Resin composition, prepreg, resin-bearing film, resin-bearing metal foil, metal-clad laminate sheet, and wiring board

The resin composition, featuring a boron nitride filler with specific particle size distribution and polyphenylene ether compounds, addresses the challenges of low dielectric constants and high thermal conductivity, achieving excellent adhesion and moldability for high-frequency and high-thermal applications.

WO2024202841A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/007178
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current resin compositions for high-frequency and high-thermal applications, such as millimeter wave radar boards and power amplifier boards, face challenges in achieving low dielectric constants, high thermal conductivity, and sufficient adhesion, with existing materials like silica not providing adequate thermal conductivity and boron nitride compositions lacking sufficient adhesion.

Method used

A resin composition incorporating a radically polymerizable compound and a boron nitride filler with specific particle size distribution, combined with polyphenylene ether compounds, to achieve low dielectric properties, high thermal conductivity, and improved adhesion, suitable for use in prepregs, metal-clad laminates, and wiring boards.

Benefits of technology

The resin composition achieves low dielectric constants, high thermal conductivity, and excellent adhesion, making it suitable for high-frequency and high-thermal applications, such as millimeter wave radar boards and power amplifier boards, while maintaining moldability and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007178_03102024_PF_FP_ABST
    Figure JP2024007178_03102024_PF_FP_ABST
Patent Text Reader

Abstract

One aspect of the present invention relates to a resin composition comprising a radically polymerizable compound (A) and an inorganic filler (B), wherein the inorganic filler (B) contains a boron nitride filler (b1), and, in the particle size distribution of the boron nitride filler (b1), the particle diameter (D10) at the 10% cumulative value is 0.5-2.0 µm, the particle diameter (D50) at the 50% cumulative value is 4.0-6.0 µm, and the particle diameter (D90) at the 90% cumulative value is 6.5-20.0 µm.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, prepreg, resin-coated film, resin-coated metal foil, metal-clad laminate, and wiring board

[0001] The present invention relates to a resin composition, a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board.

[0002] As the amount of information processed increases in various electronic devices, packaging technologies such as higher integration of semiconductor devices, higher density wiring, and multi-layering are advancing. Furthermore, wiring boards used in various electronic devices are required to be high-frequency compatible, such as millimeter-wave radar boards for automotive applications. To increase the signal transmission speed, wiring boards used in various electronic devices are required to reduce loss during signal transmission, and this is particularly true for high-frequency compatible wiring boards. To meet this requirement, substrate materials for constructing wiring boards used in various electronic devices are required to have low dielectric constants and dielectric loss tangents.

[0003] As such a substrate material, for example, a PPE-containing resin composition containing PPE (polyphenylene ether), a crosslinkable curable compound, a phosphaphenanthrene derivative, and silica has been reported (Patent Document 1).

[0004] On the other hand, electronic materials used in PA (power amplifier) ​​substrates for base stations and the like are required to have not only low dielectric constants and dielectric loss tangents but also high thermal conductivity. In this regard, the inorganic filler (silica) contained in the resin composition of Patent Document 1 may not be able to provide sufficient thermal conductivity.

[0005] In response to this, one technique that has been reported to date for improving the thermal conductivity of a resin composition is to use boron nitride as an inorganic filler with high thermal conductivity (Patent Document 2).

[0006] It is believed that the low dielectric properties, thermal conductivity, and heat resistance of the cured resin composition can be ensured by using the boron nitride filler and polyphenylene ether compound described in Patent Document 2. However, the resin composition described in Patent Document 2 may not have sufficient adhesion required for a substrate product.

[0007] The present invention has been made in view of the above circumstances, and aims to provide a resin composition that can give a cured product having low dielectric properties (low dielectric constant) and high thermal conductivity, and that further has excellent formability and adhesion when made into a substrate. Another aim of the present invention is to provide a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board that can be obtained using the resin composition.

[0008] JP 2015-67700 A International Publication No. 2021 / 059911

[0009] As a result of extensive investigations, the present inventors have found that the above object can be achieved by the following constitution, and have achieved the present invention through further investigations.

[0010] That is, a resin composition according to one embodiment of the present invention comprises a radical polymerizable compound (A) and an inorganic filler (B), the inorganic filler (B) comprises a boron nitride filler (b1), and the particle size distribution of the boron nitride filler (b1) is characterized in that the particle size (D10) at 10% cumulative total is 0.5 to 2.0 μm, the particle size (D50) at 50% cumulative total is 4.0 to 6.0 μm, and the particle size (D90) at 90% cumulative total is 6.5 to 20.0 μm.

[0011] Fig. 1 is a schematic cross-sectional view showing an example of a prepreg according to an embodiment of the present invention. Fig. 2 is a schematic cross-sectional view showing an example of a metal-clad laminate according to an embodiment of the present invention. Fig. 3 is a schematic cross-sectional view showing an example of a wiring board according to an embodiment of the present invention. Fig. 4 is a schematic cross-sectional view showing an example of a resin-coated metal foil according to an embodiment of the present invention. Fig. 5 is a schematic cross-sectional view showing an example of a resin-coated film according to an embodiment of the present invention.

[0012] Hereinafter, embodiments of the present invention will be specifically described, but the present invention is not limited to these.

[0013] [Resin Composition] The resin composition according to an embodiment of the present invention contains a radically polymerizable compound (A) and an inorganic filler (B). The inorganic filler (B) contains a boron nitride filler (b1). The particle size distribution of the boron nitride filler (b1) is such that the particle size (D10) at 10% cumulative total is 0.5 to 2.0 μm, the particle size (D50) at 50% cumulative total is 4.0 to 6.0 μm, and the particle size (D90) at 90% cumulative total is 6.5 to 20.0 μm.

[0014] The above-mentioned constitution makes it possible to obtain a resin composition having a cured product with low dielectric properties (particularly, a dielectric constant: Dk) and high thermal conductivity, and excellent adhesion and moldability when formed into a substrate, etc. Furthermore, by using the resin composition, it is possible to provide a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board having the above-mentioned excellent performance.

[0015] The cured product of the resin composition of this embodiment preferably has a thermal conductivity of 1.0 W / mK or more and a relative dielectric constant of 4.0 or less, where the relative dielectric constant is the relative dielectric constant at a frequency of 10 GHz.

[0016] First, each component of the resin composition of the present embodiment will be described.

[0017] (Radical Polymerizable Compound (A)) The radical polymerizable compound (A) of the present embodiment is not particularly limited as long as it is a compound having radical polymerizability. More specific examples of the radical polymerizable compound (A) preferably include at least one selected from the group consisting of a polyphenylene ether compound having a carbon-carbon unsaturated double bond in the molecule, a hydrocarbon-based compound having a carbon-carbon unsaturated double bond in the molecule, a maleimide compound, and an allyl compound.

[0018] Furthermore, the radical polymerizable compound (A) preferably contains a radical polymerizable compound (A1) such as a compound having a reactive unsaturated group or a compound having a maleimide group, and more preferably contains, in addition to the radical polymerizable compound (A1), a radical polymerizable compound (another radical polymerizable compound) (A2) other than the radical polymerizable compound (A1). Each of these will be described below.

[0019] (Radical Polymerizable Compound (A1)) First, the radical polymerizable compound (A1) will be described. The radical polymerizable compound (A1) used in the present embodiment is not particularly limited as long as it is a compound having radical polymerizability. Examples include compounds having a reactive unsaturated group such as a carbon-carbon unsaturated double bond, and compounds having a maleimide group. By using such a radical polymerizable compound (A1), it is possible to obtain a resin composition having low dielectric properties in the cured product.

[0020] The molecular weight of the radical polymerizable compound (A1) is preferably a weight average molecular weight of about 100 to 3000. The weight average molecular weight may be measured by a general molecular weight measurement method, and specific examples thereof include values ​​measured using gel permeation chromatography (GPC).

[0021] More specifically, the radical polymerizable compound (A1) preferably includes at least one selected from the group consisting of a polyphenylene ether compound having a carbon-carbon unsaturated double bond in the molecule, a hydrocarbon compound having a carbon-carbon unsaturated double bond in the molecule, and a maleimide compound. Each of these compounds will be described in more detail below.

[0022] Polyphenylene ether compounds Examples of polyphenylene ether compounds having a carbon-carbon unsaturated double bond in the molecule include polyphenylene ether compounds having a group represented by the following formula (1) or formula (2). It is believed that the inclusion of such a modified polyphenylene ether compound results in a resin composition that can give a cured product with low dielectric properties and high heat resistance.

[0023]

[0024] In formula (1), s represents an integer of 0 to 10. Z represents an arylene group. 1 ~R 3 are independent of each other. That is, R 1 ~R 3may be the same group or different groups. 1 ~R 3 represents a hydrogen atom or an alkyl group.

[0025] In addition, in formula (1), when s is 0, this indicates that Z is directly bonded to the end of the polyphenylene ether.

[0026] The arylene group represented by Z is not particularly limited. Examples of the arylene group include monocyclic aromatic groups such as a phenylene group, and polycyclic aromatic groups in which the aromatic ring is not monocyclic but is a polycyclic aromatic ring such as a naphthalene ring. The arylene group also includes derivatives in which a hydrogen atom bonded to the aromatic ring is substituted with a functional group such as an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group. The alkyl group is not particularly limited, and is preferably an alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0027]

[0028] In formula (2), R 4 represents a hydrogen atom or an alkyl group. The alkyl group is not particularly limited, and is preferably, for example, an alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0029] Preferred specific examples of the substituent represented by formula (1) include, for example, a substituent containing a vinylbenzyl group. Examples of the substituent containing a vinylbenzyl group include, for example, a substituent represented by formula (3) below. Furthermore, examples of the substituent represented by formula (2) include an acrylate group and a methacrylate group.

