Electrode foil, method for manufacturing electrode foil, and method for manufacturing wound capacitor

The method of forming cracks in electrode foils through surface enlarging and dividing treatments enhances flexibility and strength, addressing the challenges of winding and capacitance in wound capacitors, allowing for smooth curvature and reduced breakage.

WO2024202739A1PCT designated stage expired Publication Date: 2024-10-03NIPPON CHEMI CON CORP

Patent Information

Application Number
PCT/JP2024/006335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-21
Publication Date
2024-10-03

Smart Images

  • Figure JP2024006335_03102024_PF_FP_ABST
    Figure JP2024006335_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a method for manufacturing an electrode foil that is easy to bend smoothly during winding, and a method for manufacturing a wound capacitor. A method for manufacturing an electrode foil 1 includes a surface area expansion step (S01) for forming an expanded surface area portion on the surface of a foil having having a strip shape, and a division step (S03, S06) for forming, so as to extend in the width direction of the foil strip, a plurality of cracks 4 that divide the expanded surface area portion 3. The division step (S03, S06) is performed multiple times to increase the depth of the cracks 4 over multiple treatments.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode foil, electrode foil manufacturing method, and wound capacitor manufacturing method

[0001] The present invention relates to a method for manufacturing a wound capacitor, an electrode foil used in the wound capacitor, and a method for manufacturing the electrode foil.

[0002] Electrolytic capacitors are constructed by filling the gaps with an electrolyte to ensure close contact between the dielectric film of the anode and the opposing electrode, and include non-solid electrolytic capacitors with a liquid electrolyte, solid electrolytic capacitors with a solid electrolyte, hybrid electrolytic capacitors with both liquid and solid electrolytes, and bipolar electrolytic capacitors with a dielectric film formed on both electrodes.

[0003] These electrolytic capacitors are made by impregnating a capacitor element with an electrolyte. The capacitor element is made up of an anode foil, which is a valve metal foil such as aluminum coated with a dielectric film, and a cathode foil made of the same or another metal, facing each other, with a separator interposed between the anode foil and the cathode foil.

[0004] To achieve both compactness and large capacitance, electrolytic capacitors are sometimes made in the form of wound capacitors. The capacitor element of a wound capacitor is made by stacking an anode foil and a cathode foil with a separator sandwiched between them, and winding them into a cylindrical shape.

[0005] The capacitance of an electrolytic capacitor is proportional to the surface area of ​​the dielectric film. Typically, the electrode foil of an electrolytic capacitor undergoes a surface-enlarging process such as etching, and the enlarged surface is then subjected to a chemical conversion treatment, resulting in a dielectric film with a large surface area. In recent years, efforts have been made to enlarge the surface area of ​​the electrode foil, extending from the surface to deeper areas, in order to further increase the capacitance of electrolytic capacitors.

[0006] Japanese Patent Application Laid-Open No. 2007-149759

[0007] In recent years, in order to meet the demand for higher capacitance, smaller size, and lighter weight of electrolytic capacitors, electrode foils have been subjected to more extensive surface enlargement treatments to increase their surface area. However, this surface enlargement reduces the foil substrate area and increases the area of ​​the dielectric oxide film, which results in the electrode foil becoming brittle and hardened. This reduces the flexibility and extensibility of the electrode foil itself.

[0008] Electrode foil with reduced flexibility and stretchability cannot be deformed into a bow shape, making it difficult to smoothly curve the electrode foil while winding it, and bending stress during winding is concentrated in localized areas, causing bending in places. In the worst case, the core of the electrode foil may break.

[0009] When the electrode foil is folded in places during winding, the diameter of the capacitor element increases. Therefore, if you try to maintain the capacitance of a wound capacitor, the size of the wound capacitor will increase. Alternatively, if you try to maintain the diameter of the wound capacitor, the capacitance of the wound capacitor will decrease. Otherwise, the wound capacitor will be treated as a defective product, which will result in a decrease in yield.

[0010] In order to solve the above-mentioned problems of the prior art, the present invention aims to provide an electrode foil that can be easily curved smoothly during winding, a method for manufacturing such an electrode foil, and a method for manufacturing a wound capacitor.

[0011] In order to achieve the above-mentioned objective, the manufacturing method of the electrode foil of this embodiment includes a surface-expanding step of forming an expanded portion on the surface of the strip-shaped foil, and a dividing step of forming multiple cracks that divide the expanded portion, and the dividing step is performed multiple times.

[0012] Between any of the plurality of dividing steps, there may be provided an inter-dividing film forming step of forming an oxide film on the enlarged surface portion.

[0013] The film forming step during the dividing treatment may include a hydration treatment for forming a hydrated oxide film on the enlarged surface portion, or a chemical conversion treatment for forming a film by applying a voltage, or both.

[0014] After the surface-enlarging step and before the first dividing step, a first film forming step of forming an oxide film on the enlarged surface portion may be included.

[0015] A film formation step between the cutting steps may be included in which an oxide film is formed on the enlarged surface portion between the multiple cutting steps, and the hardness of the electrode foil obtained in the film formation step between the cutting steps may be made higher than the hardness of the electrode foil obtained in the first film formation step.

[0016] During any of the multiple cutting steps, the foil before the next cutting step may have a higher hardness than the foil before the next cutting step.

[0017] Among the multiple cutting steps, the hardness of the foil cut in the nth cutting step may be made higher than the hardness of the foil cut in any of the cutting steps prior to the n-1th cutting step.

