Insert molded body, anchor for attaching seat belt, and method for producing insert molded body

By integrating a core-shell elastomer with controlled particle size into the polyacetal resin composition and optimizing the resin to metal thickness ratio, the insert molded body's weld elongation is enhanced, addressing cracking issues and improving durability for applications such as seat belt anchors.

WO2024202730A1PCT designated stage expired Publication Date: 2024-10-03GLOBAL POLYACETAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006279
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Insert molded bodies made of polyacetal resin and metal parts are prone to cracking due to differences in linear expansion coefficients and contraction rates, often resulting in weld failures.

Method used

Incorporating a core-shell elastomer with a maximum secondary particle diameter of 1000 nm or less into the polyacetal resin composition, along with a three-layer structure and specific ratios of resin to metal thickness, to enhance weld elongation and reduce cracking risk.

Benefits of technology

The solution effectively increases weld elongation and reduces cracking in the resin part, making the insert molded article more durable and suitable for applications like seat belt attachment anchors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006279_03102024_PF_FP_ABST
    Figure JP2024006279_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This insert molded body has: a resin part formed from a resin composition containing a polyacetal resin and an elastomer; and a metal part. The elastomer includes a core-shell type elastomer. The content of polyurethane is less than 1 mass% relative to 100 mass% of the resin composition. The maximum secondary particle diameter of the core-shell type elastomer in the resin part is 1000 nm or less. The ratio of the thickness of the resin part and the thickness of the metal part in the insert molded body (resin part / metal part) has a minimum value of 1.5 or less. Also provided are: an anchor for attaching a seat belt, which is obtained using the insert molded body; and a method for producing the insert molded body.
Need to check novelty before this filing date? Find Prior Art

Description

Insert molding, seat belt anchor, and method for manufacturing insert molding

[0001] The present invention relates to an insert-molded article, a seat belt anchor, and a method for manufacturing an insert-molded article, and more particularly to an insert-molded article containing a polyacetal resin as a main component.

[0002] Polyacetal resins have high mechanical strength and rigidity, excellent oil resistance and organic solvent resistance, a well-balanced resin over a wide temperature range, and are easy to process. Therefore, polyacetal resins are widely used as a representative engineering plastic in office automation equipment, digital home appliances, automobile parts, and other industrial parts.

[0003] One known application of polyacetal resin is an insert-molded article of polyacetal resin and a metal part. For example, Patent Document 1 discloses a metal insert-molded article characterized by containing a polyacetal resin composition containing 100 parts by mass of polyacetal resin having a melt flow rate of 1.0 to 5.0 g / 10 min, 0.01 to 5 parts by mass of a hydrazide compound, 0.01 to 1 part by mass of polyethylene glycol, and a color pigment.

[0004] Japanese Patent Application Laid-Open No. 2022-098154

[0005] In insert-molded articles made of a resin part and a metal part formed from polyacetal resin, cracks are likely to occur in the resin part. This is due to stress caused by differences in the linear expansion coefficient and shrinkage rate between the resin part and the metal part. Furthermore, when cracks do occur, they tend to occur in the weld part of the resin part. That is, in insert-molded articles, it is required that the weld elongation of the resin part is high and that cracks are less likely to occur. The present invention aims to solve this problem and to provide an insert-molded article made of a resin part and a metal part, which has high weld elongation and is less likely to crack, as well as a seat belt attachment anchor and a method for manufacturing the insert-molded article.