[0030]

[0031] More specific examples of the substituent include vinylbenzyl groups (ethenylbenzyl groups) such as p-ethenylbenzyl and m-ethenylbenzyl groups, vinylphenyl groups, acrylate groups, and methacrylate groups.

[0032] In the resin composition of the present embodiment, it is more preferable that the polyphenylene ether compound has a group represented by the above formula (2), because this has the advantage of improving the reactivity with the crosslinking agent and making it easier to obtain a cured resin product with high heat resistance.

[0033] The polyphenylene ether compound has a polyphenylene ether chain in the molecule, and preferably has, for example, a repeating unit represented by the following formula (4) in the molecule.

[0034]

[0035] In formula (4), t represents 1 to 50. 5 ~R 8 are independent of each other. That is, R 5 ~R 8 may be the same group or different groups. 5 ~R 8 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group, among which a hydrogen atom and an alkyl group are preferred.

[0036] R 5 ~R 8 Specific examples of the functional groups mentioned in the above include the following:

[0037] The alkyl group is not particularly limited, but is preferably an alkyl group having 1 to 18 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0038] The alkenyl group is not particularly limited, but is preferably an alkenyl group having 2 to 18 carbon atoms, and more preferably an alkenyl group having 2 to 10 carbon atoms. Specific examples include a vinyl group, an allyl group, and a 3-butenyl group.

[0039] The alkynyl group is not particularly limited, but is preferably an alkynyl group having 2 to 18 carbon atoms, and more preferably an alkynyl group having 2 to 10 carbon atoms. Specific examples include an ethynyl group and a prop-2-yn-1-yl group (propargyl group).

[0040] The alkylcarbonyl group is not particularly limited as long as it is a carbonyl group substituted with an alkyl group, but for example, an alkylcarbonyl group having 2 to 18 carbon atoms is preferred, and an alkylcarbonyl group having 2 to 10 carbon atoms is more preferred. Specific examples include an acetyl group, a propionyl group, a butyryl group, an isobutyryl group, a pivaloyl group, a hexanoyl group, an octanoyl group, and a cyclohexylcarbonyl group.

[0041] The alkenylcarbonyl group is not particularly limited as long as it is a carbonyl group substituted with an alkenyl group, but for example, an alkenylcarbonyl group having 3 to 18 carbon atoms is preferred, and an alkenylcarbonyl group having 3 to 10 carbon atoms is more preferred. Specific examples include an acryloyl group, a methacryloyl group, and a crotonoyl group.

[0042] The alkynylcarbonyl group is not particularly limited as long as it is a carbonyl group substituted with an alkynyl group, but for example, an alkynylcarbonyl group having 3 to 18 carbon atoms is preferred, and an alkynylcarbonyl group having 3 to 10 carbon atoms is more preferred. Specific examples include a propioloyl group.

[0043] The average number of the substituents (number of terminal functional groups) at the molecular terminals per molecule of the polyphenylene ether compound is not particularly limited. Specifically, it is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1.5 to 3. If the number of terminal functional groups is too small, it tends to be difficult to obtain a cured product with sufficient heat resistance. On the other hand, if the number of terminal functional groups is too large, the reactivity becomes too high, which may cause problems such as reduced shelf life and reduced fluidity of the resin composition. In other words, when such a polyphenylene ether compound is used, insufficient fluidity may cause molding defects such as the generation of voids during multilayer molding, making it difficult to obtain a highly reliable printed wiring board.

[0044] The number of terminal functional groups of a polyphenylene ether compound may be, for example, a numerical value representing the average number of the substituents per molecule of all modified polyphenylene ether compounds present in 1 mole of the polyphenylene ether compound. The number of terminal functional groups can be measured, for example, by measuring the number of hydroxyl groups remaining in the obtained modified polyphenylene ether compound and calculating the difference from the number of hydroxyl groups in the polyphenylene ether before modification. This difference from the number of hydroxyl groups in the polyphenylene ether before modification is the number of terminal functional groups. The number of hydroxyl groups remaining in the modified polyphenylene ether compound can be measured by adding a quaternary ammonium salt (tetraethylammonium hydroxide) that associates with hydroxyl groups to a solution of the modified polyphenylene ether compound and measuring the UV absorbance of the resulting mixed solution.

[0045] Examples of the polyphenylene ether compound of the present embodiment include a modified polyphenylene ether compound represented by the following formula (5) and a modified polyphenylene ether compound represented by the following formula (6). Furthermore, as the polyphenylene ether compound of the present embodiment, these modified polyphenylene ether compounds may be used alone, or these two types of modified polyphenylene ether compounds may be used in combination.

[0046]

[0047]

[0048] In formula (5) and formula (6), R 9 ~R 16 and R 17 ~R 24 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group. 1 and X 2 each independently represents a substituent having a carbon-carbon unsaturated double bond. A and B represent repeating units represented by the following formulas (7) and (8), respectively. In addition, in formula (6), Y represents a linear, branched, or cyclic hydrocarbon having 20 or less carbon atoms.

[0049]

[0050]

[0051] In formula (7) and formula (8), m and n each represent an integer of 0 to 20. 25 ~R 28 and R 29 ~R 32 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group.

[0052] The modified polyphenylene ether compound represented by the formula (5) and the modified polyphenylene ether compound represented by the formula (6) are not particularly limited as long as they satisfy the above-mentioned constitution. Specifically, in the formulas (5) and (6), R 9 ~R 16 and R 17 ~R 24 As described above, each of R is independent. 9 ~R 16 and R 17 ~R 24may be the same group or different groups. 9 ~R 16 and R 17 ~R 24 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group, among which a hydrogen atom and an alkyl group are preferred.

[0053] In formula (7) and formula (8), m and n each preferably represent a value of 0 to 20, as described above. Furthermore, it is preferable that m and n represent a numerical value such that the sum of m and n is 1 to 30. Therefore, it is more preferable that m represents a value of 0 to 20, n represents a value of 0 to 20, and the sum of m and n represents a value of 1 to 30. Furthermore, R 25 ~R 28 and R 29 ~R 32 are independent of each other. That is, R 25 ~R 28 and R 29 ~R 32 may be the same group or different groups. 25 ~R 28 and R 29 ~R 32 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group, among which a hydrogen atom and an alkyl group are preferred.

[0054] R 9 ~R 32 is R in the above formula (4). 5 ~R 8 is the same as

[0055] In the formula (6), as described above, Y is a linear, branched, or cyclic hydrocarbon having 20 or less carbon atoms. Examples of Y include a group represented by the following formula (9).

[0056]

[0057] In the formula (9), R 33 and R34 are each independently a hydrogen atom or an alkyl group. Examples of the alkyl group include a methyl group. Examples of the group represented by formula (9) include a methylene group, a methylmethylene group, and a dimethylmethylene group, and among these, a dimethylmethylene group is preferred.

[0058] In the formula (5) and the formula (6), X 1 and X 2 are each independently a substituent having a carbon-carbon unsaturated double bond. 1 and X 2 There are no particular limitations on the substituent X as long as it is a substituent having a carbon-carbon unsaturated double bond. 1 and X 2 Examples of the substituents include the substituents represented by the formula (1) and the substituents represented by the formula (2). In the modified polyphenylene ether compound represented by the formula (5) and the modified polyphenylene ether compound represented by the formula (6), X 1 and X 2 may be the same substituent or different substituents.

[0059] More specific examples of the modified polyphenylene ether compound represented by the formula (5) include modified polyphenylene ether compounds represented by the following formula (10).

[0060]

[0061] More specific examples of the modified polyphenylene ether compound represented by formula (6) include a modified polyphenylene ether compound represented by formula (11) below and a modified polyphenylene ether compound represented by formula (12) below.

[0062]

[0063]

[0064] In the above formulas (10) and (11), m and n are the same as m and n in the above formulas (7) and (8). 1 ~R 3 , p and Z are R in the above formula (1), respectively. 1 ~R 3 , s, and Z. In the formulas (11) and (12), Y is the same as Y in the formula (9). In the formula (12), R 4 is R in the above formula (2). 4 is the same as

[0065] It is believed that by using the modified polyphenylene ether compound as described above, it is possible to improve high Tg and adhesion while maintaining low dielectric properties such as low dielectric constant and excellent heat resistance.

[0066] The modified polyphenylene ether compounds may be used singly or in combination of two or more.

[0067] The polyphenylene ether compound used in the resin composition of this embodiment can be synthesized by a known method, or a commercially available product can be used. Examples of commercially available products include "OPE-2st 1200" and "OPE-2st 2200" manufactured by Mitsubishi Gas Chemical Company, Inc., and "SA9000" manufactured by SABIC Innovative Plastics.

[0068] Hydrocarbon-based compound having a carbon-carbon unsaturated double bond in the molecule The hydrocarbon-based resin that can be used in this embodiment is not particularly limited as long as it is a hydrocarbon-based resin having an unsaturated double bond, and preferred examples thereof include hydrocarbon-based resins such as polyfunctional vinyl aromatic polymers, cyclic polyolefin resins, and vinyl aromatic compound-conjugated diene compound copolymers.