[0018] In the dividing step, the cracks may be formed so that the width of the cracks is 50 μm or less, including 0 μm, when the foil is kept flat.

[0019] In the plurality of dividing steps, the depth of the crack formed in the previous dividing step may be increased, and a new crack may be formed.

[0020] After the final dividing step, a chemical conversion treatment may be performed to form an oxide film on the inner surface of the crack while maintaining the crack openable and closable.

[0021] This method of manufacturing the electrode foil is a method of manufacturing the electrode foil before it is wound to form the capacitor element.

[0022] In order to achieve the above object, the method for manufacturing a wound capacitor of this embodiment includes a winding step of winding the electrode foil obtained by the manufacturing method.

[0023] In order to achieve the above-mentioned object, the electrode foil of this embodiment comprises a strip-shaped foil, an expanded surface portion formed on the surface of the foil, a core portion which is the remaining portion of the foil excluding the expanded surface portion, a first type of crack which divides the expanded surface portion and has a depth of less than 70% of the distance from the surface of the foil to the core portion, and a second type of crack which divides the expanded surface portion and has a depth of 70% or more of the distance from the surface of the foil to the core portion, wherein the proportion of the first type of cracks is 10% or more and 50% or less, and the proportion of the second type of cracks is 50% or more and 90% or less.

[0024] According to the present invention, the plurality of cracks open widely during winding, enabling smoothly curved winding.

[0025] 1 shows the structure of an electrode foil, where (a) is a cross-sectional view along the longitudinal direction, and (b) is a top view. It is a flow diagram showing the manufacturing process for forming cracks in the electrode foil. It is a cross-sectional view along the longitudinal direction of an electrode foil with cracks, showing the state after winding. (a1) is a cross-sectional SEM image after the first dividing process in Example 1, and (a2) has added a thick line to highlight the crack. (b1) is a cross-sectional SEM image after the second dividing process in Example 1, and (b2) has added a thick line to highlight the crack. (a1) is a surface SEM image after the first dividing process in Example 1, and (a2) has added a thick line to highlight the crack. (b1) is a surface SEM image after the second dividing process in Example 1, and (b2) has added a thick line to highlight the crack. It is a photograph of Example 1, Comparative Example 1, and Comparative Example 2. (a) is a photograph of Comparative Example 2, in which the dividing process was performed once, and (b) is a photograph of Example 1, in which the dividing process was performed twice.

[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to preferred embodiments thereof, including an electrode foil, a wound capacitor, and a method of manufacturing the same. However, the present invention is not limited to the preferred embodiments described below.

[0027] (Electrode Foil) The electrode foil 1 shown in FIG. 1 is used as an anode foil, a cathode foil, or both of a wound capacitor. The electrode foil 1 may be a low-voltage electrode foil, a medium-to-high-voltage electrode foil, or a high-voltage electrode foil. The electrode foil 1 is based on a foil of a valve metal such as aluminum, tantalum, titanium, niobium, or niobium oxide. The electrode foil 1 has a long, strip-like shape. Except for a core portion 2 at the center of the thickness of the electrode foil 1, enlarged surface portions 3 are formed on both sides of the electrode foil 1. A dielectric coating 5 is formed on the enlarged surface portions 3.

[0028] The expanded surface portion 3 has a porous structure. The porous structure is made up of tunnel-like pits, spongy pits, or voids between densely packed powder particles. The core portion 2 is the remainder of the electrode foil 1 excluding the expanded surface portion 3, or a substrate to which metal particles and the like are attached by vapor deposition, sintering, etc. In other words, the core portion 2 is, for example, an unetched layer or a substrate to which powder is vapor-deposited or sintered.

[0029] The dielectric coating 5 is formed on the uneven surface of the expanded surface portion 3. The dielectric coating 5 is typically an oxide coating formed on the surface layer of the electrode foil 1, and if the electrode foil 1 is an aluminum foil, it is an aluminum oxide layer formed by oxidizing the surface of the expanded surface portion 3. The dielectric coating 5 is formed by hydration treatment and chemical conversion treatment.

[0030] This electrode foil 1 has a plurality of cracks 4 intentionally formed on one or both of the expanded surface portions 3. The cracks 4 are formed before the winding process in which the cathode foils are wound facing each other, and remain open without being closed before and after the winding process.

[0031] Cracks 4 are fissures that have split the expanded surface portion 3. The cracks 4 extend in the strip width direction of the electrode foil 1 and cross the expanded surface portion 3. They do not need to be aligned precisely along the strip width direction; it is sufficient if most of the cracks 4 are within a range of 0 degrees to ±45 degrees relative to the strip width direction. The cracks 4 may completely or partially cross the electrode foil 1, and may extend continuously or intermittently.

[0032] The depth of the cracks 4 need not be so great as to divide the core 2. The depth of the cracks 4 may be any of the following: a depth that does not reach the core 2, a depth where the deepest part just reaches the core 2, or a depth where the deepest part bites into the core 2. It is not necessary for all cracks 4 to have the same depth.

[0033] Preferably, the cracks 4 are allowed to extend to a depth that reaches the core portion 2 or a depth that causes the deepest portion to penetrate into the core portion 2. That is, if the thickness of the expanded surface portion 3 is 20 to 100 μm on one side, the cracks 4 preferably have a depth of approximately 20 to 100 μm, matching the thickness of this expanded surface portion 3. The deeper the cracks 4 are within a range that does not destroy the core portion 2, the better the flexibility and extensibility of the electrode foil 1. This prevents the core portion 2 from buckling or breaking, and also prevents the formation of numerous fine cracks that expose unoxidized metal portions.