[0006] In light of the above-mentioned problem, the present inventors conducted research and found that, among the causes of cracking in the resin part, stress generated by differences in the linear expansion coefficient and shrinkage rate between the resin part and the metal part is the cause. To address this stress, they attempted to use a soft polyacetal resin. That is, rather than reducing the generated stress, they considered using a soft polyacetal resin to alleviate the generated stress. However, they found that blending an elastomer to impart flexibility to the polyacetal resin can sometimes reduce weld elongation. Under these circumstances, the present inventors conducted further research and found that the above-mentioned problem could be solved by selecting a core-shell elastomer as the elastomer, adjusting the maximum secondary particle diameter of the core-shell elastomer in the resin part to 1000 nm or less, and substantially eliminating the blend of polyurethane. Specifically, the above-mentioned problem was solved by the following means. <1> An insert molded article having a resin part formed from a resin composition containing a polyacetal resin and an elastomer, and a metal part, wherein the elastomer contains a core-shell elastomer, the content of polyurethane in 100% by mass of the resin composition is less than 1% by mass, the maximum secondary particle diameter of the core-shell elastomer in the resin part is 1000 nm or less, and the minimum value of the thickness ratio of the resin part to the metal part (resin part / metal part) of the insert molded article is 1.5 or less. <2> The melt volume rate (MVR) of the polyacetal resin measured according to the ISO 1133 standard at 190 ° C and 2.16 kg is 0.5 to 20 cm 3The insert molded article according to <1>, wherein the melting point is 1 / 10 minutes. <3> The insert molded article according to <1> or <2>, wherein the insert molded article has a three-layer structure in which the resin portion, the metal portion, and the resin portion are in contact with each other in the aforementioned order. <4> The insert molded article according to any one of <1> to <3>, wherein the insert molded article has a weld portion. <5> The insert molded article according to any one of <1> to <4>, wherein the maximum secondary particle diameter of the core-shell elastomer in the resin portion is 10 to 900 nm. <6> The insert molded article according to any one of <1> to <5>, wherein the content of the core-shell elastomer in the resin composition is 5 to 40 mass%. <7> The insert molded article according to any one of <1> to <6>, wherein, in the core-shell elastomer, the core contains a butadiene-containing rubber and / or an acrylate-based rubber, and the shell contains an acrylic-based resin. <8> The melt volume rate (MVR) of the polyacetal resin measured according to ISO 1133 standard at 190 ° C. and 2.16 kg is 0.5 to 20 cm 3 <9> A seat belt fastening anchor comprising the insert molded article according to any one of <1> to <8>, wherein the maximum secondary particle diameter of the core-shell elastomer in the resin portion is 10 to 900 nm, the content of the core-shell elastomer in the resin composition is 5 to 40 mass%, and the core of the core-shell elastomer comprises a butadiene-containing rubber, and the shell comprises an acrylic resin. <10> A method for producing the insert molded article according to any one of <1> to <8>, wherein the melt-kneading time is 10 minutes / 10 minutes, the insert molded article has a three-layer structure in which the resin portion, the metal portion, and the resin portion are in contact with each other in the aforementioned order, the insert molded article has a weld portion, the maximum secondary particle diameter of the core-shell elastomer in the resin portion is 10 to 900 nm, the content of the core-shell elastomer in the resin composition is 5 to 40 mass%, and the core of the core-shell elastomer comprises a butadiene-containing rubber, and the shell comprises an acrylic resin. <11> A seat belt fastening anchor comprising the insert molded article according to any one of <1> to <8>, wherein the melt-kneading time is 10 minutes / 10 minutes, the insert molded article has a three-layer structure in which the resin portion, the metal portion, and the resin portion are in contact with each other in the aforementioned order, the insert molded article has a weld portion, the maximum secondary particle diameter of the core-shell elastomer in the resin portion is 10 to 900 nm, the content of the core-shell elastomer in the resin composition is 5 to 40 mass%, and the core of the core-shell elastomer comprises a butadiene-containing rubber, and the shell

[0007] The present invention makes it possible to provide an insert-molded body having a resin part and a metal part, in which the resin part has high weld elongation and is less likely to crack, as well as an anchor for attaching a seat belt, and a method for manufacturing the insert-molded body.

[0008] 1 is a schematic diagram illustrating an insert molded body according to an embodiment of the present invention.

[0009] Hereinafter, an embodiment of the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. Note that the following present embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment. Note that in this specification, the term "to" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit. In this specification, various physical property values ​​and characteristic values ​​are those at 23°C unless otherwise specified. In this specification, "(meth)acrylic" represents both or either acrylic and methacrylic.

[0010] If the measurement methods and other aspects described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2023, unless otherwise specified. The scale of Figure 1 may not be consistent with reality.

[0011] The insert molded article of this embodiment has a resin portion formed from a resin composition containing a polyacetal resin and an elastomer, and a metal portion. The elastomer includes a core-shell elastomer, and the polyurethane content in 100% by mass of the resin composition is less than 1% by mass. The maximum secondary particle diameter of the core-shell elastomer in the resin portion is 1000 nm or less. The minimum thickness ratio of the resin portion to the metal portion (resin portion / metal portion) of the insert molded article is 1.5 or less. This configuration results in an insert molded article with excellent weld elongation in the resin portion and reduced cracking. This is presumably because the incorporation of the core-shell elastomer softens the polyacetal resin, and the resin portion is molded so that the maximum secondary particle diameter of the core-shell elastomer is 1000 nm or less. This results in an insert molded article with a soft resin portion that also has excellent weld elongation.

[0012] <Resin Part> The resin part of this embodiment is formed from a resin composition containing a polyacetal resin and an elastomer. The resin part of this embodiment is typically formed by placing a metal part in a mold and insert injection molding the resin composition. When a resin part is formed by injection molding, welds typically form at the filling end or in the insert part (around the metal fixing pin) in the mold, and these welds can cause cracks. Furthermore, depending on the shape of the molded product, multiple welds may form in locations other than those mentioned above. In this embodiment, by increasing the elongation of the welds, we have succeeded in effectively suppressing cracks in the welds.

