Silicon nitride powder and resin composition using same

The use of silicon nitride powder with enhanced properties as a filler in resin compositions addresses the limitations of thermal diffusivity in current heat dissipation materials, improving heat dissipation efficiency in electronic components by enhancing thermal conductivity and structural integrity.

WO2024202726A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006266
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current resin compositions used for heat dissipation in electronic components have limitations in thermal diffusivity, particularly with the increasing heat generation in high-integration ICs and high-current electronic devices, necessitating further improvements in thermal conductivity and diffusivity.

Method used

A silicon nitride powder with specific properties, including high β conversion rate, breaking strength, and particle morphology, is used as a filler in a resin composition to enhance thermal diffusivity, characterized by a ratio of displacement at the breaking point to maximum displacement greater than 0.22, strength at maximum displacement over 3473 MPa, and a β conversion rate of 65% or more, along with a manufacturing method involving combustion synthesis and heat treatment.

Benefits of technology

The silicon nitride powder significantly improves the thermal diffusivity of the resin composition, making it more effective in heat dissipation by maintaining structural integrity and promoting efficient heat conduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006266_03102024_PF_FP_ABST
    Figure JP2024006266_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A purpose of the present invention is to provide a silicon nitride powder used as a filler for a resin composition and capable of improving the thermal diffusivity of the resin composition. The present invention pertains to a silicon nitride powder containing a plurality of silicon nitride particles, wherein the silicon nitride particles satisfy one or more selected from the group consisting of the following (i) and (ii) in a particle compression test. (i) The ratio of the displacement of the fracture point to the maximum displacement is more than 0.22. (ii) The strength at the maximum displacement is more than 3473 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride powder and resin composition using same

[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.

[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a low-aluminum spherical β-silicon nitride powder for use as a filler in electronic packaging materials, characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 μm to 50 μm.

[0004] Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies, and silicon nitride powder obtained by said method. The silicon nitride powder has an average particle size of 1 to 50 μm, a metal oxide content of 0 to 10 wt %, and an impurity content of less than 1 wt %. Preferably, the metal oxide content in the silicon nitride powder is less than 1 wt %. The obtained sintered body has a thermal conductivity of 90 W / mK or more and a bending strength of 700 MPa or more. Preferably, the sintering conditions for the sintered body are as follows: the silicon nitride powder is mixed with MgO, Y 2 O 3 The powder is mixed with the above powder, polished, and the powder is dry-press molded, and the powder is gas-pressure sintered at 1900°C and a nitrogen gas pressure of 1 MPa for 8 hours.

[0005] Patent Document 3 discloses a silicon nitride powder suitable for producing high thermal conductivity silicon nitride sintered bodies. The silicon nitride powder is characterized by having a β fraction of 30 to 100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2 to 10 μm, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.

[0006] JP 2022-522814 A JP 2022-541208 A JP 2004-262756 A

[0007] In recent years, the increase in heat generation in ICs due to the high integration of ICs in electronic devices and the increase in heat generation in electronic components due to the use of high-current-driven electronic components due to the electrification of electric vehicles, aircraft, etc. have become problems. In order to achieve more effective heat dissipation, there is a demand for further improvement in the thermal diffusivity of resin compositions.

[0008] In Patent Document 1, increasing the sphericity of silicon nitride powder (i.e., making it into spherical particles) enables high loading into a resin composition, thereby improving the thermal diffusivity of the resin composition. However, there is still room for further investigation to further improve the thermal diffusivity.

[0009] The silicon nitride powders in Patent Documents 2 and 3 disclose silicon nitride powders for use in silicon nitride sintered bodies, and therefore do not discuss mixing them with resins to form resin compositions, nor do they discuss silicon nitride powders suitable as fillers for resin compositions.

[0010] In view of these circumstances, an object of an embodiment of the present invention is to provide a silicon nitride powder for use as a filler for a resin composition, which can improve the thermal diffusivity of the resin composition. Furthermore, an object of another embodiment of the present invention is to provide a resin composition using the silicon nitride powder.

[0011] A first aspect of the present invention is a silicon nitride powder comprising a plurality of silicon nitride particles, wherein the silicon nitride particles have a ratio of the displacement at the breaking point to the maximum displacement in a particle compression test of greater than 0.22.