[0034] More preferably, two types of cracks 4 having different depths are formed. The first type of crack 4 has a depth of less than 70% of the distance from the surface of the electrode foil 1 to the core 2, and the second type of crack 4 has a depth of 70% or more of the distance from the surface of the electrode foil 1 to the core 2.

[0035] Furthermore, it is preferable that the proportion of the first type of cracks formed in the electrode foil 1 be 10% to 50% and the proportion of the second type of cracks be 50% to 90%. With such electrode foil 1, flexibility is achieved by the second type of cracks that reach the core or near the core, and the first type of cracks, which are shallower than the second type, ensure the thickness of the core, thereby increasing strength. This results in an electrode foil that has a good balance of flexibility and strength, making it easy to bend during winding and less susceptible to breakage. An electrode foil with a proportion of the first type of cracks of 10% to 50% and a proportion of the second type of cracks outside the range of 50% to 90% may be less flexible and stronger than an electrode foil within the range.

[0036] Furthermore, as described below, the dividing step is performed multiple times on the electrode foil 1. By performing the dividing step multiple times, it becomes easier to control the groove width, groove depth, and the distance between both ends of a single crack 4 to desired values ​​compared to a single process. This is particularly effective for electrode foils for medium- to high-voltage applications, which have a thick dielectric film and low flexibility and extensibility.

[0037] As described below, the electrode foil 1 is processed in multiple dividing steps. In the first dividing step, the distance between both ends of a single crack 4 is between 40 μm and 150 μm on average, with short cracks of approximately 10 μm and long cracks of approximately 600 μm. Preferably, the distance between both ends of a crack 4 is 100 μm or more. Cracks 4 with a length of 100 μm or more further improve the flexibility and extensibility of the electrode foil 1.

[0038] In the next dividing portion forming step described later, the separation distance between the good ends of a single crack 4 easily exceeds 100 μm on average, and some long cracks are on the order of millimeters.

[0039] The groove width of crack 4 is 50 μm or less, including 0, when electrode foil 1 is flattened without being curved. The groove width of crack 4 is the length along the longitudinal direction of electrode foil 1, measured near the surface layer of electrode foil 1. A groove width of 0 means that crack 4 is open, but when electrode foil 1 is flattened without being curved, the interfaces of crack 4 are at least partially in contact.

[0040] Furthermore, the interval between adjacent cracks 4 may be an average pitch of 2.1 mm or less, and more preferably an average pitch of 250 μm or less. It has been confirmed that when the average pitch is 2.1 mm or less, the Erichsen value is larger than that of electrode foil 1 in which cracks 4 are not formed. When the average pitch of cracks 4 is 250 μm or less, the Erichsen value is particularly large.

[0041] (Method of Manufacturing Electrode Foil) FIG. 2 is a flow chart showing the manufacturing process for forming cracks 4 in the electrode foil 1. As shown in FIG. 2, first, a surface expansion treatment is performed on the surface of the strip-shaped foil (step S01). The electrode foil 1 with the expanded surface portion 3 formed thereon is subjected to a hydration treatment, which serves as the first film formation step (step S02). After the hydration treatment, which serves as the first film formation step, an initial division treatment is performed (step S03). After the initial division treatment, a hydration treatment is performed (step S04), and then a chemical conversion treatment is performed (step S05). The hydration treatment in step S04 and the chemical conversion treatment in step S05 are collectively film formation steps between division treatments for forming a dielectric film. That is, after the chemical conversion treatment in step S05, a further division treatment is performed (step S06). Finally, a chemical conversion treatment, which serves as the third film formation step, is performed (step S07).

[0042] In the surface enlargement process of step S01, the surface enlargement portion 3 is formed on the electrode foil 1. The surface enlargement process may be electrolytic etching, chemical etching, sandblasting, or the like, or may be vapor deposition or sintering of metal particles or the like onto the foil body.

[0043] As an example of a method for forming a sintered foil, a slurry in which a metal particle composition is dispersed in a solvent is applied to a current collector such as a metal foil, and then the solvent is dried and the metal particle composition is sintered by heat treatment to form an electrode layer. The sintering of the metal particle composition by this heat treatment is a surface-enlarging treatment, but is not limited to this, and the surface-enlarging treatment also includes a state in which the slurry is applied to a current collector such as a metal foil and dried.

[0044] Examples of electrolytic etching include DC etching and AC etching, in which DC or AC is applied in an acidic aqueous solution such as hydrochloric acid, where halogen ions are present. To form tunnel-shaped pits for medium- to high-voltage applications, for example, a DC current is applied in an acidic aqueous solution such as hydrochloric acid, where halogen ions are present, to form the pits, and a DC current is applied in an acidic aqueous solution such as nitric acid, to expand the pits. Chemical etching involves immersing a metal foil in an acid or alkaline solution.

[0045] In the hydration treatment in step S02, a hydrated oxide film is formed on the surface expansion portion 3. The hydrated oxide film is also called a pseudo-boehmite layer. If the valve metal is aluminum, this hydrated oxide film is made of Al 2 O 3 ・xH 2 In the hydration treatment, the surface-expanded electrode foil 1 is immersed in pure water at 80°C or higher or boiling. The immersion time can be determined based on the desired thickness of the hydrated oxide film and the balance between withstand voltage and capacitance. The hydration treatment increases the hardness of the surface-expanded portion 3, making the electrode foil 1 more susceptible to cracking and less able to stretch.