[0069] The polyfunctional vinyl aromatic polymer is preferably a polymer containing at least a polyfunctional vinyl aromatic compound and / or a derivative thereof polymerized therein, and is not particularly limited as long as it is a polymer containing a structure derived from a polyfunctional vinyl aromatic compound and / or a derivative thereof, and may be a polymer containing one or more polyfunctional vinyl aromatic compounds and / or a structure derived from a derivative thereof.

[0070] In addition to the structural units of the polyfunctional vinyl aromatic compound and / or its derivatives, the copolymer may further contain one or more structural units derived from a reactive monomer. The reactive monomer is not particularly limited, but may be, for example, a polyfunctional vinyl aromatic copolymer having structural units derived from a monovinyl aromatic compound such as styrene.

[0071] More specifically, examples of the polyfunctional vinyl compound include a polyfunctional vinyl compound having two or more vinyl groups in the molecule, such as divinylbenzene, divinylnaphthalene, divinylbiphenyl, and polybutadiene.

[0072] Maleimide Compound The maleimide resin usable in this embodiment is not particularly limited as long as it has a maleimide group in the molecule. Specific examples of the maleimide compound include monofunctional maleimide compounds having one maleimide group in the molecule, polyfunctional maleimide compounds having two or more maleimide groups in the molecule, and modified maleimide compounds. Examples of the modified maleimide compound include modified maleimide compounds in which a portion of the molecule is modified with an amine compound, modified maleimide compounds in which a portion of the molecule is modified with a silicone compound, and modified maleimide compounds in which a portion of the molecule is modified with both an amine compound and a silicone compound.

[0073] More specific examples include maleimide compounds having two or more N-substituted maleimide groups in one molecule, maleimide compounds having an indane structure, maleimide compounds having at least one group selected from an alkyl group having 6 or more carbon atoms and an alkylene group having 6 or more carbon atoms, and maleimide compounds having a benzene ring in the molecule.

[0074] The maleimide compound used in this embodiment may be a commercially available product, and examples thereof include BMI-4000, BMI-2300, BMI-TMH, BMI-4000, and BMI-5100 manufactured by Daiwa Chemical Industry Co., Ltd.; MIR-3000 and MIR-5000 manufactured by Nippon Kayaku Co., Ltd.; and BMI-689, BMI-1500, BMI-3000J, and BMI-5000 manufactured by Designer Molecules Inc.

[0075] (Other Radically Polymerizable Compounds (A2)) The resin composition of the present embodiment may further contain another radically polymerizable compound (A2) other than the above-described radically polymerizable compounds (polyphenylene ether compounds, hydrocarbon-based compounds, maleimide compounds). Such radically polymerizable compound (A2) is preferably a radically polymerizable compound that acts as a curing agent capable of reacting with the above-described radically polymerizable compound (A1) (polyphenylene ether compounds, hydrocarbon-based compounds, maleimide compounds, etc.).

[0076] Examples of such radically polymerizable compounds (A2) include allyl compounds, vinyl compounds, methacrylate compounds, acrylate compounds, and acenaphthylene compounds.

[0077] The allyl compound is a compound having an allyl group in the molecule, and examples thereof include triallyl isocyanurate compounds such as triallyl isocyanurate (TAIC), diallyl bisphenol compounds, and diallyl phthalate (DAP).

[0078] The vinyl compound is a compound having a vinyl group in its molecule. Examples of the vinyl compound include monofunctional vinyl compounds (monovinyl compounds) having one vinyl group in their molecule, and polyfunctional vinyl compounds having two or more vinyl groups in their molecule. Examples of the monofunctional vinyl compound include styrene compounds. Examples of the polyfunctional vinyl compound include polyfunctional aromatic vinyl compounds and vinyl hydrocarbon compounds. Examples of the polyfunctional aromatic vinyl compound include divinylbenzene. Examples of the vinyl hydrocarbon compound include polybutadiene compounds.

[0079] The methacrylate compound is a compound having a methacryloyl group in the molecule, and examples thereof include monofunctional methacrylate compounds having one methacryloyl group in the molecule and polyfunctional methacrylate compounds having two or more methacryloyl groups in the molecule. Examples of the monofunctional methacrylate compound include methyl methacrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate. Examples of the polyfunctional methacrylate compound include dimethacrylate compounds such as tricyclodecane dimethanol dimethacrylate (DCP).

[0080] The acrylate compound is a compound having an acryloyl group in the molecule, and examples thereof include monofunctional acrylate compounds having one acryloyl group in the molecule and polyfunctional acrylate compounds having two or more acryloyl groups in the molecule. Examples of the monofunctional acrylate compound include methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate. Examples of the polyfunctional acrylate compound include diacrylate compounds such as tricyclodecane dimethanol diacrylate.

[0081] The acenaphthylene compound is a compound having an acenaphthylene structure in the molecule. Examples of the acenaphthylene compound include acenaphthylene, alkylacenaphthylenes, halogenated acenaphthylenes, and phenylacenaphthylenes. Examples of the alkylacenaphthylenes include 1-methylacenaphthylene, 3-methylacenaphthylene, 4-methylacenaphthylene, 5-methylacenaphthylene, 1-ethylacenaphthylene, 3-ethylacenaphthylene, 4-ethylacenaphthylene, and 5-ethylacenaphthylene. Examples of the halogenated acenaphthylenes include 1-chloroacenaphthylene, 3-chloroacenaphthylene, 4-chloroacenaphthylene, 5-chloroacenaphthylene, 1-bromoacenaphthylene, 3-bromoacenaphthylene, 4-bromoacenaphthylene, and 5-bromoacenaphthylene. Examples of the phenylacenaphthylenes include 1-phenylacenaphthylene, 3-phenylacenaphthylene, 4-phenylacenaphthylene, and 5-phenylacenaphthylene. The acenaphthylene compound may be a monofunctional acenaphthylene compound having one acenaphthylene structure in the molecule, as described above, or a polyfunctional acenaphthylene compound having two or more acenaphthylene structures in the molecule.

[0082] In the present embodiment, among the above-mentioned radical polymerizable compounds, it is preferable to use, as the other radical polymerizable compound (A2), an allyl compound, a polyfunctional aromatic vinyl compound, a polyfunctional methacrylate compound, a polyfunctional acrylate compound, a polybutadiene compound, an acenaphthylene compound, a styrene compound, and the like.

[0083] The radical polymerizable compound (A) may be composed of the polyphenylene ether compound (A1), or may be composed of a radical polymerizable compound (another radical polymerizable compound) (A2) other than the polyphenylene ether compound (A1). In a preferred embodiment, the radical polymerizable compound (A) preferably contains the radical polymerizable compound (A1) described above, and more preferably contains the polyphenylene ether compound (A1) and the other radical polymerizable compound (A2). The other radical polymerizable compounds (A2) may be used alone or in combination of two or more.

[0084] The content of the radical polymerizable compound (A) in the resin composition of this embodiment is preferably about 50 to 100 mass % and more preferably about 60 to 80 mass % based on the total resin components in the resin composition (organic resin components in the resin composition). This is believed to more reliably achieve low dielectric properties in the cured product.

[0085] When the radical polymerizable compound (A) contains the radical polymerizable compound (A1), the content thereof is preferably 30 to 100 parts by mass, and more preferably 50 to 90 parts by mass, per 100 parts by mass of the radical polymerizable compound (A). When the content of the radical polymerizable compound (A1) is within the above range, the resin composition can be suitably cured, and the cured product can have a sufficiently high glass transition temperature while maintaining excellent low dielectric properties, interlayer adhesion, and flame retardancy.

[0086] (Other Thermosetting Resins and Curing Agents) The resin composition of the present embodiment may contain other thermosetting resins in addition to the radically polymerizable compound (A) described above.

[0087] Examples of thermosetting resins that can be used in this embodiment include epoxy compounds, cyanate ester compounds, phenol compounds, benzoxazine compounds, active ester compounds, etc. Among these, benzoxazine compounds are preferably used from the viewpoints of curability and moldability.

[0088] When the resin composition of the present embodiment contains the thermosetting resin in addition to the radical polymerizable compound (A), the content ratio thereof, i.e., the ratio of radical polymerizable compound (A):thermosetting resin, is preferably about 95:5 to 50:50 by mass.

[0089] (Inorganic Filler) Boron Nitride Filler (b1) The resin composition according to this embodiment contains an inorganic filler (B). The inorganic filler (B) contains a boron nitride filler (b1) having a predetermined particle size distribution. Specifically, in the particle size distribution of the boron nitride filler (b1), the particle size (D10) at 10% cumulative total is 0.5 to 2.0 μm, the particle size (D50) at 50% cumulative total is 4.0 to 6.0 μm, and the particle size (D90) at 90% cumulative total is 6.5 to 20.0 μm.

[0090] In the resin composition of this embodiment, by using a boron nitride filler (b1) having the particle size distribution described above as a boron nitride filler with high thermal conductivity, the resin composition becomes a foreign substance with good thermal conductivity, and good results are obtained in terms of moldability and adhesion when made into a substrate. If the particle size distribution of the boron nitride filler (b1) is outside the above range, the thermal conductivity tends to decrease and the moldability and adhesion tend to decrease.

[0091] In this specification, the particle size distribution is a value measured by particle size distribution measurement using a laser diffraction / scattering method, and can be measured using, for example, a laser diffraction / scattering particle size distribution measuring device "LA-960V2" (manufactured by HORIBA, Ltd.) used in the examples described later.