[0012] Aspect 2 of the present invention is the silicon nitride powder according to aspect 1, wherein the silicon nitride particles have a breaking strength of more than 727 MPa in a compression test of the particles.

[0013] Aspect 3 of the present invention is a granular ... 3 3. The silicon nitride powder according to claim 1, wherein the silicon nitride powder has a molecular weight of 1.0 or more.

[0014] A fourth aspect of the present invention is the silicon nitride powder according to any one of the first to third aspects, wherein the β-phase ratio is 65% or more.

[0015] A fifth aspect of the present invention is the silicon nitride powder according to any one of the first to fourth aspects, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0016] Aspect 6 of the present invention is the silicon nitride powder according to any one of Aspects 1 to 5, wherein the silicon nitride particles have a strength at maximum displacement of more than 3473 MPa in a compression test of the particles.

[0017] A seventh aspect of the present invention is the silicon nitride powder according to any one of the first to sixth aspects, wherein the silicon nitride particles have a ratio of fracture strength to strength at maximum displacement of 0.18 or more in a compression test of the particles.

[0018] An eighth aspect of the present invention is the silicon nitride powder according to any one of the first to seventh aspects, which satisfies the following formula (1): (|a - 23.34| / 23.34 + |b - 27.01| / 27.01 + |c - 33.63| / 33.63 + |d - 36.02| / 36.02) / 4 < 0.292 (1) In formula (1), a, b, c, and d are the diffraction angles 2θ (°) corresponding to the (110), (200), (101), and (210) planes of β-silicon nitride, respectively, in an X-ray diffraction pattern using CuKα radiation as an X-ray source.

[0019] A ninth aspect of the present invention is a silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride particles having a strength at maximum displacement of more than 3473 MPa in a particle compression test.

[0020] A tenth aspect of the present invention is the silicon nitride powder according to the ninth aspect, wherein the silicon nitride particles have a ratio of breaking strength to strength at maximum displacement of 0.18 or more in a compression test of the particles.

[0021] An eleventh aspect of the present invention is the silicon nitride powder according to the ninth or tenth aspect, which satisfies the following formula (1): (|a - 23.34| / 23.34 + |b - 27.01| / 27.01 + |c - 33.63| / 33.63 + |d - 36.02| / 36.02) / 4 < 0.292 (1) In formula (1), a, b, c, and d are the diffraction angles 2θ (°) corresponding to the (110), (200), (101), and (210) planes of β-silicon nitride, respectively, in an X-ray diffraction pattern using CuKα radiation as an X-ray source.

[0022] Aspect 12 of the present invention is a granular ... 3 12. The silicon nitride powder according to any one of Aspects 9 to 11, wherein the silicon nitride powder has a molecular weight of 1000 or more.

[0023] A thirteenth aspect of the present invention is the silicon nitride powder according to any one of the ninth to twelfth aspects, wherein the β-phase ratio is 65% or more.

[0024] Aspect 14 of the present invention is the silicon nitride powder according to any one of Aspects 9 to 13, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0025] Aspect 15 of the present invention is the silicon nitride powder according to any one of Aspects 9 to 14, wherein the silicon nitride particles have a ratio of the displacement at the breaking point to the maximum displacement in a compression test of the particles of greater than 0.22.

[0026] Aspect 16 of the present invention is the silicon nitride powder according to any one of Aspects 9 to 15, wherein the silicon nitride particles have a breaking strength of more than 727 MPa in a compression test of the particles.

[0027] A seventeenth aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to sixteenth aspects.

[0028] By using the silicon nitride powder according to the embodiment of the present invention as a filler, a resin composition having a high thermal diffusivity can be obtained.

[0029] 1 is an example of a plot of displacement (μm) vs. strength (MPa) obtained by carrying out a particle compression test on silicon nitride particles in accordance with JIS R1639-5.

[0030] [Silicon Nitride Powder] The present inventors have investigated silicon nitride powders used as fillers in resin compositions from various perspectives in order to achieve more effective heat dissipation. As a result, they have found that when the silicon nitride particles in the silicon nitride powder satisfy one or more of the following conditions (i) and (ii), the silicon nitride particles are less likely to break, for example, during the production of a resin composition, resulting in a resin composition with high thermal diffusivity: (i) the ratio of the displacement at the breaking point to the maximum displacement is greater than 0.22; (ii) the strength at the maximum displacement is greater than 3473 MPa. Hereinafter, a first embodiment of the present invention will be defined as one that satisfies at least (i), and a second embodiment of the present invention will be defined as one that satisfies at least (ii), and each of these requirements will be described in detail. In this specification, "an embodiment of the present invention" includes both "embodiment 1 of the present invention" and "embodiment 2 of the present invention."