[0046] In the cutting processes of steps S03 and S06, electrode foil 1 is wound around a shaft and travels. The cutting processes of steps S03 and S06 differ in the load applied to electrode foil 1. That is, the cutting processes of steps S03 and S06 differ in at least one of the roller hardness, roller surface roughness, roller diameter, wrap angle between electrode foil 1 entering the roller and electrode foil 1 exiting the roller, and tension with which electrode foil 1 is pulled.

[0047] The difference between the dividing treatments in step S03 and step S06 is that the first dividing treatment in step S03 is performed after the hydration treatment in step S02, which is the first film formation step, whereas the next dividing treatment in step S06 is performed after the hydration treatment in step S04, which is the film formation step between the dividing treatments, and the chemical conversion treatment in step S05.

[0048] In this case, the hardness of the electrode foil before the dividing process in step S06 by the inter-dividing film formation step is preferably harder than the hardness of the electrode foil before the dividing process in step S03. In other words, the hardness of the electrode foil before the nth dividing process in multiple dividing processes is preferably higher than the hardness of the electrode foil before any of the dividing processes up to the n-1th dividing process. As the electrode foil becomes harder, deeper cracks tend to form during the dividing process. However, if the hardness of the electrode foil is too high from the initial dividing process stage, there is a risk that the electrode foil will break during the dividing process. Therefore, by performing a film formation step that gradually increases the hardness of the electrode foil before the dividing process, the electrode foil becomes more easily cracked and less likely to stretch.

[0049] It is desirable that cracks 4 be formed in the enlarged surface portions 3 on both sides. However, from the viewpoint of the elongation of electrode foil 1 during winding, it is preferable that cracks 4 be formed at least in the enlarged surface portions 3 that are on the outside of the foil and receive tension when electrode foil 1 is wound.

[0050] In the hydration treatment in step S04 and the chemical conversion treatment in step S05, a hydrated oxide film is formed by the same treatment as in step S02 in the hydration treatment in step S04. Then, in the chemical conversion treatment in step S05, the hydrated oxide film is transformed by a chemical conversion treatment at a voltage of several tens of volts (10 V or more but less than 100 V) to form a dielectric film 5 made of a crystalline oxide such as gamma-alumina. In the chemical conversion treatment, the hydrated oxide film is grown from the interface with the unoxidized valve metal toward both surfaces of the hydrated oxide film and the valve metal, transforming the hydrated oxide film into the dielectric film 5. The chemical conversion treatment in step S07 is the final film formation step, and forms the dielectric film 5 on the inner surfaces of the cracks 4 while ensuring the product voltage resistance of the electrode foil. For example, if the product voltage resistance is medium to high, the chemical conversion treatment is preferably performed at a voltage of 200 V or more.

[0051] However, the cracks 4 are not closed by the dielectric film 5, but remain openable. By keeping the cracks openable, the cracks open first when the electrode foil is wound. This makes it difficult for stress to concentrate on the electrode foil when it is wound.

[0052] In the chemical conversion treatment, a voltage is applied to the anode foil in a chemical conversion solution that does not contain halogen ions. The chemical conversion solution can be a phosphoric acid-based chemical conversion solution such as ammonium dihydrogen phosphate, a boric acid-based chemical conversion solution such as ammonium borate, or an adipic acid-based chemical conversion solution such as ammonium adipate. The applied voltage can be determined based on the desired withstand voltage.

[0053] In the film-forming step between division processes, only voltage application may be performed without performing hydration and chemical conversion treatment. Alternatively, in the film-forming step between division processes, hydration and voltage application may be performed without immersion in a chemical conversion solution.

[0054] In this way, at the stage of the initial cutting process, there are no cracks 4 that would share the bending stress when the electrode foil is wound around the roller. Therefore, if a chemical conversion treatment of several tens of volts (10 V or more but less than 100 V) is performed before the initial cutting process to increase the hardness of the electrode foil 1 and reduce its flexibility and extensibility, the core portion 2 of the electrode foil 1 becomes more likely to buckle, and the electrode foil 1 will be bent before being wound.

[0055] Therefore, before the initial dividing process, the hardness of the expanded surface portion 3 is slightly increased by hydration in step S02, which is the first film formation step, heat treatment, or chemical conversion treatment of less than 10 V, making the expanded surface portion 3 easier to split and making it difficult to stretch the electrode foil 1, before the initial dividing process is performed. If the initial dividing process is performed without the hydration in step S02, which is the first film formation step, the electrode foil 1 is likely to stretch, resulting in a decrease in the capacitance of the electrode foil 1.

[0056] Furthermore, when cracks 4 of a target depth are formed in the initial cutting process, a large load must be applied to the electrode foil 1, which stretches the electrode foil 1. The stretched electrode foil 1 has a reduced surface area expansion ratio, which widens the groove width of the cracks 4, resulting in a decrease in capacitance. Therefore, in the initial cutting process, cracks 4 are formed within a range that does not stretch the electrode foil 1. For example, cracks 4 may be formed to a depth of about 50% of the target depth.

[0057] The range in which the electrode foil 1 does not stretch is preferably a maximum elongation rate of approximately 1.0% during the initial cutting process. If the elongation rate exceeds 1.3%, the capacitance will decrease by 1% or more at the time of the initial cutting process. Therefore, the depth of the cracks 4 formed during the initial cutting process can be adjusted, for example, by changing the roller diameter, so that the elongation rate of the electrode foil 1 is approximately 1.0% or less.