[0013] In this embodiment, the maximum secondary particle diameter of the core-shell elastomer in the resin portion is 1000 nm or less. This configuration effectively suppresses cracking in the weld. Achieving a maximum secondary particle diameter of the core-shell elastomer of 1000 nm or less can be achieved by improving the dispersibility of the core-shell elastomer in the polyacetal resin. Specifically, this can be achieved by selecting a twin-screw extruder when melt-kneading the polyacetal resin and the core-shell elastomer, increasing the rotation speed during melt-kneading, using a polyacetal resin with a low viscosity, and selecting the material of the core-shell elastomer. It is not necessary to satisfy all of these means; the desired means can be selected as appropriate. The maximum secondary particle diameter of the core-shell elastomer is a value measured according to the examples described below.

[0014] In this embodiment, the maximum secondary particle diameter of the core-shell elastomer in the polyacetal resin is preferably 900 nm or less, more preferably 600 nm or less, even more preferably 400 nm or less, even more preferably 350 nm or less, and even more preferably 279 nm or less. By setting the maximum secondary particle diameter below the upper limit, weld elongation tends to be higher. Furthermore, the maximum secondary particle diameter of the core-shell elastomer is preferably 10 nm or more, more preferably 30 nm or more, even more preferably 50 nm or more, even more preferably 70 nm or more, even more preferably 100 nm or more, and even more preferably 110 nm or more. By setting the maximum secondary particle diameter above the lower limit, handleability and availability up to the melt-kneading stage tend to be excellent. The resin portion of this embodiment is formed from a resin composition. Details of the resin composition are described below.

[0015] The thickness of the resin portion is preferably 0.5 mm or more and 20 mm or less at its thinnest part, and 0.5 mm or more and 20 mm or less at its thickest part.

[0016] <<Polyacetal Resin>> The resin composition used in this embodiment contains a polyacetal resin. The polyacetal resin used in this embodiment is not particularly limited, and may be a homopolymer containing only divalent oxymethylene groups as structural units, or a copolymer containing divalent oxymethylene groups and divalent oxyalkylene groups having 2 to 6 carbon atoms as structural units.

[0017] Examples of the oxyalkylene group having 2 to 6 carbon atoms include an oxyethylene group, an oxypropylene group, and an oxybutylene group.

[0018] In the polyacetal resin, the proportion of oxyalkylene groups having 2 to 6 carbon atoms in the total number of moles of oxymethylene groups and oxyalkylene groups having 2 to 6 carbon atoms is not particularly limited, and may be 0.5 to 10 mol %.

[0019] To produce the polyacetal resin, trioxane is typically used as the main raw material. Furthermore, cyclic formals or cyclic ethers can be used to introduce oxyalkylene groups having 2 to 6 carbon atoms into the polyacetal resin. Specific examples of cyclic formals include 1,3-dioxolane, 1,3-dioxane, 1,3-dioxepane, 1,3-dioxocane, 1,3,5-trioxepane, and 1,3,6-trioxocane. Specific examples of cyclic ethers include ethylene oxide, propylene oxide, and butylene oxide. To introduce oxyethylene groups into the polyacetal resin, 1,3-dioxolane can be used as the main raw material. To introduce oxypropylene groups, 1,3-dioxane can be used as the main raw material. To introduce oxybutylene groups, 1,3-dioxepane can be used as the main raw material. In addition, it is preferable that the amount of hemiformal terminal groups, formyl terminal groups, and terminal groups unstable to heat, acid, or base is small in the polyacetal resin. 2 A formyl terminal group is represented by —CHO.

[0020] In addition to the above, the polyacetal resins that can be used include those described in paragraphs 0018 to 0043 of JP-A-2015-074724, the contents of which are incorporated herein by reference.

[0021] The polyacetal resin has a melt volume rate (MVR) of 0.5 cm, measured at 190°C and 2.16 kg in accordance with ISO 1133. 3 / 10 minutes or more is preferable, 3 / 10 minutes or more is more preferable, 3 / 10 minutes or more is more preferable, 3 / 10 minutes or more is more preferable, and 6 cm 3 By setting the extrusion time to the lower limit or more, the resin temperature during extrusion can be suppressed, and thermal decomposition and discoloration of the resin, as well as the generation of formaldehyde, can be suppressed. In addition, the melt volume rate (MVR) of polyacetal resin measured at 190°C and 2.16 kg according to the ISO 1133 standard is 20 cm 3 / 10 minutes or less is preferable, and 18 cm 3 / 10 minutes or less is more preferable, and 13 cm 3 / 10 minutes or less is more preferable, and 10 cm 3 / 10 minutes or less is more preferable, 3 / 10 minutes or less is even more preferable. By setting the viscosity at or below the upper limit, the maximum secondary particle size of the core-shell elastomer tends to be smaller. The resin composition used in this embodiment may contain only one type of polyacetal resin, or may contain two or more types. When two or more types are contained, it is preferable that the MVR of the mixture is in the above range.