[0031] <Embodiment 1 of the Present Invention> (Ratio of Displacement at Breaking Point to Maximum Displacement) The silicon nitride powder according to embodiment 1 of the present invention comprises a plurality of silicon nitride particles, and in a particle compression test, the silicon nitride particles have a ratio of the displacement at breaking point to the maximum displacement (i.e., the maximum value of the displacement in the particle compression test) of greater than 0.22. This makes the silicon nitride particles less susceptible to fracture, for example, during the production of a resin composition, resulting in a resin composition with high thermal diffusivity. This ratio is preferably 0.24 or more, more preferably 0.26 or more, and particularly preferably 0.27 or more. The upper limit of this ratio is not particularly limited, but from the viewpoint of productivity, it may be 0.60 or less, 0.50 or less, 0.40 or less, or 0.35 or less.

[0032] The ratio of the displacement at the breaking point to the maximum displacement of the silicon nitride particles is measured as follows. First, a compression test of the silicon nitride particles is conducted in accordance with JIS R1639-5 to obtain a plot of displacement vs. test force. The test force of the plot is converted to strength based on the following formula (2) to obtain a plot of displacement (μm) vs. strength (MPa) as shown in FIG. 1. Strength (MPa) = 2.48 × test force (N) / (π × D 2 ) (2) where D is the average value of the major and minor diameters of the silicon nitride particles to be tested. The major and minor diameters can be measured by observation with an optical microscope.

[0033] In FIG. 1, if there is one region where the slope is constant, the minimum displacement where the displacement exceeds 0 and the slope is constant is defined as the breaking point P 1 The displacement is from 0 to the breaking point P 1 The region up to the breaking point P is the elastic deformation region (indicated by the double arrow). 1 Displacement d in 1 (i.e., the maximum displacement in the elastic deformation region) and the maximum displacement d 2 (i.e., maximum displacement point P 2 the ratio d 1 / d 2 is calculated as the "ratio of the displacement of the breaking point to the maximum displacement." If there are multiple regions with a constant slope, the displacement of the starting point of the region where the difference between the displacement of the end point and the displacement of the starting point of the region is the largest is calculated as the breaking point P 1 Let's say.

[0034] (Breaking Strength) In the silicon nitride powder according to embodiment 1 of the present invention, the silicon nitride particles preferably have a breaking strength of more than 727 MPa in a particle compression test. This makes the silicon nitride particles less susceptible to breaking, resulting in a resin composition with high thermal diffusivity. The breaking strength is more preferably 750 MPa or more, even more preferably 800 MPa or more, and particularly preferably 850 MPa or more. There is no particular upper limit to the breaking strength, but from the viewpoint of productivity, it may be 3000 MPa or less, less than 2750 MPa, 2000 MPa or less, or 1500 MPa or less.

[0035] The breaking strength of silicon nitride particles is measured as follows: A compression test of silicon nitride particles is carried out in accordance with JIS R1639-5, and a plot of displacement (μm) vs. strength (MPa) is obtained as shown in Figure 1. In the plot, the breaking point P 1 The strength of the breaking strength s 1 (MPa).

[0036] (Apparent Density) The apparent density of the silicon nitride powder according to embodiment 1 of the present invention is 3.17 g / cm 3 It is preferable that the density is greater than 3.18 g / cm 3 This results in a silicon nitride powder containing many silicon nitride particles with a small amount of internal voids, that is, a silicon nitride powder that is difficult to break and has high thermal diffusivity and thermal conductivity. The upper limit of the apparent density is, for example, 3.44 g / cm 3 In addition, if the apparent density is not too high, it is expected that the powder will be less likely to settle when mixed with a resin and will be easier to disperse. In order to achieve such an effect, the apparent density of the silicon nitride powder should be 3.30 g / cm 3 It is preferable that the density is 3.25 g / cm or less, and more preferably 3.25 g / cm 3 The following is the result.