[0058] If the dividing process is performed only once, cracks 4 are generated within a range that does not buckle core 2 of electrode foil 1 and does not stretch electrode foil 1, and the cracks 4 are shallow, making it impossible to increase the curvature during winding. In other words, electrode foil 1 cannot be wound tightly. Therefore, the next dividing process is performed in step S06, and cracks 4 are propagated in the depth direction.

[0059] In the cutting process of step S03, the distance between both ends of each crack 4 is between 40 μm and 150 μm on average, with cracks as short as about 10 μm and as long as about 600 μm. Preferably, the distance between both ends of each crack 4 is 100 μm or more. Cracks 4 with a length of 100 μm or more further improve the flexibility and extensibility of the electrode foil 1.

[0060] In the next dividing process in step S06, cracks 4 that share the bending stress are already present. Therefore, a film formation step is added between dividing processes to further increase the hardness of the electrode foil, making it harder than the hardness of the electrode foil obtained in the first film formation step in step S02. Then, the depth of the cracks 4 formed in the initial dividing process is extended to the target depth.

[0061] The dividing process in step S06 not only propagates the cracks 4 in the depth direction, but also connects the cracks 4 that were intermittent in the initial dividing process, and propagates the cracks 4 that were only partially formed in the strip width direction of the electrode foil 1. The cracks 4 that extend in the strip width direction enhance the effect of suppressing new cracks during winding.

[0062] In the dividing process of step S06, the distance between both ends of a single crack 4 easily exceeds 100 μm on average, and some long cracks are on the order of millimeters.

[0063] The reason why the capacitance decreases when the electrode foil 1 is stretched is because the groove width of the cracks 4 increases as the electrode foil 1 is stretched. When the groove width of the cracks 4 increases, the surface area of ​​the dielectric coating 5 decreases, causing a decrease in capacitance. When the groove width of the cracks 4 is within a range of 50 μm or less, the cracks 4 improve the flexibility and extensibility of the electrode foil 1 while suppressing a decrease in capacitance.

[0064] Furthermore, multiple cutting processes reduce frills that occur on the longitudinal edges of the electrode foil 1, improving flatness. This allows the electrode foil 1 to be tightly wound. Even with the same volume, the contained electrode foil 1 becomes longer, improving the capacitance of the wound capacitor.

[0065] Furthermore, by performing the dividing step multiple times, it becomes easier to control the groove width, groove depth, and the distance between both ends of a single crack 4 to the desired values ​​compared to performing the dividing step in a single step.

[0066] The cutting process using a roller may be performed on one or both sides of the electrode foil 1. Furthermore, when the cutting process is performed on only one side of the electrode foil 1, the direction of the electrode foil 1 wound around the roller should be the same as the direction of the electrode foil 1 wound when forming the wound capacitor. That is, the inner diameter side surface and the outer diameter side surface of the electrode foil 1 should be aligned in the same direction for the cutting process and for the winding to form the capacitor element.

[0067] In a preferred form of the dividing process using rollers, the electrode foil 1 is first divided on one side as the first dividing process (step S03), and then divided on the other side. This results in the first dividing process being performed on both sides of the electrode foil. This is followed by a film formation step (step S04 and / or step S05) during the dividing process, and then the second dividing process (step S06), which results in the dividing process being performed on one side and then divided on the other side. This method of performing the second dividing process on both sides of the electrode foil is preferred in terms of productivity.

[0068] Even if the first film formation step and the inter-cutting film formation step are not performed, performing the cutting step multiple times makes it easier to curve the foil smoothly during winding. However, by performing the first film formation step and the inter-cutting film formation step, the strength of the foil gradually increases, making it easier to form deep cut portions without bending the foil. Furthermore, even if only the inter-cutting film formation step is performed, it becomes even easier to curve the foil smoothly during winding. However, performing the first film formation step and the inter-cutting film formation step further reduces the risk of bending the foil, making it easier to form deep cut portions.

[0069] (Wound Capacitor) A typical example of a wound capacitor is an electrolytic capacitor, and examples of the electrolytic capacitor include a non-solid electrolytic capacitor in which the electrolyte is liquid and a dielectric film is formed on the anode foil, a solid electrolytic capacitor in which the electrolyte is solid and a dielectric film is formed on the anode foil, a hybrid electrolytic capacitor in which the electrolyte is both liquid and solid, and a bipolar electrolytic capacitor in which a dielectric film is formed on both the anode foil and the cathode foil.

[0070] A wound electrolytic capacitor is manufactured by placing a capacitor element impregnated with an electrolyte in a cylindrical outer case with a bottom, pulling out the anode and cathode terminals, sealing them with a seal, and then performing an aging process. The capacitor element is a wound body in which an anode foil and a cathode foil are stacked and wound with a separator between them. Electrode foil 1 is used for the anode foil, the cathode foil, or both. The separator is made of paper, synthetic fiber, or the like, and prevents shorting between the anode foil and the cathode foil.

[0071] 3 is a schematic diagram showing the state of the electrode foil 1 after winding to form a capacitor element. In this electrode foil 1, multiple cracks 4 share and bear the bending stress, and the bending stress is distributed among each crack 4. The cracks 4 have progressed deeply due to multiple cutting processes, and even if the curvature of the winding is large, the cracks 4 open wide and curve smoothly. This prevents the electrode foil 1 from being subjected to stress that would buckle or break the core 2.