[0022] The content of the polyacetal resin in the resin composition used in this embodiment is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 75% by mass or more, even more preferably 80% by mass or more, and even more preferably 85% by mass or more, based on 100% by mass of the resin composition. It is also preferably 97% by mass or less, more preferably 96% by mass or less, even more preferably 95% by mass or less, even more preferably 94% by mass or less, and even more preferably 92% by mass or less. The resin composition used in this embodiment may contain only one type of polyacetal resin, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.

[0023] <<Elastomer>> The resin composition used in this embodiment contains an elastomer. By containing an elastomer, cracking of the metal insert molded body is suppressed and the impact resistance of the obtained resin part tends to be further improved.

[0024] The elastomer used in this embodiment includes a core-shell elastomer. By including the core-shell elastomer, it is possible to impart flexibility to the resin composition. The core-shell elastomer is a polymer with a multilayer structure having a core and a shell layer that covers part or all of the core. Known examples of such elastomers include the Kane Ace series from Kaneka Corporation and the Metablen series from Mitsubishi Chemical Corporation.

[0025] While the type of core-shell elastomer used in this embodiment is not particularly limited, the core is preferably a rubber-based polymer. The rubber-based polymer preferably contains at least one selected from butadiene-containing rubber, butyl acrylate-containing rubber, 2-ethylhexyl acrylate-containing rubber, silicone-based rubber, and acrylate-based rubber, and more preferably the core contains butadiene-containing rubber and / or acrylate-based rubber. The shell is preferably a polymer of one or more monomers, such as a (meth)acrylic acid ester or an aromatic vinyl compound, and more preferably a polymer (acrylic resin) in which units derived from (meth)acrylic acid ester account for 50% by mass or more of the total. The use of an acrylic resin can further improve dispersibility in the polyacetal resin. The core-shell elastomer used in this embodiment preferably contains butadiene-containing rubber and / or acrylate-based rubber, and the shell preferably contains an acrylic resin. The use of such a core-shell elastomer tends to more effectively demonstrate the effects of the present invention.

[0026] The resin composition of this embodiment preferably contains 5% by mass or more of the core-shell elastomer, more preferably 7% by mass or more, and even more preferably 8% by mass or more. By setting the content at or above the lower limit, impact resistance tends to be further improved. The upper limit of the content of the core-shell elastomer is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and may be 15% by mass or less, 14% by mass or less, 12% by mass or less, or 11% by mass or less. Setting the content at or below the upper limit tends to effectively suppress formaldehyde released from the resin composition. The resin composition used in this embodiment may contain only one type of core-shell elastomer, or may contain two or more types. When two or more types are contained, the total amount preferably falls within the above range.

[0027] The resin composition used in this embodiment has a polyurethane content of less than 1% by mass per 100% by mass of the resin composition. By using only a small amount of polyurethane, or no polyurethane at all, the weld elongation of the resin portion of the resulting insert-molded body can be improved. More specifically, this tends to effectively prevent the polyurethane from deforming into layers due to the pressure generated at the weld portion during insert molding, which can lead to cracking. The polyurethane content per 100% by mass of the resin composition is preferably less than 0.5% by mass, more preferably less than 0.1% by mass, and even more preferably less than 0.01% by mass. The lower limit of the polyurethane content per 100% by mass of the resin composition is preferably 0% by mass. Furthermore, the content of elastomers other than core-shell elastomers (non-core-shell elastomers) per 100% by mass of the resin composition is preferably less than 1% by mass. By using only a small amount of elastomers other than core-shell elastomers (non-core-shell elastomers), or no polyurethane at all, the weld elongation of the resin portion of the resulting insert-molded body can be improved.

[0028] In the resin composition used in this embodiment, the total amount of the polyacetal resin and the core-shell elastomer preferably accounts for 90% by mass or more of the resin composition, more preferably 95% by mass or more, and even more preferably 98% by mass or more, provided that the total amount of the polyacetal resin and the core-shell elastomer does not exceed 100% by mass.