[0092] The boron nitride filler (b1) that can be used in this embodiment can be used as an inorganic filler contained in a resin composition, and is not particularly limited as long as it satisfies the above-mentioned particle size distribution requirements. Examples of boron nitride include hexagonal normal pressure phase (h-BN) and cubic high pressure phase (c-BN).

[0093] The average aspect ratio of the boron nitride filler (b1) is preferably 6 to 20. In this specification, the average aspect ratio is the value calculated by dividing the maximum length on the main surface of the boron nitride filler particle by the thickness in the direction perpendicular to the main surface. The maximum length and the thickness can be measured by observing the boron nitride filler (b1) with a scanning electron microscope (SEM), and the average aspect ratio can be calculated from these measured values. By ensuring that the average aspect ratio is 6 to 20, a resin composition can be obtained that forms a cured product with high thermal conductivity.

[0094] The content of the boron nitride filler (b1) is preferably 5 to 50 parts by volume relative to 100 parts by volume of the radically polymerizable compound (A). By adjusting the content to this range, it is believed that the effects achieved by the boron nitride filler (b1) as described above can be more reliably obtained. The content is more preferably in the range of 8 to 30 parts by volume, and even more preferably in the range of 10 to 25 parts by volume.

[0095] Silica filler (b2) The resin composition of this embodiment preferably further contains a silica filler (b2) as an inorganic filler other than the boron nitride filler (b1). The inclusion of the silica filler (b2) offers the advantages of reducing costs, ensuring adhesion, and improving thermal conductivity by increasing the loading of the inorganic filler.

[0096] The silica filler (b2) used in this embodiment is not particularly limited as long as it can be used as an inorganic filler for the resin composition. The silica in this embodiment may be a surface-treated silica filler or a non-surface-treated silica filler. In addition, examples of the surface treatment include treatment with a silane coupling agent.

[0097] Examples of the silane coupling agent include silane coupling agents having at least one functional group selected from the group consisting of a vinyl group, a styryl group, a methacryloyl group, an acryloyl group, and a phenylamino group. That is, the silane coupling agent includes compounds having at least one reactive functional group selected from a vinyl group, a styryl group, a methacryloyl group, an acryloyl group, and a phenylamino group, and further having a hydrolyzable group such as a methoxy group or an ethoxy group.

[0098] Examples of the silane coupling agent include those having a vinyl group, such as vinyltriethoxysilane and vinyltrimethoxysilane. Examples of the silane coupling agent include those having a styryl group, such as p-styryltrimethoxysilane and p-styryltriethoxysilane. Examples of the silane coupling agent include those having a methacryloyl group, such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropylethyldiethoxysilane. Examples of the silane coupling agent include those having an acryloyl group, such as 3-acryloxypropyltrimethoxysilane and 3-acryloxypropyltriethoxysilane. Examples of the silane coupling agent include those having a phenylamino group, such as N-phenyl-3-aminopropyltrimethoxysilane and N-phenyl-3-aminopropyltriethoxysilane.

[0099] The content of the silica filler (b2) is not particularly limited, but it is preferable that the volume content ratio of the boron nitride filler (b1) to the silica filler (b2) in the inorganic filler (B), i.e., the volume content of the boron nitride filler (b1) / the volume content of the silica filler (b2), is 1 to 4. This has the advantage of providing excellent adhesion and moldability while maintaining thermal conductivity.

[0100] The content of the silica filler (b2) is preferably 20 to 60 parts by volume, more preferably 30 to 50 parts by volume, based on 100 parts by volume of the radical polymerizable compound (A).

[0101] The inorganic filler (B) may further contain an inorganic filler other than the boron nitride filler (b1) and the silica filler (b2). The inorganic filler other than boron nitride and silica is not particularly limited as long as it can be used as an inorganic filler contained in the resin composition. Specific examples include metal oxides such as alumina filler, titanium oxide filler, magnesium oxide filler, and mica filler, metal hydroxides such as aluminum hydroxide filler and magnesium hydroxide filler, talc filler, aluminum borate filler, barium sulfate filler, aluminum nitride filler, silicon nitride filler, magnesium carbonate filler such as anhydrous magnesium carbonate filler, and calcium carbonate filler. Among these, anhydrous magnesium carbonate filler, alumina filler, and silicon nitride filler are preferred.

[0102] The inorganic fillers other than the boron nitride filler and the silica filler may be surface-treated or may not be surface-treated. Examples of the surface treatment include treatment with a silane coupling agent.

[0103] Furthermore, the total content of the inorganic filler (B) in the resin composition of this embodiment is preferably 5 to 70 parts by volume, and more preferably 30 to 60 parts by volume, per 100 parts by volume of the radical polymerizable compound (A).

[0104] (Phosphorus Compound (C)) The resin composition of the present embodiment preferably further contains a phosphorus-based compound (C), which can further enhance the flame retardancy.

[0105] The phosphorus compound (C) of this embodiment is not particularly limited as long as it has flame retardancy, but it preferably contains a compatible phosphorus compound (c1) that is compatible with the radical polymerizable compound (A) and an incompatible phosphorus compound (c2) that is incompatible with the radical polymerizable compound (A). This is thought to have the advantages of further enhancing flame retardancy and providing a resin composition with high heat resistance and adhesion.

[0106] The compatible phosphorus compound (c1) is not particularly limited as long as it acts as a flame retardant and is compatible with the radical polymerizable compound (A). Here, "compatible" means that the compound is finely dispersed in the radical polymerizable compound (A), for example, at the molecular level.

[0107] Specific examples of the compatible phosphorus compound (c1) include compounds containing phosphorus that do not form salts, such as phosphate ester compounds, phosphazene compounds, phosphite ester compounds, and phosphine compounds.

[0108] Examples of phosphazene compounds include cyclic and chain-like phosphazene compounds. Cyclic phosphazene compounds, also known as cyclophosphazenes, are compounds having a double bond in the molecule with phosphorus and nitrogen as constituent elements, and have a cyclic structure. Examples of phosphate ester compounds include triphenyl phosphate, tricresyl phosphate, xylenyl diphenyl phosphate, cresyl diphenyl phosphate, 1,3-phenylenebis(di-2,6-xylenyl phosphate), 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), condensed phosphate ester compounds such as aromatic condensed phosphate ester compounds, and cyclic phosphate ester compounds. Examples of phosphite ester compounds include trimethyl phosphite and triethyl phosphite. Examples of phosphine compounds include tris-(4-methoxyphenyl)phosphine and triphenylphosphine. The compatible phosphorus compounds may be used singly or in combination of two or more.

[0109] The incompatible phosphorus compound (c2) is not particularly limited as long as it acts as a flame retardant and is an incompatible phosphorus compound that is incompatible with the radical polymerizable compound (A). Here, "incompatible" means that the compound is not compatible with the radical polymerizable compound (A) and the target substance (phosphorus compound) is dispersed in the mixture like islands.

[0110] Specific examples of the incompatible phosphorus compound (c2) include compounds that contain phosphorus and form salts, such as phosphinate compounds, polyphosphate compounds, and phosphonium salt compounds, as well as phosphine oxide compounds.

[0111] Examples of phosphinate compounds include aluminum dialkylphosphinate, aluminum trisdiethylphosphinate, aluminum trismethylethylphosphinate, aluminum trisdiphenylphosphinate, zinc bisdiethylphosphinate, zinc bismethylethylphosphinate, zinc bisdiphenylphosphinate, titanyl bisdiethylphosphinate, titanyl bismethylethylphosphinate, and titanyl bisdiphenylphosphinate. Examples of polyphosphate compounds include melamine polyphosphate, melam polyphosphate, and melem polyphosphate. Examples of phosphonium salt compounds include tetraphenylphosphonium tetraphenylborate and tetraphenylphosphonium bromide. Examples of phosphine oxide compounds include phosphine oxide compounds (diphenylphosphine oxide compounds) having two or more diphenylphosphine oxide groups in the molecule, more specifically, paraxylylenebisdiphenylphosphine oxide. The incompatible phosphorus compounds may be used alone or in combination of two or more.

[0112] The content ratio of the compatible phosphorus compound (c1) to the incompatible phosphorus compound (c2) is preferably 1:1 to 1:3 by mass, and more preferably 1:2 to 2:3. Such a content ratio is believed to provide a resin composition with a high Tg in the cured product and excellent flame retardancy.

[0113] The resin composition according to the present embodiment may contain only the phosphorus compound (C) as described above as a flame retardant, or may contain a flame retardant other than the phosphorus compound (C). However, from the viewpoint of being halogen-free, it is preferable that the resin composition does not contain a halogen-based flame retardant.

[0114] When the resin composition of the present embodiment contains the phosphorus compound (C), the content thereof is preferably about 5 to 80 parts by mass, and more preferably about 10 to 60 parts by mass, per 100 parts by mass of the radical polymerizable compound (A).

[0115] (Reaction initiator) The resin composition of the present embodiment may further contain a reaction initiator. The radical polymerization (curing) reaction of the resin composition can proceed even without a reaction initiator. However, depending on the process conditions, it may be difficult to raise the temperature high enough for curing to proceed, so a reaction initiator may be added.

[0116] The reaction initiator is not particularly limited as long as it can accelerate the curing reaction of the resin composition. Specific examples include metal oxides, azo compounds, and peroxides, and preferably includes at least one of peroxides and azo compounds.