[0072] Furthermore, since the cracks 4 are formed through multiple cutting processes, the elongation of the electrode foil 1 is suppressed, the surface expansion ratio does not decrease, and the groove width of the cracks 4 does not increase, thereby suppressing a decrease in the capacitance of the wound capacitor.

[0073] Example 1 An electrode foil 1 illustrating this embodiment was fabricated as follows. First, an aluminum foil having a thickness of 120 μm, a width of 10 mm, a length of 55 mm, and a purity of 99.9% by weight or more was used as a substrate. Then, surface-expanding treatment was performed to form surface-expanding portions 3 on both sides of this aluminum foil. Specifically, the aluminum foil was immersed in an acidic aqueous solution having a solution temperature of 70° C. and a hydrochloric acid concentration of 1 mol / L and a sulfuric acid concentration of 3 mol / L, and subjected to direct current electrolysis at a current density of 0.50 A / cm. 2 A constant current of 0.40 A / cm was applied to the substrate for approximately 20 seconds. After that, the substrate was immersed in an acidic aqueous solution with a nitric acid concentration of 1 mol / L at a liquid temperature of 90°C, and subjected to direct current electrolysis at a current density of 0.40 A / cm. 2 A constant current of 1000 volts was applied for 90 seconds.

[0074] The electrode foil 1 with the enlarged surface portion 3 formed thereon was subjected to a hydration treatment. In the hydration treatment, the electrode foil 1 was immersed in distilled water at 95°C for 30 minutes. As a result, a hydrated oxide film was formed on the uneven surface of the enlarged surface portion 3. After this hydration treatment, the first cutting treatment was performed. In the first cutting treatment, the electrode foil 1 was pressed against a φ6 mm shaft at a wrap angle of 180 degrees, which indicates the area of ​​contact between the shaft and the electrode foil. This caused cracks 4 to form in the enlarged surface portion 3. The length of the electrode foil 1 was stretched by approximately 1.0% by the first cutting treatment.

[0075] After the first cutting treatment, the same hydration treatment was carried out again, and then chemical conversion treatment was carried out. The chemical conversion treatment was carried out by immersing the specimen in a 40 g / L aqueous solution of boric acid at a liquid temperature of 95°C and applying a current of 0.50 A / cm 2 A voltage of 30 V was applied while a constant current density of 1000 kJ / cm was applied. The voltage was applied for about 20 minutes, and a dielectric film 5 with a withstand voltage equivalent to about 30 V was formed.

[0076] After this chemical conversion treatment, the electrode foil 1 was subjected to a dividing treatment again. In the second dividing treatment, the electrode foil 1 was pressed against a shaft with a diameter of 10 mm at a wrap angle of 180 degrees. This caused the cracks 4 in the enlarged surface portion 3 to grow deeper and longer. After the second dividing treatment, the electrode foil 1 was subjected to a chemical conversion treatment again, and a dielectric coating 5 was formed on the inner surface of the cracks 4 as well.

[0077] The length of the electrode foil 1 was further extended by 0.3 to 0.4% by the subsequent cutting process compared to when the cutting process was not performed. The length of the electrode foil 1 after the second cutting process was extended by 1.37% compared to when the cutting process was not performed.

[0078] (Comparative Example) Electrode foils of Comparative Example 1 and Comparative Example 2 were produced in comparison with Example 1. The electrode foil of Comparative Example 1 was not subjected to a dividing treatment, and cracks 4 were not formed. In Comparative Example 1, a hydration treatment and a chemical conversion treatment were carried out after a surface enlargement treatment. The hydration treatment and chemical conversion treatment of Comparative Example 1 were the same as those of Example 1.

[0079] The electrode foil of Comparative Example 2 was subjected to a cutting treatment only once. A hydration treatment was performed before the cutting treatment, and after the cutting treatment was completed, a further hydration treatment was performed, followed by a chemical conversion treatment. The cutting treatment of Comparative Example 2 was the same as the initial cutting treatment of Example 1. The hydration treatments and chemical conversion treatments of Comparative Examples 1 and 2 were the same as the hydration treatment and chemical conversion treatment of Example 1. The length of the electrode foil of Comparative Example 2 that had undergone a single cutting treatment was elongated by 0.80% compared to when the cutting treatment was not performed.

[0080] (SEM Observation) After the initial cutting process was completed, a cross section of the electrode foil 1 of Example 1 was observed at a magnification of 350 times using a scanning electron microscope. The results are shown in (a1) and (a2) of Figure 4. (a1) of Figure 4 is a cross-sectional SEM image of Example 1 after the initial cutting process, and (a2) has a thick line added to highlight the crack 4. As shown in (a1) and (a2) of Figure 4, in the initial cutting process, the crack 4 did not reach the core portion 2, and was approximately 60% deep into the core portion 2. However, no buckling or fracture was observed in the core portion 2.

[0081] Furthermore, after the next cutting process was completed, a cross section of the electrode foil 1 of Example 1 was observed at 350x magnification using a scanning electron microscope. The results are shown in (b1) and (b2) of Figure 4. (b1) of Figure 4 is a cross-sectional SEM image of Example 1 after the next cutting process, and (b2) has a thick line added to highlight the crack 4. As shown in (b1) and (b2) of Figure 4, the crack 4, which did not reach the core portion 2 in the initial cutting process, has progressed in the depth direction, completely dividing the expanded surface portion 3 in the thickness direction, with its deepest part reaching the surface of the core portion 2. However, no buckling or fracture is observed in the core portion 2.