[0037] The apparent density of the silicon nitride powder is measured by the pycnometer method in accordance with JIS R 1620:1995. The measurement is carried out five or more times, and the average value is taken as the apparent density of the silicon nitride powder. For the measurement, for example, an Accupyc 1330 (Micromeritics) can be used.

[0038] (β-phase ratio) The β-phase ratio of the silicon nitride powder according to embodiment 1 of the present invention is preferably 65% ​​or more. A β-phase ratio of 65% or more can improve the thermal diffusivity of the silicon nitride powder and the resin composition. The β-phase ratio is more preferably 70% or more, even more preferably 80% or more, even more preferably 85% or more, and particularly preferably 90% or more.

[0039] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.

[0040] In calculating the β-phase ratio, a diffraction pattern of silicon nitride powder was obtained by powder X-ray diffraction (X-ray source: CuKα ray), and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4 The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).

[0041] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) In embodiment 1 of the present invention, the fewer grain boundaries and cavities there are inside the silicon nitride particles, the more this can contribute to improving the thermal diffusivity of the silicon nitride particles. Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an indicator of the content of grain boundaries inside the silicon nitride particles. L1 and L2 are determined by observing the cross section of the silicon nitride particle. Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where, as a result of EBSD analysis, the crystal orientation misorientation (oblique angle) exceeds 15°.

[0042] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundaries of that silicon nitride particle is L2, silicon nitride particles with a small value of L2 / L1 can be said to have a low content of boundaries. In embodiment 1 of the present invention, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles consisting of a single crystal (referred to as "single crystal particles"). Single crystal particles are resistant to fracture and have a high thermal diffusivity, which makes it easy to improve thermal diffusivity when used as a filler for resin compositions.

[0043] In embodiment 1 of the present invention, the maximum particle size of silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 10.0 μm or more, even more preferably 15.0 μm or more, and even more preferably 25.0 μm or more. Such silicon nitride particles are resistant to fracture and form long thermal conduction paths when filled into a resin, thereby improving the thermal diffusivity of the resin composition. The upper limit is not particularly limited, but may be, for example, 200.0 μm or less, 100.0 μm or less, or 80.0 μm or less.

[0044] (Elastic absorption energy) In the silicon nitride powder according to embodiment 1 of the present invention, the silicon nitride particles preferably have an elastic deformation absorption energy (also referred to as elastic absorption energy) of more than 490 (MPa μm) in a particle compression test. This is thought to allow the silicon nitride particles to store a large amount of energy imparted in the compression test, maintain elasticity, and become less susceptible to breakage. The elastic absorption energy is preferably 500 (MPa μm) or more, particularly preferably 600 (MPa μm) or more. There is no particular upper limit to the elastic absorption energy, but from the viewpoint of productivity, it may be 3000 (MPa μm) or less, less than 2500 (MPa μm), or 2000 (MPa μm) or less.

[0045] The elastic absorption energy of silicon nitride particles is calculated as follows. A compression test of silicon nitride particles is carried out in accordance with JIS R1639-5, and a plot of displacement (μm) vs. strength (MPa) is obtained as shown in Figure 1. In Figure 1, the plot, the line representing strength = 0 MPa, and the line representing displacement = d 1 The area of ​​the region surrounded by the line and the shaded area is calculated as the elastic absorption energy (MPa·μm).

[0046] The requirements for the silicon nitride powder according to embodiment 1 of the present invention have been described above. The requirements for the silicon nitride powder according to embodiment 2 of the present invention will be described below. Note that the silicon nitride powder according to embodiment 1 of the present invention may further satisfy the following requirements for the silicon nitride powder according to embodiment 2 of the present invention, which can further improve the properties.

[0047] <Embodiment 2 of the Present Invention> (Strength at Maximum Displacement) The silicon nitride powder according to embodiment 2 of the present invention comprises a plurality of silicon nitride particles, and in a particle compression test, the silicon nitride particles have a strength at maximum displacement of more than 3473 MPa. This makes the silicon nitride particles less susceptible to fracture, for example, during the production of a resin composition, resulting in a resin composition with high thermal diffusivity. The strength at maximum displacement is preferably 3500 MPa or more, more preferably 3700 MPa or more. There is no particular upper limit to the strength at maximum displacement, but from the viewpoint of productivity, it may be 20,000 MPa or less, less than 15,000 MPa, or 7,000 MPa or less.

