adhesion even when compressed during packaging. While the reason for this is unclear, it is speculated that one cause of aggregation is the re-drying of gelled regions that had absorbed moisture microscopically and locally. Because cellulose nanofibers are hydrophilic, they readily absorb water and moisture. However, adjusting the particle size to a specific particle size reduces moisture absorption, and the high circularity is thought to have reduced this aggregation. Furthermore, the initial water absorption was moderate, preventing excessive gel formation. This suggests that when the powder is used in various industries, for example, it is less susceptible to moisture effects such as humidity or steam in processes or steam resulting from evaporation of water from the powder itself, thereby suppressing gel adhesion to piping and tanks. Furthermore, both the loose bulk density and the packed bulk density were high, and furthermore, the transfer efficiency was excellent and the transfer cost was low. On the other hand, the anion-modified cellulose nanofiber powders of Comparative Examples 1 and 2, which had a large average particle size and D10, had a low circularity and aggregated due to compression during packaging. In addition, an excessive gel layer was formed due to rapid water absorption. Furthermore, both the loose bulk density and the packed bulk density were low, the transfer efficiency was low, the transfer cost was poor, and the redispersibility during weak stirring was poor.

Claims

1. A powder containing anion-modified cellulose nanofibers having an average fiber diameter of 3 nm to 500 nm, a moisture content of 20 mass% or less, an average particle diameter of less than 45 μm, and a cumulative 10% diameter (D10) in a volume-based particle diameter distribution of 10 μm or less.

2. The powder containing anion-modified cellulose nanofibers according to claim 1, having an angle of repose of 40 to 55°.

3. The powder containing anion-modified cellulose nanofibers according to claim 1, having a collapse angle of 20 to 28°.

4. The anionically modified cellulose nanofiber-containing powder according to claim 1, wherein the difference angle is 20 to 30°.

5. The powder according to any one of claims 1 to 4, which has a pH of 8 or higher when dispersed in 1% water.

Citation Information

Patent Citations

  • Method for producing cellulose nanofiber dry solid

    WO2019189318A1

  • Cellulose powder

    JP2018016818A

  • Dried cellulose fiber and method for producing the same, and method for producing resin composite

    JP2021169577A

  • Method for producing dried cellulose fiber and method for producing resin composite

    JP2021169578A

  • Dried cellulose fiber and method for producing the same, and method for producing resin composite

    JP2021169579A