[0029] <<Other Components>> The resin composition used in this embodiment may contain any conventionally known additives or fillers as long as the purpose of the present invention is not impaired. Examples of additives and fillers used in this embodiment include thermoplastic resins other than polyacetal resins, ultraviolet absorbers, antioxidants (hindered phenols, etc.), stabilizers (melamine, etc.), formaldehyde scavengers, stress relaxation agents, sliding agents, pigments, release agents, antistatic agents, carbon fibers, glass fibers, glass flakes, potassium titanate whiskers, and the like. For details of these, please refer to paragraphs 0113 to 0124 of JP 2017-025257 A and paragraphs 0032 to 0069 of JP 2022-98154 A, the contents of which are incorporated herein by reference. The resin composition used in this embodiment preferably contains, as other components, a hindered phenol antioxidant, melamine (a stabilizer), and a release agent. Furthermore, when the resin composition used in this embodiment is used for automotive applications, it preferably contains a hindered amine-based light stabilizer, an ultraviolet absorber, and a formaldehyde scavenger in addition to a hindered phenol-based antioxidant, melamine (stabilizer), and a mold release agent. The resin composition used in this embodiment may be configured to be substantially free of a colorant. "Substantially free" means that the colorant content is less than 0.01% by mass, preferably less than 0.001% by mass, per 100 parts by mass of the polyacetal resin. Furthermore, the resin composition used in this embodiment may be configured to be substantially free of a coloring pigment. "Substantially free" means that the coloring pigment content is less than 0.01% by mass, preferably less than 0.001% by mass, per 100 parts by mass of the polyacetal resin.

[0030] <Physical Properties of Resin Composition> The resin composition used in this embodiment preferably has excellent weld elongation. Specifically, the resin composition is molded into an ASTM tensile test piece (thickness 1.6 mm, gates on both ends of the test piece) with a weld portion provided in the center of the test piece, and a tensile test is performed in accordance with ASTM D638. The weld elongation is preferably 10% or more, more preferably 12% or more, and even more preferably 15% or more. The upper limit of the weld elongation is not particularly limited, but is, for example, 150% or less. The weld elongation is measured as described in the examples below.

[0031] <Method of manufacturing resin composition> The resin composition used in this embodiment contains the above-mentioned essential components and the above-mentioned optional components as needed. The manufacturing method thereof is preferably any method that results in a maximum secondary particle size in the above-mentioned range.

[0032] One method for achieving the maximum secondary particle size within the above range is to use pellets prepared by melt-kneading raw materials containing polyacetal resin and elastomer in a twin-screw extruder at a rotation speed of 90 rpm or higher. Injection molding of such pellets improves the dispersibility of the core-shell elastomer in the polyacetal resin, thereby reducing the maximum secondary particle size of the core-shell elastomer in the resin portion of the resulting insert-molded article. More specifically, the polyacetal resin and core-shell elastomer are mixed in a tumbler, extruded through a melt-kneader, extruded through a die, formed into strands, and then cut into pellets. In this case, a twin-screw extruder is preferred as the melt-kneader, since single-screw extruders are prone to secondary aggregation. In particular, the ratio L / D, which is the ratio of the screw length L (mm) to the screw diameter D (mm), is preferably 20 or more, more preferably 30 or more, and preferably 100 or less, more preferably 70 or less. By setting the L / D to 20 or more, the core-shell elastomer is easily finely dispersed, and secondary aggregation of the core-shell elastomer can be effectively suppressed. Furthermore, by setting the L / D to 100 or less, discoloration of the resin composition due to thermal degradation tends to be effectively suppressed. The screw diameter D (mm) is preferably 5 mm or more, and is preferably 40 mm or less, and more preferably 35 mm or less.

[0033] The screw rotation speed during melt-kneading is preferably 90 rpm or more, more preferably 95 rpm or more, more preferably 100 rpm or more, even more preferably 105 rpm or more, even more preferably 110 rpm or more, and even more preferably 115 rpm or more. It is also preferably 500 rpm or less, more preferably 400 rpm or less, and may be 350 rpm or less, 3000 rpm or less, 250 rpm or less, or 1200 rpm or less. By setting the screw rotation speed to 90 rpm or more, the core-shell elastomer tends to be easily finely dispersed, and the occurrence of secondary aggregation tends to be more effectively suppressed. Furthermore, by setting it to 500 rpm or less, heat generation during melt-kneading can be suppressed, and discoloration of the resin composition due to thermal degradation tends to be effectively suppressed. The optimal screw rotation speed varies depending on the extruder's bore, L / D, screw configuration, and discharge rate. Therefore, it is preferable to select the optimal rotation speed each time while checking the secondary particle diameter of the core-shell elastomer and the resin temperature during melt-kneading. The discharge rate is preferably 5 kg / hr or more, more preferably 7 kg / hr or more, and preferably 1,000 kg / hr or less, more preferably 800 kg / hr or less. By setting the discharge rate to 5 kg / hr or more, the core-shell elastomer is more easily finely dispersed, effectively suppressing the occurrence of secondary aggregation. By setting the discharge rate to 1,000 kg / hr or less, heat generation during melt-kneading can be effectively suppressed, and discoloration of the resin composition due to thermal degradation tends to be effectively suppressed. The extruder's bore is preferably 10 mm or more, more preferably 20 mm or more, and more preferably 25 mm or more. It is preferably 100 mm or less, preferably 90 mm or less, and more preferably 80 mm or less. By making the length 10 mm or more, good productivity can be obtained, and by making the length 100 mm or less, secondary aggregation of the core-shell elastomer can be effectively suppressed, and heat generation during melt-kneading can also be effectively suppressed, which tends to effectively suppress discoloration of the resin composition due to thermal degradation.