[0117] Specific examples of metal oxides include metal carboxylates.

[0118] Examples of organic peroxides include α,α'-di(t-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, benzoyl peroxide, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, chloranil, 2,4,6-tri-t-butylphenoxyl, t-butylperoxyisopropyl monocarbonate, and azobisisobutyronitrile.

[0119] Specific examples of the azo compound include 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(N-butyl-2-methylpropionamide), and 2,2'-azobis(2-methylbutyronitrile).

[0120] Among these, preferred reaction initiators are 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(N-butyl-2-methylpropionamide), etc. These reaction initiators have little effect on dielectric properties. In addition, because the reaction initiation temperature is relatively high, promotion of the curing reaction can be suppressed when curing is not necessary, such as during prepreg drying, which has the advantage of suppressing deterioration in the shelf life of the resin composition.

[0121] The above-mentioned reaction initiators may be used alone or in combination of two or more kinds.

[0122] When the resin composition of the present embodiment contains the reaction initiator, the content thereof is not particularly limited, but is, for example, preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 3.0 parts by mass, and even more preferably 0.5 to 2.0 parts by mass, relative to a total of 100 parts by mass of the radical polymerizable compound (A).

[0123] (Other Elastomers) Furthermore, in addition to the above-described radically polymerizable compound (A), the resin composition of the present embodiment may further contain a thermoplastic resin having no unsaturated group in order to more reliably ensure low dielectric properties, adhesive strength, and the like.

[0124] Examples of thermoplastic resins include thermoplastic polyphenylene ether resins, polyphenylene sulfide resins, liquid crystal polymers, polyethylene resins, polystyrene resins, polyurethane resins, polypropylene resins, ABS resins, acrylic resins, polyethylene terephthalate resins, polycarbonate resins, polyacetal resins, polyimide resins, polyamide-imide resins, polytetrafluoroethylene resins, cycloolefin polymers, cycloolefin copolymers, styrene-based elastomers, etc. The above resins may be used alone or in combination of two or more.

[0125] When the resin composition of the present embodiment contains a thermoplastic resin having no unsaturated group, the content thereof is preferably about 0.1 to 30 parts by mass, and more preferably about 1 to 15 parts by mass, per 100 parts by mass of the total of the radical polymerizable compound component (A) and the thermoplastic resin.

[0126] (Other Components) The resin composition according to the present embodiment may contain other components (other components) than the above-described components, as needed, within the scope of not impairing the effects of the present invention. Examples of other components contained in the resin composition according to the present embodiment may further include additives such as silane coupling agents, antifoaming agents, antioxidants, heat stabilizers, antistatic agents, ultraviolet absorbers, dyes, pigments, dispersants, and lubricants.

[0127] (Production Method) The method for producing the resin composition is not particularly limited, and examples thereof include a method of mixing the radical polymerizable compound (A) with other resin components as necessary, and then adding an inorganic filler, etc. Specifically, in the case of obtaining a varnish-like composition containing an organic solvent, the method described in the description of the prepreg below, etc., can be mentioned.

[0128] Furthermore, by using the resin composition according to this embodiment, it is possible to obtain a prepreg, a metal-clad laminate, a wiring board, a resin-coated metal foil, and a resin-coated film as follows: In the following description, the respective symbols represent the following: 1 prepreg, 2 resin composition or semi-cured resin composition, 3 fibrous substrate, 11 metal-clad laminate, 12 insulating layer, 13 metal foil, 14 wiring, 21 wiring board, 31 resin-coated metal foil, 32, 42 resin layer, 41 resin-coated film, 43 support film.

[0129] [Prepreg] FIG. 1 is a schematic cross-sectional view showing an example of a prepreg 1 according to an embodiment of the present invention.

[0130] 1, the prepreg 1 according to this embodiment comprises the resin composition or a semi-cured product of the resin composition 2, and a fibrous base material 3. This prepreg 1 comprises the resin composition or a semi-cured product of the resin composition 2, and the fibrous base material 3 present in the resin composition or the semi-cured product of the resin composition 2.

[0131] In this embodiment, the semi-cured product refers to a resin composition that has been partially cured to the extent that it can be further cured. That is, the semi-cured product refers to a resin composition that has been semi-cured (B-staged). For example, when a resin composition is heated, the viscosity initially gradually decreases, then curing begins, and then curing begins again, and the viscosity gradually increases. In such a case, the semi-cured state may refer to a state between when the viscosity begins to increase and when the composition is completely cured.

[0132] Furthermore, the prepreg obtained using the resin composition according to this embodiment may comprise a semi-cured product of the resin composition as described above, or may comprise the uncured resin composition itself. That is, it may be a prepreg comprising a semi-cured product of the resin composition (the resin composition in B stage) and a fibrous base material, or a prepreg comprising the resin composition before curing (the resin composition in A stage) and a fibrous base material. Furthermore, the resin composition or the semi-cured product of the resin composition may be the resin composition that has been dried or heat-dried.

[0133] When producing a prepreg, the resin composition 2 is often prepared in a varnish form and used to impregnate the fibrous base material 3, which is the base material for forming the prepreg. That is, the resin composition 2 is usually often a resin varnish prepared in a varnish form. Such a varnish-like resin composition (resin varnish) is prepared, for example, as follows.

[0134] First, each component of the resin composition that is soluble in an organic solvent is added to the organic solvent and dissolved. Heating may be performed as necessary. Subsequently, components that are insoluble in the organic solvent (e.g., inorganic fillers, etc.) are added as needed, and the mixture is dispersed using a ball mill, bead mill, planetary mixer, roll mill, etc. until a predetermined dispersion state is achieved, thereby preparing a varnish-like resin composition. The organic solvent used here is not particularly limited as long as it dissolves the radical polymerizable compound and the like and does not inhibit the curing reaction. Specific examples include toluene and methyl ethyl ketone (MEK).

[0135] The method for producing the prepreg is not particularly limited as long as it can produce the prepreg. Specifically, when producing the prepreg, the resin composition used in the present embodiment is often prepared in the form of a varnish as described above and used as a resin varnish.

[0136] Specific examples of the fibrous substrate include glass cloth, aramid cloth, polyester cloth, glass nonwoven fabric, aramid nonwoven fabric, polyester nonwoven fabric, pulp paper, and linter paper. The use of glass cloth provides a laminate with excellent mechanical strength, and flattened glass cloth is particularly preferred. A specific example of the flattening process is a method in which glass cloth is continuously pressed with a press roll at an appropriate pressure to compress the yarns flat. The thickness of commonly used fibrous substrates is, for example, 0.01 mm or more and 0.3 mm or less.

[0137] The method for producing the prepreg is not particularly limited as long as it can produce the prepreg. Specifically, when producing the prepreg, the resin composition according to the present embodiment is often prepared in the form of a varnish as described above and used as a resin varnish.

[0138] The prepreg 1 can be produced, for example, by impregnating a fibrous substrate 3 with a resin composition 2, for example, a resin composition 2 prepared in a varnish form, followed by drying. The resin composition 2 is impregnated into the fibrous substrate 3 by immersion, coating, or the like. Impregnation can be repeated multiple times as necessary. In this case, by repeating the impregnation using multiple resin compositions with different compositions and concentrations, it is possible to adjust the final composition and impregnation amount to the desired one.

[0139] The fibrous substrate 3 impregnated with the resin composition (resin varnish) 2 is heated under desired conditions, for example, at 80°C to 180°C for 1 minute to 10 minutes. This heating produces a prepreg 1 in an uncured (A-stage) or semi-cured (B-stage) state. The heating also volatilizes the organic solvent from the resin varnish, reducing or eliminating the organic solvent.

[0140] [Metal-clad laminate] FIG. 2 is a schematic cross-sectional view showing an example of a metal-clad laminate 11 according to an embodiment of the present invention.

[0141] As shown in FIG. 2, the metal-clad laminate 11 is composed of an insulating layer 12 containing a cured product of the prepreg 1 shown in FIG. 1 and a metal foil 13 laminated together with the insulating layer 12. That is, the metal-clad laminate 11 has an insulating layer 12 containing a cured product of a resin composition and a metal foil 13 provided on the insulating layer 12. The insulating layer 12 may be composed of either a cured product of the resin composition or a cured product of the prepreg. The thickness of the metal foil 13 varies depending on the performance required of the final wiring board and is not particularly limited. The thickness of the metal foil 13 can be appropriately set depending on the desired purpose, and is preferably, for example, 0.2 to 70 μm. Examples of the metal foil 13 include copper foil and aluminum foil. When the metal foil is thin, it may be a carrier-attached copper foil equipped with a release layer and a carrier to improve handling.

[0142] The method for producing the metal-clad laminate 11 is not particularly limited as long as it can produce the metal-clad laminate 11. Specifically, a method for producing the metal-clad laminate 11 using a prepreg 1 can be used. Examples of such a method include stacking one or more prepregs 1, placing a metal foil 13 such as copper foil on both sides or one side of the prepreg 1, and then heat-pressing and molding the metal foil 13 and the prepreg 1 to form an integrated laminate. In other words, the metal-clad laminate 11 can be obtained by laminating the metal foil 13 on the prepreg 1 and then heat-pressing and molding the laminate. The heat-pressing conditions can be appropriately set depending on the thickness of the metal-clad laminate 11 to be produced, the type of composition of the prepreg 1, and other factors. For example, the temperature can be 170 to 230°C, the pressure can be 3 to 5 MPa, and the time can be 60 to 150 minutes. The metal-clad laminate can also be produced without using a prepreg. For example, a method may be used in which a varnish-like resin composition is applied onto a metal foil to form a layer containing the resin composition on the metal foil, and then the layer is heated and pressed.