[0048] The strength of silicon nitride particles at the maximum displacement is measured as follows: A compression test of silicon nitride particles is carried out in accordance with JIS R1639-5, and a plot of displacement (μm) vs. strength (MPa) is obtained as shown in Figure 1. In the plot, the maximum displacement point P 2 The intensity at the maximum displacement s 2 (MPa).

[0049] (Ratio of breaking strength to strength at maximum displacement) In the silicon nitride powder according to embodiment 2 of the present invention, the silicon nitride particles preferably have a ratio of breaking strength to strength at maximum displacement of 0.18 or more in a particle compression test. This makes the silicon nitride particles less susceptible to fracture. This ratio is more preferably 0.20 or more, even more preferably greater than 0.21, even more preferably 0.22 or more, and particularly preferably greater than 0.22. There is no particular upper limit to this ratio, but from the viewpoint of productivity, it may be 0.60 or less, or 0.50 or less.

[0050] The ratio of the fracture strength to the strength at the maximum displacement of silicon nitride particles is measured as follows: A compression test of silicon nitride particles is carried out in accordance with JIS R1639-5, and a plot of displacement (μm) vs. strength (MPa) is obtained as shown in Figure 1. The fracture point P 1 Strength (breaking strength) at s 1 (MPa) and the maximum displacement point P 2 Intensity s at 2 (MPa) and the ratio s 1 / s 2 is defined as the "ratio of fracture strength to strength at maximum displacement."

[0051] (Average shift amount of diffraction angle corresponding to the (110), (200), (101) and (210) planes of β-type silicon nitride) The silicon nitride powder according to the second embodiment of the present invention is preferably one having fewer strains and defects in order to improve thermal diffusivity, and for example, the silicon nitride powder according to the second embodiment of the present invention preferably satisfies the following formula (1): (|a-23.34| / 23.34+|b-27.01| / 27.01+|c-33.63| / 33.63+|d-36.02| / 36.02) / 4<0.292 (1) In formula (1), a, b, c, and d are diffraction angles (2θ / °) corresponding to the (110) plane, (200) plane, (101) plane, and (210) plane (or (120) plane) of β-silicon nitride, respectively, in an X-ray diffraction pattern using CuKα rays as an X-ray source. In the formula (1), "23.34", "27.01", "33.63", and "36.02" are literature values ​​of the diffraction angles (2θ / °) of the (110), (200), (101), and (210) planes of β-type silicon nitride, respectively.

[0052] By satisfying the above formula (1), β-type silicon nitride with few defects and distortion can be obtained, which is thought to contribute to improving thermal diffusivity. The left side of the above formula (1) is more preferably 0.290 or less, and even more preferably 0.250 or less. The lower limit of the left side of the above formula (1) is not particularly limited, but from the viewpoint of productivity, it may be 0.005 or more, 0.010 or more, or 0.100 or more. In the above, the X-ray diffraction pattern of the silicon nitride powder can be obtained by powder X-ray diffraction (X-ray source: CuKα radiation).

[0053] (Apparent Density) The content is the same as that described in <Embodiment 1 of the present invention>, so it will be omitted.

[0054] (β Rate) This is the same as that described in <Embodiment 1 of the present invention>, so it will be omitted.

[0055] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge of 1% or less is 6.8 μm or more.) This is the same as the content described in <Embodiment 1 of the present invention>, so it will be omitted.

[0056] (Elastic Absorption Energy) This is the same as that described in <Embodiment 1 of the Present Invention>, so a description thereof will be omitted.

[0057] The requirements for the silicon nitride powder according to embodiment 2 of the present invention have been described above. The silicon nitride powder according to embodiment 2 of the present invention may further satisfy the requirements for the silicon nitride powder according to embodiment 1 of the present invention described above, thereby further improving the properties.

[0058] [Method for Producing Silicon Nitride Powder] The silicon nitride powder according to an embodiment of the present invention can be produced by a production method including the steps of: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si, (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder, (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder, and (4) heat-treating the finely pulverized silicon nitride powder to obtain silicon nitride powder. Each step is described in detail below.

[0059] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.