[0082] After the initial cutting process, the surface of the electrode foil 1 of Example 1 was observed at 150x magnification using a scanning electron microscope. The results are shown in (a1) and (a2) of Figure 5. (a1) of Figure 5 is an SEM image of the surface after the initial cutting process in Example 1, and (a2) has a thick line added to highlight the crack 4. As shown in (a1) and (a2) of Figure 5, after the initial cutting process, the crack 4 is short compared to the longitudinal direction of the electrode foil 1, and the linear distance between both ends is at most approximately 600 µm relative to the width of the electrode foil 1. However, no buckling or breakage is observed in the core portion 2.

[0083] Furthermore, after the next cutting process was completed, the surface of the electrode foil 1 of Example 1 was observed at 150x magnification using a scanning electron microscope. The results are shown in Figure 5 (b1) and (b2). Figure 5 (b1) is an SEM image of the surface after the next cutting process in Example 1, and (b2) adds thick lines to highlight the cracks 4. As shown in Figure 5 (b1) and (b2), the cracks 4, which were short during the initial cutting process, propagated in the strip width direction, reducing the intermittent area and increasing continuity. Furthermore, in many of the cracks 4, the linear distance between both ends exceeded approximately 100 μm relative to the strip width of the electrode foil 1, and some of the longest cracks exceeded both ends of the SEM observation field (approximately 800 μm). However, no buckling or fracture was observed in the core portion 2.

[0084] (Flexibility Test) One end of Example 1, Comparative Example 1, and Comparative Example 2, all of which had the same length and width, was fixed, and the other end was left free, and photographs of Example 1, Comparative Example 1, and Comparative Example 2 hanging down under their own weight were taken. The results are shown in Fig. 6. In Fig. 6, the electrode foil 1 of Example 1 is in the foreground, Comparative Example 2 is in the middle, and Comparative Example 1 is in the background.

[0085] Comparative Example 2 was subjected to a single cutting process and has crack 4. Therefore, Comparative Example 2 is more curved and sagging than Comparative Example 1, which was not subjected to a cutting process. That is, Comparative Example 2 is more flexible than Comparative Example 1, and the curvature that can be smoothly bent is larger. Example 1 was subjected to two cutting processes and crack 4 reached deep into the enlarged surface portion 3. Therefore, Example 1 is more curved and sagging than Comparative Example 2. That is, Example 1 is even more flexible than Comparative Example 2, and the curvature that can be smoothly bent is larger.

[0086] In this way, by performing the dividing process multiple times, the crack 4 progresses deeper into the electrode foil 1. It was also confirmed that by performing the dividing process multiple times, the flexibility of the electrode foil 1 increases, and the curvature at which the electrode foil 1 can be smoothly bent increases.

[0087] Furthermore, an Erichsen test was performed on the electrode foil 1 of Example 1 and Comparative Example 2. In the Erichsen test, the electrode foil 1 of Example 1 and Comparative Examples 1 and 2 were clamped at 10 kN between a die and blank holder having an inner diameter of 33 mm, and pressed into place with a spherical punch and a chisel-shaped punch. The spherical punch had a diameter of 20 mm. The chisel-shaped punch had a width of 30 mm, and its tip was spherical with a diameter of 4 mm and a radius of 2 mm in cross section. The chisel-shaped punch was pressed into the electrode foil 1 so as to be perpendicular to the strip width direction. The punch pressing speed was 0.5 mm / min.

[0088] The flexibility measured by the Erichsen test is shown in Table 1 below. Table 1 also lists the improvement in flexibility of Example 1 relative to that of Comparative Example 2. Here, the flexibility value is a numerical value defined as the slope of the load change relative to the elongation of the electrode foil 1. The smaller the change in load value relative to the elongation (the smaller the slope), that is, the smaller the flexibility value in the table, the more flexible (softer) the electrode foil 1 is, and the less force it requires to deform. (Table 1)

[0089] As shown in Table 1, the Erichsen test also confirmed that Example 1 had improved flexibility compared to Comparative Example 2. That is, the cracks 4 were deeper than those in Comparative Example 2 and extended longer in the strip width direction of the electrode foil 1, so that the electrode foil 1 of Example 1 had higher flexibility than Comparative Example 2.

[0090] (Presence or absence of frills) The long sides of Example 1, in which the dividing process was performed twice, and Comparative Example 2, in which the dividing process was performed once, were photographed. The results are shown in Figure 7. Figure 7(a) is a photograph of Comparative Example 2, and (b) is a photograph of Example 1. As shown in Figure 7(a), the distance between both ends of the frills in Comparative Example 2 was approximately 8 mm. On the other hand, as shown in Figure 7(b), the distance between both ends of the frills in Example 1 was approximately 40 mm. This confirms that Example 1 has fewer frills than Comparative Example 2. The distance between both ends of the frills is, in other words, the distance between the peaks of two mountains or the distance between the bottoms of two valleys.

[0091] The flatness of the areas near the long sides of Example 1 and Comparative Example 2 was measured. The flatness is the ratio of the difference between the creepage distance measured along the shape of the frill between both ends and the linear distance between both ends to the linear distance between both ends of the frill. The flatness measurement results are shown in Table 2 below. (Table 2)

[0092] As shown in Table 2, the flatness measurement results also confirm that Example 1 has greater flatness near the long sides than Comparative Example 2. Therefore, electrode foil 1 can be wound more densely, and the contained electrode foil 1 is longer even with the same volume, improving the capacitance of the wound capacitor.