[0143] [Wiring Board] FIG. 3 is a schematic cross-sectional view showing an example of a wiring board 21 according to an embodiment of the present invention.

[0144] 3, wiring board 21 according to this embodiment is composed of insulating layer 12, which is formed by curing prepreg 1 shown in FIG. 1, and wiring 14, which is laminated together with insulating layer 12 and formed by partially removing metal foil 13. That is, wiring board 21 has insulating layer 12 containing a cured product of a resin composition, and wiring 14 provided on insulating layer 12. Furthermore, insulating layer 12 may be made of a cured product of the resin composition, or may be made of a cured product of the prepreg.

[0145] The method for manufacturing the wiring board 21 is not particularly limited as long as the wiring board 21 can be manufactured. Specific examples include a method of manufacturing the wiring board 21 using the prepreg 1. Examples of this method include a method of manufacturing the wiring board 21 in which wiring is provided as a circuit on the surface of the insulating layer 12 by etching the metal foil 13 on the surface of the metal-clad laminate 11 manufactured as described above. That is, the wiring board 21 is obtained by forming a circuit by partially removing the metal foil 13 on the surface of the metal-clad laminate 11. In addition to the above methods, examples of the method for forming a circuit include circuit formation by a semi-additive process (SAP) or a modified semi-additive process (MSAP).

[0146] [Resin-Coated Metal Foil] FIG. 4 is a schematic cross-sectional view showing an example of a resin-coated metal foil 31 according to this embodiment.

[0147] As shown in Fig. 4, the resin-coated metal foil 31 according to this embodiment comprises a resin layer 32 containing the resin composition or a semi-cured product of the resin composition, and a metal foil 13. The resin-coated metal foil 31 has the metal foil 13 on the surface of the resin layer 32. That is, the resin-coated metal foil 31 comprises the resin layer 32 and the metal foil 13 laminated together with the resin layer 32. The resin-coated metal foil 31 may also comprise another layer between the resin layer 32 and the metal foil 13.

[0148] The resin layer 32 may contain a semi-cured product of the resin composition as described above, or may contain the uncured resin composition. That is, the resin-coated metal foil 31 may comprise a resin layer containing a semi-cured product of the resin composition (the resin composition in B-stage) and a metal foil, or a resin layer containing the resin composition before curing (the resin composition in A-stage) and a metal foil. The resin layer may contain the resin composition or a semi-cured product of the resin composition, and may or may not contain a fibrous substrate. The resin composition or the semi-cured product of the resin composition may be obtained by drying or heat-drying the resin composition. The fibrous substrate may be the same as the fibrous substrate of a prepreg.

[0149] The metal foil may be any metal foil used in metal-clad laminates, including, for example, copper foil and aluminum foil.

[0150] The resin-coated metal foil 31 and the resin-coated film 41 may be provided with a cover film or the like, as necessary. By providing a cover film, it is possible to prevent the inclusion of foreign matter, etc. The cover film is not particularly limited, but examples thereof include polyolefin film, polyester film, polymethylpentene film, and films formed by providing a release agent layer on these films.

[0151] The method for producing the resin-coated metal foil 31 is not particularly limited as long as the resin-coated metal foil 31 can be produced. Examples of the method for producing the resin-coated metal foil 31 include a method of applying the varnish-like resin composition (resin varnish) to the metal foil 13 and heating the applied resin composition. The varnish-like resin composition is applied to the metal foil 13 using, for example, a bar coater. The applied resin composition is heated, for example, at 40°C or higher and 180°C or lower for 1 minute or longer and 10 minutes or shorter. The heated resin composition is formed on the metal foil 13 as an uncured resin layer 32. The heating volatilizes the organic solvent from the resin varnish, thereby reducing or removing the organic solvent.

[0152] [Resin-Coated Film] FIG. 5 is a schematic cross-sectional view showing an example of a resin-coated film 41 according to this embodiment.

[0153] 5 , the resin-coated film 41 according to this embodiment includes a resin layer 42 containing the resin composition or a semi-cured product of the resin composition, and a support film 43. The resin-coated film 41 includes the resin layer 42 and the support film 43 laminated together with the resin layer 42. The resin-coated film 41 may also include another layer between the resin layer 42 and the support film 43.

[0154] The resin layer 42 may contain a semi-cured product of the resin composition as described above, or may contain the uncured resin composition. That is, the resin-coated film 41 may comprise a resin layer containing a semi-cured product of the resin composition (the resin composition in B-stage) and a support film, or a resin-coated film comprising a resin layer containing the resin composition before curing (the resin composition in A-stage) and a support film. The resin layer may contain the resin composition or a semi-cured product of the resin composition, and may or may not contain a fibrous substrate. The resin composition or the semi-cured product of the resin composition may be obtained by drying or heat-drying the resin composition. The fibrous substrate may be the same as the fibrous substrate of a prepreg.

[0155] Furthermore, any support film used for a resin-coated film can be used without limitation as the support film 43. Examples of the support film include electrically insulating films such as polyester film, polyethylene terephthalate (PET) film, polyimide film, polyparabanic acid film, polyether ether ketone film, polyphenylene sulfide film, polyamide film, polycarbonate film, and polyarylate film.

[0156] The resin-coated film 41 may be provided with a cover film or the like as necessary. By providing a cover film, it is possible to prevent the inclusion of foreign matter, etc. The cover film is not particularly limited, but examples thereof include a polyolefin film, a polyester film, and a polymethylpentene film.

[0157] The support film and cover film may be subjected to surface treatment such as matte treatment, corona treatment, release treatment, and roughening treatment, if necessary.

[0158] The method for producing the resin-coated film 41 is not particularly limited as long as it can produce the resin-coated film 41. Examples of methods for producing the resin-coated film 41 include a method in which the varnish-like resin composition (resin varnish) is applied to a support film 43 and heated. The varnish-like resin composition is applied to the support film 43 using, for example, a bar coater. The applied resin composition is heated, for example, at 40°C or higher and 180°C or lower for 1 minute or longer and 10 minutes or shorter. The heated resin composition is formed on the support film 43 as an uncured resin layer 42. The heating can volatilize the organic solvent from the resin varnish, thereby reducing or removing the organic solvent.

[0159] The prepreg, resin-coated film, and resin-coated metal foil obtained using the resin composition of this embodiment have excellent low dielectric properties, high thermal conductivity, and excellent adhesion when cured, making them very useful for industrial applications. Furthermore, metal-clad laminates and wiring boards having an insulating layer containing the cured resin composition of this embodiment also have the advantages of low dielectric properties, high thermal conductivity, and excellent adhesion.

[0160] This specification discloses various aspects of the technology as described above, but the main technologies among them are summarized below.

[0161] A resin composition according to a first aspect of the present invention is a resin composition comprising a radical polymerizable compound (A) and an inorganic filler (B), wherein the inorganic filler (B) comprises a boron nitride filler (b1), and the particle size distribution of the boron nitride filler (b1) is characterized in that the particle size (D10) at 10% cumulative total is 0.5 to 2.0 μm, the particle size (D50) at 50% cumulative total is 4.0 to 6.0 μm, and the particle size (D90) at 90% cumulative total is 6.5 to 20.0 μm.

[0162] A resin composition according to a second aspect of the present invention is the resin composition according to the first aspect, wherein the boron nitride filler (b1) has an average aspect ratio (maximum length on the main surface / thickness in the direction perpendicular to the main surface) of 6 to 20.

[0163] A resin composition according to a third aspect of the present invention is the resin composition of the first or second aspect, wherein the radical polymerizable compound (A) comprises at least one selected from the group consisting of a polyphenylene ether compound having a carbon-carbon unsaturated double bond in the molecule, a hydrocarbon compound having a carbon-carbon unsaturated double bond in the molecule, a maleimide compound, and an allyl compound.

[0164] A resin composition according to a fourth aspect of the present invention is the resin composition according to any one of the first to third aspects, wherein the content of the inorganic filler (B) is 5 to 70 parts by volume per 100 parts by volume of the radical polymerizable compound (A).

[0165] A resin composition according to a fifth aspect of the present invention is the resin composition according to any one of the first to fourth aspects, wherein the content of the boron nitride filler (b1) is 5 to 50 parts by volume per 100 parts by volume (solid content) of the radical polymerizable compound (A).

[0166] A resin composition according to a sixth aspect of the present invention is a resin composition according to any one of the first to fifth aspects, wherein the inorganic filler (B) comprises a silica filler (b2).

[0167] A resin composition according to a seventh aspect of the present invention is the resin composition according to the sixth aspect, wherein the volume content ratio of the boron nitride filler (b1) to the silica filler (b) in the inorganic filler (B) (volume content of the boron nitride filler (b1) / volume content of the silica filler (b)) is 1 to 4.

[0168] A resin composition according to an eighth aspect of the present invention is the resin composition according to any one of the first to seventh aspects, further comprising a phosphorus compound (C).

[0169] A resin composition according to a ninth aspect of the present invention is the resin composition of the eighth aspect, wherein the phosphorus compound (C) includes a compatible phosphorus compound (c1) that is compatible with the radical polymerizable compound (A) and an incompatible phosphorus compound (c2) that is incompatible with the radical polymerizable compound (A).