[0060] The diluent is used to adjust the amount of Si in the raw materials. A separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. For example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10 mass% of the total raw materials (including the diluent). For example, the diluent is added in an amount of 5 to 8 mass% of the total raw materials. By keeping the amount of diluent added within the above range, it becomes easier to obtain silicon nitride powder with a predetermined displacement (μm)-strength (MPa).

[0061] In an embodiment of the present invention, a diluent is mixed with the raw materials and then filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred in consideration of the risk of impurities being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and no more than 150 mm. Combustion synthesis is performed under a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within the above range enables efficient synthesis while suppressing increases in equipment costs.

[0062] When the mixed raw material is filled into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is laid on the bottom and sides of the crucible, the mixed raw material is then filled, and the top surface is covered with a layer of powder having a thickness of 1 mm to 80 mm. The thickness of the powder is 100 mm or less, preferably 1 mm to 80 mm. Covering the powder with the powder keeps the mixed raw material warm, making it easier to obtain silicon nitride powder having a predetermined displacement (μm)-strength (MPa).

[0063] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.

[0064] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).

[0065] Step (3): Obtaining Finely Pulverized Silicon Nitride Powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. Pulverization is performed using a pulverizing device such as a jet mill or a ball mill. If necessary, the resulting finely pulverized powder may be classified. Classification can be performed by sieving, wet classification, or the like. Wet classification produces dense silicon nitride, which makes it easier to obtain silicon nitride particles with a high ratio of fracture point displacement to maximum displacement in particle compression tests. Furthermore, adjusting the number of classifications to an optimal range adjusts the external energy applied to the silicon nitride particles, thereby making it easier to obtain silicon nitride particles with high strength at maximum displacement in particle compression tests.

[0066] Step (4): Step of Obtaining Silicon Nitride Powder The finely pulverized silicon nitride powder is heat-treated to obtain silicon nitride powder. The heat treatment forms an oxide film on the surface of the silicon nitride particles, chemically stabilizing the silicon nitride particles. The heat treatment is carried out in air at a temperature of 500°C or higher and 1200°C or lower, preferably higher than 800°C and lower than 1100°C. The heat treatment time can be adjusted appropriately depending on the heat treatment temperature. The heat treatment time is, for example, 5 hours.

[0067] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to the embodiment of the present invention can be produced by crushing, classifying, and pulverizing the synthesized silicon nitride crystals.

[0068] [Resin Composition] The resin composition according to the embodiment of the present invention contains a resin and the silicon nitride powder according to the embodiment of the present invention. The resin / silicon nitride powder blending ratio of the resin composition according to the embodiment of the present invention can be appropriately determined depending on the purpose and / or application. As an example, the resin composition (composite) may contain 5 to 75 volume % of resin and 95 to 25 volume % of silicon nitride powder. The filling rate of the silicon nitride powder in the resin composition refers to the content (vol %) of the silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.

[0069] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.

[0070] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.

[0071] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.

[0072] The silicon nitride powder according to the embodiment of the present invention and a resin composition containing the silicon nitride powder are particularly suitable for use as a heat-dissipating material. Thus, one aspect of the present disclosure can provide a heat-dissipating silicon nitride powder and a heat-dissipating resin composition.

[0073] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.

[0074] <Preparation of Silicon Nitride Powder> Si powder (particle size = 5 μm) and silicon nitride powder (particle size = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5 to 8 mass% of the total raw materials (including diluent). The mixed powder was filled into a carbonaceous, heat-resistant container with a layer of powder 1 mm to 80 mm thick on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was then covered with a layer of powder 1 mm to 80 mm thick. A lid made of a carbonaceous, heat-resistant material was then placed in the container, and synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve for each sample is shown in Table 1.

[0075] The obtained coarsely pulverized powder was further pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). A nanojetmizer with the model number listed in Table 1 was used for pulverization. The obtained pulverized powder was classified using the method listed in Table 1. Note that a portion of the pulverized powder (referred to as sample No. 2) was not classified. The D50 of the classified powder of the obtained sample No. 5 was 12.0 μm, and the D50 of the classified powder of sample No. 6 was 25.2 μm. The obtained classified powders (samples No. 1, No. 3, No. 5, and No. 6) and the pulverized powder (sample No. 2) were then placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) listed in Table 1 to obtain silicon nitride powders (samples Nos. 1 to 3, 5, and 6).