[0034] The cylinder temperature during melt-kneading can be set arbitrarily, but is preferably set according to the torque during extrusion and the temperature of the resin composition during melt-kneading (discharge from the die). A preferred cylinder temperature is 170°C or higher from the viewpoint of the melting temperature of the polyacetal resin, and 240°C or lower from the viewpoint of thermal degradation and thermal decomposition of the polyacetal resin. It is also possible to set a portion of the extruder cylinder to 170°C or lower or 240°C or higher within a range that does not affect melt-kneading.

[0035] The temperature of the resin composition during melt-kneading (discharging from the die) may be equal to or higher than the temperature at which the polyacetal resin melts, specifically equal to or higher than the melting temperature of the polyacetal resin, but is preferably 170°C or higher, more preferably 190°C or higher, and is preferably 250°C or lower, more preferably 230°C or lower. By setting the melting temperature to 170°C or higher, sufficient melting is achieved, tending to improve productivity. Furthermore, by setting the temperature to 250°C or lower, discoloration of the resin composition due to thermal degradation tends to be effectively suppressed.

[0036] Although the screw configuration of the twin-screw extruder is not particularly limited, one preferred embodiment has at least two kneading sections. The kneading sections have kneading disks and mainly contribute to melting the resin and dispersing the elastomer.

[0037] <Metal Part> The insert molded article of this embodiment has a metal part. The metal material constituting the metal part is not particularly limited, and a molded article made of a known metal can be appropriately selected depending on the application. For example, the metal part can be selected from iron, various stainless steels, aluminum and its alloys, copper, magnesium, titanium, and alloys containing these. The surface of the metal part may be previously subjected to a surface treatment such as anodizing or painting. The metal part used in this embodiment can be a metal part molded into a desired shape depending on the application. Before insert molding, the desired shape can be formed by pouring molten metal into a mold of the desired shape, or it can be machined into the desired shape by cutting using a machine tool or the like. The thickness of the metal part is preferably 0.5 mm or more at its thinnest part and 20 mm or less. The thickness of the thickest part of the metal part is preferably 0.5 mm or more and 20 mm or less. Note that the metal part does not necessarily have to be made entirely of metal; the interior of the metal part may be hollow or filled with other materials.

[0038] <Insert Molded Article> The insert molded article of this embodiment typically has a weld. The weld refers to a weld formed at the interface between multiple resin flows that converge within the mold cavity during molding of the insert molded article. More specifically, FIG. 1 is a schematic diagram illustrating the insert molded article of this embodiment, showing a cross section of the insert molded article. In FIG. 1, 1 indicates the flow direction of the resin composition of the insert molded article, 2 (dotted line portion) indicates the weld, 3 indicates the metal portion, and 4 indicates the resin portion. When the resin composition is injected from direction 1 with metal portion 3 placed in the mold, a weld is formed in portion 2. The insert molded article of this embodiment may have one or more welds, but typically has two or more. Furthermore, a practical upper limit for the number of welds is 100 or less, and may be 50 or less, or even 10 or less.

[0039] The insert-molded body of this embodiment preferably has a three-layer structure in which a resin portion, a metal portion, and a resin portion are in contact in the aforementioned order. Here, the two resin portions may or may not be continuous, but are typically continuous. An example of a configuration in which two resin portions are continuous is the configuration shown in FIG. 1 above. That is, in FIG. 1, resin portions 4 are located on both sides of metal portion 3. When viewed from the flow direction 1 of the resin composition, the metal portion and the resin portion form a three-layer structure in which the metal portion and the resin portion are in contact in the aforementioned order, and the resin portions are continuous. Because the resin portions are continuous in this manner, the flow direction of the resin composition becomes two-way in the portion containing the metal portion, forming a weld. More preferably, the insert-molded body of this embodiment preferably has the entire surface of the inserted metal portion covered with the resin portion. However, portions of the entire surface of the metal portion that cannot be covered with the resin composition during molding, such as holes for fixing the inserted metal portion during molding, are excluded.