[0170] A resin composition according to a tenth aspect of the present invention is the resin composition of the ninth aspect, wherein the compatible phosphorus compound (c1) comprises at least one selected from the group consisting of a phosphate ester compound, a phosphazene compound, a phosphite ester compound, and a phosphine compound.

[0171] A resin composition according to an eleventh aspect of the present invention is the resin composition of the ninth aspect, wherein the incompatible phosphorus compound (c2) includes at least one selected from the group consisting of phosphinate compounds, polyphosphate compounds, phosphonium salt compounds, and phosphine oxide compounds.

[0172] A resin composition according to a twelfth aspect of the present invention is the resin composition according to any one of the first to eleventh aspects, wherein the thermal conductivity of the cured product is 1.0 W / mK or more and the relative dielectric constant of the cured product is 4.0 or less.

[0173] A prepreg according to a thirteenth aspect of the present invention comprises the resin composition of any one of the first to twelfth aspects or a semi-cured product of the resin composition, and a fibrous base material.

[0174] A resin-coated film according to a fourteenth aspect of the present invention comprises a resin layer containing the resin composition of any one of the first to twelfth aspects or a semi-cured product of the resin composition, and a support film.

[0175] A resin-coated metal foil according to a fifteenth aspect of the present invention comprises a resin layer containing the resin composition of any one of the first to twelfth aspects or a semi-cured product of the resin composition, and a metal foil.

[0176] A metal-clad laminate according to a sixteenth aspect of the present invention has an insulating layer containing a cured product of the resin composition according to any one of the first to twelfth aspects or a cured product of the prepreg according to the thirteenth aspect, and a metal foil.

[0177] A wiring board according to a seventeenth aspect of the present invention has an insulating layer containing a cured product of the resin composition of any one of the first to twelfth aspects or a cured product of the prepreg of the thirteenth aspect, and wiring.

[0178] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0179] Examples 1 to 9 and Comparative Examples 1 to 8 In these examples, each component used in preparing the resin composition will be described.

[0180] <Radical Polymerizable Compound (A)> (Radical Polymerizable Compound (A1)) PPE1: polyphenylene ether compound having a methacryloyl group at its terminal (SA9000 manufactured by SABIC Innovative Plastics, weight average molecular weight Mw 2000, number of terminal functional groups 2)

[0181] PPE2: A modified polyphenylene ether obtained by reacting polyphenylene ether with chloromethylstyrene. Specifically, this modified polyphenylene ether was obtained by the following reaction.

[0182] First, 200 g of polyphenylene ether (SA90 manufactured by SABIC Innovative Plastics, 2 terminal hydroxyl groups, weight average molecular weight Mw 1700), 30 g of a 50:50 mass ratio mixture of p-chloromethylstyrene and m-chloromethylstyrene (chloromethylstyrene: CMS manufactured by Tokyo Chemical Industry Co., Ltd.), 1.227 g of tetra-n-butylammonium bromide as a phase transfer catalyst, and 400 g of toluene were charged into a 1-liter three-neck flask equipped with a temperature controller, a stirrer, a cooling device, and a dropping funnel, and the mixture was stirred. The polyphenylene ether, chloromethylstyrene, and tetra-n-butylammonium bromide were stirred until they were dissolved in toluene. The mixture was gradually heated, and finally heated until the liquid temperature reached 75 ° C. Then, an aqueous sodium hydroxide solution (20 g sodium hydroxide / 20 g water) was added dropwise to the solution as an alkali metal hydroxide over 20 minutes. The mixture was then stirred at 75°C for an additional 4 hours. Next, the contents of the flask were neutralized with 10% by mass hydrochloric acid, and a large amount of methanol was added. This caused a precipitate to form in the liquid in the flask. That is, the product contained in the reaction solution in the flask was reprecipitated. The precipitate was then filtered, washed three times with a mixture of methanol and water in a mass ratio of 80:20, and then dried under reduced pressure at 80°C for 3 hours.

[0183] The obtained solid is 1 H-NMR (400MHz, CDCl 3 , TMS). As a result of NMR measurement, a peak derived from a vinylbenzyl group (ethenylbenzyl group) was confirmed at 5 to 7 ppm. This confirmed that the obtained solid was a modified polyphenylene ether compound having a vinylbenzyl group (ethenylbenzyl group) as the substituent at the molecular end in the molecule. Specifically, it was confirmed that it was an ethenylbenzylated polyphenylene ether. The obtained modified polyphenylene ether compound was represented by the above formula (14), in which Y is a dimethylmethylene group (represented by formula (12), and R in formula (12) 33 and R 34 is a methyl group), Z is a phenylene group, and R 1The compound was a modified polyphenylene ether compound in which R3 was a hydrogen atom and n was 1.

[0184] The number of terminal functional groups of the modified polyphenylene ether was measured as follows.

[0185] First, the modified polyphenylene ether was accurately weighed. The weight at that time was designated X (mg). Then, this weighed modified polyphenylene ether was dissolved in 25 mL of methylene chloride, and 100 μL of a 10 mass% ethanol solution of tetraethylammonium hydroxide (TEAH) (TEAH:ethanol (volume ratio) = 15:85) was added to the solution, and the absorbance (Abs) at 318 nm was measured using a UV spectrophotometer (UV-1600 manufactured by Shimadzu Corporation). Then, from the measurement results, the number of terminal hydroxyl groups of the modified polyphenylene ether was calculated using the following formula.

[0186] Residual OH amount (μmol / g) = [(25×Abs) / (ε×OPL×X)]×10 6 Here, ε is the extinction coefficient and is 4700 L / mol·cm, and OPL is the cell optical path length and is 1 cm.

[0187] The calculated residual OH amount (number of terminal hydroxyl groups) of the modified polyphenylene ether was almost zero, which indicated that the hydroxyl groups of the polyphenylene ether before modification were almost entirely modified. This indicated that the decrease from the number of terminal hydroxyl groups of the polyphenylene ether before modification was the number of terminal hydroxyl groups of the polyphenylene ether before modification. In other words, it was found that the number of terminal hydroxyl groups of the polyphenylene ether before modification was the number of terminal functional groups of the modified polyphenylene ether. In other words, the number of terminal functional groups was two.

[0188] The molecular weight distribution of the modified polyphenylene ether was measured by GPC. The weight average molecular weight (Mw) was calculated from the molecular weight distribution. The Mw was found to be 1,900.

[0189] (Radical polymerizable compound (A2)) Allyl compound: triallyl isocyanurate (TAIC) (TAIC manufactured by Nippon Kasei Chemical Co., Ltd.) Vinyl compound: divinylbenzene (DVB manufactured by Nippon Steel & Sumitomo Metal Corporation)

[0190] <Inorganic filler (B)> (Boron nitride filler (b1)) Boron nitride filler 1: "SGP" manufactured by Denka Company Limited Boron nitride filler 2: "AP10S" manufactured by MARUKA Corporation Boron nitride filler 3: "ABN-5" manufactured by Hyaku ■ High-Tech Materials Technology Co., Ltd. (■ Hakuni Gamae Nitride Fuyu) (Silica filler (b2)) Silica filler: "FB-7SDC" manufactured by Denka Company Limited (Other inorganic fillers) Aluminum oxide filler: "DAW-03DC" manufactured by Denka Company Limited

[0191] <Phosphorus Compound (C)> Compatible phosphorus compound (c1): aromatic condensed phosphate ester compound (PX-200, manufactured by Daihachi Chemical Industry Co., Ltd.) Incompatible phosphorus compound (c2): diphenylphosphine oxide compound, PQ60, manufactured by Shinichi Chemical Co., Ltd.

[0192] <Reaction initiator> Organic peroxide: PBP (1,3-bis(butylperoxyisopropyl)benzene; Perbutyl P manufactured by NOF Corporation)

[0193] (Preparation Method) First, each component other than the inorganic filler was added to toluene in the composition shown in Table 1 in parts by mass (parts by volume of inorganic filler only) and mixed. The mixture was stirred for 60 minutes. Thereafter, the filler (parts by mass) was added to the resulting liquid, and the amount of toluene added was adjusted so that the solids concentration of the resin composition after dispersion was 65 parts by mass. The mixture was then stirred for 60 minutes to perform primary dispersion of the filler. The inorganic filler was then subjected to secondary dispersion using a bead mill to obtain a varnish-like resin composition (varnish).

[0194] Next, an evaluation substrate (cured prepreg) was obtained as follows.

[0195] A fibrous substrate (glass cloth: #1078 type, L glass, manufactured by Asahi Kasei Corporation) was impregnated with the resulting varnish and then heated and dried for 3 minutes at 120°C to produce a prepreg. One of each of the resulting prepregs was then stacked, and copper foil (FV-WS, manufactured by Furukawa Electric Co., Ltd., copper foil thickness: 35µm) was attached to both sides of the stack. The stack was heated to 200°C at a heating rate of 4°C / min, and heated and pressed at 200°C for 120 minutes at a pressure of 3 MPa to produce a copper-clad laminate with a thickness of 130µm.

[0196] Test Example 1 In the measurement of thermal conductivity described below, cured prepregs having three different thicknesses were used, and in the evaluation test of dielectric properties (dielectric constant), a copper-clad laminate having four prepregs from which the copper foil had been removed (cured prepreg) was used.