[0093] (Aging Evaluation) The electrode foil 1 of Example 1 and the electrode foil of Comparative Example 2 were wound as anode foils to produce capacitor elements. Aluminum foil was used as the cathode foil. The cathode foil had an enlarged surface portion 3 formed thereon, but no dielectric coating 5 formed thereon. Cellulose fiber was used as the separator.

[0094] The capacitor element using electrode foil 1 of Example 1 and the capacitor element using electrode foil of Comparative Example 2 were impregnated with an electrolyte and housed in a cylindrical outer case with a bottom. The anode and cathode terminals were pulled out and sealed with a sealer. A gamma-butyrolactone solution of amidinium phthalate salt was used as the electrolyte. In this way, a wound capacitor using electrode foil 1 of Example 1 and a wound capacitor using electrode foil of Comparative Example 2 were produced.

[0095] The fabricated wound capacitors were subjected to an aging treatment, and the amount of electricity required for the aging treatment was measured. The aging treatment was performed by applying a rated voltage at a temperature of 100°C. During the aging treatment, the change in current flowing between the anode and cathode terminals was measured. The amount of electricity (C) was then measured when the current value decreased to 30% of the value at the start of aging.

[0096] The measurement results of the quantity of electricity are shown in Table 3 below. Table 3 below shows the calculated ratio of the quantity of electricity of Example 1 to the quantity of electricity of Comparative Example 2. (Table 3)

[0097] As shown in Table 3, the amount of electricity consumed in the aging treatment in Example 1 was smaller than that in Comparative Example 2. This confirmed that in Example 1, cracks 4 were deeper than in Comparative Example 2 and extended longer in the strip width direction of electrode foil 1, and therefore the occurrence of finer cracks was suppressed compared to Comparative Example 2.

[0098] The total elongation rate during the cutting process of the wound capacitor of Example 1 was greater than that of Comparative Example 2. However, the wound capacitor of Example 1 could be curved more smoothly even with a larger curvature than that of Comparative Example 2, and a longer electrode foil 1 could be accommodated within the same volume. Therefore, the wound capacitor of Example 1 had a higher capacitance than that of Comparative Example 2.

[0099] 1 Electrode foil 2 Core portion 3 Enlarged surface portion 4 Crack 5 Dielectric film

Claims

1. A method for manufacturing an electrode foil, comprising: a surface-expanding step of forming an enlarged portion on the surface of a band-shaped foil; and a dividing step of forming a plurality of cracks that divide the enlarged portion, wherein the dividing step is performed a plurality of times.

2. A method for manufacturing an electrode foil according to claim 1, further comprising a step of forming an oxide film on the enlarged surface portion during the cutting process between any of the cutting steps.

3. The method for manufacturing an electrode foil according to claim 2, wherein the film-forming step during the dividing process includes a hydration process for forming a hydrated oxide film on the enlarged surface portion, or a chemical conversion process for forming a film by applying a voltage, or both.

4. A method for manufacturing an electrode foil according to claim 1, further comprising a first film forming step of forming an oxide film on the enlarged surface portion after the surface enlarging step and before the first dividing step.

5. A method for producing an electrode foil according to claim 4, further comprising an inter-cutting film forming step of forming an oxide film on the enlarged surface portion between any of the multiple cutting steps, and the hardness of the electrode foil obtained in the inter-cutting film forming step is made higher than the hardness of the electrode foil obtained in the first film forming step.

6. The method of manufacturing an electrode foil according to claim 1, wherein during any one of the multiple cutting steps, the hardness of the foil before the next cutting step is made higher than that of the previous foil.

7. A method for manufacturing an electrode foil according to claim 1, characterized in that the hardness of the foil cut in the nth cutting step among the multiple cutting steps is made higher than the hardness of the foil cut in any cutting step prior to the (n-1)th cutting step.

8. A method for manufacturing an electrode foil according to claim 1, wherein in the dividing step, the cracks are formed with a groove width of 50 μm or less (including 0) while the foil is kept flat.

9. A method for manufacturing an electrode foil as described in claim 1, characterized in that in the multiple dividing steps, the depth of the crack formed in the previous dividing step is increased and a new crack is formed.

10. A method for manufacturing an electrode foil according to claim 1, further comprising, after the final dividing step, a chemical conversion treatment for forming an oxide film on the inner surface of the crack while maintaining the crack openable and closable.

11. A method for producing a wound capacitor, comprising a winding step of winding the electrode foil obtained by the method of claim 1.

12. An electrode foil comprising: a band-shaped foil; an expanded portion formed on the surface of the foil; a core portion which is the remaining portion of the foil excluding the expanded portion; a first type of crack dividing the expanded portion and having a depth of less than 70% of the distance from the surface of the foil to the core portion; and a second type of crack dividing the expanded portion and having a depth of 70% or more of the distance from the surface of the foil to the core portion, wherein the proportion of the first type of cracks is 10% or more and 50% or less, and the proportion of the second type of cracks is 50% or more and 90% or less.

Citation Information

Patent Citations

  • Electrode structure and manufacturing method thereof

    JP2022532284A

  • Electrode foil, winding capacitor, electrode foil manufacturing method, and winding capacitor manufacturing method

    WO2017171028A1

  • Aluminum conversion foil, electrode for aluminum electrolytic capacitors, and method for manufacturing aluminum conversion foil

    WO2020241174A1

  • Electrode foil for electrolytic capacitor, and electrolytic capacitor

    WO2022137582A1

Cited By

  • Laminated foil for aluminum electrolytic capacitor, preparation method of laminated foil and aluminum electrolytic capacitor

    CN119889932A