[0040] The insert molded article of this embodiment can be preferably used in a structure in which the ratio of the thickness of the resin portion to the thickness of the metal portion (resin portion / metal portion) is small, the load on the resin portion is large, and the structure is prone to cracking. Specifically, the minimum value of the ratio of the thickness of the resin portion to the thickness of the metal portion (resin portion / metal portion) of the insert molded article of this embodiment is 1.5 or less, and can also be 1.2 or less, 1.0 or less, 0.9 or less, 0.8 or less, 0.75 or less, 0.65 or less, 0.60 or less, 0.55 or less, or 0.50 or less. Even when the ratio is below the upper limit, the resin portion of the insert molded article of this embodiment is less likely to crack and can be used favorably. The minimum value of the ratio of the thickness of the resin portion to the thickness of the metal portion (resin portion / metal portion) of the insert molded article of this embodiment is preferably 0.1 or more, more preferably 0.15 or more, even more preferably 0.2 or more, even more preferably 0.22 or more, and even more preferably 0.25 or more. By setting the ratio above the lower limit, cracking of the metal insert molded article can be effectively suppressed.

[0041] The insert-molded article is preferably produced using pellets obtained by melt-kneading a resin composition containing a polyacetal resin and an elastomer using a twin-screw extruder at a rotation speed of 90 rpm or more. The resin composition here is the resin composition described above.

[0042] The insert molded article of this embodiment has excellent weld elongation and can be suitably used for safety parts such as seat belt anchors (particularly seat belt anchors for automobile seat belts) and seat belt tongues. Examples of seat belt anchors include those described in FIG. 1 and paragraph 0095 of JP 2022-98154 A, the contents of which are incorporated herein by reference. In addition to the above, the insert molded article of this embodiment can be widely used for other automotive parts, building materials, electrical and electronic parts, office equipment parts, everyday miscellaneous goods parts, etc.

[0043] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.

[0044] 1. Raw materials The following raw materials were used:

[0045] 2. Examples 1 to 5 and Comparative Examples 1 to 7 <Production of Resin Composition (Pellets)> The components shown in Tables 2 and 3 were uniformly mixed in the proportions (parts by mass) shown in Tables 2 and 3 using a Super Mixer manufactured by Kawada Manufacturing Co., Ltd. The resulting mixture was melt-shear mixed using a twin-screw or single-screw extruder having the screw diameter shown in Tables 2 or 3 at a cylinder temperature of 200°C and at the screw rotation speed and die discharge speed shown in Tables 2 or 3 to produce pellets of the resin composition. The twin-screw extruder used was model PCM-30 manufactured by Ikegai Corporation, and the single-screw extruder used was model VS-40 manufactured by Tanabe Plastic Machinery Co., Ltd. The temperature of the resin composition at the time of die discharge was measured using a K thermocouple.

[0046] <Weld Elongation (%)> The pellets obtained above were heat-treated for 4 hours in a hot air circulation dryer at a temperature of 80°C. Next, the dried pellets were used in an injection molding machine with a cylinder temperature set to 195°C and a mold temperature set to 80°C to prepare ASTM tensile test pieces (thickness 1.6 mm) having a weld portion in the center. A tensile test was performed in accordance with ASTM D638 to measure the weld elongation. The injection molding machine used was an EC-100S manufactured by Shibaura Machine Co., Ltd. The results are shown in Tables 2 and 3 below. The units are shown in %.

[0047] <Flexural Modulus (MPa)> The pellets obtained above were heat-treated for 4 hours in a hot air circulation dryer at a temperature of 80°C. Next, the dried pellets were injection-molded using an injection molding machine with a cylinder temperature of 195°C and a mold temperature of 90°C in accordance with the ISO 9988-2 standard. Thus, a 4 mm thick multipurpose test piece (ISO test piece) was obtained. Next, a bending test was performed on this 4 mm thick multipurpose test piece (ISO test piece) using a fully automatic bending tester at a bending test speed of 2 mm / min according to the method described in ISO 178, and the bending modulus was measured. The injection molding machine used was an EC-100S manufactured by Shibaura Machine Co., Ltd. The fully automatic bending tester used was one manufactured by Shimadzu Corporation. The results are shown in Tables 2 and 3 below. The units are shown in MPa.