[0076]

[0077] Various measurements were performed on the obtained Samples Nos. 1 to 3, 5, and 6 (Examples) and, as a comparative example, a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as “Sample No. 4”).

[0078] (1) Maximum displacement d 2 Displacement d of the breaking point relative to 1 The ratio d 1 / d 2 A compression test was conducted on silicon nitride particles in a sample (silicon nitride powder) in accordance with JIS R1639-5, and a plot of displacement vs. test force was obtained. The test force on the plot was converted to strength based on the following formula (2), and a plot of displacement (μm) vs. strength (MPa) was obtained. Strength (MPa) = 2.48 × test force (N) / (π × D 2 ) (2) where D is the average value of the major and minor diameters of the silicon nitride particles to be tested. The major and minor diameters were measured by observation with an optical microscope.

[0079] In the plot of displacement (μm) vs. strength (MPa), the minimum displacement where the displacement exceeds 0 and the slope is 0 is defined as the fracture point P1 and the breaking point P 1 Displacement d in 1 and maximum displacement d 2 (i.e., maximum displacement point P 2 the ratio d 1 / d 2 was calculated.

[0080] (2) Breaking strength s 1 In the above displacement (μm)-strength (MPa) plot, the breaking point P 1 The strength of the sample (silicon nitride powder) is calculated as the breaking strength s of the silicon nitride particles. 1 (MPa).

[0081] (3) Apparent Density The apparent density of the sample (silicon nitride powder) was measured in accordance with JIS R 1620:1995. The measurement method and conditions were as follows: Measurement method: Gas substitution method Sample drying: 200°C, 8 hours or more Apparatus used: Accupyc 1330 (Micromeritics) Measurement conditions Number of purges: 10 Purge filling pressure: 15.0 psig Number of measurements: 5 Measurement filling pressure: 15.0 psig Equilibrium pressure: 0.005 psig / min Measurement with set precision: Yes Allowable error of variation: 0.05% Sample cell size: 10 cm 3

[0082] (4) β-Proportion The X-ray diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation; X-ray output: 45 kV, 200 mA; graphite monochromator; diffraction angle (2θ): step scan in 0.02° increments in the range of 2 to 90°; scanning speed: 21.7 deg / min.

[0083] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 to 6, the powder X-ray diffraction patterns obtained confirmed that the samples were composed solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.

[0084] (5) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A ​​cross-sectional observation specimen was prepared using the sample (silicon nitride particles). To prepare the cross-sectional observation specimen, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The specimen was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.

[0085] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)

[0086] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa

[0087] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner wall of the cavity (if there was a cavity within the silicon nitride particle). Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where the crystal orientation misorientation (oblique angle) exceeds 15° as a result of EBSD analysis.

[0088] This measurement was carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.

[0089] (6) Elastic absorption energy The above displacement (μm)-strength (MPa) plot, the strength = 0 MPa line, and the displacement = d 1 The area of ​​the region surrounded by the line and the shaded area was calculated as the elastic absorption energy (MPa·μm) of the silicon nitride particles in the sample (silicon nitride powder).

[0090] (7) Strength s at maximum displacement 2 In the above displacement (μm)-strength (MPa) plot, the maximum displacement point P 2 The intensity at the maximum displacement s 2 (MPa).

[0091] (8) Strength s at maximum displacement 2 Breaking strength s 1 The ratio s 1 / s 2 In the above displacement (μm)-strength (MPa) plot, the breaking point P 1 Strength (breaking strength) at s 1 (MPa) and the maximum displacement point P 2 Intensity s at 2 (MPa) and the ratio s 1 / s 2 was calculated.

[0092] (9) Average shift amount of diffraction angle corresponding to the (110), (200), (101), and (210) planes of β-type silicon nitride In the above X-ray diffraction pattern, a, b, c, and d were obtained as the diffraction angles (2θ / °) corresponding to the (110), (200), (101), and (210) planes (or (120) planes) of β-type silicon nitride, respectively. The obtained values ​​a to d were substituted into the above formula (1), and the value of the left side of the above formula (1) was calculated.