[0197] To evaluate moldability and adhesion, four prepregs prepared as described above were stacked to prepare a copper-clad laminate with a thickness of 0.5 mm and a copper foil thickness of 18 μm. A grid pattern with a residual copper ratio of 50% was formed on the surface of the laminate. This laminate was used as the core material, and prepregs were placed on both sides, followed by secondary molding. The copper foil on the surface was then etched. The laminate obtained by the above method (evaluation substrate 1) was used in moldability and adhesion tests.

[0198] Each of the evaluation samples prepared as described above was evaluated by the following methods.

[0199] [Particle size distribution of boron nitride filler] The particle size distribution of the boron nitride filler in each example and comparative example was determined by measurement using a laser diffraction / scattering particle size distribution measuring device LA-960V2 (manufactured by Horiba, Ltd.). The specifications of the device are as follows: Measurement principle: Mie scattering theory Measurement method: Flow measurement Measurement range: 0.01 μm to 5000 μm Light source: LD (650 nm), approximately 5 mW, LED (405 mm), approximately 3 mW Detector: 1 ring-shaped 64-segment silicon photodiode, 5 4-channel array detectors, 3 silicon photodetectors Refractive index: 2.250-0.005i

[0200] The specifications of the measurement unit (circulation system) are as follows: Dispersion: ultrasonic probe Circulation: centrifugal pump Mixing: rotor Flow cell material: synthetic quartz

[0201] The particle size distribution measurement conditions are as follows.

[0202] Each measurement sample was placed in a flow cell via a sample bath using toluene as a dispersion solvent, and laser diffraction / scattering particle size distribution measurement was carried out in a stirred state.

[0203] The particle size distribution was analyzed and calculated using the analysis software LA-960 for Windows attached to the LA-960V2. The peak in the particle size distribution was determined by calculating the volume ratio of the measured particle size distribution.

[0204] [Average Aspect Ratio of Boron Nitride Filler] The aspect ratio was defined as the maximum length on the main surface divided by the thickness in the direction perpendicular to the main surface. Using a scanning electron microscope (Flex SEM1000II manufactured by Hitachi High-Technologies Corporation), the maximum length on the main surface of the boron nitride filler particle divided by the thickness in the direction perpendicular to the main surface was measured for n = 10, and the average aspect ratio was calculated.

[0205] [Dielectric Properties (Dielectric Constant)] The dielectric constant (Dk) of the evaluation substrate (cured prepreg) at 10 GHz was measured by a cavity resonator perturbation method. Specifically, the dielectric loss tangent of the evaluation substrate at 10 GHz was measured using a network analyzer (N5230A manufactured by Keysight Technologies, Inc.). The pass criterion in this example was Dk<4.0.

[0206] [Moldability] Regarding moldability, the evaluation substrate 1 was visually observed, and those in which voids were observed were rated as "failed," and those in which no voids were observed were rated as "passed."

[0207] [Adhesion] Regarding adhesion, boiling solder heat resistance was evaluated using the evaluation board 1. First, the evaluation board 1 was boiled in hot water for 4 hours, and then immersed in a solder bath at 288°C for 20 seconds. The immersed sample was visually inspected for the occurrence of blistering. Samples that blistered were judged as "failed," and samples that did not blister were judged as "passed."

[0208] [Thermal Conductivity] The thermal conductivity of the obtained evaluation substrate (cured product of prepreg) was measured by a method in accordance with ASTM D5470. Specifically, the thermal conductivity of the obtained evaluation substrate (cured product of four laminated prepregs) was measured using a thermal property evaluation device (T3Ster DynTIM Tester manufactured by Mentor Graphics). The pass criterion for thermal conductivity in this example was set to 1.0 W / m K or more.

[0209] The results of the above evaluations are shown in Table 1.

[0210]

[0211] (Discussion) As can be seen from Table 1, in all of the examples using the resin composition of the present invention, it was possible to obtain a cured product having low dielectric properties (relative dielectric constant) (Dk<4.0) and high thermal conductivity (1.0 W / m·K or more), and it was confirmed that a resin composition having adhesion under conditions more severe than those hitherto available could be provided.

[0212] On the other hand, Comparative Examples 1-2, 5, and 7, which used boron nitride fillers whose D10, D50, and D90 in the particle size distribution were all larger than the limits of the present invention, resulted in poor moldability. Furthermore, Comparative Examples 3-4 and 6, which used boron nitride fillers whose D10, D50, and D90 in the particle size distribution were all smaller than the limits of the present invention, also failed to achieve a level of adhesion sufficient for substrate production. Furthermore, Comparative Example 8, which did not contain a boron nitride filler, failed to achieve sufficient thermal conductivity.

[0213] This application is based on Japanese Patent Application No. 2023-57185, filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0214] In order to express the present invention, the present invention has been properly and sufficiently described above through embodiments with reference to specific examples, drawings, etc., but it should be recognized that those skilled in the art can easily make changes and / or improvements to the above-described embodiments. Therefore, unless changes or improvements made by those skilled in the art deviate from the scope of the claims set forth in the claims, such changes or improvements are construed as being encompassed within the scope of the claims.

[0215] The present invention has wide industrial applicability in the technical fields of electronic materials, electronic devices, optical devices, and the like.

Claims

1. A resin composition comprising a radically polymerizable compound (A) and an inorganic filler (B), wherein the inorganic filler (B) comprises a boron nitride filler (b1), and the particle size distribution of the boron nitride filler (b1) has a particle size (D10) at 10% cumulative total of 0.5 to 2.0 μm, a particle size (D50) at 50% cumulative total of 4.0 to 6.0 μm, and a particle size (D90) at 90% cumulative total of 6.5 to 20.0 μm.

2. The resin composition according to claim 1, wherein the average aspect ratio of the boron nitride filler (b1) (maximum length on the main surface / thickness in the direction perpendicular to the main surface) is 6 to 20.

3. The resin composition according to claim 1, wherein the radical polymerizable compound (A) comprises at least one selected from the group consisting of a polyphenylene ether compound having a carbon-carbon unsaturated double bond in the molecule, a hydrocarbon compound having a carbon-carbon unsaturated double bond in the molecule, a maleimide compound, and an allyl compound.

4. The resin composition according to claim 1, wherein the content of the inorganic filler (B) is 5 to 70 parts by volume per 100 parts by volume of the radical polymerizable compound (A).

5. The resin composition according to claim 1, wherein the content of the boron nitride filler (b1) is 5 to 50 parts by volume per 100 parts by volume of the radical polymerizable compound (A).

6. The resin composition according to claim 1, wherein the inorganic filler (B) comprises a silica filler (b2).

7. The resin composition according to claim 6, wherein in the inorganic filler (B), the volume content ratio of the boron nitride filler (b1) to the silica filler (b) (volume content of the boron nitride filler (b1) / volume content of the silica filler (b)) is 1 to 4.

8. The resin composition according to claim 1, further comprising a phosphorus compound (C).

9. The resin composition described in claim 8, wherein the phosphorus compound (C) includes a compatible phosphorus compound (c1) that is soluble in the radical polymerizable compound (A) and an incompatible phosphorus compound (c2) that is insoluble in the radical polymerizable compound (A).

10. The resin composition according to claim 9, wherein the compatible phosphorus compound (c1) comprises at least one selected from the group consisting of phosphate ester compounds, phosphazene compounds, phosphite ester compounds, and phosphine compounds.

11. The resin composition according to claim 9, wherein the incompatible phosphorus compound (c2) comprises at least one selected from the group consisting of a phosphinate compound, a polyphosphate compound, a phosphonium salt compound, and a phosphine oxide compound.

12. The resin composition according to claim 1, wherein the cured product has a thermal conductivity of 1.0 W / mK or more and a relative dielectric constant of 4.0 or less.

13. A prepreg comprising the resin composition according to any one of claims 1 to 12 or a semi-cured product of said resin composition and a fibrous base material.

14. A resin-coated film comprising a resin layer containing the resin composition according to any one of claims 1 to 12 or a semi-cured product of said resin composition, and a support film.

15. A resin-coated metal foil comprising a resin layer containing the resin composition according to any one of claims 1 to 12 or a semi-cured product of said resin composition, and a metal foil.

16. A metal-clad laminate comprising an insulating layer containing a cured product of the resin composition according to any one of claims 1 to 12, and a metal foil.

17. A wiring board comprising an insulating layer containing a cured product of the resin composition according to any one of claims 1 to 12, and wiring.

18. A metal-clad laminate comprising an insulating layer containing the cured product of the prepreg according to claim 13 and a metal foil.

19. A wiring board comprising an insulating layer containing the cured product of the prepreg according to claim 13 and wiring.

Citation Information

Patent Citations

  • Hexagonal boron nitride sintered compact having low density and low gas permeability and method of producing the same

    JP2001348276A

  • Heat-dissipating resin composition, substrate for LED mounting, and reflector

    JP2010100682A

  • Thermal conductivity rubber composition that excels in insulation, flame retardancy, mechanical property, and flexibility, and where circuit contact failure is not caused, molding and sheet comprising the rubber composition, and manufacturing method of the same

    JP2013127035A

  • Circuit connection material, connection structure of circuit member and manufacturing method of connection structure of circuit member

    JP2015096603A

  • Boron nitride agglomerate, thermosetting resin composition containing same, and use thereof

    US20210221743A1

Cited By

  • Resin composition, and prepreg, film with resin, metal foil with resin, metal-clad laminate, and wiring board each using same

    WO2025142543A1