[0048] <Maximum Secondary Particle Diameter (nm) of Core-Shell Elastomer> A specimen for scanning electron microscope (SEM) observation was cut from the center of the ISO test specimen obtained above using a diamond knife, parallel to the flow direction of the resin composition during molding. Osmium tetroxide was vapor-deposited on the observation surface of the obtained SEM specimen, and then an SEM image was obtained using a scanning electron microscope (SEM). The maximum length of the elastomer-derived island-like portions was determined from the obtained SEM image to be the maximum secondary particle diameter of the elastomer. Osmium tetroxide was vapor-deposited using an "Osmium Coater" manufactured by Meiwafosis Co., Ltd. at 8 mA for 60 seconds. A scanning electron microscope (SEM) S-4800 manufactured by Hitachi High-Technologies Corporation was used to obtain SEM images under the following conditions: acceleration voltage: 1 kV, signal: LA100(U), emission current: 6 μA, and probe current: Normal.

[0049] <Failure Time (hr) of Insert Molded Body> The pellets obtained above were heat-treated for 4 hours in a hot air circulation dryer at 80°C. Next, the dried pellets were used in an injection molding machine with a cylinder temperature of 195°C and a mold temperature of 80°C to produce metal insert molded pieces with a resin-to-metal thickness ratio (minimum value, resin thickness / metal thickness) of 0.5. A 2mm thick S55C insert metal was used, which was heated to 80°C on a hot plate before molding and then placed in the mold immediately before molding. The injection molding machine used was an EC-100S manufactured by Shibaura Machine Co., Ltd. The insert molded body obtained above was placed in a hot air oven at 90°C and checked every 120 hours up to 1500 hours. Five experts visually inspected the insert molded body, and the time (unit: hours) at which three or more experts judged it to have broken was evaluated. The results are shown in Tables 2 and 3 below.

[0050]

[0051]

[0052] As is clear from the above results, the insert moldings of the present invention had excellent weld elongation (Examples 1 to 5). In contrast, when the core-shell elastomer was not included (Comparative Example 1 and Comparative Example 5), the weld elongation was low and the time to failure of the insert moldings was short. Furthermore, even when the core-shell elastomer was included, when the maximum secondary particle diameter of the core-shell elastomer exceeded 1,000 nm (Comparative Examples 2 to 4 and 7), the weld elongation was low and the time to failure of the insert moldings was short.

[0053] 1 Flow direction of resin composition of insert molded body 2 Weld portion 3 Metal portion 4 Resin portion

Claims

1. An insert molded body having a resin part formed from a resin composition containing polyacetal resin and an elastomer, and a metal part, wherein the elastomer contains a core-shell elastomer, the content of polyurethane in 100% by mass of the resin composition is less than 1% by mass, the maximum secondary particle diameter of the core-shell elastomer in the resin part is 1000 nm or less, and the thickness ratio of the resin part of the insert molded body to the thickness of the metal part (resin part / metal part) is a minimum of 1.5 or less.

2. The melt volume rate (MVR) of the polyacetal resin measured according to ISO 1133 standard at 190°C and 2.16 kg is 0.5 to 20 cm 3 2. The insert molded article according to claim 1, wherein the hardness is 10 / 10 minutes.

3. The insert molded body according to claim 1, wherein the insert molded body has a three-layer structure in which the resin part, the metal part, and the resin part are in contact with each other in the stated order.

4. The insert molded article according to claim 1, wherein the insert molded article has a weld portion.

5. The insert molding according to claim 1, wherein the maximum secondary particle size of the core-shell elastomer in the resin portion is 10 to 900 nm.

6. The insert molded article according to claim 1, wherein the content of the core-shell elastomer in the resin composition is 5 to 40 mass %.

7. The insert molding according to claim 1, wherein in the core-shell elastomer, the core contains a butadiene-containing rubber and / or an acrylate-based rubber, and the shell contains an acrylic-based resin.

8. The melt volume rate (MVR) of the polyacetal resin measured according to ISO 1133 standard at 190 ° C and 2.16 kg is 0.5 to 20 cm 32. The insert molded body according to claim 1, wherein the resin part, the metal part, and the resin part are in contact with each other in this order, the insert molded body has a weld part, the maximum secondary particle diameter of the core-shell elastomer in the resin part is 10 to 900 nm, the content of the core-shell elastomer in the resin composition is 5 to 40 mass%, and in the core-shell elastomer, a core contains a butadiene-containing rubber and a shell contains an acrylic resin.

9. A seat belt mounting anchor comprising the insert molding according to any one of claims 1 to 8.

10. A method for producing an insert molded article according to any one of claims 1 to 8, comprising using pellets obtained by melt-kneading a resin composition containing a polyacetal resin and an elastomer in a twin-screw extruder at a rotation speed of 90 rpm or more.

Citation Information

Patent Citations

  • Automobile interior part

    JP2015074724A

  • Polyacetal resin composition and polyacetal resin molded article

    JP2017025257A

  • Metal insert molded body and seat belt attachment anchor

    JP2022098154A

  • Method of manufacturing adhesion body

    JP2013141794A

  • Composite gear and manufacturing method thereof

    JP2016183764A