[0093] (10) Thermal diffusivity of resin composition (composite) Epoxy resin (main agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8140, curing agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8143) and a sample (silicon nitride powder) were mixed in a blending ratio (volume ratio) of 50:50, and the mixture was stirred and mixed using a Foam Mixer (manufactured by Thinky Corporation) to obtain an epoxy resin-filler (silicon nitride powder) composite. The filling rate of the silicon nitride powder in the resin composition was 50% by volume.

[0094] A 1 mm thick aluminum plate with a 1 cm x 10 cm rectangular hole was prepared as a mold frame. A PET film (back side film) coated with a release agent was attached to the back side of the mold frame so as to cover the rectangular hole, with the release agent-coated surface facing the mold frame. After the stirred composite was poured into the rectangular hole of the mold frame, a PET film (front side film) coated with a release agent was attached on top of it, with the release agent-coated surface facing the mold frame and resin composition. Furthermore, light pressure was applied from above with a metal roller to fit the composite into the rectangular hole of the mold frame. Another aluminum plate was placed on top of the front side film, and the composite was cured by heating at 100°C for 1 hour. After curing was complete, the aluminum plate was allowed to cool, and when the temperature of the aluminum plate had dropped to approximately room temperature, the aluminum plate was removed. The PET films on the front and back sides of the cured composite were then peeled off, respectively, to obtain a sheet-like sample for measuring thermal diffusivity.

[0095] The thermal diffusivity of the obtained sheet-like sample was measured. Measurement specimens measuring 10 mm in length, 10 mm in width, and 1 mm in thickness were prepared from the sheet-like sample of the resin composition described above, and the thermal diffusivity was measured at room temperature using temperature wave thermal analysis (TWA). The measurement device used was an iPhase Mobile manufactured by iPhase Corporation. The thermal diffusivity was measured at three random points on one measurement specimen, and the average value was calculated from the measurement results of the three points.

[0096] The measurement results are summarized in Tables 2 and 3.

[0097]

[0098]

[0099] The measurement results are discussed below. The resin compositions using the silicon nitride powder of Samples Nos. 1 to 3, 5, and 6, which satisfied the requirements of Embodiment 1 and / or Embodiment 2 of the present invention, exhibited excellent thermal diffusivity. On the other hand, the resin composition using the silicon nitride powder of Sample No. 4, which did not satisfy the requirements of Embodiments 1 and 2 of the present invention, exhibited poor thermal diffusivity.

[0100] This application claims priority from Japanese Patent Application No. 2023-058730, filed March 31, 2023. Japanese Patent Application No. 2023-058730 is incorporated herein by reference.

Claims

1. A silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride particles having a ratio of the displacement at the breaking point to the maximum displacement in a particle compression test of greater than 0.

22.

2. The silicon nitride powder according to claim 1, wherein the silicon nitride particles have a breaking strength of more than 727 MPa in a compression test of the particles.

3. A silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride particles having a strength at maximum displacement of greater than 3473 MPa in a particle compression test.

4. The silicon nitride powder according to claim 3, wherein the silicon nitride particles have a ratio of breaking strength to strength at the maximum displacement of 0.18 or more in a compression test of the particles.

5. The silicon nitride powder according to claim 3 or 4, which satisfies the following formula (1): (|a-23.34| / 23.34+|b-27.01| / 27.01+|c-33.63| / 33.63+|d-36.02| / 36.02) / 4<0.292 ... (1) In formula (1), a, b, c and d are diffraction angles (°) corresponding to the (110), (200), (101) and (210) planes of β-type silicon nitride, respectively, in an X-ray diffraction pattern using a CuKα ray as an X-ray source.

6. Apparent density is 3.17 g / cm 3 The silicon nitride powder according to claim 1 or 3, wherein the silicon nitride powder has a molecular weight of more than 10000.

7. Silicon nitride powder according to claim 1 or 3, having a β-conversion rate of 65% or more.

8. The silicon nitride powder according to claim 1 or 3, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary line to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

9. A resin composition comprising a resin and the silicon nitride powder according to claim 1 or 3.

Citation Information

Patent Citations

  • Method of producing high purity silicon nitride powder

    JP2020023406A

  • Ultra-pure, low-radioactivity spherical β silicon nitride powder, its manufacturing method and applications

    JP2022522311A

  • Columnar particles of β-silicon nitride, composite particles, sintered substrate for heat radiation, resin composite, inorganic composite, method for producing columnar particles of β-silicon nitride, and method for producing composite particles